Composite molded products and grooved plastic molded products

Laser-irradiated grooves with specific angles and depths in resin molded products enhance bonding strength, addressing the weakness in composite molded products without fibrous inorganic fillers, thereby increasing overall product strength.

JP7560962B2Active Publication Date: 2024-10-03POLYPLASTICS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020083760
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-12
Publication Date
2024-10-03
Estimated Expiration
2040-05-12

AI Technical Summary

Technical Problem

Existing composite molded products face challenges in strength when joining resin molded products without fibrous inorganic fillers, such as glass fibers.

Method used

Forming grooves on the surface of a first resin molded product using laser irradiation with a specific angle (0<θ<90°) and depth (1/2 or more of the groove length in the lateral direction) to enhance bonding strength, using a resin A with a thermal decomposition temperature of 300°C or higher, and integrating it with another resin molded product.

Benefits of technology

The grooved structure acts as an anchor, significantly increasing the strength of the composite molded product by enhancing bonding resistance against tensile forces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560962000004
    Figure 0007560962000004
  • Figure 0007560962000005
    Figure 0007560962000005
  • Figure 0007560962000006
    Figure 0007560962000006
Patent Text Reader

Abstract

To provide a composite molded product capable of further increasing a strength when bonded to another molded product even in the case where a resin molded product does not contain an inorganic filler such as glass fiber.SOLUTION: A composite molded product 5 is formed by molding with resin B6 together with a first molded product 1 made of resin A having a groove formed on a surface of a junction by laser irradiation. The resin A does not contain a fibrous inorganic compound. A thermal decomposition temperature of the resin A in an air by TGA is 300°C or higher. Moreover, a difference between the thermal decomposition temperature of the resin A and a higher value of a melting point or a glass transition temperature is 130°C or more. When a vertical direction of the junction is 0°, an angle θ in a depth direction of the groove satisfies 0<θ<90°.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite molded product and a grooved resin molded product for forming the composite molded product. [Background technology]

[0002] In recent years, in fields such as automobiles, electrical appliances, and industrial equipment, there has been a growing trend to replace some metal molded products with resin molded products in order to meet the demands for reducing carbon dioxide emissions and manufacturing costs. As a result, composite molded products that integrate resin molded products with metal molded products have become widespread. In addition, composite molded products that integrate molded products made of the same or different materials have also become widespread.

[0003] As a manufacturing method for a composite molded product in which one molded product is integrated with another molded product, for example, Patent Document 1 proposes forming a nanostructure on the surface of one resin molded product by irradiating the surface with electromagnetic radiation, and then bringing the other resin molded product into contact with the surface, filling it, molding it, and integrating them.

[0004] Patent Document 2 proposes a technique in which grooves are formed by laser on the joining surface of a first resin molded product containing glass fibers, and a second resin is injection molded onto the joining surface to produce a composite molded product. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2011-529404 [Patent Document 2] JP 2015-91642 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, there is room for further improvement in the strength when one molded article is joined to another molded article, particularly when the resin molded article does not contain an inorganic filler such as glass fiber.

[0007] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a composite molded product that can further increase the strength when joined to another molded product, even if the resin molded product does not contain a fibrous inorganic filler such as glass fiber. [Means for solving the problem]

[0008] The object of the present invention has been achieved by the following. 1) A composite molded product which is an integrated product of a first molded product made of resin A having grooves formed on the surface of the joint by laser irradiation and resin B, said resin A does not contain fibrous inorganic compounds, said resin A has a thermal decomposition temperature in air measured by TGA of 300°C or higher and the difference between the thermal decomposition temperature of said resin A and the higher of its melting point or glass transition temperature is 130°C or higher, and the angle θ of the depth direction of said groove when the perpendicular direction of said joint is taken as 0° is 0<θ<90°. 2) The composite molded product according to 1) above, wherein the angle θ in the depth direction is 10<θ<80°. 3) The composite molded product according to 1) or 2) above, wherein the depth of the groove is at least 1 / 2 of the length of the groove in the short direction. 4) A grooved resin-molded product made of resin A in which grooves are formed on the surface of a joint by laser irradiation, and the angle θ of the depth direction of the groove is 0<θ<90°, assuming that the perpendicular direction to the joint is 0°. Effect of the Invention

[0009] In the composite molded product of the present invention, the groove angle θ serves as an anchor that bonds more firmly and prevents damage to the molded product, resulting in a marked increase in the strength of the composite molded product. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a schematic diagram of a first molded product showing a groove angle θ of the present invention. [Diagram 2] 1 is an example of an embodiment of a composite molded product of the present invention. [Diagram 3] 1 is another example of an embodiment of the composite molded product of the present invention. [Figure 4] 2 is a schematic diagram showing striped grooves formed in a joint of a first molded product of the present invention. FIG. [Diagram 5] FIG. 2 is a schematic cross-sectional view showing the striped grooves of the present invention. [Figure 6] 3 is a schematic diagram showing a lattice-shaped groove formed in a joint of a first molded product of the present invention. FIG. [Figure 7] FIG. 2 is a schematic diagram showing a tensile test of the composite molded product of the present invention. [Figure 8] FIG. 1 is a schematic cross-sectional view of a conventional composite molded product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following embodiments and can be modified as appropriate within the scope of the object of the present invention. Note that, where the description overlaps, the description may be omitted as appropriate, but this does not limit the gist of the invention.

[0012] <Composite molded products> The composite molded product of the present invention is a composite molded product formed by integrating a first molded product made of resin A, in which a groove is formed on the surface of the joint by laser irradiation, with resin B by molding, and is characterized in that the angle θ of the depth direction of the groove when the vertical direction of the joint is defined as 0° is 0<θ<90°.

[0013] <1st molded product> ≪Groove≫ A first molded product has a surface on which a plurality of grooves are formed. In the present invention, the first molded product, which is a resin molded product with grooves, is integrated with another molded product at the surface having the grooves as a joint to produce a composite molded product.

[0014] The anchor effect is enhanced by providing a plurality of grooves on the surface of the first molded product. The plurality of grooves may be formed by folding back a single groove adjacent to each other, or may be formed by multiple grooves.

[0015] The grooves may be arranged in a line like contour lines with both ends connected, or in stripes without intersecting, or in a lattice pattern with intersecting grooves, or in polka dots. When the grooves are arranged in a lattice pattern, they may be rhombic.

[0016] The length of the groove is not particularly limited, and when the groove is short, the shape of the opening may be rectangular, round, or elliptical. In order to obtain an anchor effect, the longer the groove, the better.

[0017] The distance between adjacent grooves in the present invention is preferably 0.5 to 8 times the width of the groove, i.e., if the groove width is 200 μm, then 150 μm to 1600 μm, and more preferably 1 to 4 times the width of the groove, i.e., if the groove width is 200 μm, then 200 μm to 800 μm.

[0018] The interval between adjacent grooves is preferably 1000 μm or less if the grooves are in a diagonal lattice shape, and more preferably 1000 μm or less if they are linear in one direction. The depth of the groove is at least 1 / 2, preferably at least 1 time, and more preferably at least 3 times the length of the short side of the groove.

[0019] <Groove depth angle θ> Fig. 1 is a schematic diagram of the first molded product of the present invention. The upper part is the joint, the arrow direction is the vertical direction to the joint, and θ is the angle in the depth direction of the groove. θ is 0<θ<90°, preferably 10≦θ≦80°, more preferably 15≦θ≦70°, and particularly preferably 20≦θ≦60°.

[0020] By adding an angle θ to the depth direction of the groove, the bonding strength of the first molded part in the composite molded product can be greatly improved compared to when θ = 0°. In particular, the angle θ acts as resistance against vertical tensile forces, resulting in a significant effect.

[0021] <Resin A of the first molded product> Resin A of the first molded product is capable of forming grooves by laser irradiation, and may be a thermoplastic resin or a thermosetting resin. The thermal decomposition temperature of resin A can be measured by TGA in air and is 300°C or higher, preferably 400°C or higher, and more preferably 450°C or higher.

[0022] The difference between the thermal decomposition temperature of resin A and the higher of the melting point or the glass transition temperature is preferably 130° C. or more, more preferably 150° C. or more, and most preferably 200° C. or more. If it is less than 130° C., when resin A is gasified by laser irradiation to form grooves, the surrounding area melts, making it difficult to process fine shapes.

[0023] Examples of resins suitable for the first molded product include polyphenylene sulfide (PPS), liquid crystal polymer (LCP), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polypropylene (PP), polyethylene (PE), polystyrene (PS), and polyamide (PA).

[0024] Resin A may contain other components within the scope of not impairing the effects of the present invention. Examples of other components include additives such as nucleating agents, pigments, antioxidants, stabilizers, plasticizers, lubricants, release agents, and flame retardants.

[0025] <Method of forming grooves by laser irradiation> This can be obtained by irradiating the first molded article of the present invention with a laser to partially remove the resin and form a plurality of grooves.

[0026] The laser irradiation is set based on the type of material to be irradiated and the output of the laser device, etc., but unless an appropriate amount of energy is irradiated into the resin to form a groove, it may be difficult to form a groove of the specified width and depth, so it is preferable to perform the laser irradiation in multiple steps.

[0027] In addition, to form fine grooves, it is effective to use a pulsed wave laser rather than a continuous wave laser. Continuous waves tend to melt the surrounding area, making it difficult to control the laser output and speed to form fine grooves. The pulse width of the pulsed wave is preferably about 50 ns or less.

[0028] The angle θ can be adjusted by irradiating the joint with a laser at the same angle as θ. A laser absorbent such as a pigment or dye can be added to Resin A to improve absorption of laser irradiation. Carbon black is preferred as the laser absorbent.

[0029] If the presence of a carbonized resin layer can be confirmed by Raman spectroscopic analysis of the groove portion, it can be determined that the groove has been formed by irradiation with laser light.

[0030] <Composite molded products> Figures 2 and 3 are schematic diagrams of enlarged cross sections of the composite molded product of the present invention. In Figure 2, grooves are formed in parallel in the same direction, and the θ of each groove is the same. Figure 3 shows a composite molded product with grooves having θ in opposite directions. In addition to 0<θ<90°, θ=0° may also be included. In that case, it is preferable that 60% or more of the groove area is 0<θ<90°.

[0031] <Resin B> There is no particular restriction on the type of thermoplastic or thermosetting resin as long as it is an injection moldable resin for Resin B. Examples include polyphenylene sulfide (PPS), liquid crystal polymer (LCP), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyacetal (POM), polypropylene (PP), polyethylene (PE), polystyrene (PS), polycarbonate (PC), polyamide (PA), etc.

[0032] <Method of forming composite molded products> The composite molded product of the present invention can be obtained not only by multiple molding, but also by heating a resin molded product, such as ultrasonic welding, hot plate welding, laser welding, high-frequency induction heating welding, hot press molding, etc. In addition, it can also be obtained by painting, printing, room temperature curing, heat curing, moisture curing, two-component curing, UV curing, hot melt curing, etc. of adhesives.

[0033] In the case of double molding, the first molded product is placed in a mold, and thermoplastic resin B is injected into the mold with the surface having the groove as the contact surface. At that time, resin B also enters the groove, and by cooling in this state, a composite molded product can be formed.

[0034] In this way, with double molding, the pressure applied when resin B is injected into the mold makes it easy to fill the inside of the groove. EXAMPLES

[0035] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, measurements were carried out in an atmosphere of 23°C and 50% RH. <Example 1>

[0036] The materials used in the examples are as follows: <Resin A> A-1 PPS: Polyplastics Co., Ltd. DURAFIDE (registered trademark) 0220A9 HD9100 A-2 LCP: Polyplastics Co., Ltd. LAPEROS (registered trademark) A9500VD3003 A-3 POM: Polyplastics Co., Ltd. Duracon (registered trademark) M90-44 CD3068

[0037] <Resin B> B-1 POM: Polyplastics Co., Ltd. Duracon (registered trademark) M450-44 CF2001

[0038] <Preparation of the first molded product> <Preparation of test specimens> The first molded product was prepared in the shape of an Izod test piece according to ASTM D256 (W12.7×D6.4×L63.5 mm, no notch was created). Resin A was injection molded into an ASTM Izod test specimen mold under the following molding conditions. PPS: Cylinder temperature 310℃, mold temperature 140℃ LCP: Cylinder temperature 310℃, mold temperature 80℃ POM: Cylinder temperature 190℃, mold temperature 80℃

[0039] Next, a laser irradiation device was used to treat the surface of the joint with a laser with an irradiation diameter of 80 μm from a specified angle, producing a first molded product. The striped pattern was irradiated to create grooves with a pitch of 1.0 mm, a width of 80 μm, and a depth of approximately 1,000 μm, as shown in Figures 4 and 5. The lattice pattern was irradiated to create grooves with a pitch of 2.0 mm in the same direction, a width of 80 μm, and a depth of 300 μm, as shown in Figures 6 and 5.

[0040] In the table, "reverse" refers to the second irradiation angle, which was in a V-shape, and indicates that irradiation was performed from the opposite side, 180°, from the first irradiation position.

[0041] <Laser irradiation conditions> Laser wavelength: 1064nm Laser irradiation diameter: 80μm Irradiation device: Keyence laser marker MD-X1520 Laser power: 22.5W Irradiation speed: 20mm / s Pulse width: 4.6ns

[0042] <Production of composite molded products> The test piece prepared above was double-molded with resin B using an ASTM bending test piece mold under conditions of a cylinder temperature of 190°C and a mold temperature of 80°C to produce an ASTM bending test piece (12.7 x 6.4 x 127 D790) mm as shown in Figure 7. The cross-sectional area of ​​the joint was 81.3 mm 2(12.7 x 6.4 mm).

[0043] <Bonding strength measurement> The composite molded product samples were subjected to the measurement of the tensile breaking strength of the ASTM bending test pieces using a universal testing machine, and the tensile stress was calculated from the cross-sectional area of ​​the joint. The results are shown in Tables 1 and 2. Breaking speed: 10mm / min Testing machine: Shimadzu universal testing machine AG-20kNXDplus

[0044] <Weight loss temperature> 10 mg of resin A was weighed out and heated at 10° C. / min in an air atmosphere using a Seiko Electronics TG / DTA6200, and the temperature at which the weight loss reached 1% was recorded as the weight loss temperature.

[0045] <Melting point, glass transition temperature> 5 mg of resin A was weighed out, and the melting point was measured under nitrogen at 10°C / min using a Perkinelmer DIAMOND DSC. Note that A-2LCP is a liquid crystal polymer, and exhibits liquid crystallinity in the molten state, so the glass transition temperature was not measured.

[0046] [Table 1]

[0047] [Table 2]

[0048] [Table 3]

[0049] From Tables 1 and 2 it can be seen that the grooves of the present invention having 0<θ<90° provide improved bond strength relative to θ=0. [Explanation of symbols]

[0050] 1 1st molded product (resin A) 2 Vertical direction of joint 3 grooves 4 Joint 5 Composite molded product 6 Resin B P tensile tension

Claims

1. A first molded product made of resin A having a groove formed on the surface of the joint by laser irradiation, and a composite molded product integrated with resin B by molding, The resin A does not contain a fibrous inorganic compound, The thermal decomposition temperature of the resin A in air by TGA is 300° C. or higher, and the difference between the thermal decomposition temperature of the resin A and the higher of the melting point or the glass transition temperature is 130° C. or higher; The angle θ of the groove in the depth direction when the vertical direction of the joint is 0° is 0<θ<90°, The grooves are formed in a striped or lattice pattern in the composite molded product.

2. 2. The composite molded product according to claim 1, wherein the angle θ in the depth direction satisfies 10°≦θ≦80°.

3. A grooved resin molded product made of resin A in which grooves are formed on the surface of a joint by laser irradiation, The resin A does not contain a fibrous inorganic compound, The thermal decomposition temperature of the resin A in air by TGA is 300° C. or higher, and the difference between the thermal decomposition temperature of the resin A and the higher of the melting point or the glass transition temperature is 130° C. or higher; The angle θ of the groove in the depth direction is 0<θ<90°, where the perpendicular direction of the joint is 0°. The grooved resin molded product has grooves formed in a stripe or lattice pattern.

Citation Information

Patent Citations

  • Composite component and method for manufacturing a composite component

    JP2011529404A

  • Composite molding and method for producing the same

    JP2014018995A

  • Grooved resin molded article

    JP2015091642A

  • Grooved resin molded part

    WO2014125999A1

  • Production method for bonded structure, and bonded structure

    WO2016027777A1