Manufacturing method of pellets and compacts with low porosity

By controlling pore formation in pellets made from thermoplastic resin and cellulose nanofibers, the issue of surface defects and yellowness in molded bodies is addressed, resulting in improved appearance and productivity.

JP7561086B2Active Publication Date: 2024-10-03ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021093204
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-13
Filing Date
2021-06-02
Publication Date
2024-10-03
Estimated Expiration
2040-05-13

AI Technical Summary

Technical Problem

The production of molded articles using thermoplastic resin and cellulose nanofibers often results in the formation of pores within the pellets, leading to surface defects such as silver streaks and increased yellowness in the molded bodies.

Method used

The pellets are formulated with controlled pore content, limited to 10 or less per 100 pellets, and a pore area ratio of 4.0% or less in the TD cross section, along with specific angle and size parameters, to minimize pore formation and improve appearance.

Benefits of technology

This approach results in molded articles with reduced defects and suppressed yellowing, enhancing the appearance and productivity of the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561086000002
    Figure 0007561086000002
  • Figure 0007561086000003
    Figure 0007561086000003
  • Figure 0007561086000004
    Figure 0007561086000004
Patent Text Reader

Abstract

To provide a pellet that comprises a thermoplastic resin and a cellulose nanofiber and can produce a molded body having good appearance and suppressed yellowing, and to provide a method for producing molded body using the same.SOLUTION: In one embodiment, there is provided a pellet comprising a thermoplastic resin and a cellulose nanofiber, and in which the number of void-containing pellet per 100 pellets is 10 or less. Further, in one embodiment, there is provided a method for producing molded body that includes a step of preparing said pellet and a step of injection molding the pellets in a mold to yield a molded body.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pellet having a low porosity and a method for producing a molded article using the pellet. [Background technology]

[0002] Conventionally, various fillers have been blended into molded articles mainly made of thermoplastic resins in order to improve their physical properties, and in recent years, due to growing interest in environmental issues, the use of cellulose derived from natural products as the filler has been considered. In the production of molded articles containing thermoplastic resins and cellulose, a resin composition containing thermoplastic resins and cellulose is generally extruded in a molten state into a strand shape, cooled, and then cut with a pelletizer to form pellets, and the pellets are then melted again and molded into the desired molded article.

[0003] Recently, attention has been focused on cellulose nanofibers (CNFs), which have an extremely fine structure and are expected to have an excellent effect of improving physical properties in molded products. Regarding the production of pellets containing thermoplastic resin and cellulose nanofibers, Patent Document 1 describes a molding material mixture containing at least one substrate selected from resins and fibers and cellulose nanofibers, characterized in that a hydrophobic polymer is chemically bonded to at least a portion of the -OH groups of the cellulose nanofibers, and the substrate and cellulose nanofibers are pulverized or pelletized. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-16896 A Summary of the Invention [Problem to be solved by the invention]

[0005] The technology described in Patent Document 1 aims to prevent the occurrence of hydrogen bonds between cellulose fibers by blocking at least a portion of the -OH groups of cellulose nanofibers with a hydrophobic polymer, thereby obtaining a molding material mixture that is stable in the pulverized or pellet form. However, the inventors' studies have revealed that when a resin composition containing a thermoplastic resin and cellulose nanofibers is molded into pellets, voids are likely to form inside the pellets (especially in the center), and that when a molded product is produced using pellets containing such voids as a raw material, silver streaks (defective appearance) are likely to occur on the surface of the molded product, and furthermore, the yellowness of the molded product increases.

[0006] The present invention aims to solve the above-mentioned problems and provide pellets containing a thermoplastic resin and cellulose nanofibers, which enable the production of a molded article that has a good appearance and is suppressed from yellowing, and a method for producing a molded article using the pellets. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above problems, the present inventors have found that pellets in which the pores are appropriately controlled can be used to produce molded articles in which the occurrence of poor appearance such as silver streaks and yellowing is suppressed, and have completed the present invention. That is, the present invention includes the following aspects.

[0008] [1] Pellets of a resin composition containing a thermoplastic resin and a cellulose nanofiber, wherein the number of void-containing pellets per 100 pellets is 10 or less. [2] The pellet according to the above-mentioned embodiment 1, wherein the ratio of the void area to the cross-sectional area in the TD cross section of the pellet is 4.0% or less. [3] The pellet according to the above embodiment 1 or 2, wherein the number of void-containing pellets per 100 pellets is 1 or less. [4] The pellet according to any one of the above embodiments 1 to 3, wherein the angle between the MD direction of the pellet and the normal direction to the cut surface of the pellet is 5° to 30°. [5] The pellet according to any one of the above embodiments 1 to 4, wherein the short axis of the pellet in TD cross section is 2 mm to 5 mm. [6] The pellet according to any one of aspects 1 to 5, comprising 0.1 to 30% by mass of the cellulose nanofibers. [7] The pellet according to any one of the above aspects 1 to 6, wherein the cellulose nanofibers have a fiber diameter of 50 to 1,000 nm and a fiber length / fiber diameter (L / D) ratio of 30 or more. [8] The pellet according to any one of the above aspects 1 to 7, wherein the cellulose nanofibers are hydrophobized cellulose nanofibers. [9] The pellet according to any one of the above aspects 1 to 8, wherein the thermoplastic resin is a polyamide-based resin and / or a polyolefin-based resin.

[10] The pellet according to any one of the above embodiments 1 to 9, further comprising an elastomer.

[11] The pellet according to any one of the above aspects 1 to 10, further comprising cellulose nanocrystals having a diameter of 100 nm or less and an L / D ratio of less than 30, or cellulose microfibers having a fiber diameter of more than 1 μm to 50 μm, or a mixture thereof.

[12] The pellet according to any one of the above aspects 1 to 11, wherein the difference Tcc-Tcp between the cooling-down crystallization peak temperature Tcc of the resin composition measured by a differential scanning calorimeter and the cooling-down crystallization peak temperature Tcp of the thermoplastic resin measured by a differential scanning calorimeter is 5°C to 30°C.

[13] The pellet according to any one of the above aspects 1 to 12, wherein the ratio Ve / Vc of the total volume of pores in the pellet (Ve) to the total volume of the cellulose nanofibers (Vc) per 100 pellets is 0 vol.% to 4 vol.%.

[14] The resin composition further comprises a resin crystallization temperature lowering agent, 14. The resin composition according to any one of the above-mentioned aspects 1 to 13, wherein the resin crystallization temperature lowering agent is a compound that lowers the temperature-lowering crystallization peak temperature of the resin composition by 5 to 30° C. as measured by a differential scanning calorimeter.

[15] Preparing a pellet according to any one of the above aspects 1 to 14; and A step of injection molding the pellets in a mold to obtain a molded body; A method for producing a molded body, comprising the steps of: Effect of the Invention

[0009] According to the present invention, there can be provided pellets containing a thermoplastic resin and cellulose nanofibers, which enable the production of a molded article having a good appearance and suppressed yellowing, and a method for producing a molded article using the pellets. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a diagram illustrating a cut surface of a pellet. [Diagram 2] FIG. 2 is a diagram illustrating an aspect in which the cut surface of the pellet is inclined. [Diagram 3] FIG. 3 is a diagram illustrating an aspect in which the cut surface of the pellet is inclined. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, exemplary embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0012] [pellet] One aspect of the present invention provides a pellet containing a thermoplastic resin and cellulose nanofibers. In one aspect, the number of void-containing pellets per 100 pellets is 10 or less. In this disclosure, the term "void-containing pellet" refers to a pellet having at least one visible void when the pellet is cut in the pellet TD direction (i.e., the TD direction (transverse direction) when the pellet is formed) at the center of the pellet MD direction (i.e., the MD direction (machine direction) when the pellet is formed) and the pellet TD cross section obtained is observed under a microscope. Specifically, each of 100 randomly selected pellets is cut in the center of the pellet MD direction and further flattened with a microtome to obtain a TD cross section. The morphological image of this TD cross section is photographed under a microscope at a magnification of 20 times and an observation field of 10 mm x 14 mm, and the pellet having a visible void is determined to be a void-containing pellet.

[0013] The cause of voids in pellets containing thermoplastic resin and cellulose nanofibers is thought to be that the cellulose nanofibers act as a nucleating agent for the thermoplastic resin when the strands are cooled after the cellulose nanofibers are mixed with the molten thermoplastic resin to form strands. In particular, when the cooling rate of the strands is high, the crystallization of the thermoplastic resin, which solidifies the strands, proceeds more rapidly near the surface than inside the strands, and voids are likely to occur inside the strands. In addition, the fact that the cellulose nanofibers may exhibit thixotropy in the resin composition is also thought to be a cause of voids. That is, in the production of pellets, a resin composition containing a thermoplastic resin and cellulose nanofibers is usually melt-mixed (for example, melt-kneaded) and then cooled, and the shear force applied to the resin composition during melt mixing is generally relatively low. Under such low shear force, the high viscosity of the resin composition due to the thixotropy of the cellulose nanofibers is thought to generate voids. When a molded body is produced using pellets having such voids as a molding material, the presence of air during molding is thought to cause poor appearance of the molded body and yellowing due to deterioration of the resin composition. The pellet according to one embodiment of the present invention has few voids, and is therefore useful for producing a molded article having a good appearance and suppressed yellowing.

[0014] Furthermore, having a small number of void-containing pellets improves the penetrating ability of the pellets when melting them to produce a molded body, thereby shortening the molding cycle, which is advantageous in terms of improving productivity and suppressing decomposition of the thermoplastic resin and cellulose nanofibers.

[0015] In one embodiment, the number of void-containing pellets per 100 pellets containing a thermoplastic resin and cellulose nanofibers is 10 or less, preferably 8 or less, more preferably 5 or less, even more preferably 3 or less, even more preferably 1 or less, and most preferably 0, from the viewpoint of obtaining a molded body with few appearance defects and yellowing. The number of void-containing pellets is preferably as small as possible from the viewpoint of obtaining a molded body with few appearance defects and yellowing, but from the viewpoint of ease of pellet production, it can be, for example, 1 or more, or 3 or more, or 5 or more. That is, in one embodiment, the number ratio of void-containing pellets needs to be 10% by number or less, preferably 8% by number or less, more preferably 5% by number or less, even more preferably 3% by number or less, even more preferably 1% by number or less, and most preferably 0% by number.

[0016] In the pellet TD cross section, the ratio of the pore area to the cross section area (hereinafter also referred to as the pore area ratio) is preferably 4.0% or less, more preferably 2.5% or less, and even more preferably 1.0% or less, from the viewpoint of obtaining a molded product with few appearance defects and yellowing. The pore area ratio is a value obtained by the following method. First, for 100 randomly selected pellets, the pore-containing pellets are identified by the method disclosed herein. For the pore-containing pellets, the pore area in the TD cross section is measured using the attached software of a microscope, the ratio of the pore area to the total cross section area of ​​100% of the TD cross section is calculated, and the average value of the pore-containing pellets as a whole is taken as the pore area ratio. Note that the pore area ratio is taken as 0% when there is no pore-containing pellet among the 100 randomly selected pellets. The pore area ratio is preferably as low as possible from the viewpoint of obtaining a molded product with few defects and yellowing, and is most preferably 0%, but from the viewpoint of ease of production of the pellets, it can be, for example, 0.5% or more, 1.0% or more, or 2.0% or more. In a more preferred embodiment, the number of void-containing pellets per 100 pellets is 8 or less, or 5 or less, or 3 or less, and the void area ratio is within any of the above ranges. In a particularly preferred embodiment, the number of void-containing pellets per 100 pellets is 0 (hence, the void area ratio is 0%).

[0017] The shape of the pellets can be selected depending on the purpose, and typical examples include a sphere, an ellipsoid, a cylinder, an elliptical cylinder, etc. The shape of the pellet TD cross section is typically a circle (when the pellet is a sphere, a cylinder, etc.) or an ellipse (when the pellet is an ellipsoid, an elliptical cylinder, etc.), but it can also be a polygon (triangle, square, pentagon, hexagon, etc.), an irregular shape (star, C-shape, O-shape, etc.), etc.

[0018] In one embodiment, the minor axis of the pellet TD cross section may be, for example, 1 mm or more, or 2 mm or more, or 2.2 mm or more, or 2.5 mm or more, and, for example, 5 mm or less, or 4 mm or less, or 3 mm or less, in terms of facilitating mass production of pellets and molded bodies using the pellets. In the present disclosure, the minor axis of the pellet TD cross section means the maximum value of the diameters that the inscribed circle may have when the inscribed circle is drawn with respect to the outer shape of the pellet TD cross section (there may be one or more diameters depending on the shape of the pellet TD cross section). For example, when the pellet TD cross section is circular, the minor axis is the diameter of the circle, and when the pellet TD cross section is elliptical, the minor axis is the minor axis length of the ellipse.

[0019] As a more specific example, when the pellets are spherical or ellipsoidal, the minor axis of the pellet TD cross section is preferably 2 mm to 5 mm. When the pellets are cylindrical or elliptical cylindrical, the minor axis of the pellet TD cross section is preferably 2 mm to 5 mm, and the pellet MD length is preferably 2 mm to 5 mm. The above minor axis and length are preferably set to the lower limit or more from the viewpoint of operational stability during extrusion, and are preferably set to the upper limit or less from the viewpoint of biteability into a molding machine in post-processing.

[0020] FIG. 1 is a diagram for explaining a pellet cut surface, and FIGS. 2 and 3 are diagrams for explaining an embodiment in which the pellet cut surface is inclined. Referring to FIG. 1, when cutting a strand into pellets 1 (i.e., pelletizing), in many cases, the normal direction L1 of the cut surface S1 is approximately parallel to the strand MD direction L. However, depending on the production conditions, such as a condition in which the strand temperature is high during pelletizing, a condition in which a large-scale facility is used (i.e., a large amount of composition is discharged), and a condition in which the line speed is high, as shown in FIGS. 2 and 3, the normal directions L1 and L2 may be inclined (i.e., not approximately parallel) at angles θ1 and θ2 (note that these angles refer to the acute angle) with respect to the strand MD direction L. The pellet cut surface may be one surface such as the pellet cut surface S1 shown in FIG. 2, two surfaces such as the pellet cut surfaces S1 and S2 shown in FIG. 3, or three or more surfaces. In a typical embodiment, the pellet cut surface is substantially flat.

[0021] 2 and 3, in one embodiment, the angles θ1, θ2 of the normal directions S1, S2 of the pellet cut surfaces S1, S2 with respect to the pellet MD direction L may be 5° to 30° in terms of ease of mass production of pellets and moldings using the pellets. The pellet shape can be controlled relatively uniformly in small-scale production, but it is difficult to control it uniformly in mass production (for example, on a 100 kg / h scale). Pellets with the above angles of 5° to 30° are easy to mass-produce and are preferred. More preferably, the above angles may be 8° to 20°, or 10° to 15°. The above angles are values ​​obtained by the following method. First, each of ten randomly selected pellets is cut in a direction selected by visual observation so as to pass through the center of the pellet in the TD direction and maximize the inclination angle of the pellet cut surface described later, and further flattened with a microtome to obtain an MD cross section. The morphological image of this MD cross section is photographed with a microscope at a magnification of 20 times and an observation field of 10 mm x 14 mm. On the morphological image, the pellet MD direction axis and the normal to the line segment corresponding to the pellet MD end face are defined, and the angle between the pellet MD direction axis and the normal is measured. The number average value of 10 pellets is obtained as the pellet cut surface inclination angle.

[0022] The pellets contain a thermoplastic resin and cellulose nanofibers, and in one embodiment, may further contain any additional components. Examples of each component are described below.

[0023] ≪Thermoplastic resin≫ As the thermoplastic resin, various resins can be used, including crystalline resins having a melting point within the range of 100° C. to 350° C., and amorphous resins having a glass transition temperature within the range of 100° C. to 250° C. The thermoplastic resin may be composed of one or more types of polymers, which may be homopolymers or copolymers.

[0024] The melting point of the crystalline resin referred to here is the peak top temperature of the endothermic peak that appears when the temperature is increased from 23°C at a rate of 10°C / min using a differential scanning calorimeter (DSC). When two or more endothermic peaks appear, it refers to the peak top temperature of the endothermic peak on the highest temperature side. The enthalpy of the endothermic peak at this time is preferably 10 J / g or more, more preferably 20 J / g or more. In addition, when measuring, it is preferable to use a sample that is heated once to a temperature condition of the melting point + 20°C or more to melt the resin, and then cooled to 23°C at a rate of 10°C / min.

[0025] The glass transition temperature of the amorphous resin referred to here means the peak top temperature at which the storage modulus is greatly reduced and the loss modulus is maximized when measured using a dynamic viscoelasticity measuring device at a heating rate of 2°C / min from 23°C and an applied frequency of 10Hz. When two or more loss modulus peaks appear, it refers to the peak top temperature of the peak on the highest temperature side. In this case, the measurement frequency is preferably at least once every 20 seconds to improve the measurement accuracy. There is no particular restriction on the method of preparing the measurement sample, but from the viewpoint of eliminating the influence of molding distortion, it is preferable to use a cut piece of a hot press molded product, and it is preferable from the viewpoint of thermal conduction that the size (width and thickness) of the cut piece is as small as possible.

[0026] Examples of thermoplastic resins include polyamide-based resins, polyester-based resins, polyacetal-based resins, polycarbonate-based resins, polyacrylic-based resins, polyphenylene ether-based resins (including modified polyphenylene ethers obtained by blending or graft polymerizing polyphenylene ethers with other resins), polyarylate-based resins, polysulfone-based resins, polyphenylene sulfide-based resins, polyethersulfone-based resins, polyketone-based resins, polyphenylene ether ketone-based resins, polyimide-based resins, polyamideimide-based resins, polyetherimide-based resins, polyurethane-based resins, polyolefin-based resins (e.g., α-olefin (co)polymers), polyvinyl-based resins, and various ionomers.

[0027] These may be used alone or in combination of two or more. When two or more are used in combination, they may be used as a polymer alloy. In addition, the above-mentioned thermoplastic resin may be modified with at least one compound selected from unsaturated carboxylic acids, their acid anhydrides, or their derivatives.

[0028] Among these, from the viewpoints of heat resistance, moldability, designability, and mechanical properties, one or more resins selected from the group consisting of polyolefin resins, polyamide resins, polyester resins, polyacetal resins, polyacrylic resins, polyphenylene ether resins, and polyphenylene sulfide resins are preferred. In addition, when the thermoplastic resin is a polyamide resin and / or a polyolefin resin, the advantages of the pellet according to this embodiment are particularly significant, and are therefore preferred.

[0029] Polyolefin resins are polymers obtained by polymerizing monomer units containing olefins (e.g., α-olefins). Specific examples of polyolefin resins include, but are not limited to, ethylene (co)polymers exemplified by low-density polyethylene (e.g., linear low-density polyethylene), high-density polyethylene, ultra-low-density polyethylene, and ultra-high-molecular-weight polyethylene, polypropylene, poly-1-butene, poly-1-pentene, polymethylpentene, ethylene-α-olefin copolymers or modified products thereof (e.g., ethylene-propylene copolymer, ethylene-butene copolymer, and modified products thereof), copolymers of olefins (e.g., α-olefins) and other monomer units (e.g., ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid methyl ester copolymer, etc.), and copolymers of olefins (e.g., α-olefins) and other monomer units (e.g., ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid methyl ester copolymer, etc.). Examples of the polyolefin resin include polyolefins obtained by converting at least a part of the carboxyl groups of a copolymer of ethylene and / or propylene with an unsaturated carboxylic acid and / or an unsaturated carboxylic acid ester into a metal salt, halogenated isobutylene-paramethylstyrene copolymers, and modified products thereof. The polyolefin resin may be a cyclic olefin resin.

[0030] The most preferred polyolefin resin here is polypropylene. In particular, polypropylene having a melt mass flow rate (MFR) of 3 g / 10 min or more and 100 g / 10 min or less, measured at 230 ° C. and a load of 2.16 kgf according to ISO1133, is preferred. The lower limit of MFR is more preferably 5 g / 10 min, even more preferably 6 g / 10 min, and most preferably 8 g / 10 min. The upper limit is more preferably 75 g / 10 min, even more preferably 60 g / 10 min, and most preferably 40 g / 10 min. From the viewpoint of improving the toughness of the composition, it is desirable that MFR does not exceed the above upper limit, and from the viewpoint of the fluidity of the composition, it is desirable that MFR does not exceed the above lower limit.

[0031] In addition, in order to increase the affinity with cellulose, acid-modified polyolefin resins can also be suitably used. The acid can be appropriately selected from maleic acid, fumaric acid, succinic acid, phthalic acid and their anhydrides, polycarboxylic acids such as citric acid, etc. Among these, maleic acid or its anhydride is preferred because it is easy to increase the modification rate. There is no particular restriction on the modification method, but a method in which the resin is heated to a melting point or higher in the presence / absence of a peroxide and melt-kneaded is common. As the acid-modified polyolefin resin, all of the above-mentioned polyolefin resins can be used, but polypropylene is particularly suitable.

[0032] The acid-modified polyolefin resin may be used alone, but it is more preferable to use it in combination with an unmodified polyolefin resin in order to adjust the modification rate as a composition. For example, when a mixture of unmodified polypropylene and acid-modified polypropylene is used, the ratio of the acid-modified polypropylene to the total polypropylene is preferably 0.5% by mass to 50% by mass. A more preferable lower limit is 1% by mass, more preferably 2% by mass, even more preferably 3% by mass, particularly preferably 4% by mass, and most preferably 5% by mass. A more preferable upper limit is 45% by mass, more preferably 40% by mass, even more preferably 35% by mass, particularly preferably 30% by mass, and most preferably 20% by mass. In order to maintain the interfacial strength with cellulose, it is preferably the lower limit or more, and in order to maintain the ductility as a resin, it is preferably the upper limit or less. The lower limit of the acid modification rate of the acid-modified polyolefin resin is preferably 0.01% by mass, more preferably 0.1% by mass, even more preferably 0.3% by mass, particularly preferably 0.5% by mass, and most preferably 0.7% by mass. The upper limit is preferably 10% by mass, more preferably 5% by mass, even more preferably 3% by mass, particularly preferably 2% by mass, and most preferably 1.5% by mass. In order to maintain the interfacial strength with cellulose, the lower limit or more is preferable, and in order to maintain the mechanical properties of the acid-modified polyolefin, the upper limit or less is preferable.

[0033] The melt mass flow rate (MFR) of the acid-modified polypropylene, measured at 230°C and a load of 2.16 kgf according to ISO1133, is preferably 50 g / 10 min or more in order to enhance affinity with the cellulose interface. A more preferred lower limit is 100 g / 10 min, even more preferably 150 g / 10 min, and most preferably 200 g / 10 min. There is no particular upper limit, but it is 500 g / 10 min in order to maintain mechanical strength. By setting the MFR within this range, it is possible to enjoy the advantage that it is more likely to exist at the interface between cellulose and resin.

[0034] Examples of polyamide resins that are preferable as the thermoplastic resin include, but are not limited to, polyamide 6, polyamide 11, polyamide 12, etc., which are obtained by polycondensation reaction of lactams; diamines such as 1,6-hexanediamine, 2-methyl-1,5-pentanediamine, 1,7-heptanediamine, 2-methyl-1-6-hexanediamine, 1,8-octanediamine, 2-methyl-1,7-heptanediamine, 1,9-nonanediamine, 2-methyl-1,8-octanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, and m-xylylenediamine; and butanedioic acid, pentanedioic acid, hexanedioic acid, heptanedioic acid, octanedioic acid, etc. Examples of the copolymers include polyamide 6,6, polyamide 6,10, polyamide 6,11, polyamide 6,12, polyamide 6,T, polyamide 6,I, polyamide 9,T, polyamide 10,T, polyamide 2M5,T, polyamide MXD,6, polyamide 6,C, polyamide 2M5,C, etc., which are obtained as copolymers with dicarboxylic acids such as tanedioic acid, nonanedioic acid, decanedioic acid, benzene-1,2-dicarboxylic acid, benzene-1,3-dicarboxylic acid, benzene-1,4-dicarboxylic acid, cyclohexane-1,3-dicarboxylic acid, cyclohexane-1,4-dicarboxylic acid, etc.; and copolymers in which these are copolymerized (one example is polyamide 6,T / 6,I).

[0035] Among these polyamide resins, aliphatic polyamides such as polyamide 6, polyamide 11, polyamide 12, polyamide 6,6, polyamide 6,10, polyamide 6,11, and polyamide 6,12, and alicyclic polyamides such as polyamide 6,C and polyamide 2M5,C are more preferred.

[0036] Although there is no particular limitation on the terminal carboxyl group concentration of the polyamide resin, the lower limit is preferably 20 μmol / g, more preferably 30 μmol / g, and the upper limit of the terminal carboxyl group concentration is preferably 150 μmol / g, more preferably 100 μmol / g, and even more preferably 80 μmol / g.

[0037] In the polyamide resin, the ratio of the carboxyl end group to the total end groups ([COOH] / [total end groups]) is preferably 0.30 to 0.95. The lower limit of the carboxyl end group ratio is more preferably 0.35, even more preferably 0.40, and most preferably 0.45. The upper limit of the carboxyl end group ratio is more preferably 0.90, even more preferably 0.85, and most preferably 0.80. The carboxyl end group ratio is preferably 0.30 or more from the viewpoint of dispersibility in cellulose pellets, and is preferably 0.95 or less from the viewpoint of the color tone of the obtained resin composition.

[0038] The terminal group concentration of the polyamide resin can be adjusted by a known method, for example, by adding a terminal regulator that reacts with terminal groups, such as a diamine compound, a monoamine compound, a dicarboxylic acid compound, a monocarboxylic acid compound, an acid anhydride, a monoisocyanate, a monoacid halide, a monoester, or a monoalcohol, to the polymerization solution so that the terminal group concentration is a predetermined value during polymerization of the polyamide.

[0039] Examples of the terminal regulator that reacts with the terminal amino group include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthalenecarboxylic acid, β-naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid, and phenylacetic acid; and mixtures of a plurality of terminal regulators arbitrarily selected from the above. Among these, from the viewpoints of reactivity, stability of the blocked terminal, and price, one or more terminal regulators selected from the group consisting of acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, and benzoic acid are preferred, and acetic acid is most preferred.

[0040] Examples of the terminal regulator that reacts with the terminal carboxyl group include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, etc., alicyclic monoamines such as cyclohexylamine, dicyclohexylamine, etc., aromatic monoamines such as aniline, toluidine, diphenylamine, naphthylamine, etc., and any mixtures thereof. Among these, one or more terminal regulators selected from the group consisting of butylamine, hexylamine, octylamine, decylamine, stearylamine, cyclohexylamine, and aniline are preferred in terms of reactivity, boiling point, stability of the blocked terminal, price, etc.

[0041] The concentrations of these amino end groups and carboxyl end groups are as follows: 1 From the viewpoints of accuracy and simplicity, it is preferable to determine the concentration of each end group from the integral value of the characteristic signal corresponding to each end group by H-NMR. As a method for determining the concentration of these end groups, the method described in JP-A-7-228775 is specifically recommended. When using this method, deuterated trifluoroacetic acid is useful as a measurement solvent. 1 The number of H-NMR scans must be at least 300, even when an instrument with sufficient resolution is used. Alternatively, the concentration of the terminal group can be measured by a titration method as described in JP-A-2003-055549. However, in order to minimize the influence of additives, lubricants, etc., 1 Quantitation by H-NMR is more preferred.

[0042] The polyamide resin preferably has a viscosity number [VN] of 60 to 200 mL / g, more preferably 70 to 180 mL / g, further preferably 70 to 140 mL / g, and particularly preferably 70 to 120 mL / g, measured in concentrated sulfuric acid at 30° C. A polyamide resin having an intrinsic viscosity in the above range is advantageous in that it improves the flowability in a mold when a molded article is produced by injection molding of the resin composition, and improves the appearance of the molded article.

[0043] In this disclosure, "viscosity number" is an index of viscosity measured in 96% sulfuric acid according to ISO 307.

[0044] The polyester resin preferred as the thermoplastic resin is not particularly limited, but one or more selected from polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), polyarylate (PAR), polyhydroxyalkanoic acid (PHA) (polyester resin made of 3-hydroxyalkanoic acid), polylactic acid (PLA), polycarbonate (PC), etc. can be used. Among these, more preferred polyester resins include PET, PBS, PBSA, PBT, and PEN, and more preferably PBS, PBSA, and PBT.

[0045] In addition, the polyester resin can freely change the terminal group depending on the monomer ratio during polymerization and the presence or absence and amount of addition of a terminal stabilizer, but the carboxyl terminal group ratio ([COOH] / [total terminal groups]) to the total terminal groups of the polyester resin is preferably 0.30 to 0.95. The lower limit of the carboxyl terminal group ratio is more preferably 0.35, even more preferably 0.40, and most preferably 0.45. The upper limit of the carboxyl terminal group ratio is more preferably 0.90, even more preferably 0.85, and most preferably 0.80. The carboxyl terminal group ratio is preferably 0.30 or more from the viewpoint of dispersibility in cellulose pellets, and is preferably 0.95 or less from the viewpoint of the color tone of the obtained composition.

[0046] Polyacetal resins preferred as thermoplastic resins are homopolyacetals made from formaldehyde and copolyacetals containing trioxane as the main monomer and, for example, 1,3-dioxolane as a comonomer component. Both can be used, but from the viewpoint of thermal stability during processing, copolyacetals are preferably used. In particular, the amount of the comonomer component (for example, 1,3-dioxolane) is preferably within the range of 0.01 to 4 mol%. A more preferred lower limit of the amount of the comonomer component is 0.05 mol%, further preferably 0.1 mol%, and particularly preferably 0.2 mol%. A more preferred upper limit is 3.5 mol%, further preferably 3 mol%, particularly preferably 2.5 mol%, and most preferably 2.3 mol%. From the viewpoint of thermal stability during extrusion processing and molding processing, it is desirable to set the lower limit within the above-mentioned range, and from the viewpoint of mechanical strength, it is desirable to set the upper limit within the above-mentioned range.

[0047] Examples of vinyl resins preferred as thermoplastic resins include vinyl aliphatic (co)polymers (polyvinyl chloride, vinyl chloride-ethylene copolymers, and ethylene-vinyl acetate copolymers (which are also olefin resins) and saponified products thereof, etc.), vinyl aromatic (co)polymers (polystyrene, block copolymers of conjugated dienes and vinyl aromatic hydrocarbons, hydrogenated block copolymers of conjugated dienes and vinyl aromatic hydrocarbons, etc.), acrylic (co)polymers (poly(meth)acrylic acid esters, etc.), and acrylonitrile (co)polymers (acrylonitrile-butadiene-styrene (ABS) resins, acrylonitrile-styrene (AS) resins, etc.).

[0048] <Cellulose nanofiber> From the viewpoint of obtaining good dispersibility of the cellulose nanofibers in pellets or molded bodies, the fiber diameter of the cellulose nanofibers is preferably 50 nm or more, or 60 nm or more, or 70 nm or more, and from the viewpoint of obtaining a good effect of improving the physical properties of the molded body by the cellulose nanofibers, in one embodiment, it is 1000 nm or less, and preferably 600 nm or less, 400 nm or less, or 200 nm or less. The above fiber diameter is a value determined as the spherical equivalent diameter (volume average particle diameter) of the particles when the cumulative volume is 50% using a laser diffraction / scattering particle size distribution analyzer.

[0049] The fiber diameter can be measured by the following method. Cellulose nanofibers are mixed in a planetary mixer (e.g., 5DM-03-R, manufactured by Shinagawa Kogyosho Co., Ltd., with a hook-type stirring blade) at 126 rpm for 30 minutes at room temperature and normal pressure, then suspended in pure water at a concentration of 0.5% by mass, dispersed at a rotation speed of 15,000 rpm for 5 minutes using a high-shear homogenizer (e.g., Nippon Seiki Co., Ltd., trade name "Excel Auto Homogenizer ED-7", processing conditions), and centrifuged at a centrifugal force of 39,200 m. 2 The supernatant was collected after centrifugation at 116,000m / s for 10 minutes. 2 The mixture is centrifuged at 1000 / s for 45 minutes, and the supernatant after centrifugation is collected. The volume-frequency particle size distribution obtained using this supernatant with a laser diffraction / scattering particle size distribution analyzer (e.g., Horiba, Ltd., trade name "LA-910" or trade name "LA-950", ultrasonic treatment for 1 minute, refractive index 1.20) is determined to be the cumulative 50% particle size (i.e., the spherical equivalent diameter of the particles when the cumulative volume is 50% of the total volume of the particles) as the volume-average particle size.

[0050] The L / D ratio of the cellulose nanofibers in one embodiment is 30 or more, or 40 or more, or 50 or more, or 100 or more. There is no particular upper limit, but in one embodiment, from the viewpoint of handleability, it is 10,000 or less. In order to ensure that the molded article produced using the pellets of the present disclosure exhibits good mechanical properties with a small amount of cellulose nanofibers, it is desirable that the L / D ratio of the cellulose nanofibers be within the above-mentioned range.

[0051] In the present disclosure, the length (L) and diameter (D) of each of the cellulose nanofibers and cellulose nanocrystals and cellulose microfibers (hereinafter also referred to as cellulose components) as optional additional components, and the L / D ratio calculated from these, are obtained by dispersing an aqueous dispersion of the cellulose component using a high-shear homogenizer (for example, Nippon Seiki Co., Ltd., product name "Excel Auto Homogenizer ED-7") under processing conditions: rotation speed 15,000 rpm x 5 minutes, diluting the aqueous dispersion with pure water to 0.1 to 0.5 mass%, casting it on mica, and air-drying it as a measurement sample, and measuring it with an optical microscope, a high-resolution scanning microscope (SEM), or an atomic force microscope (AFM). Specifically, the length (L) and diameter (D) of 100 randomly selected cellulose components are measured in an observation field where the magnification is adjusted so that at least 100 cellulose components are observed, and the (L / D) ratio is calculated. The number average values ​​for the 100 cellulose fibers are defined as the length (L), diameter (D) and (L / D) ratio.

[0052] The cellulose nanofiber may be cellulose obtained by treating pulp or the like with hot water of 100°C or higher to hydrolyze and weaken the hemicellulose portion, and then defibrating the cellulose by a pulverization method using a high-pressure homogenizer, microfluidizer, ball mill, disc mill, or the like.

[0053] In one embodiment, the cellulose nanofibers may be modified (i.e., modified cellulose nanofibers). Examples of modified cellulose nanofibers include those in which cellulose is modified with one or more modifying agents selected from an esterifying agent, a silylating agent, an isocyanate compound, a halogenated alkylating agent, an alkylene oxide, and / or a glycidyl compound. In a preferred embodiment, the cellulose nanofibers are unmodified or modified without an oxoacid-modifying group (i.e., a site in which the hydroxyl group of cellulose is converted with an oxoacid (e.g., a carboxylic acid) or a salt thereof (e.g., a carboxylate)), and preferred examples of the modified cellulose nanofibers are those modified with the modifying agents listed above. The esterifying agent as the modifying agent includes an organic compound having at least one functional group that can react with the hydroxyl group on the surface of the cellulose nanofiber to esterify it. The esterification can be carried out by the method described in paragraph

[0108] of WO 2017 / 159823. The esterifying agent may be a commercially available reagent or product.

[0054] Suitable examples of the esterifying agent include, but are not limited to, aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthalenecarboxylic acid, β-naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid, and phenylacetic acid; and mixtures of any of these acids, and esters of these acids with vinyl alcohol (for example, vinyl acetate, vinyl propionate, and butyric acid). vinyl, vinyl valerate, vinyl caproate, vinyl caprylate, vinyl laurate, etc.), as well as symmetric anhydrides (e.g., acetic anhydride, maleic anhydride, cyclohexane-carboxylic anhydride, benzene-sulfonic anhydride), mixed acid anhydrides (e.g., butyric anhydride-valeric anhydride), cyclic anhydrides (e.g., succinic anhydride, phthalic anhydride, naphthalene-1,8:4,5-tetracarboxylic dianhydride, cyclohexane-1,2,3,4-tetracarboxylic 3,4-anhydride), ester acid anhydrides (e.g., acetic acid 3-(ethoxycarbonyl)propanoic anhydride, benzoylethyl carbonate), etc., selected arbitrarily from the above-mentioned acids.

[0055] Among these, from the standpoint of reactivity, stability, cost, etc., acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, esters of these acids with vinyl alcohol, benzoic acid, acetic anhydride, maleic anhydride, succinic anhydride, and phthalic anhydride can be preferably used.

[0056] The silylating agent as a modifier includes a Si-containing compound having at least one reactive group capable of reacting with the hydroxyl group on the surface of cellulose or the group after hydrolysis thereof. The silylating agent may be a commercially available reagent or product.

[0057] Suitable examples of the silylating agent include, but are not limited to, chlorodimethylisopropylsilane, chlorodimethylbutylsilane, chlorodimethyloctylsilane, chlorodimethyldodecylsilane, chlorodimethyloctadecylsilane, chlorodimethylphenylsilane, chloro(1-hexenyl)dimethylsilane, dichlorohexylmethylsilane, dichloroheptylmethylsilane, trichlorooctylsilane, hexamethyldisilazane, 1,3-divinyl-1,1,3,3-tetramethyldisilazane, 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisilazane, 1,3-N-dioctyltetramethyldisilazane, and the like. Examples of the silane include diisobutyltetramethyldisilazane, diethyltetramethyldisilazane, N-dipropyltetramethyldisilazane, N-dibutyltetramethyldisilazane, 1,3-di(para-t-butylphenethyl)tetramethyldisilazane, N-trimethylsilylacetamide, N-methyldiphenylsilylacetamide, N-triethylsilylacetamide, t-butyldiphenylmethoxysilane, octadecyldimethylmethoxysilane, dimethyloctylmethoxysilane, octylmethyldimethoxysilane, octyltrimethoxysilane, trimethylethoxysilane, and octyltriethoxysilane.

[0058] Among these, hexamethyldisilazane, octadecyldimethylmethoxysilane, dimethyloctylmethoxysilane, and trimethylethoxysilane are preferably used in terms of reactivity, stability, cost, and the like.

[0059] The halogenated alkylating agent as a modifying agent includes an organic compound having at least one functional group capable of reacting with the hydroxyl groups on the surface of the cellulose to halogenated alkylate it. The halogenated alkylating agent may be a commercially available reagent or product.

[0060] Suitable examples of the halogenated alkylating agent include, but are not limited to, chloropropane, chlorobutane, bromopropane, bromohexane, bromoheptane, iodomethane, iodoethane, iodooctane, iodooctadecane, iodobenzene, etc. Among these, bromohexane and iodooctane are preferably used in terms of reactivity, stability, cost, etc.

[0061] The isocyanate compound as a modifier includes an organic compound having at least one isocyanate group capable of reacting with a hydroxyl group on the surface of cellulose. The isocyanate compound may be a blocked isocyanate compound capable of regenerating an isocyanate group by removing a blocking group at a specific temperature, or may be a dimer or trimer of polyisocyanate, a modified product such as biuretized isocyanate, polymethylene polyphenyl polyisocyanate (polymeric MDI), etc. These may be commercially available reagents or products.

[0062] Suitable examples of the isocyanate compound include, but are not limited to, aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic polyisocyanates, araliphatic polyisocyanates, blocked isocyanate compounds, polyisocyanates, and the like. For example, tetramethylene diisocyanate, dodecamethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2-methylpentane-1,5-diisocyanate, 3-methylpentane-1,5-diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane), tolylene diisocyanate (TDI), 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, anate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate), dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, α,α,α,α-tetramethylxylylene diisocyanate, blocked isocyanate compounds obtained by reacting the above-mentioned isocyanate compounds with an oxime-based blocking agent, a phenol-based blocking agent, a lactam-based blocking agent, an alcohol-based blocking agent, an active methylene-based blocking agent, an amine-based blocking agent, a pyrazole-based blocking agent, a bisulfite-based blocking agent, or an imidazole-based blocking agent, and the like.

[0063] Among these, TDI, MDI, hexamethylene diisocyanate, and blocked isocyanates made from modified hexamethylene diisocyanate and hexamethylene diisocyanate are preferably used from the standpoints of reactivity, stability, cost, and the like.

[0064] From the viewpoints of reactivity and stability, the upper limit of the dissociation temperature of the blocking group of the blocked isocyanate compound is preferably 210° C., more preferably 190° C., and even more preferably 150° C. The lower limit is preferably 70° C., more preferably 80° C., and even more preferably 110° C. Examples of blocking agents that have a dissociation temperature of the blocking group within this range include methyl ethyl ketone oxime, ortho-secondary butylphenol, caprolactam, sodium bisulfite, 3,5-dimethylpyrazole, and 2-methylimidazole.

[0065] The alkylene oxide and / or glycidyl compound as the modifier includes an organic compound having at least one alkylene oxide group, glycidyl group and / or epoxy group capable of reacting with the hydroxyl group on the surface of the cellulose. The alkylene oxide and / or glycidyl compound may be a commercially available reagent or product.

[0066] Suitable examples of the alkylene oxide and / or glycidyl compound include, but are not limited to, glycidyl ethers such as methyl glycidyl ether, ethyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, 2-methyloctyl glycidyl ether, phenyl glycidyl ether, p-tertiary butylphenyl glycidyl ether, sec-butylphenyl glycidyl ether, n-butylphenyl glycidyl ether, phenylphenol glycidyl ether, cresyl glycidyl ether, and dibromocresyl glycidyl ether; glycidyl esters such as glycidyl acetate and glycidyl stearate; ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, and the like; Examples of polyhydric alcohol glycidyl ethers include polyhydric alcohol glycidyl ethers such as glycerol diglycidyl ether, 1,4-butanediol diglycidyl ether, hexamethylene glycol diglycidyl ether, resorcinol diglycidyl ether, bisphenol A diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, polybutylene glycol diglycidyl ether, glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol tetraglycidyl ether, sorbitol polyglycidyl ether, sorbitan polyglycidyl ether, polyglycerol polyglycidyl ether, and diglycerol polyglycidyl ether.

[0067] Among these, 2-methyloctyl glycidyl ether, hexamethylene glycol diglycidyl ether, and pentaerythritol tetraglycidyl ether are preferably used in terms of reactivity, stability, cost, and the like.

[0068] In one embodiment, the cellulose nanofiber is a hydrophobized cellulose nanofiber. The above-mentioned exemplified modifiers can be suitably used to produce the hydrophobized cellulose nanofiber. Among them, the hydrophobized cellulose nanofiber is preferably an acetylated cellulose nanofiber.

[0069] The content of cellulose nanofibers in the pellets is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 3% by mass or more, and particularly preferably 5% by mass or more, from the viewpoint of obtaining the desired property-improving effect of the cellulose nanofibers on the molded body while maintaining good dispersibility of the cellulose nanofibers in the pellets or molded body and obtaining the desired property-improving effect of the cellulose nanofibers, and from the viewpoint of production costs, the content is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less.

[0070] <Additional Ingredients> The pellet may optionally contain additional components in addition to the thermoplastic resin and cellulose nanofibers. Examples of the additional components include cellulose nanocrystals, cellulose microfibers, elastomers, surface treatment agents, compatibilizers, plasticizers, colorants, pigments, flow control agents, antioxidants, UV absorbers, UV dispersants, inorganic fillers, lubricants, etc. These components may be used alone or in combination of two or more. These components may also be commercially available reagents or products.

[0071] <Cellulose nanocrystals and cellulose microfibers> In a preferred embodiment, the additional component comprises cellulose nanocrystals having a diameter of 100 nm or less and L / D of less than 30, or cellulose microfibers having a fiber diameter of more than 1 μm to 50 μm, or a mixture thereof.

[0072] The diameter of the cellulose nanocrystals is, in one embodiment, 100 nm or less, or 80 nm or less, or 70 nm or less, and in one embodiment, 3 nm or more, or 5 nm or more, or 10 nm or more. The L / D of the cellulose nanocrystals is, in one embodiment, less than 30, or 20 or less, or 15 or less, or 10 or less, and in one embodiment, 1 or more, or 2 or more, or 4 or more, or 5 or more.

[0073] The fiber diameter of the cellulose microfiber is, in one embodiment, more than 1 μm, or 2 μm or more, or 5 μm or more, or 10 μm or more, and in one embodiment, 50 μm or less, or 45 μm or less, or 40 μm or less, or 30 μm or less, or 20 μm or less, or 15 μm or less. The L / D ratio of the cellulose microfiber is, in one embodiment, 30 or more, or 50 or more, or 70 or more, and in one embodiment, 2000 or less, or 1000 or less, or 500 or less.

[0074] In one embodiment, the cellulose nanocrystals and / or cellulose microfibers may be modified. Examples of the modifications may be the same as those described above for the cellulose nanofibers.

[0075] <Elastomer> In the present disclosure, elastomer means a material (specifically, a natural or synthetic polymer material) that is elastic at room temperature (23°C). Specific examples of elastomers include natural rubber, conjugated diene compound polymers, aromatic compound-conjugated diene copolymers, hydrogenated aromatic compound-conjugated diene copolymers, polyolefin-based elastomers, polyester-based elastomers, polyurethane-based elastomers, polyamide-based elastomers, and elastomers having a core-shell structure. In one embodiment, the elastomer is a polymer different from a thermoplastic resin. Among these, aromatic compound-conjugated diene copolymers, hydrogenated aromatic compound-conjugated diene copolymers, polyolefin-based elastomers, and elastomers having a core-shell structure are preferred from the viewpoint of ease of modification reaction to obtain elastomers having acidic functional groups, which will be described later. Furthermore, among aromatic compound-conjugated diene copolymers and hydrogenated products of aromatic compound-conjugated diene copolymers, aromatic compound-conjugated diene block copolymers and hydrogenated products of aromatic compound-conjugated diene block copolymers are more preferred, and among polyolefin-based elastomers, copolymers of ethylene and α-olefins are more preferred.

[0076] The aromatic compound-conjugated diene block copolymer referred to here is a block copolymer composed of a polymer block (A) mainly made of an aromatic vinyl compound and a polymer block (B) mainly made of a conjugated diene compound. Block copolymers in which the bonding type of each block is either AB type, ABA type, or ABAB type are preferred from the viewpoint of impact strength expression, and ABA type or ABAB type is more preferred.

[0077] The mass ratio of the aromatic vinyl compound to the conjugated diene compound in the block copolymer is preferably 10 / 90 to 70 / 30. More preferably, it is 15 / 85 to 55 / 45, and most preferably 20 / 80 to 45 / 55. Furthermore, these may be blended with two or more compounds having different mass ratios of the aromatic vinyl compound to the conjugated diene compound. Specific examples of the aromatic vinyl compound include styrene, α-methylstyrene, vinyltoluene, etc., and one or more compounds selected from these are used, among which styrene is particularly preferred.

[0078] Specific examples of the conjugated diene compound include butadiene, isoprene, piperylene, 1,3-pentadiene, etc., and one or more compounds selected from these are used, but among these, butadiene, isoprene, and combinations thereof are preferred. When butadiene is used as the conjugated diene compound of the block copolymer, the microstructure of the polybutadiene block portion preferably has a 1,2-vinyl content or a total amount of the 1,2-vinyl content and the 3,4-vinyl content of 5 to 80% on a molar basis, more preferably 10 to 50%, and most preferably 15 to 40%, from the viewpoint of suppressing crystallization of the soft segment.

[0079] The hydrogenated block copolymer of an aromatic vinyl compound and a conjugated diene compound refers to a block copolymer of an aromatic vinyl compound and a conjugated diene compound, which is hydrogenated to control the aliphatic double bonds of the polymer block mainly composed of a diene compound to a range of more than 0% to 100%. From the viewpoint of suppressing thermal degradation during processing, the hydrogenation rate of the hydrogenated block copolymer is preferably 50% or more, more preferably 80% or more, and most preferably 98% or more.

[0080] From the viewpoint of both impact strength and fluidity, the molecular weight of each of the block copolymer of an aromatic vinyl compound and a conjugated diene compound and its hydrogenated product is preferably a number average molecular weight (Mn) of 10,000 to 500,000, and most preferably 40,000 to 250,000. The number average molecular weight referred to here is a value measured by a GPC apparatus using chloroform as an elution solvent at a measurement temperature of 40°C, and converted into a polystyrene standard polymer.

[0081] These aromatic vinyl compound-conjugated diene compound block copolymers may be used in combination of two or more types having different bonding forms, different molecular weights, different aromatic vinyl compound types, different conjugated diene compound types, different 1,2-vinyl contents or the total amount of 1,2-vinyl content and 3,4-vinyl content, different aromatic vinyl compound component contents, different hydrogenation rates, etc.

[0082] As the polyolefin elastomer, from the viewpoint of impact resistance, ethylene-α-olefin copolymers can be suitably used. Examples of monomers that can be copolymerized with ethylene units include aliphatic substituted vinyl monomers such as propylene, butene-1, pentene-1, 4-methylpentene-1, hexene-1, heptene-1, octene-1, nonene-1, decene-1, undecene-1, dodecene-1, tridecene-1, tetradecene-1, pentadecene-1, hexadecene-1, heptadecene-1, octadecene-1, nonadecene-1, or eicosene-1, isobutylene, and aromatic vinyl monomers such as styrene and substituted styrene, ester vinyl monomers such as vinyl acetate, acrylic acid esters, methacrylic acid esters, glycidyl acrylic acid esters, glycidyl methacrylic acid esters, and hydroxyethyl methacrylic acid esters, acrylamide, allylamine, vinyl-p-aminobenzene, and nitrogen-containing vinyl monomers such as acrylonitrile, and dienes such as butadiene, cyclopentadiene, 1,4-hexadiene, and isoprene.

[0083] Preferably, it is a copolymer of ethylene and one or more α-olefins having 3 to 20 carbon atoms, more preferably a copolymer of ethylene and one or more α-olefins having 3 to 16 carbon atoms, and most preferably a copolymer of ethylene and one or more α-olefins having 3 to 12 carbon atoms. From the viewpoint of impact resistance, the molecular weight of the ethylene-α-olefin copolymer is preferably 10,000 or more, more preferably 10,000 to 100,000, and even more preferably 20,000 to 60,000, as measured by a gel permeation chromatography measuring device using 1,2,4-trichlorobenzene as a solvent at 140°C and using polystyrene standards. From the viewpoint of impact resistance, the molecular weight distribution (weight average molecular weight / number average molecular weight: Mw / Mn) is preferably 3 or less, and even more preferably 1.8 to 2.7.

[0084] Moreover, the preferred content of ethylene units in the ethylene-α-olefin copolymer is 30 to 95% by mass based on the total amount of the ethylene-α-olefin copolymer, from the viewpoint of ease of handling during processing.

[0085] These preferred ethylene-α-olefin copolymers can be produced, for example, by the production methods described in JP-B-4-12283, JP-A-60-35006, JP-A-60-35007, JP-A-60-35008, JP-A-5-155930, JP-A-3-163088, and U.S. Pat. No. 5,272,236.

[0086] In the present disclosure, the elastomer having a core-shell structure includes a core-shell type impact modifier having a core that is a particulate rubber and a shell that is a glassy graft layer formed on the outside of the core. As the rubber component as the core, butadiene rubber, acrylic rubber, silicone-acrylic composite rubber, etc. can be suitably used. In addition, glassy polymers such as styrene resin, acrylonitrile-styrene copolymer, acrylic resin, etc. can be suitably used for the shell. For example, when the thermoplastic resin is a polyamide resin, an elastomer having a core-shell structure having a butadiene rubber core and an acrylic resin shell can be suitably used from the viewpoint of compatibility with the polyamide.

[0087] In one embodiment, at least a part of the elastomer has an acidic functional group. In the present disclosure, the term "an elastomer has an acidic functional group" means that the acidic functional group is added to the molecular skeleton of the elastomer via a chemical bond. In the present disclosure, the term "acidic functional group" means a functional group capable of reacting with a basic functional group, and specific examples include a hydroxyl group, a carboxyl group, a carboxylate group, a sulfo group, and an acid anhydride group. When at least a part of the elastomer has an acidic functional group, the affinity between the elastomer and the cellulose nanofibers is high, which is preferable.

[0088] When the elastomer has acidic functional groups, the amount of the acidic functional groups added in the elastomer is, from the viewpoint of affinity with cellulose nanofibers, preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.2% by mass or more, and preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less, based on 100% by mass of the elastomer. The number of acidic functional groups is a value obtained by measuring a calibration curve sample, in which an acidic substance has been mixed in advance, with an infrared absorption spectrometer, and measuring the sample based on a calibration curve that has been prepared using the characteristic absorption band of the acid.

[0089] Examples of elastomers having an acidic functional group include elastomers having a core-shell structure having a shell layer formed using acrylic acid or the like as a copolymerization component, and elastomers which are modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof to an ethylene-α-olefin copolymer, polyolefin, aromatic compound-conjugated diene copolymer, or a hydrogenated product of an aromatic compound-conjugated diene copolymer, containing acrylic acid or the like as a monomer, in the presence or absence of a peroxide.

[0090] In a preferred embodiment, the elastomer is an anhydride modified elastomer.

[0091] Among these, modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof in the presence or absence of a peroxide onto a polyolefin elastomer, an aromatic compound-conjugated diene copolymer, or a hydrogenated product of an aromatic compound-conjugated diene copolymer are more preferred, and among these, modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof in the presence or absence of a peroxide onto an ethylene-α-olefin copolymer or a hydrogenated product of an aromatic compound-conjugated diene block copolymer are particularly preferred.

[0092] Specific examples of the α,β-unsaturated dicarboxylic acid and its derivatives include maleic acid, fumaric acid, maleic anhydride, and fumaric anhydride, with maleic anhydride being particularly preferred.

[0093] When the elastomer has an acidic functional group, the elastomer may be a mixture of an elastomer having an acidic functional group and an elastomer not having an acidic functional group. The mixing ratio of the elastomer having an acidic functional group and the elastomer not having an acidic functional group, when the total of the two is 100 mass%, is preferably 10 mass% or more, more preferably 20 mass% or more, even more preferably 30 mass% or more, and most preferably 40 mass% or more, from the viewpoint of maintaining high toughness and physical property stability of the resin composition. There is no particular upper limit, and substantially all of the elastomer may be an elastomer having an acidic functional group, but from the viewpoint of not causing problems in flowability, it is desirable to have 80 mass% or less.

[0094] In the resin composition, the amount of the elastomer relative to 100 parts by mass of the thermoplastic resin is preferably within the range of 1 to 50 parts by mass. The upper limit is more preferably 40 parts by mass, more preferably 35 parts by mass, even more preferably 30 parts by mass, and most preferably 25 parts by mass. In order to maintain good rigidity and heat resistance of the resin composition, it is desirable to set the amount below the above upper limit. The lower limit is more preferably 2 parts by mass, even more preferably 3 parts by mass, even more preferably 4 parts by mass, and most preferably 5 parts by mass. In order to increase the toughness and physical property stability of the resin composition, it is preferable to set the amount above the above lower limit.

[0095] When the elastomer phase forms a particulate dispersed phase (dispersed particles) in the resin composition, the dispersed particle diameter is preferably 3 μm or less, more preferably 2 μm or less, and most preferably 1 μm or less, as a number average particle diameter. There is no particular lower limit, but it is, for example, 0.1 μm. From the viewpoint of high toughness and physical property stability, it is preferable to set it within the above range.

[0096] It is preferable that the elastomer has a high uniformity of the dispersed particle diameter. From this viewpoint, it is preferable that the volume ratio of dispersed particles having a particle diameter of 1 μm or more to the total dispersed particles of the elastomer is 30 volume % or less. The upper limit is more preferably 25 volume %, further preferably 20 volume %, even more preferably 15 volume %, and most preferably 10 volume %. In the volume-based dispersed particle diameter distribution, even if there are only a few coarse particles, the volume ratio of dispersed particles having a particle diameter of 1 μm or more is suddenly expressed as being large. When the above volume ratio is within the above range, the uniformity of the dispersed particle diameter is high, which is preferable. From the viewpoint of ease of production of the resin composition, the above volume ratio may be, for example, 2 volume % or more, or 5 volume % or more.

[0097] Methods for improving the uniformity of the dispersed particle size of the elastomer include a method of producing a resin composition by extrusion kneading the compounding components of the resin composition, and finely dispersing the elastomer by increasing the screw rotation speed during extrusion kneading to impart high shear strain to the compounding components, a method of imparting extensional flow strain to the compounding components by arranging screw parts with uniformly distributed narrow clearances, such as seal rings, and a method of passing a molten polymer through a special narrow slit and imparting extensional flow strain at the slit. Any of these methods may be used, but since the method of imparting high shear causes a significant rise in the polymer temperature during processing, the method using extensional flow strain is more preferable.

[0098] Methods for observing the dispersion form include cutting a resin composition in the form of a molded body, pellets, etc. into ultrathin slices, staining the thermoplastic resin phase with phosphotungstic acid, etc., and observing it with a transmission electron microscope, and a method for uniformly leveling the surface of a resin composition in the form of a molded body, pellets, etc., immersing it in a solvent that selectively dissolves only the elastomer, extracting the elastomer, and observing it with a scanning electron microscope. The obtained image is binarized with an image analyzer, and the diameters of the dispersed particles (at least 500 randomly selected) in the dispersed phase are calculated as the equivalent circle diameter, and the particle diameters of each particle are counted, so that the number average particle diameter of the dispersed particles and the volume ratio of particles with a predetermined particle diameter (for example, the above-mentioned particle diameter of 1 μm or more) can be calculated.

[0099] <Surface treatment agent> Suitable examples of the surface treatment agent include compounds having a hydrophilic segment and a hydrophobic segment in the molecule. More specifically, examples of the surface treatment agent include copolymers (e.g., block copolymers of propylene oxide and ethylene oxide, block copolymers of tetrahydrofuran and ethylene oxide) obtained by using one or more compounds that provide hydrophilic segments (e.g., polyethylene glycol) and one or more compounds that provide hydrophobic segments (e.g., polypropylene glycol, poly(tetramethylene ether) glycol (PTMEG), polybutadiene diol, etc.).

[0100] The preferred content of the surface treatment agent in the pellets is, from the viewpoint of increasing the dispersibility of the cellulose nanofibers in the pellets, preferably 0.1% by mass or more, or 0.2% by mass or more, or 0.5% by mass or more, and from the viewpoint of suppressing plasticization of the molded body and maintaining good strength, preferably 50% by mass or less, or 30% by mass or less, or 20% by mass or less, or 18% by mass or less, or 15% by mass or less, or 10% by mass or less, or 5% by mass or less.

[0101] The preferred amount of surface treatment agent per 100 parts by mass of cellulose nanofiber is, from the viewpoint of increasing the dispersibility of the cellulose nanofiber in the pellet, preferably 0.1 parts by mass or more, or 0.5 parts by mass or more, or 1 part by mass or more, and from the viewpoint of suppressing plasticization of the molded body and maintaining good strength, preferably 100 parts by mass or less, or 99 parts by mass or less, or 90 parts by mass or less, or 80 parts by mass or less, or 70 parts by mass or less, or 50 parts by mass or less, or 40 parts by mass or less.

[0102] <Antioxidants> As the antioxidant, from the viewpoint of the effect of preventing deterioration due to heat, a hindered phenol-based antioxidant, a sulfur-based antioxidant, or a phosphorus-based antioxidant is preferable, a phosphorus-based antioxidant and a hindered phenol-based antioxidant are more preferable, and a combination of a phosphorus-based antioxidant and / or a hindered phenol-based antioxidant with a hindered amine light stabilizer (HALS) is even more preferable.

[0103] A preferred amount of the antioxidant is, based on the total weight of the pellet, preferably 0.01% by weight or more, or 0.02% by weight or more, or 0.03% by weight or more, or 0.05% by weight or more, and preferably 5% by weight or less, or 4% by weight or less, or 3% by weight or less, or 2% by weight or less, or 1% by weight or less.

[0104] <Inorganic fillers> Examples of the inorganic filler include fibrous particles, plate-like particles, inorganic pigments, etc. The fibrous particles and plate-like particles may have an average aspect ratio of 5 or more. The amount of the inorganic filler in the pellets is preferably 0.002 parts by mass to 50 parts by mass relative to 100 parts by mass of the thermoplastic resin, from the viewpoint of improving the handleability when molding the pellets into a molded article.

[0105] <Lubricating oil> Examples of lubricating oils include natural oils (engine oils, cylinder oils, etc.), synthetic hydrocarbons (paraffinic oils, naphthenic oils, aromatic oils, etc.), silicone oils, etc. The molecular weight of the lubricating oil may be, for example, 100 or more, or 400 or more, or 500 or more, and may be, for example, 5 million or less, or 2 million or less, or 1 million or less.

[0106] The melting point of the lubricating oil may be, for example, −50° C. or higher, or −30° C. or higher, or −20° C. or higher, and may be, for example, 50° C. or lower, or 30° C. or lower, or 20° C. or lower. The melting point is 2.5° C. lower than the pour point of the lubricating oil, and the pour point can be measured in accordance with JIS K2269.

[0107] The content of the lubricating oil per 100 parts by mass of the thermoplastic resin is preferably 0.1 parts by mass or more, or 0.2 parts by mass or more, or 0.3 parts by mass or more from the viewpoint of improving wear resistance, and is preferably 5.0 parts by mass or less, or 4.5 parts by mass or less, or 4.2 parts by mass or less from the viewpoint of avoiding undesirable softening of the molded body.

[0108] The total amount of additional components in the pellets may be, for example, 0.01% by weight or more, or 0.1% by weight or more, or 1% by weight or more, and may be, for example, 20% by weight or less, or 10% by weight or less, or 5% by weight or less.

[0109] In a preferred embodiment, the pellets contain 50% to 99% by mass of a thermoplastic resin, 1% to 30% by mass of cellulose nanofibers, and 0.01% to 20% by mass of additional components. In another preferred embodiment, the pellets contain 70% to 99% by mass of a thermoplastic resin, 1% to 10% by mass of cellulose nanofibers, and 0.01% to 30% by mass of additional components, or 75% to 99% by mass of a thermoplastic resin, 1% to 5% by mass of cellulose nanofibers, and 0.01% to 20% by mass of additional components.

[0110] <Resin crystallization temperature lowering agent> The crystallization temperature lowering agent of the present disclosure is a compound that lowers the temperature-lowering crystallization peak temperature of the resin composition of the present disclosure by 5 to 30°C as measured by a differential scanning calorimeter (DSC) (i.e., the resin composition containing the crystallization temperature lowering agent has a temperature-lowering crystallization peak temperature that is 5 to 30°C lower than the same resin composition that does not contain the crystallization temperature lowering agent). The temperature-lowering crystallization peak temperature is preferably lowered by 5°C to 25°C or 10°C to 20°C by the crystallization temperature lowering agent. The temperature-lowering crystallization peak temperature of the present disclosure is the peak top temperature of the crystallization peak when the thermoplastic resin is a crystalline resin and the thermoplastic resin is heated to a melting point +30°C at a heating rate of 10°C / min, or to a glass transition point +30°C at a heating rate of 10°C / min, and then cooled at a rate of 10°C / min using DSC. By using the crystallization temperature lowering agent, when the thermoplastic resin and cellulose nanofibers are melt-mixed and then cooled to produce pellets of the resin composition, the crystallization of the resin composition due to cooling can be promoted slowly, and voids within the pellets can be reduced.

[0111] Examples of the crystallization temperature lowering agent include pentaerythritol, dipentaerythritol, trimethylolethane, nigrosine, etc., and pentaerythritol is particularly preferred.

[0112] The mass ratio of the crystallization temperature lowering agent relative to 100 mass% of the resin composition is preferably 0.01 mass% to 10 mass%, or 0.05 mass% to 5 mass%, or 0.8 mass% to 3 mass%.

[0113] [Properties of resin composition] In one aspect, the difference Tcc-Tcp between the cooling-down crystallization peak temperature Tcc of the resin composition and the cooling-down crystallization peak temperature Tcp of the thermoplastic resin contained in the resin composition (the highest peak temperature when multiple types of thermoplastic resins with different cooling-down crystallization peak temperatures are present) is preferably 5° C. to 30° C., or 5° C. to 25° C., or 10° C. to 20° C. In a resin composition having a Tcc-Tcp in the above range, crystallization due to cooling of the resin composition tends to proceed easily when the thermoplastic resin and the cellulose nanofiber are melt-mixed and then cooled to produce pellets of the resin composition, but the resin composition of the present embodiment has reduced voids in the pellets even in such a resin composition.

[0114] In one embodiment, the ratio Ve / Vc of the pores (Ve) in the pellets to the total volume (Vc) of the cellulose nanofibers per 100 pellets is preferably 0% to 4% by volume, or 0% to 3% by volume, or 0% to 1% by volume, from the viewpoint of obtaining pellets with less voids compared to the amount of cellulose nanofibers used. Ve / Vc is calculated by the following formula. Ve / Vc = (pore area ratio × pore-containing pellet ratio) / (cellulose volume ratio when pores are not present × (100-pore area ratio × pore-containing pellet ratio / 100)) × 100 The volume ratio of cellulose in the absence of pores is calculated from the amount of each component added to the resin composition and the density.

[0115] [Pellet production] The pellets of the present disclosure can be produced, for example, by using a single-screw or twin-screw extruder to melt-knead a thermoplastic resin, cellulose nanofibers, and any additional components, extrude them into strands, and cool and solidify them in a water bath to obtain pellets. Examples of the method for melt-kneading a thermoplastic resin, cellulose nanofibers, and any additional components include the following methods. (1) A method of melt-kneading a thermoplastic resin, cellulose nanofibers, and any additional components all at once. (2) A method in which a thermoplastic resin and, if necessary, any additional components are melt-kneaded, and then cellulose nanofibers and, if necessary, any additional components are added, and the mixture is further melt-kneaded. (3) A method in which a thermoplastic resin, cellulose nanofibers, and any additional components are melt-kneaded, and then the cellulose nanofibers and water, and any additional components as necessary, are mixed, and then the whole is melt-kneaded. (4) A method in which a thermoplastic resin and, if necessary, any additional components are melt-kneaded, and then the thermoplastic resin and cellulose nanofibers mixed in a desired ratio, as well as any additional components, are added and further melt-kneaded. (5) The above components (1) to (4) are added in any ratio in separate portions to the top and side of a single-screw or twin-screw extruder, and melt-kneaded.

[0116] In the extruder, the properties of the pellets can be changed by controlling the melt temperature, screw diameter, resin discharge rate, number of die holes, die hole diameter, etc., and by controlling the cooling conditions of the strands discharged from the extruder, such as the air-cooling distance between the extruder die and the water surface of the strand bath, the strand bath temperature, the strand bath immersion length, the strand take-up speed, etc. From the viewpoint of reducing pellets containing voids, it is useful to control the melt kneading temperature, the resin discharge rate, the number of die holes, the air-cooling distance, the strand bath temperature, and the strand immersion length.

[0117] The design conditions of the extruder include the screw diameter, the number of die holes, and the die hole diameter. The cooling conditions of the strand discharged from the extruder include the air-cooling distance between the extruder die and the water surface of the strand bath, the strand bath temperature, the immersion length of the strand bath, and the range of the strand take-up speed.

[0118] The melt kneading temperature can be adjusted according to the type of thermoplastic resin. The cooling rate of the strand can be reduced by increasing the air-cooling distance between the extruder die and the water surface of the strand bath, increasing the water temperature in the strand bath, etc. For example, the melting temperature is set to about +20 to +100°C above the melting point of the crystalline thermoplastic resin or the glass transition point of the amorphous thermoplastic resin, and the cooling rate of the strand is controlled, thereby lengthening the time until the temperature of the resin composition drops from the melting temperature to below the melting point of the crystalline thermoplastic resin or the glass transition point of the amorphous thermoplastic resin during strand cooling.

[0119] For example, when the thermoplastic resin is an aliphatic polyamide resin, the conditions include a melt kneading temperature of 180°C to 300°C, and strand cooling conditions of an air cooling distance of 150 to 300 mm, a strand bath temperature of 40°C, and an immersion length of 300 to 500 mm.

[0120] In addition, when the thermoplastic resin is a polypropylene-based resin, the conditions include a melt kneading temperature of 180°C to 250°C, and strand cooling conditions of an air cooling distance of 150 to 300 mm, a strand bath temperature of 40°C, and an immersion length of 500 to 2000 mm.

[0121] The cooled strand is cut into pellets, the shape of which may vary depending on the cutting method used during extrusion processing. For example, pellets cut by a cutting method called underwater cutting tend to be spherical, pellets cut by a cutting method called hot cutting tend to be spherical or ellipsoidal, and pellets cut by a cutting method called strand cutting tend to be cylindrical.

[0122] [Uses of pellets and manufacturing method of compacts] The pellets of this embodiment can be subjected to various molding methods such as extrusion molding (cold runner method, hot runner method), injection molding, injection compression molding, gas-assisted injection molding, foam injection molding, ultra-thin injection molding (ultra-high speed injection molding), vacuum molding, blow molding, decorative molding, other material molding, low pressure molding, in-mold composite molding (insert molding, outsert molding), etc. to manufacture a molded body. In injection molding, the advantages of using the pellets of this disclosure are particularly evident.

[0123] One aspect of the present invention is a process for preparing a pellet of the present disclosure; A step of injection molding the pellets in a mold to obtain a molded body; The present invention provides a method for producing a molded article, comprising: a) forming a molded article by molding the molded article with a pellet according to the present disclosure; b) forming a molded article by molding the molded article with a pellet according to the present disclosure; c) forming a molded article by molding the molded article with a pellet according to the present disclosure; and c) forming a molded article by molding the molded article with a pellet according to the present disclosure. From the viewpoint of particularly significant advantages of reducing yellowing and appearance defects of the molded article by using the pellet according to the present disclosure, examples of suitable injection molding machines include hydraulic, electric, and hydraulic-electric hybrid injection molding machines as drive systems, and plunger, pre-plasticizing, and screw injection molding machines as injection structures. From the above viewpoint, examples of suitable molding conditions include a melting temperature of +20 to 100°C (the melting point of the crystalline thermoplastic resin or the glass transition point of the amorphous thermoplastic resin) and a mold temperature of -50 to 200°C (the melting point of the crystalline thermoplastic resin or the glass transition point of the amorphous thermoplastic resin).

[0124] The molded article may be provided in various shapes such as a sheet, a film, a fiber, various solid or hollow molded articles, etc. The uses of the molded article can be exemplified in various ways, such as industrial machine parts (e.g., electromagnetic device housings, roll materials, transport arms, medical device parts, etc.), general machine parts, automobile, railway, vehicle parts, etc. (e.g., outer plates, chassis, aerodynamic parts, seats, friction materials inside transmissions, etc.), ship parts (e.g., hulls, seats, etc.), aviation-related parts (e.g., fuselages, main wings, tails, movable surfaces, fairings, cowls, doors, seats, interior materials, etc.), spacecraft and artificial satellite parts (motor cases, main wings, structures, antennas, etc.), electronic and electrical equipment parts, etc. Examples of applications include gasoline components (e.g. personal computer cases, mobile phone cases, office automation equipment, audiovisual equipment, telephones, facsimiles, home appliances, toys, etc.), construction and civil engineering materials (e.g. rebar substitute materials, truss structures, cables for suspension bridges, etc.), daily necessities, sports and leisure goods (e.g. golf club shafts, fishing rods, tennis or badminton rackets, etc.), casing components for wind power generation, containers and packaging materials, for example materials for high-pressure containers filled with hydrogen gas, etc., such as those used in fuel cells.

[0125] In addition, when the molded product is provided as a resin composite film, it is suitable for reinforcing laminates in printed wiring boards.Other uses include, for example, insulating tubes, insulating levers, arc-extinguishing plates, operating rods, insulating spacers, cases, wind tunnels, end bells, wind sinks in generators, transformers, rectifiers, circuit breakers, and controllers, switch boxes, cases, crossbars, insulating shafts, fan blades, mechanical parts, transparent resin substrates, speaker diaphragms, eta diaphragms, television screens, fluorescent lamp covers, antennas, horn covers, radomes, cases, mechanical parts, wiring substrates, electronic equipment parts for aircraft, rockets, and artificial satellites, railway parts, ship parts, bathtubs, septic tanks, corrosion-resistant equipment, chairs, safety helmets, pipes, tank trucks, cooling towers, floating breakwaters, buried underground tanks, containers, and the like.

[0126] Among these, molded articles containing cellulose nanofibers are suitable for use in automobile parts and electronic product parts that require resin molding, since they can take advantage of the excellent heat resistance of the molded articles. EXAMPLES

[0127] The present embodiment will be described in detail below with reference to examples, but the present invention is not limited to these examples. The main physical properties were measured by the following methods.

[0128] [Evaluation method] <Crystallization peak temperature upon cooling of thermoplastic resin and resin composition> The measurement was performed by the following method. Equipment: Differential scanning calorimeter (PERKINELMER DSC8500) Condition: Cell: Aluminum Carrier gas: Nitrogen (50ml / min) Temperature program: 20℃→250℃ (100℃ / min) 250℃ (held for 5 minutes) 250℃→20℃(10℃ / min)

[0129] <Ratio of total volume of pores (Ve) to total volume of cellulose nanofibers (Vc) per 100 pellets> It was calculated using the following formula. Ve / Vc = (pore area ratio × pore-containing pellet ratio) / (cellulose volume ratio when pores are not present × (100-pore area ratio × pore-containing pellet ratio / 100)) × 100 The void area ratio and the void-containing pellet ratio were measured by the methods described below. The volume ratio of cellulose in the absence of pores was calculated from the amount of each component added to the resin composition and its density. In this case, the density was 1.14 g / cm for polyamide 6 (PA6). 3 , Polypropylene (PP) 0.90g / cm 3 , Maleic anhydride modified ethylene-octene copolymer (MEOR) 0.87g / cm 3 , cellulose nanocrystals (CNC) and cellulose nanofibers (CNF) 1.50g / cm 3 , Hydrophobized cellulose nanofiber (hydrophobized CNF) 1.43g / cm 3 , Pentaerythritol (PET) 1.40g / cm3 It was calculated as:

[0130] <Number of pellets containing voids per 100 pellets (percentage of pellets containing voids)> Each of 100 randomly selected pellets was cut at the center of the pellet in the MD direction and further flattened with a microtome (HM340, manufactured by Thermo Fisher Scientific Co., Ltd.) to obtain a TD cross section. The morphological image of this TD cross section was photographed with a microscope (VHX-5000, manufactured by Keyence Co., Ltd.) at a magnification of 20 times (observation field: 10 mm x 14 mm), and pellets having visible pores were determined to be pore-containing pellets. The number of pore-containing pellets among the 100 pellets was counted to obtain the pore-containing pellet ratio.

[0131] <The ratio of the void area to the cross-sectional area of ​​the TD cross section of a pellet containing voids (void area ratio)> Using the same method as in the evaluation of the number of void-containing pellets per 100 pellets above, 100 pellets were selected and the morphology of the TD cross section was observed. The void area in the TD cross section of the void-containing pellets was measured using the software attached to the microscope, and the ratio of the void area to the total cross-sectional area of ​​the TD cross section (100%) was calculated, and the average value for all the void-containing pellets was taken as the void area ratio. If there was not even one void-containing pellet among the 100 pellets, the void area ratio was 0%.

[0132] <The angle between the pellet MD direction and the normal direction of the pellet cut surface (pellet cut surface inclination angle)> Each of ten randomly selected pellets was cut in a direction selected by visual inspection so as to pass through the center of the pellet in the TD direction and maximize the pellet cut surface inclination angle described below, and further flattened with a microtome (HM340, manufactured by Thermo Fisher Scientific Co., Ltd.) to obtain an MD cross section. A morphological image of this MD cross section was photographed with a microscope (VHX-5000, manufactured by Keyence Co., Ltd.) at a magnification of 20 times (observation field: 10 mm x 14 mm). On the morphological image, the pellet MD direction axis and a normal to the line segment corresponding to the pellet MD end face were defined, and the angle between the pellet MD direction axis and the normal was measured. The number average value of the ten pellets was obtained as the pellet cut surface inclination angle.

[0133] <Appearance of molded product> The pellets were injection molded into the shape of a multipurpose test piece according to ISO 294-3. The surfaces of the 30 multipurpose test pieces were visually observed and evaluated according to the following criteria. Good: 0 silver streaks Acceptable: 1 to less than 10 silver streaks Bad: 10 or more silver streaks

[0134] <Molding cycle> The pellets were injection molded into the shape of a multipurpose test piece according to ISO 294-3. The average molding cycle (seconds) for 30 pieces was recorded as the molding cycle.

[0135] <Yellowness (YI)> The pellets were injection molded into the shape of a multipurpose test piece according to ISO 294-3, and the YI was measured according to JIS K7373.

[0136] [Materials used] <Thermoplastic resin> Polyamide 6 (PA6) UBE Nylon 1013B (Ube Industries, Ltd.) Carboxyl end group ratio: ([COOH] / [total end groups]) = 0.6 Viscosity number (VN) of polyamide measured in 96% by weight sulfuric acid = 95 Polypropylene (PP) Novatec PP MA1B (Japan Polypropylene Corporation) MFR(230℃, 2.16kgf)=21g / 10min

[0137] <Elastomer> Maleic anhydride modified ethylene-octene copolymer (MEOR) Fusabond MN-493D (DowDuPont) MFR(190℃, 2.16kgf)=1.2g / 10min Octene content = 28% by mass Melting point = 55°C (DSC method: heating rate 10°C / min) Maleic anhydride addition rate = 1.0 mass%

[0138] <Cellulose> [Preparation Example 1] Cellulose nanocrystal (hereinafter referred to as CNC) Commercially available DP pulp (average degree of polymerization 1600) was cut and hydrolyzed in a 10% by mass aqueous hydrochloric acid solution at 105°C for 30 minutes. The resulting acid-insoluble residue was filtered, washed, and pH adjusted to prepare a crystalline cellulose dispersion with a solid content concentration of 14% by mass and a pH of 6.5. This crystalline cellulose dispersion was spray-dried to obtain a dried crystalline cellulose product. Next, the dried product obtained above was fed to an airflow type mill (STJ-400 model, manufactured by Seishin Enterprise Co., Ltd.) at a feed rate of 10 kg / hr and pulverized to obtain CNC as a crystalline cellulose fine powder. The properties of the obtained CNCs were evaluated and the diameter was found to be 30 nm and the L / D ratio was 8.

[0139] To the obtained aqueous dispersion of CNC, 5 parts by mass of polyethylene glycol with a molecular weight of 20,000 (hereinafter referred to as PEG20000) was added per 100 parts by mass of CNC, and then the mixture was vacuum dried at approximately 40°C using a revolution / rotation type mixer (EME V-mini300) to obtain CNC powder.

[0140] [Preparation Example 2] Cellulose nanofiber (hereinafter referred to as CNF) After cutting the linter pulp, it was heated in hot water of 120°C or higher for 3 hours using an autoclave, and the refined pulp from which the hemicellulose portion had been removed was squeezed and highly shortened and fibrillated in pure water to a solid content of 1.5% by mass by beating, and then defibrated at the same concentration using a high-pressure homogenizer (operating pressure: 10 treatments at 85 MPa) to obtain defibrated cellulose. Here, the beating process used a disc refiner, and the pulp was treated for 4 hours with a beating blade with high cutting function (hereinafter referred to as a cutting blade), and then beaten for an additional 1.5 hours using a beating blade with high defibration function (hereinafter referred to as a defibration blade). The properties of the obtained CNF were evaluated and it was found that the diameter was 90 nm and the L / D ratio was more than 30 (approximately 300).

[0141] To the obtained aqueous dispersion of CNF, 5 parts by mass of PEG20000 was added per 100 parts by mass of CNF, and then the mixture was vacuum dried at approximately 40°C using a revolution / rotation type mixer (EME V-mini300) to obtain CNF powder.

[0142] [Preparation Example 3] Hydrophobized CNF (hereinafter referred to as hydrophobized CNF) (defibration process) The raw material linter pulp was stirred in dimethyl sulfoxide (DMSO) at room temperature for 1 hour at 500 rpm using a single-shaft mixer (Imex DKV-1 φ125 mm dissolver).Then, the raw material was fed to a bead mill (Imex NVM-1.5) using a hose pump and circulated for 120 minutes using only DMSO to obtain a defibrated slurry.

[0143] (Defibrillation and acetylation process) Then, 11 parts by mass of vinyl acetate and 1.63 parts by mass of sodium bicarbonate were added to the bead mill device per 100 parts by mass of the defibrated slurry, and the device was further circulated for 60 minutes to obtain a hydrophobic CNF slurry.

[0144] During circulation operation, the rotation speed of the bead mill was 2500 rpm and the peripheral speed was 12 m / s. The beads used were made of zirconia and had a diameter of 2.0 mm, and the filling rate was 70% (the slit gap of the bead mill at this time was 0.6 mm). During circulation operation, the slurry temperature was controlled at 40°C using a chiller to absorb heat generated by friction.

[0145] To the obtained hydrophobized CNF slurry, 192 parts by mass of pure water was added per 100 parts by mass of defibrated slurry, and after thorough stirring, it was concentrated in a dehydrator. The obtained wet cake was dispersed again in the same amount of pure water, stirred, and concentrated, and this washing procedure was repeated a total of five times.

[0146] The properties of the obtained hydrophobic CNF were evaluated, and it was found to have a diameter of 65 nm and an L / D ratio of 30 or more (approximately 450).

[0147] To the obtained aqueous dispersion of hydrophobic CNF (solid content: 10% by mass), 5 parts by mass of PEG20000 was added per 100 parts by mass of hydrophobic CNF, and then the mixture was vacuum dried at approximately 40°C using a revolution / rotation type mixer (EME V-mini300) to obtain hydrophobic CNF powder.

[0148] <Resin crystallization temperature lowering agent> Pentaerythritol (PET) (Tokyo Chemical Industry Co., Ltd.) CAS:115-77-5

[0149] [Example 1] 90 parts by mass of PA6 and 10 parts by mass of CNF obtained in Preparation Example 2 were mixed, melt-kneaded at a kneading temperature of 250°C in a twin-screw extruder (TEM-37SS manufactured by Toshiba Machine Co., Ltd., screw diameter 37 mm) and extruded into a strand shape. At this time, the resin discharge rate of the twin-screw extruder was 20 kg / h, and the number of holes in the die was 3 holes. The distance from the die hole to the water surface of the strand bath was adjusted so that the air-cooling distance until the strand coming out of the die landed in the water was 150 mm. Thereafter, it was cooled to an immersion length of 400 mm in a strand bath with the water temperature adjusted to 40°C, and then cut with a strand cutter to obtain pellets.

[0150] [Comparative Example 1, Example 2] Pellets were obtained in the same manner as in Example 1, except that the pellet production conditions were changed as shown in Table 1.

[0151] [Comparative Examples 2 and 3, Examples 3 to 7 and 9] Pellets were obtained in the same manner as in Example 1, except that the twin-screw extruder was changed to a TEM-75SS (screw diameter 75 mm) manufactured by Toshiba Machine Co., Ltd. and the pellet production conditions were changed as shown in Table 1.

[0152] [Example 8] Pellets were obtained in the same manner as in Example 3, except that the pellet production conditions were changed as shown in Table 1, the take-up speed of the strand cutter was adjusted to a slower speed, and the minor axis of the pellet TD cross section was set to the value shown in Table 1.

[0153] [Example 10] 70 parts by mass of PA6, 20 parts by mass of MEOR, and 10 parts by mass of CNF were mixed and melt-kneaded, and pellets were obtained in the same manner as in Example 3 except that the pellet production conditions were changed as shown in Table 1.

[0154] [Example 11] 90 parts by mass of PA6, 5 parts by mass of CNC obtained in Preparation Example 1, and 5 parts by mass of CNF obtained in Preparation Example 2 were mixed and melt-kneaded, and pellets were obtained in the same manner as in Example 3, except that the pellet production conditions were changed as shown in Table 1.

[0155] [Examples 12 and 13] 90 parts by mass of PA6 and 10 parts by mass of the hydrophobic CNF obtained in Preparation Example 3 were mixed and melt-kneaded, and pellets were obtained in the same manner as in Example 3 except that the pellet production conditions were changed as shown in Table 1. [Example 14] 89 parts by mass of PA6, 1 part by mass of PET, and 10 parts by mass of the hydrophobic CNF obtained in Preparation Example 3 were mixed and melt-kneaded, and pellets were obtained in the same manner as in Example 3, except that the pellet production conditions were changed as shown in Table 1.

[0156] [Comparative Example 4, Example 15] 90 parts by mass of PP and 10 parts by mass of CNF obtained in Preparation Example 2 were mixed and melt-kneaded at a kneading temperature of 200°C. Pellets were obtained in the same manner as in Example 3, except that the pellet production conditions were changed as shown in Table 1.

[0157] [Reference example 1] Pellets were obtained in the same manner as in Example 1, except that in step 3, no cellulose aggregates were used and only polyamide (PA) was melt-kneaded. The results are shown in Table 1.

[0158] [Table 1]

[0159] From the results shown in Table 1, in Examples 1 to 15, the molded bodies were less yellowed and had good appearances, even though the pellets contained cellulose nanofibers. For example, in Examples 2, 6, 7, 11, and 12, in which the water temperature was relatively high and the solidification rate of the thermoplastic resin was slow, the pore-containing pellet ratio was 0%, and the generation of pores was reduced to a level comparable to that of Reference Example 1, which did not use cellulose nanofibers, and the molded bodies showed good appearances that were comparable to those of Reference Example 1, which did not use cellulose nanofibers. Furthermore, in Example 8, in which the pellet size was increased, and in Examples 10 and 15, in which the type of thermoplastic resin was changed, molded bodies with less yellowing and good appearances were obtained. In Examples 12 and 13, in which hydrophobized CNF was used, the molded bodies were particularly less yellowed. In Example 14, in which a resin crystallization temperature lowering agent was added, a molded body with a shorter molding cycle and less yellowing was obtained. [Industrial Applicability]

[0160] The pellets according to the present invention are useful for producing molded articles having good appearance and suppressed yellowing. [Explanation of symbols]

[0161] 1,2,3 Pellets S1, S2 Pellet cut surface L Pellet MD direction L1,L2 normal direction θ1,θ2 angle

Claims

1. A pellet of a resin composition containing a crystalline thermoplastic resin and a cellulose nanofiber having a fiber diameter of 1000 nm or less, the pellet has a cut surface; The angle between the pellet MD direction and the normal direction of the pellet cut surface is 5° to 30°, A pellet having 10 or less voids per 100 pellets.

2. 2. The pellet according to claim 1, wherein the ratio of the void area to the cross-sectional area in the TD cross section of the pellet is 4.0% or less.

3. 3. The pellet according to claim 1, wherein the number of void-containing pellets per 100 pellets is 1 or less.

4. The pellet according to any one of claims 1 to 3, wherein the short axis of the pellet TD cross section is 2 mm to 5 mm.

5. The pellet according to any one of claims 1 to 4, comprising 0.1 to 30% by mass of the cellulose nanofibers.

6. The pellet according to any one of claims 1 to 5, wherein the cellulose nanofibers have a fiber diameter of 50 to 1000 nm and a fiber length / fiber diameter (L / D) ratio of 30 or more.

7. The pellet according to any one of claims 1 to 6, wherein the cellulose nanofibers are hydrophobized cellulose nanofibers.

8. The pellet according to any one of claims 1 to 7, wherein the thermoplastic resin is a polyamide-based resin and / or a polyolefin-based resin.

9. The pellet according to any one of claims 1 to 8, further comprising an elastomer.

10. The pellet according to any one of claims 1 to 9, further comprising cellulose nanocrystals having a diameter of 100 nm or less and an L / D of less than 30, or cellulose microfibers having a fiber diameter of more than 1 μm to 50 μm, or a mixture thereof.

11. The difference Tcc-Tcp between the temperature-lowering crystallization peak temperature Tcc of the resin composition measured by a differential scanning calorimeter and the temperature-lowering crystallization peak temperature Tcp of the thermoplastic resin measured by a differential scanning calorimeter is 5 ° C. to 30 ° C. The pellet according to any one of claims 1 to 10.

12. The ratio Ve / Vc of the total volume of pores (Ve) of the pellets to the total volume of cellulose nanofibers (Vc) per 100 pellets is 0% by volume to 4% by volume. The pellet according to any one of claims 1 to 11.

13. The resin composition further comprises a resin crystallization temperature lowering agent, The resin crystallization temperature lowering agent is a compound that lowers the temperature-lowering crystallization peak temperature of the resin composition measured by a differential scanning calorimeter by 5 to 30 ° C. The pellet according to any one of claims 1 to 12.

14. Providing a pellet according to any one of claims 1 to 13, and A step of injection molding the pellets in a mold to obtain a molded body; A method for producing a molded body, comprising the steps of:

Citation Information

Patent Citations

  • Thermoplastic resin pellet excellent in moldability

    JP2000015631A

  • Microcellulose-based fiber-containing resin composition and method for producing the same

    JP2011006609A

  • Molding material mixture and manufacturing method therefor

    JP2018016896A

  • Fiber-reinforced composite material

    JP2019056088A