Support roll segment for continuous casting machine and continuous casting machine

Ferritic-austenitic duplex stainless steel with a specific pitting corrosion index and yield strength, along with salt bath nitrocarburizing treatment, addresses corrosion and deformation issues in support rolls, enhancing durability and productivity in continuous casting machines.

JP7560738B2Active Publication Date: 2024-10-03NIPPON STEEL CORPORATION
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021068843
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-15
Publication Date
2024-10-03
Estimated Expiration
2041-04-15

AI Technical Summary

Technical Problem

Conventional support rolls in continuous casting machines face issues with corrosion and plastic deformation due to high temperatures and corrosive environments, particularly when exposed to fluorine-containing mold flux, leading to reduced durability and increased maintenance needs.

Method used

The use of ferritic-austenitic duplex stainless steel for the frame and roll shaft, with a pitting corrosion index (PREN) of 20 or more and a 0.2% yield strength of 345 MPa, combined with salt bath nitrocarburizing treatment, enhances corrosion resistance and mechanical properties.

Benefits of technology

The solution provides excellent corrosion resistance and reduced plastic deformation, improving durability and reducing maintenance frequency, thereby increasing the productivity of continuous casting machines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560738000004
    Figure 0007560738000004
  • Figure 0007560738000005
    Figure 0007560738000005
  • Figure 0007560738000006
    Figure 0007560738000006
Patent Text Reader

Abstract

To provide a support roll segment which is laid in a high-temperature and highly corrosive environment, and can be used in a high-temperature and highly corrosive environment, in such conditions that a large load is applied.SOLUTION: Support roll segments arranged between a lower end 11a of a casting mold 11 of a continuous casting machine 10 and a position separated by 2800 mm along a transfer path of a casting piece include a frame and a plurality of support rolls 13. A support roll 13 includes a roll shaft part. When such aging processing that the frame and roll shaft part hold a 0.2% proof stress of 345 MPa or more and a corrosion index of 20 or more, at 475°C for 500 hrs is performed, thereafter, a Charpy impact test is performed and Brinell hardness is measured, support roll segments for a continuous casting machine consisting of ferritic-austenitic duplex stainless steel which does not raise fracture transition temperature, and does not reduce upper shelf energy, or does not increase Brinell hardness, as compared to the stainless steel before the aging processing are selected.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a support roll segment for a continuous casting machine and a continuous casting machine. [Background technology]

[0002] Conventionally, there has been a risk of internal or surface cracks occurring in blooms, billets, and other slabs cast by continuous casting machines due to bulging, which tries to expand the solidified shell outward. To address this issue, support rolls are provided below the mold of the continuous casting machine to support the slab pulled out of the mold. The support rolls are placed in a relatively high-temperature, highly corrosive environment, and are subjected to the load from the slab. For this reason, the optimal materials and structures are selected and adopted, particularly for the roll shafts of the support rolls and the frames that support them.

[0003] For example, Patent Document 1 describes a foot roll for continuous casting, which is located at an initial solidification position immediately below a mold in a continuous steel casting apparatus and has a 2.3 to 3.3 mm thick welded overlay layer of a cobalt-based alloy formed on the surface of the base material by overlay welding.

[0004] Patent Document 2 describes a continuous casting machine in which a slab support roll and a slab support side roll are arranged below the casting mold, approximately 10 m from the meniscus, and each roll is made of SUS630, a 13Cr martensitic stainless steel. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-1502 A [Patent Document 2] JP 2003-275853 A Summary of the Invention [Problem to be solved by the invention]

[0006] The foot rolls immediately below the mold described in Patent Document 1 form an overlay welded layer made of a cobalt-based alloy, and are intended to mainly improve the durability of the roll surface. Similarly, the slab supporting side rolls described in Patent Document 2 are intended to prevent uneven wear of the roll surface. In other words, neither of the techniques described in Patent Documents 1 and 2 takes into consideration the roll shaft portion or the frame supporting the roll shaft portion.

[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a support roll segment that can be used in a high-temperature, highly corrosive environment and under conditions in which a large load is applied, and a continuous casting machine equipped with the support roll segment. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention employs the following configuration. [1] A support roll segment disposed between the lower end of the mold of a continuous casting machine and a position 2,800 mm away along the conveying path of the cast piece, a frame; and a plurality of support rolls rotatably supported by the frame for supporting the strip drawn from the mold, Each of the plurality of support rolls is provided with a roll shaft portion, the frame and the roll shaft are made of ferritic-austenitic duplex stainless steel; The ferritic-austenitic duplex stainless steel has a 0.2% yield strength of 345 MPa or more, a pitting corrosion index (PREN) expressed by the following formula (2) of 20 or more, and when aging treatment is performed at 475°C for 500 hours and then a Charpy impact test specified in JIS Z 2242:2018 is performed and the Brinell hardness is measured, the fracture transition temperature does not increase, the upper shelf energy does not decrease, and the Brinell hardness does not increase, compared to before the aging treatment. PREN=[Cr]+3.3[Mo]+16[N] …(1) In the formula (1), [Cr], [Mo], and [N] are the contents (mass%) of Cr, Mo, and N in the ferritic-austenitic duplex stainless steel, respectively. [2] A support roll segment for a continuous casting machine as described in [1], characterized in that the surface of the ferritic-austenitic duplex stainless steel is subjected to a salt bath soft nitriding treatment. [3] The support roll segment for a continuous casting machine according to [1] or [2], characterized in that the cast piece is a bloom or a billet. [4] A mold; a support roll segment positioned below the mold; The support roll segment includes a frame and a plurality of support rolls rotatably supported by the frame to support a cast piece drawn from the mold, Each of the plurality of support rolls is provided with a roll shaft portion, the frame and the roll shaft portion, which are arranged between the lower end of the mold and a position 2800 mm away along the conveying path of the cast piece, are made of ferritic-austenitic duplex stainless steel; The ferritic-austenitic duplex stainless steel has a 0.2% yield strength of 345 MPa or more, a pitting corrosion index (PREN) expressed by the following formula (2) of 20 or more, and when aging treatment is performed at 475°C for 500 hours and then a Charpy impact test specified in JIS Z 2242:2018 is performed and the Brinell hardness is measured, the fracture transition temperature does not increase, the upper shelf energy does not decrease, and the Brinell hardness does not increase, compared to before the aging treatment. PREN=[Cr]+3.3[Mo]+16[N] …(2) In the formula (2), [Cr], [Mo], and [N] are the contents (mass%) of Cr, Mo, and N in the ferritic-austenitic duplex stainless steel, respectively. [5] A continuous casting machine as described in [4], characterized in that the surface of the ferritic-austenitic duplex stainless steel is subjected to a salt bath soft nitriding treatment. [6] The continuous casting machine according to [4] or [5], wherein the cast piece is a bloom or a billet. Effect of the Invention

[0009] According to the support roll segment for a continuous casting machine of the present invention, the frame and the roll shaft are made of ferritic-austenitic duplex stainless steel having a 0.2% yield strength of 345 MPa or more, a pitting corrosion index (PREN) of 20 or more, and no increase in fracture transition temperature, no decrease in upper shelf energy, or no increase in Brinell hardness before and after aging treatment at 475°C for 500 hours. Therefore, even when these are placed in a high-temperature and highly corrosive environment and used under conditions where a large load is applied, they can exhibit excellent corrosion resistance and, since the amount of plastic deformation is small, durability can be improved.

[0010] Furthermore, according to the continuous casting machine of the present invention, the frame and roll shaft parts arranged within a range of 2800 mm from the bottom end of the mold are made of ferritic-austenitic duplex stainless steel having a 0.2% yield strength of 345 MPa or more, a pitting corrosion index (PREN) of 20 or more, and no increase in fracture transition temperature, no decrease in upper shelf energy, or no increase in Brinell hardness before and after aging treatment at 475°C for 500 hours, so that even when these are placed in a high-temperature and highly corrosive environment and used under conditions where a large load is applied, they can exhibit excellent corrosion resistance and have a small amount of plastic deformation, thereby improving durability. This reduces the frequency of maintenance work on the continuous casting machine and improves productivity of cast strip. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic explanatory diagram of a continuous casting machine according to an embodiment of the present invention. FIG. [Diagram 2] FIG. 2 is a front schematic view showing a support roll segment according to an embodiment of the present invention. [Diagram 3] FIG. 2 is an exploded front schematic view showing a support roll segment according to an embodiment of the present invention. [Figure 4] FIG. 2 is a side schematic view showing a frame and a support roll that constitute a support roll segment according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a side schematic view showing a frame and a support roll that constitute a support roll segment according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In the continuous casting of special steel wire rods, internal cracks are likely to occur in the slab due to the large amount of additives added to the molten steel, the fast casting speed (casting speed: 1.0 m / s or more), the small cross section and the dimensional restrictions on the rolls, etc. Therefore, in order to suppress bulging of the slab, it is necessary to support the slab by placing multiple support rolls directly under the mold.

[0013] Therefore, when arranging a plurality of support rolls directly below the mold, a device called a support roll segment, in which a plurality of support rolls are attached to a frame, is generally arranged directly below the mold.

[0014] Meanwhile, various machines constituting a continuous casting machine are used in an environment where heat resistance, corrosion resistance and predetermined mechanical properties are required, and the materials that can be used are limited. Conventionally, 18Cr stainless steels such as "SUS304" and "SUS630" were used for the roll shafts and frames of the support roll segments arranged in the range from the bottom end of the mold to a position of 2800 mm along the cast slab transport path. However, these stainless steels have insufficient capabilities in terms of corrosion resistance and mechanical properties, and both the roll shafts and the frames may undergo plastic deformation, resulting in a decrease in the ability to suppress bulging. As a countermeasure, it is possible to increase the load capacity by increasing the shaft diameter of the roll shafts or increasing the thickness of the frame, but since a large number of support rolls must be arranged in a narrow range in a continuous casting machine as mentioned above, it is sometimes difficult to adjust the shaft diameter and thickness.

[0015] In addition, when mold flux used in continuous casting adheres to the stainless steel roll shaft and frame, they may be corroded significantly. In particular, when mold flux containing fluorine is used, the corrosion tends to be severe.

[0016] 18Cr stainless steel is generally considered to be somewhat inferior in corrosion resistance to chlorine, and there has been no particular knowledge about its corrosion resistance to fluorine. However, the present inventors have discovered that in environments where the stainless steel is subjected to high temperatures and large loads, such as continuous casting equipment, the corrosion resistance of 18Cr stainless steel caused by fluorine becomes a problem.

[0017] In addition, the above-mentioned circumstances regarding the plastic deformation and corrosion of the support roll segments are not limited to the continuous casting of special steel wire rods, but are generally applicable to continuous casting machines for producing slabs for general steel wire rods, thick steel plates, thin steel plates, and other slabs, and therefore improvement of the support roll segments has been required in these cases as well.

[0018] As a result of intensive research, the present inventors have found that the problems of corrosion and plastic deformation due to load can be solved by using a specific ferritic-austenitic stainless steel as the material for the roll shaft and frame. Hereinafter, an embodiment of the present invention will be described.

[0019] The support roll segment of this embodiment is a support roll segment for a continuous casting machine, which is arranged between a lower end of a mold of a continuous casting machine and a position 2800 mm away from the lower end of the mold along a strip transport path, and which has a frame and a plurality of support rolls rotatably supported by the frame to support the strip pulled out of the mold, and each of the plurality of support rolls is provided with a roll shaft portion, and the frame and the roll shaft portion are made of ferritic-austenitic duplex stainless steel, which has a 0.2% yield strength of 345 MPa or more and a pitting corrosion index (PREN) represented by the following formula (2) of 20 or more, and when a Charpy impact test specified in JIS Z 2242:2018 is performed and the Brinell hardness is measured after aging treatment at 475°C for 500 hours, the fracture transition temperature does not increase, the upper shelf energy does not decrease, and the Brinell hardness does not increase, compared to before the aging treatment. PREN=[Cr]+3.3[Mo]+16[N] …(A) Here, [Cr], [Mo], and [N] in formula (A) are the Cr, Mo, and N contents (mass%) of the ferritic-austenitic duplex stainless steel, respectively. The continuous casting machine of this embodiment is a continuous casting machine in which the above-mentioned frame and roll shaft portion are provided between the lower end of the mold and a position 2800 mm away along the transport path of the cast slab.

[0020] The support roll segment and the continuous casting machine of this embodiment will be described below. Fig. 1 is a schematic diagram of the continuous casting machine.

[0021] A continuous casting machine 10 shown in FIG. 1 includes a mold 11, a nozzle 12 for injecting molten steel into the mold 11, and a plurality of support rolls 13 located below the mold 11. Three molds 11 are installed in the continuous casting machine 10 shown in FIG. 1. The three molds 11 are arranged along the back side of the paper surface of FIG. 1, and only one mold 11 located at the front side is shown in FIG. 1. The continuous casting machine 10 includes a curved band 15 for curving a continuously cast slab 20 produced from the mold 11, a straightening band 16 for bending back the curved continuously cast slab 20 (hereinafter referred to as the slab 20), and a horizontal band 17 for transporting the slab 20 in a horizontal direction. The support rolls 13 in FIG. 1 are arranged in the area of ​​the curved band 15. The rolls arranged in the straightening band 16 and the horizontal band 17 are segment rolls. The support rolls 13 are incorporated in a support roll segment S described later. The continuous casting machine 10 is also provided with transport paths 32 for transporting the rectangular cast pieces 20 drawn out from the three molds 11. Each transport path 32 directly below the mold 11 is partitioned by a plurality of support rolls 13.

[0022] The mold 11 is cylindrical with a rectangular hole, and produces a slab 20 with a cross section that matches the shape of this rectangular hole. The mold 11 is equipped with a primary cooling means (not shown) for cooling the molten steel in the rectangular hole. The location indicated by the reference symbol 11a is the lower end of the mold 11.

[0023] Next, Fig. 2 shows a schematic diagram of a support roll segment S, and Fig. 3 shows an exploded schematic diagram of the support roll segment S. Each support roll segment S is provided with 7 to 10 stages of support rolls 13, and a plurality of such support roll segments S are arranged along the transport direction of the slab 20 to form the transport path 32 of the continuous casting machine shown in Fig. 1. Note that spray nozzles (not shown) are arranged between the support rolls 13 as secondary cooling means, so that the slab 20 can be cooled.

[0024] 2 and 3 define transport paths 32 for transporting the slab 20 provided in the continuous casting machine 10. That is, in each transport path 32, a long side support roll 31A that contacts the long side of the slab to support the long side and a short side support roll 31B that contacts the short side of the slab to support the short side are disposed adjacent to the transport path 32 so as to surround the transport path 32.

[0025] The support roll segment S is provided with a plurality of frames 33A to 33F. The support roll segment S shown in Figs. 2 and 3 is configured by combining a total of six frames 33A to 33F. Each of the frames 33A to 33F is configured with a support body 34 and a plurality of bearing bodies 35 provided on the support body 34. The frames 33A to 33F constituting the support roll segment S shown in Figs. 2 and 3 include frames 33A, 33B, 33C, and 33F in which the bearing body 35 is disposed only on one side of the support body 34 as shown in Figs. 2 to 4, and frames 33D and 33E in which the bearing body 35 is disposed on both sides of the support body 34 as shown in Figs. 2, 3, and 5.

[0026] A support roll 13 is attached to the bearing body 35 of each of the frames 33A to 33F. Each support roll 13 is composed of a roll body 31a and a roll shaft portion 31b inserted into the rotation center shaft of the roll body 31a. The roll shaft portion 31b is fixed to the bearing body 35. The roll body 31a is supported rotatably relative to the roll shaft portion 31b.

[0027] Next, the materials of the frames 33A to 33F and the roll shaft portion 31b will be described. In the support roll segment S and the continuous casting machine 10 of this embodiment, at least the frame and the roll shaft part arranged between the lower end 11a of the mold 11 and a position 2800 mm away along the conveying path 32 of the slab 20 must be made of ferritic-austenitic duplex stainless steel. The surface temperature of the slab 20 is relatively high between the lower end 11a of the mold 11 and a position 2800 mm away along the conveying path 32 of the slab 20. Mold flux is attached to the surface of the slab 20 immediately after it is pulled out of the mold 11. When the mold flux falls off the surface of the slab 20, it falls onto the frame and the roll shaft part located in the range from the lower end 11a of the mold 11 to a position 2800 mm away. In the region more than 2800 mm away from the lower end 11a of the mold 11 along the conveying path 32 of the slab, the water-soluble component of the mold flux is dissolved and diluted in the cooling water that cools the slab 20, so that the frame and the roll shaft part are less damaged. In this way, the frame and roll shaft located within a range of 2800 mm from the lower end 11a of the mold 11 are in a high-temperature environment and are susceptible to corrosion by mold flux. In conventional continuous casting machines, the durability of the frame and roll shaft parts was insufficient.

[0028] In this embodiment, the frame and roll shaft parts arranged between the lower end 11a of the mold 11 and a position 2800 mm away from the mold 11 along the slab transport path 32 are made of ferritic-austenitic duplex stainless steel (hereinafter sometimes referred to as duplex stainless steel) having a 0.2% yield strength of 345 MPa or more, a pitting corrosion index (PREN) expressed by the following formula (2) of 20 or more, and in which, when a Charpy impact test specified in JIS Z 2242:2018 is performed and the Brinell hardness is measured after aging treatment at 475°C for 500 hours, the fracture transition temperature does not increase, the upper shelf energy does not decrease, or the Brinell hardness does not increase compared to before aging treatment. The frame includes a support body 34 and a bearing body 35, and both the support body 34 and the bearing body 35 are made of the ferritic-austenitic duplex stainless steel according to this embodiment.

[0029] PREN=[Cr]+3.3[Mo]+16[N] …(B) Here, [Cr], [Mo], and [N] in formula (B) are the Cr, Mo, and N contents (mass%) of the ferritic-austenitic duplex stainless steel, respectively.

[0030] Duplex stainless steel generally suffers from a phenomenon called 475°C embrittlement. For example, embrittlement occurs when heated to about 300°C to 550°C for a certain period of time, resulting in increased hardness and decreased ductility and toughness. It is called 475°C embrittlement because embrittlement occurs particularly rapidly around 475°C. However, when the surface temperature of the frame and roll shaft parts arranged between the bottom end of the mold of the continuous casting machine according to this embodiment and a position 2800 mm away along the slab transport path was measured, it was found to be less than 140°C at most. When the duplex stainless steel according to this embodiment is subjected to an aging treatment at 475°C for 500 hours and then subjected to a Charpy impact test as specified in JIS Z 2242:2018 and the Brinell hardness is measured, the fracture transition temperature does not increase, the upper shelf energy does not decrease, and the Brinell hardness does not increase compared to before the aging treatment. In other words, the duplex stainless steel is unlikely to become embrittled at high temperatures at 475°C. Therefore, even if the duplex stainless steel is applied to a frame and a roll shaft portion whose surface temperature is at most less than 140°C, the possibility of embrittlement occurring is extremely low.

[0031] In this embodiment, the fracture transition temperature, upper shelf energy, and Brinell hardness are measured for a duplex stainless steel after aging treatment at a soaking temperature of 475°C for a soaking time of 500 hours, and for a duplex stainless steel before aging treatment. Then, it is confirmed whether the fracture transition temperature does not increase, the upper shelf energy does not decrease, or the Brinell hardness does not increase after aging treatment.

[0032] The fracture transition temperature is measured in accordance with JIS Z 2242:2018. The test piece is a standard test piece specified in JIS Z 2242:2018, and is a V-notch. The test temperature range is 20 to -100°C. The fracture transition temperature is determined by obtaining a transition curve in accordance with Appendix D of JIS Z 2242:2018, and the fracture transition temperature is the temperature at which the ductile fracture ratio is 50%.

[0033] The upper shelf energy is defined as the absorbed energy in the upper shelf region on the transition curve created when measuring the fracture transition temperature.

[0034] The Brinell hardness is measured in accordance with JIS Z 223:2008, with an indenter diameter of 10 mm and a test force of 3000 kgf.

[0035] Furthermore, the duplex stainless steel according to this embodiment has a 0.2% yield strength of 345 MPa or more. By making the 0.2% yield strength 345 MPa or more, even if a load is applied from the slab to the support roll due to the effect of bulging, there is no risk of plastic deformation of the frame and the roll shaft.

[0036] Furthermore, the duplex stainless steel according to this embodiment has a pitting corrosion index (PREN) of 20 or more. The frame and roll shaft according to this embodiment are placed in an environment where mold flux containing fluorine is likely to adhere and they are susceptible to corrosion, but by using a material with a pitting corrosion index (PREN) of 20 or more, corrosion resistance can be ensured. The pitting corrosion index (PREN) is preferably 24 or more. There is no particular need to limit the upper limit of the pitting corrosion index (PREN), but it may be, for example, 50 or less.

[0037] In addition, the duplex stainless steel according to this embodiment has a linear expansion coefficient of 13×10 -6 K -1 This can reduce plastic deformation of the frame and the roll shaft due to heat. Furthermore, the duplex stainless steel according to this embodiment preferably has a Brinell hardness HBW of at least 200. This makes it possible to prevent plastic deformation of the frame and the roll shaft portion.

[0038] Duplex stainless steels that satisfy the above conditions include, for example, lean duplex steels SUS821L1 and SUS323L, general-purpose duplex steels SUS329J1, SUS329J3L, and SUS329J4L, and super duplex steel SUS327L1.

[0039] The main chemical components and pitting corrosion index (PREN) of the above duplex stainless steels are as follows: SUS821L1:21Cr-2Ni-3Mn-1Cu-0.17N, PREN=24. SUS323L:23Cr-4Ni-0.15N, PREN=25. SUS329J1L:25Cr-4.5Ni-2Mo, PREN=32. SUS329J3L:25Cr-5Ni-3Mo-0.15N, PREN=37. SUS329J4L:25Cr-6Ni-3Mo-0.15N, PREN=37. SUS327L1:25Cr-7Ni-4Mo-0.28N, PREN=43.

[0040] Among these, SUS327L1 has a PREN of 43, a 0.2% yield strength of 550 MPa or more, and a linear expansion coefficient of 12.7 × 10 -6 K -1 , the Brinell hardness HBW is 310, which is the most preferable.

[0041] In addition, it is preferable that the surface of the ferritic-austenitic duplex stainless steel is subjected to a salt bath soft nitriding treatment, which can further increase the durability of the frame and the roll shaft.

[0042] The support roll segment S and the continuous casting machine 10 of this embodiment are preferably used to produce a bloom or a billet as the cast piece 20. However, the present invention is not limited to the production of blooms or billets, and is also applicable to continuous casting machines that produce cast pieces for general steel wire rods, thick steel plates, thin steel plates, and other cast pieces.

[0043] As described above, according to the support roll segment S for a continuous casting machine of this embodiment, the frame and roll shaft portion arranged in the range from the lower end 11a of the mold 11 to 2800 mm along the conveying path 32 are made of ferritic-austenitic duplex stainless steel, and the ferritic-austenitic duplex stainless steel has a 0.2% yield strength of 345 MPa or more and a pitting corrosion index (PREN) expressed by the following formula (2) of 20 or more. When a Charpy impact test specified in JIS Z 2242:2018 is performed and the Brinell hardness is measured after aging treatment at 475°C for 500 hours, the fracture transition temperature does not increase, the upper shelf energy does not decrease, and the Brinell hardness does not increase compared to before the aging treatment. Therefore, even when these are placed in a high-temperature and highly corrosive environment and used under conditions where a large load is applied, they can exhibit excellent corrosion resistance and can increase durability because the amount of plastic deformation is small.

[0044] In addition, according to the continuous casting machine of this embodiment, the frame and roll shaft parts arranged within a range of 2800 mm from the bottom end of the mold are made of ferritic-austenitic duplex stainless steel, which has a 0.2% proof stress of 345 MPa or more, a pitting corrosion index (PREN) expressed by the following formula (2) of 20 or more, and when a Charpy impact test specified in JIS Z 2242:2018 is performed and the Brinell hardness is measured after aging treatment at 475°C for 500 hours, the fracture transition temperature does not increase, the upper shelf energy does not decrease, and the Brinell hardness does not increase compared to before aging treatment. Therefore, even when these are placed in a high-temperature and highly corrosive environment and used under conditions where a large load is applied, they can exhibit excellent corrosion resistance and the amount of plastic deformation is small, thereby improving durability. This reduces the frequency of maintenance work on the continuous casting machine and improves the productivity of cast slabs. EXAMPLES

[0045] In the continuous casting machine shown in FIG. 1 equipped with the support roll segments shown in FIG. 2 and FIG. 3, the number of charges that the support roll segments could be used continuously was measured when continuous casting was performed over a number of charges. In the present invention example, the frame (support body, bearing body) and roll shaft portion arranged between the lower end of the mold and a position of 2800 mm were made of SUS327L1, and in the comparative example, SUS304. The surface of each stainless steel was subjected to salt bath soft nitriding treatment. Table 1 shows the physical property values ​​of SUS327L1 and SUS304. As a result of the measurement, the support roll segment of the comparative example could be used continuously from 768 to 797 charges without maintenance, while the support roll segment of the present invention example could be used continuously from 1441 to 1537 charges without maintenance, and the life of the support roll segment of the present invention example was extended by 1.9 times compared to the conventional example.

[0046] In addition, when SUS327L1 was subjected to aging treatment at 475°C for 500 hours and then subjected to a Charpy impact test specified in JIS Z 2242:2018 and the Brinell hardness was measured, the fracture transition temperature did not increase, the upper shelf energy did not decrease, and the Brinell hardness did not increase compared to before the aging treatment.

[0047] [Table 1]

[0048] During maintenance, the corrosion state of the roll shaft portion located between the bottom end of the mold and a position 2800 mm away was checked. The results are shown in Table 2. In the comparative example, the corrosion of the roll shaft portion in the range between the bottom end of the mold and 400 mm away was severe, and the corrosion of the roll shaft portion in the range between the bottom end of the mold and 2700 mm away was also significant, but in the inventive example, the corrosion of the roll shaft portion and the roll body was almost nonexistent. The corrosion state of the frame was almost the same as the corrosion result of the roll shaft portion. In Table 2, ◎ indicates that the ratio of the corroded area on the entire surface of the roll shaft portion was 0%, ○ indicates that the ratio of the corroded area on the entire surface of the roll shaft portion was more than 0% and 50% or less, △ indicates that the ratio of the corroded area on the entire surface of the roll shaft portion was more than 50% and less than 100%, and × indicates that the ratio of the corroded area on the entire surface of the roll shaft portion was 100%.

[0049] [Table 2]

[0050] The amount of plastic deformation of the roll shaft was also evaluated. For the roll shafts located between the lower end of the mold and a position 2800 mm away, the amount of plastic deformation of the central axis of the roll shaft after use and the central axis of the roll shaft before use were measured. The results are shown in Table 3 below. The average amount of plastic deformation of the examples of the present invention was about 1 / 7 of that of the comparative examples.

[0051] [Table 3] [Explanation of symbols]

[0052] 10... continuous casting machine, 11... mold, 11a... lower end of mold, S... support roll segment, 13... support roll, 31A... support roll for long side, 31B... support roll for short side, 31a, roll body, 31b... roll shaft portion, 32... conveying path for cast strip, 33A to 33F... frames.

Claims

1. A support roll segment disposed between a lower end of a mold of a continuous casting machine and a position 2800 mm away along a conveying path of a cast piece, a frame; and a plurality of support rolls rotatably supported by the frame for supporting the strip drawn from the mold, Each of the plurality of support rolls is provided with a roll shaft portion, The frame and the roll shaft portion are made of ferritic-austenitic duplex stainless steel, The ferritic-austenitic duplex stainless steel has a 0.2% yield strength of 345 MPa or more, a pitting corrosion index (PREN) represented by the following formula (2) of 20 or more, and when subjected to an aging treatment at 475°C for 500 hours and then a Charpy impact test specified in JIS Z 2242:2018 is performed and the Brinell hardness is measured, the fracture transition temperature does not increase, the upper shelf energy does not decrease, and the Brinell hardness does not increase, compared to before the aging treatment. A support roll segment for a continuous casting machine. PREN=[Cr]+3.3[Mo]+16[N]...(1) In the formula (1), [Cr], [Mo], and [N] respectively represent the contents (mass%) of Cr, Mo, and N in the ferritic-austenitic duplex stainless steel.

2. 2. The support roll segment for a continuous casting machine according to claim 1, wherein a surface of the ferritic-austenitic duplex stainless steel is subjected to a salt bath soft nitriding treatment.

3. 3. The support roll segment for a continuous casting machine according to claim 1, wherein the strand is a bloom or a billet.

4. A mold and a support roll segment positioned below the mold; The support roll segment includes a frame and a plurality of support rolls rotatably supported by the frame to support a cast piece drawn from the mold, Each of the plurality of support rolls is provided with a roll shaft portion, The frame and the roll shaft portion, which are arranged between the lower end of the mold and a position 2800 mm away along the conveying path of the cast piece, are made of ferritic-austenitic duplex stainless steel, The ferritic-austenitic duplex stainless steel has a 0.2% yield strength of 345 MPa or more, a pitting corrosion index (PREN) represented by the following formula (2) of 20 or more, and when aging treatment is performed at 475°C for 500 hours and then a Charpy impact test specified in JIS Z 2242:2018 is performed and the Brinell hardness is measured, the fracture transition temperature does not increase, the upper shelf energy does not decrease, and the Brinell hardness does not increase, compared to before the aging treatment. PREN=[Cr]+3.3[Mo]+16[N]...(2) In the formula (1), [Cr], [Mo], and [N] respectively represent the contents (mass%) of Cr, Mo, and N in the ferritic-austenitic duplex stainless steel.

5. 5. The continuous casting machine according to claim 4, wherein the surface of the ferritic-austenitic duplex stainless steel is subjected to a salt bath soft nitriding treatment.

6. 6. The continuous casting machine according to claim 4, wherein the cast piece is a bloom or a billet.

Citation Information

Patent Citations

  • Composite roll for continuous casting used for nonnwaterrcooling zone

    JP1980068161A

  • Composite roll for continuous casting

    JP1982085959A

  • The piping system in the continuous casting equipment

    JP1985001556U

  • Roll for continuous casting

    JP1988115659A

  • Roll for arbor sleeve type continuous casting

    JP1988192544A