Crosslinked Aliphatic Polyketones

Crosslinking aliphatic polyketones with diamine sources forms imine groups, addressing heat and mechanical stability issues, enabling efficient, solvent-free processing and expanding application possibilities.

JP7560563B2Active Publication Date: 2024-10-02CARL FREUDENBERG KG
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022546691
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-18
Filing Date
2021-02-05
Publication Date
2024-10-02
Estimated Expiration
2041-02-05

AI Technical Summary

Technical Problem

Existing thermoplastic aliphatic polyketones suffer from limitations in heat resistance and mechanical stability, which restrict their application potential, particularly due to their low continuous use temperature and brittleness, and current crosslinking methods are complex, solvent-dependent, and unsuitable for thermoplastic processing.

Method used

Crosslinking aliphatic polyketones with a diamine source to form imine groups, using di(aminophenyl) compounds or polyamides, allowing for thermoplastic processing without solvents and achieving improved heat resistance and mechanical stability.

Benefits of technology

The method results in aliphatic polyketones with enhanced heat resistance, higher maximum use temperature, improved stiffness, and reduced flammability, while maintaining good processability and chemical resistance, suitable for various industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560563000033
    Figure 0007560563000033
  • Figure 0007560563000034
    Figure 0007560563000034
  • Figure 0007560563000001
    Figure 0007560563000001
Patent Text Reader

Abstract

The present invention relates to moldings comprising a polymer matrix containing crosslinked aliphatic polyketones (PK), as well as to a method for producing such moldings. Furthermore, the invention relates to the use of such moldings in the fields of automotive, maritime, aviation and spaceflight, rail vehicles, the oil and gas industry, the food and packaging industry, and medical technology, in particular as sealing articles, thrust washers, backup rings, valves, connectors, insulators, snap hooks, bearings, bushings, films, powders, coatings, fibers, seals and O-rings, pipes and conduits, cables, sheathing and jacketing, and housings for electrical or chemical applications, comprising or consisting of such moldings.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a molding comprising a polymer matrix containing crosslinked aliphatic polyketones (PK), as well as a method for producing such a molding.Furthermore, the present invention relates to the use of such moldings in the fields of automotive, maritime, aviation and spaceflight, rail vehicles, oil and gas industry, food and packaging industry and medical technology, in particular as sealing articles, thrust washers, backup rings, valves, connectors, insulators, snap hooks, bearings, bushings, films, powders, coatings, fibers, sealing and O-rings, pipes and conduits, cables, jackets and jackets, and housings for electrical or chemical applications, comprising or consisting of such moldings.

[0002] 2. Background of the Invention Thermoplastically processable plastics (thermoplastics) are widespread due to the productivity of their manufacture, reversible deformability and in many cases due to their high-quality technical properties, and today they are standard products in industrial production. Thermoplastics consist of essentially linear polymer chains, i.e. they are not crosslinked and are generally only slightly branched or unbranched. However, thermoplastics have inherent conditioned limitations with regard to their heat resistance and are therefore not optimal for all application areas of polymeric materials. It is therefore desirable to increase the heat resistance of thermoplastics without sacrificing advantages such as processability, good mechanical properties or high chemical resistance. Here, multiply crosslinked polymers (thermosetting resins, thermosets), in which the macromolecules are linked to each other by covalent bonds, are advantageous. At low temperatures, they are in a hard-elastic state, also called the glass range. If thermosetting resins are heated beyond this range, they generally quickly reach the range of thermal decomposition. There is therefore great interest in developing materials that combine the advantages of both thermoplastic and thermosetting resins, i.e., materials that can be cheaply deformed and at the same time exhibit high resistance to heat deformation.

[0003] Aliphatic polyketones (PK) are thermoplastics with good mechanical properties, especially high impact strength and good resistance to media. They have an alternating structure of ethylene or propylene groups, respectively followed by keto groups (carbonyl groups), where the proportion of propylene groups is generally small and variable. PK is distinguished in particular by good strength properties, high impact strength values ​​at low temperatures, high mechanical fatigue strength, low tendency to creep deformation, and good sliding and wear behavior.

[0004] Aliphatic polyketones (PK) are linearly constructed polymers made from carbon monoxide and α-olefins, where the monomer units in the polymer chain are strictly alternating. Today, instead of the classical polyketone copolymers made only from carbon monoxide and ethylene, almost exclusively polyketone terpolymers are used. These polyketone terpolymers consist of carbon monoxide, ethylene and preferably small amounts of propylene.

[0005] [ka]

[0006] The reason for using terpolymers instead of copolymers is the significantly reduced brittleness of terpolymers. Due to their strictly alternating polymer chains with a very low defect rate (one defect per million monomer units) and the large number of polar keto groups, polyketone copolymers of carbon monoxide and ethylene are highly crystalline and very hard, but also very brittle, significantly limiting their potential applications as polymer materials. By adding a small amount of propylene (about 5%) during the synthesis, it was possible to disrupt the crystallinity and reduce the melting point from 255°C (copolymer of carbon monoxide and ethylene) to 220°C (terpolymer), resulting in a very tough polymer that is not brittle. Among them, aliphatic polyketones stand out in terms of high impact strength, low creep behavior, high chemical resistance, and good tribological properties. However, PK also has inherent limitations in terms of heat resistance, typical of thermoplastics, as mentioned above. It is therefore disadvantageous to use PK at maximum continuous use temperatures of about 80°C to 100°C (heat distortion resistance HDT / A according to ISO 75). The application possibilities of this polymer class are therefore significantly limited.

[0007] It would therefore be advantageous to be able to increase the continuous use temperature of aliphatic polyketones. To further increase the heat resistance and mechanical stability of PK, it was proposed to crosslink the polymer chains. This principle has already been successfully applied to polyaryletherketones (PAEKs).

[0008] Aliphatic polyketones differ from polyaryletherketones (PAEKs), such as polyetheretherketones (PEEKs), in that they do not contain aromatic rings and ether groups. Polyaryletherketones (PAEKs), such as polyetheretherketones (PEEKs), are semicrystalline, high-performance polymers with high heat and medium resistance. They consist of alternating keto, ether, and aryl groups. One advantage of PAEKs is their thermoplastic processability. However, thermoplastics have inherent limitations in terms of heat resistance. To increase the heat resistance and mechanical stability of PAEKs, it has been proposed to crosslink the polymer chains. In the prior art, a method is used for crosslinking PAEKs with diamines. In the process, imine bonds (Schiff bases) are formed, which can impart higher stability to the crosslinked polymer. The disadvantage here is that such crosslinked polymers are not flowable. They cannot therefore be easily thermoplastically processed from the polymer melt.

[0009] Methods for chemical crosslinking of polyetheretherketone (PEEK) with diamines have been known since the 1980s. Here, polyetheretherketone is first modified in diphenylsulfone as solvent by binding paraphenylenediamine. The solvent must subsequently be separated by drying and further washing. The problem is that in the described methods, and here even in the case of covalent bonds, crosslinking bonds are already formed. Here, on the one hand, the heat resistance increases, but on the other hand, the glass transition temperature also increases and thermoplastic processability is lost. The resulting polymer mass is therefore not crosslinked thermoplastically from the melt, but by hot pressing.

[0010] Furthermore, it is known to first modify PAEK by a similar reaction of PEEK and phenylenediamine in diphenylsulfone as solvent, which is then crosslinked by hot pressing after solvent separation and washing. Thermoplastic processability is also not described. Investigations have shown that these products have more stability than non-crosslinked PEEK, but they still need improvement.

[0011] WO 2010 / 011725 describes various amine crosslinkers for crosslinking PAEK, however, this document contains only a single synthesis example illustrating the crosslinking of PAEK with diphenylamine according to the previously cited publication, where the reaction first takes place in diphenylsulfone as solvent.

[0012] A method for crosslinking PAEK with non-amine crosslinkers is proposed in US Pat. No. 6,887,408.

[0013] In order to crosslink PAEK, the prior art also proposed functionalizing the polymer itself with crosslinkable amino groups. Such a method is described, for example, in US Patent Application Publication No. 2017 / 0107323. The drawback here is that the functionalization of PAEK with amino groups is relatively cumbersome. Moreover, the crosslinking of functionalized PAEK cannot be controlled as simply and variably as with low molecular weight crosslinkers.

[0014] WO 2020 / 056052 describes a crosslinkable polymer composition comprising at least one aromatic polymer and at least one crosslinking compound capable of crosslinking the at least one aromatic polymer. Derivatives of fluorene, diphenylmethane, and dihydroanthracene are used as the crosslinking compound.

[0015] The methods described in the prior art for crosslinking of PAEK with diamines as low molecular weight crosslinkers are carried out in the presence of a high proportion of solvent, where the production of shaped bodies is carried out by hot pressing (compression molding). These products are more temperature stable than comparable non-crosslinked PAEKs. However, PAEKs crosslinked in this way have the disadvantage that they have a relatively low rigidity, since the crystallinity of the PAEK is lost when the polymer is dissolved in the solvent. In further processing, the crystallinity can only be restored to a low extent, if at all, due to the inherent steric hindrance of the chains by the crosslinking sites. Furthermore, these methods have the disadvantage that they are overall very complicated, since they require a large number of work steps due to the removal of the solvent. A further disadvantage is that the shaped bodies are produced by hot pressing, which limits their applicability compared to thermoplastic processing. Hot pressing and comparable methods are carried out with non-flowable materials that cannot be converted into a thermoplastic melt. Thereby, the deformability is limited and thin-walled or complex-shaped shaped bodies cannot be produced. For these reasons, such methods can only be automated to a very limited extent. Therefore, efficient and cheap industrial production cannot be achieved based on known solvent-based methods.

[0016] WO 2010 / 011725 describes in a very general way the production of shaped bodies by extrusion from crosslinked PAEK. However, this is only a theoretical approach, since the production of the product is only carried out on a laboratory scale and in a hot press. There is no evidence that PAEK crosslinked with low molecular weight crosslinkers can be extruded, let alone that products with advantageous properties can be obtained. The skilled person also has low expectations of success that PAEK and crosslinkers containing amino groups can be plasticized in an extruder and subsequently subjected to a molding step. On the one hand, there is the problem that crosslinking already starts at the high melt temperature at which the components have to be mixed and processed. On the other hand, it was not expected that PAEK would be mixable and processable with such amine crosslinkers in the absence of solvents. In practice, in the incorporation of low molecular weight components into polymers, separation processes are often observed. However, in order to obtain a stable product, a homogeneous distribution of the crosslinker in the polymer is essential.

[0017] WO 2020 / 030599 describes a method for producing crosslinked molded bodies containing PAEK, in which the crosslinker is a di(aminophenyl) compound in which two aminophenyl rings are linked to each other via an aliphatic group having a carbocyclic group. Specifically, as the crosslinker component, 1-(4-aminophenyl)-1,3,3-trimethylindan-5-amine DAPI (CAS number 54628-89-6), an isomer mixture having 1-(4-aminophenyl)-1,3,3-trimethylindan-6-amine, or an isomer mixture having CAS number 68170-20-7 is used. On the one hand, the high cost of producing the crosslinker is a disadvantage. On the other hand, the physicochemical properties of PAEK crosslinked by DAPI need to be improved.

[0018] Similar to polyaryletherketones, aliphatic polyketones contain keto groups that can react with amines to form Schiff bases. However, since aliphatic polyketones tend to tautomerize their keto groups to their corresponding enol forms at high temperatures, which then lead to uncontrolled further reactions of these enol groups, these reactions are usually the main competitors for crosslinking, making the above mentioned methods less transferable to aliphatic polyketones.

[0019] However, it would be highly desirable to obtain crosslinked aliphatic polyketones, as these can be superior in terms of improved mechanical properties, as well as improved heat distortion resistance, reduced creep behavior, and increased chemical resistance, among others.

[0020] Furthermore, since volatile diamines are associated with significant hazards to users and high environmental burdens at high temperatures, it would be further desirable to design the above-described methods and the reagents used therein such that they do not pose any hazards to users or the environment.

[0021] The problem underlying the present invention is to provide a method and a shaped body which overcomes the above-mentioned drawbacks.

[0022] Therefore, materials based on aliphatic polyketones (PK) should be provided that have improved heat resistance, lower flammability, and higher stiffness (elastic modulus) at high temperatures. Furthermore, they should have good chemical resistance and low creep tendency.

[0023] In particular, the object of the present invention is to provide moldings that have materials with improved stability, but are still easily processable.These materials should be able to be produced in a simple manner, efficiently and inexpensively, and in particular should be able to be thermoplastically processed.It is desirable to be able to avoid inefficient methods, such as hot pressing.

[0024] These methods should also be as environmentally friendly as possible and be possible to carry out without exposing the users to danger.

[0025] Surprisingly, the problem underlying the present invention is solved by a method, a molding, and a sealing article, in which polyketones are crosslinked by a special diamine source while forming imine groups. Here, to produce a molding, a plasticized mixture of polyketones and a diamine source can first be subjected to a molding process. Subsequently, the molding can be subjected to crosslinking.

[0026] Summary of the Invention The first subject of the present invention is a shaped body comprising a matrix in which an aliphatic polyketone is crosslinked with the formation of imine groups by means of at least one diamine source as a crosslinking agent, said diamine source being - di(aminophenyl) compounds in which two aminophenyl rings are linked to each other via an aliphatic group having a carbocyclic group; Formulae (I), (II) and (III) [ka]

[0027] [In the formula, R 1 , R 2 , R 3 , and R 4 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 11 , and R12 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by R 13 , R 14 , R 15 , R 16 , R 17 , and R 18 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by X is selected from a bond, oxygen, sulfur, carbonyl, sulfonyl, sulfoxide, C1-C6 alkylene, C2-C6 alkenylene, and phenylene; R a is halogen, nitro, cyano, hydroxyl, carboxyl, amino, C6-C 12 aryl, where the aryl group is unsubstituted or selected from R c is replaced by R b is selected from halogen, nitro, cyano, amino, C1-C4 alkyl, and C1-C4 haloalkyl; R c is selected from halogen, nitro, cyano, C1-C4 alkyl, and C1-C4 haloalkyl. A diamine compound selected from the compounds - an oligomer / polymer having at least two amide groups; - saturated alicyclic compounds having at least two primary amino groups, oligomers / polymers incorporating these, - A mixture of them The molded body is selected from the group consisting of:

[0028] A further subject of the invention is a method for producing a shaped body, comprising the steps of: i) providing a mixture containing at least one aliphatic polyketone and at least one crosslinker; ii) producing a shaped body from the mixture obtained in step i); and iii) heat treating the molded body at a temperature at which the aliphatic polyketone is crosslinked; Including, wherein the crosslinking agent is - di(aminophenyl) compounds in which two aminophenyl rings are linked to each other via an aliphatic group having a carbocyclic group; Formulae (I), (II) and (III) [ka]

[0029] [In the formula, R 1 , R 2 , R 3 , and R 4 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 11 , and R 12are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by R 13 , R 14 , R 15 , R 16 , R 17 , and R 18 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by X is selected from a bond, oxygen, sulfur, carbonyl, sulfonyl, sulfoxide, C1-C6 alkylene, C2-C6 alkenylene, and phenylene; R a is halogen, nitro, cyano, hydroxyl, carboxyl, amino, C6-C 12 aryl, where the aryl group is unsubstituted or selected from R c is replaced by R b is selected from halogen, nitro, cyano, amino, C1-C4 alkyl, and C1-C4 haloalkyl; R c is selected from halogen, nitro, cyano, C1-C4 alkyl, and C1-C4 haloalkyl. A diamine compound selected from the compounds - an oligomer / polymer having at least two amide groups; - saturated alicyclic compounds having at least two primary amino groups, oligomers / polymers incorporating these, - A mixture of them A method is selected from the following:

[0030] The subject of the invention is also the shaped bodies obtainable by this process.

[0031] Further subject matter is a composition comprising at least one polyketone (PK) and - di(aminophenyl) compounds in which two aminophenyl rings are linked to each other via an aliphatic group having a carbocyclic group; Formulae (I), (II) and (III) [ka]

[0032] [In the formula, R 1 , R 2 , R 3 , and R 4 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 11 , and R 12 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from Ra and the aryl group is unsubstituted or substituted by R b is replaced by R 13 , R 14 , R 15 , R 16 , R 17 , and R 18 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by X is selected from a bond, oxygen, sulfur, carbonyl, sulfonyl, sulfoxide, C1-C6 alkylene, C2-C6 alkenylene, and phenylene; R a is halogen, nitro, cyano, hydroxyl, carboxyl, amino, C6-C 12 aryl, where the aryl group is unsubstituted or selected from R c is replaced by R b is selected from halogen, nitro, cyano, amino, C1-C4 alkyl, and C1-C4 haloalkyl; R c is selected from halogen, nitro, cyano, C1-C4 alkyl, and C1-C4 haloalkyl. A diamine compound selected from the compounds - an oligomer / polymer having at least two amide groups; - saturated alicyclic compounds having at least two primary amino groups, as well as oligomers / polymers incorporating these, - A mixture of them and at least one crosslinking agent selected from A polymer mixture comprising:

[0033] A further subject of the invention is the use of the mouldings as defined above and below or obtained by the process defined above and below in the fields of automotive, maritime, aviation and spaceflight, rail vehicles, oil and gas industry, food and packaging industry and medical technology, in particular as sealing articles, thrust washers, backup rings, valves, connectors, insulators, snap hooks, bearings, bushings, films, powders, coatings, fibres, sealing and O-rings, pipes and conduits, cables, jackets and sheaths and housings for electrical or chemical applications, which consist of the mouldings according to the invention or which are obtained by the process according to the invention or contain such mouldings.

[0034] Summary of the Invention Hereinafter, the terms "crosslinker" and "diamine source" are used synonymously.

[0035] The shaped body according to the invention and the method according to the invention have the following advantages: Potentially harmful substances for the environment and for health, such as volatile aromatic amines, are avoided in the process according to the invention.

[0036] The crosslinked polyketones used according to the invention and the moulded bodies according to the invention are distinguished by improved heat resistance and higher maximum use temperatures than non-crosslinked PK.

[0037] The process according to the invention is distinguished by its low costs: the diamine sources used according to the invention are generally commercially available raw materials which have low production costs.

[0038] - Polyamides can serve as a source of low molecular weight polyamides and diamines. Depending on the reaction conditions, it is possible to adjust which crosslinking components are formed from the polyamide. Thus, by using polyamides as diamine sources, it is also possible to crosslink PK with low boiling aliphatic diamines, which would not normally be possible for process / safety / environmental reasons.

[0039] The process according to the invention is technically simple to carry out, since only two components (preferably two granules) have to be brought and mixed.

[0040] The moldings according to the invention have good tribological properties, in particular very good wear behavior, which makes them suitable materials for use under abrasive wear conditions, for example as sealing and sliding bearing materials in conveyor systems for aggressive and abrasive media.

[0041] The shaped bodies according to the invention exhibit less swelling.

[0042] - REACH registration of these polymers is not required as long-established components are used.

[0043] The process according to the invention is sustainable: the non-crosslinked residues can be easily and simply recycled and do not have to be sent to waste.

[0044] Polyketone Basically, any aliphatic polyketone can be used as the polymer component. According to the invention, aliphatic polyketones (PK) are linearly constructed polymers produced from carbon monoxide and α-olefins, where the monomer units in the polymer chain are preferably strictly alternating. Aliphatic polyketones differ from polyaryletherketones (PAEK), such as polyetheretherketones (PEEK), in that they do not contain aromatic rings and ether groups. According to the invention, preferred PKs are polyketone terpolymers. These polyketone terpolymers consist of carbon monoxide, ethylene and preferably small amounts of propylene.

[0045] [ka]

[0046] According to the invention, the aliphatic polyketones have a linear polymer chain consisting of alternating alkylene units and keto groups. The alkylene units preferably comprise ethylene units as the main component, particularly preferably ethylene units as the main component combined with 1-methylethylene units. The aliphatic polyketones can differ in their average molecular weight and in the ratio of the starting materials carbon monoxide, ethylene and further alkenes, such as propylene or 1- or 2-butylene, used in the preparation. The aliphatic polyketones have keto groups that can be linked forming imine bonds. According to the invention, mixtures of various aliphatic polyketones, differing for example in their molecular weight or their composition, can also be used. However, it is preferred to use a single PK, since this allows a higher crystallinity and associated temperature stability to be achieved.

[0047] In a preferred embodiment, the aliphatic polyketone has an average molecular weight M in the range of 60000 g / mol to 100000 g / mol. n (number average) or average molecular weight M in the range of 132000g / mol to 320000g / mol w(weight average) (determined by GPC measurements). The polydispersity of the aliphatic polyketone is preferably 2.2 to 3.2. The aliphatic polyketone preferably further has a glass transition temperature of 10 to 14° C., a melting point of 218 to 226° C. and / or a recrystallization temperature of 170 to 182° C. (determined by DSC, DIN EN ISO 11357-1 to 3, heating rate of 20° C. / min). It has been found that the PK crosslinked according to the invention has particularly advantageous properties, in particular improved mechanical and chemical properties.

[0048] Preferably, the aliphatic polyketone (PK) has a melting point of 2 cm at 240° C. 3 / 10 minutes~200cm 3 / 10 min range, especially 6 cm 3 / 10 minutes~60cm 3 The polyketones have a melt flow index (MFR) in the range of 1 / 10 min. The measurement is carried out according to DIN ISO 1133, where the material is melted at 240 ° C, a stamp load of 2.16 kg is applied, and then the flowability is determined. An example of a particularly suitable aliphatic polyketone is, for example, M330A from Hyosung. The melt flow index is generally correlated with the molecular weight of the polymer chain. According to the present invention, such a melt flow index has been found to be advantageous, since good thermoplastic processability and miscibility are achieved, and a homogeneous product having high stability and, here, in particular, high rigidity can also be obtained.

[0049] Suitable PKs are commercially available, for example M230A (MFR=150g / 10min at 240°C and 2.16kg), M330A (MFR=60g / 10min at 240°C and 2.16kg), M340A (MFR=60g / 10min at 240°C and 2.16kg), M630A (MFR=6g / 10min at 240°C and 2.16kg) and M640A (MFR=6g / 10min at 240°C and 2.16kg) from Hyosung Corporation Co., Ltd, and AKRO-PLASTIC GmbH's AKROTEK® PK-VM (MFR=60 g / 10 min at 240° C. and 2.16 kg), AKROTEK® PK-HM (MFR=6 g / 10 min at 240° C. and 2.16 kg) and AKROTEK® PK-XM (MFR=2 g / 10 min at 240° C. and 2.16 kg).

[0050] In particular, it is preferred here to use PKs having a melt flow index as mentioned above and a crosslinker in an amount of 0.05% to 15% by weight, in particular 0.1% to 5% by weight, based on the total amount of PK and crosslinker. In a preferred embodiment, the proportion of the crosslinker is 0.1 to 1.5% by weight, in particular 0.4 to 1.0% by weight, based on the total amount of PK and crosslinker. If the proportions and properties of the starting materials are as described above, a particularly good processability of the product can be achieved. In particular, a particularly high stiffness, characterized by a high tensile modulus. Furthermore, such PKs can be processed at temperatures that still allow thermoplastic mixing with the crosslinker, without the crosslinking reaction proceeding too quickly during the provision of the mix (=step i)). Thereby, a plasticized mass is obtained that can be very well used in the molding process (=step ii)) for producing shaped bodies. The shaped bodies thus obtained can subsequently be subjected to a thermoplastic treatment (=step iii), in which the final material properties are achieved by crosslinking of the PK.

[0051] According to the invention, the moldings are preferably based on PK. Here, "based on PK" means that PK is the substantial structured polymer component of the molding. In one embodiment, it is preferred that PK is the only polymer component of the molding. In a further embodiment, PK is present in a mixture with further polymers, in particular thermoplastic polymers. Preferred further polymers are, inter alia, thermoplastic polyurethanes (TPUs), as well as other thermoplastic elastomers, polyesters, liquid crystal polyesters (LCPs), polybutylene terephthalates (PBTs), polyethylene terephthalates (PETs) and polycarbonates (PCs). Here, the preferred weight ratio of PK to further polymers, in particular thermoplastic further polymers, is 1:1 to 100:1, preferably 5:1 to 100:1, particularly preferably 10:1 to 100:1. Furthermore, the moldings may contain fillers, for example fibers, and / or conventional additives, such as processing aids, and / or functional components. Here, the crosslinked PK forms a matrix in which the additives, if any, present, are homogeneously distributed.

[0052] Crosslinking Agent Preferably, the at least one crosslinker is at least 80% by weight, in particular at least 90% by weight, in particular at least 99% by weight, based on the total weight of the crosslinker. - di(aminophenyl) compounds in which two aminophenyl rings are linked to each other via an aliphatic group having a carbocyclic group; a diamine compound selected from compounds of formulae (I), (II) and (III), - an oligomer / polymer having at least two amide groups; - saturated alicyclic compounds having at least two primary amino groups, oligomers / polymers incorporating these, - A mixture of them The diamine source is selected from:

[0053] In a preferred embodiment, the at least one crosslinker contains at least 80% by weight, in particular at least 90% by weight, and in particular at least 99% by weight, based on the total weight of the crosslinker, of a diamine source selected from oligomers / polymers having at least two amide groups, saturated alicyclic compounds having at least two primary amino groups, oligomers / polymers incorporating these, and mixtures thereof.

[0054] The amount of crosslinker is adjusted in view of the desired degree of crosslinking. Preferably, the proportion of crosslinker is 0.05% to 15% by weight, in particular 0.1% to 5% by weight, based on the total amount of aliphatic polyketone and crosslinker. In a preferred embodiment, the proportion of crosslinker is 0.1 to 1.5% by weight, in particular 0.4 to 1.0% by weight. It has been found that the stability of products with such a crosslinker proportion can be particularly advantageous.

[0055] In a preferred embodiment, the crosslinking agent has a boiling point of at least 300°C, in particular at least 350°C, in certain implementations at least 400°C, at 1013 mbar. This is advantageous because such crosslinking agents have a relatively low vapor pressure at the required high processing temperatures. Preferably, the boiling point of the crosslinking agent is in the range of 300°C to 500°C, in particular in the range of 350°C to 500°C, at 1013 mbar. The melting point of the crosslinking agent is advantageously lower than the melting point of the aliphatic polyketone (PK). Thereby, good processability and low risk to the user are achieved.

[0056] In a preferred embodiment, the diamine source used as a crosslinker is an oligomer / polymer having at least two amide groups.

[0057] In the following, the term polyamide is used synonymously with an oligomer / polymer having at least two amide groups.

[0058] If polyamides are referred to below as crosslinkers, this term also includes products formed during the reaction in the process according to the invention having lower molecular weights (e.g. from hydrolytic cleavage of amide groups forming amino groups capable of reacting with keto groups of PK), insofar as they are capable of crosslinking PK. In this respect, both the polyamides used to provide the mixture of PK and crosslinker, and any amino-group-containing oligomers and diamine monomers consisting of them, can function as crosslinkers.

[0059] In the following, homopolyamides and copolyamides are summarized under the notation polyamide. In the context of the present invention, to denote polyamides, abbreviations somewhat common in the art are used, which consist of the letters PA followed by numbers and letters. Some of these abbreviations are defined in DIN EN ISO 1043-1. H2N-(CH2) z Polyamides derivable from aminocarboxylic acids of the type -COOH or the corresponding lactams are identified as PA Z, where Z represents the number of carbon atoms in the monomer. Thus, for example, PA6 represents a polymer from ε-caprolactam or ε-aminocaproic acid. H2N-(CH2) x -NH2 and HOOC-(CH2) y Polyamides derivable from diamines and dicarboxylic acids of the -COOH type are identified as PA xy, where x represents the number of carbon atoms in the diamine and y represents the number of carbon atoms in the dicarboxylic acid. To represent copolyamides, these components are listed in the order of their quantity percentages, separated by slashes. Thus, for example, PA66 / 610 is a copolyamide from hexamethylenediamine, adipic acid and sebacic acid. For the monomers used according to the invention with aromatic or cycloaliphatic groups, the following letter abbreviations are used: T = terephthalic acid, I = isophthalic acid, MXDA = m-xylylenediamine, IPDA = isophoronediamine, PACM = 4,4'-methylenebis(cyclohexylamine), MACM = 2,2'-dimethyl-4,4'-methylenebis(cyclohexylamine).

[0060] Polyamides can be described by the monomers used to make them. Polyamide-forming polymers are monomers suitable for forming polyamides.

[0061] In a preferred embodiment, the crosslinking agent comprises a polymer having at least two amide groups, wherein the polymer comprises in polymerized form polyamide-forming monomers, the monomers being A) unsubstituted or substituted aromatic dicarboxylic acids and derivatives of unsubstituted or substituted aromatic dicarboxylic acids; B) unsubstituted or substituted aromatic diamines; C) aliphatic or cycloaliphatic dicarboxylic acids; D) aliphatic or cycloaliphatic diamines; E) monocarboxylic acids, F) monoamines, G) at least trivalent amines; H) lactams, I) w-amino acids, and K) Compounds other than A) to I) which are capable of co-condensing with them, as well as mixtures thereof. is selected from.

[0062] In a preferred embodiment of the present invention, a polyamide is used as a crosslinking agent, preferably having a melting point of up to 260° C. In particular, an aliphatic polyamide is used, provided that at least one of components A) or B) and at least one of components C) or D) are present here, provided that in a particular embodiment, at least one component A) and at least one component D) are present.

[0063] The aromatic dicarboxylic acids A) are preferably selected from unsubstituted or substituted phthalic acid, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid or diphenyldicarboxylic acid, respectively, and also derivatives and mixtures of the aromatic dicarboxylic acids mentioned above. The substituted aromatic dicarboxylic acids A) preferably have at least one C1-C4 alkyl group. Particularly preferably, the substituted aromatic dicarboxylic acids A) have one or two C1-C4 alkyl groups. These are preferably selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl, particularly preferably methyl, ethyl and n-butyl, very particularly preferably methyl and ethyl, in particular methyl. The substituted aromatic dicarboxylic acids A) may also have further functional groups that do not interfere with the amidation, such as, for example, 5-sulfoisophthalic acid, its salts and derivatives. Among these, the sodium salt of 5-sulfoisophthalic acid dimethyl ester is preferred. Preferably, the aromatic dicarboxylic acid A) is selected from unsubstituted terephthalic acid, unsubstituted isophthalic acid, unsubstituted naphthalenedicarboxylic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid and 5-sulfoisophthalic acid. Particularly preferably, terephthalic acid, isophthalic acid or a mixture of terephthalic acid and isophthalic acid is used as aromatic dicarboxylic acid A).

[0064] The aromatic diamine B) is preferably selected from bis(4-aminophenyl)methane, 3-methylbenzidine, 2,2-bis(4-aminophenyl)propane, 1,1-bis(4-aminophenyl)cyclohexane, 1,2-diaminobenzene, 1,4-diaminobenzene, 1,4-diaminonaphthalene, 1,5-diaminonaphthalene, 1,3-diaminotoluene, m-xylylenediamine, N,N'-dimethyl-4,4'-biphenyldiamine, bis(4-methylaminophenyl)methane, 2,2-bis(4-methylaminophenyl)propane, or mixtures thereof. Particularly preferably, m-xylylenediamine is used as aromatic diamine.

[0065] The aliphatic or cycloaliphatic dicarboxylic acids C) are preferably selected from oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecane-1,11-dicarboxylic acid, dodecane-1,12-dicarboxylic acid, maleic acid, fumaric acid or itaconic acid, cis- and trans-cyclohexane-1,2-dicarboxylic acid, cis- and trans-cyclohexane-1,3-dicarboxylic acid, cis- and trans-cyclohexane-1,4-dicarboxylic acid, cis- and trans-cyclopentane-1,2-dicarboxylic acid, cis- and trans-cyclopentane-1,3-dicarboxylic acid, and mixtures thereof.

[0066] The aliphatic or cycloaliphatic diamine D) is preferably selected from ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, 2-methyl-1,8-octamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 2-methylpentamethylenediamine, 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 5-methylnonamethylenediamine, 2,4-dimethyloctamethylenediamine, 5-methylnonanediamine, bis(4-aminocyclohexyl)methane, 3,3'-dimethyl-4,4'diaminodicyclohexylmethane, and mixtures thereof.

[0067] Particularly preferably, the diamine D) is selected from hexamethylenediamine, 2-methylpentamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, 1,3-bis(aminomethyl)cyclohexane and 1,4-bisaminomethylcyclohexane, 5-amino-2,2,4-trimethyl-1-cyclopentanemethylamine, 5-amino-1,3,3-trimethylcyclohexanemethylamine (isophoronediamine), 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, [3-(aminomethyl)-2-bicyclo[2.2.1]heptanyl]methanamine, aminated dimeric fatty acids, and mixtures thereof. In a preferred embodiment of the invention, the aqueous solution contains at least one diamine D) selected from hexamethylenediamine, bis(4-aminocyclohexyl)methane (PACM), 3,3'-dimethyl-4,4'diaminodicyclohexylmethane (MACM), isophoronediamine (IPDA), and mixtures thereof.

[0068] The monocarboxylic acid E) functions as an end-capping for the polyamide oligomer used according to the invention. Essentially, all monocarboxylic acids are suitable that can react with at least a portion of the available amino groups under the reaction conditions of the polyamide condensation. Suitable monocarboxylic acids E) are aliphatic monocarboxylic acids, cycloaliphatic monocarboxylic acids and aromatic monocarboxylic acids. These include acetic acid, propionic acid, n-, iso- or tert-butyric acid, valeric acid, trimethylacetic acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, cyclohexanecarboxylic acid, benzoic acid, methylbenzoic acid, 1-naphthalenecarboxylic acid, 2-naphthalenecarboxylic acid, phenylacetic acid, oleic acid, ricinoleic acid, linoleic acid, linolenic acid, erucic acid, fatty acids from soybean, linseed, castor bean and sunflower, acrylic acid, methacrylic acid, tertiary saturated monocarboxylic acids (for example Versatic® acid from Royal Dutch Shell plc), and mixtures thereof.

[0069] When using unsaturated carboxylic acids or their derivatives as monocarboxylic acid E), it may be useful to add commercially available polymerization inhibitors to the aqueous solution. Particularly preferably, the monocarboxylic acid E) is selected from acetic acid, propionic acid, benzoic acid, and mixtures thereof. In a very particularly preferred embodiment, the aqueous solution contains only acetic acid as monocarboxylic acid E). In a further very particularly preferred embodiment, the aqueous solution contains only propionic acid as monocarboxylic acid E). In a further very particularly preferred embodiment, the aqueous solution contains only benzoic acid as monocarboxylic acid E).

[0070] The monoamines F) here function as end-capping of the polyamide oligomers used according to the invention. Essentially all monoamines capable of reacting with at least a portion of the available carboxylic acid groups under the reaction conditions of the polyamide condensation are suitable. Suitable monoamines F) are aliphatic, cycloaliphatic and aromatic monoamines. These include methylamine, ethylamine, propylamine, butylamine, hexylamine, heptylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, cyclohexylamine, dicyclohexylamine, aniline, toluidine, diphenylamine, naphthylamine and mixtures thereof.

[0071] Suitable at least trivalent amines G) are N'-(6-aminohexyl)hexane-1,6-diamine, N'-(12-aminododecyl)-dodecane-1,12-diamine, N'-(6-aminohexyl)dodecane-1,12-diamine, N'-[3-(aminomethyl)-3,5,5-trimethylcyclohexyl]hexane-1,6-diamine, N'-[3-(aminomethyl)-3,5,5-trimethylcyclohexyl]dodecane-1,12-diamine, N'-[(5-amino-1,3,3-trimethylcyclohexyl)methyl]hexane-1,6-diamine, N '-[(5-amino-1,3,3-trimethylcyclohexyl)methyl]dodecane-1,12-diamine, 3-[[[3-(aminomethyl)-3,5,5-trimethylcyclohexyl]amino]methyl]-3,5,5-trimethylcyclohexanamine, 3-[[(5-amino-1,3,3-trimethylcyclohexyl)methylamino]methyl]-3,5,5-trimethylcyclohexanamine, 3-(aminomethyl)-N-[3-(aminomethyl)-3,5,5-trimethylcyclohexyl]-3,5,5-trimethylcyclohexanamine. Preferably, at least trivalent amines G) are not used.

[0072] Suitable lactams H) are ε-caprolactam, 2-piperidone (δ-valerolactam), 2-pyrrolidone (γ-butyrolactam), capryllactam, enantholactam, lauryllactam, and mixtures thereof.

[0073] Suitable ω-amino acids I) are 6-aminocaproic acid, 7-aminoheptanoic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and mixtures thereof.

[0074] Suitable compounds K) which are different from A) to I) and which can be co-condensed with them are at least trivalent carboxylic acids, diaminocarboxylic acids, etc. Suitable compounds K) are furthermore 4-[(Z)-N-(6-aminohexyl)-C-hydroxycarbonimidoyl]benzoic acid, 3-[(Z)-N-(6-aminohexyl)-C-hydroxycarbonimidoyl]benzoic acid, (6Z)-6-(6-aminohexylimino)-6-hydroxyhexanecarboxylic acid, 4-[(Z)-N-[(5-amino-1,3,3-trimethylcyclohexyl)methyl]-C-hydroxycarbonimidoyl]benzoic acid, 3-[(Z)-N-[(5-amino-1,3,3-trimethylcyclohexyl)methyl]-C-hydroxycarbonimidoyl]benzoic acid, 4-[(Z)-N-[3-(aminomethyl)-3,5,5-trimethylcyclohexyl]-C-hydroxycarbonimidoyl]benzoic acid, 3-[(Z)-N-[3-(aminomethyl)-3,5,5-trimethylcyclohexyl]-C-hydroxycarbonimidoyl]benzoic acid, and mixtures thereof.

[0075] In a further preferred embodiment of the present invention, a crosslinker selected from polyamides, their copolymers and mixtures thereof is used, where the crosslinker has a melting range of 200°C to 250°C, preferably a melting range of 220°C to 240°C, in particular a melting range of 220°C to 230°C.

[0076] In a further preferred embodiment, the at least one crosslinking agent is selected from saturated alicyclic compounds having at least two primary amino groups and oligomers / polymers incorporating them. Suitable compounds are those whose boiling point is above 300°C. In a preferred embodiment, these compounds are present as liquids in step i). Thus, they can function as an internal solvent in melt mixing. Preferably, the saturated alicyclic compounds are aminated fatty acid dimers (dimer fatty acids).

[0077] As used herein, the term "fatty acid dimer" refers to the dimerized product of the reaction of two or more mono- or polyunsaturated fatty acids. Such fatty acid dimers are well known in the art and typically exist as mixtures.

[0078] Aminated dimer fatty acids (also known as aminated dimerized fatty acids or dimer acids) refer to mixtures produced by the oligomerization of unsaturated fatty acids. The starting materials include unsaturated C 12 ~C 22 The fatty acids can be used to produce dimeric fatty acids. 12 ~C 22 Depending on the number and position of the double bonds of the fatty acids, the amino groups of the dimeric fatty acids are linked to each other by hydrocarbon groups having mainly 24 to 44 carbon atoms. These hydrocarbon groups can be unbranched or branched and can have double bonds, C6 alicyclic hydrocarbon groups or C6 aromatic hydrocarbon groups, where alicyclic and / or aromatic groups can also be present in condensation. Preferably, the groups linking the amino groups of the dimeric fatty acids do not have aromatic hydrocarbon groups and very particularly preferably do not have unsaturated bonds. C 18 Particularly preferred are fatty acid dimers, i.e. fatty acid dimers having 36 carbon atoms.They can be obtained, for example, by dimerizing oleic acid, linoleic acid and linolenic acid and mixtures thereof.Dimerization is optionally followed by hydrogenation and then amination.

[0079] In certain embodiments, the saturated alicyclic compound is [ka] It is.

[0080] In certain embodiments, the saturated alicyclic compound is [ka] It is.

[0081] A particular embodiment is a polymer that incorporates at least one aminated dimeric fatty acid. A further more particular embodiment is a polymer that incorporates at least one aminated dimeric fatty acid. [ka] or [ka] is a polymer that incorporates

[0082] In a further preferred embodiment, the at least one crosslinker is a mixture containing an oligomer / polymer having at least one amide group and a saturated alicyclic compound having at least two primary amino groups.

[0083] In a further preferred embodiment, the at least one crosslinker is a mixture containing an oligomer / polymer having at least one amide group and an oligomer / polymer containing, as polymerized incorporation, at least one saturated alicyclic compound having at least two primary amino groups.

[0084] In a further preferred embodiment, at least one crosslinker is represented by formula (I), (II), and (III): [ka]

[0085] [In the formula, R 1 , R 2 , R 3 , and R 4 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 11 , and R 12 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by R 13 , R 14 , R 15 , R 16 , R 17 , and R 18 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by X is selected from a bond, oxygen, sulfur, carbonyl, sulfonyl, sulfoxide, C1-C6 alkylene, C2-C6 alkenylene, and phenylene; Ra is halogen, nitro, cyano, hydroxyl, carboxyl, amino, C6-C 12 aryl, where the aryl group is unsubstituted or selected from R c is replaced by R b is selected from halogen, nitro, cyano, amino, C1-C4 alkyl, and C1-C4 haloalkyl; R c is selected from halogen, nitro, cyano, C1-C4 alkyl, and C1-C4 haloalkyl. The diamine compound is selected from the following compounds:

[0086] Examples of C1-C4 alkyl groups are especially methyl, ethyl, propyl, isopropyl, n-butyl, 2-butyl, sec-butyl and tert-butyl.

[0087] Examples of C1-C6 alkyl groups are in particular the abovementioned C1-C4 alkyl groups, as well as n-pentyl and n-hexyl.

[0088] Preferably, C1-C4 haloalkyl represents one of the above-listed C1-C4 alkyl groups, preferably having 1, 2, 3, 4 or 5, preferably 1, 2 or 3 halogen substituents, such as, for example, trifluoromethyl.

[0089] Halogen represents fluorine, chlorine, bromine and iodine, preferably fluorine, chlorine and bromine.

[0090] Unsubstituted C6~C 14 Aryl preferably represents phenyl, naphthyl, anthracenyl, phenanthrenyl, naphthacenyl, in particular phenyl or naphthyl. 14 Aryl has one, two, three, four or more than four groups suitably selected from halogen, nitro, cyano, C1-C4 alkyl, and C1-C4 haloalkyl.14 Examples of aryl are tolyl, xylyl and mesityl.

[0091] Suitably, C1-C6 alkylene represents -CH2-, -CH2-CH2-, -CH2-CH2-CH2-, -CH2-CH2-CH2-CH2-CH2-, or -C(CH3)2-.

[0092] In a preferred embodiment, at least one crosslinker is represented by formula (I) or (II): [In the formula, R 2 , R 3 , R 5 , R 6 , R 7 , R 8 , R 10 , and R 11 represents hydrogen, R 1 and R 4 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by R 9 and R 12 are each independently hydrogen, halogen, nitro, cyano, hydroxy, amino, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C6-C 14 aryl, where the alkyl, alkenyl, and alkynyl groups are unsubstituted or selected from R a and the aryl group is unsubstituted or substituted by R b is replaced by X is selected from a bond, oxygen, sulfur, carbonyl, sulfonyl, sulfoxide, C1-C6 alkylene, C2-C6 alkenylene, and phenylene; R ais halogen, nitro, cyano, hydroxyl, carboxyl, amino, C6-C 12 aryl, where the aryl group is unsubstituted or selected from R c is replaced by R b is selected from halogen, nitro, cyano, amino, C1-C4 alkyl, and C1-C4 haloalkyl; and R c is selected from halogen, nitro, cyano, C1-C4 alkyl, and C1-C4 haloalkyl. It is a compound of the formula:

[0093] In a particularly preferred embodiment, at least one crosslinker has formula (Ia) or (II.a) [ka] is a compound of During the ceremony, R 1 , R 4 , R 9 and R 12 and X has the following meaning: [Table 1]

[0094] In a further preferred embodiment, the crosslinker has the formula (III.a) and (III.b): [ka] The compound is selected from the group consisting of

[0095] In certain embodiments, the crosslinker is selected from (III.a1) and (III.b1): [ka] The compound is selected from the group consisting of

[0096] In a further preferred embodiment, at least one crosslinker is a di(aminophenyl) compound in which two aminophenyl rings are linked together through an aliphatic group bearing a carbocyclic group.

[0097] The di(aminophenyl) compounds used as crosslinkers (or as diamine sources) have two aminophenyl rings bonded to each other. These compounds are therefore primary diamines. Here, in one embodiment of the present invention, each phenyl ring has only a single amino group. However, it is equally conceivable that the phenyl rings have, independently of each other, two or three amino groups. These compounds are of low molecular weight and are not polymeric. The phenyl rings may have, in addition to the amino groups, further substituents such as alkyl or halogen groups. The two aminophenyl rings are bonded to each other via an aliphatic group. The aliphatic group consists only of carbon and hydrogen and is not aromatic. The di(aminophenyl) compounds used as crosslinkers (or as diamine sources) preferably have no further double or triple bonds, apart from the two phenyl rings. The aliphatic group has a carbocyclic group. The carbocyclic group here is a hydrocarbon ring which may have, for example, 4 to 7 carbon atoms, preferably 5 or 6 carbon atoms. The carbocyclic group here may include a double bond of the phenyl ring. Preferably, the carbocyclic group has only a single aliphatic hydrocarbon ring. Preferably, the aliphatic group has a total of 5 to 15 carbon atoms, especially 6 to 8 carbon atoms. Due to the aliphatic group between the carbocyclic groups, the two phenyl rings are not conjugated.

[0098] According to the present invention, it has surprisingly been found that PK crosslinked with such di(aminophenyl) compounds has particularly advantageous properties: in particular, the crosslinked PK has improved thermal stability and increased mechanical stability.

[0099] In a preferred embodiment, the di(aminophenyl) compound used as a crosslinker (or diamine source) is a cyclized compound in which only one of the two phenyl rings is cyclized with a carbocyclic group. Cyclization (condensation) refers to joining an additional ring to a ring of a cyclic molecule. The two cyclized rings share two carbon atoms and therefore share one CC double bond of the phenyl ring. The use of such a cyclized crosslinker has the advantage that it can form a particularly tight and regular bond between PK chains, thereby achieving a particularly high temperature stability and rigidity of the product.

[0100] The amino groups of the di(aminophenyl) compounds used as crosslinkers (or diamine sources) can be essentially at any position of the phenyl group, i.e., ortho, meta, or para to the aliphatic compounds of the two phenyl rings. In embodiments in which each phenyl group has only a single amino group, it is preferred that the two amino groups are as far apart as possible from each other. This can be achieved when the two amino groups are attached in the para position to the aliphatic compounds and / or at the 4- and 4'-positions of the phenyl rings. Thus, in a preferred embodiment, the diaminodiphenyl compound is a 4,4'-diaminodiphenyl compound. In general, the advantage of the amino groups being as far apart as possible from each other can be that the formation of undesired intramolecular reactions that would result in the crosslinker making two bonds with the same PK polymer chain is reduced. Such intramolecular reactions with the crosslinker can disrupt the crystal structure of the PK without crosslinking, thereby reducing the stability of the product.

[0101] In a preferred embodiment of the invention, the di(aminophenyl) compound used as the crosslinker (or as the diamine source) is an asymmetric compound.

[0102] In a preferred embodiment of the present invention, the di(aminophenyl) compound used as the crosslinker (or as the diamine source) has the general formula (IV): [ka]

[0103] [In the formula, R 19 and R 20 are independently selected from H, substituted or unsubstituted alkyl having 1 to 20 carbon atoms, in particular 1 to 4 carbon atoms, in particular methyl or ethyl, substituted or unsubstituted aryl having 5 to 12 carbon atoms, F, and Cl, where Z is an aliphatic group having a carbocyclic group. wherein each phenyl ring is substituted with one, two or three groups R 19 or R 20 Preferably, the phenyl ring may bear the group R 19 and / or R 20 Particularly preferably, the group R 19 and R 20 are each H. Further groups R 19 and R 20 Crosslinkers without PK are relatively well available and can be processed into more stable crosslinked PKs.

[0104] The group Z may be attached to each phenyl group via two or one bond. Preferably, the group Z is attached to a phenyl group via two bonds and to a second phenyl group via one bond.

[0105] In a further preferred embodiment of the present invention the crosslinker has the general formula (IV.a) [ka]

[0106] [In the formula, x is a group Z to R 19 3 or 4 depending on the number of bonds in the phenyl ring substituted with y is the R to Z group 20 3 or 4 depending on the number of bonds in the phenyl ring substituted with base R 19are selected, independently in each occurrence, from hydrogen, unsubstituted or substituted alkyl having 1 to 20 carbon atoms, unsubstituted or substituted aryl having 5 to 14 carbon atoms, F, and Cl; base R 20 are selected, independently in each occurrence, from hydrogen, unsubstituted or substituted alkyl having 1 to 20 carbon atoms, unsubstituted or substituted aryl having 5 to 14 carbon atoms, F, and Cl; Z is an aliphatic group having a carbocyclic group, where Z is attached to each of the two phenyl rings through one or two bonds. It is a compound of the formula:

[0107] Preferably, Z is connected to R via two bonds. 19 In compound (IV.a), x represents 3. Preferably, Z is linked through one bond to R 20 In compound (IV.a), y is 4. In particular, x is 3 and y is 4. In particular, Z together with the two phenyl rings forms an indane skeleton to which the phenyl rings are attached.

[0108] In the compounds of formulae (IV) and (IV.a), alkyl having 1 to 20 carbon atoms preferably includes C1-C6 alkyl and further n-heptyl, n-octyl, 2-ethylhexyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-pentadecyl, n-hexadecyl, n-heptadecyl, n-octadecyl, n-nonadecyl, arachinyi and their structural isomers as defined above. Alkyl having 1 to 4 carbon atoms, in particular methyl or ethyl, is particularly preferred.

[0109] Substituted alkyl having 1 to 20 carbon atoms has at least one (e.g. 1, 2, 3, 4 or more than 4) substituents preferably selected from halogen, nitro, cyano, and C1 to C4 alkoxy. In particular, substituted alkyl represents C1 to C4 haloalkyl, preferably having 1, 2, 3, 4 or 5, preferably 1, 2 or 3 halogen substituents. This includes, for example, trifluoromethyl.

[0110] In the compounds of formulae (IV) and (IV.a), the unsubstituted aryl having 5 to 14 carbon atoms preferably represents phenyl, naphthyl, anthracenyl and phenanthrenyl, in particular phenyl or naphthyl. The unsubstituted aryl having 5 to 12 carbon atoms is in particular phenyl or naphthyl. Preferably, the substituted aryl having 5 to 14 carbon atoms or the substituted aryl having 5 to 12 carbon atoms has one, two, three, four or more than four groups, preferably selected from halogen, nitro, cyano, C1-C4 alkyl and C1-C4 haloalkyl. Examples of the substituted aryl having 5 to 14 carbon atoms or the substituted aryl having 5 to 12 carbon atoms are tolyl, xylyl, mesityl.

[0111] In the compounds of formula (IV.a), the group R 19 is suitably selected from hydrogen, substituted or unsubstituted alkyl having 1 to 4 carbon atoms, F and Cl. Particularly preferred is the group R 19 is selected from hydrogen and unsubstituted alkyl having 1 to 4 carbon atoms.

[0112] In the compounds of formula (IV.a), the group R 20 is suitably selected from hydrogen, substituted or unsubstituted alkyl having 1 to 4 carbon atoms, F and Cl. Particularly preferred is the group R 20 is selected from hydrogen and unsubstituted alkyl having 1 to 4 carbon atoms.

[0113] Preferably, each phenyl ring is provided with a group R different from hydrogen. 19 or R20 In certain embodiments, the group R 19 and R 20 All of the groups R 19 and R 20 Compounds of formula (IV.a) in which all represent hydrogen are relatively well available and can be processed into more stable crosslinked PKs.

[0114] In a preferred embodiment, the crosslinker has the general formula (V): [ka]

[0115] [In the formula, R 19 and R 20 are independently selected from H, substituted or unsubstituted alkyl having 1 to 20 carbon atoms, in particular having 1 to 4 carbon atoms, in particular methyl or ethyl, substituted or unsubstituted aryl having 5 to 12 carbon atoms, F and Cl, R 21 is a carbocyclic group, which has 2 to 3 carbon ring atoms and which may be substituted with at least one alkyl group having 1 to 4 carbon atoms, in particular methyl or ethyl. Particularly preferred are compounds of the group R 19 and R 20 are each H. Thus, the carbocyclic group R 21 is a pentyl or hexyl group. Such crosslinkers have the advantage that a particularly good combination of temperature stability and mechanical stability of the crosslinked PK can be obtained.

[0116] In a preferred embodiment, the crosslinker has the general formula (Va): [ka]

[0117] [In the formula, R 21 are selected as described above] Such crosslinkers have the advantage that a particularly good combination of temperature and mechanical stability of the crosslinked PK can be obtained.

[0118] In a preferred embodiment, the crosslinker has the formula (V.a1): [ka] has.

[0119] This compound provided a particularly advantageous combination of temperature and mechanical stability to crosslinked PK in the tests carried out. Its chemical name is 1-(4-aminophenyl)-1,3,3-trimethylindan-5-amine (CAS number 54628-89-6).

[0120] In a further preferred embodiment, the crosslinker has the formula (V.b1): [ka] has.

[0121] This compound likewise provides a particularly advantageous combination of temperature and mechanical stability of crosslinked PK in the tests carried out. Its chemical name is 1-(4-aminophenyl)-1,3,3-trimethylindan-6-amine.

[0122] In a further preferred embodiment, the crosslinker contains a mixture of compounds of formula (V.a1) and (V.b1), which likewise results in a particularly advantageous combination of temperature and mechanical stability of the crosslinked PK in the tests carried out.

[0123] In a further preferred embodiment, the crosslinker has formula (VII): [ka] has.

[0124] This crosslinker likewise results in a particularly advantageous combination of temperature and mechanical stability of the crosslinked PK in the tests carried out. The chemical name is 1-(4-aminophenyl)-1,3,3-trimethylindanamine (CAS number 68170-20-7), where the amino group may be present in all positions on the aromatic ring of the indan. Mixtures of 1-(4-aminophenyl)-1,3,3-trimethylindanamine in which the amino group is in different positions on the aromatic ring of the indan are also included.

[0125] According to the invention, it is preferred to use a single specific crosslinking agent in order to obtain material properties that are as uniform as possible, however, it is also possible to use a mixture of two or more crosslinking agents.

[0126] The process according to the invention involves a crosslinking reaction in which the polymer chains of the polyketone are covalently and intramolecularly linked to one another.

[0127] Step i) In step (i), a mixture containing a polyketone and a crosslinking agent is provided. The mixture provided in step (i) can be produced by conventional compounding methods. In step i), preferably, at least one polyketone, at least one crosslinking agent, optionally fillers and reinforcing agents, and optionally further additives different therefrom are melt-mixed or dry-mixed (compounded).

[0128] In mixing in the melt or melt mixing, the polymers are heated above their melting temperature and intensively mixed by rolling, kneading or extrusion. Here, the temperature in step (i) is preferably adjusted so that the mixture is well processable and has a suitable viscosity for compounding. Furthermore, the temperature in step (i) is preferably adjusted so that no substantial reaction occurs between the polyketone and the crosslinker. Furthermore, the residence time at the temperature at which the reaction between the PK and the crosslinker has already taken place should be kept as short as possible. In contrast to PAEK, where the reactivity of the reacting carbonyl groups is reduced by the mesomeric effect of the adjacent phenylene groups, the amine crosslinking of the PK by the crosslinker described according to the invention preferably starts already in the melt. According to the invention, it is not necessary that the crosslinker is already covalently bonded to the PK via an amine bond, as is the case in the methods described in the prior art. This is advantageous, since according to the invention, such a further reaction step can be omitted, which needs to be precisely controlled to prevent undesired further reaction of the intermediate and premature crosslinking resulting therefrom.

[0129] In one embodiment, in step i), at least one polyketone, at least one crosslinking agent, optionally fillers and reinforcing agents, and optionally further additives different therefrom, are fed into an extruder and mixed while plasticizing, and optionally granulated.

[0130] The temperature in the melt mixing step i) is preferably in the range of 220 to 260°C.

[0131] In a further embodiment, in step i), preferably at least one polyketone, at least one crosslinking agent, optionally fillers and reinforcing agents, and optionally further additives different therefrom are dry mixed. The above-listed components can be mixed by any known dry mixing technique. A dry mixture (dry blend) of polyketone, at least one crosslinking agent, optionally fillers and reinforcing agents, and optionally further additives different therefrom is obtained.

[0132] The temperature during dry mixing in step i) is lower than the softening range of PK, and is preferably in the range of 0°C to 100°C.

[0133] During the preparation of the mixture, intensive mixing is carried out by suitable means such as stirring or kneading equipment to achieve uniform distribution of crosslinking agent in the polymer.This is very important to obtain uniform material properties from the viewpoint of stability.Preferably, after preparation, the crosslinkable mixture is further processed in step (ii) without further intermediate steps that change the composition.

[0134] Upon mixing (blending), intermediate products, such as granules, can be obtained, which are stable for long periods at temperatures in the range below 80° C., preferably below 50° C., in particular below ambient temperature, and can, for example, be stored intermediately and / or transported elsewhere for further processing.

[0135] In a particularly preferred embodiment of the present invention, the mixture does not contain a solvent. In particular, no external solvent is added to the mixture. Surprisingly, according to the present invention, it has been found that the mixture of PK and crosslinker can be processed without the use of a solvent, where intimate mixing is performed.

[0136] Preferably, the mixture is heated to a temperature at which it is in liquid or flowable (plasticized) form, whereby, in order to obtain a homogeneous mixture, it is preferable to select a temperature and a residence time such that no significant crosslinking occurs.

[0137] In a preferred embodiment, the crosslinking agent is added continuously to the PK for the preparation of the mixture in step i). Here, these components can be present in liquid or solid form. In this way, a particularly homogeneous mixture can be obtained. Here, the addition of the crosslinking agent is preferably carried out with homogeneous mixing, for example with stirring, kneading, rolling and / or extrusion. In a preferred embodiment, the crosslinking agent is provided in the form of a concentrate. This has the advantage that the crosslinking agent can be better dosed, which can improve the homogeneity of the mixture. Overall, by adding the crosslinking agent continuously, a particularly homogeneous mixture can be obtained, whereby a particularly regular crosslinking is achieved. This makes it possible to avoid the occurrence of areas with different degrees of crosslinking, which can lead to inhomogeneity and possibly damage of the product under thermal or mechanical load. In this way, particularly good properties can be achieved with respect to temperature stability and mechanical stability.

[0138] Step (ii) In step (ii), a molded body is produced from the mixture. Here, step (ii) of producing a molded body includes all measures that bring the mixture into a three-dimensional shape that is retained in the cured crosslinked state. The production of the molded body is preferably carried out by molding methods common to thermoplastics. Here, the production of the molded body is preferably carried out before and / or during crosslinking. Here, it is generally not critical whether the mixture used in step ii) already contains a small proportion of crosslinked products. Particularly preferably, the molding is carried out before step (iii), since the mixture is advantageously thermoplastically processable and moldable before crosslinking, in particular by hot pressing, extrusion, injection molding and / or 3D printing.

[0139] If in step i) the mixing of the components is carried out by dry mixing, in step ii) the dry mixture is melted and subjected to a shaping step, as previously described.

[0140] In one embodiment, steps i) and ii) proceed separately and sequentially.

[0141] In a preferred embodiment, the production of the shaped body is carried out in step (ii) by thermoplastic deformation. This means that the mixture can be formed from the melt in an uncrosslinked and / or at least significantly uncrosslinked state, since otherwise thermoplastic processing would no longer be possible. If too many crosslinking points are present, the PK intermediate is no longer flowable and can no longer be easily thermoplastically formed. The mixture needs to be exposed to high processing temperatures only for a short time before molding. Therefore, the thermoplastic processing is preferably carried out so that the residence time of the mixture in the equipment is as short as possible. Here, the processing is preferably carried out so that a significant part of the crosslinking reaction, here for example more than 80%, more than 90% or more than 95% of the crosslinking, takes place only after molding, i.e. in step (iii).

[0142] In a preferred embodiment, the mixture is processed in step (ii) by extrusion, hot pressing, injection molding, and / or 3D printing, during which it is deformed. These methods are particularly suitable for simple and efficient processing of thermoplastic polymer compositions. "Deformation" refers to changing the shape that was initially given to it again later. Typical deformation methods include bending, embossing, stretching, and deep drawing.

[0143] Here, extrusion can be carried out by known methods. In extrusion, a solid to viscous settable mass is continuously extruded under pressure through a forming orifice (also called a nozzle, die or mouthpiece). Here, a body with the cross section of the orifice, called an extrudate, is produced of any theoretical length. Preferably, extrusion is carried out at a temperature of at least 220°C, preferably between 220°C and 265°C, in particular between 230°C and 250°C.

[0144] Hot pressing is a method in which a molding material is introduced into a preheated cavity. A plunger is then used to close the cavity. The pressure causes the molding material to assume the shape defined by the mold. Preferably, hot pressing is carried out at a temperature of at least 220°C, preferably between 220°C and 265°C, in particular between 230°C and 250°C.

[0145] Injection molding (often also called injection molding or injection molding) is a molding method used in plastics processing. Here, the plastic is plasticized by an injection molding machine and injected under pressure into a mold, an injection mold. In the mold, the material cools down to a solid state again and is removed as a molded body after the mold is opened. The hollow space (cavity) of the mold determines the shape and surface structure of the product.

[0146] In 3D printing, the molding material according to the invention can be molded, for example, by means of a method known as Fused Deposition Modeling (FDM). FDM is essentially based on three elements: a printing bed (on which the desired object is printed), a filament spool (providing the printing material) and a printing head (also called extruder). A filament made of thermoplastic molding material is unrolled during the method and fed into the extruder, where it is melted and deposited layer by layer on the printing plate.

[0147] Particularly preferably, the processing is carried out by extrusion followed by injection moulding. The mixture of PK and crosslinker, if not already present in liquid form, is melted in the process. This mixture is preferably introduced in step (ii) into an extruder, injection moulding machine or hot press, melted at an elevated temperature, for example in the range of 220°C to 250°C, and brought into the desired shape.

[0148] Step (iii) Step (iii) involves obtaining a crosslinked molded body by heat treating the molded body at a temperature at which the PK is crosslinked. This allows the PK to be intermolecularly crosslinked with the crosslinking agent. The polyamide is hydrolyzed and decomposed into diamine components. In the crosslinking, the formation of two imine bonds occurs between the two keto groups of the PK chains and the two amino groups of the free diamines of the crosslinking agent. The crosslinks obtained in the form of imines are also called Schiff bases, since the imine nitrogens are not bound to hydrogen atoms but to organic molecules. Here, the crosslinking is carried out as completely as possible, so that as many amino groups as possible of the crosslinking agent used react with the carbonyl groups of the PK. The advantages of complete crosslinking are an improved resistance to heat distortion and an improved stiffness (elastic modulus). Nevertheless, even partial crosslinking should be included in the term "crosslinked". If a sufficient amount of crosslinking agent was not used to completely integrate all the PK chains into the network, only partial crosslinking may be present. In this case, the material generally has a higher breaking strain than a fully crosslinked material. The imine bond gives the molded body high stability. According to the present invention, the molded body is preferably a PK-based molded body. Here, "PK-based" means that PK is the substantial structural polymer component of the molded body. In one embodiment, it is preferred that PK is the only polymer component of the molded body.

[0149] The crosslinking agent usable according to the present invention has a relatively high melting point and boiling point, so that the temperature in step (iii) can be adjusted to be relatively high. This is advantageous because such crosslinking reactions are generally favored at high temperatures. However, preferably, this temperature is lower than the melting range of the PK and lower than the softening point of the molding that is not yet fully crosslinked.

[0150] Surprisingly, it was found that in the system according to the invention the crosslinking reaction already occurs below the melting range of the polymer and the molding, which was unexpected since it was generally assumed that the crosslinking reaction would preferably occur above the melting range of the polymer and the molding.

[0151] Moreover, the prior art assumes that such crosslinking reactions occur relatively quickly, within minutes or hours. According to the present invention, it has been found that the crosslinked PK can have particularly advantageous properties if the heating of the molded body in step (iii) is carried out for a period of preferably at least 1 hour, for example up to 1 hour and up to 2 days, depending on the crosslinking temperature. It has been found that such a heat treatment can significantly improve the thermal stability, elastic modulus and tensile strength.

[0152] It has been found that the stiffness of samples, especially at high temperatures, can be improved by heat treatment. Here, it has been observed that stiffness can be significantly improved by heat treatment for a certain period of time, followed by saturation, where further heat post-treatment does not improve stiffness or only slightly improves it. However, further heat post-treatment generally shows an improvement in heat distortion resistance. It has been found that heat distortion resistance can also be increased by longer heat post-treatment.

[0153] In a preferred embodiment, the molded body obtained in step (ii) is subjected to a heat treatment for a relatively short time. The heat treatment of the molded body in step (iii) is preferably carried out for a maximum of 6 hours, for example, 5 minutes to 6 hours, even more preferably 0.5 minutes to 5 hours, in particular 1 hour to 4 hours. Here, it is advantageous to be able to reduce the self-crosslinking reaction of the aliphatic polyketone that proceeds in parallel.

[0154] Alternatively, it may be advantageous to subject the shaped body in step (iii) to a heat treatment for a longer time, preferably at least 6 hours, in particular more than 2 days. In a further embodiment of the invention, the heat treatment is carried out over a period of 2 to 10 days, in particular 2 to 6 days. Preferably, the heat treatment is carried out with the exclusion of oxygen.

[0155] In a preferred embodiment, the heat treatment in step (iii) is carried out at a temperature of at least 160° C., preferably at least 180° C. Preferably, the temperature in step (iii) is between 160° C. and 240° C., particularly preferably between 190° C. and 230° C., in particular between 190° C. and 210° C. At such temperatures, efficient three-dimensional crosslinking can proceed sufficiently quickly, without the thermoplastically produced article being adversely affected, for example by undesired deformations of the shaped bodies.

[0156] The mouldings are cooled after crosslinking and can be supplied for their use or can be further processed.

[0157] As described above, both the mixture in step (i) and the shaped body may contain fillers and reinforcing materials and / or optionally different additives, where the crosslinked PK forms a matrix in which the optionally present fillers and reinforcing materials and / or additives are homogeneously distributed.

[0158] Suitable fillers and reinforcing materials are selected, for example, from glass fibers in the form of glass cloth, glass mat, glass fleece, glass silk roving or cut glass silk, wollastonite, calcium carbonate, glass beads, quartz flour, silicon nitride and boron, amorphous silica, asbestos, magnesium carbonate, calcium silicate, calcium metasilicate, kaolin, mica, feldspar, talc, and mixtures thereof.

[0159] Suitable additives are selected from antioxidants, UV and heat stabilizers, lubricants and release agents, colorants such as dyes and pigments, nucleating agents, softening agents, and mixtures.

[0160] For example, fillers and reinforcing materials can be used in an amount of up to 80% by weight, for example 0.1% to 80% by weight, in particular 1% to 60% by weight, based on the total weight of the components used to produce the shaped body.

[0161] For example, the additives can be used in an amount of up to 20% by weight, for example 0.1% to 20% by weight, more particularly 0.1% to 18% by weight, each based on the total weight of the components used to produce the shaped body.

[0162] The moldings can be obtained in particular by the method according to the invention described in the context of the present invention. The moldings preferably have the advantageous properties described for the crosslinked PK in the context of the present invention. In the context of the present invention, the term moldings refers to a product from the crosslinked PK with a defined three-dimensional shape. Here, the moldings do not have to be a defined object, but can be, for example, a coating. The moldings can be made of or contain the crosslinked PK, for example as a composite or laminate.

[0163] In a preferred embodiment, the shaped body according to the invention is subsequently annealed. In a first variant, the shaped body according to the invention is subsequently annealed for a period of 5 minutes to 6 hours. In a second variant, the shaped body according to the invention is subsequently annealed for a period of more than 6 hours up to several days. Through the various variants, respectively other advantageous properties can be achieved.

[0164] Preferably, the shaped body is subsequently annealed for a period of 5 minutes to 6 hours and has advantageous improved mechanical properties, characterized by an increased tensile modulus, an increased yield stress and an increased yield strain, compared to the shaped body from non-crosslinked PK. Preferably, the shaped body according to the invention, subsequently annealed for a period of 5 minutes to 6 hours, has a tensile modulus of at least 1800 MPa, in particular at least 1900 MPa, particularly preferably at least 2000 MPa. Preferably, the shaped body according to the invention, subsequently annealed for a period of 5 minutes to 6 hours, has a yield strength of at least 65 MPa, in particular at least 68 MPa, particularly preferably at least 70 MPa. Preferably, the shaped body according to the invention, subsequently annealed for a period of 5 minutes to 6 hours, has an improved yield strain of at least 20%, particularly preferably at least 23%.

[0165] Preferably, the moldings are subsequently annealed for a period of more than 6 hours to several days and show an advantageous increased stiffness, characterized by a high tensile modulus and increased tensile strength, compared to moldings from non-crosslinked PK. However, if the crosslinking is too strong, the yield strain is considerably reduced. Preferably, the moldings subsequently annealed for a period of more than 6 hours to several days have a tensile modulus of at least 2000 MPa, in particular at least 2250 MPa, particularly preferably at least 2500 MPa. In particular, the tensile modulus is 2000 MPa to 3000 MPa or 2250 MPa to 3000 MPa. In contrast, the tensile modulus of non-crosslinked PK is 1400 to 1800 MPa. The tensile modulus is determined according to DIN EN ISO 527-2.

[0166] Since the breaking strain of the material may decrease with increasing crosslinking, it may be desirable not to completely crosslink the PK in the molded body. Therefore, the degree of crosslinking is preferably adjusted for the desired application, for example, by the proportion of crosslinker and the type and duration of heat treatment.

[0167] Here, the degree of crosslinking is preferably not measured directly, but is determined by suitable test methods, such as high temperature tensile tests, whether the molded body has the desired properties. At very high temperatures, it is recommended to determine the dynamic modulus of elasticity.

[0168] These moldings can be used in particular in technical fields where high mechanical stability, especially high rigidity, is required. They are especially suitable for applications in the fields of automobiles, marine, aviation and spaceflight, rail vehicles, oil and gas industry, food and packaging industry and medical technology, especially as sealing articles, preferably sealing and O-rings, bushings, films, powders, coatings, fibers, bearings, backup rings, valves, thrust washers, connecting elements, snap hooks, pipes or conduits, cables, sheathing and jacketing, housings or components thereof. They are especially suitable for applications where high chemical resistance and resistance to wear are required. This is especially relevant for applications in oil and gas transportation, aviation and spaceflight technology and chemical industry, here in the manufacture of safety-related parts, as well as in the fields of power generation and the automotive industry. Also possible applications are connectors and insulators in the electronics field, since crosslinking leads to good insulating properties.

[0169] The method, moldings and sealing articles according to the invention solve the problem underlying the invention. They have improved heat resistance and higher mechanical stability compared to non-crosslinked PK, combined with good processability. In particular, these moldings have high stiffness, especially above the glass transition temperature. High stiffness is associated with reduced creep behavior at high temperatures. Improved heat resistance is shown both at maximum temperature and at continuous use temperature. Here, these products show very good chemical resistance and reduced flammability, since the material does not melt due to crosslinking and does not drip flammable material.

[0170] Moreover, the molded bodies according to the present invention can be produced simply and efficiently by thermoplastic molding methods. For example, production can be carried out by simple extrusion. Furthermore, the crosslinking agents used have relatively high boiling points and low volatility, so that these methods can be carried out in an environmentally friendly manner and without exposing users to danger.

[0171] The present invention shall be illustrated by the following examples without being limited to the specifically described embodiments.

[0172] Working Example [Brief description of the drawings]

[0173] [Figure 1] FIG. 1 shows the results of a rheological study of two mouldings according to the invention (PK with 1.00% DAPI, post-treated by heat for 1 h, as described in Example 2 (dark grey curve) and PK with 1.00% DAPI, post-treated by heat for 2 h, as described in Example 3 (light grey curve)) in comparison with a standard base material (PK without heat treatment (black curve)). The storage modulus G′ (symbols: squares) and the loss modulus G″ (symbols: triangles) are plotted on the Y-axis. The measurement time is plotted on the X-axis. [Diagram 2] FIG. 1 shows the change in the complex dynamic modulus with increasing temperature for a molded body according to the invention (PK with 1.00% DAPI, heat treated, measurement points indicated by asterisks) compared to a standard base material (PK without heat treatment, measurement points indicated by squares).

[0174] With regard to the standards stated, the editions in effect on the filing date apply unless otherwise stated.

[0175] Abbreviation: DAPI: 1-(4-aminophenyl)-1,3,3-trimethylindan-6-amine and its isomers PK: Aliphatic Poly Rike ton (MVR:60cm 3 / 10 minutes (@240℃ / 2.16kg), Smp:220℃) Example 1 A mixture of DAPI isomers with CAS number 68170-20-7 (crosslinker of formula VII) was mixed in a twin-screw compounder at a melting point of about 220° C. and a viscosity of 60 cm 3 The mixture is mixed into a commercial PK with an MVR of 10 min (240°C and weight load of 2.16 kg) and the strands are chopped into granules.

[0176] The granules are processed into test specimens in an injection mould and subsequently also subjected to a thermal post-treatment in a vacuum oven for a period of 1 hour.

[0177] After completion of the thermal post-treatment, tensile tests were performed per ISO 527-2 and values ​​were compared to the non-crosslinked PK base material (Table 1).

[0178] [Table 2]

[0179] Chemical post-crosslinking increased the tensile modulus of PK by approximately 13% compared to the non-crosslinked base material, and also increased the yield stress by approximately 11% and the yield strain by approximately 24% compared to the non-crosslinked base material.

[0180] Example 2 A mixture of DAPI isomers with CAS number 68170-20-7 (crosslinker of formula VII) was mixed in a twin-screw compounder at a melting point of about 220° C. and a viscosity of 60 cm 3 The mixture is mixed into a commercial PK with an MVR of 10 min (240°C and weight load of 2.16 kg) and the strands are chopped into granules.

[0181] The granules are processed into test specimens in an injection mould and subsequently also subjected to a thermal post-treatment in a vacuum oven for a period of 2 hours.

[0182] After completion of the thermal post-treatment, tensile tests were performed per ISO 527-2 and values ​​were compared to the non-crosslinked PK base material (Table 2).

[0183] [Table 3]

[0184] Chemical post-crosslinking increased the tensile modulus of PK by approximately 14% compared to the non-crosslinked base material, and also increased the yield stress by approximately 13% and the yield strain by 31% compared to the non-crosslinked base material.

[0185] In addition to the tensile test, a rheological study was carried out on an Anton Paar rheometer type MCR-302, which shows the chemical post-crosslinking of aliphatic polyketones with the crosslinker DAPI. In comparison with a standard base material (PK without heat treatment), two mouldings according to the invention (PK with 1.00% DAPI, post-treated by heat for 1 hour, as described in Example 2 and PK with 1.00% DAPI, post-treated by heat for 2 hours, as described in Example 3) were investigated. The test conditions are listed in Table 3.

[0186] [Table 4]

[0187] Example 4 A mixture of DAPI isomers with CAS number 68170-20-7 (crosslinker of formula VII) was mixed in a twin-screw compounder at a melting point of about 220° C. and a viscosity of 60 cm 3 The mixture is mixed into a commercial PK with an MVR of 10 min (240°C and weight load of 2.16 kg) and the strands are chopped into granules.

[0188] The granules are processed in an injection moulding machine to give test pieces and are subsequently subjected to a thermal aftertreatment, likewise under a protective gas atmosphere in a heating oven over a period of 6 days.

[0189] After completion of the thermal post-treatment, tensile tests were performed per ISO 527-2 and values ​​were compared to the non-crosslinked PK base material (Table 4).

[0190] [Table 5]

[0191] Post-crosslinking more than doubled the tensile modulus of PK compared to the non-crosslinked base material. The crosslinked material no longer exhibits ductile behavior and the ultimate strength is approximately 10 MPa higher than the non-crosslinked material. The elasticity of the material is significantly limited by the crosslinking points, which reduces the breaking strain to 2.5%.

[0192] The uncrosslinked PK base material melts at approximately 220° C., whereas no further melting is observed in the post-crosslinked material.

[0193] The uncrosslinked base material and the post-crosslinked PK were tested by DMA in a T-sweep, where the results shown in Figure 2 were obtained. Dynamic Mechanical Analysis (DMA) is a thermal method for determining the physical properties of plastics. The temperature gradient (temperature sweep) indicates the change in dynamic modulus and therefore stiffness over the measured temperature range.

[0194] The temperature gradient was measured using a specimen strip (approximately 4 mm wide, 3 mm thick, and 45 mm long) under the following conditions: heating rate 2 K / min, contact force 0.5 N, frequency 1.0 Hz, average strain 0.5%, and strain amplitude + / - 0.1%. These results are shown graphically in Figure 2.

[0195] FIG. 2 shows the change in the complex dynamic modulus with increasing temperature for a molded body according to the invention (PK with 1.0% DAPI, heat treated, measurement points shown by asterisks) compared to the standard base material PK (PK without heat treatment, measurement points shown by squares).

[0196] These results show that the PK crosslinked according to the invention has advantageous thermal properties. The material shows an increased modulus (see Table 4) and an increased resistance to heat distortion, as already demonstrated in tensile tests according to ISO 527-2. While the significant decrease in modulus in the non-crosslinked PK from about 210° C. onwards is due to melting of the material, the loss in modulus in the crosslinked material is not due to melting but to the formation of cracks in the material.

Claims

1. A molded article comprising a matrix in which an aliphatic polyketone is crosslinked while forming an imine group with at least one diamine source as a crosslinking agent, the diamine source being: - General formula (V): 【Chemical 1】 [In the formula, R 19 and R 20 are each independently selected from H, substituted or unsubstituted alkyl having 1 to 20 carbon atoms, substituted or unsubstituted aryl having 5 to 12 carbon atoms, F, and Cl; R 21 is a carbocyclic group having 2 to 3 carbon ring atoms and optionally substituted with at least one alkyl group having 1 to 4 carbon atoms; - Compound 【Chemistry 2】 or an oligomer / polymer containing this compound by polymerization; and - their mixtures is selected from wherein the proportion of the crosslinking agent is 0.05% by weight to 15% by weight based on the total amount of the aliphatic polyketone and the crosslinking agent.

2. 2. The molding according to claim 1, which comprises at least one filler and reinforcing material, and / or additives different therefrom.

3. A method for producing a molded body, comprising: i) providing a mixture containing at least one aliphatic polyketone and at least one crosslinker; ii) producing a shaped body from the mixture obtained in step i); and iii) heat-treating the molded body at a temperature at which the aliphatic polyketone is crosslinked; Including, wherein the crosslinking agent is - General formula (V): 【Chemistry 3】 [In the formula, R 19 and R 20 are each independently selected from H, substituted or unsubstituted alkyl having 1 to 20 carbon atoms, substituted or unsubstituted aryl having 5 to 12 carbon atoms, F, and Cl; R 21 is a carbocyclic group having 2 to 3 carbon ring atoms and optionally substituted with at least one alkyl group having 1 to 4 carbon atoms; - Compound 【Chemistry 4】 or an oligomer / polymer containing this compound by polymerization; and - their mixtures is selected from wherein the proportion of the crosslinking agent is 0.05% by weight to 15% by weight based on the total amount of the aliphatic polyketone and the crosslinking agent.

4. The crosslinker is represented by formula (V.a1): 【Chemistry 5】 4. The method of claim 3, wherein the compound is

5. 5. The method according to claim 3 or 4, wherein in step i) the at least one aliphatic polyketone, the at least one crosslinking agent, optionally fillers and reinforcing agents, and optionally further additives different therefrom, are melt-mixed or dry-mixed.

6. 6. The method according to claim 3, wherein in step i), the at least one aliphatic polyketone, the at least one crosslinking agent, optionally fillers and reinforcing agents, and optionally further additives different therefrom, are fed to an extruder, mixed while plasticizing, and optionally granulated.

7. The aliphatic polyketone has a viscosity of 2 cm at 240° C. as measured by DIN ISO 1130. 3 / 10 minutes to 200cm 3 7. The method of claim 3, wherein the melt viscosity is in the range of 1 / 10 min. / 10 min.

8. 8. The method of claim 3, wherein the mixture does not contain an entrained solvent.

9. 9. The process according to any one of claims 3 to 8, wherein the temperature in step ii) is at least 220°C.

10. 10. The method according to any one of claims 3 to 9, wherein the mixture in step ii) is processed by extrusion, hot pressing, injection molding, and / or 3D printing.

11. 11. The method according to any one of claims 3 to 10, wherein the shaped body obtained in step ii) is subjected to a heat treatment in step iii) for 5 minutes to 6 hours.

12. 11. The method according to any one of claims 3 to 10, wherein the shaped body obtained in step ii) is subjected to a heat treatment in step iii) for 0.5 minutes to 5 hours.

13. 13. The method according to claim 11 or 12, wherein the heat treatment in step iii) is carried out at a temperature of at least 160°C.

14. at least one aliphatic polyketone (PK); - General formula (V): 【Chemistry 6】 [In the formula, R 19 and R 20 are each independently selected from H, substituted or unsubstituted alkyl having 1 to 20 carbon atoms, substituted or unsubstituted aryl having 5 to 12 carbon atoms, F, and Cl; R 21 is a carbocyclic group having 2 to 3 carbon ring atoms and optionally substituted with at least one alkyl group having 1 to 4 carbon atoms; - Compound 【Chemistry 7】 or an oligomer / polymer containing this compound by polymerization; and - their mixtures and at least one cross-linking agent selected from Contains wherein the proportion of the crosslinking agent is 0.05% by weight to 15% by weight based on the total amount of the aliphatic polyketone and the crosslinking agent.

15. Use of a shaped body as defined in claim 1 or 2 or a shaped body obtainable by the method as defined in claims 3 to 13 in the fields of automotive, maritime, aviation and spaceflight, rail vehicles, oil and gas industry, food and packaging industry and medical technology.

16. 3. Sealing articles, thrust washers, backup rings, valves, connectors, insulators, snap hooks, bearings, bushings, films, powders, coatings, fibers, sealings and O-rings, pipes and conduits, cables, sheathing and jacketing, housings for electrical or chemical applications, which consist of or contain the moldings according to claim 1 or 2.

Citation Information

Patent Citations

  • Polyketone / polyhexamethylene terephthalamide alloy material and preparation method thereof

    CN106633786A

  • Curable polymer composition

    JP1984168057A