Ethylene acid copolymer ionomers with improved creep resistance.
Ethylene acid copolymers with specific monomer compositions and magnesium neutralization enhance creep resistance, allowing ionomers to function effectively at higher temperatures.
Patent Information
- Application Number
- JP2021501275
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-07-31
- Filing Date
- 2019-07-26
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2039-07-26
AI Technical Summary
Ionomers exhibit limited creep resistance at temperatures above 60°C, leading to deformation under stress, which restricts their use in applications requiring higher temperature stability.
Development of ethylene acid copolymers with specific compositions, including 2 to 20% monocarboxylic acid and 2 to 15% unsaturated dicarboxylic acid monomers, neutralized by magnesium cations, achieving less than 25% dimensional change under 20 psi at 100°C for 30 minutes.
The new ionomers demonstrate improved creep resistance at elevated temperatures while maintaining optical clarity and toughness, enabling their use in applications beyond 60°C.
Smart Images

Figure 0007561115000001 
Figure 0007561115000002
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 62 / 712,596, filed July 31, 2018, the entire disclosure of which is incorporated herein by reference.
[0002] Embodiments of the present disclosure relate generally to ionomer resins, and specifically to ionomers comprising the polymerization reaction products of ethylene, monocarboxylic acid monomers, unsaturated dicarboxylic acid monomers, alkyl acrylate monomers, and combinations thereof, which are at least partially neutralized with magnesium cations. [Background technology]
[0003] Ionomers are commonly used materials in a variety of applications because they have higher tensile strength, excellent clarity, good abrasion resistance, and high stiffness than their precursor acid copolymers. For example, ionomers of ethylene acid copolymers have found utility in many applications, such as food packaging, foam parts, injection molded parts (e.g., cosmetic containers), and golf ball components.
[0004] Although ionomers can be utilized in many applications, their limited service temperature limits the use of ionomers in applications requiring creep resistance at temperatures above 60° C. For example, ionomers may deform under stress at temperatures above 60° C. Dynamic mechanical thermal analysis reveals a significant decrease in the mechanical strength of ionomers at approximately 60° C., which correlates with the onset of dissociation of ionic aggregates. Summary of the Invention
[0005] Therefore, it would be beneficial to develop alternative ionomers that have improved creep resistance while maintaining the physical and chemical properties of ionomers, such as optical clarity and toughness.
[0006] In one or more embodiments, the ionomers of the present disclosure include ethylene acid copolymers comprising the polymerization reaction product of ethylene with 2 to 20 weight percent of a monocarboxylic acid monomer, based on the total weight percent of monomers present in the ethylene acid copolymer, and 2 to 15 weight percent of an unsaturated dicarboxylic acid monomer, based on the total weight percent of monomers present in the ethylene acid copolymer. The ionomers include those in which 10 to 70 mole percent of the total acid units of the ethylene acid copolymer are neutralized with magnesium cations. The ionomers exhibit less than 25% dimensional change at a temperature of 100° C. under a stress of 20 psi for 30 minutes.
[0007] In one or more embodiments, the ionomer comprises a first ethylene acid copolymer and a second ethylene acid copolymer. The first ethylene acid copolymer is a polymerization reaction product of ethylene, 2-20% by weight of a monocarboxylic acid, based on the total weight percent of monomers present in the first ethylene acid copolymer, and 0-40% by weight of an alkyl acrylate, based on the total weight percent of monomers present in the first ethylene acid copolymer. The second ethylene acid copolymer of the ionomer is a polymerization reaction product of ethylene, 0-20% by weight of a monocarboxylic acid, based on the total weight percent of monomers present in the second ethylene acid copolymer, 0-40% by weight of an alkyl acrylate, based on the total weight percent of monomers present in the second ethylene acid copolymer, and 2-15% by weight of an unsaturated dicarboxylic acid monomer, based on the total weight percent of monomers present in the second ethylene acid copolymer. The ratio of the first ethylene acid copolymer to the second ethylene acid copolymer in the ionomer is 90 / 10% to 10 / 90% by weight. At least 70 mole percent of the total acid units in the ionomer are neutralized, and from 10 to 70 mole percent of the total acid units in the blend are neutralized with magnesium cations. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs. In case of conflict, the present specification, including definitions, will control.
[0009] Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of various embodiments, suitable methods and materials are described herein.
[0010] Unless otherwise stated, all percentages, parts, ratios, etc. are by weight. When an amount, concentration, or other value or parameter is given, either as a range, a preferred range, or a list of lower and higher preferred values, this should be understood to specifically disclose all ranges formed from any pairing of any lower range limit or preferred value with any higher range limit or preferred value, regardless of whether the range is separately disclosed. When a range of numerical values is recited herein, unless otherwise indicated, the range is intended to include its endpoints, as well as all integers and fractions within the range. It is not intended that the scope of the present invention be limited to the specific values recited when defining the range.
[0011] When the term "about" is used in describing a value or an end point of a range, the disclosure should be understood to include the specific value or end point referred to.
[0012] As used herein, the terms "comprises," "comprising," "includes," "including," "containing," "characterized by," "has," "having," or any other variations thereof, are intended to cover a non-exclusive inclusion. For example, a process, method, article, or apparatus that includes a list of elements is not necessarily limited to those elements and may include other elements that are not expressly listed or that are inherent to such process, method, article, or apparatus. Further, unless expressly stated otherwise, "or" refers to an inclusive or and not an exclusive or.
[0013] The transitional phrase "consisting essentially of" limits the scope of the claim to the specified materials or steps, and those that do not materially affect the basic and novel characteristic(s) of the disclosure. If applicant has defined an embodiment or portion thereof with open-ended terms, such as "comprising," the description should be construed to also describe such embodiments using the term "consisting essentially of," unless otherwise noted.
[0014] The use of "a" or "an" is used to describe elements and components of various embodiments. This is merely for convenience and to give a general sense of the various embodiments. This description should be read to include one or at least one, and it also includes the plural, unless it is clear that the singular form means otherwise.
[0015] The term "polymer" refers to a polymeric compound prepared by polymerizing monomers, whether the monomers are the same or different types. Thus, the general term polymer encompasses the terms "homopolymer" and "copolymer." The term "homopolymer" refers to a polymer prepared from only one type of monomer, while the term "copolymer" refers to a polymer prepared from two or more different monomers, and for purposes of this disclosure, may include "terpolymer" and "interpolymer."
[0016] The term "monocarboxylic acid monomer" refers to a molecule having a reactive moiety, such as vinyl or vinylene, which can combine with other monomers to form a carboxylic acid (-C(O)OH) moiety that is not included in the polymer and is not a reactive moiety. For example, (meth)acrylic acid is a monocarboxylic acid monomer in which vinylene is the reactive moiety and a carboxylic acid is present. The term "(meth)acrylic acid" includes methacrylic acid and / or acrylic acid, and "(meth)acrylate" includes methacrylate, acrylate, or a combination of methacrylate and acrylate.
[0017] The term "unsaturated dicarboxylic acid monomer" as used in this disclosure means a molecule having a reactive moiety, such as vinyl or vinylene, which can combine with other monomers to form two carboxylic acid (-C(O)OH) moieties that are not included in the polymer and the reactive moiety. Additionally, "unsaturated dicarboxylic acid monomer" includes dicarboxylic acid derivative monomers (half esters and anhydrides).
[0018] Various embodiments are directed to ionomers with improved creep resistance comprising neutralized blends of ethylene acid copolymers. The ethylene acid copolymer comprises a polymerization reaction product of ethylene, monocarboxylic acid monomers, and unsaturated dicarboxylic acid monomers. In the ionomer, 10% to 70% of the total acid units of the ethylene acid copolymer are neutralized with magnesium cations. The ionomers with improved creep resistance exhibit less than 25% dimensional change at 20 psi at a temperature of 100° C. for 30 minutes. In one or more embodiments, the ionomers exhibit less than 25%, less than 20%, less than 15%, or less than 10% dimensional change at 100° C. under 20 psi stress for 30 minutes.
[0019] In one or more embodiments, the ethylene acid copolymer is the polymerization product of ethylene, a monocarboxylic acid monomer, and an unsaturated dicarboxylic acid monomer. The monocarboxylic acid monomer may include, for example, one or more of acrylic acid, methacrylic acid, or a combination thereof.
[0020] In one or more embodiments, the monocarboxylic acid monomer may be present in an amount of 2% to 20% by weight, based on the total weight of monomers present in the ethylene acid copolymer. All individual values and subranges within "2% to 20% by weight" are disclosed as separate embodiments. For example, the monocarboxylic acid monomer may be present in an amount of 5% to 15% by weight, 3% to 19% by weight, or 4% to 10% by weight, based on the total weight of monomers present in the ethylene acid copolymer.
[0021] In one or more embodiments, the amount of unsaturated dicarboxylic acid monomer may be 2 to 15 weight percent of unsaturated dicarboxylic acid monomer, based on the total weight percent of monomers present in the ethylene acid copolymer. All individual values and subranges encompassed by "2 weight percent to 15 weight percent" are disclosed as separate embodiments. For example, the unsaturated dicarboxylic acid monomer may be present in an amount of 5 weight percent to 15 weight percent, 3 weight percent to 10 weight percent, or 4 weight percent to 10 weight percent, based on the total weight of monomers present in the ethylene acid copolymer. In embodiments, the dicarboxylic acid may include maleic anhydride, maleic anhydride monomethyl ester, maleic anhydride monoethyl ester, maleic anhydride monopropyl ester, maleic anhydride monobutyl ester, or combinations thereof.
[0022] In an embodiment of the ionomer of the present disclosure, the ionomer may include a blend of two polymer resins, a first ethylene acid copolymer and a second ethylene acid copolymer, where one of the first ethylene acid copolymer or the second ethylene acid copolymer contains an unsaturated dicarboxylic acid monomer.
[0023] In one or more embodiments, the ionomer may comprise a neutralized blend of a first ethylene acid copolymer and a second ethylene acid copolymer. In one or more embodiments, the ratio of the first ethylene acid copolymer to the second ethylene acid copolymer is 90 / 10% to 10 / 90% by weight. In various embodiments, the neutralized blend comprises 60-90% by weight of the first ethylene acid copolymer or 60-80% by weight of the first ethylene acid copolymer, based on the total weight of the blend. In some embodiments, the neutralized blend comprises 60-90% by weight of the second ethylene acid copolymer or 60-80% by weight of the second ethylene acid copolymer, based on the total weight of the blend.
[0024] Ionomers of the present disclosure may include 10-60% of the total acid units of the blend neutralized with magnesium cations. In some embodiments of the ionomers, 20%-50%, 20%-60%, 25%-60%, or 30%-55% of the total acid units of the blend are neutralized with magnesium cations.
[0025] In various embodiments, the first ethylene acid copolymer is the polymerization reaction product of ethylene, from 2 to 20 weight percent of a monocarboxylic acid, based on the total weight percent of monomers present in the first ethylene acid copolymer, and from 0 to 40 weight percent of an alkyl acrylate, based on the total weight percent of monomers present in the first ethylene acid copolymer.
[0026] In one or more embodiments, the second ethylene acid copolymer is the polymerization reaction product of ethylene, 0 to 20 weight percent of a monocarboxylic acid, based on the total weight percent of monomers present in the second ethylene acid copolymer, 0 to 40 weight percent of an alkyl acrylate, based on the total weight percent of monomers present in the second ethylene acid copolymer, and 2 to 15 weight percent of an unsaturated dicarboxylic acid monomer, based on the total weight percent of monomers present in the second ethylene acid copolymer.
[0027] In one or more embodiments, the monocarboxylic acid monomer may be present in the first ethylene acid copolymer or the second ethylene acid copolymer in an amount of 0% to 20% by weight, based on the total weight of monomers present in the ethylene acid copolymer. All individual values and subranges encompassed by "0% to 20% by weight" are disclosed as separate embodiments. For example, the monocarboxylic acid monomer may be present in an amount of 2% to 20% by weight, 5% to 30% by weight, or 4% to 10% by weight, based on the total weight of monomers present in the ethylene acid copolymer.
[0028] In one or more embodiments, the amount of unsaturated dicarboxylic acid monomer in the second ethylene acid copolymer can be 2 to 15 weight percent of the unsaturated dicarboxylic acid monomer, based on the total weight percent of the monomers present in the ethylene acid copolymer. All individual values and subranges encompassed by "2 weight percent to 15 weight percent" are disclosed as separate embodiments. For example, the unsaturated dicarboxylic acid monomer can be present in an amount of 5 weight percent to 15 weight percent, 3 weight percent to 10 weight percent, or 4 weight percent to 10 weight percent, based on the total weight of the monomers present in the second ethylene acid copolymer. In embodiments, the dicarboxylic acid can include maleic anhydride, maleic anhydride monomethyl ester, maleic anhydride monoethyl ester, maleic anhydride monopropyl ester, maleic anhydride monobutyl ester, or combinations thereof.
[0029] In various embodiments, the first ethylene acid copolymer or the second ethylene acid copolymer may include an alkyl acrylate. In some embodiments, the first ethylene acid copolymer further includes 0% to 40% by weight of an alkyl acrylate, based on the total weight of monomers present in the ethylene acid copolymer. All individual values and subranges encompassed by "0% to 40% by weight" are disclosed as separate embodiments. The first ethylene acid copolymer or the second ethylene acid copolymer may include, for example, 1% to 30% by weight of an alkyl acrylate. The alkyl acrylate may be, by way of example and without limitation, ethyl acrylate, methyl acrylate, n-butyl acrylate, isobutyl acrylate, or combinations thereof. In various embodiments, the alkyl acrylate has an alkyl group having 1 to 8 carbons. This is referred to as C2-C8-alkyl acrylate. In certain embodiments, the alkyl acrylate is n-butyl acrylate.
[0030] In one or more embodiments of the ethylene acid copolymer, the first ethylene acid copolymer, or the second ethylene acid copolymer, the unsaturated dicarboxylic acid monomer comprises a precursor acid copolymer of a dicarboxylic acid or a reaction product of a derivative of a dicarboxylic acid. The unsaturated dicarboxylic acid monomer may include maleic acid, itaconic acid, fumaric acid, maleic acid monoethyl ester (MAME), maleic anhydride monopropyl ester, maleic anhydride monoethyl ester, maleic anhydride monobutyl ester, or combinations thereof, and C1-C4-alkyl half esters of these acids, and anhydrides of these acids, including maleic anhydride, maleic anhydride monomethyl ester, maleic anhydride monoethyl ester, and itaconic anhydride. In some embodiments, the unsaturated dicarboxylic acid monomer may include, but is not limited to, maleic anhydride, ethyl hydrogen maleate, and methyl hydrogen maleate. The carboxylic acid or anhydride units of these monomers can be neutralized with metal ions in exactly the same way as the monocarboxylic acid carboxylic acid units are shown, but the neutralization of the unsaturated dicarboxylic acid monomer may have different effects on the properties of the polymer, including its nature and melting behavior. Dicarboxylic acids can be dehydrated to form intra-chain anhydride units within the polymer (ie, within the chain rather than bridging inter-chain anhydride units).
[0031] In various embodiments of the ethylene acid copolymer, the first ethylene acid copolymer and the second ethylene acid copolymer can comprise at least 60 weight percent of monomers derived from ethylene. All individual values and subranges encompassed by "60 weight percent" are disclosed herein as separate embodiments, for example, the ethylene acid copolymer, the first ethylene acid copolymer, and the second ethylene acid copolymer of the present disclosure can comprise at least 60 weight percent of units derived from ethylene, at least 70 weight percent of units derived from ethylene, at least 80 weight percent of units derived from ethylene, or from 60 to 95 weight percent of units derived from ethylene, or from 80 to 98 weight percent of units derived from ethylene.
[0032] The ionomers of the present disclosure include neutralized blends of ethylene acid copolymers or neutralized blends of a first ethylene acid copolymer and a second ethylene acid copolymer. The term "neutralized blends" includes fully or partially neutralized ethylene acid copolymers. The ethylene acid copolymers may contain neutralized and non-neutralized monocarboxylic acid units, neutralized, mononeutralized, and non-neutralized dicarboxylic acid units, and in-chain anhydride units.
[0033] When referring to total neutralized acid units, monocarboxylic acids contribute one acid unit, dicarboxylic acids contribute two acid units, anhydrides such as maleic anhydride are considered to contribute two acid units, and half esters are considered to contribute one acid unit. The calculation of the neutralization percentage is based on the number of acid units considered to be present as above, and the number of metal equivalents added. In fact, anhydride units may remain anhydride units rather than changing to acid units. Upon neutralization, the anhydride monomer units may form dimetal salts, monometal salts, or non-neutralized unsaturated dicarboxylic acid monomers, or may not change the anhydride units as anhydride units and function as if there were no acid functionality. Half esters of unsaturated dicarboxylic acid monomers are counted as having only one acid, but may actually be converted to unsaturated dicarboxylic acid monomers or anhydrides, with various possibilities related to neutralization as above. However, as mentioned above, regardless of the number of acid groups (free or neutralized) actually present, the calculated neutralization percentage is based on the number of acid units based on the known molar amounts of monocarboxylic and dicarboxylic acid comonomers. Therefore, taking into account various variations in possible unsaturated dicarboxylic acid monomers and salts, the actual percentage of neutralized acid groups as a percentage of the total of neutralized and unneutralized free acid groups may differ from the calculated neutralization percentage, which is based on the amount of monocarboxylic acid or unsaturated dicarboxylic acid monomers in the ionomer. The difference is due to the anhydride units counting as two acid units rather than acid units.
[0034] In some embodiments, the ionomer may include cations other than Mg cations in addition to the Mg cations in the blend. The blend may be neutralized with at least one additional cation of a neutralizing salt. The neutralizing salt of the at least one additional metal cation may be selected from the group of zinc salts, lithium salts, and sodium salts. In some embodiments, the ionomer may include 0%-10%, 1%-10%, 5%-20%, 5%-30%, or 10%-50% of the total acid units of the blend are neutralized with sodium cations of a neutralizing salt, lithium cations of a neutralizing salt, zinc cations of a neutralizing salt, or combinations thereof.
[0035] In various embodiments, the ionomers exhibit improved creep resistance at high temperatures while maintaining their elasticity and expandability.
[0036] Ethylene acid copolymers can be prepared by standard free radical copolymerization techniques using high pressure and operating continuously. Monomers are fed to the reaction mixture in a ratio related to the activity of the monomers and the amount desired to be incorporated. In this way, a uniform, nearly random distribution of monomer units along the chain is achieved. Unreacted monomers can be recycled. Additional information regarding the preparation of ethylene acid copolymers with alkyl acrylate monomers can be found in U.S. Pat. Nos. 3,264,272 and 4,766,174, each of which is incorporated herein by reference in its entirety.
[0037] The blend can be produced by any means known to those skilled in the art. It is substantially melt processable and can be produced by combining one or more ethylene acid copolymers or ionomers of ethylene acid copolymers, one or more fatty acids or salts thereof, a basic metal compound, and a neutralization composition comprising a trivalent metal cation to produce a mixture and heating the mixture under conditions sufficient to produce the composition. Heating can be carried out at temperatures ranging from 80°C to 350°C, 120°C to 300°C, or 160°C to 260°C, and under pressures corresponding to the temperature, for periods of from 30 seconds to 2 or 3 hours. The blend can be produced by melt blending the ethylene acid copolymer and / or ionomers thereof with one or more fatty acids or salts thereof and simultaneously or thereafter combining sufficient amounts of a basic metal compound and a trivalent metal cation. A salt blend of the components can be made or the components can be melt blended in an extruder. For example, a Werner & Pfleiderer twin screw extruder can be used to simultaneously mix and process the ethylene acid copolymer and the organic acid (or salt) with the metal compound.
[0038] The blends may further include minor amounts of additives including plasticizers, stabilizers including viscosity stabilizers, hydrolysis stabilizers, primary and secondary antioxidants, ultraviolet light absorbers, antistatic agents, dyes, pigments or other colorants, inorganic fillers, flame retardants, lubricants, reinforcing agents such as glass fibers and flakes, synthetic (e.g., aramid) fibers or pulps, foaming or blowing agents, processing aids, slip additives, antiblock agents such as silica or talc, release agents, tackifying resins, or combinations of two or more thereof. Inorganic fillers such as calcium carbonate may also be incorporated into the blends.
[0039] These additives may be present in the blend in amounts ranging from 0.01% to 40% by weight, 0.01% to 25% by weight, 0.01% to 15% by weight, 0.01% to 10% by weight, or 0.01% to 5% by weight. Incorporation of the additives may be by any known process, such as, for example, dry blending, extrusion of a mixture of the various components, conventional masterbatch techniques, etc.
[0040] In some embodiments, ionomers according to the present disclosure exhibit load-bearing capability at temperatures above the melting temperature of the ionomer, as measured by differential scanning calorimetry (DSC).
[0041] According to various embodiments, the ionomers can be used to form foams or molded articles. For example, in embodiments, the ionomers can be combined with additives used to control the foam properties to form foams of various shapes. In some embodiments, the foams can be extruded from a twin screw extruder or the like, as known to those skilled in the art.
[0042] The blowing agents (also called blowing agents) used to produce the foams can be physical or chemical blowing agents. As used herein, a "physical blowing agent" is a low boiling liquid that volatilizes under curing conditions to form a foaming gas. Exemplary physical blowing agents include hydrocarbons, fluorocarbons, hydrofluorocarbons, hydrofluoroolefins, hydrochlorofluoroolefins, and other halogenated compounds. Other suitable chemical blowing agents can include, for example, sodium bicarbonate, ammonium bicarbonate, azodicarbonamide, dinitrosopentamethylenediamine, and sulfonyl hydrazides. Blowing agents such as water or carbon dioxide, added as a gas or liquid, or generated in situ by reaction of water with polyisocyanates, can also be used. Blowing agents can be used in mixtures of two or more, and chemical and physical blowing agents can be used together to adjust the expansion decomposition temperature and the foaming process.
[0043] The foam composition may further include free radical initiators or crosslinkers, co-curing agents, activators, and any other type of additives typically used in similar compositions, including, but not limited to, pigments, adhesion promoters, fillers, nucleating agents, rubbers, stabilizers, and processing aids.
[0044] The free radical initiator or crosslinker can include, by way of example and not limitation, an organic peroxide, such as a dialkyl organic peroxide. Examples of organic peroxides suitable for use include 1,1-di-t-butylperoxy-3,3,5-trimethylcyclohexane, t-butyl-cumyl peroxide, dicumyl-peroxide, 2,5-dimethyl-2,5-di(tert-butyl-peroxyl)hexane, 1,3-bis(tert-butyl-peroxyl-isopropyl)benzene, or a combination of two or more thereof.
[0045] Co-curing agents include trimethylolpropane triacrylate (and similar compounds), N,Nm-phenylene dimaleimide, triallyl cyanurate, or combinations of two or more thereof.
[0046] The activator may include an activator for the blowing agent and may include one or more metal oxides, metal salts, or organometallic complexes. Examples include ZnO, Zn stearate, MgO, or a combination of two or more thereof.
[0047] Foams can be produced by many methods, such as compression molding, injection molding, and a combination of extrusion and molding. The process can include mixing the components of the foam composition under heat to form a melt. The components can be mixed and blended using any technique known and used in the art, including Banbury, intensive mixer, two-roll mill, and extruder. Time, temperature, and shear rate can be adjusted to ensure dispersion without premature crosslinking or foaming.
[0048] After mixing, molding can be performed. Sheeting or calendar rolls can be used to create sheets of appropriate dimensions for foaming. Extruders can be used to mold the composition into pellets.
[0049] The foaming can be done in compression molding at a temperature and time to complete the decomposition of the peroxide and the blowing agent. The pressure, molding temperature, and heating time can be controlled. The foaming can be done using an injection molding machine by using pellets made from the foaming composition. The resulting foam can be further molded to the dimensions of the final product by any means known in the art, including thermoforming and compression molding.
[0050] In various embodiments, the resulting polymer foam compositions can be substantially closed cell and can be useful in a variety of articles, for example, footwear applications, including midsoles or insoles.
[0051] In one or more embodiments, the molded article exhibits less than 25%, less than 20%, less than 15%, or less than 10% dimensional change under a stress of 20 psi at 100° C. for 30 minutes.
[0052] The ionomers of the present invention may be prepared by standard neutralization techniques, as disclosed in U.S. Patent No. 3,264,272 (Rees), which is incorporated herein by reference. The resulting ionomer compositions of the present disclosure may have an MI of 0.01 to 100 grams / 10 minutes, preferably 0.1 to 30 grams / 10 minutes, according to ASTM D-1238, measured using a 2160 gram weight and 210° C. In one or more embodiments, the ionomers have a density of 0.920 to 0.980 g / cc.
[0053] The ethylene acid copolymer, first ethylene acid copolymer, and second ethylene acid copolymer of the present disclosure can be prepared by standard free radical copolymerization methods using high pressure operating continuously. Monomers are fed to the reaction mixture in a ratio related to the reactivity of the monomers and the amount desired to be incorporated. In this way, a uniform and nearly random distribution of monomer units along the chain is achieved. Polymerization in this manner is well known and is described in U.S. Pat. No. 4,351,931 (Armitage), which is incorporated herein by reference. Other polymerization techniques are described in U.S. Pat. No. 5,028,674 (Hatch et al.) and U.S. Pat. No. 5,057,593 (Statz), both of which are incorporated herein by reference. EXAMPLES
[0054] Test procedure Melt index (MI) is measured using ASTM D-1238 using a weight of 2160 grams.
[0055] Melting points (Tm) were measured using differential scanning calorimetry (DSC). Differential scanning calorimetry (DSC) is measured on a TA Instruments Q1000 DSC equipped with an RCS cooling attachment and an autosampler. Melting points (Tm) of samples are measured according to ASTM D3418.
[0056] The composition of the ionomers was determined using Perkin-Elmer Fourier Transform Infrared Spectroscopy (FTIR). Compression molded films of 5 mil thickness were used for FTIR analysis.
[0057] The following examples are provided to illustrate various embodiments, but are not intended to limit the scope of the claims. All parts and percentages are by weight unless otherwise indicated. Approximate properties, characters, parameters, etc. are provided below for various examples, comparative examples, and materials used in the examples and comparative examples. In addition, the description of the raw materials used in the examples is as follows:
[0058] Example 1 - Creep Resistance of Ethylene Acid Copolymers Creep resistance is a function of time, temperature, and load weight (stress). A simple test was employed to differentiate the creep resistance of ionomers with and without MAME, a dicarboxylic acid comonomer neutralized with various metal cations. Creep tests were performed by measuring the dimensional change (vertical) of a film specimen mounted under dead load in a cross-flow air oven equipped with a shelf rack to hold the specimen holder. Creep tests were performed on press-molded film strips 10 mils thick, 1 inch wide, and 3 inches long cut from compression molded film. The films were hung with a dead load of 100 grams in an oven initially set at 100°C. The deformation of the film specimens was measured after 30 minutes in the oven. The oven temperature was then increased to 120°C for testing.
[0059] The results, as summarized in Table 1, include data derived from inventive Examples 1.1-1.2, comparative terpolymer Examples CT1.1-CT1.4, and comparative copolymer Examples CC1.1-CC1.3. The polymer compositions of Examples 1.1-1.2 are magnesium metal cation (Mg) neutralized samples of ethylene / methyl acrylate / monoethyl maleate (E / MAA / MAME) terpolymers. Inventive Examples 1.1-1.2 and comparative terpolymer Examples CT1.1-CT1.4 are all ionomers neutralized with various metal cations to various degrees of neutralization based on an E / MAA / MAME (73 / 11 / 6 wt%) terpolymer with an MI of approximately 100 g / 10 min as measured according to ASTM D1238 using 2.16 kg at 190°C.
[0060] The polymer compositions of Comparative CC1-CC3 include E / MAA (85 / 15 wt%) neutralized with Na, Zn, and Mg cations. The melting temperatures of the samples are reported. Creep resistance tests were performed in a cross-flow air oven equipped with a shelf rack to hold the specimen holders. Each sample was in the form of a 10 mil (1 mil = 1 / 1000 inch) thick film, with the specimens measuring 3 inches long by 1 inch wide hung under a dead load of 100 grams. The films fell to the bottom of the oven as they lost their load-bearing capacity. [Table 1]
[0061] The results in Table 1 show that the Na, Zn, and Mg neutralized samples of Comparatives CC1.1-CC1.3 all failed at 100°C. Film specimens that dropped to the bottom of the oven due to loss of load-bearing capacity were considered to have failed the creep test at 100°C, a temperature above the melting temperature of the sample. Ionomer samples are expected to lose load-bearing capacity at temperatures above their melting temperature. Comparatives CT1.1-CT1.4, which contained Na, Li, Zn, and Na / Zn cations to neutralize the acid E / MAA / MAME terpolymer, failed at 100°C. The results of Example 1.1 showed that the Mg ionomer of E / MAA / MAME terpolymer passed the creep test at 100°C. The results of Example 1.2 showed that the Mg (40% neutralized) passed the creep test at 100°C and 120°C. Based on the results in Table 1, the Mg ionomer with EE / MAA / MAME acidic terpolymer had better physical properties from these samples Na, Zn, Li, or Na / Zn ionomers. The Mg ionomer in Examples 1.1 and 1.2 was the only resin with creep resistance above the melting point of the sample.
[0062] Example 2 - Creep resistance of ionomer blends The results are blends of various ionomer samples of both E / MAA / MAME terpolymers and E / MAA copolymers, as summarized in Table 2. The blends were prepared in a 26 mm twin screw extruder equipped with mixing screws using melt temperatures between 220°C and 250°C. The creep temperature is defined as when the film reaches a deformation of 25% strain under a load of 110 grams.
[0063] Examples 2.1.-2.6 include polymer resin blends of Ethylene Acid Copolymer A, Ethylene Acid Copolymer B, and Ethylene Acid Copolymer C.
[0064] Ethylene Acid Copolymer A ("Polymer A") is a Mg ionomer of an ethylene acid copolymer comprising the polymerization reaction product of ethylene and 15 wt.% methacrylic acid, where a nominal 50 mol % of the total acid units are neutralized with Mg cations. The ionomer has a melt index (MI) of 0.8 g / 10 min as measured according to ASTM D1238 at 190°C and 2.16 kg.
[0065] Ethylene acid copolymer B ("Polymer B") is a Zn ionomer of an ethylene acid copolymer comprising the polymerization reaction product of ethylene, 11 wt.% methacrylic acid, and 6 wt.% monoethyl maleic anhydride, where a nominal 50% of the total acid units are neutralized with zinc cations. The ionomer has a MI of 1.0 g / 10 min according to ASTM D1238 at 210°C and 2.16 kg.
[0066] Ethylene Acid Copolymer C ("Polymer C") is a Mg ionomer of an ethylene acid copolymer comprising the polymerization reaction product of ethylene, 11 wt.% methacrylic acid, and 6 wt.% monoethyl maleic anhydride, with a nominal 18% of the total acid units neutralized with zinc cations. The ionomer has a MI of 1.1 g / 10 min according to ASTM D1238 at 210°C and 2.16 kg. [Table 2]
[0067] The results in Table 2 showed that Examples 2.2, 2.5, and 2.6, which contained both MAME and Mg cations, achieved creep resistance above their melting temperature. The ionomers of Examples 2.2, 2.5, and 2.6 contained MAME and Mg cations. Since these example polymers were the only polymers that achieved creep resistance above their melting temperature, it is believed that the MAME content and Mg content act synergistically to enhance creep resistance. Thus, the data showed that Mg cation content and MAME content are the two variables that lead to higher creep resistance.
[0068] Creep tests for Table 2 were performed by measuring the dimensional change (vertical) of film specimens mounted under dead load in a cross-flow air oven equipped with a shelf rack to hold the specimen holders. Creep tests were performed on press-molded film strips 10 mil thick, 1 inch wide, and 3 inches long cut from a 10 mil thick compression molded film. The films were hung under a dead load of 110 grams in an oven initially set at 80°C. The deformation of the film specimens was measured after 30 minutes in the oven, then the oven temperature was increased by 10°C. The creep temperature was determined when the film specimens reached a deformation of 25% strain.
Claims
1. 1. An ionomer comprising an ethylene acid copolymer, The ethylene acid copolymer is Ethylene, 2 to 20 weight percent of a monocarboxylic acid monomer, based on the total weight percent of monomers present in the ethylene acid copolymer; and 2 to 15 weight percent, based on the total weight percent of monomers present in the ethylene acid copolymer, of an unsaturated dicarboxylic acid monomer or a half ester of an unsaturated dicarboxylic acid monomer; 10 to 70 mole percent of the total acid units of said ethylene acid copolymer are neutralized with magnesium cations; The ionomer has a compressibility of 20 psi (1.406 Kg / cm) at a temperature of 100° C. 2 ) for 30 minutes, exhibiting less than 25% dimensional change; The half ester of the unsaturated dicarboxylic acid monomer is a dicarboxylic acid derivative monomer selected from maleic anhydride monomethyl ester, maleic anhydride monoethyl ester, maleic anhydride monopropyl ester, maleic anhydride monobutyl ester, and combinations thereof. , ionomer.
2. 1. An ionomer comprising a first ethylene acid copolymer and a second ethylene acid copolymer, the first ethylene acid copolymer comprising: Ethylene, 2 to 20 weight percent of a monocarboxylic acid, based on the total weight percent of monomers present in said first ethylene acid copolymer; and 0 to 40 weight percent alkyl acrylate, based on the total weight percent of monomers present in said first ethylene acid copolymer; the second ethylene acid copolymer comprising: Ethylene, 0 to 20 weight percent of a monocarboxylic acid, based on the total weight percent of monomers present in the second ethylene-based polymer; 0 to 40 weight percent of an alkyl acrylate, based on the total weight percent of monomers present in said second ethylene acid copolymer; and 2 to 15 weight percent, based on the total weight percent of monomers present in said second ethylene acid copolymer, of an unsaturated dicarboxylic acid monomer or a half ester of an unsaturated dicarboxylic acid monomer; the ratio of the first ethylene acid copolymer to the second ethylene acid copolymer is from 90 / 10% by weight to 10 / 90% by weight; at least 70 mole percent of the total acid units of a blend of said first ethylene acid copolymer and said second ethylene acid copolymer are neutralized, and 10 to 70 mole percent of the total acid units of said blend are neutralized with magnesium cations; The half ester of the unsaturated dicarboxylic acid monomer is a dicarboxylic acid derivative monomer selected from maleic anhydride monomethyl ester, maleic anhydride monoethyl ester, maleic anhydride monopropyl ester, maleic anhydride monobutyl ester, and combinations thereof. Ionomer.
3. 2. The ionomer of claim 1, wherein the monocarboxylic acid monomer comprises one or more of acrylic acid, methacrylic acid, or a combination thereof.
4. The ionomer according to any one of claims 1 to 3, wherein the unsaturated dicarboxylic acid monomer is maleic anhydride.
5. 3. The ionomer of claim 2, wherein the blend is further neutralized with at least one additional metal cation selected from the group consisting of Zn, Li, and Na.
6. 6. The ionomer of claim 2 or 5, wherein the total acid units of the blend are neutralized in the range of 70 to 80 mole percent, and 20 to 60 mole percent of the total acid units of the blend are neutralized with the magnesium cation of the magnesium salt.
7. 3. The ionomer of claim 2, wherein the alkyl acrylate comprises methyl acrylate, ethyl acrylate, n-butyl acrylate, or isobutyl acrylate, or combinations thereof.
Citation Information
Patent Citations
Highly flame-retardant resin composition
JP1995018136A
Novel ionomers based on copolymers of ethylene containing both mono- and dicarboxylic acids and polyamide blends containing such ionomers
JP2002513434A
Highly elastic thermoplastic elastomer composition
JP2002527597A
Golf ball material, golf ball, and method for preparing golf ball material
JP2008023332A
Golf ball material, golf ball, and method for producing golf ball material
JP2008163331A