Mold for continuous casting and method for continuous casting of steel

The multi-stage taper and protrusion design in the continuous casting mold addresses the challenges of uneven cooling and solidification shrinkage in difficult-to-cast steels, enhancing slab quality and mold durability.

JP7560725B2Active Publication Date: 2024-10-03NIPPON STEEL CORPORATION
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020174540
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-16
Publication Date
2024-10-03
Estimated Expiration
2040-10-16

AI Technical Summary

Technical Problem

In continuous casting of steel, particularly difficult-to-cast steels like peritectic steels, the solidification shrinkage of the solidified shell is large due to phase transformation, leading to issues such as uneven cooling, bulging, and sharp corner formation, which can result in cracks, scale accumulation, and reduced mold life.

Method used

A continuous casting mold with a multi-stage taper design, featuring a strongly tapered uppermost part and protrusions at the corners, with specific taper ratios and distances to ensure uniform heat removal and reduce frictional forces, preventing cracks and bulging.

Benefits of technology

The mold design improves the shape and quality of the cast slabs by reducing corner cracks, preventing bulging, and extending mold life while maintaining uniform solidification and reducing operational issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560725000007
    Figure 0007560725000007
  • Figure 0007560725000008
    Figure 0007560725000008
  • Figure 0007560725000009
    Figure 0007560725000009
Patent Text Reader

Abstract

To secure solidification uniformity in molten steel and suppress corner cracking in a cast slab.SOLUTION: A mold for continuous casting to be used in a continuous casting facility where steel is continuously casted includes: a pair of long side copper plates; and a pair of short side copper plates that is held between the pair of long side copper plates, and that is movable along a long side direction of the long side copper plates. The short side copper plate has: two or more gradients differing in a casting direction so that a plurality of tapered parts is formed on an internal surface side of the mold to be supplied with molten steel; and protrusions extending in the casting direction, at both ends in a short side direction on the internal surface side. A tapering rate of the tapered parts at the uppermost stream side in the casting direction is 1.1% / m-3.5% / m. In a plan view of the mold, the protrusion is formed such that a length of a contact part contacting the molten steel is shorter than a sum of a short side direction length and a long side direction length of the mold, and a difference thereof is 3 mm or more.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a continuous casting mold used in a continuous casting facility for continuously casting steel, and a method for continuously casting steel using the same. [Background technology]

[0002] In continuous casting of molten steel, when molten steel is poured into a mold, the part of the molten steel in contact with the mold solidifies to form a solidified shell, which is then pulled out below the mold. The solidification of the molten steel progresses further in the secondary cooling zone below the mold, and finally a continuously cast slab is formed. The side of the mold that comes into contact with the molten steel is made of water-cooled copper plates. The continuous casting mold of a continuous casting device that casts slabs is made using two long-side copper plates and two short-side copper plates, and is assembled so that the two short-side copper plates are sandwiched between the two long-side mold plates. The width of the short-side copper plates is approximately equal to the thickness of the slab to be cast.

[0003] In the process in which the solidifying shell moves downward in the mold, the solidifying shell solidifies and shrinks as the solidification progresses. Therefore, the solidified shell, which starts solidifying at the meniscus position of the molten metal in the mold, shrinks when it reaches the lower end of the mold, and the width and thickness of the solidifying slab are smaller than those at the meniscus position. In continuous casting of slabs, since the width of the slab is wider than the thickness, the amount of solidification shrinkage in the width direction of the slab is large, and a gap is likely to occur between the mold and the solidified shell. If a gap occurs between the mold and the solidified shell below the mold due to the solidification and shrinkage of the solidified shell, heat transfer from the solidified shell to the mold is hindered, the mold cannot be sufficiently cooled, and the solidified shell, which loses support from the mold, expands outward, causing bulging.

[0004] Therefore, at least the short sides of the mold are tapered. By tapering, we mean narrowing the distance between the opposing short sides at the bottom of the mold compared to the distance at the meniscus position above the mold.

[0005] If the taper amount of the narrow side is too small, the contact between the solidified shell and the narrow side mold plate becomes uneven, causing imbalance in cooling. As a result, internal cracks due to uneven growth of the solidified shell and vertical cracks are likely to occur on the surface of the slab corresponding to the part where the solidified thickness is particularly thin near the corner of the solidified shell on the long side. If the taper amount of the narrow side is too large, the contact between the solidified shell and the narrow side copper plate becomes strong, and excessive stress is applied to the solidified shell. As a result, the solidified shell breaks, and breakout occurs due to shell breakage. In addition, the increased friction between the solidified shell and the mold may cause a shortened mold life.

[0006] The surface of the conventional copper plate on the narrow side that contacts the solidified shell is processed to be flat from the top to the bottom. It is a so-called single taper. However, the solidification shrinkage speed of the solidified shell is not constant at each position in the casting direction in the mold, and is fast near the meniscus and slows down as it approaches the bottom end of the mold. Therefore, it is considered that the surface of the solidified shell that contacts the copper plate on the narrow side is not flat, but is curved such that the taper amount of the solidified shell decreases toward the bottom of the mold. For example, Patent Documents 1 and 2 disclose a method of casting using a mold in which the copper plate on the narrow side has a multi-stage taper with two or more stages in the casting direction. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2008-49385 A [Patent Document 2] JP 2009-160645 A [Patent Document 3] Patent No. 5999294 Summary of the Invention [Problem to be solved by the invention]

[0008] Here, in the case of difficult-to-cast steels such as peritectic steels that undergo δ-γ transformation during solidification, the solidification shrinkage of the solidified shell is large due to the phase transformation during solidification. For this reason, it is required to strongly taper the topmost taper of the multi-stage taper of the mold so that it can follow the solidification shrinkage. However, it was found that if the topmost taper of the mold in which the short-side copper plate is formed with multiple tapers is further strongly tapered during casting, the corner shape of the slab becomes sharp. Figure 6 shows examples of the cross-sectional shapes of slabs cast using two types of mold shapes.

[0009] First, in typical continuous casting using a mold with right-angled mold corners and a taper rate of the narrow copper plate of 1.0% / m or less, molten steel is removed from both the long and short sides near the corners between the long and short copper plates. As a result, solidification proceeds faster near the corners than in the width centers of the long and short copper plates, causing the corners to solidify and shrink. Meanwhile, bulging occurs in the width center due to the static pressure of the molten steel, causing deformation that causes the slab to bulge outward. As a result, the slab bulges outward toward the width center, as shown in slab shape A in Figure 6, and the corners, where solidification shrinkage is greater, have a slightly pointed shape.

[0010] In addition, in a mold having right-angled corners and multiple tapers, if the top taper is made a strong taper with a taper rate of 1.1% / m or more in the short side copper plate in order to reduce the air gap between the slab and the mold, this will promote heat removal from the mold and slab near the corners, and the corners of the slab will become sharper than those of slab shape A, as shown in slab shape B in Figure 6.

[0011] When the corners of a slab are sharpened in this way, scale tends to accumulate in the recesses of the off-corner parts, increasing the possibility of scratches occurring during rolling. For this reason, there is a need for a technology that can improve the shape of the slab while making the topmost tapered part more strongly tapered.

[0012] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a continuous casting mold and a continuous casting method for steel that are capable of improving the shape of a cast slab while making the uppermost tapered portion strongly tapered. [Means for solving the problem]

[0013] In order to solve the above problems, according to one aspect of the present invention, there is provided a continuous casting mold for use in continuous casting equipment for continuously casting steel, the mold comprising a pair of long-side copper plates and a pair of short-side copper plates that are sandwiched between the pair of long-side copper plates and can move along the long-side direction of the long-side copper plates, the short-side copper plates having two or more different gradients in the casting direction so that multiple tapered portions are formed on the inner surface side of the mold to which molten steel is supplied, the short-side copper plates have protrusions extending in the casting direction at both ends in the short-side direction on the inner surface side, the taper rate of the tapered portion on the most upstream side in the casting direction is 1.1% / m or more and 3.5% / m or less, and the protrusions are formed so that, when the mold is viewed in a plane, the length of the contact portion that comes into contact with molten steel is shorter than the sum of the short-side and long-side lengths of the mold, and the difference is 3 mm or more.

[0014] The distance in the casting direction from the average position of the meniscus to the first taper change point of the copper plate on the narrow side may be 50 mm or more and 300 mm or less.

[0015] The taper rate of the tapered portion on the most downstream side in the casting direction may be 0.5% / m or more and less than 1.9% / m, and may be equal to or less than the taper rate of the tapered portion on the upstream side.

[0016] The mold may be formed to have two tapers.

[0017] In addition, in order to solve the above-mentioned problems, according to another aspect of the present invention, there is provided a method for continuously casting steel, which comprises a pair of long-side copper plates and a pair of short-side copper plates that are sandwiched between the pair of long-side copper plates and can move along the long-side direction of the long-side copper plates, and the short-side copper plates have two or more different gradients in the casting direction so that a plurality of tapered portions are formed on the inner surface side of the mold to which molten steel is supplied, and the short-side copper plates have protrusions extending in the casting direction at both end portions in the short-side direction on the inner surface side, the taper rate of the tapered portion on the most upstream side in the casting direction being 1.1% / m or more and 3.5% / m or less, and the protrusions are formed so that, when the mold is viewed in plan, the length of the contact portion that comes into contact with molten steel is shorter than the sum of the lengths of the mold in the short-side direction and the long-side direction, and the difference is 3 mm or more. Effect of the Invention

[0018] As described above, according to the present invention, the uppermost tapered portion can be strongly tapered, and the shape of the cast slab can be improved. [Brief description of the drawings]

[0019] [Figure 1] 1 is an explanatory diagram showing a schematic configuration of a continuous casting facility according to an embodiment of the present invention. FIG. [Diagram 2] FIG. 4 is a schematic cross-sectional view showing the shape of a mold according to the embodiment. [Figure 3A] FIG. 2 is a schematic diagram showing the shape of a mold when the corner portion is a right-angle corner. [Figure 3B] FIG. 2 is a schematic diagram showing an example of a shape of a corner portion of a mold. [Figure 3C] 10A to 10C are schematic diagrams showing other examples of the shape of the corner portion of the mold. [Figure 3D] 10A to 10C are schematic diagrams showing other examples of the shape of the corner portion of the mold. [Figure 3E] 10A to 10C are schematic diagrams showing other examples of the shape of the corner portion of the mold. [Figure 4] FIG. 2 is a schematic diagram showing examples of cross-sectional shapes of slabs cast using a mold with right-angled corners (without a protrusion) and a mold with a protrusion formed therein. [Diagram 5] 3 is a cross-sectional view taken along line II in FIG. 2. [Figure 6] FIG. 2 is a schematic diagram showing examples of cross-sectional shapes of slabs cast using molds of two different shapes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are designated by the same reference numerals, and duplicated explanations will be omitted.

[0021] [1. Configuration of continuous casting equipment] First, a schematic configuration of a continuous casting facility equipped with a mold according to one embodiment of the present invention will be described with reference to Figures 1 and 2. Figure 1 is an explanatory diagram showing a schematic configuration of a continuous casting facility 1 according to this embodiment. Figure 2 is a schematic cross-sectional view showing the shape of a mold 10 according to this embodiment. Note that Figure 2 shows the mold 10 cut at an arbitrary position in the casting direction (vertical direction).

[0022] The continuous casting equipment 1 according to this embodiment is an equipment for continuously casting molten steel 2 using a mold 10 for continuous casting to produce a cast piece 3. The continuous casting equipment 1 shown in Fig. 1 is a vertical bending type continuous casting equipment 1, but the present invention is not limited to this example and is applicable to various other types of continuous casting equipment such as a curved type or a vertical type. The continuous casting equipment 1 includes the mold 10, a ladle 4, a tundish 5, a submerged nozzle 6, and a secondary cooling device 7.

[0023] The ladle 4 is a movable container for transporting the molten steel 2 from the outside to the tundish 5. The ladle 4 is disposed above the tundish 5, and the molten steel 2 in the ladle 4 is supplied to the tundish 5. The tundish 5 is disposed above the mold 10, and stores the molten steel 2 therein, and removes inclusions in the molten steel 2. The submerged nozzle 6 extends downward from the lower end of the tundish 5 toward the mold 10, and its tip is immersed in the molten steel 2 in the mold 10. The submerged nozzle 6 continuously supplies the molten steel 2 from which inclusions have been removed in the tundish 5, into the mold 10.

[0024] The mold 10 is a rectangular cylindrical mold formed according to the width and thickness of the slab 3. As shown in FIG. 2, the mold 10 according to this embodiment is assembled using a pair of short-side copper plates 11 and a pair of long-side copper plates 13, with the pair of short-side copper plates 11 sandwiched from both sides in the short-side direction (X direction) by the inner surfaces 13a of the pair of long-side copper plates 13. The pair of short-side copper plates 11 are configured to be movable along the long-side direction (Y direction) of the long-side copper plates 13. That is, the mold 10 according to this embodiment is a mold with variable width. The shape of the mold 10 will be described in detail later.

[0025] The copper plates 11 and 13 constituting the mold 10 are, for example, water-cooled copper plates. The molten steel 2 in contact with the inner surfaces 11a and 13a of the copper plates 11 and 13 is cooled to produce a slab 3 including a liquid portion 3b inside a solidified shell 3a. As the solidified shell 3a moves downward in the mold 10, the solidification of the liquid portion 3b inside proceeds, and the thickness of the solidified shell 3a gradually increases. The slab 3 including the solidified shell 3a and the liquid portion 3b is pulled out from the lower end of the mold 10.

[0026] The secondary cooling device 7 is provided in a secondary cooling zone 9 below the mold 10, and cools the slab 3 pulled out from the lower end of the mold 10 while supporting and transporting it. The secondary cooling device 7 has multiple pairs of support rolls 8 arranged on both sides of the slab 3 in the thickness direction, and multiple spray nozzles (not shown) that spray cooling water onto the slab 3. The support rolls 8 provided in the secondary cooling device 7 are arranged in pairs on both sides of the slab 3 in the thickness direction, and function as a support transport means that supports and transports the slab 3. Supporting the slab 3 from both sides in the thickness direction with the support rolls 8 can prevent breakout and bulging of the slab 3 during solidification in the secondary cooling zone 9.

[0027] The support rolls 8 form a transport path (pass line) for the slab 3 in the secondary cooling zone 9. As shown in Fig. 1, this pass line is vertical immediately below the mold 10 (vertical zone 9A), then curves in a curved shape (curved zone 9B), and finally becomes horizontal (horizontal zone 9C). The support rolls 8 are composed of a support roll provided in the vertical zone 9A for supporting the slab 3 immediately after it has been pulled out of the mold 10, a pinch roll which is a driven roll for pulling the slab 3 out of the mold 10, and segment rolls provided in the curved zone 9B and horizontal zone 9C for supporting and guiding the slab 3 along the pass line.

[0028] The slab 3 that has passed through the secondary cooling zone 9 is then cut to a predetermined length by a slab cutter (not shown) installed downstream of the horizontal zone 9C. The cut slab 3 moves on a table roll and is transported to the equipment for the next process. The overall configuration of the continuous casting equipment 1 has been described above.

[0029] [2. Mold shape] [2-1. Overview] In this embodiment, in the mold 10 of the continuous casting equipment 1, in order to improve the shape of the cast slab while making the uppermost taper portion strongly tapered, a protrusion protruding toward the space inside the mold is formed on the inner surface 11a of the short side copper plate 11 at the mold corner. The protrusion refers to a portion where the short side copper plate 11 is deformed to fill the right-angle corner of the mold 10.

[0030] Here, Fig. 3A shows the shape of the corners of the mold 10 when they are right-angled corners. Also, Figs. 3B to 3E show examples of the shapes of the corners of the mold 10 according to this embodiment. Note that Figs. 3A to 3E show one of the four corners of the mold 10. The shape of the protrusions 12 may be the same for all four corners, or may include different shapes for the four corners in accordance with requirements for subsequent processes.

[0031] For example, as shown in FIG. 3B, the protrusion 12 may be formed so that the right-angle corner is filled by a straight line 12a connecting the short-side copper plate 11 and the long-side copper plate 13 when the mold 10 is viewed from above. The triangular chamfered shape shown in FIG. 3B is also called a chamfer shape. Alternatively, as shown in FIG. 3C, the protrusion 12 may be formed so that the right-angle corner is filled by a circular arc 12b connecting the short-side copper plate 11 and the long-side copper plate 13 when the mold 10 is viewed from above. In other words, the protrusion 12 may be R-shaped.

[0032] 3D, the protrusion 12 may be formed so that the right-angle corner is filled by two circular arcs 12c and 12d when the mold 10 is viewed from above. In this case, the circular arc 12c in contact with the long-side copper plate 13 may be formed so as to be convex toward the inside of the mold 10 and to be in contact with the long-side copper plate 13 at an angle as close to perpendicular as possible. The circular arc 12d in contact with the short-side copper plate 11 may be formed so as to be convex toward the corner side of the mold 10 and to be in contact with the short-side copper plate 11 at an angle as small as possible.

[0033] 3E, the protrusion 12 may be formed so as to fill the right-angle corner with two arcs 12e, 12g and one straight line 12f connecting the two arcs 12e, 12g when the mold 10 is viewed from above. In this case, as in FIG. 3D, the arc 12e in contact with the long-side copper plate 13 may be formed so as to be convex toward the inside of the mold 10 and to be in contact with the long-side copper plate 13 at an angle as close to perpendicular as possible. The arc 12g in contact with the short-side copper plate 11 may be formed so as to be convex toward the corner side of the mold 10 and to be in contact with the short-side copper plate 11 at an angle as small as possible.

[0034] The shape of the corners of the mold 10 as shown in FIGS. 3D and 3E is easy to process and can suppress deformation at the corners.

[0035] By using a mold 10 having a protrusion as shown in FIG. 3B to FIG. 3E, a bevel having a chamfered edge can be continuously cast. FIG. 4 shows examples of cross-sectional shapes of slabs cast using the mold with a right-angled corner (without a protrusion) shown in FIG. 3A and the mold with a circular arc-shaped protrusion shown in FIG. 3C. As shown in FIG. 4, the corners of the slab cast using the mold with a right-angled corner were sharpened. On the other hand, the corners of the slab cast using the mold with a protrusion were chamfered because the corner shape of the mold was transferred to the slab. It was confirmed that the sharpening of the corners of the slab was eliminated by forming a protrusion 12 on the inner surface 11a of the short-side copper plate 11 at the mold corner.

[0036] On the other hand, when casting a slab with chamfered corners, providing a protrusion at the corner of the mold reduces the contact length between the molten steel and the copper plate compared to when the corner is right-angled, and reduces the amount of heat dissipation at the corner of the mold. Therefore, the surface temperature of the corner of the slab increases. When a protrusion is provided at the corner of the mold, the shell thickness decreases compared to when the mold has right-angled corners due to the reduced amount of heat dissipation.

[0037] In addition, in the early stage of solidification, when the mold has right-angle corners, gaps occur mainly near the short sides of the corners, but when a protrusion is provided at the corners, gaps occur at the protrusion itself and near the short sides of the corners consisting of the protrusion and the short side copper plate surface. In other words, when a protrusion is provided at the corner of the mold, the area where gaps occur is larger than in the case of right-angle corners.

[0038] For this reason, the heat transfer from the solidified shell to the mold is hindered, and the solidified shell cannot be sufficiently cooled. This is not limited to the case where a triangular protrusion is provided at the corner, but also applies to the case where a protrusion is provided at the corner of the mold as shown in Figures 3C to 3E, in which the contact length between the molten steel and the copper plate is reduced compared to the case where the mold has a right-angle corner. Regarding this, as described above, by making the tapered portion of the copper plate on the short side strongly tapered, it is possible to promote the heat transfer from the mold and the cast piece near the corner. Therefore, for a multi-stage tapered mold, by making the tapered portion of the top stage strongly tapered and providing a protrusion inside the mold, it is possible to exhibit the functions of each shape.

[0039] Furthermore, by using a mold with a protrusion inside, the surface temperature of the slab cast using such a mold is higher than that of a slab cast using a mold with right-angle corners, and corner cracks on the surface of the slab can be prevented. This is due to the following mechanism.

[0040] The molten steel poured into the mold is removed from the long side and the short side at the corners of the mold. Therefore, due to the effect of two-sided cooling, the corners of the mold have a larger amount of heat removal than the center of the width of the long side copper plate, and the surface temperature drops. In the secondary cooling zone after leaving the mold, the temperature of the center of the long side width of the slab is about 900°C, but the temperature of the corners of the slab may be 800°C or lower. When the temperature of the corners of the slab is 800°C or lower, cracks occur in the corners. This is because the slab is bent in the continuous casting machine in a temperature range where ductility is lost, called the embrittlement region, and tensile stress acts on the slab. Therefore, the effect of two-sided cooling is suppressed by providing protruding parts rather than making the corners of the mold at right angles (for example, Patent Document 3). This makes it possible to make the temperature of the corners of the slab in the secondary cooling zone the same as that of the center of the long side width (i.e., 800°C or higher). As a result, the corners are not overcooled as compared with the central portion of the long side width, and corner cracks in the slab can be reduced.

[0041] Continuous casting using a mold in which the topmost taper is strongly tapered and a protrusion is provided inside the mold is also effective for hard-to-cast steels such as peritectic steels, which have a large solidification shrinkage of the solidified shell due to phase transformation during solidification. By using a mold with such a shape, it is possible to prevent the occurrence of vertical cracks, corner cracks, and internal cracks on the surface of the slab, improve the cross-sectional shape of the slab, and prevent scratches during rolling, thereby improving the quality of the slab during continuous casting of hard-to-cast steels.

[0042] [2-2.Basic configuration] The shape of the mold 10 according to this embodiment will be described with reference to Fig. 2 and Fig. 5. Fig. 5 is a cross-sectional view taken along line II in Fig. 2. In Fig. 2 and Fig. 5, the shape of the mold 10 is exaggerated in order to easily explain the configuration of the mold 10.

[0043] As described above, the mold 10 according to this embodiment is composed of a pair of short-side copper plates 11 and a pair of long-side copper plates 13. When the mold 10 is viewed from above in the height direction, as shown in FIG. 2, a substantially rectangular space (corresponding to the "rectangular space" of the present invention) V is formed in the mold 10 by the pair of short-side copper plates 11 and the pair of long-side copper plates 13. The inner surface 11a of the short-side copper plate 11 of the mold 10 according to this embodiment is provided with protrusions 12 that protrude into the space V at both ends in the short side direction. The protrusions 12 extend along the height direction of the mold 10 (also called the Z direction or casting direction).

[0044] Here, the short side copper plate 11 has two or more different gradients in the casting direction so that the mold 10 has a plurality of tapered portions and is a multi-stage taper. The multi-stage taper is formed so that the gradient (i.e., the taper rate) becomes smaller toward the downstream side in the casting direction. In the initial solidification stage of the upper stage of the mold 10 (i.e., the upstream side in the casting direction), the thickness of the solidified shell is thin and heat is removed from the molten steel in large amounts, so the solidification shrinkage of the solidified shell is large. For this reason, it is necessary to make the gradient of the taper relatively large. On the other hand, at the lower end of the mold 10 (i.e., the most downstream side in the casting direction), the solidified shell is thick because it has grown, and heat removal from the molten steel is small compared to the upper stage of the mold. For this reason, the solidification shrinkage of the solidified shell is small, and the gradient of the taper is relatively small. Due to this mechanism, the gradient of the tapered portion in the upper stage of the mold 10 is made large, and the gradient of the tapered portion is set to gradually decrease toward the downstream side in the casting direction where solidification progresses.

[0045] If the gradient of the tapered portion of the upper stage of the mold 10, called a reverse taper, is made small and the gradient of the tapered portion is gradually increased toward the downstream side in the casting direction, the following problems are considered to occur. First, in the upper stage of the mold 10, the gradient of the tapered portion is small despite the large solidification shrinkage of the solidified shell, so that the air gap at the corner cannot be sufficiently reduced. This causes internal cracks and reduces the internal quality of the slab. On the other hand, in the lower end of the mold 10, the gradient of the tapered portion is large despite the small solidification shrinkage of the solidified shell, so that the slab and the mold come into strong contact with each other, generating a large frictional force. The mold copper plate wears due to the constraint by the mold, reducing the mold life, reducing productivity, and there is also a concern of the occurrence of breakouts, in which the slab breaks. Therefore, the multi-stage taper is formed so that the gradient becomes smaller toward the downstream side in the casting direction.

[0046] For example, the mold 10 shown in Figures 2 and 5 has a two-stage taper because the short-side copper plate 11 has two different gradients θ1 and θ2. In Figures 2 and 5, the inner surface 11a of the short-side copper plate 11 that forms the taper on the most upstream side (i.e., upward) in the casting direction is referred to as the first inclined surface 11a1, and the inner surface 11a of the short-side copper plate 11 that forms the taper on the most downstream side (i.e., downward) in the casting direction is referred to as the second inclined surface 11a2. In addition, in the mold 10, the taper formed by the first inclined surface 11a1 is referred to as the first taper portion T1, and the taper formed by the second inclined surface 11a2 is referred to as the second taper portion T2.

[0047] At this time, the taper ratio R of the taper portion on the most upstream side in the casting direction (i.e., the first taper portion T1) is set to 1.1% / m or more and 3.5% / m or less. The taper ratio R [% / m] is expressed by the following formula (1).

[0048] R = {(W T -W B ) / W V / ΔL}×100 (1)

[0049] In the above formula (1), W T [m] is the distance between the opposing short-side copper plates 11 at the upper position, W B [m] is the distance between the opposing short-side copper plates 11 at the lower position, W V [m] is the distance between the opposing short side copper plates 11 at any position in the casting direction (hereinafter, also referred to as the "reference distance"), and ΔL [m] is the length in the casting direction between the upper position and the lower position. T and the spacing W at the lower position B may be any distance between the upper and lower positions in the casting direction in a tapered portion having the same gradient, and the positions in the casting direction may be selected arbitrarily.

[0050] For example, in the first taper portion T1, the interval W T The distance W0 at the upper end of the mold 10 is set as the distance W Bmay be the interval W1 at the lower end of the first taper portion T1. In this case, ΔL is the length X1 of the first taper portion T1 in the casting direction. Similarly, in the second taper portion T2, the interval W T is the distance W1 at the upper end of the second taper portion T2, and the distance W B may be the interval W2 at the lower end of the mold 10. In this case, ΔL is the length X2 of the second tapered portion T2 in the casting direction. Here, the reference interval W V is the distance W between the short side copper plates 11 at the average position of the meniscus M It was decided.

[0051] If the taper rate of the first taper portion T1 is less than 1.1% / m, a gap will be generated between the mold 10 and the slab at the corners of the mold 10, hindering the growth of the solidified shell. This will result in a thinner solidified shell near the corners of the slab, and after it leaves the mold 10, bulging will occur in the slab due to the static pressure of the molten steel, generating tensile stress. In this case, since the thin portion of the solidified shell has low strength, it may cause internal cracks and affect product quality. Therefore, the taper rate of the first taper portion T1 is set to 1.1% / m or more.

[0052] On the other hand, if the taper of the top stage is larger than 3.5% / m, the mold 10 and the cast piece come into strong contact with each other. This causes a large frictional restraint force to act on the solidified shell, which may cause the solidified shell to break. If the solidified shell breaks, a breakout occurs in which unsolidified molten steel flows out to the outside. For this reason, the taper rate of the first taper portion T1 is set to 3.5% / m or less.

[0053] Table 1 shows the results of investigating the taper ratio of the tapered portion on the most upstream side in the casting direction and the occurrence of internal cracks and breakouts in the slab. Table 1 shows the results of investigating the occurrence of internal cracks and breakouts in the slab when the taper ratio of the tapered portion on the most upstream side in the casting direction (i.e., the first tapered portion T1) is changed when a slab with a slab width of 1250 to 2300 mm and a slab thickness of 200 to 400 mm is cast using the continuous casting equipment shown in Figures 1, 2, and 5. The shape of the protruding portion 12 of the mold 10 is such that, when the mold 10 is viewed from above, the length C of the contact portion that comes into contact with the molten steel is 36 mm, and the length C of the mold 10 in the short side direction is 20 mm. X 30 mm, and the length C of the long side of the mold 10 Y The shape of the triangle is 20 mm.

[0054] [Table 1]

[0055] From the results in Table 1, it can be seen that in order to prevent internal cracks and breakouts from occurring in the slab, the taper ratio of the taper section on the most upstream side in the casting direction should be 1.1% / m or more and 3.5% / m or less. The taper ratios in Table 1 were calculated using the above formula (1). At this time, the standard interval W V is the distance W between the short side copper plates 11 at the average position of the meniscus M It was decided.

[0056] Furthermore, the mold 10 according to this embodiment is provided with protruding portions 12. Providing the protruding portions 12 can prevent the phenomenon in which the corners of the slab are overcooled compared to the central portion of the long side width. The shape of the protruding portions 12 may be triangular when the mold 10 is viewed from above, as shown in Figs. 2 and 3B. However, the present invention is not limited to such an example, and the protruding portions 12 may have other shapes, as shown in Figs. 3C to 3E. The length C of the contact portion of the protruding portions 12 that comes into contact with the molten steel when the mold 10 is viewed from above is longer than the length C of the mold 10 in the short side direction. X and the length of the long side C Yand the difference is 3 mm or more. That is, the length C of the contact portion of one protrusion 12 satisfies the following formula (2).

[0057] 3[mm]≦{(C X +C Y )-C} (2)

[0058] For example, the length C1 of the straight line 12a of the protrusion 12 shown in FIG. 3B and the length C1 of the arc 12b of the protrusion 12 shown in FIG. 3C are the length C of the contact portion in contact with the molten steel (C=C1). In addition, in the protrusion 12 shown in FIG. 3D, the length C of the contact portion in contact with the molten steel is expressed by the sum of the length C1 of the arc 12c and the length C2 of the arc 12d (C=C1+C2). In addition, in the protrusion 12 shown in FIG. 3E, the length C of the contact portion in contact with the molten steel is expressed by the sum of the length C1 of the arc 12e, the length C2 of the arc 12g, and the length C3 of the straight line 12f (C=C1+C2+C3). When the length C of the contact portion of one protrusion 12 is expressed in this way, each of the four protrusions 12 at the corners of the mold 10 is formed to satisfy the above formula (2).

[0059] The relationship of the above formula (2) is the length C of the contact part in contact with the molten steel and the length C of the mold 10 in the short side direction. X and length C in the long side direction Y The result is based on the results of a solidification analysis using a numerical simulation in which the sum of the length C of the contact portion is changed. X and length C in the long side direction Y and the difference ΔC(=(C X +C Y When the length C of the contact portion in contact with the molten steel is less than 3 mm, the surface temperature of the corner portion does not increase, and the effect of the protrusion 12 is not exhibited. X and length C in the long side direction Y and the difference ΔC must be 3 mm or more.

[0060] When the difference ΔC was 3 mm or more, the corner surface temperature gradually increased, but when it exceeded 20 mm, the increase in the corner surface temperature was saturated even if the difference ΔC was further increased. On the other hand, when the casting cross section is narrowed, the yield rate decreases (i.e., productivity deteriorates). Therefore, the difference ΔC (=(C X +C Y )-C) may be 20 mm or less.

[0061] Here, Table 2 shows the length C of the contact part in contact with the molten steel and the length C of the mold 10 in the short side direction. X and length C in the long side direction Y The difference between the sum of ΔC(=(C X +C Y )-C) were changed. Table 2 shows the results of investigating the quality of the slab when the shape of the protruding portion 12 of the mold used in casting a slab with a width of 1250 to 2300 mm and a thickness of 200 to 400 mm was changed using the continuous casting equipment shown in Figures 1, 2 and 5, and the occurrence of surface cracks in the slab was investigated. The taper rate of the tapered portion on the most upstream side in the casting direction was set to 2.0% / m. The taper rate was calculated using the above formula (1). At this time, V is the distance W between the short side copper plates 11 at the average position of the meniscus M It was decided.

[0062] The surface cracks of the slabs were evaluated as follows: A: No surface cracks B: Almost no surface cracks C: Small surface cracks occur, but they can be removed and there is no problem with product quality. D: Surface cracks are noticeable and there is a problem with the product quality.

[0063] [Table 2]

[0064] From the results of Table 2, in order to prevent the occurrence of surface cracks in the slab, the length C of the contact part in contact with the molten steel should be set to the length C of the mold 10 in the short side direction. Xand the length of the long side C Y It can be seen that it is sufficient to make the difference ΔC shorter than the sum of the above and to make the difference ΔC 3 mm or more. Furthermore, when the difference ΔC exceeds 20 mm, the increase in the corner surface temperature is saturated even if the difference ΔC is further increased. Therefore, from the viewpoint of suppressing the decrease in yield, it is sufficient to make the difference ΔC 20 mm or less.

[0065] As long as the above formula (2) is satisfied, the contact portion of the protrusion 12 may, when the mold 10 is viewed in a plane, have a shape, for example, having one or more corners, may have a shape defined by one or more arcs (curves) as shown in Figure 3C or Figure 3D, or may have a shape defined by a combination of straight lines and arcs (curves) as shown in Figure 3E.

[0066] Here, when the protrusion 12 is provided at the corner of the mold 10, the contact length between the molten steel and the copper plate is reduced compared to when the corner is a right angle, and the amount of heat removal from the mold corner is reduced. Therefore, the surface temperature of the slab corner increases. On the other hand, the thickness of the solidified shell is reduced compared to when the corner is a right angle due to the reduced amount of heat removal. In addition, when the protrusion is provided at the corner of the mold, the gap between the mold and the slab at the early stage of solidification occurs in a wider area compared to when the corner is a right angle. Therefore, the heat removal from the solidified shell to the mold is hindered, the mold cannot be sufficiently cooled, and the solidified shell remains thin. As a result, bulging occurs, and the solidified shell of the slab cracks near the corner of the long side copper plate, where the solidified shell is thinner than the center of the long side width, and there is a possibility that an internal defect called internal cracking occurs.

[0067] In order to prevent internal defects, the copper plate on the short side of the mold 10 is tapered. However, if the mold 10 has a strong taper with a large gradient over the entire casting direction, the frictional restraint force between the mold 10 and the cast piece increases, and breakouts may occur. In particular, when the mold 10 has a protrusion 12, when considering the short-side copper plate 11 on which the protrusion 12 is provided alone, the length C of the contact part that comes into contact with the molten steel is longer than the short-side length C of the mold 10. X (i.e., C>C X) As a result, the contact area between the mold 10 and the slab increases, and the frictional restraint force is more likely to increase.

[0068] However, as described above, in the mold 10 according to this embodiment, the short-side copper plate 11 is provided with two or more different gradients in the casting direction so that a plurality of tapered portions are formed on the inner surface side of the mold 10. As a result, even if the protrusions 12 are provided, it is possible to suppress non-uniform solidification of the corners of the slab in the upper part of the mold 10, where solidification shrinkage is large, and to alleviate strong contact between the slab and the mold 10 in the lower part of the mold 10, where solidification shrinkage is small.

[0069] Furthermore, in the mold 10 according to this embodiment, the narrow side copper plate 11 is provided with a gradient such that the taper ratio R of the taper portion (i.e., the first taper portion T1) on the most upstream side in the casting direction is 1.1% / m or more and 3.5% / m or less. This makes it possible to prevent the gradient of the narrow side copper plate 11 from being too small, which would cause gaps to occur near the corners of the long side copper plate 13 and inhibit the growth of the solidified shell. In addition, it is possible to prevent the gradient of the narrow side copper plate 11 from being too large, which would increase the frictional force between the mold 10 and the slab and cause breakout due to rupture of the solidified shell.

[0070] In the mold 10 according to this embodiment, two or more different gradients are provided in the short-side copper plate 11 in the casting direction so that a plurality of tapered portions are formed on the inner surface side of the mold 10. The plurality of tapered portions are formed so that the gradient (i.e., taper rate) becomes smaller toward the downstream side in the casting direction.

[0071] As a method of providing multiple gradients in the casting direction on the inner surface of the short-side copper plate 11 of the mold 10, for example, a method of using a parabolic taper with a curved inner surface is also available. However, since the taper ratio of the taper part on the most upstream side in the casting direction is a large value exceeding 3.5% / m, a large frictional restraint force acts on the solidified shell, which may cause the solidified shell to break. If the solidified shell breaks, there is a possibility that an operational trouble such as a breakout in which unsolidified molten steel flows out to the outside may occur. In addition, in a parabolic taper mold, the taper ratio varies greatly due to the fluctuation of the meniscus position. Therefore, when the meniscus position varies due to clogging of the submerged entry nozzle, a portion with a small taper ratio is generated, and vertical cracks occur in the cast slab.

[0072] Furthermore, when continuous casting is performed in succession to prevent the immersion nozzle from being damaged by slag, the meniscus position is changed during casting, but in a parabolic taper mold, the range in which the taper rate is appropriate is narrow, so the number of times continuous casting can be performed in succession is reduced, and casting efficiency is reduced. For this reason, in the mold 10 according to this embodiment, two or more different gradients are provided in the short-side copper plate 11 in the casting direction so that multiple taper portions are formed on the inner surface side of the mold 10.

[0073] In addition, a mold using a parabolic taper with a curved inner surface has a complex shape and is difficult to process, which increases the manufacturing cost. On the other hand, by forming two tapered portions T1 and T2 on the inner side of the mold 10 as shown in Figure 5, the shape of the mold 10 is not complicated, and it is possible to set an appropriate gradient on the short side copper plate 11 at low cost with easy processing.

[0074] By continuously casting steel using such a mold 10, uniform solidification of the molten steel can be ensured and corner cracks of the cast piece can be suppressed.

[0075] [2-3. Additional configuration] By adding the following configuration to the basic configuration of the mold 10 described above, it is possible to ensure more uniform solidification of the molten steel and suppress corner cracks in the cast slab.

[0076] (a) Position of the first taper change point For example, the distance X in the casting direction from the average position M of the meniscus position to the first taper change point P1 of the short side copper plate 11 (hereinafter also referred to as the "first taper change point") M (Hereafter, simply "Distance X M The distance X may be 50 mm or more and 300 mm or less. Since the meniscus position changes during casting, the average position M of the meniscus position is used as the reference here. M By making the taper ratio of the first taper portion T1 50 mm or more, the range with a large taper ratio can be made longer. This makes it possible to suppress the generation of a gap between the mold and the slab by making the taper of the top stage of the multi-stage taper large, and it is possible to fully obtain the effect of promoting the growth of the solidified shell. In other words, it is possible to suppress the thickness of the slab shell from becoming thin, and suppress the occurrence of internal cracks. As a result, even if minute internal cracks occur when the taper ratio of the first taper portion T1 is 1.1% / m or more, the effect can be suppressed to a level that does not affect product quality.

[0077] In addition, the distance X in the casting direction from the average meniscus position M to the first taper change point P1 M By setting the taper ratio to 300 mm or less, it is possible to prevent the range with a large taper ratio from becoming too long, which would cause strong contact between the mold 10 and the slab. This makes it possible to suppress the occurrence of breakouts, in which the solidified shell breaks and unsolidified molten steel flows out, due to a large frictional restraining force acting on the solidified shell.

[0078] Here, in Table 3, the distance X in the casting direction from the average meniscus position M to the first taper change point P1 is M Table 3 shows the results of investigating whether or not internal cracks and breakouts occurred in the slab. MThe results show that the occurrence of internal cracks and breakouts in the slab was investigated by changing the standard interval W. The taper ratio of the taper part on the most upstream side in the casting direction was set to 2.0% / m. The taper ratio was calculated using the above formula (1). V is the distance W between the short side copper plates 11 at the average position of the meniscus M The shape of the protruding portion 12 of the mold 10 is such that, in a plan view of the mold 10, the length C of the contact portion that comes into contact with the molten steel is 36 mm, and the length C of the short side of the mold 10 is 10 mm. X 30 mm, and the length C of the long side of the mold 10 Y The shape of the triangle is 20 mm.

[0079] [Table 3]

[0080] From the results of Table 3, in order to prevent internal cracks and breakouts from occurring in the slab, the distance X in the casting direction from the average position M of the meniscus position to the first taper change point P1 of the short side copper plate 11 is M It can be seen that the distance should be set to 50 mm or more and 300 mm or less.

[0081] In addition, the distance X M When the distance X is 100 mm, even if the taper rate of the first taper portion T1 is 2.3% / m or more, no internal cracks occurred in the slab. M When the distance X is 200 mm, even if the taper rate of the first taper portion T1 is 1.9% / m or more, no internal cracks occurred in the slab. M By setting the taper length to 300 mm, no internal cracks were generated even when the taper rate of the first taper portion T1 was 1.1% / m or more.

[0082] (b) Taper ratio of the taper section at the most downstream side in the casting direction The taper ratio of the tapered portion on the most downstream side in the casting direction may be 0.5% / m or more and less than 1.9% / m, and may be equal to or less than the taper ratio of the upstream taper portion. For example, in the mold 10 shown in FIG. 5, the second tapered portion T2 is the tapered portion on the most downstream side in the casting direction. Here, the taper ratio is calculated using the above formula (1). The reference interval W V is the distance W between the short side copper plates 11 at the average position of the meniscus M It was decided.

[0083] If the taper rate of the tapered portion on the most downstream side in the casting direction is 0.5% / m or more, a gap is unlikely to occur between the solidified shell that has solidified and shrunk and the mold 10. As a result, splashes of cooling water used to spray-cool the slab after it leaves the mold 10 and water vapor will not enter the gap, and corrosion of the copper plate of the mold 10 can be suppressed.

[0084] On the other hand, if the taper ratio of the tapered portion on the most downstream side in the casting direction is less than 1.9% / m, the taper ratio does not become too high relative to the solidification shrinkage of the slab, and strong contact between the mold 10 and the slab can be suppressed. Because the solidified shell has grown sufficiently in the lower part of the mold 10, the solidified shell rarely breaks and breaks out. However, by preventing the taper ratio from becoming too high, strong contact between the grown solidified shell and the copper plate of the mold 10 does not occur, and wear on the surface of the copper plate of the mold 10 can be suppressed.

[0085] In this way, by setting the taper rate of the tapered section on the most downstream side in the casting direction to be 0.5% / m or more but less than 1.9% / m and equal to or less than the taper rate of the tapered section on the upstream side, the life of the copper plate of the mold 10 can be extended and the frequency of replacement of the copper plate can be reduced.

[0086] Table 4 shows the results of investigating the taper ratio of the taper part on the most downstream side in the casting direction and the presence or absence of corrosion and wear of the copper plate of the mold 10 after 2000 charges. Table 4 shows the results of investigating the presence or absence of corrosion and wear of the copper plate of the mold 10 after 2000 charges when the taper ratio of the taper part on the most downstream side in the casting direction (i.e., the second taper part T2) was changed when casting a slab with a slab width of 1250 to 2300 mm and a slab thickness of 200 to 400 mm using the continuous casting equipment shown in Figures 1, 2, and 5. The taper ratio of the taper part on the most upstream side in the casting direction was set to 2.0% / m. The shape of the protruding part 12 of the mold 10 is such that, when the mold 10 is viewed from above, the length C of the contact part that contacts the molten steel is 36 mm, and the length C of the short side direction of the mold 10 is 1.0 mm. X 30 mm, and the length C of the long side of the mold 10 Y The shape of the triangle is 20 mm.

[0087] [Table 4]

[0088] The results in Table 4 also show that by setting the taper rate of the tapered section on the most downstream side in the casting direction to be 0.5% / m or more but less than 1.9% / m and equal to or less than the taper rate of the upstream tapered section, the occurrence of corrosion and wear of the copper plate of the mold 10 can be suppressed and the life of the copper plate of the mold 10 can be extended.

[0089] (c) Relationship between the taper ratio of the most upstream taper section and the most downstream taper section in the casting direction The taper ratio of the tapered portion on the most upstream side in the casting direction may be 1.1 to 2.0 times that of the tapered portion on the most downstream side in the casting direction. For example, in the mold 10 shown in Fig. 5, the first tapered portion T1 is the tapered portion on the most upstream side in the casting direction, and the second tapered portion T2 is the tapered portion on the most downstream side in the casting direction.

[0090] Table 5 shows the results of investigating the taper ratio of the tapered portion on the most upstream side in the casting direction relative to the taper ratio of the tapered portion on the most downstream side in the casting direction (hereinafter also referred to as the "taper ratio"), and the occurrence of internal cracks and breakouts in the slab. Table 5 shows the results of investigating the occurrence of internal cracks and breakouts in the slab when the taper ratio was changed when casting a slab with a slab width of 1250 to 2300 mm and a slab thickness of 200 to 400 mm using the continuous casting equipment shown in Figures 1, 2, and 5. The taper ratio of the tapered portion on the most upstream side in the casting direction was 2.0% / m. The taper ratio was calculated using the above formula (1). At this time, the standard interval W V is the distance W between the short side copper plates 11 at the average position of the meniscus M The shape of the protruding portion 12 of the mold 10 is such that, in a plan view of the mold 10, the length C of the contact portion that comes into contact with the molten steel is 36 mm, and the length C of the short side of the mold 10 is 10 mm. X 30 mm, and the length C of the long side of the mold 10 Y The shape of the triangle is 20 mm.

[0091] [Table 5]

[0092] As shown in Table 5, a taper ratio of 1.1 or more can suppress the occurrence of internal cracks in the slab. Also, a taper ratio of 2.0 or less can suppress the occurrence of breakouts. This shows that it is desirable to set the taper ratio to 1.1 or more and 2.0 or less (i.e., the taper ratio of the tapered section on the most upstream side in the casting direction is 1.1 to 2.0 times the taper ratio of the tapered section on the most downstream side in the casting direction). EXAMPLES

[0093] Using the continuous casting equipment shown in Figures 1, 2 and 5, slabs with a slab width of 1250 to 2300 mm and a slab thickness of 200 to 400 mm were cast. At this time, the taper ratio of the taper section (first taper section T1) on the most upstream side in the casting direction, the taper ratio of the taper section (second taper section T2) on the most downstream side in the casting direction, and the position of the first taper change point were changed, and the quality of the produced slabs, the stability of operation, and the copper plate life of the mold were verified. The verification results are shown in Table 6 below. The quality of the slab, the stability of operation, and the copper plate life of the mold were evaluated based on the following evaluation criteria. The taper ratio was calculated using the above formula (1). At this time, the standard interval W V is the distance W between the short side copper plates 11 at the average position of the meniscus M The shape of the protruding portion 12 of the mold 10 is such that, in a plan view of the mold 10, the length C of the contact portion that comes into contact with the molten steel is 36 mm, and the length C of the short side of the mold 10 is 10 mm. X 30 mm, and the length C of the long side of the mold 10 Y The shape of the triangle is 20 mm.

[0094] The quality of the slabs was evaluated based on the presence or absence of internal cracks in the produced slabs. A: No internal cracks B: Almost no internal cracks C: Small internal cracks occur, but there is no problem with the quality of the product. D: Internal cracks have occurred, and there is a problem with the quality of the product.

[0095] The stability of operation was evaluated based on the occurrence of breakouts. A: No breakouts occurred, and there were no small traces of broken solidified shell on the surface of the slab. B: Almost no breakouts, no small traces of broken solidified shell on the slab surface C: Almost no breakouts occurred. There were small marks on the surface of the slab where the solidified shell had broken, but these could be removed in the post-processing process, and there was no problem with the product quality. D: Breakout occurs

[0096] The lifespan of the copper plate of the mold was evaluated according to the following criteria for damage caused by corrosion of the copper plate and damage caused by wear. A: No need to replace until 2000 charges (Excellent productivity) B: No exchange required up to 1500 charges C: No need to replace until 1000 charges (productivity is somewhat low) D: Replacement required after 1000 charges or less (significantly low productivity)

[0097] [Table 6]

[0098] As shown in Table 6, in Examples 1 to 14, the taper ratio of the first taper portion T1, which is the taper portion on the most upstream side in the casting direction, was 1.1% / m or more and 3.5% / m or less, so there was no problem with the quality of the slab, and the operation was stable. On the other hand, in Comparative Example 1, the taper ratio of the first taper portion T1 was smaller than 1.1% / m, so no breakout occurred, but internal cracks occurred in the slab. In Comparative Example 2, the taper ratio of the first taper portion T1 was greater than 3.5% / m, so the occurrence of internal cracks in the slab was reduced compared to Comparative Example 1, but breakouts occurred.

[0099] In Examples 4 to 6 and 8 to 14, the distance in the casting direction from the average meniscus position to the first taper change point ("First taper change point position" in Table 6) was 50 mm or more and 300 mm or less, which resulted in a further reduction in the occurrence of internal cracks and breakouts in the slab. Furthermore, in Examples 8 to 13, the taper ratio of the second taper section T2, which is the taper section on the most downstream side in the casting direction, was 0.5% / m or more and less than 1.9% / m, and was equal to or less than the taper ratio of the upstream taper section, which extended the copper plate life and increased productivity.

[0100] In addition, as Comparative Examples 3 and 4, the same verification was also carried out for the case where there was one taper portion formed inside the mold (i.e., the case of a single taper). As a result, when a strong taper with a relatively large gradient was provided as in Comparative Example 3, almost no internal cracks occurred in the slab, but the frictional restraining force between the mold and the slab increased, and breakouts occurred. In this way, in the case of a single taper, it is difficult to set the gradient of the taper portion large because breakouts occur, but from the results of Examples 3 and 4 and Table 1 above, it is possible to provide a taper portion with a larger gradient by providing multiple taper portions inside the mold. As a result, even if a protruding portion is provided, it is possible to suppress the solidification non-uniformity of the corners of the slab in the upper part of the mold where solidification shrinkage is large, and it is possible to alleviate strong contact between the slab and the mold 10 in the lower part of the mold where solidification shrinkage is small. In addition, when the gradient was made smaller than that of Comparative Example 3 as in Comparative Example 4, breakouts did not occur, but internal cracks occurred in the slab.

[0101] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention. [Explanation of symbols]

[0102] 10 Mold 11 Short side copper plate 11a Inner surface of short side copper plate 12 Protrusion 12a, 12f straight line 12b, 12c, 12d, 12e, 12g Arc 13 Long side copper plate 13a Inner surface of long copper plate T1 First taper section T2 2nd taper section

Claims

1. A continuous casting mold used in a continuous casting facility for continuously casting steel, comprising: A pair of long-side copper plates, A pair of short-side copper plates that are sandwiched between the pair of long-side copper plates and can move along the long-side direction of the long-side copper plates; Equipped with The short side copper plate is The casting mold has two or more different gradients in the casting direction so that a plurality of tapered portions are formed on the inner surface side of the mold to which molten steel is supplied, The inner surface has protrusions extending in the casting direction at both ends in the short side direction, The taper ratio of the taper portion on the most upstream side in the casting direction is 1.1% / m or more and 3.5% / m or less, The taper ratios of the plurality of tapered portions are set to gradually decrease from the upstream side to the downstream side in the casting direction, The protrusion is formed so that, when the mold is viewed in a plane, the length of the contact portion that comes into contact with molten steel is shorter than the sum of the lengths of the mold in the short side and long side directions, and the difference is 3 mm or more. The taper rate R [% / m] is expressed by the following formula (1). R={(W T −W B ) / W V / ΔL}×100 (1) Here, W T [m] is the distance between the opposing copper plates on the narrow side at their upper positions, W B [m] is the distance between the opposing copper plates on the narrow side at their lower positions, W V [m] is the distance between the opposing copper plates on the narrow side at a predetermined position in the casting direction (reference distance), and ΔL [m] is the length in the casting direction between the upper and lower positions. Note that, in the reference distance, the casting direction position is within a range of 50 mm to 300 mm above the taper change point of the copper plate on the narrow side that is furthest upstream in the casting direction.

2. 2. The continuous casting mold according to claim 1, wherein the taper rate of the tapered portion on the most downstream side in the casting direction is equal to or greater than 0.5% / m and less than 1.9% / m, and is equal to or less than the taper rate of the tapered portion on the upstream side.

3. The continuous casting mold according to claim 1 or 2, wherein the mold has two of the tapered portions.

4. The surface connecting the short side copper plate and the long side copper plate formed on the inside of the mold by the protrusion is, when the mold is viewed in a plane, A straight line connecting the short side copper plate and the long side copper plate; A line connecting the short side copper plate and the long side copper plate and consisting of a convex arc toward the corner side of the mold; A line connecting the short side copper plate and the long side copper plate, which connects an arc that is convex toward the inside of the mold and has one end in contact with the long side copper plate, and an arc that is convex toward the corner side of the mold and has one end in contact with the short side copper plate; or A line connecting the short side copper plate and the long side copper plate, the line consisting of a first arc convex toward the inside of the mold and one end of which is in contact with the long side copper plate, a second arc convex toward the corner side of the mold and one end of which is in contact with the short side copper plate, and a straight line connecting the other end of the first arc and the other end of the second arc; The continuous casting mold according to any one of claims 1 to 3, having any one of the shapes of:

5. A method for continuous casting of steel, comprising the steps of: A pair of long-side copper plates, A pair of short-side copper plates that are sandwiched between the pair of long-side copper plates and can move along the long-side direction of the long-side copper plates; Equipped with The short side copper plate is The casting mold has two or more different gradients in the casting direction so that a plurality of tapered portions are formed on the inner surface side of the mold to which molten steel is supplied, The inner surface has protrusions extending in the casting direction at both ends in the short side direction, The taper ratio of the taper portion on the most upstream side in the casting direction is 1.1% / m or more and 3.5% / m or less, The taper ratios of the plurality of tapered portions are set to gradually decrease from the upstream side to the downstream side in the casting direction, The method for continuous casting steel includes casting steel using a continuous casting mold, the protrusion being formed such that, in a plan view of the mold, the length of a contact portion that contacts molten steel is shorter than the sum of the lengths of the mold in the short side and long side directions, and the difference is 3 mm or more. The taper rate R [% / m] is expressed by the following formula (1). R={(W T −W B ) / W V / ΔL}×100 (1) Here, W T [m] is the distance between the opposing short side copper plates at the upper position, W B [m] is the distance between the opposing short side copper plates at the lower position, W V [m] is the distance between the opposing short side copper plates at a predetermined casting direction position (reference distance), and ΔL [m] is the casting direction length between the upper position and the lower position. The reference distance is the distance [m] between the copper plates on the short side at the average position of the meniscus of the molten metal in the mold.

6. A method for continuous casting of steel as described in claim 5, wherein the distance in the casting direction from the average position of the meniscus position to the first taper change point of the short side copper plate is 50 mm or more and 300 mm or less.

7. A method for continuously casting steel as described in claim 5 or 6, which continuously casts a slab having a slab width of 1250 to 2300 mm and a slab thickness of 200 to 400 mm.

Citation Information

Patent Citations

  • Control device of reactor control rod

    JP1984099294A

  • Continuous casting of high-carbon steel

    JP1996150440A

  • Continuous casting mold

    JP2008049385A

  • Continuous casting method and continuous casting mold

    JP2009160645A

  • Casting mold for continuous casting of steel and continuous casting method of steel

    JP2012157872A