Methacrylic resin composition, resin modifier, molded article and film, and method for producing film
A tailored methacrylic resin composition with specific polymer ratios and properties addresses heat shrinkage and mechanical weaknesses, enhancing transparency and strength in optical films.
Patent Information
- Application Number
- JP2021535378
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-30
- Filing Date
- 2020-07-29
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2040-07-29
AI Technical Summary
Existing methacrylic resin compositions face issues with high heat shrinkage rates and inadequate mechanical properties, particularly when the content of certain components exceeds a certain threshold, leading to suboptimal performance in applications such as optical members and films.
A novel methacrylic resin composition comprising specific molecular weight ranges and ratios of methacrylic polymers (A) and (B), along with controlled molecular weight distribution and refractive index differences, is developed to enhance transparency, heat resistance, and mechanical strength.
The composition achieves high transparency, excellent surface smoothness, and improved mechanical strength, with reduced thermal deformation and faster solvent evaporation during film production, resulting in efficient and high-quality optical films.
Smart Images

Figure 0007561128000001 
Figure 0007561128000002 
Figure 0007561128000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a methacrylic resin composition, a resin modifier, a molded article and a film, and a method for producing the film. [Background technology]
[0002] Methacrylic resins (polymers mainly containing structural units derived from methacrylic acid esters) are excellent in transparency, light resistance, surface hardness, etc. By molding a resin composition containing a methacrylic resin, various optical members such as light guide plates, lenses, sheets, and films can be obtained.
[0003] Patent Document 1 discloses a (meth)acrylic resin composition containing a (meth)acrylic resin A having a weight average molecular weight of preferably 200,000 or less and a (meth)acrylic resin B having a glass transition temperature lower than that of the (meth)acrylic resin A and a weight average molecular weight of preferably 100,000 or more and 1,000,000 or less, with a weight ratio of the (meth)acrylic resin A to the (meth)acrylic resin B being preferably 80 / 20 to 40 / 60, and a film containing the same. Patent Document 1 states that if the content of the (meth)acrylic resin B is excessively large, the heat shrinkage rate of the obtained (meth)acrylic resin film is likely to be large.
[0004] Patent Document 2 discloses a methacrylic resin (M1) having an α-relaxation temperature Tα1 of 137° C. or higher when dynamic viscoelasticity is measured at 1 Hz in a tensile mode, a molecular weight distribution of preferably 1.0 to 1.4, and a weight average molecular weight of 40,000 to 200,000, and a methacrylic resin (M2) having an α-relaxation temperature Tα2 of 132° C. or lower when dynamic viscoelasticity is measured at 1 Hz in a tensile mode, and a weight average molecular weight of preferably 40,000 to 200,000. -1 The present invention discloses a methacrylic resin composition in which, when the melt viscosities at the melting points are η1 and η2, respectively, η1>η2 and the mass ratio of the methacrylic resin (M1) / methacrylic resin (M2) is 2 / 98 to 29 / 71.
[0005] Patent Document 3 discloses a dope composition containing a methacrylic resin having a weight-average molecular weight of 250,000 or more and an additive such as a phenolic compound, a styrene copolymer, or a novolak resin having a weight-average molecular weight of less than 50,000. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-110757 A [Patent Document 2] WO2018 / 021449A1 [Patent Document 3] WO2015 / 098676A1 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a novel methacrylic resin composition, a resin modifier, a molded article and a film, and a method for producing the film. [Means for solving the problem]
[0008] The present invention encompasses the following aspects.
[0009] [1] Weight average molecular weight Mw A is 30,000 or more, and the number average molecular weight Mn A Weight average molecular weight Mw A A methacrylic polymer (A) having a weight average molecular weight Mw B is 80,000 to 3,000,000 and the weight average molecular weight Mw A and a methacrylic polymer (B) having a molecular weight of 2.5 times or more; Methacrylic polymer (B) shear rate 122 sec -1 And melt viscosity η at 260℃ BThe shear rate of the methacrylic polymer (A) is 122 s -1 And melt viscosity η at 260℃ A Higher than The mass ratio of the methacrylic polymer (A) to the methacrylic polymer (B) is 2 / 98 to 39 / 61, and The peak top molecular weight M with the highest weight fraction differential value in the weight-based differential molecular weight distribution curve Pt is between 100,000 and 2,000,000, Methacrylic resin.
[0010] [2] The highest peak top molecular weight M in the weight-based differential molecular weight distribution curve Ph The methacrylic resin according to [1], wherein the sum of the weight fraction differential values of components having a molecular weight of 1 / 20 or less of the total weight fraction differential values of all components is 2% or less, and the sum of the weight fraction differential values of components having a molecular weight of 15,000 or less is 2% or less of the total weight fraction differential values of all components.
[0011] [3] Weight average molecular weight Mw A is 40000 to 140000, and the weight average molecular weight Mw B The methacrylic resin according to [1] or [2], wherein the molecular weight is 160,000 to 2,000,000. [4] Refractive index n of methacrylic polymer (A) dA and the refractive index n of the methacrylic polymer (B) dB Absolute difference between |n dA -n dB The methacrylic resin according to any one of [1] to [3], wherein | is 0.005 or less. [5] A resin composition comprising the methacrylic resin according to any one of [1] to [4] and an elastomer.
[0012] [6] The weight average molecular weight Mw is 40,000 to 140,000, the ratio of the weight average molecular weight Mw to the number average molecular weight Mn is 1.0 to 1.4, and the refractive index n dA resin modifier comprising a methacrylic polymer (A) having a molecular weight of 1.485 to 1.495, a triad syndiotacticity (rr) of 63 to 80%, a glass transition temperature of 125°C or higher, and containing 100 mass% of structural units derived from methyl methacrylate. [7] The resin modifier according to [6], wherein the methacrylic polymer (A) has a weight-based differential molecular weight distribution curve in which the sum of weight fraction differential values of components having a molecular weight of 15,000 or less is 2% or less of the sum of weight fraction differential values of all components.
[0013] [8] A molded article comprising the methacrylic resin according to any one of [1] to [4].
[0014] [9] A film containing the methacrylic resin according to any one of [1] to [4] and having a thickness of 20 μm or more and 200 μm or less.
[10] The film according to [9], which is for optical use.
[0015]
[11] A dope comprising the methacrylic resin according to any one of [1] to [4] and an organic solvent.
[0016]
[12] The dope according to
[11] is cast onto a casting support, and then removing the organic solvent.
[13] The method according to
[12] , wherein the thickness of the film is 20 μm or more and 200 μm or less. Effect of the Invention
[0017] The methacrylic resin or resin composition of the present invention has high transparency and high heat resistance. The molded article of the present invention, for example, a film, has high transparency, high heat resistance, and high mechanical strength, and is excellent in surface smoothness, surface hardness, or impact resistance. The film manufacturing method of the present invention requires a short time for evaporation of the organic solvent, and has high production efficiency for a film excellent in surface smoothness, surface hardness, or impact resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The methacrylic resin of the present invention contains a methacrylic polymer (A) and a methacrylic polymer (B).
[0019] The methacrylic polymer (A) is a random polymer mainly containing structural units derived from methacrylic acid esters. This methacrylic polymer (A) can be used as a resin modifier.
[0020] Examples of the methacrylic acid ester include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, and butyl methacrylate; aryl methacrylates such as phenyl methacrylate; and cycloalkyl methacrylates such as cyclohexyl methacrylate and norbornenyl methacrylate. Among these, alkyl methacrylates are preferred, and methyl methacrylate is most preferred.
[0021] The amount of structural units derived from methacrylic acid ester contained in the methacrylic polymer (A) is preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 98 mass% or more, still more preferably 99 mass% or more, and most preferably 100 mass% based on the total structural units of the methacrylic polymer (A). In the methacrylic polymer (A), the content of structural units derived from methyl methacrylate, among the structural units derived from methacrylic acid esters, is preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 98 mass% or more, still more preferably 99 mass% or more, and most preferably 100 mass% based on the total structural units of the methacrylic polymer (A).
[0022] The methacrylic polymer (A) may contain a structural unit derived from a monomer other than methacrylic acid ester. Examples of the monomer other than methacrylic acid ester include acrylic acid alkyl esters such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate; acrylic acid aryl esters such as phenyl acrylate; acrylic acid cycloalkyl esters such as cyclohexyl acrylate and norbornenyl acrylate; aromatic vinyl compounds such as styrene and α-methylstyrene; acrylamide; methacrylamide; acrylonitrile; and methacrylonitrile; and vinyl monomers having only one polymerizable carbon-carbon double bond in one molecule.
[0023] Weight average molecular weight Mw of methacrylic polymer (A) A Mw is usually 30,000 or more, preferably 40,000 to 200,000, more preferably 40,000 to 140,000, and further preferably 40,000 to 100,000. A If Mw is 30,000 or more, the impact resistance and toughness of the molded product tend to be improved. A There is no particular upper limit for Mw A When the molecular weight is 200,000 or less, the fluidity of the methacrylic resin or resin composition tends to be at a sufficient level to provide good molding processability.
[0024] The methacrylic polymer (A) has a number average molecular weight Mn A Weight average molecular weight Mw A Ratio (Mw A / Mn A ) is usually 1.0 to 1.4, preferably 1.01 to 1.4, more preferably 1.05 to 1.4, and further preferably 1.05 to 1.3. A / Mn A When a methacrylic polymer (A) having Mw is used, a molded product having excellent mechanical strength can be easily obtained. A and Mn Ais a value calculated based on a chromatogram measured by gel permeation chromatography and converted into the molecular weight of standard polystyrene.
[0025] Gel permeation chromatography can be performed as follows. Tetrahydrofuran is used as the eluent, and two TSKgel SuperMultipore HZM-M columns manufactured by Tosoh Corporation and a SuperHZ4000 column connected in series are used as the column. An HLC-8320 (product number) manufactured by Tosoh Corporation equipped with an RI (differential refractometer) is used as the analyzer. 4 mg of sample resin is dissolved in 5 ml of tetrahydrofuran, and then filtered through a 0.1 μm filter to obtain a sample solution. The temperature of the column oven is set to 40° C., and 20 μl of the sample solution is injected at an eluent flow rate of 0.35 ml / min to measure the chromatogram. The chromatogram is a chart in which the electric signal (detection intensity Y) derived from the refractive index difference between the sample solution and the reference solution is plotted against the elution time (retention time). The conversion of the standard polystyrene into the molecular weight is performed based on a calibration curve. The calibration curve is created by measuring the chromatogram of each standard polystyrene having a molecular weight in the range of 400 to 5,000,000 by gel permeation chromatography and plotting the elution time versus the logarithmic value of the molecular weight.
[0026] In the weight-based differential molecular weight distribution curve of the methacrylic polymer (A), the sum of the weight fraction differential values of components having a molecular weight of 15,000 or less (M≦15,000) is preferably 5% or less, more preferably 3% or less, and even more preferably 2% or less, relative to the sum of the weight fraction differential values of all components. The smaller the sum of the weight fraction differential values of components having a molecular weight of 15,000 or less, the higher the strength of the methacrylic resin composition tends to be. The weight-based differential molecular weight distribution curve is a plot of the logarithm of molecular weight (log(M)) on the horizontal axis and the weight fraction differential value (dw / d(log(M))) obtained by differentiating the weight fraction W by the logarithm of molecular weight (log(M)) on the vertical axis. A and Mn AThe molecular weight of the standard polystyrene is calculated based on the chromatogram used to calculate the molecular weight of the standard polystyrene on the horizontal axis. 1) Draw a baseline on the chromatogram and identify the peaks. 2) Using the logarithm of the molecular weight of the standard polystyrene versus elution time calibration curve (calibration curve), convert the elution time into molecular weight. 3) Calculate the peak area and the weight fraction for each elution time. 4) Plot the logarithm of molecular weight on the horizontal axis and the weight fraction on the vertical axis. 5) The weight fractions are successively integrated, and an integrated molecular weight distribution curve is obtained by plotting the logarithm of the molecular weight on the horizontal axis and the integrated value of the weight fraction on the vertical axis. 6) Calculate the differential value (weight fraction differential value dw / d(log(M))) of the integral molecular weight distribution curve for each molecular weight. 7) Plot the logarithm of the molecular weight, log(M), on the horizontal axis and the weight fraction derivative, dw / d(log(M)), on the vertical axis to obtain a differential molecular weight distribution curve. The total weight fraction differential value in a given molecular weight range can be represented by the area enclosed by the differential molecular weight distribution curve and the line of zero weight fraction differential value in the given molecular weight range.
[0027] The glass transition temperature of the methacrylic polymer (A) is preferably 125° C. or higher, more preferably 127° C. or higher, and even more preferably 129° C. or higher. The upper limit of the glass transition temperature of the methacrylic polymer (A) is preferably 140° C. As the glass transition temperature of the methacrylic polymer (A) increases, the heat resistance of the methacrylic resin or resin composition of the present invention increases, and deformation such as thermal shrinkage tends to be less likely to occur.
[0028] The triad syndiotacticity (rr) of the methacrylic polymer (A) has a lower limit of 63%, preferably 65%, more preferably 72%, and an upper limit of preferably 90%, more preferably 85%, and even more preferably 80%. When the triad syndiotacticity (rr) of the methacrylic polymer (A) is 63% or more, the methacrylic resin or resin composition of the present invention has high heat resistance and tends to be less prone to deformation such as thermal shrinkage. In addition, when the triad syndiotacticity (rr) of the methacrylic polymer (A) is within the above range, the strength of the methacrylic resin or resin composition of the present invention is particularly improved. This is believed to be because the carbonyl-carbonyl interaction between the methacrylic polymer (A) and the methacrylic polymer (B) is improved.
[0029] Here, triad syndiotacticity (rr) is the ratio of two chains (diads) in a chain of three consecutive structural units (triad) that are both racemo (denoted as rr). Note that in the chains (diads) of structural units in a polymer molecule, those with the same configuration are called meso, and those with the opposite configuration are called racemo, and are denoted as m and r, respectively. Triad syndiotacticity (rr) (%) in deuterated chloroform at 30°C 1 The H-NMR spectrum is measured, and the area (X) of the region from 0.6 to 0.95 ppm and the area (Y) of the region from 0.6 to 1.35 ppm when TMS is set to 0 ppm are measured from the spectrum, and the concentration can be calculated using the formula: (X / Y)×100.
[0030] The method for producing the methacrylic polymer (A) is not particularly limited as long as the methacrylic polymer (A) satisfying the above-mentioned physical property values can be obtained. From the viewpoint of productivity, an anionic polymerization method is preferred. More preferably, in the anionic polymerization method, the polymerization temperature, polymerization time, the type and amount of the chain transfer agent, the type and amount of the polymerization initiator, etc. are appropriately set so as to satisfy the above-mentioned physical property values, thereby producing the methacrylic polymer (A).
[0031] Examples of the anionic polymerization method include a method in which anionic polymerization is carried out using an organic alkali metal compound as a polymerization initiator in the presence of a mineral acid salt such as an alkali metal or alkaline earth metal salt (see JP-B-7-25859), a method in which anionic polymerization is carried out using an organic alkali metal compound as a polymerization initiator in the presence of an organoaluminum compound (see JP-A-11-335432), and a method in which anionic polymerization is carried out using an organic rare earth metal complex as a polymerization initiator (see JP-A-6-93060).
[0032] In the anionic polymerization method, it is preferable to use an alkyl lithium such as n-butyl lithium, sec-butyl lithium, isobutyl lithium, or tert-butyl lithium as a polymerization initiator. From the viewpoint of productivity, it is preferable to use an organoaluminum compound in the presence of the alkyl lithium. As the organoaluminum, AlR 1 R 2 R 3 Compounds represented by the formula (R 1 , R 2 and R 3 each independently represents an alkyl group which may have a substituent, a cycloalkyl group which may have a substituent, an aryl group which may have a substituent, an aralkyl group which may have a substituent, an alkoxy group which may have a substituent, an aryloxy group which may have a substituent, or an N,N-disubstituted amino group. 2 and R 3 may be an arylenedioxy group which may have a substituent and which is formed by bonding these. Specific examples of the organoaluminum compound include isobutylbis(2,6-di-tert-butyl-4-methylphenoxy)aluminum, isobutylbis(2,6-di-tert-butylphenoxy)aluminum, isobutyl[2,2'-methylenebis(4-methyl-6-tert-butylphenoxy)]aluminum, and the like. In the anionic polymerization method, ethers, nitrogen-containing compounds, and the like may be coexisted in order to control the polymerization reaction.
[0033] The methacrylic polymer (A) is useful as a resin modifier, and is particularly useful as a modifier for the methacrylic polymer (B).
[0034] The methacrylic polymer (B) is a random polymer mainly containing structural units derived from a methacrylic acid ester.
[0035] Examples of the methacrylic acid ester include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, and butyl methacrylate; aryl methacrylates such as phenyl methacrylate; and cycloalkyl methacrylates such as cyclohexyl methacrylate and norbornenyl methacrylate. Among these, alkyl methacrylates are preferred, and methyl methacrylate is most preferred. The amount of structural units derived from methacrylic acid ester contained in the methacrylic polymer (B) is preferably 80 mass % or more, more preferably 90 mass % or more, based on the total structural units of the methacrylic polymer (B).
[0036] The methacrylic polymer (B) may contain structural units derived from acrylic esters. Examples of acrylic esters include alkyl acrylates such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate; aryl acrylates such as phenyl acrylate; and cycloalkyl acrylates such as cyclohexyl acrylate and norbornenyl acrylate. The amount of structural units derived from acrylic esters contained in the methacrylic polymer (B) is preferably 0 to 20% by mass, more preferably 0 to 10% by mass, based on the total structural units of the methacrylic polymer (B).
[0037] The methacrylic polymer (B) may contain structural units derived from monomers other than methacrylic acid esters and acrylic acid esters. Examples of monomers other than methacrylic acid esters and acrylic acid esters include α,β-unsaturated monocarboxylic acids such as acrylic acid and methacrylic acid; unsaturated group-containing divalent carboxylic acids such as maleic acid, fumaric acid, and itaconic acid; aromatic vinyl compounds such as styrene and α-methylstyrene; α,β-unsaturated nitriles such as acrylonitrile and methacrylonitrile; maleic anhydride, maleimide, N-substituted maleimide, and glutaric anhydride. The amount of structural units derived from monomers other than methyl methacrylate and acrylic acid esters contained in the methacrylic polymer (B) is preferably 20% by mass or less, more preferably 10% by mass or less, based on the total structural units of the methacrylic polymer (B).
[0038] Weight average molecular weight Mw of methacrylic polymer (B) B Mw is preferably 80,000 or more, more preferably 80,000 to 3,000,000, more preferably 120,000 to 2,500,000, and even more preferably 160,000 to 2,000,000. B When the Mw is 80,000 or more, the impact resistance and toughness of the methacrylic resin or resin composition tend to be improved. B There is no particular upper limit for Mw from the standpoint of impact resistance and toughness. B Methacrylic polymers (B) with Mw exceeding 3,000,000 tend to be difficult to manufacture. B When the molecular weight is 160,000 or more, the strength of the methacrylic resin or resin composition is particularly improved. This is believed to be because the carbonyl-carbonyl interaction between the methacrylic polymer (A) and the methacrylic polymer (B) is improved.
[0039] The methacrylic polymer (B) has a number average molecular weight Mn B Weight average molecular weight Mw B Ratio (Mw B / Mn B ) is preferably 1.7 to 2.6, more preferably 1.7 to 2.5, and even more preferably 1.7 to 2.3.B / Mn B When a methacrylic polymer (B) having Mw is used, a molded product having excellent mechanical strength can be easily obtained. B and Mn B is a value calculated based on a chromatogram measured by gel permeation chromatography and converted into the molecular weight of standard polystyrene.
[0040] The methacrylic polymer (B) has a glass transition temperature of preferably 100° C. or higher, more preferably 105° C. or higher. The upper limit of the glass transition temperature of the methacrylic polymer (B) is preferably 140° C. When the glass transition temperature of the methacrylic polymer (B) is within this range, the heat resistance of the methacrylic resin or resin composition is increased, and deformation such as thermal shrinkage tends to be less likely to occur.
[0041] The methacrylic polymer (B) has a triad syndiotacticity (rr) of preferably 45 to 63%, more preferably 49 to 60%. When the triad syndiotacticity (rr) of the methacrylic polymer (B) is within the above range, the heat resistance and molding processability of the methacrylic resin or resin composition tend to be well balanced.
[0042] The method for producing the methacrylic polymer (B) is not particularly limited as long as the methacrylic polymer (B) satisfying the above-mentioned physical property values can be obtained. From the viewpoint of reactive active sites, the method for producing the methacrylic polymer (B) can include radical polymerization, anionic polymerization, etc. From the viewpoint of the form of the polymerization reaction liquid, the method for producing the methacrylic polymer (B) can include emulsion polymerization, solution polymerization, bulk polymerization, suspension polymerization, etc. Among these, from the viewpoint of high productivity and ease of high molecular weight, radical emulsion polymerization, radical bulk polymerization, or radical suspension polymerization is preferred, and radical bulk polymerization is more preferred.
[0043] Specific examples of polymerization initiators used in bulk polymerization or suspension polymerization include t-hexylperoxyisopropyl monocarbonate, t-hexylperoxy 2-ethylhexanoate, 1,1,3,3-tetramethylbutylperoxy 2-ethylhexanoate, t-butylperoxypivalate, t-hexylperoxypivalate, t-butylperoxyneodecanoate, t-hexylperoxyneodecanoate, 1,1,3,3-tetramethylbutylperoxypival ...1,1,3,3-tetramethylbutylperoxypivalate, 1,1,3,3-tetramethylbutylperoxypivalate, 1,1,3,3-tetramethylbutylperoxypivalate, 1,1,3,3-tetramethylbutylperoxypivalate, 1,1,3,3-tetramethylbutylperoxypivalate, 1,1,3,3-tetramethylbutylperoxypivalate, 1,1,3,3-tetramethylbutylperoxypivalate, 1,1,3,3-tetramethylbutylperoxypivalate, 1,1,3,3-tetramethylbutylperoxypivalate, 1, Examples of the polymerization initiator used in emulsion polymerization include peroxides such as tetramethylbutylperoxyneodecanoate, 1,1-bis(t-hexylperoxy)cyclohexane, benzoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, and lauroyl peroxide; and azo compounds such as 2,2'-azobis(2-methylpropionitrile), 2,2'-azobis(2-methylbutyronitrile), and dimethyl 2,2'-azobis(2-methylpropionate). Among these, t-hexylperoxy 2-ethylhexanoate, 1,1-bis(t-hexylperoxy)cyclohexane, and dimethyl 2,2'-azobis(2-methylpropionate) are preferred. Specific examples of the polymerization initiator used in emulsion polymerization include persulfate-based initiators such as potassium persulfate and ammonium persulfate; and redox-based initiators such as persulfoxylate / organic peroxide, and persulfate / sulfite. The polymerization initiator can be used alone or in combination of two or more. The amount of the polymerization initiator used may be set so as to obtain a methacrylic polymer (B) that satisfies the above-mentioned physical property values, and can be appropriately set within the range of, for example, preferably 0.0001 to 0.02 parts by mass, more preferably 0.001 to 0.01 parts by mass, and even more preferably 0.005 to 0.007 parts by mass, relative to 100 parts by mass of the monomer to be subjected to the polymerization reaction.
[0044] The polymerization initiator used in the bulk polymerization generates reactive radicals. The polymerization initiator has a one-hour half-life temperature of preferably 60 to 140° C., more preferably 80 to 120° C. The polymerization initiator also has a hydrogen abstraction ability of preferably 20% or less, more preferably 10% or less, and further preferably 5% or less.
[0045] The hydrogen abstraction ability can be known from technical documents of polymerization initiator manufacturers (for example, NOF Corporation technical document "Hydrogen Abstraction Ability and Initiator Efficiency of Organic Peroxides" (created in April 2003)). The hydrogen abstraction ability can also be measured by a radical trapping method using α-methylstyrene dimer, i.e., the α-methylstyrene dimer trapping method. This measurement is generally performed as follows. First, the polymerization initiator is cleaved in the presence of α-methylstyrene dimer as a radical trapping agent to generate radical fragments. Among the generated radical fragments, radical fragments with low hydrogen abstraction ability are added to the double bond of α-methylstyrene dimer and captured. On the other hand, radical fragments with high hydrogen abstraction ability abstract hydrogen from cyclohexane, generating a cyclohexyl radical, which is added to the double bond of α-methylstyrene dimer and captured, generating a cyclohexane capture product. Therefore, cyclohexane or cyclohexane trapping products are quantified, and the ratio (molar fraction) of radical fragments with high hydrogen abstraction power to the theoretical amount of radical fragments generated is calculated, and this is taken as the hydrogen abstraction power.
[0046] Examples of chain transfer agents used in bulk polymerization include alkyl mercaptans such as n-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, 1,4-butanedithiol, 1,6-hexanedithiol, ethylene glycol bisthiopropionate, butanediol bisthioglycolate, butanediol bisthiopropionate, hexanediol bisthioglycolate, hexanediol bisthiopropionate, trimethylolpropane tris-(β-thiopropionate), and pentaerythritol tetrakisthiopropionate. Among these, monofunctional alkyl mercaptans such as n-octyl mercaptan and n-dodecyl mercaptan are preferred. These chain transfer agents can be used alone or in combination of two or more. The amount of the chain transfer agent used may be set so as to obtain a methacrylic polymer (B) that satisfies the above-mentioned physical property values, and may be appropriately set within the range of, for example, preferably 0 to 0.5 parts by mass, more preferably 0.05 to 0.4 parts by mass, and even more preferably 0.06 to 0.25 parts by mass, relative to 100 parts by mass of the monomer to be subjected to the polymerization reaction. The amount of the chain transfer agent used may be appropriately set within the range of, preferably 2500 to 10000 parts by mass, more preferably 3000 to 9000 parts by mass, relative to 100 parts by mass of the polymerization initiator.
[0047] In the suspension polymerization, a suspension stabilizer can be used. Examples of the suspension stabilizer include organic colloidal polymeric substances, inorganic colloidal polymeric substances, inorganic fine particles, and combinations of these with surfactants.
[0048] In emulsion polymerization, an emulsifier can be used. Examples of the emulsifier include anionic emulsifiers such as dialkyl sulfosuccinates (e.g., sodium dioctyl sulfosuccinate, sodium dilauryl sulfosuccinate), alkyl benzene sulfonates (e.g., sodium dodecyl benzene sulfonate), and alkyl sulfates (e.g., sodium dodecyl sulfate); nonionic emulsifiers such as polyoxyethylene alkyl ethers and polyoxyethylene nonyl phenyl ether; nonionic and anionic emulsifiers such as polyoxyethylene nonyl phenyl ether sulfates (e.g., sodium polyoxyethylene nonyl phenyl ether sulfate), polyoxyethylene alkyl ether sulfates (e.g., sodium polyoxyethylene alkyl ether sulfate), and alkyl ether carboxylates (e.g., sodium polyoxyethylene tridecyl ether acetate). These emulsifiers may be used alone or in combination of two or more. In addition, the average number of repeating ethylene oxide units in the example compounds of the nonionic emulsifiers and nonionic / anionic emulsifiers is preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less, in order to prevent the foaming property of the emulsifier from becoming extremely high.
[0049] In emulsion polymerization or suspension polymerization, the resin is extracted from the reaction product liquid by a known method after the polymerization reaction is completed. In emulsion polymerization, the resin can be extracted from the reaction product liquid (emulsion) by salting-out coagulation method, freeze-coagulation method, spray drying method, etc. Among these, the salting-out coagulation method and freeze-coagulation method are preferred because impurities contained in the resin can be easily removed by washing with water. It is preferable to filter the emulsion with a wire mesh with an opening of 50 μm or less before the coagulation step, since foreign matter mixed in the emulsion can be removed.
[0050] The methacrylic resin of the present invention has a shear rate of 122 s -1 And melt viscosity η at 260℃ B However, the shear rate of the methacrylic polymer (A) is 122 s -1 And melt viscosity η at 260℃ A Higher than . Melt viscosity η B and melt viscosity η A The difference between is preferably 1000 Pa·s or more, and more preferably 1500 Pa·s or more. In addition, the methacrylic resin of the present invention has a weight average molecular weight Mw of the methacrylic polymer (B). B is the weight average molecular weight Mw A It is 2.5 times or more, preferably 3 times or more.
[0051] The methacrylic resin of the present invention has a refractive index n dA and the refractive index n of the methacrylic polymer (B) dB Absolute difference between |n dA -n dB is preferably 0.005 or less.
[0052] The amount of the methacrylic polymer (A) contained in the methacrylic resin of the present invention is preferably 2 to 39 mass%, more preferably 5 to 30 mass%, even more preferably 5 to 20 mass%, and most preferably 5 to 16 mass%, based on the methacrylic resin, from the viewpoint of achieving both heat resistance and moldability or surface smoothness in a good condition.
[0053] The amount of the methacrylic polymer (B) contained in the methacrylic resin of the present invention is preferably 61 to 98 mass%, more preferably 70 to 95 mass%, even more preferably 80 to 95 mass%, and most preferably 84 to 95 mass%, relative to the methacrylic resin, from the viewpoint of achieving a good balance between heat resistance or mechanical strength and molding processability.
[0054] In the methacrylic resin of the present invention, the mass ratio of the methacrylic polymer (A) to the methacrylic polymer (B) is from 2 / 98 to 39 / 61, more preferably from 5 / 95 to 30 / 70, and further preferably from 5 / 95 to 20 / 80.
[0055] The methacrylic resin of the present invention has a peak top molecular weight M Pt However, the peak top molecular weight M is preferably 100,000 to 2,000,000, more preferably 120,000 to 2,000,000, and further preferably 160,000 to 2,000,000. Pt When the molecular weight is within this range, a molded product having excellent strength, hardness, and surface smoothness can be obtained.
[0056] The methacrylic resin of the present invention has a peak top molecular weight M Ph Components with a molecular weight of 1 / 20 or less (M≦1 / 20M Ph ) is preferably 2% or less, more preferably 1.5% or less, based on the total weight fraction differential values of all components. In the weight-based differential molecular weight distribution curve of the methacrylic resin of the present invention, the sum of the weight fraction differential values of components having a molecular weight of 15,000 or less (M≦15,000) is preferably 2% or less, more preferably 1.75% or less, relative to the sum of the weight fraction differential values of all components. By having a small amount of the above-mentioned low molecular weight components, the effects of the methacrylic resin or resin composition of the present invention are further improved.
[0057] The methacrylic resin composition of the present invention contains the methacrylic resin of the present invention. The methacrylic resin composition of the present invention may contain the methacrylic resin of the present invention and an additional resin other than the methacrylic resin. Examples of other resins include olefin-based thermoplastic resins such as polyethylene, polypropylene, ethylene-propylene copolymers, and poly(4-methyl-1-pentene); halogen-containing thermoplastic resins such as vinyl chloride and chlorinated vinyl resins; acrylic thermoplastic resins; styrene-based thermoplastic resins such as polystyrene, styrene-methyl methacrylate copolymer, styrene-acrylonitrile copolymer, and acrylonitrile-butadiene-styrene copolymer; polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyamides such as nylon 6, nylon 66, and nylon 610; polyacetal; polycarbonate; polyphenylene oxide; polyphenylene sulfide; polyether ether ketone; polysulfone; polyether sulfone; polyoxybenzylene; polyamide imide; rubbery polymers such as ABS resins and ASA resins blended with polybutadiene rubber and acrylic rubber, and cellulose resins such as polyvinyl butyral and cellulose acylate. In the methacrylic resin composition of the present invention, these other resins may be in a compatible state with the methacrylic resin of the present invention, or may be in a phase-separated state.
[0058] The methacrylic resin composition of the present invention may contain the methacrylic resin of the present invention, an elastomer, and, if necessary, the other resins described above.
[0059] The elastomer is mixed with the methacrylic resin in a compatible state or in a phase-separated state. The elastomer is preferably mixed with the methacrylic resin in a phase-separated state to form a dispersed phase. The shape of the dispersed phase is not particularly limited, and examples thereof include a spherical shape, an ellipsoidal shape, a rod shape, a flat shape, and a string shape. The size of the dispersed phase is not particularly limited, and the average particle size is preferably 0.05 to 1 μm, more preferably 0.07 to 0.5 μm, and even more preferably 0.10 to 0.4 μm.
[0060] The elastomer is preferably made of a polymer containing a structural unit derived from an acrylic acid ester. Examples of the acrylic acid ester include alkyl acrylates such as methyl acrylate, ethyl acrylate, and butyl acrylate; aryl acrylates such as phenyl acrylate and benzyl acrylate; and cycloalkyl acrylates such as cyclohexyl acrylate and norbornenyl acrylate. Among these, alkyl acrylates are preferred, and butyl acrylate is most preferred. The amount of structural units derived from acrylic ester contained in the elastomer is preferably 30% by mass or more, more preferably 35% by mass or more and 90% by mass or less, and further preferably 40% by mass or more and 80% by mass or less.
[0061] The elastomer may have a structural unit derived from a vinyl monomer having only one polymerizable carbon-carbon double bond in one molecule, in addition to the structural unit derived from an acrylic ester. Examples of the vinyl monomer include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, and 2-ethylhexyl methacrylate; aryl methacrylates such as phenyl methacrylate; cycloalkyl methacrylates such as cyclohexyl methacrylate and norbornenyl methacrylate; aralkyl methacrylates such as benzyl methacrylate; aromatic vinyl compounds such as styrene and α-methylstyrene; acrylamide; methacrylamide; acrylonitrile; and methacrylonitrile.
[0062] The amount of the elastomer contained in the methacrylic resin composition of the present invention is preferably 0 to 50% by mass, more preferably 0 to 40% by mass, and further preferably 0 to 30% by mass, based on the mass of the methacrylic resin composition. The amount of the elastomer can be appropriately set from the viewpoints of chemical resistance, heat resistance, flexural modulus, processability, etc.
[0063] The elastomer is not particularly limited by the form of its molecular chain, and examples thereof include linear polymer elastomers (e.g., random copolymer elastomers, block copolymer elastomers, etc.), branched polymer elastomers (e.g., graft copolymer elastomers, star block copolymer elastomers), etc. Among these, the elastomer preferably contains a block copolymer elastomer consisting of a polymer block mainly having structural units derived from a methacrylic acid ester and a polymer block having structural units derived from an acrylic acid ester.
[0064] The elastomer may be particles containing a crosslinked rubber polymer containing structural units derived from an acrylic acid ester (hereinafter referred to as crosslinked rubber particles).
[0065] The average particle size of the crosslinked rubber particles is preferably 0.05 to 1 μm, more preferably 0.07 to 0.5 μm, and even more preferably 0.10 to 0.4 μm. By using crosslinked rubber particles having an average particle size within such a range, particularly an average particle size of 0.15 to 0.3 μm, toughness can be achieved without impairing rigidity or surface hardness even with a small amount of the crosslinked rubber particles. The average particle size is the average value in the volume-based particle size distribution measured by a light scattering method.
[0066] The crosslinked rubber particles preferably comprise an inner layer and an outermost layer covering the inner layer. The inner layer may comprise only a core layer, or may comprise a core layer and an intermediate layer covering the core layer. The intermediate layer may be a single layer made of one polymer, or may be a multilayer made of different polymers. From the viewpoint of transparency, the crosslinked rubber particles are made of two adjacent layers with a refractive index n d The difference is preferably less than 0.01, more preferably less than 0.008, and even more preferably less than 0.005.
[0067] The mass ratio of the inner layer to the outermost layer in the crosslinked rubber particle is preferably 60 / 40 to 95 / 5, and more preferably 70 / 30 to 90 / 10.
[0068] Examples of crosslinked rubber particles include two-layer particles having a core layer made of a crosslinked rubber polymer (II) and an outermost layer made of a thermoplastic polymer (III) covering the core layer; three-layer particles having a core layer made of a crosslinked polymer (I), an intermediate layer made of a crosslinked rubber polymer (II) covering the core layer, and an outermost layer made of a thermoplastic polymer (III) covering the intermediate layer; and four-layer particles having a core layer made of a crosslinked rubber polymer (II), a first intermediate layer made of a crosslinked polymer (I) covering the core layer, a second intermediate layer made of a crosslinked rubber polymer (II) covering the first intermediate layer, and an outermost layer made of a thermoplastic polymer (III) covering the second intermediate layer.
[0069] The thermoplastic polymer (III) is a polymer comprising structural units derived from an alkyl methacrylate ester having an alkyl group having 1 to 8 carbon atoms and, if necessary, structural units derived from a monofunctional monomer other than the alkyl methacrylate ester. It is preferable that the thermoplastic polymer (III) does not contain structural units derived from a polyfunctional monomer.
[0070] The amount of structural units derived from an alkyl methacrylate ester having an alkyl group having 1 to 8 carbon atoms constituting the thermoplastic polymer (III) is 80 to 100 mass %, preferably 85 to 95 mass %, based on the mass of the thermoplastic polymer (III).
[0071] Examples of methacrylic acid alkyl esters having an alkyl group having 1 to 8 carbon atoms (hereinafter sometimes referred to as methacrylic acid C1-8 alkyl esters) include methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, propyl methacrylate, cyclohexyl methacrylate, etc. Of these, methyl methacrylate is preferred.
[0072] The amount of structural units derived from monofunctional monomers other than C1-8 alkyl methacrylate constituting the thermoplastic polymer (III) is 0 to 20% by mass, preferably 5 to 15% by mass, based on the mass of the thermoplastic polymer (III). Examples of monofunctional monomers other than methacrylic acid C1-8 alkyl esters include acrylic esters such as methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and propyl acrylate; aromatic vinyl compounds such as styrene, p-methylstyrene, and α-methylstyrene; and maleimide compounds such as N-propylmaleimide, N-cyclohexylmaleimide, and No-chlorophenylmaleimide.
[0073] The amount of the thermoplastic polymer (III) is preferably 40 to 75% by mass, more preferably 50 to 70% by mass, and further preferably 55 to 65% by mass, based on the mass of the crosslinked rubber particles.
[0074] The crosslinked polymer (I) comprises structural units derived from methyl methacrylate, structural units derived from a monofunctional monomer other than methyl methacrylate, and structural units derived from a polyfunctional monomer.
[0075] The amount of structural units derived from methyl methacrylate constituting the crosslinked polymer (I) is 40 to 98.5% by mass, preferably 45 to 95% by mass, based on the mass of the crosslinked polymer (I).
[0076] The amount of structural units derived from monofunctional monomers other than methyl methacrylate constituting the crosslinked polymer (I) is 1 to 59.5% by mass, preferably 5 to 55% by mass, based on the mass of the crosslinked polymer (I). Examples of monofunctional monomers other than methyl methacrylate include methacrylic acid esters other than methyl methacrylate, such as ethyl methacrylate, butyl methacrylate, and cyclohexyl methacrylate; acrylic acid esters such as methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and propyl acrylate; aromatic vinyl compounds such as styrene, p-methylstyrene, and α-methylstyrene; and maleimide compounds such as N-propylmaleimide, N-cyclohexylmaleimide, and No-chlorophenylmaleimide.
[0077] The amount of the structural unit derived from the polyfunctional monomer constituting the crosslinked polymer (I) is 0.05 to 0.4 mass %, preferably 0.1 to 0.3 mass %, based on the mass of the crosslinked polymer (I). Examples of the polyfunctional monomer include ethylene glycol dimethacrylate, propylene glycol dimethacrylate, triethylene glycol dimethacrylate, hexanediol dimethacrylate, ethylene glycol diacrylate, propylene glycol diacrylate, triethylene glycol diacrylate, allyl methacrylate, and triallyl isocyanurate.
[0078] The amount of the crosslinked polymer (I) is preferably from 5 to 40% by mass, more preferably from 7 to 35% by mass, and further preferably from 10 to 30% by mass, based on the mass of the crosslinked rubber particles.
[0079] The crosslinked rubber polymer (II) comprises structural units derived from an alkyl acrylate ester having an alkyl group having 1 to 8 carbon atoms and / or structural units derived from a conjugated diene, and structural units derived from a polyfunctional monomer.
[0080] The amount of structural units derived from an alkyl acrylate having an alkyl group having 1 to 8 carbon atoms and / or structural units derived from a conjugated diene constituting the crosslinked rubber polymer (II) is 98.3 to 99 mass %, preferably 95 to 98 mass %, based on the mass of the crosslinked rubber polymer (II).
[0081] Examples of the alkyl acrylate ester having an alkyl group having 1 to 8 carbon atoms include methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and propyl acrylate.
[0082] Examples of conjugated dienes include 1,3-butadiene and isoprene.
[0083] The amount of structural units derived from the polyfunctional monomer constituting the crosslinked rubber polymer (II) is 1 to 1.7 mass %, preferably 1.2 to 1.6 mass %, more preferably 1.3 to 1.5 mass %, based on the mass of the crosslinked rubber polymer (II). Examples of the polyfunctional monomer include ethylene glycol dimethacrylate, propylene glycol dimethacrylate, triethylene glycol dimethacrylate, hexanediol dimethacrylate, ethylene glycol diacrylate, propylene glycol diacrylate, triethylene glycol diacrylate, allyl methacrylate, and triallyl isocyanurate.
[0084] From the viewpoint of improving flex resistance, the ratio of the mass of the structural units derived from the polyfunctional monomer in the crosslinked polymer (I) to the mass of the structural units derived from the polyfunctional monomer in the crosslinked rubber polymer (II) is preferably 0.05 to 0.25, more preferably 0.1 to 0.2. The glass transition temperature of the crosslinked rubber polymer (II) is preferably lower than the glass transition temperature of the crosslinked polymer (I).
[0085] The amount of the crosslinked rubber polymer (II) is preferably from 20 to 55% by mass, more preferably from 25 to 45% by mass, and further preferably from 30 to 40% by mass, based on the mass of the crosslinked rubber particles.
[0086] The molecular chains of the crosslinked polymer (I) and the crosslinked rubber polymer (II) are preferably connected by a graft bond. The molecular chains of the crosslinked rubber polymer (II) and the thermoplastic polymer (III) are preferably connected by a graft bond. The graft bond is a bond that connects the main chain and the branch portion produced by a polymerization method (graft polymerization method) that uses a substituent bonded to the main chain of an already completed polymer as a reactive site and extends a new branch portion from the reactive site.
[0087] The resin composition of the present invention may contain conventional additives to the extent that the physical properties such as transparency, strength, etc. are not impaired. Examples of additives that can be used include ultraviolet absorbers, stabilizers, release agents, antistatic agents, flame retardants, plasticizers, dispersants, flow control agents, leveling agents, antifoaming agents, surface modifiers, heat resistance improvers, water repellency improvers, and optical enhancers.
[0088] Examples of the plasticizer include phthalate esters, fatty acid esters, trimellitates, phosphates, polyesters, and epoxy plasticizers.
[0089] Examples of the ultraviolet absorbent include benzotriazole-based, 2-hydroxybenzophenone-based, and salicylic acid phenyl ester-based, etc. For example, triazoles such as 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, and 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, and benzophenones such as 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, and 2,2'-dihydroxy-4-methoxybenzophenone can be exemplified.
[0090] Examples of the release agent include higher alcohols such as cetyl alcohol and stearyl alcohol; and higher fatty acid esters of glycerin such as stearate monoglyceride and stearate diglyceride.
[0091] Examples of the flame retardant include organic halogen flame retardants such as tetrabromobisphenol A, decabromodiphenyl oxide, and brominated polycarbonate; and non-halogen flame retardants such as antimony oxide, aluminum hydroxide, zinc borate, and tricresyl phosphate.
[0092] The antistatic agent may, for example, be stearamidopropyl dimethyl-β-hydroxyethyl ammonium nitrate.
[0093] Examples of the surface modifier include polybutadiene and CTBN (carboxylate-terminated nitrile butadiene rubber).
[0094] Examples of the stabilizer include 2,6-di-t-butyl-4-methylphenol and 6-ethoxy-1,2-dihydro-2,2,4-trimethylquinoline.
[0095] The leveling agent may include a fluorine-based surfactant.
[0096] The antifoaming agent may include an acrylic copolymer, silicone, and the like.
[0097] These additives may be used alone or in combination of two or more. The amount of the additive may be, for example, 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the methacrylic resin composition.
[0098] The resin composition of the present invention may be in a solid state or a liquid state. The solid resin composition can be produced or prepared by mixing the methacrylic polymer (A), the methacrylic polymer (B), and, if necessary, additional components such as other resins, elastomers, and additives. The mixing can be performed by melt kneading using a mixing means such as a mixer such as a ribbon blender, a tumble mixer, or a Henschel mixer, or a kneader such as an open roller, a kneader, a Banbury mixer, or an extruder. These mixing means may be used alone or in combination of two or more. The resin composition of the present invention is not limited by the mixing order of the methacrylic polymer (A), the methacrylic polymer (B), and other components mixed as necessary. For example, the methacrylic polymer (A) and the methacrylic polymer (B) may be mixed to obtain the methacrylic resin of the present invention, and then other components may be mixed therewith to obtain the resin composition of the present invention; the methacrylic polymer (A), the methacrylic polymer (B) and other components may be mixed together to obtain the resin composition of the present invention; the methacrylic polymer (A) and other components may be mixed together and then the methacrylic polymer (B) may be mixed therewith to obtain the resin composition of the present invention; or the methacrylic polymer (B) and other components may be mixed together and then the methacrylic polymer (A) may be mixed therewith to obtain the resin composition of the present invention.
[0099] The liquid resin composition is obtained by dissolving or dispersing the methacrylic polymer (A), the methacrylic polymer (B), and other components as required in a liquid medium. Examples of the liquid medium include hydrocarbons (benzene, toluene, etc.), halogen-based solvents (dichloromethane, etc.), ethers (diethyl ether, tetrahydrofuran, etc.), esters (ethyl acetate, etc.), ketones (acetone, ethyl methyl ketone, diisopropyl ketone, cyclohexanone, etc.), and alcohols (methanol, ethanol, butanol, etc.). These liquid media may be used alone or in combination of two or more. The procedure for adding the methacrylic polymer (A), the methacrylic polymer (B), and other components as required to the liquid medium is not particularly limited.
[0100] The molded article of the present invention contains the methacrylic resin or resin composition of the present invention. The molded article of the present invention can be obtained by subjecting the methacrylic resin or solid resin composition of the present invention to molding using, for example, an injection molding method, an injection compression molding method, an extrusion molding method (e.g., a T-die method, an inflation method, etc.), a calendar method, a thermoforming method (particularly, a hot press method), a transfer molding method, a blow molding method, a melt casting method, or the like. The molded article of the present invention can be obtained by molding the liquid resin composition of the present invention (for example, a dope) using, for example, a solvent casting method.
[0101] The film or sheet, which is one embodiment of the molded article of the present invention, may be one that has not been subjected to a stretching treatment (unstretched film) or may be a stretched film that has been subjected to a stretching treatment. The film of the present invention can be used as an optical film or optical sheet. The stretching may be either uniaxial stretching (for example, longitudinal stretching or transverse stretching) or biaxial stretching (for example, equal stretching or biased stretching). The stretching ratio may be, for example, about 1.1 to 10 times in each direction (or one direction) in uniaxial stretching and biaxial stretching, preferably about 1.2 to 5 times, and more preferably about 1.3 to 3 times. The strength of the film of the present invention may be improved by stretching. The thickness of the film is, for example, 1 to 1000 μm, preferably 3 to 800 μm, more preferably 5 to 500 μm, and most preferably 20 to 200 μm.
[0102] The dope of the present invention contains the methacrylic resin of the present invention, an organic solvent, and other components as necessary. Examples of organic solvents preferably used in the dope include halogenated hydrocarbons such as dichloromethane; and alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, t-butanol, 1-pentanol, 2-methyl-2-butanol, and cyclohexanol. The amount of the methacrylic resin of the present invention contained in the dope is preferably 5 to 70% by mass, more preferably 10 to 60% by mass, and even more preferably 15 to 50% by mass. The amount of the organic solvent contained in the dope is preferably 30 to 95% by mass, more preferably 40 to 90% by mass, and even more preferably 50 to 85% by mass.
[0103] The dope of the present invention may contain additives for solvent casting. Examples of the additives for solvent casting include moisture permeability reducing compounds, peeling promoters, retardation (Rth) control agents, inorganic fine particles (matting agents), plasticizers such as phthalate esters and phosphate esters, Re expression agents, ultraviolet absorbing agents, and antioxidants.
[0104] The dope is preferably prepared at a temperature of 0°C or higher (room temperature or high temperature). The dope can be prepared by mixing the methacrylic resin, the organic solvent, and, if necessary, other components and, if necessary, solvent casting additives. The mixing procedure is not particularly limited, and for example, a mixture of each component may be added to an organic solvent to dissolve, each component may be added sequentially to an organic solvent during stirring to dissolve, or solutions of each component may be prepared in advance and mixed. The dissolution of the methacrylic resin or resin composition of the present invention may be performed at normal pressure, below the boiling point of the main solvent, or above the boiling point of the main solvent under pressure. In addition, it may be performed by a cooling dissolution method as described in JP-A-9-95544, JP-A-9-95557, or JP-A-9-95538, or at a high pressure as described in JP-A-11-21379. Among these, it is preferable to dissolve the methacrylic resin or resin composition of the present invention by applying pressure at a temperature equal to or higher than the boiling point of the main solvent.
[0105] The method for producing the film of the present invention includes casting the dope of the present invention on a support to obtain a liquid film, and removing the organic solvent from the liquid film. The casting of the dope is performed, for example, by supplying the dope from a storage tank to a die using a pump, discharging the dope from a die slit, and applying the dope to a rotating metallic endless belt. The thickness of the liquid film is adjusted so that the film thickness is preferably 20 to 200 μm from the viewpoint of film strength and processability. The thickness of the liquid film can be adjusted by changing the amount of dope supplied, the speed of the endless belt (support), etc. A solid film is obtained on the support by removing the organic solvent, and the solid film is peeled off from the support. Since the organic solvent may remain in the solid film peeled off from the support, the solid film can be subjected to a drying treatment. The drying treatment can be performed, for example, under conditions in which the time required for the amount of organic solvent remaining in the solid film to decrease from 20% by mass to 0.1% by mass is preferably less than 40 minutes, more preferably 30 minutes or less, and even more preferably 25 minutes or less. Furthermore, the film after drying may be subjected to a heat treatment, a stretching treatment, etc. The descriptions in paragraphs
[0617] to
[0889] of JP2005-104148A regarding the structures of the casting die, the reduced pressure chamber, the support, etc., the co-casting, the peeling method, the stretching, the drying conditions in each step, the handling method, the curl, the winding method after flatness correction, the solvent recovery method, the film recovery method, etc. are quoted here.
[0106] The present invention will be described in more detail below with reference to examples and comparative examples. Note that the present invention is not limited to the following examples. The present invention also includes all aspects that are formed by any combination of the items expressing the technical features, such as the characteristic values, forms, manufacturing methods, and uses, described above.
[0107] The physical properties of the methacrylic polymer, etc., and the methacrylic resin, the methacrylic resin composition and the dope were evaluated as follows.
[0108] (Polymerization conversion rate) A column (InertCap 1 manufactured by GL Sciences Inc.; df=0.4 μm, 0.25 mm I.D.×60 m) was connected to a gas chromatograph GC-14A manufactured by Shimadzu Corporation, and measurements were performed under the following conditions: injection temperature was 180° C., detector temperature was 180° C., and column temperature was increased from 60° C. (held for 5 minutes) to 200° C. at a rate of 10° C. / min and then held for 10 minutes. The polymerization conversion was calculated based on the results.
[0109] (Triad syndiotacticity (rr), imidization rate) Resin samples were tested under the following conditions: 1 H-NMR spectrum was measured. Equipment: Nuclear magnetic resonance equipment (Bruker ULTRA SHIELD 400 PLUS) Solvent: deuterated chloroform Measured nuclides: 1 H Measurement temperature: room temperature Number of times accumulated: 64 1 In the H-NMR spectrum, the area (X) of the region from 0.6 to 0.95 ppm and the area (Y) of the region from 0.6 to 1.35 ppm when TMS was set to 0 ppm were measured, and the value calculated by (X / Y) × 100 was taken as the triad syndiotacticity (rr) (%). 1 In the H-NMR spectrum, the area (A) of the peak derived from the O-CH3 group in the methyl methacrylate unit at around 3.5 to 3.8 ppm and the area (B) of the peak derived from the N-CH3 group in the N-methylglutarimide unit at around 3.0 to 3.3 ppm were measured, and the imidization rate was calculated by [B / (A+B)]×100.
[0110] [Weight average molecular weight Mw, number average molecular weight Mn, peak top molecular weight M Pt ] Chromatograms were measured using gel permeation chromatography (GPC) under the following conditions, and the values converted to the molecular weight of standard polystyrene (Mw, Mn, M PtThe baseline was defined as a line connecting the point where the slope of the peak on the high molecular weight side of the GPC chart changes from zero to positive as viewed from the early retention time, and the point where the slope of the peak on the low molecular weight side changes from negative to zero as viewed from the early retention time. GPC equipment: Tosoh Corporation, HLC-8320 Detector: Differential refractive index detector Column: Two TSKgel SuperMultipore HZM-M columns and a SuperHZ4000 column manufactured by Tosoh Corporation were connected in series. Eluent: Tetrahydrofuran Eluent flow rate: 0.35ml / min Column temperature: 40℃ Calibration curve: Created using data from 10 standard polystyrene points
[0111] (Melt viscosity η) After drying the resin sample at 80°C for 12 hours, it was subjected to a temperature test at 260°C and a shear rate of 122 sec using a Capillograph 1D manufactured by Toyo Seiki Co., Ltd. -1 The melt viscosity η was measured under the following conditions.
[0112] (Refractive index n d ) The refractive index of the resin sample was measured at a wavelength of 587.6 nm (helium d line) using "KPR-200" manufactured by Kalnew Optical Co., Ltd.
[0113] (Average particle size) The rubber particle dispersion sample was measured by the light scattering method (volume conversion) using a laser diffraction / scattering type particle size distribution measuring device LA-910 manufactured by Horiba, Ltd. The median diameter was used as the particle size.
[0114] (glass transition temperature Tg) In accordance with JIS K7121, a DSC curve was measured using a differential scanning calorimeter (Shimadzu Corporation, DSC-50 (product number)) by heating a resin sample to 230°C, then cooling to room temperature, and then heating from room temperature to 230°C at a rate of 10°C / min. The midpoint glass transition temperature determined from the DSC curve measured during the second heating was taken as the glass transition temperature in the present invention.
[0115] (Charpy impact strength, Rockwell hardness, transparency I) The resin sample was subjected to hot press molding at 260°C to obtain a molded sample of 80 mm x 10 mm x 4 mm. The molded sample was measured for unnotched Charpy impact strength using a digital impact tester manufactured by Toyo Seiki Co., Ltd. in accordance with JIS K7111 1eU. The measurement was performed 10 times, and the average value was taken as the Charpy impact strength. The Rockwell hardness of the molded product samples was measured using a Rockwell hardness tester (manufactured by Toyo Seiki Co., Ltd., Rockwell hardness tester) in accordance with JIS K7202. The haze of the molded product samples was measured using a haze meter (HM-150, manufactured by Murakami Color Research Laboratory) in accordance with JIS K7136, and transparency I was evaluated according to the following criteria. Good: Haze is less than 5%. ×: Haze is 5% or more.
[0116] (Drying time) A dope with a solid content concentration of 16% by mass was cast onto a metal support so that the thickness after drying would be 56 μm. When the remaining amount of organic solvent reached 20% by mass after air drying, the solid film obtained on the support was peeled off from the support. The peeled solid film was trimmed to obtain a solid film sample of 6 cm x 6 cm. The solid film sample was fixed to a metal frame and dried at normal pressure at 140°C with a damper opening of 50% using an Espec PHH-202 circulating thermostatic chamber. The remaining amount of organic solvent was measured every 5 minutes. The remaining amount of solvent can be expressed by the following formula. Remaining amount of solvent (mass%)=[(XY) / Y]×100 Here, X is the mass of the solid film during drying, and Y is the mass of the solid film when the drying reaches equilibrium. The measurement was performed twice and the average value was calculated. A drying characteristic curve was created by plotting the drying time on the horizontal axis and the remaining amount of organic solvent on the vertical axis. From the drying characteristic curve, the drying time when the remaining amount of organic solvent was 0.1 mass% was obtained.
[0117] (Surface smoothness) A fluorescent light was reflected on the surface of a solid film sample having a residual organic solvent amount of 0.1% by mass, and the reflected image was observed with the naked eye to judge the surface smoothness according to the following criteria. ×: Fluorescent light image fluctuates 〇: The fluorescent light image does not fluctuate
[0118] (Transparency II) For solid film samples with a residual organic solvent content of 0.1 mass %, the haze was measured using a haze meter (HM-150, manufactured by Murakami Color Laboratory) in accordance with JIS K7136, and transparency II was evaluated according to the following criteria. Good: Haze is less than 1%. ×: Haze is 1% or more.
[0119] (Film impact resistance) A solid film sample with a residual organic solvent content of 0.1% by mass was trimmed to obtain a test piece with a length of 60 mm and a width of 10 mm. It was folded once over the entire width direction of 30 mm from the edge so that the crease was on the outside. At this time, it was observed whether it separated into two or more pieces. This was done three times, and the impact resistance of the film was judged according to the following criteria. ○: No breaks all three times ×: Breaks at least once out of three times
[0120] Production Example 1 (Production of Methacrylic Polymer (A-1)) The inside of an autoclave equipped with a stirring blade and a three-way cock was replaced with nitrogen. 1600 kg of toluene, 60 kg of 1,2-dimethoxyethane, 42.1 kg (24.3 mol) of a toluene solution of isobutylbis(2,6-di-t-butyl-4-methylphenoxy)aluminum with a concentration of 0.45 M, and 4.82 kg (8.1 mmol) of a sec-butyllithium solution with a concentration of 1.3 M (solvent: cyclohexane 95% by mass / n-hexane 5% by mass) were charged into the autoclave at room temperature. 550 kg of methyl methacrylate purified by distillation was added dropwise to the autoclave over 30 minutes at 15° C. while stirring. After the dropwise addition, the autoclave was stirred for 90 minutes at 15° C. The color of the solution changed from yellow to colorless. At this point, the polymerization conversion rate of methyl methacrylate was 100%. 1500 kg of toluene was added to the obtained solution to dilute it. The diluted solution was poured into a large amount of methanol to obtain a precipitate. The obtained precipitate was dried at 80° C. and 140 Pa for 24 hours to obtain a methacrylic polymer (A-1). Methacrylic polymer (A-1) had Mw of 70,000, a proportion of components with a molecular weight of 15,000 or less (M≦15,000) of 0.17% by mass, a melt viscosity η of 1,200 Pa s, Mw / Mn of 1.1, triadosyndiotacticity (rr) of 75%, Tg of 131°C, and the amount of structural units derived from methyl methacrylate was 100% by mass. The physical properties of methacrylic polymer (A-1) are shown in Table 1.
[0121] Production Example 2 (Production of Methacrylic Polymer (A-2)) The inside of an autoclave equipped with a stirring blade and a three-way cock was replaced with nitrogen. 1600 kg of toluene, 80 kg of 1,2-dimethoxyethane, 73.3 kg (42.3 mol) of a toluene solution of isobutylbis(2,6-di-t-butyl-4-methylphenoxy)aluminum with a concentration of 0.45 M, and 8.44 kg (14.1 mmol) of a sec-butyllithium solution with a concentration of 1.3 M (solvent: cyclohexane 95% by mass / n-hexane 5% by mass) were charged into the autoclave at room temperature. 550 kg of methyl methacrylate purified by distillation was added dropwise to the autoclave over 30 minutes at 15° C. while stirring. After the dropwise addition, the autoclave was stirred for 90 minutes at 15° C. The color of the solution changed from yellow to colorless. At this point, the polymerization conversion rate of methyl methacrylate was 100%. 1500 kg of toluene was added to the obtained solution to dilute it. The diluted solution was poured into a large amount of methanol to obtain a precipitate. The obtained precipitate was dried at 80° C. and 140 Pa for 24 hours to obtain a methacrylic polymer (A-2). Methacrylic polymer (A-2) had an Mw of 40,000, a proportion of components with a molecular weight of 15,000 or less (M≦15,000) of 1.52 mass%, a melt viscosity η of 450 Pa s, an Mw / Mn of 1.1, a triadosyndiotacticity (rr) of 75%, a Tg of 130°C, and 100 mass% of structural units derived from methyl methacrylate. The physical properties of methacrylic polymer (A-2) are shown in Table 1.
[0122] Production Example 3 (Production of Methacrylic Polymer (A-3)) The inside of an autoclave equipped with a stirring blade and a three-way cock was replaced with nitrogen. 1600 kg of toluene, 110 kg of 1,2-dimethoxyethane, 119.0 kg (68.7 mol) of a toluene solution of isobutylbis(2,6-di-t-butyl-4-methylphenoxy)aluminum with a concentration of 0.45 M, and 13.71 kg (22.9 mmol) of a sec-butyllithium solution with a concentration of 1.3 M (solvent: cyclohexane 95% by mass / n-hexane 5% by mass) were charged into the autoclave at room temperature. 550 kg of methyl methacrylate purified by distillation was added dropwise to the autoclave over 30 minutes at 15° C. while stirring. After the dropwise addition, the autoclave was stirred for 90 minutes at 15° C. The color of the solution changed from yellow to colorless. At this point, the polymerization conversion rate of methyl methacrylate was 100%. 1500 kg of toluene was added to the obtained solution to dilute it. The diluted solution was then poured into a large amount of methanol to obtain a precipitate. The obtained precipitate was dried at 80° C. and 140 Pa for 24 hours to obtain a methacrylic polymer (A-3). Methacrylic polymer (A-3) had Mw of 25,000, a proportion of components with a molecular weight of 15,000 or less (M≦15,000) of 7.06 mass%, a melt viscosity η of 150 Pa s, Mw / Mn of 1.1, triadosyndiotacticity (rr) of 76%, Tg of 130°C, and the amount of structural units derived from methyl methacrylate was 100 mass%. The physical properties of methacrylic polymer (A-3) are shown in Table 1.
[0123] Production Example 4 (Production of Methacrylic Polymer (A-4)) The atmosphere in an autoclave equipped with a stirrer and a sampling tube was replaced with nitrogen. 100 parts by mass of purified methyl methacrylate, 0.0065 parts by mass of 2,2'-azobis(2-methylpropionitrile (hydrogen abstraction ability: 1%, 1-hour half-life temperature: 83°C), and 0.290 parts by mass of n-octyl mercaptan were added and stirred to obtain a raw material liquid. Nitrogen was fed into this raw material liquid to remove dissolved oxygen. The raw material liquid was poured into a tank reactor connected to an autoclave by piping up to 2 / 3 of the capacity. While maintaining the temperature at 140°C, the polymerization reaction was first started in a batch mode. When the polymerization conversion rate reached 55% by mass, the raw material liquid was supplied from the autoclave to the tank reactor at a flow rate that gave an average residence time of 120 minutes while maintaining the temperature at 140°C, and at the same time, the reaction liquid was withdrawn from the tank reactor at a flow rate equivalent to the supply flow rate of the raw material liquid, and the polymerization reaction was switched to a continuous flow mode. After the switchover, the polymerization conversion rate in a steady state was 45% by mass. The reaction liquid discharged from the tank reactor in a steady state was supplied to a multi-tube heat exchanger with an internal temperature of 230°C at a flow rate that gave an average residence time of 2 minutes and heated. The heated reaction liquid was then introduced into a flash evaporator, and volatile matters mainly composed of unreacted monomers were removed to obtain a molten resin. The molten resin from which the volatile matters had been removed was supplied to a twin-screw extruder with an internal temperature of 230°C, discharged in the form of strands, and cut by a pelletizer to obtain a pellet-shaped methacrylic polymer (A-4). Methacrylic polymer (A-4) had Mw of 80,000, a proportion of components with a molecular weight of 15,000 or less (M≦15,000) of 6.92% by mass, a melt viscosity η of 700 Pa s, Mw / Mn of 1.87, triadosyndiotacticity (rr) of 52%, Tg of 120°C, and the amount of structural units derived from methyl methacrylate was 100% by mass. The physical properties of methacrylic polymer (A-4) are shown in Table 1.
[0124] Production Example 5 (Production of Methacrylic Polymer (A-5)) A twin-screw extruder (manufactured by Technobel Co., Ltd.; product name KZW20TW-45MG-NH-600) consisting of a transport section, a melt-kneading section, a devolatilizing section and a discharge section, was set at a screw speed of 120 rpm and a temperature of 250° C. The methacrylic polymer (A-4) was fed at 2 kg / hr to the transport section, and monomethylamine was injected at 0.08 kg / hr into the melt-kneading section of the twin-screw extruder, to react the methacrylic polymer (A-4) with monomethylamine. A kneading block was installed in the melt-kneading section, and a reverse flight was installed on the screw at the end of the reaction zone. In the volatilizing section set at 20 Torr (about 2.7 kPa), the by-products and excess monomethylamine were volatilized and discharged through a vent. The strand-like molten resin extruded from a die provided at the end of the discharge part of the twin-screw extruder was cooled in a water tank and then cut with a pelletizer to obtain a pellet-like methacrylic polymer (A-5a).
[0125] A twin-screw extruder (manufactured by Technobel Co., Ltd.; product name KZW20TW-45MG-NH-600) consisting of a transport section, a melt kneading section, a devolatilizing section and a discharge section, was set at a screw speed of 100 rpm and a temperature of 230 ° C. The methacrylic polymer (A-5a) was fed at 1 kg / hr to the transport section, and a liquid consisting of 1.6 parts by mass of dimethylcarbonate and 0.2 parts by mass of triethylamine was injected at 0.01 kg / hr into the melt kneading section of the twin-screw extruder, to react the dimethylcarbonate with the carboxy group in the methacrylic polymer (A-5a). A kneading block was installed in the melt kneading section, and a reverse flight was installed on the screw at the end of the reaction zone. In the volatilizing section set at 20 Torr (about 2.7 kPa), the by-products and excess dimethyl carbonate were volatilized and discharged through a vent. The strand-like molten resin extruded from a die provided at the end of the discharge section of the twin-screw extruder was cooled in a water tank and then cut with a pelletizer to obtain pellets of a methacrylic polymer [A-5b].
[0126] Methacrylic resin (A-5b) was supplied at 1 kg / hr to the transport section of a twin-screw extruder (manufactured by Technobel Co., Ltd.; product name KZW20TW-45MG-NH-600), which was composed of a transport section, a melt-kneading section, a devolatilization section, and a discharge section, and was set at a screw speed of 100 rpm and a temperature of 230° C. In the devolatilization section, which was set at 20 Torr (approximately 2.7 kPa), volatile matters such as unreacted materials were volatilized and discharged through a vent. The strand-like molten resin extruded from a die provided at the end of the discharge part of the twin-screw extruder was cooled in a water tank and then cut with a pelletizer to obtain a pellet-like methacrylic polymer (A-5). The methacrylic polymer (A-5) had an Mw of 80,000, an Mw / Mn of 1.8, a proportion of components with a molecular weight of 15,000 or less (M≦15,000) of 6.60 mass%, an imidization rate of 7.0 mol%, and a glass transition temperature of 130° C. The physical properties of the methacrylic polymer (A-5) are shown in Table 1.
[0127] Production Example 6 A methacrylic polymer (B-1) was obtained by suspension polymerization, which had 100.0% by mass of structural units derived from methyl methacrylate and an Mw of 420,000. The physical properties of the methacrylic polymer (B-1) are shown in Table 1.
[0128] Production Example 7 (Production of Methacrylic Polymer (B-2)) 89 parts by mass of purified methyl methacrylate and 11 parts by mass of methyl acrylate were placed in an autoclave equipped with a stirrer and a sampling tube to obtain a monomer mixture. 0.0026 parts by mass of a polymerization initiator (2,2'-azobis(2-methylpropionitrile (AIBN), hydrogen abstraction ability: 1%, 1-hour half-life temperature: 83°C) and 0.09 parts by mass of a chain transfer agent (n-octyl mercaptan) were added and dissolved in the monomer mixture to obtain a raw material liquid. Oxygen in the production apparatus was expelled with nitrogen. The raw material liquid was discharged at a constant rate from the autoclave and supplied to a continuous flow tank-type reactor controlled at a temperature of 140°C at a flow rate that gave an average residence time of 150 minutes, and bulk polymerization was performed. The reaction liquid was collected from the sampling tube of the reactor and measured by gas chromatography, and the polymerization conversion rate was 43% by mass.
[0129] The liquid discharged from the reactor was heated to 240°C and fed at a constant flow rate to a twin-screw extruder controlled at 260°C. In the twin-screw extruder, the volatile matter mainly composed of unreacted monomers was removed, and the resin component was extruded in the form of strands. The strands were cut with a pelletizer to obtain a pellet-shaped methacrylic polymer (B-2). The physical properties of the methacrylic polymer (B-2) are shown in Table 1.
[0130] Production Example 8 (Production of Methacrylic Polymer (B-3)) The atmosphere in an autoclave equipped with a stirrer and a sampling tube was replaced with nitrogen. 98.9 parts by mass of purified methyl methacrylate, 1.1 parts by mass of methyl acrylate, 0.0050 parts by mass of 2,2'-azobis(2-methylpropionitrile (hydrogen abstraction ability: 1%, 1-hour half-life temperature: 83°C), and 0.26 parts by mass of n-octyl mercaptan were added and stirred to obtain a raw material liquid. Nitrogen was fed into the raw material liquid to remove dissolved oxygen in the raw material liquid. The raw material liquid was poured into the tank reactor connected to the autoclave by piping up to 2 / 3 of the reactor volume. The raw material liquid supply port to the tank reactor and the reaction liquid discharge port from the tank reactor were closed, and the temperature was maintained at 140°C to start a batch polymerization reaction. When the polymerization conversion rate reached 55% by mass, the raw material liquid supply port to the tank reactor and the reaction liquid discharge port from the tank reactor were opened, and the raw material liquid was supplied from the autoclave to the tank reactor at a flow rate that gave an average residence time of 150 minutes, and the reaction liquid was withdrawn from the tank reactor at a flow rate equivalent to the supply flow rate of the raw material liquid, and the temperature was maintained at 140°C, and the polymerization reaction was switched to a continuous flow polymerization reaction. After the switchover, the polymerization conversion rate in a steady state was 55% by mass.
[0131] The liquid discharged from the reactor was heated to 230°C and fed at a constant flow rate to a twin-screw extruder controlled at 240°C. In the twin-screw extruder, volatile components mainly composed of unreacted monomers were removed, and the resin components were extruded in the form of strands. The strands were cut with a pelletizer to obtain a pellet-shaped methacrylic polymer (B-3). The physical properties of the methacrylic polymer (B-3) are shown in Table 1.
[0132] [Table 1]
[0133] Production Example 9 (Production of Crosslinked Rubber Particles (C-1)) In a reactor equipped with a stirrer, a thermometer, a nitrogen gas inlet, a monomer inlet tube and a reflux condenser, 1050 parts by mass of deionized water, 1 part by mass of sodium alkyl diphenyl ether disulfonate and 0.05 parts by mass of sodium carbonate were charged, and the inside of the reactor was sufficiently replaced with nitrogen gas to make it substantially oxygen-free. Then, the inside temperature was set to 80°C. 0.01 parts by mass of potassium persulfate was added thereto and stirred for 5 minutes. Next, 26.3 parts by mass of a monomer mixture consisting of 93.7% by mass of methyl methacrylate (MMA), 6.1% by mass of methyl acrylate (MA) and 0.2% by mass of allyl methacrylate (ALMA) was continuously dripped over 20 minutes. After the dripping was completed, the polymerization reaction was carried out for another 30 minutes so that the polymerization conversion rate was 98% or more. Next, 0.05 parts by mass of a 3% aqueous solution of potassium persulfate was added to the reactor and stirred for 5 minutes. After that, 157.4 parts by mass of a monomer mixture consisting of 79.1% by mass of n-butyl acrylate, 17.1% by mass of styrene, and 3.8% by mass of allyl methacrylate was continuously added dropwise over 40 minutes. After the dropwise addition was completed, the polymerization reaction was continued for another 30 minutes so that the polymerization conversion rate was 98% or more. Next, 0.5 parts by mass of a 3% aqueous solution of potassium persulfate was added to the reactor and stirred for 5 minutes. Then, 341 parts by mass of a monomer mixture containing 93.7% by mass of methyl methacrylate, 6.0% by mass of methyl acrylate, and 0.3% by mass of n-octyl mercaptan (nOM, chain transfer agent) was continuously added dropwise over 100 minutes. After the addition was completed, the polymerization reaction was continued for another 60 minutes so that the polymerization conversion rate was 98% or more, and an emulsion containing crosslinked rubber particles (C-1) with an average particle size of 0.1 μm was obtained. The emulsion was then frozen at -30°C for 4 hours. The frozen emulsion was poured into 80°C hot water in an amount twice that of the frozen emulsion, and thawed to obtain a slurry. The slurry was kept at 80°C for 20 minutes. It was then dehydrated and dried at 70°C to obtain a powder consisting of a coagulated product of crosslinked rubber particles (C-1).
[0134] Production Example 10 (Production of Block Copolymer (D-1)) The inside of a 20-liter reaction tank was degassed and replaced with nitrogen, and then 0.35 kg of a toluene solution containing 10.29 kg of dry toluene, 0.019 kg of hexamethyltriethylenetetramine, and 0.17 mol of isobutylbis(2,6-di-t-butyl-4-methylphenoxy)aluminum was added at room temperature, and 0.077 mol of sec-butyllithium was further added. 0.50 kg of methyl methacrylate was added thereto and reacted at room temperature for 1 hour. Subsequently, the polymerization liquid was cooled to -25°C, and a mixture of 1.21 kg of n-butyl acrylate and 0.48 kg of benzyl acrylate was dropped over 1 hour. Subsequently, 1.23 kg of methyl methacrylate was added, and the reaction liquid was returned to room temperature and stirred for 8 hours. Next, 0.30 kg of methanol was added to the reaction liquid to terminate the polymerization. The reaction solution was poured into a large amount of methanol, and the precipitate was collected to obtain a triblock block copolymer (D-1) consisting of a methyl methacrylate polymer block (a1-1)-n-butyl acrylate / benzyl acrylate polymer block (a2)-methyl methacrylate polymer block (a1-2). The mass ratio of (a1-1):(a2):(a1-2) was 14.6:49.5:35.9. The block copolymer (D-1) had Mw of 62,600, Mw / Mn of 1.11, and a refractive index n d The thermal expansion coefficient was 1.493, the tensile modulus was 612 MPa, and the temperature at which the storage modulus G' suddenly decreased in a graph plotting the relationship between G' and temperature (order-disorder transition temperature (ODTT); JIS B0103-5113)) was 207°C.
[0135] Example 1 10 parts by mass of methacrylic polymer (A-1) and 90 parts by mass of methacrylic polymer (B-1) were kneaded and extruded using a twin-screw kneading extruder (TEX-44α, L / D=40, manufactured by Japan Steel Works, Ltd.) at a cylinder temperature of 260°C and a screw rotation speed of 100 rpm to obtain pellet-shaped methacrylic resin [1]. The evaluation results of methacrylic resin [1] are shown in Table 2.
[0136] Examples 2 to 3, Comparative Examples 1 to 7, and Reference Example 1 Methacrylic resins [2] to
[11] were obtained in the same manner as in Example 1, except that the mass ratios of the methacrylic polymers (A-1) to (A-5) and the methacrylic polymers (B-1) to (B-3) were changed to those shown in Table 2. The evaluation results of the methacrylic resins [2] to
[11] are shown in Table 2.
[0137] [Table 2]
[0138] TIFF0007561128000003.tif155148
[0139] Example 4 100 parts by mass of the methacrylic resin [1], 483 parts by mass of dichloromethane, and 42 parts by mass of methanol were put into a mixing tank and stirred at 25°C to dissolve the methacrylic resin [1], thereby obtaining a dope [1] with a solid content concentration of 16% by mass. The evaluation results of the dope [1] are shown in Table 3.
[0140] Examples 5 to 6, Comparative Examples 8 to 15 and Reference Example 2 Dopes [2] to
[11] with a solid content concentration of 16 mass% were obtained in the same manner as in Example 4, except that the methacrylic resin [1] was changed to the methacrylic resins [2] to
[11] , respectively. The evaluation results of the dopes [2] to
[11] are shown in Table 3.
[0141] [Table 3]
[0142] TIFF0007561128000005.tif53148
[0143] Example 7 10 parts by mass of methacrylic polymer (A-1), 70 parts by mass of methacrylic polymer (B-1), and 20 parts by mass of crosslinked rubber particles (C-1) were kneaded and extruded using a twin-screw kneading extruder (TEX-44α, L / D=40, manufactured by Japan Steel Works, Ltd.) at a cylinder temperature of 260°C and a screw rotation speed of 100 rpm to obtain a pellet-shaped methacrylic resin composition
[12] . The evaluation results of the methacrylic resin composition
[12] are shown in Table 4.
[0144] Example 8, Comparative Example 16 and Reference Example 3 Methacrylic resin compositions
[13] to
[15] were obtained in the same manner as in Example 7, except that the methacrylic polymers (A-1) and (A-3), the methacrylic polymer (B-1), the crosslinked rubber particles (C-1) and the block copolymer (D-1) were changed to the mass ratios shown in Table 4. The evaluation results of the methacrylic resin compositions
[13] to
[15] are shown in Table 4.
[0145] [Table 4]
[0146] Example 9 100 parts by mass of the methacrylic resin composition
[12] , 483 parts by mass of dichloromethane, and 42 parts by mass of methanol were put into a mixing tank, and stirred at 25°C to dissolve the methacrylic resin composition
[12] , thereby obtaining a dope
[12] with a solid content concentration of 16% by mass. The evaluation results of the dope
[12] are shown in Table 5.
[0147] Example 10, Comparative Example 17 and Reference Example 4 Dopes
[13] to
[15] having a solid content concentration of 16 mass% were obtained in the same manner as in Example 9, except that the methacrylic resin composition
[12] was replaced with the methacrylic resin compositions
[13] to
[15] , respectively. The evaluation results of the dopes
[13] to
[15] are shown in Table 5.
[0148] [Table 5]
[0149] As described above, the methacrylic resin or the methacrylic resin composition of the present invention can provide a molded product having high transparency, high strength, excellent surface smoothness, and excellent heat resistance. In addition, the dope of the present invention has a high drying speed and is excellent in suitability for production by a casting method.
Claims
1. Weight average molecular weight Mw A is 40,000 to 140,000, and the number average molecular weight Mn A Weight average molecular weight Mw A A methacrylic polymer (A) having a weight average molecular weight Mw B is 160,000 to 2,000,000 and the weight average molecular weight Mw A and a methacrylic polymer (B) having a molecular weight of 2.5 times or more, Methacrylic polymer (B) shear rate 122 sec -1 And the melt viscosity η at a temperature of 260° C. B The shear rate of the methacrylic polymer (A) is 122 s -1 And the melt viscosity η at a temperature of 260° C. A Higher than The mass ratio of the methacrylic polymer (A) to the methacrylic polymer (B) is 2 / 98 to 39 / 61; and In a weight-based differential molecular weight distribution curve, the sum of weight fraction differential values of components having a molecular weight of 1 / 20 or less of the peak top molecular weight M Ph having the highest molecular weight is 2% or less of the sum of weight fraction differential values of all components, and the sum of weight fraction differential values of components having a molecular weight of 15,000 or less is 2% or less of the sum of weight fraction differential values of all components, and the sum of weight fraction differential values of components having a molecular weight of 15,000 or less is 2% or less of the sum of weight fraction differential values of all components. Pt is 100,000 to 2,000,000, Methacrylic resin.
2. The methacrylic resin according to claim 1, wherein the methacrylic polymer (A) has a refractive index n d of 1.485 to 1.495, a triad syndiotacticity (rr) of 63 to 80%, and contains 100 mass% of structural units derived from methyl methacrylate.
3. Refractive index n of methacrylic polymer (A) dA and the refractive index n of the methacrylic polymer (B) dB Absolute value of difference with |n dA -n dB The methacrylic resin according to claim 1 or 2, wherein | is 0.005 or less.
4. A resin composition comprising the methacrylic resin according to any one of claims 1 to 3 and an elastomer.
5. A molded body comprising the methacrylic resin according to any one of claims 1 to 3.
6. A film comprising the methacrylic resin according to any one of claims 1 to 3 and having a thickness of 20 μm or more and 200 μm or less.
7. The film of claim 6 which is for optical use.
8. A dope comprising the methacrylic resin according to any one of claims 1 to 3 and an organic solvent.
9. The dope according to claim 8 is cast onto a support to obtain a liquid membrane; A method for producing a film comprising removing the organic solvent from the liquid film.
10. The method according to claim 9, wherein the thickness of the film is from 20 μm to 200 μm.
Citation Information
Patent Citations
(METH)acrylic resin composition and (METH)acrylic resin film using the same
JP2015110757A
Dope composition, polarizing plate protective film, polarizing plate protective film manufacturing method, polarizing plate and liquid crystal display device
WO2015098676A1
Methacrylic resin composition and molded body
WO2017200032A1
Methacrylate resin composition, method for producing same, molded body, film, laminated film, and laminated molded body
WO2018021449A1
Acrylic resin biaxially oriented film and method for producing same
WO2018147234A1