Austenitic Stainless Steel

An austenitic stainless steel with a tailored composition and controlled Nb and W content forms a Laves phase along grain boundaries, addressing the balance of creep strength and ductility in high-temperature environments, ensuring structural integrity and performance.

JP7560732B2Active Publication Date: 2024-10-03NIPPON STEEL CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021006260
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-14
Filing Date
2021-01-19
Publication Date
2024-10-03
Estimated Expiration
2041-01-19

AI Technical Summary

Technical Problem

Existing austenitic stainless steel materials do not adequately balance high creep strength and creep ductility in high-temperature environments of 800°C or higher, particularly when exposed to chemical substances like hydrocarbons.

Method used

The development of an austenitic stainless steel material with a specific chemical composition that includes controlled amounts of elements such as C, Si, Mn, P, S, Cr, Ni, Nb, W, B, Al, and others, with a total solid solution Nb and W content of 3.2% by mass or more, and adherence to formulas (1) and (2), promoting the formation of Laves phase along grain boundaries for enhanced precipitation strengthening.

Benefits of technology

The material achieves both high creep strength and creep ductility in high-temperature environments exceeding 800°C, maintaining structural integrity and performance under challenging conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560732000001
    Figure 0007560732000001
  • Figure 0007560732000002
    Figure 0007560732000002
Patent Text Reader

Abstract

To provide an austenitic stainless steel material having a high creep strength and a high creep ductility even in a high-temperature environment at 800°C or more.SOLUTION: An austenitic stainless steel material according to the present disclosure has a chemical composition that includes, in mass %: C: 0.060% or less; Si: 1.0% or less; Mn: 2.00% or less; P: 0.0010 to 0.0400%; S: 0.010% or less; Cr: 10 to 25%; Ni: 25 to 45%; Nb: 0.2 to 2.0%; W: 2.5 to 6.0%; B: 0.0010 to 0.0100%: Al: 2.5 to 4.5%; and the balance being Fe and impurities, and satisfies Formulae (1) and (2), and the sum of the content of dissolved Nb and the content of dissolved W is 3.2 mass% or more. (W / 184+Nb / 93) / (C / 12)≥5.5 (1), (W / 184+Nb / 93) / (B / 11)≤450 (2). Into each symbol of element in the formulae (1) and (2), a content of the corresponding element is substituted in mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to steel materials, and more particularly to austenitic stainless steel materials. [Background technology]

[0002] Steel materials used in chemical plant equipment such as oil refineries and petrochemical plants are used for long periods of time in high-temperature environments containing chemical substances such as hydrocarbons. Therefore, steel materials used in chemical plant equipment are required to have not only oxidation resistance and carburization resistance, but also high creep strength in high-temperature environments. Austenitic stainless steel materials are used as steel materials for such chemical plant equipment applications.

[0003] It is known that in order to improve the oxidation resistance and carburization resistance of austenitic stainless steel materials in the above-mentioned high-temperature environment, it is effective to contain 2.0% or more of Al. When an austenitic stainless steel material contains 2.0% or more of Al, a coating mainly composed of Al2O3 (hereinafter referred to as an alumina coating) is formed on the surface of the steel material instead of a coating mainly composed of Cr2O3 (hereinafter referred to as a chromia coating). The alumina coating is formed more densely than the chromia coating. Therefore, the alumina coating suppresses the penetration of oxygen and carbon in a high-temperature environment into the steel material. As a result, the oxidation resistance and carburization resistance of the austenitic stainless steel material are improved.

[0004] Austenitic stainless steel materials forming an alumina coating are disclosed, for example, in International Publication No. WO 2010 / 113830 (Patent Document 1), International Publication No. WO 2018 / 088070 (Patent Document 2), and JP 2012-505314 A (Patent Document 3).

[0005] The austenitic stainless steel material disclosed in Patent Document 1 has a cast body of a heat-resistant alloy containing, in mass%, C: 0.05-0.7%, Si: more than 0% and not more than 2.5%, Mn: more than 0% and not more than 3.0%, Cr: 15-50%, Ni: 18-70%, Al: 2-4%, rare earth elements: 0.005-0.4%, W: 0.5-10% and / or Mo: 0.1-5%, with the balance being Fe and unavoidable impurities. A barrier layer is formed on the surface of the cast body, and the barrier layer is an Al2O3 layer having a thickness of 0.5 μm or more, and 80 area % or more of the outermost surface of the barrier layer is Al2O3. Cr-based particles having a higher Cr concentration than the alloy matrix are dispersed at the interface between the Al2O3 layer and the cast body. This document states that the barrier layer (Al2O3 layer) has a small amount of Cr oxide on the outermost surface and Cr-based particles are dispersed at the interface between the Al2O3 layer and the casting, so that the barrier layer is less likely to peel off and oxidation resistance and carburization resistance can be maintained. Furthermore, this document states that the inclusion of Ti, Zr, and Nb to form carbides increases the creep rupture strength of austenitic stainless steel materials.

[0006] The tube disclosed in Patent Document 2 is used in a high-temperature atmosphere and is made of a heat-resistant alloy containing, by mass%, Cr: 15% or more, Al: 2.0% or more, and Ni: 18% or more, and the inner surface has an arithmetic mean roughness (Sa) of three-dimensional surface roughness of 1.5≦Sa≦5.0 and a deviation degree (Ssk) of surface height distribution of |Ssk|≦0.30. It is described that the tube disclosed in this document can increase the area ratio of the alumina barrier layer formed on the inner surface of the tube by setting the surface roughness of the tube in an appropriate range. Furthermore, this document describes that the creep strength of the austenitic stainless steel material is increased by adding Nb to form carbides.

[0007] The nickel-chromium alloy disclosed in Patent Document 3 contains, in mass %, C: 0.4-0.6%, Cr: 28-33%, Fe: 15-25%, Al: 2-6%, Si: 2% or less, Mn: 2% or less, Nb: 1.5% or less, Ta: 1.5% or less, W: 1.0% or less, Ti: 1.0% or less, Zr: 1.0% or less, Y: 0.5% or less, Ce: 0.5% or less, Mo: 0.5% or less, N: 0.1% or less, with the remainder being Ni and impurities derived from the melting method. This document describes that the nickel-chromium alloy has the above-mentioned chemical composition, thereby obtaining high oxidation resistance and high creep rupture strength. Specifically, it describes that the nickel-chromium alloy contains Nb, Ti, Ta, and W to form carbides and / or carbonitrides, thereby obtaining high creep strength. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2010 / 113830 [Patent Document 2] International Publication No. 2018 / 088070 [Patent Document 3] Special Publication No. 2012-505314 Summary of the Invention [Problem to be solved by the invention]

[0009] In the above Patent Documents 1 to 3, in order to increase creep strength, carbides and / or carbonitrides are mainly generated during use in a high-temperature environment, and precipitation strengthening of the carbides and / or carbonitrides is utilized. Meanwhile, steel materials for chemical plant equipment applications may be exposed to high-temperature environments of 800°C or higher that contain chemical substances such as the above-mentioned hydrocarbons. In this specification, a high-temperature environment of 800°C or higher that contains chemical substances such as hydrocarbons is also simply referred to as a "high-temperature environment of 800°C or higher." In such a high-temperature environment of 800°C or higher, not only high creep strength but also high creep ductility is required. Patent Documents 1 to 3 do not discuss the compatibility of creep strength and creep ductility in a high-temperature environment of 800°C or higher.

[0010] An object of the present disclosure is to provide an austenitic stainless steel material having high creep strength and high creep ductility even in high temperature environments of 800°C or higher. [Means for solving the problem]

[0011] The austenitic stainless steel material according to the present disclosure has In mass%, C: 0.060% or less, Si: 1.0% or less, Mn: 2.00% or less, P: 0.0010~0.0400%, S: 0.010% or less, Cr: 10-25%, Ni: 25-45%, Nb: 0.2-2.0%, W: 2.5-6.0%, B: 0.0010~0.0100%, Al: 2.5-4.5%, N: 0~0.030%, Cu: 0-2.0%, Ta: 0 to 3.0%, Mo: 0-3.0%, Ti: 0 to 0.20%, V: 0~0.5%, Hf: 0~0.10%, Zr: 0-0.20%, Ca: 0-0.008%, Rare earth elements (REM): 0 to 0.10%, and The balance is Fe and impurities, and has a chemical composition that satisfies formula (1) and formula (2), The total content of solute Nb and solute W is 3.2 mass % or more. (W / 184+Nb / 93) / (C / 12)≧5.5 (1) (W / 184+Nb / 93) / (B / 11)≦450 (2) Here, the content of each element in formulas (1) and (2) is substituted in mass % for each element symbol corresponding to the element. Effect of the Invention

[0012] The austenitic stainless steel material of the present disclosure has high creep strength and high creep ductility even in high temperature environments of 800°C or higher. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present inventors have investigated and examined austenitic stainless steel materials that can achieve both high creep strength and high creep ductility in high temperature environments of 800°C or higher that contain chemical substances such as hydrocarbons, and have obtained the following findings.

[0014] As described in Patent Documents 1 to 3, precipitation strengthening by the formation of carbides and carbonitrides (hereinafter referred to as carbides, etc.) is a means for enhancing creep strength in high-temperature environments. Indeed, in a temperature range below 800°C, precipitation strengthening by carbides, etc. effectively enhances creep strength. However, in a high-temperature environment of 800°C or higher, precipitation strengthening by carbides, etc. may not be able to maintain creep strength sufficiently. In a high-temperature environment of 800°C or higher, carbides once formed in the steel material may dissolve again during use of the steel material. In this case, it is considered that the carbides can no longer function as precipitation strengthening, and creep strength cannot be maintained.

[0015] Therefore, the present inventors have studied precipitation strengthening factors in high-temperature environments of 800°C or higher, which are an alternative to precipitation strengthening by carbides and the like. As a result, it has been found that if a Laves phase (Fe2(W,Nb)) containing W and Nb is generated instead of carbides such as Nb carbide during use of a steel material in a high-temperature environment of 800°C or higher, precipitation strengthening can be maintained even in a high-temperature environment of 800°C or higher, and high creep strength can be obtained. The Laves phase containing W and Nb has a higher melting point than carbides such as Nb carbide. Therefore, in a high-temperature environment of 800°C or higher, the Laves phase containing W and Nb is less likely to form a solid solution than carbides and the like. As a result, precipitation strengthening can be easily maintained even in a high-temperature environment of 800°C or higher, and high creep strength can be obtained in a high-temperature environment of 800°C or higher.

[0016] In order to generate a Laves phase containing W and Nb, it is necessary to suppress the generation of W carbide and Nb carbide, etc., and utilize W and Nb for the generation of the Laves phase. Therefore, the present inventors considered suppressing the C content of the austenitic stainless steel material in order to suppress the generation of W carbide, Nb carbide, etc. As a result of the investigation, it was found that if the C content is 0.060% or less in the chemical composition described below, the generation of W carbide, Nb carbide, etc. can be sufficiently suppressed during use in a high-temperature environment, and a Laves phase containing W and Nb can be generated.

[0017] The present inventors further investigated means for improving creep ductility in a high-temperature environment of 800°C or higher. Strengthening grain boundaries is effective for improving creep ductility. If the Laves phase containing W and Nb is finely formed along the grain boundaries, the grain boundaries are strengthened by precipitation strengthening. As a result, it is considered that both high creep strength and high creep ductility can be achieved in a high-temperature environment of 800°C or higher. In order for the Laves phase containing W and Nb to form along the grain boundaries during use of the steel material in a high-temperature environment of 800°C or higher, it is effective for the steel material to contain B.

[0018] Based on the above findings, the inventors of the present invention have investigated the chemical composition of austenitic stainless steel material, and as a result, the following is found to be present in mass %: C: 0.060% or less, Si: 1.0% or less, Mn: 2.00% or less, P: 0.0010-0.0400%, S: 0.010% or less, Cr: 10-25%, Ni: 25-45%, Nb: 0.2-2.0%, W: 2.5-6.0%, B: 0.0010-0.0100%, Al: 2.5-4.5%, N: 0-0.030%, Cu: 0-2.0%, Ta: 0-3.0%, Mo: It was believed that an austenitic stainless steel material with a chemical composition of C: 0-3.0%, Ti: 0-0.20%, V: 0-0.5%, Hf: 0-0.10%, Zr: 0-0.20%, Ca: 0-0.008%, rare earth elements (REM): 0-0.10%, and the balance being Fe and impurities, may be able to achieve both high creep strength and high creep ductility in high temperature environments of 800°C or higher.

[0019] However, even in the austenitic stainless steel material having the above-mentioned chemical composition, there are cases where high creep strength and high creep ductility are not sufficiently obtained in a high-temperature environment of 800°C or higher. Therefore, the present inventors further investigated means for obtaining high creep strength and high creep ductility in a high-temperature environment of 800°C or higher in the austenitic stainless steel material having the above-mentioned chemical composition. As a result, it was found that in an austenitic stainless steel material having the above-mentioned element contents in the chemical composition, the chemical composition further satisfies formula (1) and formula (2), and the total of the solid solution Nb content and the solid solution W content is 3.2 mass% or more, thereby increasing the creep strength and creep ductility in a high-temperature environment of 800°C or higher. These matters will be described below.

[0020] [Regarding formula (1) and formula (2)] Assuming that the content of each element in the chemical composition is within the above-mentioned range and that the sum of the solute Nb content and the solute W content described below is 3.2 mass% or more, by satisfying the following formulas (1) and (2), it is possible to sufficiently achieve both high creep strength and high creep ductility in high-temperature environments of 800°C or more. (W / 184+Nb / 93) / (C / 12)≧5.5 (1) (W / 184+Nb / 93) / (B / 11)≦450 (2) Here, the content of each element in formulas (1) and (2) is substituted in mass % for each element symbol corresponding to the element.

[0021] It is defined as F1=(W / 184+Nb / 93) / (C / 12). When F1 is less than 5.5, the C content is too high compared to the W content and Nb content in the steel. In this case, even if the C content is 0.060% or less, W carbides and Nb carbides are more likely to be generated preferentially than the Laves phase containing W and Nb during use in a high-temperature environment of 800°C or higher. Therefore, the amount of Laves phase containing W and Nb generated is insufficient. As a result, the creep strength and creep ductility in a high-temperature environment of 800°C or higher are reduced. If F1 is 5.5 or more, the Laves phase containing W and Nb is sufficiently generated in a high-temperature environment of 800°C or higher. Therefore, assuming that the content of each element in the chemical composition of the steel is within the above-mentioned range, formula (2) is satisfied, and the total amount of the solid-solution Nb content and the solid-solution W content is 3.2 mass% or more, if F1 is 5.5 or more, the creep strength and creep ductility of the steel in a high-temperature environment are improved.

[0022] It is defined as F2=(W / 184+Nb / 93) / (B / 11). When F2 exceeds 450, the B content is too small compared to the W and Nb contents that constitute the Laves phase. In this case, the Laves phase containing W and Nb does not form along the grain boundaries, and the Laves phase containing W and Nb is likely to form in clumps. Therefore, during use in a high-temperature environment of 800°C or higher, the Laves phase cannot sufficiently cover the grain boundaries, resulting in insufficient grain boundary strengthening. As a result, the creep strength and creep ductility of the steel material in a high-temperature environment of 800°C or higher are reduced. If F2 is 450 or less, the Laves phase containing W and Nb forms along the grain boundaries during use in a high-temperature environment of 800°C or higher, and the grain boundaries are sufficiently covered by the Laves phase. Therefore, assuming that the content of each element in the chemical composition of the steel is within the range of this embodiment, formula (1) is satisfied, and the sum of the solute Nb content and the solute W content is 3.2 mass% or more, if F2 is 450 or less, the creep strength and creep ductility of the steel in a high temperature environment will be improved.

[0023] [Total of solute Nb content and solute W content] On the premise that the content of each element in the chemical composition of the steel is within the above-mentioned range and formula (1) and formula (2) are satisfied, the total of the solute Nb content and the solute W content is set to 3.2 mass% or more. If the solute Nb content and the solute W content in the austenitic stainless steel material are high, a Laves phase containing W and Nb is likely to be formed in the steel material when the austenitic stainless steel material is used in a high-temperature environment of 800°C or more. Furthermore, even if all W and Nb do not form a Laves phase, if the W and Nb that did not form the Laves phase are solid-solubilized in the austenitic stainless steel material, the creep strength and creep ductility are increased in a high-temperature environment of 800°C or more due to solid-solution strengthening. In other words, if the amount of solid solution of Nb and W in the austenitic stainless steel material is increased, the formation of the Laves phase containing W and Nb is promoted during the use of the austenitic stainless steel material in a high-temperature environment of 800°C or more, and the steel material is further solid-solution strengthened.

[0024] If the total of the solute Nb content and the solute W content is less than 3.2% by mass, the solute Nb content and the solute W content are too small. In this case, the Laves phase containing W and Nb is not sufficiently formed in a high-temperature environment of 800°C or higher. Furthermore, the solute Nb and the solute W that contribute to solution strengthening are too small. Therefore, the creep strength and creep ductility in a high-temperature environment of 800°C or higher are reduced. If the total of the solute Nb content and the solute W content is 3.2% by mass or more, the Laves phase containing W and Nb is sufficiently formed in a high-temperature environment of 800°C or higher, and the solute Nb and the solute W that did not form the Laves phase solid-solution strengthen the steel material. Therefore, assuming that the content of each element in the chemical composition of the steel material is within the range of this embodiment and satisfies formulas (1) and (2), if the total of the solute Nb content and the solute W content is 3.2% by mass or more, the creep strength and creep ductility of the steel material in a high-temperature environment are improved.

[0025] The austenitic stainless steel material of this embodiment has been completed based on the above technical concept. The austenitic stainless steel material of this embodiment has the following configuration.

[0026] [1] In mass%, C: 0.060% or less, Si: 1.0% or less, Mn: 2.00% or less, P: 0.0010~0.0400%, S: 0.010% or less, Cr: 10-25%, Ni: 25-45%, Nb: 0.2-2.0%, W: 2.5-6.0%, B: 0.0010~0.0100%, Al: 2.5-4.5%, N: 0~0.030%, Cu: 0-2.0%, Ta: 0 to 3.0%, Mo: 0-3.0%, Ti: 0 to 0.20%, V: 0~0.5%, Hf: 0~0.10%, Zr: 0-0.20%, Ca: 0-0.008%, Rare earth elements (REM): 0 to 0.10%, and The balance is Fe and impurities, and has a chemical composition that satisfies formula (1) and formula (2), The total of the solute Nb content and the solute W content is 3.2 mass% or more; Austenitic stainless steel. (W / 184+Nb / 93) / (C / 12)≧5.5 (1) (W / 184+Nb / 93) / (B / 11)≦450 (2) Here, the content of each element in formulas (1) and (2) is substituted in mass % for each element symbol corresponding to the element.

[0027] [2] An austenitic stainless steel material according to [1], The chemical composition is Cu: 0.1-2.0%, Ta: 0.1 to 3.0%, Mo: 0.1-3.0%, Ti: 0.01 to 0.20%, and V: 0.1 to 0.5%, containing one or more elements selected from the group consisting of Austenitic stainless steel material.

[0028] [3] An austenitic stainless steel material according to [1] or [2], The chemical composition is Hf: 0.01 to 0.10%, and Zr: 0.01 to 0.20%, containing one or more elements selected from the group consisting of Austenitic stainless steel.

[0029] [4] An austenitic stainless steel material according to any one of [1] to [3], The chemical composition is Ca: 0.001 to 0.008%, and Rare earth elements (REM): 0.01 to 0.10%. Austenitic stainless steel.

[0030] The austenitic stainless steel material of this embodiment will be described in detail below. "%" for elements means mass % unless otherwise specified.

[0031] [Chemical composition] The chemical composition of the austenitic stainless steel material of this embodiment contains the following elements.

[0032] C: 0.060% or less Carbon (C) is inevitably contained. That is, the C content is more than 0%. C is likely to combine with Nb, W, etc. to form carbides. If Nb carbides, etc. and W carbides are formed, the amount of Laves phase containing W and Nb produced at the grain boundaries decreases. Therefore, in a high-temperature environment of 800°C or higher, creep strength and creep ductility decrease. If the C content exceeds 0.060%, even if the contents of other elements are within the range of this embodiment, creep strength and creep ductility decrease significantly for the above-mentioned reasons. Therefore, the C content is 0.060% or less. The preferred upper limit of the C content is 0.057%, more preferably 0.050%, and even more preferably 0.030%. It is preferable that the C content is as low as possible. However, excessive reduction of the C content increases the manufacturing cost. Therefore, in terms of industrial production, the preferred lower limit of the C content is 0.001%, and even more preferably 0.002%.

[0033] Si: 1.0% or less Silicon (Si) is inevitably contained. That is, the Si content is more than 0%. Si deoxidizes steel in the steelmaking process. If even a small amount of Si is contained, the above effect can be obtained to some extent. However, if the Si content exceeds 1.0%, the hot workability of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the Si content is 1.0% or less. The preferred lower limit of the Si content is 0.1%, and more preferably 0.2%. The preferred upper limit of the Si content is 0.9%, and more preferably 0.8%, and even more preferably 0.7%.

[0034] Mn: 2.00% or less Manganese (Mn) is inevitably contained. That is, the Mn content is more than 0%. Mn combines with S in the steel material to form MnS, which improves the hot workability of the steel material. If even a small amount of Mn is contained, the above effect can be obtained to some extent. However, if the Mn content exceeds 2.00%, even if the contents of other elements are within the range of this embodiment, the hardness of the steel material becomes excessively high, and the hot workability and weldability of the steel material decrease. Therefore, the Mn content is 2.00% or less. The preferred lower limit of the Mn content is 0.01%, more preferably 0.10%, more preferably 0.20%, more preferably 0.30%, and more preferably 0.40%. The preferred upper limit of the Mn content is 1.90%, more preferably 1.80%, more preferably 1.50%, more preferably 1.30%, more preferably 1.20%, and more preferably 1.00%.

[0035] P: 0.0010~0.0400% Phosphorus (P) segregates to grain boundaries in a high-temperature environment and suppresses the segregation of S to grain boundaries. Therefore, creep strength is increased. If the P content is less than 0.0010%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the P content exceeds 0.0400%, the hot workability and weldability of the steel material are reduced even if the contents of other elements are within the range of this embodiment. Therefore, the P content is 0.0010 to 0.0400%. The preferred lower limit of the P content is 0.0020%, more preferably 0.0040%, and even more preferably 0.0060%. The preferred upper limit of the P content is 0.0380%, more preferably 0.0360%, and even more preferably 0.0340%.

[0036] S: 0.010% or less Sulfur (S) is unavoidably contained. That is, the S content is more than 0%. If the S content exceeds 0.010%, the hot workability and creep ductility in a high temperature environment of the steel material will decrease even if the contents of other elements are within the range of this embodiment. Therefore, the S content is 0.010% or less. It is preferable that the S content is as low as possible. However, excessive reduction in the S content increases the manufacturing cost of the steel material. Therefore, in consideration of normal industrial production, the preferable lower limit of the S content is 0.001%, and more preferably 0.002%.

[0037] Cr: 10~25% Chromium (Cr) enhances the oxidation resistance and corrosion resistance of the steel when it is used in a high-temperature environment. If the Cr content is less than 10%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Cr content exceeds 25%, even if the contents of other elements are within the range of this embodiment, in a high-temperature environment, Cr in the steel combines with C derived from the atmospheric gas (hydrocarbon gas) in the high-temperature environment, and an excessive amount of Cr carbides are generated on the surface of the base material. In this case, the formation of Al2O3 on the steel surface is not sufficiently promoted, and the carburization resistance of the steel decreases. Therefore, the Cr content is 10 to 25%. The preferred lower limit of the Cr content is 11%, more preferably 12%, more preferably 13%, and more preferably 14%. The preferred upper limit of the Cr content is 24%, more preferably 23%, more preferably 22%, more preferably 21%, and more preferably 20%.

[0038] Ni: 25~45% Nickel (Ni) stabilizes austenite and enhances the creep strength of steel in a high-temperature environment. Ni also enhances the carburization resistance of steel. If the Ni content is less than 25%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Ni content exceeds 45%, even if the contents of other elements are within the range of this embodiment, an excessive amount of intermetallic compounds containing Al (for example, γ' phase (Ni3Al) etc.) is generated, and the hot workability of the steel in a high-temperature environment of the steel is reduced. Therefore, the Ni content is 25 to 45%. The preferred lower limit of the Ni content is 26%, more preferably 27%, more preferably 28%, more preferably 29%, and more preferably 30%. The preferred upper limit of the Ni content is 44%, more preferably 43%, more preferably 42%, more preferably 41%, and more preferably 40%.

[0039] Nb: 0.2-2.0% Niobium (Nb) strengthens the solid solution of the steel material during use in a high-temperature environment, thereby increasing the creep strength. Nb also forms a Laves phase (Fe2(Nb,W)) and, through precipitation strengthening, increases the creep strength and creep ductility of the steel material in a high-temperature environment of 800°C or higher. If the Nb content is less than 0.2%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Nb content exceeds 2.0%, the weldability decreases even if the contents of other elements are within the range of this embodiment. If the Nb content exceeds 2.0%, intermetallic compounds represented by the Laves phase and the gamma double prime phase (γ'' phase (Ni3Nb)) are excessively generated, thereby decreasing the toughness of the steel material, even if the contents of other elements are within the range of this embodiment. Therefore, the Nb content is 0.2 to 2.0%. The preferable lower limit of the Nb content is 0.3%, and more preferably 0.4%. The upper limit of the Nb content is preferably 1.9%, more preferably 1.8%, and further preferably 1.7%.

[0040] W: 2.5-6.0% Tungsten (W) strengthens the steel material by solid solution during use in a high-temperature environment, thereby increasing the creep strength. W also forms a Laves phase (Fe2(Nb,W)) and, through precipitation strengthening, increases the creep strength and creep ductility of the steel material in a high-temperature environment of 800°C or higher. If the W content is less than 2.5%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the W content exceeds 6.0%, the hot workability of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the W content is 2.5 to 6.0%. The preferred lower limit of the W content is 2.8%, more preferably 3.0%, and more preferably 3.2%. The preferred upper limit of the W content is 5.8%, more preferably 5.6%, and more preferably 5.4%.

[0041] B: 0.0010~0.0100% Boron (B) segregates to grain boundaries during use of steel in high-temperature environments, enhancing grain boundary strength. Furthermore, B suppresses the coarsening of the Laves phase containing W and Nb during use of steel in high-temperature environments of 800°C or higher, and promotes the formation of the Laves phase along grain boundaries. This enhances the creep strength and creep ductility of the steel in high-temperature environments of 800°C or higher. If the B content is less than 0.0010%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of this embodiment. On the other hand, if the B content exceeds 0.0100%, the weldability and hot workability of the steel are reduced even if the contents of other elements are within the ranges of this embodiment. Therefore, the B content is 0.0010 to 0.0100%. The preferred lower limit of the B content is 0.0011%, more preferably 0.0012%, more preferably 0.0014%, and even more preferably 0.0018%. The upper limit of the B content is preferably 0.0095%, more preferably 0.0090%, and further preferably 0.0085%.

[0042] Al: 2.5% to 4.5% Aluminum (Al) forms an Al2O3 coating mainly composed of Al2O3 on the surface of the steel material during use in a high-temperature environment. Al2O3 is more thermodynamically stable than Cr2O3. Therefore, if an Al2O3 coating is formed on the surface of the steel material in a high-temperature environment, rather than an oxide film mainly composed of Cr2O3, the oxidation resistance and carburization resistance of the steel material are improved. If the Al content is less than 2.5%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Al content exceeds 4.5%, even if the contents of other elements are within the range of this embodiment, excessive amounts of coarse intermetallic compounds containing Al (for example, γ' phase (Ni3Al), etc.) are generated during the manufacturing process, and the hot workability of the steel material is reduced. Therefore, the Al content is 2.5% to 4.5%. The preferable lower limit of the Al content is 2.6%, more preferably 2.7%, and even more preferably 2.8%. The upper limit of the Al content is preferably 4.3%, more preferably 4.1%, and even more preferably 3.9%. In the chemical composition of the austenitic stainless steel material of this embodiment, the Al content means the total Al content contained in the austenitic stainless steel material.

[0043] The balance of the chemical composition of the austenitic stainless steel material of this embodiment is composed of Fe and impurities. Here, the impurities refer to substances that are mixed in from raw materials such as ore and scrap, or the manufacturing environment, during industrial production of the austenitic stainless steel material, and are permissible within a range that does not adversely affect the austenitic stainless steel material of this embodiment.

[0044] [Optional element] The austenitic stainless steel material of this embodiment may further contain N instead of a portion of Fe.

[0045] N: 0~0.030% Nitrogen (N) is an optional element and may not be contained. That is, the N content may be 0%. When it is contained, that is, when the N content is more than 0%, N stabilizes austenite. If even a small amount of N is contained, the above effect can be obtained to some extent. However, when the N content exceeds 0.030%, N bonds with Al to form AlN at or near the grain boundary. AlN formed at or near the grain boundary reduces the hot workability of the steel material. Therefore, the N content is 0 to 0.030%. The preferable lower limit of the N content is 0.001%, and more preferably 0.002%. The preferable upper limit of the N content is 0.025%, more preferably 0.022%, and more preferably 0.020%.

[0046] The austenitic stainless steel material of this embodiment may further contain, in place of a portion of Fe, one or more elements selected from the group consisting of Cu, Ta, Mo, Ti, and V. These elements are optional elements, and all of them further increase the creep strength of the steel material in a high-temperature environment of 800° C. or higher.

[0047] Cu: 0-2.0% Copper (Cu) is an optional element and may not be contained. That is, the Cu content may be 0%. When it is contained, that is, when the Cu content is more than 0%, Cu further increases the strength of the steel material at room temperature and the creep strength of the steel material in a high temperature environment of 800°C or more by precipitation strengthening. If even a small amount of Cu is contained, the above effect can be obtained to some extent. However, if the Cu content exceeds 2.0%, the ductility and hot workability of the steel material decrease even if the contents of other elements are within the range of this embodiment. Therefore, the Cu content is 0 to 2.0%. The preferable lower limit of the Cu content is 0.1%, more preferably 0.2%, and more preferably 0.5%. The preferable upper limit of the Cu content is 1.9%, and more preferably 1.8%.

[0048] Ta: 0 to 3.0% Tantalum (Ta) is an optional element and may not be contained. That is, the Ta content may be 0%. When it is contained, that is, when the Ta content is more than 0%, Ta dissolves in the Laves phase to increase the amount of Laves phase produced, and further enhances the creep strength and creep ductility of the steel material in a high-temperature environment of 800°C or higher. If even a small amount of Ta is contained, the above effect can be obtained to a certain extent. However, if the Ta content exceeds 3.0%, the hot workability of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the Ta content is 0 to 3.0%. The preferred lower limit of the Ta content is 0.1%, more preferably 0.2%, and more preferably 0.5%. The preferred upper limit of the Ta content is 2.9%, and more preferably 2.8%.

[0049] Mo: 0-3.0% Molybdenum (Mo) is an optional element and may not be contained. That is, the Mo content may be 0%. When it is contained, that is, when the Mo content is more than 0%, Mo dissolves in the austenite parent phase, and further increases the creep strength of the steel material in a high-temperature environment of 800°C or higher by solid solution strengthening. If even a small amount of Mo is contained, the above effect can be obtained to a certain extent. However, if the Mo content exceeds 3.0%, the hot workability of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the Mo content is 0 to 3.0%. The preferred lower limit of the Mo content is 0.1%, more preferably 0.5%, and more preferably 0.7%. The preferred upper limit of the Mo content is 2.5%, more preferably 2.2%, and more preferably 2.0%.

[0050] Ti: 0 to 0.20% Titanium (Ti) is an optional element and may not be contained. That is, the Ti content may be 0%. When titanium (Ti) is contained, that is, when the Ti content is more than 0%, Ti generates a Laves phase during use of the steel material in a high-temperature environment of 800°C or higher, and further enhances the creep strength and creep ductility of the steel material by precipitation strengthening. If even a small amount of Ti is contained, the above effect can be obtained to a certain extent. However, if the Ti content exceeds 0.20%, even if the contents of other elements are within the range of this embodiment, an excessive amount of intermetallic compounds represented by the Laves phase is generated, and the creep ductility of the steel material in a high-temperature environment decreases, and the hot workability of the steel material decreases. Therefore, the Ti content is 0 to 0.20%. The preferable lower limit of the Ti content is 0.01%, more preferably 0.02%, and more preferably 0.03%. The preferable upper limit of the Ti content is 0.18%, more preferably 0.15%, and more preferably 0.12%.

[0051] V: 0 to 0.5% Vanadium (V) is an optional element and may not be contained. That is, the V content may be 0%. When it is contained, that is, when the V content is more than 0%, V generates a Laves phase during use of the steel material in a high-temperature environment of 800°C or more, and further enhances the creep strength and creep ductility of the steel material by precipitation strengthening. If even a small amount of V is contained, the above effect can be obtained to a certain extent. However, if the V content exceeds 0.5%, the hot workability of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the V content is 0 to 0.5%. The preferable lower limit of the V content is 0.1%. The preferable upper limit of the V content is 0.4%, and more preferably 0.3%.

[0052] The austenitic stainless steel material of this embodiment may further contain one or more elements selected from the group consisting of Hf and Zr in place of a portion of Fe. These elements are optional elements, and each of them promotes the formation of an Al2O3 coating on the surface of the steel material in a high-temperature environment, thereby improving the oxidation resistance and carburization resistance of the steel material.

[0053] Hf: 0~0.10% Hafnium (Hf) is an optional element and may not be contained. That is, the Hf content may be 0%. When it is contained, that is, when the Hf content is more than 0%, Hf promotes the formation of an Al2O3 coating on the surface of the steel material during the manufacturing process of the steel material and / or during the use of the steel material in a high-temperature environment, thereby improving the oxidation resistance and carburization resistance of the steel material. If even a small amount of Hf is contained, the above effect can be obtained to a certain extent. However, if the Hf content exceeds 0.10%, even if the contents of other elements are within the range of this embodiment, an excessive amount of intermetallic compounds is formed in the steel material, and the hot workability of the steel material is reduced. Therefore, the Hf content is 0 to 0.10%. The preferable lower limit of the Hf content is 0.01%, more preferably 0.02%, and more preferably 0.03%. The preferable upper limit of the Hf content is 0.09%, more preferably 0.08%, and more preferably 0.07%.

[0054] Zr: 0 to 0.20% Zirconium (Zr) is an optional element and may not be contained. That is, the Zr content may be 0%. When it is contained, that is, when the Zr content is more than 0%, Zr promotes the formation of an Al2O3 coating on the surface of the steel material during the manufacturing process of the steel material and / or during the use of the steel material in a high-temperature environment, thereby improving the oxidation resistance and carburization resistance of the steel material. If even a small amount of Zr is contained, the above effect can be obtained to a certain extent. However, if the Zr content exceeds 0.20%, even if the contents of other elements are within the range of this embodiment, an excessive amount of intermetallic compounds is formed in the steel material, and the hot workability of the steel material is reduced. Therefore, the Zr content is 0 to 0.20%. The preferable lower limit of the Zr content is 0.01%, more preferably 0.02%, and more preferably 0.03%. The preferable upper limit of the Zr content is 0.17%, more preferably 0.15%, and more preferably 0.12%.

[0055] The austenitic stainless steel material of this embodiment may further contain one or more elements selected from the group consisting of Ca and rare earth elements (REM) in place of a portion of Fe. These elements are optional elements, and all of them improve the hot workability of the steel material.

[0056] Ca: 0 to 0.008% Calcium (Ca) is an optional element and may not be contained. That is, the Ca content may be 0%. When it is contained, that is, when the Ca content is more than 0%, Ca fixes S as sulfides. This improves the hot workability of the steel material. If even a small amount of Ca is contained, the above effect can be obtained to some extent. However, if the Ca content exceeds 0.008%, the toughness and hot workability of the steel material decrease even if the contents of other elements are within the range of this embodiment. Therefore, the Ca content is 0 to 0.008%. The preferable lower limit of Ca is 0.001%, more preferably 0.002%, and further preferably 0.003%. The preferable upper limit of Ca content is 0.007%.

[0057] Rare earth elements (REM): 0~0.10% Rare earth elements (REM) are optional elements and may not be contained. That is, the REM content may be 0%. When contained, that is, when the REM content is more than 0%, REM combines with S to form sulfides and fix S. This improves the hot workability of the steel. Fixation of S also suppresses interfacial segregation of S, and the corrosion resistance of the steel is also improved. Even if even a small amount of REM is contained, the above effects can be obtained to a certain extent. However, if the REM content exceeds 0.10%, inclusions such as oxides become excessively large, and the hot workability and weldability of the steel are reduced. Therefore, the REM content is 0 to 0.10%. The preferable lower limit of the REM content is 0.01%, more preferably 0.03%, and more preferably 0.05%. The preferable upper limit of the REM content is 0.09%, more preferably 0.08%, and more preferably 0.07%.

[0058] In this specification, REM is a general term for 17 elements in total, including Sc, Y, and lanthanoids. When the REM contained in the austenitic stainless steel material of this embodiment is one of these elements, the REM content means the content of the element contained. When the REM contained in the austenitic stainless steel material of this embodiment is two or more types, the REM content means the total content of those elements. REM is generally contained in misch metal.

[0059] [Regarding formula (1) and formula (2)] The chemical composition of the austenitic stainless steel material of this embodiment further satisfies the following formulas (1) and (2). (W / 184+Nb / 93) / (C / 12)≧5.5 (1) (W / 184+Nb / 93) / (B / 11)≦450 (2) Here, the content of each element in formulas (1) and (2) is substituted in mass % for each element symbol corresponding to the element.

[0060] [Regarding formula (1)] F1 is defined as (W / 184+Nb / 93) / (C / 12). F1 is an index of the amount of Laves phase generated during use of steel in a high-temperature environment. When F1 is less than 5.5, the C content is too high compared to the W and Nb contents in the steel. In this case, in the steel used in a high-temperature environment of 800°C or higher, W carbides and Nb carbides are generated in excess rather than the Laves phase containing W and Nb. Therefore, the amount of Laves phase generated at the grain boundaries is too small. As a result, the creep strength and creep ductility of the steel in a high-temperature environment of 800°C or higher are reduced. If F1 is 5.5 or more, the Laves phase containing W and Nb is sufficiently generated in the steel used in a high-temperature environment of 800°C or higher. As a result, assuming that the content of each element in the chemical composition of the steel is within the range of this embodiment and the steel satisfies formula (2), if F1 is 5.5 or more, the creep strength and creep ductility of the steel in a high temperature environment of 800°C or more are improved. The preferred lower limit of F1 is 6.0, more preferably 6.5, even more preferably 7.0, and even more preferably 7.5. The upper limit of F1 is not particularly limited, but is, for example, 649.0.

[0061] [Regarding formula (2)] It is defined as F2=(W / 184+Nb / 93) / (B / 11). F2 is an index of the coverage of the grain boundary by the Laves phase. When F2 exceeds 450, the B content is too small relative to the W and Nb contents that constitute the Laves phase. In this case, in the steel material used in a high-temperature environment of 800°C or higher, the Laves phase containing W and Nb is not formed along the grain boundary, and the Laves phase containing W and Nb is formed in a block shape. Therefore, the Laves phase containing W and Nb is unlikely to sufficiently cover the grain boundary. As a result, the creep strength and creep ductility of the steel material in a high-temperature environment of 800°C or higher are reduced. When F2 is 450 or less, the B content is sufficiently large relative to the W and Nb contents that constitute the Laves phase. In this case, in a steel material used in a high-temperature environment of 800°C or higher, B segregated at the grain boundary promotes the formation of a Laves phase containing W and Nb, and the Laves phase containing W and Nb is formed along the grain boundary, and the grain boundary is sufficiently covered by the Laves phase containing W and Nb. As a result, the creep strength and creep ductility of the steel material in a high-temperature environment of 800°C or higher are improved. The preferred upper limit of F2 is 420, more preferably 400, more preferably 350, more preferably 300, and more preferably 290. The lower limit of F2 is not particularly limited, but is, for example, 17.

[0062] [Method of chemical composition analysis of austenitic stainless steel materials] The chemical composition of the austenitic stainless steel material of this embodiment can be determined by a known compositional analysis method. Specifically, when the austenitic stainless steel material is a steel pipe, a drill is used to drill a hole at the center of the wall thickness to generate chips, and the chips are collected. When the austenitic stainless steel material is a steel plate, a drill is used to drill a hole at the center of the plate width and thickness to generate chips, and the chips are collected. When the austenitic stainless steel material is a steel bar, a drill is used to drill a hole at the R / 2 position to generate chips, and the chips are collected. Here, the R / 2 position means the center position of the radius R in a cross section perpendicular to the longitudinal direction of the steel bar.

[0063] The collected chips are dissolved in acid to obtain a solution. The solution is subjected to ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry) to perform elemental analysis of the chemical composition. The C content and S content are determined by the well-known high-frequency combustion method (combustion-infrared absorption method). The N content is determined by the well-known inert gas fusion-thermal conductivity method.

[0064] [Total of solute Nb content and solute W content] In the austenitic stainless steel material of this embodiment, the content of each element in the chemical composition is within the range of this embodiment, and satisfies formulas (1) and (2), and further, the total of the solute Nb content and the solute W content is 3.2 mass% or more.

[0065] If W and Nb are sufficiently dissolved, the formation of the Laves phase containing W and Nb is promoted during use in a high-temperature environment. If the total of the dissolved Nb content and the dissolved W content is less than 3.2 mass%, the dissolved Nb and dissolved W are too little. In this case, the Laves phase containing W and Nb is not sufficiently formed in a high-temperature environment of 800°C or higher. Furthermore, the dissolved Nb and dissolved W that contribute to solution strengthening are too little. As a result, the creep strength and creep ductility in a high-temperature environment of 800°C or higher are reduced.

[0066] If the total of the solute Nb content and the solute W content is 3.2% by mass or more, the Laves phase containing W and Nb is sufficiently formed in a high-temperature environment of 800°C or more, and the grain interior and grain boundary of the steel material are precipitation strengthened by the Laves phase. Furthermore, the solute Nb and solute W not contained in the Laves phase strengthen the steel material. Therefore, the creep strength and creep ductility of the steel material in a high-temperature environment of 800°C or more are improved. The lower limit of the total of the solute Nb content and the solute W content is more preferably 3.4% by mass, more preferably 3.7% by mass, and even more preferably 3.8% by mass. The upper limit of the total of the solute Nb content and the solute W content is not particularly limited, but is, for example, 7.9% by mass.

[0067] [Method for measuring solute Nb content and solute W content] The solute Nb content and the solute W content are determined by the extraction residue method. Specifically, a test piece is taken from the austenitic stainless steel material. The cross section perpendicular to the longitudinal direction of the test piece may be circular or rectangular. When the austenitic stainless steel material is a steel pipe, the test piece is taken so that the center of the cross section perpendicular to the longitudinal direction of the test piece is the center of the thickness of the steel pipe, and the longitudinal direction of the test piece is the longitudinal direction of the steel pipe. When the austenitic stainless steel material is a steel plate, the test piece is taken so that the center of the cross section perpendicular to the longitudinal direction of the test piece is the center of the plate width and the center of the plate thickness of the steel plate, and the longitudinal direction of the test piece is the longitudinal direction of the steel plate. When the austenitic stainless steel material is a steel bar, the test piece is taken so that the center of the cross section perpendicular to the longitudinal direction of the test piece is the R / 2 position of the steel bar, and the longitudinal direction of the test piece is the longitudinal direction of the steel bar.

[0068] The surface of the collected test piece is polished by approximately 50 μm in a preliminary electrolytic polishing to obtain a new surface. The electrolytically polished test piece is electrolyzed (main electrolysis) in an electrolyte (10% acetylacetone + 1% tetraammonium + methanol). The electrolyte after the main electrolysis is passed through a 0.2 μm filter to capture the residue. The resulting residue is decomposed with acid, and the mass of Nb in the residue and the mass of W in the residue are determined by ICP (inductively coupled plasma) emission spectrometry. Furthermore, the mass of the base material (austenitic stainless steel material) subjected to the main electrolysis is determined. Specifically, the mass of the test piece before the main electrolysis and the mass of the test piece after the main electrolysis are measured. The value obtained by subtracting the mass of the test piece after the main electrolysis from the mass of the test piece before the main electrolysis is defined as the mass of the base material subjected to the main electrolysis.

[0069] The mass of Nb in the residue is divided by the amount of base material electrolyzed, and the result is subtracted from the Nb content contained in the chemical composition of the austenitic stainless steel material. That is, the solute Nb content is calculated based on the following formula (i). Furthermore, the mass of W in the residue is divided by the amount of base material electrolyzed, and the result is subtracted from the W content contained in the chemical composition of the austenitic stainless steel material. That is, the solute W content is calculated based on the following formula (ii). The obtained solute Nb content and solute W content are added together to calculate the total solute Nb content and solute W content. Solute Nb content = Nb content in chemical composition (mass%) - Nb mass in residue / base material mass x 100 (i) Solute W content = W content in chemical composition (mass%) - W mass in residue / base material mass x 100 (ii)

[0070] [Shape of the austenitic stainless steel material according to this embodiment] The shape of the austenitic stainless steel material of this embodiment is not particularly limited. The austenitic stainless steel material of this embodiment may be a steel pipe, a steel plate, or a steel bar. The austenitic stainless steel material of this embodiment may also be a forging.

[0071] [Applications of the austenitic stainless steel material of this embodiment] The austenitic stainless steel material of this embodiment is suitable for use in equipment used in high-temperature environments of 800°C or higher. For example, such equipment is a chemical plant facility typified by oil refining and petrochemical processing in high-temperature environments where the atmosphere containing carbon-containing chemical substances reaches 800°C or higher. An example of such a chemical plant is an ethylene production plant. The austenitic stainless steel material of this embodiment can also be used in equipment used in high-temperature environments of less than 800°C.

[0072] The austenitic stainless steel material of this embodiment can be used in equipment other than chemical plant equipment, such as thermal power plant boiler equipment (e.g., boiler tubes) that is expected to be used in high-temperature environments of 800°C or higher, similar to chemical plant equipment.

[0073] [Method of manufacturing austenitic stainless steel material according to this embodiment] A method for producing an austenitic stainless steel material according to this embodiment will be described below. The method for producing an austenitic stainless steel material described below is one example of the method for producing an austenitic stainless steel material according to this embodiment. Therefore, an austenitic stainless steel material having the above-mentioned configuration may be produced by a production method other than the production method described below. However, the production method described below is a preferred example of the method for producing an austenitic stainless steel material according to this embodiment.

[0074] The manufacturing method of the austenitic stainless steel material of this embodiment includes a step of preparing a material (preparation step), a step of manufacturing an intermediate steel material by hot working the material (hot working step), a step of pickling the intermediate steel material after the hot working step and then cold working it as necessary (cold working step), and a step of solution treating the intermediate steel material after the cold working step (solution treatment step). Each step will be described below.

[0075] [Preparation process] In the preparation step, a material having the above-mentioned chemical composition is prepared. The material may be supplied from a third party or may be manufactured. The material may be an ingot, a slab, a bloom, or a billet. When manufacturing the material, the material is manufactured by the following method. Molten steel having the above-mentioned chemical composition is manufactured. For example, molten steel is manufactured by a well-known method using an electric furnace, an AOD (Argon Oxygen Decarburization) furnace, a VOD (Vacuum Oxygen Decarburization) furnace, or the like. An ingot is manufactured by an ingot casting method using the manufactured molten steel. A slab, a bloom, or a billet (cylindrical material) may be manufactured by a continuous casting method using the manufactured molten steel. A billet may be manufactured by hot working the manufactured ingot, slab, or bloom. For example, a cylindrical billet may be manufactured by hot forging an ingot, and the billet may be used as the material (cylindrical material). In this case, the temperature of the material immediately before the start of hot forging is not particularly limited, but is, for example, 1000 to 1300° C. There is no particular limit to the method of cooling the material after hot forging.

[0076] [Hot processing process] In the hot working step, the raw material prepared in the preparation step is subjected to hot working to produce an intermediate steel material. The intermediate steel material may be, for example, a steel pipe, a steel plate, or a steel bar.

[0077] When the intermediate steel material is a steel pipe, the following processing is performed in the hot working step. First, a cylindrical material is prepared. A through hole is formed along the central axis of the cylindrical material by machining. The cylindrical material with the through hole formed therein is subjected to hot extrusion, typically the Ugine-Sejournet process, to manufacture the intermediate steel material (steel pipe). The temperature of the material immediately before hot extrusion is not particularly limited. The temperature of the material immediately before hot extrusion is, for example, 1000 to 1300°C. Instead of the hot extrusion method, a hot punch pipe manufacturing method may be performed.

[0078] Instead of hot extrusion, piercing and rolling according to the Mannesmann process may be performed to manufacture a steel pipe. In this case, a round billet is pierced and rolled by a piercing machine. When piercing and rolling is performed, the piercing ratio is not particularly limited, but is, for example, 1.0 to 4.0. The pierced and rolled round billet is further hot rolled by a mandrel mill, a reducer, a sizing mill, or the like to produce a mother pipe. The cumulative reduction in area in the hot working process is not particularly limited, but is, for example, 20 to 80%. The temperature of the material immediately before piercing and rolling is, for example, 1000 to 1300°C.

[0079] When the intermediate steel material is a steel plate, the hot working step uses, for example, one or more rolling mills equipped with a pair of work rolls. A material such as a slab is hot rolled using the rolling mill to produce a steel plate. The material is heated before hot rolling. The heated material is hot rolled. The temperature of the material immediately before hot rolling is, for example, 1000 to 1300°C.

[0080] In the case where the intermediate steel material is a steel bar, the hot working process includes, for example, a rough rolling process and a finish rolling process. In the rough rolling process, the material is hot worked to produce a billet. In the rough rolling process, for example, a blooming mill is used. Specifically, the material is bloomed by the blooming mill to produce a billet. In the case where a continuous rolling mill is installed downstream of the blooming mill, the billet after blooming may be further hot rolled by the continuous rolling mill to produce a billet of a smaller size. In the continuous rolling mill, for example, a horizontal stand having a pair of horizontal rolls and a vertical stand having a pair of vertical rolls are alternately arranged in a row. In the rough rolling process, a material such as a bloom is produced into a billet. The material temperature immediately before the rough rolling process is not particularly limited, but is, for example, 1000 to 1300°C. In the finish rolling process, the billet is first heated. The heated billet is hot rolled by the continuous rolling mill to produce a steel bar. The heating temperature in the heating furnace in the finish rolling step is not particularly limited, but is, for example, 1000 to 1300°C.

[0081] [Cold working process] The cold working step is carried out as necessary. In other words, the cold working step does not have to be carried out. When the cold working step is carried out, the intermediate steel material is subjected to pickling treatment and then cold working. When the intermediate steel material is a steel pipe or a steel bar, the cold working is, for example, cold drawing. When the intermediate steel material is a steel plate, the cold working is, for example, cold rolling. By carrying out the cold working step, strain is imparted to the intermediate steel material before the solution treatment step. This allows recrystallization to occur and grain regulation to occur during the solution treatment step. The reduction in area in the cold working step is not particularly limited, but is, for example, 10 to 90%.

[0082] [Solution treatment process] In the solution treatment process, the intermediate steel material after the hot working process or the cold working process is subjected to solution treatment. The solution treatment is performed in the following manner. The intermediate steel material is charged into a heat treatment furnace. In the furnace in an air atmosphere, the intermediate steel material is held at the solution treatment temperature T (℃) and then quenched.

[0083] The solution treatment temperature T may be in a known temperature range. For example, the solution treatment temperature T is 1150 to 1280° C. The holding time t at the solution treatment temperature is, for example, 1 to 60 minutes.

[0084] The solution treatment is performed such that the solution treatment temperature T and the holding time t at the solution treatment temperature T are within the above-mentioned ranges, and further the following formula (iii) is satisfied. T×{t (1 / 3) +(Nb / 93+W / 184)×50} / 100≧25···(iii) Here, Nb in formula (iii) means the Nb content (mass%) in the chemical composition of the austenitic stainless steel material. W means the W content (mass%) in the chemical composition of the austenitic stainless steel material. T means the solution treatment temperature T (°C). t means the holding time t (min) at the solution treatment temperature T (°C).

[0085] F3 = T × {t (1 / 3)+ (Nb / 93+W / 184) × 50} / 100. The solution treatment conditions are appropriately set according to the Nb content and W content in the chemical composition of the austenitic stainless steel material, and the solute Nb content and solute W content are increased. If F3 is less than 25, the total of the solute Nb content and solute W content in the austenitic stainless steel material is less than 3.2 mass%. In this case, the creep strength and creep ductility of the austenitic stainless steel are reduced in a high-temperature environment of 800°C or higher.

[0086] The austenitic stainless steel material of this embodiment can be manufactured by the above steps. The above-mentioned manufacturing method is one example of the manufacturing method of the austenitic stainless steel material of this embodiment. Therefore, the manufacturing method of the austenitic stainless steel material of this embodiment is not limited to the above-mentioned manufacturing method.

[0087] As described above, the austenitic stainless steel material of this embodiment has the above-mentioned chemical composition and satisfies formulas (1) and (2). Furthermore, the total of the solute Nb content and the solute W content in the steel material is 3.2 mass% or more. As a result, when used in a high-temperature environment of 800°C or more, the steel material has high creep strength and high creep ductility. EXAMPLES

[0088] [Manufacturing of austenitic stainless steel materials] Molten steel having the chemical composition shown in Table 1 was produced.

[0089] [Table 1]

[0090] Using the molten steel, an ingot with an outer diameter of 120 mm and a weight of 30 kg was produced. The ingot was hot forged to produce a steel plate with a thickness of 30 mm. The temperature of the ingot before hot forging was 1250°C. Furthermore, the steel plate was hot rolled to produce a steel plate (intermediate steel material) with a thickness of 15 mm. The steel plate temperature before hot working (hot rolling) was in the range of 1050 to 1250°C. The intermediate steel material (steel plate) after hot rolling was cold rolled to produce a steel plate with a thickness of 10.5 mm and a width of 80 mm. The intermediate steel material after cold rolling was solution treated at the solution treatment temperature T (°C) and holding time t (min) shown in Table 2. Table 2 also shows the F3 value in the solution treatment. The intermediate steel material after the holding time t at the solution treatment temperature T was water cooled. By the above steps, austenitic stainless steel materials (steel plates) of each test number were manufactured.

[0091] [Chemical composition analysis of steel] The chemical composition of the austenitic stainless steel material (steel plate) of each test number was determined by the following method. A drill was used to drill holes at the center of the plate width and thickness of the steel material (steel plate) to generate chips, which were then collected. The collected chips were dissolved in acid to obtain a solution. ICP-AES was performed on the solution to perform elemental analysis of the chemical composition. The C content and S content were determined by the well-known high-frequency combustion method (combustion-infrared absorption method). The N content was determined by the well-known inert gas fusion-thermal conductivity method. As a result, the chemical composition of the steel material of each test number was as shown in Table 1.

[0092] [Measurement of solute Nb content and solute W content] The dissolved Nb content and dissolved W content were determined by the extraction residue method. Test pieces were taken from the austenitic stainless steel material (steel plate) of each test number. The center of the cross section perpendicular to the longitudinal direction of the test piece was the center position of the plate width and the center position of the plate thickness of the austenitic stainless steel material (steel plate), and the test piece was taken so that the longitudinal direction of the test piece was the longitudinal direction of the austenitic stainless steel material (steel plate). The surface of the taken test piece was polished to about 50 μm by preliminary electrolytic polishing to obtain a new surface. The electrolytically polished test piece was electrolyzed (main electrolysis) with an electrolytic solution (10% acetylacetone + 1% tetraammonium + methanol). The electrolytic solution after the main electrolysis was passed through a 0.2 μm filter to capture the residue. The obtained residue was decomposed with acid, and the Nb mass in the residue and the W mass in the residue were determined by ICP-AES. Furthermore, the mass of the main electrolyzed base material (austenitic stainless steel material) was determined. Specifically, the mass of the test piece before the main electrolysis and the mass of the test piece after the main electrolysis were measured. The mass of the test piece before the main electrolysis minus the mass of the test piece after the main electrolysis was defined as the mass of the base material electrolyzed. The mass of Nb in the residue was divided by the mass of the base material electrolyzed, and subtracted from the Nb content contained as the chemical composition of the austenitic stainless steel material. That is, the dissolved Nb content was calculated based on the following formula (i). Furthermore, the mass of W in the residue was divided by the mass of the base material electrolyzed, and subtracted from the W content contained as the chemical composition of the austenitic stainless steel material. That is, the dissolved W content was calculated based on the following formula (ii). The obtained dissolved Nb content and dissolved W content were summed up to calculate the total of the dissolved Nb content and the dissolved W content. The total of the dissolved Nb content and the dissolved W content (mass%) is shown in Table 2. Solute Nb content = Nb content in chemical composition (mass%) - Nb mass in residue / base material mass x 100 (i) Solute W content = W content in chemical composition (mass%) - W mass in residue / base material mass x 100 (ii)

[0093] [Table 2]

[0094] [Creep strength and creep ductility evaluation test] Creep rupture test specimens conforming to JIS Z 2271 (2010) were prepared from the center of the sheet width and center of the sheet thickness of each test number. The creep rupture test specimen had a diameter of 6 mm and a parallel portion length of 30 mm. The parallel portion was parallel to the rolling direction of the steel sheet. Using the prepared creep rupture test specimens, creep rupture tests conforming to JIS Z 2271 (2010) were conducted. Specifically, the creep rupture test specimens were heated at 800°C, and then the creep rupture tests were conducted. The test stress was 10 MPa, and the creep rupture time (hours) and creep rupture reduction (%) were obtained.

[0095] [Evaluation of creep strength] If the creep rupture time was 2000 hours or more, the creep strength in high temperature environments was judged to be high (indicated as "E" (Excellent) in Table 2). On the other hand, if the creep rupture time was less than 2000 hours, the creep strength in high temperature environments was judged to be low (indicated as "B" (Bad) in Table 2).

[0096] [Evaluation of creep ductility] When the creep rupture reduction is 30% or more, it is judged that the creep ductility in a high temperature environment is excellent (represented as "E" (Excellent) in Table 2). On the other hand, when the creep rupture reduction is less than 30%, it is judged that the creep ductility in a high temperature environment is poor (represented as "B" (Bad) in Table 2).

[0097] [Test Results] The test results are shown in Table 2. Referring to Tables 1 and 2, in test numbers 1 to 13, the contents of each element in the chemical composition were appropriate, satisfying formula (1) and formula (2), and the total of the solute Nb content and the solute W content was 3.2 mass% or more. Therefore, the austenitic stainless steel materials of these test numbers obtained high creep strength in a high temperature environment and also obtained high creep ductility.

[0098] On the other hand, in test number 14, the C content was too high, and therefore the creep strength and creep ductility were low in a high temperature environment.

[0099] Test No. 15 had a low W content, which resulted in low creep strength and creep ductility in a high temperature environment.

[0100] Test No. 16 had a low B content, which resulted in low creep ductility in a high temperature environment.

[0101] Test No. 17 had a low P content, which resulted in low creep strength in high temperature environments.

[0102] Test No. 18 had a low Nb content, which resulted in low creep strength and creep ductility in a high temperature environment.

[0103] In test number 19, although the content of each element in the chemical composition was appropriate, F1 did not satisfy formula (1). As a result, the creep strength and creep ductility were low in a high-temperature environment.

[0104] In test numbers 20 and 21, although the contents of each element in the chemical composition were appropriate, F2 did not satisfy formula (2). As a result, the creep strength and creep ductility were low in a high-temperature environment.

[0105] In test number 22, the contents of each element in the chemical composition, F1 and F2, were appropriate, but the total of the solute Nb content and the solute W content was too low. As a result, the creep strength and creep ductility were low in a high-temperature environment.

[0106] The above describes the embodiments of the present invention. However, the above-described embodiments are merely examples for carrying out the present invention. Therefore, the present invention is not limited to the above-described embodiments, and the above-described embodiments can be appropriately modified and carried out without departing from the spirit of the present invention.

Claims

1. In mass percent, C: 0.060% or less, Si: 1.0% or less, Mn: 2.00% or less, P: 0.0010-0.0400%, S: 0.010% or less, Cr: 10-25%, Ni: 25-45%, Nb: 0.2-2.0%, W: 2.5-6.0%, B: 0.0010 to 0.0100%, Al: 2.5-4.5%, N: 0 to 0.030%, Cu: 0-2.0%, Ta: 0-3.0%, Mo: 0-3.0%, Ti: 0 to 0.20%, V: 0 to 0.5%, Hf: 0-0.10%, Zr: 0 to 0.20%, Ca: 0-0.008%, Rare earth elements (REM): 0 to 0.10%; and The balance is Fe and impurities, and has a chemical composition that satisfies formula (1) and formula (2), The total of the solute Nb content and the solute W content is 3.2 mass% or more; Austenitic stainless steel material. (W / 184+Nb / 93) / (C / 12)≧5.5 (1) (W / 184+Nb / 93) / (B / 11)≦450 (2) Here, the content of each element in formulas (1) and (2) is substituted in mass % for each element symbol corresponding to the element.

2. 2. The austenitic stainless steel material according to claim 1, The chemical composition is Cu: 0.1-2.0%, Ta: 0.1-3.0%, Mo: 0.1 to 3.0%, Ti: 0.01 to 0.20%, and V: 0.1 to 0.5%, containing one or more elements selected from the group consisting of; Austenitic stainless steel material.

3. The austenitic stainless steel material according to claim 1 or 2, The chemical composition is Hf: 0.01 to 0.10%, and Zr: 0.01 to 0.20%; Austenitic stainless steel material.

4. The austenitic stainless steel material according to any one of claims 1 to 3, The chemical composition is Ca: 0.001 to 0.008%, and Rare earth elements (REM): 0.01 to 0.10%. Austenitic stainless steel material.

Citation Information

Patent Citations

  • Twin crystal reinforced aluminum-contained austenite heat resisting stainless steel and preparation method and application thereof

    CN110079737A

  • Nickel-chromium alloy

    JP2012505314A

  • Stainless steel

    JP2018095929A

  • Alloy pipe

    JP2020169346A

  • Low-cost cast creep-resistant austenitic stainless steels that form alumina for high temperature oxidation resistance

    US20190226065A1