Steel bars for mechanical structures
A steel composition combining indium with bismuth, tin, or tellurium enhances machinability and maintains hot ductility, addressing the cost and environmental concerns of lead replacement in machine structure steels.
Patent Information
- Application Number
- JP2020034167
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-28
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2040-02-28
AI Technical Summary
Existing steel compositions used in machine structures, such as automobile parts, face challenges in achieving sufficient machinability while reducing the cost and environmental impact of lead (Pb) replacement elements like indium (In), which also affect manufacturability due to decreased hot ductility.
A steel composition that includes indium in combination with bismuth (Bi), tin (Sn), or tellurium (Te), along with controlled ratios and additives, to enhance machinability by promoting indium-based inclusions, while maintaining hot ductility and reducing indium content.
The steel composition achieves improved machinability with reduced indium content, ensuring hot ductility and cost-effectiveness, suitable for high-speed cutting processes.
Smart Images

Figure 0007560714000007 
Figure 0007560714000008 
Figure 0007560714000009
Abstract
Description
[Technical field]
[0001] The present invention Machine structure rod Steel, especially for automobile parts Machine structure rod Regarding steel. [Background technology]
[0002] General machinery products such as automobiles, construction machinery, and industrial machinery contain multiple parts such as gears and shafts. Many of these parts are manufactured by cutting. Therefore, the steel used as the material for these parts must have excellent machinability. It is known that machinability is measured by chip disposal, tool life, cutting resistance, etc.
[0003] It has been known for some time that the inclusion of Pb improves machinability. However, since Pb is an environmentally hazardous substance, there is a need for technology to improve machinability by reducing the Pb content as much as possible from the perspective of environmental protection.
[0004] There have been some inventions that focus on In as an alternative element to Pb. For example, Patent Document 1 discloses that the inclusion of a wide range of In, from a trace amount to a large amount, improves the tool life when a tool made of high-speed steel (hereinafter referred to as "HSS tool") is used to drill holes at 40 to 50 m / min. Furthermore, Patent Document 2 discloses that a relatively small amount of In is contained, which improves chip disposal when cutting with a high-speed steel tool at 10 to 40 m / min. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 62-33743 [Patent Document 2] Japanese Patent Application Publication No. 7-54099 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the conventional techniques have some problems. Since In is generally an expensive element, in order to use it as a Pb substitute, it is desirable that In has a large effect of improving machinability that is commensurate with the cost.
[0007] Patent Document 1 simply contains In, and it is difficult to say that it has a sufficient effect worth the cost. Furthermore, In may reduce ductility in high temperature ranges, i.e., hot ductility, and may reduce manufacturability during continuous casting, hot rolling, and hot forging, but no technology has been proposed to solve this problem.
[0008] Patent Document 2 proposes a technology that not only contains In but also enhances the effects of containing In. However, the application of this technology is limited to a range where the In content is low to begin with, and therefore is insufficient as a technology to replace Pb.
[0009] The present invention has been devised in view of the above-mentioned problems, and its object is to reduce the In content as much as possible in order to ensure sufficient hot ductility to ensure manufacturability in addition to reducing costs, while enhancing the effect of improving machinability. Machine structure rod The purpose is to provide steel. [Means for solving the problem]
[0010] In order to solve the above problems, the inventors of the present invention investigated the mechanism by which In improves machinability. When the In content is low, it dissolves in steel, but when the In content is increased, it precipitates and exists as In-based inclusions in addition to the dissolved In. It is these In-based inclusions that mainly contribute to the improvement of machinability.
[0011] As a result of investigating various methods for further enhancing the machinability improving effect of In, it was found that the combined addition of In and Bi, In and Sn, or In and Te was effective.
[0012] When Bi is added alone, it exists as Bi particles in the steel, and it is widely known that it improves machinability in the same way as Pb. On the other hand, when In and Bi are added in combination, composite particles of Bi and In particles precipitate, which increases the amount of In present as inclusions, that is, In-based inclusions, and is thought to improve machinability. It has been found that to achieve this effect, it is best to add a certain amount of Bi relative to the In content.
[0013] Since both Sn and In tend to segregate at grain boundaries and also bond with each other, it is believed that the combined addition of Sn and In promotes segregation, increasing the concentration locally and increasing the presence of In-based inclusions. It was discovered that to achieve this effect, it is best to include a certain amount of Sn relative to the In content.
[0014] When Te is added alone, it is mainly present as MnTe particles in steel, and it is widely known that it improves machinability. On the other hand, when In and Te are added in combination, In and Te form compounds in steel and precipitate as a compound, and these In-based inclusions improve machinability. In addition, it was found that compounds of In and Te are often formed in contact with MnS, and in order to sufficiently precipitate In and Te compounds, it is effective to increase the presence ratio of MnS, which crystallizes from the liquid phase during solidification and becomes relatively coarse. In other words, it was found that in order to obtain the effect of improving machinability, in addition to appropriately controlling the content ratio of In and Te to form In and Te compounds, it is also effective to appropriately control the content ratio of Mn and S to obtain sufficient crystallized MnS.
[0015] In addition, in all cases of combined addition, the presence of In-based inclusions was observed around oxides such as Al2O3. Based on this result, it was found that in order to increase the amount of In-based inclusions even with the same In content, it is preferable to increase the amount of oxides such as Al2O3 within a range that does not significantly affect mechanical properties such as fatigue strength.
[0016] Based on the above findings, the present inventors have succeeded in improving machinability while maintaining hot ductility with a small In content by the combined addition of In and Bi, In and Sn, and In and Te, and have thus completed the present invention. Machine structure rod The steels are as follows:
[0017] (1) The components are in mass%: C: 0.05-0.85%, Si: 0.01 to 3.00%, Mn: 0.01 to 3.00%, Cr: 0.01-3.00%, P: 0.100% or less, S: 0.001~0.150% or less, In: 0.0003~0.0600%, Al: 0.002 to 0.050%, N: 0.0030 to 0.0250%, and O: 0.0050% or less and Bi: 0.0001 to 0.0950%, Sn: 0.0001 to 0.3000%, and Te: 0.0001 to 0.0300%, and the balance being Fe and impurities. At least one of the following formulas 1, 2, and 3 is satisfied: If formula 3 is satisfied, formula 4 is also satisfied. Machine structure rod steel. 0.010≦[Bi%] / [In%] (Formula 1) 0.200≦[Sn%] / [In%] (Formula 2) 0.700≦[In%] / [Te%] (Formula 3) 22.00≦[Mn%] / [S%]≦150.00 (Formula 4) Here, [In%], [Bi%], [Sn%], [Te%] and [Mn%] represent the mass% content of In, Bi, Sn, Te and Mn in the steel, respectively, and 0 is substituted if not contained. (2) The above Machine structure rod The steel further comprises, in mass percent: O: 0.0050% or less, and Insol.Al: 0.0060% or less The present invention relates to a method for producing Machine structure rod steel. (3) The above Machine structure rod The steel further comprises, in mass percent: Ca: 0.0050% or less, Mg: 0.0050% or less, Zr: 0.0050% or less, and REM: 0.0050% or less The composition according to claim 1 or 2, characterized in that it contains one or more of the following: Machine structure rod steel. (4) The above Machine structure rod The steel further comprises, in mass percent: Ti: 1.000% or less, Nb: 1.000% or less, and V:1.000% or less The present invention relates to a method for manufacturing a pharmaceutical composition comprising the steps of: Machine structure rod steel. (5) The above Machine structure rod The steel further comprises, in mass percent: Mo: 1.00% or less Ni: 1.40% or less, Cu: 1.40% or less, and B: 0.0050% or less The present invention relates to a method for manufacturing a semiconductor device, comprising the steps of: Machine structure rod steel. (6) The above Machine structure rod The steel further comprises, in mass percent: Sb: 0.5000% or less, Se: 0.5000% or less, Zn: 0.5000% or less, and Pb: 0.09% or less The present invention relates to a method for manufacturing a pharmaceutical composition comprising the steps of: Machine structure rod steel. Effect of the Invention
[0018] According to the steel for machine structural use of the present invention, the In content is reduced as much as possible, while ensuring hot ductility and exhibiting a high effect of improving machinability. Machine structure rod You can get steel. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a diagram showing the relationship between Bi / In and machinability (cutting resistance [N]) for steels of examples and comparative examples that have similar hardness before cutting and contain Bi. [Diagram 2] FIG. 2 is a diagram showing the relationship between the Sn / In ratio and machinability (cutting resistance [N]) for steels of examples and comparative examples that have similar hardness before cutting and contain Sn. [Diagram 3] FIG. 3 is a diagram showing the relationship between In / Te and machinability (cutting resistance [N]) for steels of examples and comparative examples that have similar hardness before cutting and contain Te. [Figure 4] FIG. 4 is a diagram showing the relationship between Mn / S and machinability (cutting resistance [N]) for steels of examples and comparative examples that have similar hardness before cutting and contain Te. [Diagram 5] FIG. 2 is a diagram showing the relationship between the hardness (HV) before cutting and the machinability (cutting resistance [N]) of the steels of the examples and the comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention Machine structure rod The steel and the cutting method thereof will be described. First, Machine structure rod The reasons for limiting the steel composition are explained below. In the following explanation, "%" for the content of each element means "mass%" unless otherwise specified. Also, [In%], [Bi%], [Sn%], [Te%] and [Mn%] represent the mass% content of In, Bi, Sn, Te and Mn in the steel, respectively.
[0021] (C: 0.05~0.85%) C is an element that is contained to ensure the strength of steel. If the C content is less than 0.05%, the hardness decreases, and the strength is insufficient when the steel is used without heat treatment after cutting. In addition, there is a risk that sufficient strength will not be obtained when the final processed product is quenched and tempered for use. For this reason, the C content is set to 0.05% or more. On the other hand, if the C content is more than 0.85%, a large amount of carbides is generated, deteriorating the machinability. For this reason, the C content is set to 0.85% or less. The preferable lower limit of the C content is 0.16%, and the preferable upper limit is 0.60%.
[0022] (Si: 0.01 to 3.00%) Si is generally contained as a deoxidizing element, but it also has the effect of strengthening ferrite and imparting temper softening resistance. However, if the Si content is less than 0.01%, a sufficient deoxidizing effect cannot be obtained. On the other hand, if the Si content exceeds 3.00%, the steel becomes too hard and embrittles. Therefore, the Si content is set to 0.01 to 3.00%. The preferable lower limit of the Si content is 0.06%, the more preferable lower limit is 0.20%, the preferable upper limit is 2.00%, and the more preferable upper limit is 1.30%.
[0023] (Mn: 0.01 to 3.00%) Mn is an element necessary for fixing and dispersing sulfur (S) in steel as MnS, and for improving hardenability and securing strength after hardening by dissolving in the matrix. However, if the Mn content is less than 0.01%, S in the steel combines with Fe to form FeS, making the steel brittle. On the other hand, if the Mn content exceeds 3.00%, the hardenability becomes too high, leading to a significant increase in hardness and a decrease in machinability. Therefore, the Mn content is set to 0.01 to 3.00%. The preferred lower limit of the Mn content is 0.10%, and more preferably 0.20%. The preferred upper limit of the Mn content is 1.80%, and more preferably 1.70%.
[0024] (Cr: 0.01~3.00%) Cr is a solid solution strengthening element for steel, and when parts are quenched and tempered for use, it improves the hardenability and imparts temper softening resistance to improve fatigue strength after quenching. If the Cr content is less than 0.01%, these effects cannot be obtained. On the other hand, if the Cr content exceeds 3.00%, Cr carbides are generated and the steel becomes embrittled. Therefore, the Cr content is set to 0.01 to 3.00%. The preferred lower limit of the Cr content is 0.05%, and more preferably 0.10%. The preferred upper limit of the Cr content is 2.00%, and more preferably 1.30%.
[0025] (P:0.100% or less) P is an impurity. Since P segregates at the austenite grain boundaries and causes grain boundary cracking during hot working, the P content is set to 0.100% or less. The preferred upper limit of the P content is 0.030%, and more preferably 0.010% or less. Since it is desirable to reduce the P content as much as possible, there is no particular lower limit, but restricting the P content to less than 0.001% involves excessive costs. Therefore, the range of the P content may be 0.001% or more.
[0026] (S:0.001~0.150%) S combines with Mn to form MnS. MnS has the effect of improving machinability, and in order to obtain this effect, it is preferable to contain S at 0.001% or more. On the other hand, if the S content exceeds 0.150%, the toughness and fatigue strength are significantly reduced. Therefore, the S content is set to 0.001 to 0.150%. The preferred lower limit of the S content is 0.005%, and more preferably 0.010%. The preferred upper limit of the S content is 0.080%, and more preferably 0.050%.
[0027] (In:0.0003~0.0600%) In reduces ductility at 800°C or higher, which reduces the yield of continuous casting and rolling, and reduces manufacturability during hot forging in part manufacturing. In addition, since In is generally an expensive element, its content is reduced as much as possible, and its upper limit is set to 0.0600%. On the other hand, In not only has the effect of improving machinability by itself, but also has the effect of improving machinability by adding it in combination with Bi, Sn, and Te in the present invention, so it is preferable to contain 0.0003% or more of In. In order to obtain the effect of improving machinability by adding it in combination, the lower limit of the In content can be 0.0004%, 0.0005%, or 0.0006%. On the other hand, from the viewpoints of ensuring hot ductility and reducing costs, the upper limit of the In content can be 0.0500%, 0.0200%, 0.0100%, 0.0080%, 0.0050%, 0.0040%, 0.0030%, 0.0020%, 0.0010%, 0.0009%, or 0.0008%.
[0028] (Bi: 0.0001 to 0.0950%, and 0.010 or less [Bi%] / [In%]) When Bi is contained together with In, In and Bi precipitate in the steel as a compound, improving machinability. The term "composite precipitation" as used here includes the cases where In and Bi form a compound, and where they are close to each other and exist as simple substances. If Bi exists together with In, the effect of improving machinability due to complex precipitation is obtained, so the lower limit of Bi is set to 0.0001%. On the other hand, if the Bi content exceeds 0.0950%, the ductility at 800°C or higher decreases, causing a decrease in the yield of continuous casting and hot rolling, and a decrease in manufacturability during hot forging in part manufacturing. For this reason, the Bi content is set to 0.0001% or more and 0.0950% or less. In order to obtain the effect of improving machinability by combined addition, the lower limit of the Bi content can take values of 0.0002%, 0.0003%, 0.0005%, 0.0007%, 0.0009%, 0.0010%, 0.0020%, 0.0030%, 0.0040%, and 0.0050%. On the other hand, from the viewpoint of ensuring hot ductility, the upper limit of the Bi content can be 0.0900%, 0.0850%, 0.0800%, 0.0750%, 0.0700%, 0.0650%, 0.064%, 0.0600%, 0.0500%, 0.0400%, 0.0300%, 0.0200%, 0.0100%, 0.0090%, 0.0080%, or 0.0070%.
[0029] To obtain the effect of improving machinability due to the above-mentioned complex precipitation of In and Bi, it is preferable to contain a certain amount of Bi relative to the In content, and specifically, the ratio of the Bi to In content (mass%) in the steel ([Bi%] / [In%]) should be 0.010 or more (Figure 1). The lower limit of [Bi%] / [In%] can be 0.020, 0.050, 0.080, 0.100, 0.150, 0.200, 0.250, 0.300, 0.350, or 0.400. The upper limit of [Bi%] / [In%] is not particularly limited, but may be the value obtained by dividing the upper limit of the Bi content by the lower limit of the In content. Specifically, when the lower limit of the In content is 0.0003% and the upper limit of the Bi content is 0.0950%, the ratio becomes 316.7, so this may be used as the upper limit.
[0030] (Sn:0.0001~0.3000%, 0.200≦[Sn%] / [In%]) Both Sn and In tend to segregate at grain boundaries, and adding them in combination with In promotes the segregation of In and increases the number of In-based inclusions, improving machinability. The presence of Sn together with In promotes the segregation of In, and the In-based inclusions improve machinability, so the lower limit of the Sn content is set to 0.0001%. On the other hand, if the Sn content exceeds 0.3000%, the ductility at 800°C or higher decreases, causing a decrease in the yield rate of continuous casting and hot rolling, and a decrease in manufacturability during hot forging in part manufacturing. For this reason, the Sn content is set to 0.0001% or more and 0.3000% or less. In order to obtain the effect of improving machinability by the combined addition, the lower limit of the Sn content may be 0.0002%, 0.0003%, 0.0005%, 0.0007%, 0.0009%, 0.0010%, 0.0020%, 0.0030%, 0.0040%, or 0.0050%. On the other hand, in order to ensure hot ductility, the upper limit of the Sn content may be 0.2800%, 0.2500%, 0.2300%, 0.2000%, 0.1800%, 0.1500%, 0.1300%, or 0.100%.
[0031] To obtain the effect of promoting the segregation of In by including Sn, it is preferable to include a certain amount of Sn relative to the In content, and specifically, the ratio of the Sn to In content (mass%) in the steel ([Sn%] / [In%]) should be 0.200 or more (Figure 2). The lower limit of [Sn%] / [In%] can be 0.230, 0.250, 0.280, 0.300, 0.350, 0.400, 0.450, 0.500, 0.550, or 0.600. The upper limit of [Sn%] / [In%] is not particularly limited, but may be the value obtained by dividing the upper limit of the Sn content by the lower limit of the In content. Specifically, the lower limit of the In content is 0.0003%, and the upper limit of the Sn content is 0.3000%, which is the value that becomes 1000, so this may be used as the upper limit.
[0032] (Te:0.0001~0.0300%, 0.700≦[In%] / [Te%]) When Te is contained together with In, In and Te form a compound in the steel and precipitate as a complex, improving machinability. The term "composite precipitation" as used here includes the cases where In and Te form a compound, and where In and MnTe are in close proximity. If Te exists together with In, the effect of improving machinability due to complex precipitation is obtained, so the lower limit of Te is set to 0.0001%. On the other hand, if the Te content exceeds 0.0300%, the ductility at 800°C or higher decreases, causing a decrease in the yield of continuous casting and hot rolling, and a decrease in manufacturability during hot forging in part manufacturing. For this reason, the Te content is set to 0.0001% or more and 0.0300% or less. In order to obtain the effect of improving machinability by the combined addition, the lower limit of the Te content may be 0.0002%, 0.0003%, 0.0005%, 0.0007%, 0.0009%, 0.0010%, 0.0015%, 0.0020%, 0.0025%, 0.0030%, 0.0035%, 0.0040%, 0.0045%, or 0.0050%. On the other hand, in order to ensure hot ductility, the upper limit of the Te content may be 0.0280%, 0.0250%, 0.0200%, 0.0180%, 0.0150%, 0.0120%, 0.0100%, 0.0090%, 0.0080%, or 0.0070%.
[0033] To obtain the above-mentioned effect of improving machinability due to the complex precipitation of In and Te, it is advisable to appropriately control the ratio of the In and Te contents, specifically, the ratio of the In and Te contents (mass%) in the steel ([In%] / [Te%]) should be 0.700 or more (Fig. 3). The lower limit of [In%] / [Te%] can be 0.750, 0.800, 0.850, 0.900, 0.950, 1.00, 1.050, 1.100, 1,150, or 1.200. The upper limit of [In%] / [Te%] is not particularly limited, but may be set to the value obtained by dividing the upper limit of the In content by the lower limit of the Te content. However, since there is an upper limit to the In content, [In%] / [Te%] is naturally limited by the upper limit of the In content.
[0034] (22.00≦[Mn%] / [S%]≦150.00) In order to promote the precipitation of In and Te compounds, it is effective to increase the coarse crystallized MnS, and for this purpose, the ratio of Mn and S content (mass%) in the steel ([Mn%] / [S%]) should be 22.00 or more and 150.00 or less (Figure 4). If [Mn%] / [S%] is less than 22.00, the ratio of fine MnS precipitated in the solid phase becomes high, and the effect of promoting the precipitation of In and Te compounds is not sufficiently obtained. The lower limit of [Mn%] / [S%] can be 22.20, 22.50, 23.00, 25.00, 27.50, 30.00, 32.50, 35.00, 37.50, 40.00, 50.00, 60.00, 70.00, 80.00, or 90.00. On the other hand, if [Mn%] / [S%] is greater than 150.00, there will be a lot of Mn that does not contribute to the formation of MnS, making it easier for MnTe to form, which will inhibit the formation of In and Te compounds. The upper limit of [Mn%] / [S%] can be 145.00, 140.00, 135.00, 130.00, 125.00, 120.00, 115.00, or 110.00.
[0035] (Al: 0.002~0.050%) Al combines with N to form AlN, which has the effect of suppressing grain coarsening in the austenite region. In order to obtain this effect, the Al content should be 0.002% or more. On the other hand, if Al is contained in excess, it tends to remain as coarse oxides, and fatigue properties deteriorate. Therefore, the Al content is set to a range of 0.002 to 0.050%. The preferred lower limit of the Al content is 0.005%, and more preferably 0.010%. The preferred upper limit of the Al content is 0.040%, and more preferably 0.030%. The Al content here means the total Al content.
[0036] (N:0.0030~0.0250%) N (nitrogen) combines with Al, V, etc. in steel to form carbonitrides, which pin the austenite grain boundaries, suppress grain growth, and refine the structure transformed from austenite. To obtain this effect, it is advisable to include 0.0030% or more. On the other hand, if N is excessively included in excess of 0.0250%, the ductility at high temperatures of 1000°C or higher decreases, causing a decrease in yield during continuous casting and hot rolling. For this reason, the N content must be 0.0250% or less. The preferred lower limit of the N content is 0.0040%, and more preferably 0.0050%. The preferred upper limit of the N content is 0.0200%, and more preferably 0.0150%. The present invention Machine structure rod In addition to the basic components described above, the steel may contain one or more elements selected from the following elements as steel components.
[0037] (O:0.0050% or less) When the O (oxygen) content is high, it tends to remain as coarse oxides, which deteriorates fatigue properties. For this reason, in the present invention, the upper limit of the O content is set to 0.0050% or less. On the other hand, there is no particular restriction on the lower limit of O, but since O forms oxide-based inclusions and may improve machinability by increasing the number of In particles, in order to obtain this effect, it is preferable that the O content be 0.0009% or more.
[0038] (Insol.Al: 0.0060% or less) In order to control the form of the In-based inclusions, it is preferable to disperse Al contained in the steel as Al2O3 in the steel. Insol.Al, which is acid-insoluble Al, is regarded as the amount of Al present as Al2O3, and this amount is measured. On the other hand, if the amount of insol.Al is large, coarse oxides are likely to remain, and there is a concern that fatigue properties will deteriorate. For this reason, insol.Al is preferably 0.0060% or less. There is no particular limit on the lower limit of insol.Al, but in order to sufficiently secure In-based inclusions of a predetermined size, it is preferable that insol.Al is 0.0011% or more. The lower limit of insol.Al can be 0.0012%, 0.0015%, 0.0018%, 0.0020, 0.0025%, or 0.0030%. In addition, the upper limit of insol. Al can take the values of 0.0058%, 0.0055%, 0052%, 0.0050, 0.0048%, and 0.0045%.
[0039] Insol.Al is measured by subjecting the acid-insoluble residue to ICP (inductively coupled plasma) analysis. In this embodiment, the collected sample is decomposed with aqua regia, and the solution is filtered using filter paper (type 5 C). The extracted residue is heated and melted using a melting agent, and the melt is cooled and solidified. Next, the solidified melt is dissolved using nitric acid or the like, and measured by ICP (inductively coupled plasma) analysis. The reagents used and sample preparation may refer to JIS G 1257:2013 Iron and steel - Atomic absorption spectrometry method.
[0040] (Ca: 0.0050% or less, Mg: 0.0050% or less, Zr: 0.0050% or less, and REM: 0.0050% or less (Type 1 or Type 2 or more) Ca, Mg, Zr, and REM (rare earth elements) are all deoxidizing elements that generate oxides in steel and control the form of MnS in steel, thereby contributing to improving mechanical properties. In order to obtain these effects, Ca, Mg, Zr, and REM may be contained within a range that does not impair the properties of the steel of the present invention. Each element may be contained preferably in an amount of 0.0001% or more. On the other hand, if Ca, Mg, Zr, and REM are contained in an amount exceeding 0.0050%, the oxides become coarse and the fatigue strength decreases. Therefore, the contents of Ca, Mg, Zr, and REM are all set to 0.0050% or less, and preferably 0.0020% or less.
[0041] Here, REM denotes a rare earth metal element, and is one or more selected from Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. The content of the REM means the total content of these elements.
[0042] (Ti: 1.000% or less, Nb: 1.000% or less, V: 1.000% or less, either one or more of the following) Ti, Nb and V form fine carbides, nitrides and carbonitrides with C and N, suppressing grain growth and abnormal grain growth during heating in the austenite temperature range, contributing to fine homogenization of the structure and improving impact properties. To achieve this effect, one or more of Ti, Nb and V may be contained. Each element is preferably 0.005% or more, more preferably 0.010% or more, and even more preferably 0.020% or more. On the other hand, if Ti, Nb and V are all contained in excess of 1.000%, hard carbides are formed and machinability is reduced. Therefore, Ti, Nb and V are all set to 1.000% or less. The preferred contents of Ti and Nb are 0.200% or less, more preferably 0.150% or less, and even more preferably 0.040% or less. V is preferably 0.500% or less, more preferably 0.320% or less.
[0043] (Mo: 1.00% or less, Ni: 1.40% or less, Cu: 1.40% or less, and B: 0.0050% or less, one or two types) Mo, Ni, Cu and B are all elements that improve hardenability. To obtain this effect, they may be contained within a range that does not impair the excellent properties of the steel of the present invention. Preferably, Mo, Ni and Cu may all be contained in an amount of 0.01% or more, and B may be contained in an amount of 0.0003% or more. On the other hand, if Mo exceeds 1.00%, the hardenability becomes too high, which leads to a significant increase in hardness, and the workability during cutting and forging decreases. For this reason, the Mo content is set to 1.00% or less, preferably 0.30% or less. If Ni and Cu both exceed 1.40%, the hardenability becomes too high, which leads to a significant increase in hardness, similar to Mo, and the workability decreases. For this reason, the upper limits of the Ni and Cu contents are each set to 1.40% or less. If B is contained in an amount exceeding 0.0050%, the effect is saturated. Therefore, when B is contained, the B content is preferably 0.0003% or more, more preferably 0.0010% or more, and is preferably 0.0050% or less, more preferably 0.0025% or less.
[0044] (Sb: 0.5000% or less, Se: 0.5000% or less, Zn: 0.5000% or less, and Pb: 0.09% or less, type 1 or type 2) Sb and Se are elements that have the effect of improving machinability. To obtain this effect, they may be contained within a range that does not impair the properties of the steel of the present invention. Preferably, Sb and Se may be contained in an amount of 0.0003% or more. On the other hand, if Sb and Se exceed 0.5000%, hot brittleness appears, which may cause defects or make hot rolling difficult, so Sb and Se are each preferably 0.5000% or less, and more preferably 0.2000% or less. Zn is also an element that has the effect of improving machinability, and to obtain this effect, they may be contained within a range that does not impair the properties of the steel of the present invention. Preferably, Zn may be contained in an amount of 0.0003% or more. On the other hand, if Zn exceeds 0.5000%, it becomes difficult to manufacture the steel, so it is preferably 0.5000% or less.
[0045] Pb is an element that has been used in the past to improve machinability. However, since it is an environmentally hazardous substance, it is preferable to have as little Pb as possible from the viewpoint of environmental protection, and the Pb content is limited to 0.09% or less. More preferably, it is 0.05% or less, 0.03% or less, or 0.02% or less.
[0046] The present invention Machine structure rod The composition of the steel is as described above, with the balance being Fe and impurities. Note that impurities may be mixed into the steel depending on the conditions of raw materials, materials, manufacturing equipment, etc., but this is permissible as long as it does not impair the characteristics of the present invention.
[0047] In the present invention, the effect of improving machinability is obtained by increasing the amount of In-based inclusions in the steel. In this specification, the In-based inclusions refer to In particles, In compounds, and In precipitates, including In simple particles, composite precipitates of Bi and In, In particles precipitated at a locally increased concentration due to the composite addition of Sn, and composite precipitates of In and Te. The inventors further investigated the appropriate number density of In-based inclusions, and found that the number density of In-based inclusions having a circle equivalent diameter of 2.0 μm or more is 0.5 pieces / mm 2 It was revealed that it is preferable that the number density of In-based inclusions having an equivalent circle diameter of less than 2.0 μm is less likely to become the starting point for crack generation during cutting and may have a small effect of providing lubrication on the tool, and that the number density of In-based inclusions having an equivalent circle diameter of 2.0 μm or more is preferably 0.5 pieces / mm 2 If it is less than this, the effect of improving the machinability may be small.
[0048] The circle equivalent diameter and number density of In-based inclusions can be measured by the following method. A steel bar sample is cut in a cross section (longitudinal section) including the axial direction of the steel bar, and a specimen including the longitudinal section is taken. The observation surface of the sample is not corroded, but is observed as is with a scanning electron microscope (SEM), a photograph is taken, and multiple fields of view are observed at 200x magnification to obtain a total observation area of approximately 50 mm2. 2 It was calculated as:
[0049] In-based inclusions have a larger atomic weight than iron, so they are observed as a bright contrast in the backscattered electron image. Therefore, they are identified based on the contrast in the backscattered electron image. When Bi, Pb, and Te are contained in the steel, metallic Bi, metallic Pb, and Te compounds may be present, and these are also observed as a bright contrast in the backscattered electron image, so it may be difficult to distinguish them from In-based inclusions. In such cases, energy dispersive X-ray analysis (EDS) is used to identify the In-based inclusions.
[0050] Next, an image analyzer is used to calculate the circle-equivalent diameter of the In-based inclusions identified by the above-mentioned method. The circle-equivalent diameter refers to the diameter of a circle having an area equal to the projected area of the measured particle, and is specifically calculated by the following formula. Equivalent circle diameter = 2 × {(area of the particle) ÷ π} 1 / 2
[0051] The hardness of the steel of the present invention, i.e., the hardness before cutting the steel of the present invention as a work material, is preferably in the range of 120HV to 320HV. If the hardness of the steel before cutting is less than 120HV, the strength required for use without heat treatment after cutting is insufficient, while if it exceeds 320HV, the machinability decreases. The hardness is Vickers hardness, and it is recommended to measure the hardness at the cross section at the position where cutting is performed or at a cross section at a position having the same hardness as that position, in accordance with JIS Z 2244:2009, with a measurement load of 10 kg. However, if the measurement is performed at a position too close to the surface, there is a possibility that appropriate measurement cannot be performed. In the measurement, the hardness is measured at a position 0.5 mm or more away from the surface of the steel on the cross section.
[0052] It is generally known that the machinability of steel, which is a workpiece, decreases when the structure contains bainite or martensite. Therefore, the structure of the steel of the present invention before cutting as a workpiece may be a mixed structure of ferrite and pearlite or a pearlite structure. However, the effect of the present invention is not affected by the structure and can be obtained with any structure. For example, even if the structure is tempered martensite, the effect of the present invention can be enjoyed without being hindered. After quenching and tempering Machine structure rod In the case of steel, the structure is mainly tempered martensite, specifically, 90% or more of the area ratio in the cross section is tempered martensite.The hardness is preferably 250HV (measurement load 10kg) or more.
[0053] [Manufacturing method] The present invention Machine structure rod The method of manufacturing the steel will be described. Molten steel having the above-mentioned composition is melted by a conventional melting method such as a converter, and formed into a steel material such as a slab by a conventional casting method such as a continuous casting method. The steel material is then heated and subjected to conventional hot working such as hot rolling or hot forging to form a desired shape, thereby producing the steel of the present invention. Machine structure rod The steel can be manufactured by the cutting process. However, it is preferable to adjust the manufacturing conditions so that the hardness of the steel of the present invention is adjusted to the range of 120 to 320 HV. For example, in order to adjust the hardness to this preferred range, the steel may be subjected to a heat treatment such as annealing or spheroidizing annealing before the cutting process.
[0054] [Invention Machine structure rod Steel cutting method The steel of the present invention is particularly effective under cutting conditions with a relatively high cutting speed, specifically, a cutting speed of 60 m / min or more, but the cutting speed is not limited in the cutting method of the steel of the present invention. The cutting method can be performed with various tools such as drills, lathes, gear cutters, end mills, milling cutters, taps, etc., and any of these cutting tools may be used. In addition, cutting tools include high speed steels, cemented carbide, cermets, and those with ceramic coatings by chemical vapor deposition (CVD) or physical vapor deposition (PVD), but the type of these tool materials is not limited in the cutting process of the present invention.
[0055] Furthermore, as a lubrication method, wet, dry, semi-dry, such as MQL (Minimum Quantity Lubrication), and the like are known, but the effects of the present invention are not limited to these lubrication methods. Note that MQL is a method in which the amount of lubricant (cutting oil) is 200 cm per hour. 3 However, in actual steel processing, the amount of lubricant is about 50 cm per hour. 3 The lubricant is generally applied by mixing the lubricant with air and spraying it in mist form. In some cases, mist water may also be mixed in. EXAMPLES
[0056] Next, an example will be described, but the conditions in the example are merely an example of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to this example of conditions. Various conditions can be adopted in the present invention as long as the object is achieved without departing from the gist of the present invention.
[0057] After the steel having the composition shown in Table 1 (Tables 1-1 to 1-3 are collectively referred to as Table 1), was melted, the steel billets were hot forged into two shapes: a square steel bar with a cross-sectional size of 60 mm x 60 mm, and a round steel bar with a diameter of 50 mm. The forged steel bars were held at 1100°C for 1 hour, and then subjected to a heating and cooling treatment in which they were air-cooled. Note that "REM" in the composition shown in Table 1 is the total content of La, Ce, and Nd.
[0058] A square steel bar was cut in a cross section perpendicular to the length direction, and a sample was cut out so that a position 15 mm away from the center in the width direction and 15 mm away in the thickness direction (hereinafter referred to as the "middle position") on the obtained square cross section could be observed, embedded in resin, polished, and the Vickers hardness at the same position was measured in accordance with JIS Z 2244:2009. The measurement was performed with a load of 10 kg. In addition, a sample was cut out in the same manner, and after nital etching, the structure of the middle position of the cross section of the sample was observed with an optical microscope.
[0059] Further, samples of a predetermined size were obtained from the above square steel bar by cutting, and the amount of insol. Al contained in the samples was measured by the above-mentioned method.
[0060] The results of the hardness measurements are shown in Table 2 (Tables 2-1 to 2-3 are collectively referred to as Table 2) as "hardness before cutting." In the table, "hardness before cutting" refers to the average value of three hardness measurements performed at the above-mentioned intermediate position. "Ferrite-pearlite" in Table 2 means a mixed structure of ferrite and pearlite, and "pearlite" means a single-phase pearlite structure. The structure of the steel material before cutting used in this example was a mixed structure of ferrite and pearlite, or a single-phase pearlite structure.
[0061] Number density (pieces / mm 2 The number density of In-based inclusions was measured by cutting a cross section (longitudinal cross section) including the axial direction from the square bar at a depth of 15 mm and measuring the total area to be inspected to 50 mm 2 The samples were collected and the temperature was measured by the above method.
[0062] The observation surface of the sample was not corroded, but was observed as it was with a scanning electron microscope (SEM), photographs were taken, In-based inclusions were identified from the photographs, and the number of In-based inclusions with a circle equivalent diameter of 2.0 μm or more was counted using an image analyzer. 2 ) divided by the number density (pieces / mm 2 ) was decided.
[0063] Next, a cutting test was carried out on the steel bar. Specifically, a square test piece of 50 x 50 x 115 mm cut out from the square steel bar after the heating and cooling treatment was subjected to cutting under the following conditions using a carbide-coated drill with an oil hole having a diameter of 4.98 mm, a total length of 170 mm, and a cutting edge length of 124 mm.
[0064] Circumferential speed: 90m / min Feed: 0.15mm / rev Hole depth: 100mm Lubrication conditions: MQL (highly biodegradable synthetic ester) approximately 1.0 cm 3 / hour) Internal oil supply via drill oil hole
[0065] Before the cutting test, a guide hole with a diameter of 5.0 mm and a depth of 15 mm was formed in the square test piece. Therefore, the above-mentioned hole depth of 100 mm includes the depth of this guide hole. Machinability was evaluated by measuring the cutting resistance (thrust) when cutting under the above conditions. A smaller cutting resistance value indicates better machinability.
[0066] The present invention Machine structure rod Steel is assumed to be used as a component without heat treatment after cutting, and also to be used after heat treatment such as quenching and tempering. In other words, it is desirable to ensure not only the "hardness before cutting" but also the hardness when heat treatment is performed after cutting. Therefore, the hardness after quenching and tempering was investigated as follows.
[0067] A round bar test piece of Φ10×50 mm was cut out so that the part corresponding to the above-mentioned intermediate position of the square steel bar after the above-mentioned heating and cooling treatment was the center of the circular cross section, and the test piece was held at 950° C. for 30 minutes, water quenched, and then tempered by holding at 550° C. for 90 minutes. Next, a sample was cut out so that the circular cross section perpendicular to the length direction of the test piece could be observed, embedded in resin, and polished, and the Vickers hardness at the position intermediate between the center of the circle of the circular cross section and the steel surface was measured three times in accordance with JIS Z 2244:2009. The measurement was performed with a load of 10 kg. The average value is shown in Table 2 as "hardness after quenching and tempering". The present invention Machine structure rod The hardness of each steel after quenching and tempering is 250 HV or more, and it has sufficient strength characteristics for use as components.
[0068] Furthermore, hot ductility was investigated by a high temperature tensile test as follows. A Φ10×170mm tensile test piece was prepared in the longitudinal direction of the steel bar from a Φ50 round steel bar after heating and cooling treatment. The round steel bar was machined so that the midpoint between the center and the periphery of the cross section was located at the center of the circular cross section of the tensile test piece. Hot ductility was evaluated by heating to 1250°C and holding for 1 minute, then lowering the temperature to 1000°C, and holding for 1 minute after reaching 1000°C, at which point the strain rate reached 5×10 -3 A tensile test was performed at 1000 / s, and the reduction in area was evaluated. If the reduction in area was 35% or more, the hot ductility was deemed to pass ("OK"), and if it was less than 35%, it was deemed to fail ("NG").
[0069] The hardness before cutting, steel structure, cutting resistance, high-temperature tensile test results, and hardness after quenching and tempering are shown in Table 2.
[0070] In addition, cutting resistance is generally affected by hardness. In addition, in the present invention, it is necessary to ensure hot ductility. Therefore, the machinability was evaluated by comparing steel materials with the same hardness before cutting, on the premise that the hot ductility was acceptable.
[0071] Figure 5 shows the relationship between hardness (HV) before cutting and machinability (cutting resistance [N]). When comparing the Examples and Comparative Examples in Figure 5 (where the hot ductility is acceptable (OK)) at the same level of hardness before cutting, it can be seen that the Examples have lower cutting resistance than the Comparative Examples. Hereinafter, Examples whose hardness before cutting differs from the Comparative Examples whose hot ductility is acceptable within the range of ±5HV will be referred to as "hardness before cutting is about the same as that of the Comparative Examples." Moreover, the effects of containing Bi, Sn, Te and In in combination are shown in Figs. FIG. 1 shows the relationship between Bi / In and machinability (cutting resistance [N]) for steels of examples and comparative examples that contain Bi and have similar hardness before cutting, 231 to 239 HV. FIG. 2 shows the relationship between Sn / In and machinability (cutting resistance [N]) for steels of examples and comparative examples that have similar hardness before cutting, 225 to 234 HV, and contain Sn. FIG. 3 shows the relationship between In / Te and machinability (cutting resistance [N]) for steels of examples and comparative examples that have similar hardness before cutting, 232 to 239 HV, and contain Te. FIG. 4 shows the relationship between Mn / S and machinability (cutting resistance [N]) for steels of examples and comparative examples that have similar hardness before cutting, 175 to 183 HV, and contain Te.
[0072] Steels Nos. 78 and 79 had excessive In content, and therefore failed the reduction in area in the high temperature tensile test. Steel No. 80 had an excessive Bi content, and therefore failed the reduction in area in the high temperature tensile test. Steel No. 81 has an excessive Sn content and therefore fails the reduction in area in the high temperature tensile test. Steel No. 82 has an excessive Te content, and therefore fails the reduction in area in the high temperature tensile test. Since the In content of steel No. 83 is insufficient, the cutting resistance is higher than that of the example steels having the same level of hardness before cutting. No. 83 has the same level of hardness as Nos. 4, 28, 29, and 49 to 53.
[0073] The steels of Nos. 84 and 85 have a small [Bi%] / [In%] value, and therefore have a higher cutting resistance than the steels of the examples with the same level of hardness before cutting. No. 84 has the same level of hardness before cutting as Nos. 15-19, 37-40, and 63-68, and No. 85 has the same level of hardness before cutting as Nos. 12-19, 35-40, and 60-68. The steels of Nos. 86, 87 and 88 have a small [Sn%] / [In%] value, and therefore have a higher cutting resistance than the steels of the examples having the same level of hardness before cutting. No. 86 has the same hardness as Nos. 21, 22, 42, 43, 70, 71 and 75, No. 87 has the same hardness as Nos. 12-19, 34-39 and 60-67, and No. 88 has the same hardness as Nos. 10, 11, 33-35, 58 and 59. Since the values of [In%] / [Te%] are small for steels No. 89, 90 and 91, the cutting resistance is higher than that of the steels of the examples with the same level of hardness before cutting. No. 89 has the same hardness as Nos. 4-6, 28-30 and 50-54, No. 90 has the same hardness as Nos. 13-19, 36-40 and 63-68, and No. 91 has the same hardness as Nos. 12-19, 35-40 and 60-68.
[0074] The steels Nos. 92 and 93 have a small [Mn%] / [S%] value, and therefore have a higher cutting resistance than the steels of the examples with the same level of hardness before cutting. No. 92 has the same hardness as Nos. 4, 28, 29, and 49-53, and No. 93 has the same hardness as Nos. 12-19, 36-40, and 60-68. The steels Nos. 94 and 95 have a large [Mn%] / [S%] value, and therefore have a high cutting resistance compared to the steels of the examples that have the same level of hardness before cutting. No. 94 has the same hardness as Nos. 3, 48, and 49, and No. 95 has the same hardness as Nos. 17-20, 40, and 66-68.
[0075] Since the steel No. 96 has an excessive C content, it has a higher cutting resistance than the steels of the examples that have the same level of hardness before cutting. Steel No. 97 has an excessive Se content and therefore fails the reduction in area in the high temperature tensile test. Nos. 1 to 77 have a composition within the range of the present invention, and therefore have better cutting resistance and reduction of area in a high-temperature tensile test than the comparative steels having the same level of hardness before cutting.
[0076] [Table 1-1]
[0077] [Table 1-2]
[0078] [Table 1-3]
[0079] [Table 2-1]
[0080] [Table 2-2]
[0081] [Table 2-3] [Industrial Applicability]
[0082] The present invention can be widely used in all industrial fields, such as industrial machinery and transportation machinery.
Claims
1. The components are expressed as follows, by mass%: C: 0.05-0.85%, Si: 0.01-3.00%, Mn: 0.01 to 3.00%, Cr: 0.01-3.00%, P: 0.100% or less, S: 0.001-0.150%, In: 0.0003 to 0.0600%, Al: 0.002-0.050%, N: 0.0030 to 0.0250%, and O: 0.0050% or less and Bi: 0.0001-0.0950%, Sn: 0.0001 to 0.3000%, and Te: 0.0001 to 0.0300%, and the balance being Fe and impurities, At least one of the following formulas 1, 2, and 3 is satisfied: A steel bar for machine structures, characterized in that when formula 3 is satisfied, formula 4 is also satisfied. 0.010≦[Bi%] / [In%]...(Formula 1) 0.230≦[Sn%] / [In%]...(Formula 2) 0.700≦[In%] / [Te%]...(Formula 3) 22.00≦[Mn%] / [S%]≦150.00 (Formula 4) Here, [In%], [Bi%], [Sn%], [Te%] and [Mn%] represent the mass% contents of In, Bi, Sn, Te and Mn in the steel, respectively, and 0 is substituted if none is contained.
2. The steel bar for mechanical structure further comprises, in mass%, O: 0.0050% or less, and Insol. Al: 0.0060% or less The steel bar for machine structure according to claim 1, further comprising:
3. The steel bar for mechanical structure further comprises, in mass%, Ca: 0.0050% or less, Mg: 0.0050% or less, Zr: 0.0050% or less, and REM: 0.0050% or less 3. The steel bar for machine structure according to claim 1, further comprising one or more of the following:
4. The steel bar for mechanical structure further comprises, in mass%, Ti: 0.200% or less, Nb: 0.200% or less, and V: 0.500% or less The steel bar for machine structure according to any one of claims 1 to 3, characterized in that it contains one or more of the following:
5. The steel bar for mechanical structure further comprises, in mass%, Mo: 1.00% or less, Ni: 1.40% or less, Cu: 1.40% or less, and B: 0.0050% or less The steel bar for machine structure according to any one of claims 1 to 4, characterized in that it contains one or more of the following:
6. The steel bar for mechanical structure further comprises, in mass%, Sb: 0.0151% or less, Se: 0.0469% or less, Zn: 0.0009% or less, and Pb: 0.029% or less The steel bar for machine structure according to any one of claims 1 to 5, characterized in that it contains one or more of the following:
Citation Information
Patent Citations
Machine structural steel
JP1987033743A
Steel for machine structural use having good chip disposability and cutting tool life and lower anisotropy of mechanical properties
JP1993125483A
Steel for machine structure use excellent in machinability
JP1995054099A
Coin lifter
JP2002035215A
Spring steel
JP2015120940A