Flame retardant polyamide composition
A combination of phosphinate, phosphorous acid, and melamine in a flame-retardant polyamide composition addresses thermal and electrical safety challenges, achieving high thermal stability, mechanical strength, and compliance with stringent flammability and electrical safety standards.
Patent Information
- Application Number
- JP2022142852
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-02-29
- Filing Date
- 2022-09-08
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2037-02-20
AI Technical Summary
Existing halogen-free flame-retardant polyamide compositions do not meet high thermal stability, mechanical properties, and electrical safety standards, particularly in terms of glow wire ignition temperature and comparative tracking index, while also facing issues like polymer degradation and migration effects.
A combination of phosphinate, phosphorous acid, and melamine condensation products, along with fillers and reinforcing materials, is used to enhance the flame-retardant polyamide composition, maintaining electrical and mechanical properties and preventing migration.
The composition achieves high thermal stability, good mechanical properties, and meets stringent flammability and electrical safety standards, including a glow wire ignition temperature of 960°C and a comparative tracking index above 550 volts, with improved flow properties and no polymer degradation or discoloration.
Smart Images

Figure 0007561168000001 
Figure 0007561168000002 
Figure 0007561168000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a flame-retardant polyamide composition and a molded article comprising the flame-retardant polyamide composition. [Background technology]
[0002] Many plastics are flammable due to their chemical composition. In order to achieve the high flame retardancy requirements demanded by plastics processors and in some cases by legislators, plastics must usually be finished with flame retardants. For this purpose, many different flame retardants and flame retardant synergists are known and commercially available. Based on the more favorable secondary combustion properties in terms of combustion gas concentration and composition, and for ecological reasons, preferably non-halogenated flame retardant systems have been used for some time.
[0003] Among the non-halogenated flame retardants, the salts of phosphinic acids (phosphinates) have proven to be very effective, especially for thermoplastic polymers (DE-A-2252258 and DE-A-2447727). Here, some derivatives of this flame retardant class are appreciated and used successfully due to their less negative effect on the mechanical properties of thermoplastic molding materials.
[0004] Furthermore, synergistic combinations of phosphinates with certain nitrogen-containing compounds, in particular melamine derivatives, have been found which act more effectively as flame retardants in a whole series of polymers than the phosphinates alone (WO-A-2002 / 28953, WO-A-97 / 01664 and DE-A-19734437 and DE-A-19737727).
[0005] It has further been found that the flame retardant action of various phosphinates in thermoplastic polymers can also be significantly improved by the addition of small amounts of nitrogen-free inorganic or mineral compounds, and that said additions can also improve the flame retardant action of phosphinates in combination with nitrogen-containing synergists (EP-A-0024167, WO-A-2004 / 016684). In particular, the combination of phosphinates with melamine polyphosphates leads in polyamides to a V-0 grade according to the UL94 test.
[0006] The use of phosphinate-containing flame retardant systems initially leads to partial polymer decomposition, discoloration of the polymer and smoke evolution during processing, especially at processing temperatures above 300° C. However, these difficulties could be mitigated by the addition of basic or amphoteric oxides, hydroxides, carbonates, silicates, borates or stannates (WO-A-2004 / 022640).
[0007] To further improve the thermal stability, WO2012 / 045414 (Patent Document 10) discloses the combination of a phosphinate salt with a salt of phosphite. The flame retardant effect of the phosphinate salt can thereby be significantly improved, especially in aliphatic polyamides. Compared to the use of melamine polyphosphate as a synergist, after storage at high temperature and humidity, Blooming No Ausbluehungen are observed. WO-A-2014 / 135256 describes flame-retardant polyamides with phosphinates and phosphites as synergists and reinforcements and further additives. The polyamide molding materials thus obtained show good thermal stability and no tendency to migration. Flammability class UL94 V-0 and creep resistance (Comparative Tracking Index, CTI) of 600 volts are achieved.
[0008] Halogen-free polyamide compositions often do not show sufficient glow-wire results in terms of the so-called glow-wire ignition temperature (GWIT) according to IEC 60335, meaning that the tip of the glow-wire at 750° C. leads to undesired ignition of the polyamide. The use of flame-retardant polyamide molding compositions in household appliances that are left standing requires a GWIT of 750° C. or higher.
[0009] US-A-2007 / 299171 (Patent Document 12) discloses thermoplastic, especially polyamides, comprising a phosphinate (F1), a reaction product of melamine and phosphoric acid (F2) and a condensation product of melamine (F3), with F1+F2 being at least 13%, preferably at least 15%, based on the total composition. By using F1, F2 and F3 simultaneously, a GWIT of 775°C is reached. A disadvantage of such a preparation is that the use of the reaction product of melamine and phosphoric acid can cause migration effects. Furthermore, the thermal stability at about 300°C is limited, and at even higher processing temperatures polymer degradation and destruction can occur.
[0010] US2014 / 0371357 describes a thermoplastic polyamide having 10-40% by weight of glass fiber, 10-40% by weight of melam and 0-15% of a halogen-free flame retardant, the polyamide containing up to 10 mol% of aromatic monomer units. A GWIT of at least 800°C is achieved; the halogen-free flame retardant can be a metal phosphinate. A drawback of using melam is the high loading level of 30-35% to achieve UL94 V-0 and GWIT>750°C, which reduces the flowability and mechanical properties of the polyamide compound. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] DE-A-2252258 [Patent Document 2] DE-A-2447727 [Patent Document 3] WO-A-2002 / 28953 [Patent Document 4] WO-A-97 / 01664 [Patent Document 5] DE-A-19734437 [Patent Document 6] DE-A-19737727 [Patent Document 7] EP-A-0024167 [Patent Document 8] WO-A-2004 / 016684 [Patent Document 9] WO-A-2004 / 022640 [Patent Document 10] WO2012 / 045414 [Patent Document 11] WO-A-2014 / 135256 [Patent Document 12] US-A-2007 / 299171 [Patent Document 13] US2014 / 0371357 Summary of the Invention [Problem to be solved by the invention]
[0012] It was therefore an object of the present invention to provide a halogen-free, flame-retardant thermoplastic polyamide composition (molding material) based on a phosphinate-containing flame retardant system, which has high thermal stability and good mechanical properties, which reliably achieves both UL94 V-0 for test specimens up to a wall thickness of 0.4 mm and the glow-wire requirements of a Glow Wire Flammability Index (GWFI) of 960° C. and a GWIT of 775° C. for all tested wall thicknesses, which does not show migration effects, which shows good flowability and which exhibits high electrical values (Comparative Tracking Index (CTI) >550 V). [Means for solving the problem]
[0013] It has now surprisingly been found that the glow-wire resistance of phosphinate-containing flame-retardant thermoplastic polyamides can be significantly improved if the molding material comprises, in addition to the phosphinate (component B), a salt of phosphorous acid (also called phosphonic acid) HP(=O)(OH)2 (component C)) and a condensation product of melamine (component D). In this special combination, the well-balanced property profile of the electrical and mechanical properties of the polyamide is well maintained. The molding material thus obtained surprisingly does not show migration of the flame retardant used. Furthermore, the polyamide composition (molding material) comprises, as component E), fillers and / or reinforcing materials.
[0014] Thermoplastics are primarily processed in the melt. The structural and state changes involved are hardly tolerated by plastics without changing their chemical structure. Crosslinking, oxidation, molecular weight changes and therefore changes in physical and technical properties can occur. To reduce the load on the polymer during processing, various additives are used depending on the plastic.
[0015] In many cases, various additives are used simultaneously, each of which has a specific task. For example, antioxidants and stabilizers are used so that plastics can withstand processing without chemical damage and are stable over time against external influences such as heat, UV light, weather and oxygen (air). In addition to improving the flow behavior, lubricants prevent the plastic melt from sticking too strongly to hot machine parts and act as dispersants for pigments, filler materials and reinforcing materials.
[0016] The use of flame retardants can affect the stability of plastics during processing in the melt. In order to ensure sufficient flame retardancy of plastics according to international standards, flame retardants often have to be added in high doses. Due to their chemical reactivity required for flame retardant action at high temperatures, flame retardants can impair the processing stability of plastics. For example, increased polymer degradation, crosslinking reactions, degassing or discoloration can occur.
[0017] For example, polyamides are stabilized by small amounts of copper halides as well as aromatic amines and sterically hindered phenols, where achieving long-term stability at high continuous use temperatures is of great importance (H. Zweifel (Ed.): “Plastics Additives Handbook”, No. 5, Carl Hanser Verlag, München, 2000, pp. 80-84).
[0018] The polyamide composition of the present invention comprises as component F) a phosphonite or a phosphite or a phosphonite / phosphite mixture and as component G) a generally C 14 ~C 40 The copolymer may contain esters or salts of long chain aliphatic carboxylic acids (fatty acids) having a chain length of 0.1 to 0.5.
[0019] The subject of the present invention is therefore a flame-retardant polyamide composition comprising: As component A) 1 to 96% by weight of one or more thermoplastic polyamides and as component B) 2 to 25% by weight of a dialkylphosphinic acid salt of the formula (I)
[0020] [ka] [In the formula, R 1 and R 2 are the same or different and are linear, branched or cyclic C1-C 18 -Alkyl, C6-C 18 -Aryl, C7-C 18 -Arylalkyl and / or C7-C 18 -alkylaryl, M means Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K and / or protonated nitrogen bases; m is 1 to 4; n is 1 to 4. As component C), 1 to 20% by weight of a salt of phosphorous acid as component D) 1 to 20% by weight of one or more condensation products of melamine, As component E), 0 to 50% by weight of fillers and / or reinforcing materials, As component F), 0 to 2% by weight of a phosphite or phosphonite or a mixture thereof, and as component G), 0 to 2% by weight of normal C 14 ~C 40 Esters or salts of long chain aliphatic carboxylic acids (fatty acids) having a chain length of The sum of the above components is always 100% by weight.
[0021] Preferably, the flame retardant polyamide composition is 15 to 89.9% by weight of component A), 5 to 20% by weight of component B), 2 to 10% by weight of component C), 2 to 20% by weight of component D), 1 to 50% by weight of component E), 0 to 2% by weight of component F) and 0.1 to 1% by weight of component G) Includes.
[0022] Particularly preferably, the flame-retardant polyamide composition is 15 to 75.8% by weight of component A), 5 to 20% by weight of component B), 2 to 10% by weight of component C), 2 to 10% by weight of component D), 15 to 35% by weight of component E), 0.1 to 1% by weight of component F), and 0.1 to 1% by weight of component G) Includes.
[0023] Particularly preferably, the flame-retardant polyamide composition is 35 to 65.8% by weight of component A), 5 to 20% by weight of component B), 2 to 7% by weight of component C), 2 to 7% by weight of component D), 25 to 35% by weight of component E), 0.1 to 5% by weight of component F), and 0.1 to 5% by weight of component G) Includes.
[0024] In another embodiment, the flame retardant polyamide composition comprises: 35 to 96% by weight of component A), 2 to 25% by weight of component B), 1 to 20% by weight of component C), 1 to 20% by weight of component D), 0 to 50% by weight of component E), 0 to 2% by weight of component F) and 0 to 2% by weight of component G) Includes.
[0025] Preferably, the flame retardant polyamide composition has a Comparative Tracking Index (CTI) of greater than 550 volts measured in accordance with International Electrotechnical Commission standard IEC-60112 / 3.
[0026] Preferably, the flame retardant polyamide composition achieves a rating of V-0 according to UL-94 for test specimen thicknesses of 3.2 mm to 0.4 mm.
[0027] Preferably, the flame retardant polyamide composition has a Glow Wire Flammability Index (GWFI) of 960° C. according to IEC-60695-2-12 at a test specimen thickness of 0.4 to 3 mm.
[0028] Preferably, the flame retardant polyamide composition has a glow wire ignition temperature index (GWIT) of 750° C. or more according to IEC-60695-2-13 for a test piece having a thickness of 0.4 to 3 mm.
[0029] Preferably, the polyamide (PA) is selected from the group of PA 6, PA 6,6, PA 4,6, PA12, PA 6,10, PA 4,10, PA 10,10, PA 11, PA 6T / 66, PA 6T / 6, PA 4T, PA 9T, PA 10T, polyamide-copolymers, polyamide-blends and combinations thereof.
[0030] Preferably, component A) is polyamide 66 or a copolymer or polymer blend from polyamide 66 and polyamide 6.
[0031] Preferably, component A) is a polyamide PA 6T / 66, PA6T / 6, PA4T, PA9T and / or PA10T.
[0032] Preferably, component D) is characterized in that it is melam, melem and / or melon.
[0033] Particularly preferably, component D) is melem.
[0034] Preferably, in component B), R 1 , R 2 are identical or different and denote methyl, ethyl, n-propyl, isopropyl, n-butyl, tert.-butyl, n-pentyl and / or phenyl.
[0035] Preferably, the salt of phosphorous acid (component (C)) corresponds to the general formula (II) [HP(=O)O2] 2- M m+ (II) [In the formula, M means Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na and / or K. Preferably, the salt of phosphorous acid (component (C)) is selected from the group consisting of aluminum phosphite Al(H2PO3)3, secondary aluminum phosphite Al2(HPO3)3, aluminum phosphite tetrahydrate Al2(HPO3)3*4aq, aluminum phosphonate, basic aluminum phosphite Al(OH)(H2PO3)2*2aq, Al7(HPO3)9(OH)6(1,6-hexanediamine) 1.5 *12H2O, Al2(HPO3)3*xAl2O3*nH2O (x=1-2.27, n=1-50) and / or Al4H6P 16 O 18It is.
[0036] Preferably, the salt of phosphorous acid is also an aluminum phosphite of formula (III), (IV) and / or (V) Formula (III): Al2(HPO3)3x (H2O)q (q ranges from 0 to 4). Formula (IV): Al 2.00 M z (HPO3) y (OH) v x (H2O) w (M represents an alkali metal ion, z is between 0.01 and 1.5. y means 2.63 to 3.5, v ranges from 0 to 2, and w means 0 to 4); Formula (V): Al 2,00 (HPO3) u (H2PO3) t x (H2O) s (u means 2 to 2.99, t means 2 to 0.01, and s means 0 to 4), and / or mixtures of aluminum phosphites of formula (III) with sparingly soluble aluminum salts and nitrogen-free foreign ions, mixtures of aluminum phosphites of formula (V) with aluminum salts, mixtures of aluminum phosphites of formula (III), (IV) and / or (V) with aluminum phosphites [Al(H2PO3)3], secondary aluminum phosphites [Al2(HPO3)3], basic aluminum phosphites [Al(OH)(H2PO3)2*2aq], aluminum phosphite tetrahydrate [Al2(HPO3)3*4aq], aluminum phosphonates, Al7(HPO3)9(OH)6(1,6-hexanediamine). 1.5 *12H2O, Al2(HPO3)3*xAl2O3*nH2O (x=1-2.27 and n=1-50) and / or Al4H6P 16 O 18 It is a mixture of.
[0037] Preferably, component C) has an average particle size of 0.2 to 100 μm.
[0038] Preferably, said reinforcing filler or material (component E)) is glass fiber.
[0039] Preferably, as component F, a phosphite of formula (IX) is used P(OR1)3(IX)
[0040] Preferably, the phosphonite is of the general structure R-[P(OR 5 )2] m (VI) [In the formula, R is a monovalent or polyvalent aliphatic, aromatic or heteroaromatic organic group, and R 5 Structure (XII)
[0041] [ka] or a compound having two groups R 5 forms a bridging group of structure (VIII)
[0042] [ka] Where: A is a direct bond, O, S, C 1-18 -Alkylene (linear or branched), C 1-18 -alkylidene (linear or branched), in which R 6 are, independently of each other, C 1-12 -Alkyl (linear or branched), C 1-12 -Alkoxy and / or C 5-12 -cycloalkyl, and n is an integer from 0 to 5. m means 1 to 4].
[0043] Preferably, component G) is an alkali metal, alkaline earth metal, aluminum and / or zinc salt of a long-chain fatty acid having 14 to 40 C atoms and / or a reaction product of a long-chain fatty acid having 14 to 40 C atoms with a polyhydric alcohol, such as ethylene glycol, glycerol, trimethylolpropane and / or pentaerythritol.
[0044] The flame-retardant polyamide composition of the present invention according to any one of claims 1 to 22 can further contain a telomer.
[0045] Telomers, in the narrower sense, can result from the multiple addition of olefins (ethylene, propylene) to a phosphoric acid source (H3PO2, sodium hypophosphite).
[0046] In this case, preferably, the telomer is of formula (X) H-(C w H 2w ) k P(O)(OM)(C x H 2x ) l -H(X) In formula (X), k is an integer from 1 to 9. l stands for 1 to 9, w means 2 to 9, x is an integer from 2 to 9. M means Mg, Ca, Al, Sb, Sn, Ge, Ti, Fe, Zr, Zn, Ce, Bi, Sr, Mn, Li, Na, K and / or protonated nitrogen bases; And the group (C w H 2w ) k and (C x H 2x ) l can be linear or branched.
[0047] Preferably, the telomer is a metal salt of ethylbutylphosphinic acid, dibutylphosphinic acid, ethylhexylphosphinic acid, butylhexylphosphinic acid, ethyloctylphosphinic acid, sec-butylethylphosphinic acid, 1-ethylbutyl-butyl-phosphinic acid, ethyl-1-methylpentyl-phosphinic acid, di-sec-butylphosphinic acid (di-1-methyl-propylphosphinic acid), propyl-hexylphosphinic acid, dihexylphosphinic acid, hexyl-nonylphosphinic acid, propyl-nonylphosphinic acid, dinonylphosphinic acid, dipropylphosphinic acid, butyl-octylphosphinic acid, hexyl-octylphosphinic acid, dioctylphosphinic acid.
[0048] In a broader sense, telomers can also result from the addition of a phosphoric acid source to an organic group, which can also be formed, for example, from a radical initiator and a solvent.
[0049] In that case, the telomer is of formula (XI)
[0050] [ka] [In the formula, R 1 , R 2 are the same or different, C6-C 10 -Arylene, C7-C 20 -Alkyl arylene, C7-C 20 -aryl alkylene and / or C3-C 16 -cycloalkyl or -bicycloalkyl, M means Mg, Ca, Al, Sb, Sn, Ge, Ti, Fe, Zr, Zn, Ce, Bi, Sr, Mn, Li, Na, K and / or protonated nitrogen bases.
[0051] Preferably, in formula (X), w and x each represent 2 to 4; and k and l each represent 1 to 4.
[0052] Particularly preferably, in formula (X), w and x each represent 2 or 3, and k and l each represent 1 to 3.
[0053] Preferably, in formula (X) and / or (XI), M independently of each other denotes Al, Ti, Fe or Zn, respectively.
[0054] Preferably, the telomer is ethyl(cyclopentylethyl)phosphinic acid, butyl(cyclopentylethyl)phosphinic acid, ethyl(cyclohexylethyl)phosphinic acid, butyl(cyclohexylethyl)phosphinic acid, ethyl(phenylethyl)phosphinic acid, butyl(phenylethyl)phosphinic acid, ethyl(4-methylphenylethyl)phosphinic acid, ethylphenylphosphinic acid. Butyl(4-methylphenylethyl)phosphinic acid, butylcyclopentylphosphinic acid, butylcyclohexylethylphosphinic acid, butylphenylphosphinic acid, ethyl(4-methylphenyl)phosphinic acid and / or butyl(4-methylphenyl)phosphinic acid metal salts, the metals of which are from the group Mg, Ca, Al, Sb, Sn, Ge, Ti, Fe, Zr, Zn, Ce, Bi, Sr, Mn, Li, Na and / or K.
[0055] In a broader sense, telomers can also result from the addition of a phosphoric acid source to organic groups which arise, for example, in the course of decomposition of a photoinitiator.
[0056] Hydroxymethylethyl-ethylphosphinic acid, 1-hydroxy-1-methylpropyl-ethylphosphinic acid, butyl-ethylphosphonic acid ester, acyl-ethylphosphonic anhydride, butyl-ethylphosphonic acid, butylethylphosphinic acid, ethylphosphinyl isobutyronitrile (1-cyano-1-methylethyl-ethylphosphinic acid), propylethylphosphinic acid, t-butyl-ethylphosphonic acid ester, t-butyl-ethylphosphinic acid, ethylphosphinylacetic acid, hydroxymethylbutyl-ethylphosphinic acid, 3-hydroxy-3-methylpentyl-ethylphosphinic acid, propoxyethyl-ethylphosphinic acid, phenylethyl-ethylphosphinic acid, 2-ethylphosphinylethyl-lauric acid ester, ethylpentylphosphinic acid, t-butoxyethyl-ethylphosphinic acid, ethylphosphinyl isohexanoic acid nitrile, hexylethylphosphinic acid, ethylphosphinyl ethyl sulfate, ethylphosphinyl butyric acid.
[0057] The invention also relates to a three-dimensional article comprising the flame-retardant polyamide composition according to any one of claims 1 to 23, characterized in that it is a moulded body, an injection moulded part, an extruded material and / or an extruded part.
[0058] Furthermore, the present invention relates to the use of the flame-retardant polyamide composition according to any one of claims 1 to 23 in or for plug connectors, current contact parts in power distribution equipment (earth leakage breakers), printed circuit boards, sealants, power plugs, circuit breakers, lamp housings, LED housings, capacitor housings, coil parts in or on circuit boards and ventilators for ground wires, plugs; housings for plugs, for cables, for flexible printed circuit boards, for mobile phone charging cables, engine covers, textile coatings and other products.
[0059] Preferably, component A) consists of at least 75% by weight of polyamide 66 and at most 25% by weight of polyamide 6.
[0060] Surprisingly, it has been found that the flame-retardant polyamide compositions of the present invention have a good flame-retardant effect (V-0 and GWFI / GWIT) in combination with improved flowability, high thermal stability and high impact strength. Polymer degradation is prevented or greatly reduced, adhesion to moulds and Blooming Moreover, the flame retardant polyamide compositions of the present invention exhibit only slight discoloration upon processing in the melt.
[0061] As component A), the composition according to the invention comprises at least one thermoplastic polyamide.
[0062] Thermoplastic polyamides are understood according to Hans Domininghaus' "Die Kunststoffe und ihre Eigenschaften" (Plastics and Their Properties), 5th Edition (1998), p. 14, to be polyamides whose molecular chains have no or a variable amount of side chains of a certain length, which soften when heated and can be molded in almost any way.
[0063] The polyamides preferred in the present invention can be produced according to various methods, can be synthesized from various components, and in the case of specific applications, can be combined alone or with processing aids, stabilizers or even polymer alloy partners, preferably elastomers, to form materials with specific established property combinations. Blends with some other polymers, preferably polyethylene, polypropylene, ABS, are also suitable, where one or more compatibilizers can be optionally used. The properties of polyamides can be improved by the addition of elastomers, for example in terms of impact strength, especially when they are reinforced polyamides. The many combination possibilities allow a very large number of products with different properties.
[0064] Numerous processes are known for the preparation of polyamides, in which, depending on the desired end product, different monomer building blocks, different chain regulators for the adjustment of the target molecular weight, or even monomers with reactive groups for the subsequent intended aftertreatment are used.
[0065] Technically relevant processes for the preparation of polyamides mostly proceed via polycondensation in the melt. In this series, the hydrolytic polymerization of lactams is also understood as polycondensation.
[0066] Preferably, the polyamides (PA) to be used as component A) are semicrystalline polyamides which can be prepared starting from diamines and dicarboxylic acids and / or lactams having at least 5 ring members, or the corresponding amino acids.
[0067] The starting materials include aliphatic and / or aromatic dicarboxylic acids, preferably adipic acid, 2,2,4- and 2,4,4-trimethyladipic acid, azelaic acid, sebacic acid, isophthalic acid, terephthalic acid, aliphatic and / or aromatic diamines, preferably tetramethylenediamine, hexamethylenediamine, 1,9-nonanediamine, 2,2,4- and 2,4,4-trimethylhexamethylenediamine, isomeric diaminodicyclohexylmethane, diaminodicyclohexylpropane, bis-aminomethylcyclohexane, phenylenediamine, xylylenediamine, aminocarboxylic acids, preferably aminocaproic acid or the corresponding lactams. Copolyamides from a number of the above monomers are included. Particularly preferably caprolactam is used, especially preferably [epsilon]-caprolactam.
[0068] Furthermore, most compounds based on PA6, PA66 and other aliphatic or / and aromatic polyamides or copolyamides are particularly suitable, in which the polyamide groups in the polymer chain contain 3 to 11 methylene groups.
[0069] Preferably, said polyamides and copolyamides are polyamide 12, polyamide 4, polyamide 4,6, polyamide 6, polyamide 6,6, polyamide 6,9, polyamide 6,10, polyamide 6,12, polyamide 6,66, polyamide 7,7, polyamide 8,8, polyamide 9,9, polyamide 10,9, polyamide 10,10, polyamide 11, polyamide 12, etc. These are, for example, available under the trade name Nylon (登録商標) ,DuPont, Ultramid (登録商標) ,BASF, Akulon (登録商標) ,DSM,Zytel (登録商標) ,DuPont;Durethan (登録商標) , Bayer and Grillamid (登録商標) , known from Ems Chemie.
[0070] Also suitable are aromatic polyamides derived from m-xylene, diamines and adipic acid; polyamides made from hexamethylenediamine and iso- and / or terephthalic acid and, optionally, elastomers as modifiers, such as poly-2,4,4-trimethylhexamethylene-terephthalamide or poly-m-phenyleneisophthalamide, block copolymers of the above polyamides with polyolefins, olefin copolymers, ionomers or chemically bonded or grafted elastomers or polyethers, such as polyethylene glycol, polypropylene glycol or polytetramethylene glycol. In addition, there are also polyamides or copolyamides modified with EPDM or ABS; as well as polyamides condensed during processing ("RIM-polyamide systems").
[0071] In one preferred embodiment, the composition according to the invention comprises, besides the thermoplastic polyamide used according to the invention, at least one further thermoplastic polymer, particularly preferably at least one further polyamide.
[0072] Aliphatic polyamides are preferred, in particular PA6 and PA66 and PA6T / 66 and PA6T / 6. Particularly preferred are mixtures of polyamide 66 and polyamide 6, preferably with more than 50% by weight of polyamide 66 and less than 50% by weight of polyamide 6, particularly preferably with less than 25% by weight of polyamide 6, each based on the total amount of polyamide.
[0073] Blends of polyamide 66 with one or more partially aromatic amorphous polyamides are also preferred.
[0074] In a preferred embodiment, the polymer used in addition to the thermoplastic polyamide may be mixed with customary additives, in particular release agents, stabilizers and / or flow aids, in the melt or applied to the surface. The starting materials for the thermoplastic polyamides of component A) are obtained synthetically, for example from petrochemical raw materials, and / or from regenerated raw materials via chemical or biochemical processes.
[0075] Other flame retardants or flame retardant synergists not specifically mentioned here can also be used. In particular, nitrogen-containing flame retardants, such as melamine cyanurate, melamine phosphate and melamine polyphosphate, can be added. Further phosphorus flame retardants, such as aryl phosphates or red phosphorus, can also be used. Furthermore, salts of aliphatic and aromatic sulfonic acids and mineral flame retardant additives, such as aluminum hydroxide and / or magnesium hydroxide, Ca-Mg-carbonate hydrate (e.g. DE-A-4236122), can also be used. Further flame retardant synergists selected from the group of oxygen-, nitrogen- or sulfur-containing metal compounds, preferably zinc oxide, zinc borate, zinc stannate, zinc hydroxystannate, zinc sulfide, molybdenum oxide, titanium dioxide, magnesium oxide, magnesium carbonate, calcium carbonate, calcium oxide, titanium nitride, boron nitride, magnesium nitride, zinc nitride, zinc phosphate, calcium phosphate, calcium borate, magnesium borate or mixtures thereof can also be mentioned.
[0076] Suitable flame retardant additives are preferably carbon formers, particularly preferably phenol-formaldehyde resins, polycarbonates, polyimides, polysulfones, polyethersulfones or polyetherketones, as well as antidrip agents, in particular tetrafluoroethylene polymers.
[0077] The flame retardants can be added in pure form and via a masterbatch or compact.
[0078] Preferably, component B is an aluminium or zinc salt of diethylphosphinic acid.
[0079] Preferably, in the aluminum phosphite of the formula (III), q means 0.01 to 0.1.
[0080] Preferably, in the aluminum phosphite of formula (IV), z means 0.15 to 0.4. y means 2.80~3, v is between 0.1 and 0.4, and w ranges from 0.01 to 0.1.
[0081] Preferably, in the aluminum phosphite of formula (V), u means 2.834~2.99, t means 0.332 to 0.03, and s means 0.01 to 0.1.
[0082] Preferably, the condensed melamine compound is melam or melem.
[0083] [ka] As component E), the flame-retardant polyamide composition of the invention may in a further preferred embodiment comprise at least one filler or reinforcing material.
[0084] Here, mixtures of two or more different fillers and / or reinforcing materials, preferably based on talc, mica, silicates, quartz, titanium dioxide, wollastonite, kaolin, amorphous silica, nanoscale minerals, particularly preferably montmorillonite or nanoboehmite, magnesium carbonate, chalk, feldspar, barium sulfate, glass spheres, and / or fiber-forming fillers and / or reinforcing materials based on carbon fibers and / or glass fibers, can also be used. Preference is given to using mineral particulate fillers based on talc, mica, silicates, quartz, titanium dioxide, wollastonite, kaolin, amorphous silica, magnesium carbonate, chalk, feldspar, barium sulfate and / or glass fibers. Particular preference is given to using mineral particulate fillers based on talc, wollastonite, kaolin and / or glass fibers, with glass fibers being very particularly preferred.
[0085] Furthermore, particularly preferably, acicular mineral fillers can also be used. By acicular mineral fillers, in the present invention, it is understood that mineral fillers have a very pronounced acicular character. Preference is given to acicular wollastonite. The above minerals preferably have a length to diameter ratio of 2:1 to 35:1, particularly preferably 3:1 to 19:1, and especially preferably 4:1 to 12:1. The average grain size of the acicular minerals usable in the present invention, as measured with a CILAS grain sizer, is preferably less than 20 μm, particularly preferably less than 15 μm, and especially preferably less than 10 μm.
[0086] In a preferred embodiment, the fillers and / or reinforcing materials may be surface-modified, preferably with an adhesion promoter or adhesion promoter system, particularly preferably based on silanes. However, pretreatment is not necessary. In particular when using glass fibers, in addition to silanes, polymer dispersions, film formers, branching agents and / or glass fiber processing aids may also be used.
[0087] The glass fibres which are particularly preferably used as component E) in the present invention, generally having a fibre diameter of 7 to 18 μm, preferably 9 to 15 μm, are added as continuous fibres or as chopped or crushed glass fibres. These fibres may be finished with a suitable size system and adhesion promoter or adhesion promoter system, preferably silane-based.
[0088] The polyamide composition of the present invention may further comprise further additives.In the sense of the present invention, preferred additives are antioxidants, UV stabilizers, gamma radiation stabilizers, hydrolysis stabilizers, antistatic agents, emulsifiers, nucleating agents, softeners, processing aids, impact modifiers, dyes and pigments.The said additives may be used alone or in mixtures or in the form of masterbatches.
[0089] Suitable antioxidants are, for example, alkylated monophenols, such as 2,6-di-tert-butyl-4-methylphenol; alkylthiomethylphenols, such as 2,4-di-octylthiomethyl-6-tert-butylphenol; hydroquinone and alkylated hydroquinones, such as 2,6-di-tert-butyl-4-methoxyphenol; tocopherols, such as α-tocopherol, β-tocopherol, γ-tocopherol, δ-tocopherol and mixtures thereof (vitamin E); hydroxylated thiodiphenyl ethers, such as 2,2'-thio-bis(6-tert-butyl-4-methylphenol), 2,2'-thio-bis(4-octylphenol), 4,4'-thio-bis-(6-tert-butyl-3-methylphenol), 4,4'-thio-bis-(6-tert-butyl-2-methylphenol), 4,4'-thio-bis-(3,6-di-sec.-amylphenol), 4,4'-bis-(2,6-dimethyl-4-hydroxyphenyl)-disulfide; alkylidene-bisphenols, such as 2,2'-methylene-bis-(6-tert-butyl-4-methylphenol; O-, N- and S-benzyl compounds, such as 3,5,3',5'-tetra-tert-butyl-4,4'-dihydroxydibenzyl ether; hydroxybenzylated aromatics, such as dioctadecyl-2,2-bis-(3,5-di-tert-butyl-2-hydroxybenzyl)-malonate; hydroxybenzyl-aromates, such as 1,3,5-tris-(3,5-di-tert-butyl)-4-hydroxy benzyl)-2,4,6-trimethylbenzene, 1,4-bis-(3,5-di-tert-butyl-4-hydroxybenzyl)-2,3,5,6-tetramethylbenzene, 2,4,6-tris-(3,5-di-tert-butyl-4-hydroxybenzyl)-phenol; triazine compounds such as 2,4-bis-octylmercapto-6(3,5-di-tert-butyl-4-hydroxyanilino)-1,3,5-triazine; benzylphosphonates such as dimethyl-2,5-di-tert-butyl-4-hydroxybenzylphosphonate; acylaminophenols, 4-hydroxylauric acid amide, 4-hydroxystearic acid anilide, N-(3,5-di-tert-butyl-4-hydroxyphenyl)-carbamic acid octyl ester; β-(3.Esters of 5-di-tert-butyl-4-hydroxyphenyl)-propionic acid and monohydric or polyhydric alcohols;Esters of β-(5-tert-butyl-4-hydroxy-3-methylphenyl)-propionic acid and monohydric or polyhydric alcohols;Esters of β-(3,5-dicyclohexyl-4-hydroxyphenyl)-propionic acid and monohydric or polyhydric alcohols;Esters of 3,5-di-tert-butyl-4-hydroxyphenylacetic acid and monohydric or polyhydric alcohols amides of β-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid, such as N,N'-bis-(3,5-di-tert-butyl-4-hydroxyphenylpropionyl)-hexamethylenediamine, N,N'-bis-(3,5-di-tert-butyl-4-hydroxyphenylpropionyl)-trimethylenediamine, N,N'-bis-(3,5-di-tert-butyl-4-hydroxyphenylpropionyl)-hydrazine.
[0090] Particularly preferably, sterically hindered phenols are used alone or in combination with phosphites, where N,N'-bis[3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionyl]hexamethylenediamine (e.g. Irganox, BASF SE, Ludwigshafen, Germany) is preferred. (登録商標) 1098) is particularly preferred.
[0091] Suitable UV absorbers and light stabilizers are, for example, 2-(2'-hydroxy-phenyl)-benzotriazoles, such as 2-(2'-hydroxy-5'-methylphenyl)-benzotriazole; 2-hydroxybenzophenones, such as 4-hydroxy, 4-methoxy, 4-octoxy, 4-decyloxy-, 4-dodecyloxy-, 4-benzyloxy-, 4,2',4-trihydroxy-, 2'-hydroxy-4,4'-dimethoxy-derivatives; optionally substituted esters of benzoic acid, such as 4-tert-butyl-phenylsalicylate, phenylsalicylate, octylphenyl-salicylate, dibenzoylresorcin, bis-(4-tert-butylbenzoyl)-resorcin, benzoylresorcin, 3,5-di-tert-butyl-4-hydro hydroxybenzoic acid-2,4-di-tert-butylphenyl ester, 3,5-di-tert-butyl-4-hydroxybenzoic acid hexadecyl ester, 3,5-di-tert-butyl-4-hydroxybenzoic acid-octadecyl ester, 3,5-di-tert-butyl-4-hydroxybenzoic acid-2-methyl-4,6-di-tert-butylphenyl ester, acrylates such as α-cyano-β,β-diphenylacrylic acid-ethyl ester or -isooctyl ester, α-carbomethoxy-cinnamic acid methyl ester, α-cyano-β-methyl-p-methoxy-cinnamic acid methyl ester or butyl ester, α-carbomethoxy-p-methoxy-cinnamic acid methyl ester, N-(β-carbo-methoxy-β-cyanovinyl)-2-methyl-indoline.
[0092] As colorants, preferably inorganic pigments are used, in particular titanium dioxide, ultramarine blue, iron oxide, zinc sulfide or carbon black, and also organic pigments, preferably phthalocyanines, quinacridones, perylenes, and dyes, preferably nigrosines and anthraquinones.
[0093] Suitable polyamide stabilizers are, for example, copper salts in combination with iodides and / or phosphorus compounds, and salts of divalent manganese.
[0094] Suitable basic costabilizers are melamine, polyvinylpyrrolidone, dicyandiamide, triallyl cyanurate, urea derivatives, hydrazine derivatives, amines, polyamides, polyurethanes, alkali metal and alkaline earth metal salts of higher fatty acids, such as Ca stearate, Zn stearate, Mg behenate, Mg stearate, Na ricinoleate, K palmitate, antimony catecholate or tin catecholate.
[0095] Suitable nucleating agents are, for example, 4-tert-butylbenzoic acid, adipic acid and diphenylacetic acid, aluminum oxide or silicon dioxide, particularly preferably talc, without being limited to this list.
[0096] As flow aids, it is possible to use preferably copolymers of at least one α-olein and at least one methacrylic or acrylic ester of an aliphatic alcohol. Particular preference is given here to copolymers in which the α-olefin is composed of ethene and / or propene and the methacrylic or acrylic ester contains, as the alcohol component, a linear or branched alkyl group having 6 to 20 C atoms. Very particular preference is given to acrylic acid-(2-ethyl)-hexyl ester.
[0097] Copolymers suitable for the present invention as flow aids are characterized by low molecular weight in addition to composition.Therefore, suitable copolymers for the composition to be protected from thermal decomposition according to the present invention are in particular copolymers having a melt flow index (MFI) value of at least 100g / 10min, preferably at least 150g / 10min, particularly preferably at least 300g / 10min at 190°C and a load of 2.16kg.MFI serves to characterize the flow state of the melt of thermoplastics and is in accordance with ISO1133 or ASTM D1238 standards.In the context of the present invention, all statements regarding MFI or MFI are consistently measured or determined according to ISO 1133 at 190°C and a test weight of 2.16kg.
[0098] Preferably, the softener added is dioctyl phthalate, dibenzyl phthalate, butyl benzyl phthalate, hydrocarbon oil or N-(n-butyl)benzenesulfonamide.
[0099] The invention also relates to products, preferably fibres, films or mouldings, obtainable from the compositions according to the invention by injection moulding or extrusion.
[0100] Suitable phosphinates (component B)) are described in PCT / WO97 / 39053, which is expressly incorporated by reference. Particularly preferred phosphinates are aluminum-, calcium- and zinc phosphinates.
[0101] Preferred salts of phosphorous acid (component C)) are salts which are insoluble or sparingly soluble in water.
[0102] Particularly preferred salts of phosphorous acid are the aluminium-, calcium- and zinc salts.
[0103] Particularly preferably, component C) is a reaction product from phosphorous acid and an aluminum compound.
[0104] Preference is given to aluminum phosphites having CAS numbers 15099-32-8, 119103-85-4, 220689-59-8, 56287-23-1, 156024-71-4, 71449-76-8 and 15099-32-8.
[0105] Preferably, the aluminum phosphite has a particle size of 0.2 to 100 μm.
[0106] The preparation of the preferred aluminum phosphites is carried out by reacting an aluminum source with a phosphorus source and optionally a template in a solvent at 20-200° C. for a period of up to 4 days. To this end, the aluminum source and the phosphorus source are mixed for 1-4 hours, heated under hydrothermal conditions or under reflux, filtered, washed and dried, for example at 110° C.
[0107] Preferred sources of aluminum are aluminum isopropoxide, aluminum nitrate, aluminum chloride and aluminum hydroxide (eg pseudoboehmite).
[0108] Preferred phosphorus sources are phosphorous acid, (acid) ammonium phosphites, alkali metal phosphites or alkaline earth metal phosphites.
[0109] Preferred alkali metal phosphites are disodium phosphite, disodium phosphite hydrate, trisodium phosphite and potassium hydrogen phosphite.
[0110] A preferred disodium phosphite hydrate is Brueggolen phosphate hydrate from Brueggemann. (登録商標) It's H10.
[0111] Preferred templates are 1,6-hexanediamine, guanidine carbonate or ammonia.
[0112] The preferred alkaline earth metal phosphite is calcium phosphite.
[0113] Here, the preferred ratio of aluminum, phosphorus and solvent is 1:1:3.7 to 1:2.2:100 mol. The preferred ratio of aluminum to template is 1:0 to 1:17 mol. The preferred pH value of the reaction solution is 3 to 9. The preferred solvent is water.
[0114] Particularly preferably, in said uses, salts of the same phosphinic acid, such as phosphites, are used, ie for example aluminum dialkylphosphinate together with aluminum phosphite or zinc dialkylphosphinate together with zinc phosphite.
[0115] Preferably, component G) is an alkali metal, alkaline earth metal, aluminum and / or zinc salt of a long-chain fatty acid having 14 to 40 C atoms and / or a reaction product of a long-chain fatty acid having 14 to 40 C atoms with a polyhydric alcohol, such as ethylene glycol, glycerol, trimethylolpropane and / or pentaerythritol. Particularly preferably, it is an aluminum, calcium or zinc stearate or calcium montanate.
[0116] Further suitable flame retardants are preferably aryl phosphates, phosphonates, salts of diphosphorous acid as well as red phosphorus.
[0117] Preferably, as component F, a phosphite of formula (IX) is used P(OR1)3(IX) In the formula, R1 has the above meaning.
[0118] Preferably, in the case of the phosphonite, the group R is C 4- C 18 -Alkyl (linear or branched), C 4- C 18 -Alkylene (linear or branched), C 5- C 12 -Cycloalkyl, C 5- C 12 -Cycloalkylene, C 6- C 24 -aryl or -heteroaryl, C 6- C 24 -arylene or -heteroarylene, which may be further substituted; R1 is a compound of structure (IX) or (VI), wherein: R2 are independent of each other, C 1- C8-Alkyl (linear or branched), C 1- C8-alkoxy, cyclohexyl; A is a direct bond, O, C 1- C8-Alkylene (linear or branched), C 1-C8-alkylidene (linear or branched), and n is 0 to 3; m is 1 to 3.
[0119] Particularly preferably, in the case of the above phosphonites, the group R is cyclohexyl, phenyl, phenylene, biphenyl and biphenylene; R1 is a compound of structure (IX) or (VI), R2 are independent of each other, C 1- C8-Alkyl (linear or branched), C 1- C8-alkoxy, cyclohexyl A is a direct bond, O, C 1- C6-alkylidene (linear or branched), and n is 1 to 3; m is 1 or 2.
[0120] Additionally, mixtures of the above claimed compounds are claimed in combination with phosphites.
[0121] Particularly preferably, the compounds according to the above definition are prepared by Friedel-Crafts reaction of aromatics or heteroaromatics, such as benzene, biphenyl- or diphenyl ether, with phosphorus trihalides, preferably phosphorus trichloride, in the presence of Friedel-Crafts catalysts, such as aluminum chloride, zinc chloride, iron chloride, etc., and the subsequent reaction with phenols on which structures (IX) and (VI) are based, whereby mixtures of excess phosphorus trihalides and phosphites formed from the above phenols according to the above reaction sequence are expressly included.
[0122] Additionally, of these groups of compounds, the following structures (XII) and (XIII) are preferred:
[0123] [ka] where n can be 0 or 1, and these mixtures may optionally further comprise some compound (XIV) or (XV):
[0124] [ka] Component G) is typically C 14 ~C 40 Suitable are esters or salts of long-chain aliphatic carboxylic acids (fatty acids) having a chain length of 1 to 1000 . The esters are reaction products of the above carboxylic acids with customary polyhydric alcohols, such as ethylene glycol, glycerol, trimethylolpropane or pentaerythritol. The salts of the above carboxylic acids include, in particular, the alkali metal or alkaline earth metal salts, or the aluminum and zinc salts.
[0125] Preferably, component G) is an ester or salt of stearic acid, such as glycerol monostearate or calcium stearate.
[0126] Preferably, component G) is also the reaction product of montan wax acid and ethylene glycol.
[0127] Preferably, the reaction product is a mixture of ethylene glycol-mono-montan wax acid ester, ethylene glycol-dimontan wax acid ester, montan wax acid and ethylene glycol.
[0128] Preferably, component G) is also the reaction product of a montan wax acid and a calcium salt.
[0129] Particularly preferably, the reaction product is a mixture of 1,3-butanediol-mono-montan wax acid ester, 1,3-butanediol-di-montan wax acid ester, montan wax acid, 1,3-butanediol, calcium montanate and a calcium salt.
[0130] The composition of the present invention according to any one of claims 1 to 20 preferably has a glow wire ignition temperature (GWIT) of 775°C or higher according to IEC-60695-2-13 at a test specimen thickness of 0.4 to 3 mm.
[0131] The additives can be introduced into the plastics in various process steps. Thus, in the case of polyamides, it is possible to mix the additives into the polymer melt already at the beginning or end of the polymerization / polycondensation or in a subsequent compounding step. Furthermore, there are processing processes in which the additives are added even later. This is especially the case when using pigment- and additive masterbatches. Furthermore, it is also possible to introduce, in particular, powdery additives into optionally warm polymer pellets by a drying process using drums.
[0132] The invention also finally relates to a process for the production of flame-retardant polymer moldings, in which the flame-retardant polymer molding materials of the invention are processed at higher temperatures by injection molding (e.g. in an Aarburg Allrounder type injection molding machine) and compression, foam injection molding, gas injection molding, blow molding, film molding, calendaring, laminating or coating to give flame-retardant polymer moldings. EXAMPLES
[0133] example 1. Ingredients used Commercially available polyamides (component A): Polyamide 6.6 (PA 6.6-GV): Ultramid (登録商標) A27 (BASF SE, D) Polyamide 6: Ultramid (登録商標) B27 (BASF SE, D) Polyamide 6T / 66: Vestamid HTplus M1000 (Evonik, D) Polyamide 10T: Vestamid HTplus M3000 (Evonik, D)
[0134] Component E): Glass fiber PPG HP3610 (PPG, NL) with a diameter of 10 μm and a length of 4.5 mm
[0135] Flame retardant (component B): Aluminum salt of diethylphosphinic acid, hereafter referred to as DEPAL
[0136] Flame retardant (component C): Aluminum salt of phosphorous acid, hereafter referred to as PHOPAL
[0137] Flame retardant (component D): Delacal360 (Melam) Delacal420 (Melem) Delacal 500 (Melon), all from Delamin Ltd, UK
[0138] Comparison: MPP, Melamine Polyphosphate, Melapur (登録商標) 200 / 70, BASF AG, D
[0139] Phosphonite (component F): Sandostab (登録商標) P-EPQ, Clariant GmbH, D
[0140] Wax component (component G): Licowax (登録商標) E, Clariant Produkte (Deutschland) GmbH, D (Montan wax acid ester)
[0141] 2. Production, processing and testing of flame-retardant polyamide molding materials The flame retardant components were mixed with the phosphonite, lubricants and stabilizers in the ratios given in the table and were compounded via the side feeder of a twin-screw extruder (type Leistritz ZSE 27 / 44D) into PA6.6 at temperatures of 260-310° C. or into PA6 at 250-275° C. Glass fibers were added via a second side feeder. The homogenized polymer strands were withdrawn, cooled in a water bath and subsequently granulated.
[0142] After thorough drying, the molding materials were processed into test specimens in an injection molding machine (type Arburg 320 C Allrounder) at material temperatures of 250-300°C and tested and classified for flame retardancy according to the UL94 test (Underwriter Laboratories).
[0143] UL94 is the fire resistance class for: V-0: Afterflame time is 10 seconds or less, total afterflame time when exposed to flame 10 times is 50 seconds or less, no burning drips, no burnout of test piece, after flame exposure the afterflame time of the test piece is 30 seconds or less. V-1: Afterflame time after flame application is 30 seconds or less, total afterflame time after 10 flame applications is 250 seconds or less, afterflame time of the test piece after flame application is 60 seconds or less, other criteria are the same as V-0. V-2: Cotton indicator is ignited by burning droplets. Other criteria are the same as V-1. Unclassifiable (ucl): Does not meet fire resistance class V-2.
[0144] The glow-wire resistance was measured on the basis of the glow-wire test GWFI (glow-wire flammability index) according to IEC 60695-2-12 and on the basis of the glow-wire flammability test GWIT (glow-wire ignition temperature) according to IEC 60695-2-13. In the GWFI test, a glow-wire is used at temperatures between 550 and 960 °C on three test specimens (for example plates of the shape 60X60X1.5 mm) to determine the highest temperature at which the after-flame time does not exceed 30 seconds and the sample does not burn and fall off. In the GWIT test, by means of a comparable measurement, the glow-wire ignition temperature is determined, which is 25 K higher (30 K between 900 °C and 960 °C) than the highest glow-wire temperature that does not cause ignition within the application time of the glow-wire in three consecutive tests. Here, a flame with a burning time of more than 5 seconds is considered as ignition.
[0145] The flowability of the molding material was measured by determining the melt volume flow rate (MVR) at 275°C / 2.16kg. A higher MVR value means better flowability for the injection process. However, a large increase in MVR value may also indicate polymer degradation.
[0146] All tests in each series were carried out under identical conditions (temperature program, screw configuration, injection parameters, etc.) for comparability, unless otherwise stated.
[0147] The results of using the flame retardant-stabilizer mixtures according to the invention are shown in Examples B1 to B3. All amounts are expressed as % by weight and are based on the plastic molding composition including flame retardants, additives and reinforcing agents.
[0148] [Table 1]
[0149] Only with the inventive combination of polyamide, glass fiber, DEPAL, PHOPAL and melam or melem is it possible to achieve a flammability class of UL94 V-0 at 0.4 mm while at the same time achieving a GWIT above 775°C and a CTI of 600 Volts, 65 kJ / m 2 Impact strength of over 10 kJ / m 2 It has ultra-high notched impact strength and no discoloration (yellowness index <20). Blooming Moreover, only these compositions according to the invention show the desired whiteness. The use of DEPAL without PHOPAL (V1) does not achieve V-0, and the combination of DEPAL with MPP (V4) does indeed achieve V-0 and a GWIT of 775°C, but the polyamide molding composition shows no discoloration and Blooming Similarly, a CTI of 600V is not achieved. The combination of DEPAL and PHOPAL does not achieve a GWIT >= 775°C, and the combination of DEPAL and Melam (V3) does not meet UL94 V-0 and GWIT 775°C.
[0150] [Table 2]
[0151] Tests on polyamide 6 show a similar picture: only the inventive combinations of polyamide 6 with glass fibres, DEPAL, PHOPAL and Melem, have at the same time a UL94 V-0 at 0.4 mm, a GWIT>=775°C, a CTI of 600V, Blooming Thus, molding compositions are obtained which are free of .gamma. and have good flowability and good mechanical properties.
[0152] [Table 3]
[0153] Also for polyamide 10T, only the inventive combination of polyamide with glass fibres, DEPAL, PHOPAL and MELEM, simultaneously has UL94 V-0 at 0.4 mm, GWIT>=775°C, CTI 600V, Blooming The combination of DEPAL and MPP cannot be processed into PA10T.
[0154] [Table 4]
[0155] In polyamide 6T / 66, the inventive combination of polyamide with glass fiber, DEPAL, PHOPAL and MELOND simultaneously has UL94 V-0 at 0.4 mm, GWIT>=775°C, CTI 600V, Blooming The combination of DEPAL and MPP is not processable even in PA6T / 66.
[0156] Overall, only the combination of the present invention achieves all the required parameters. In addition, the present application relates to the invention described in the claims, but may also include the following as other aspects. 1. As component A), 1 to 96% by weight of one or more thermoplastic polyamides, and as component B), 2 to 25% by weight of a dialkylphosphinic acid salt of formula (I) [ka] [In the formula, R 1 and R 2 are the same or different and may be linear, branched or cyclic C 1 -C 18 -Alkyl, C 6 -C 18 -aryl, C 7 -C 18 -arylalkyl and / or C 7 -C 18 -alkylaryl, M means Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K and / or protonated nitrogen bases; m is 1 to 4; n is 1 to 4. As component C), 1 to 20% by weight of a salt of phosphorous acid, As component D) 1 to 20% by weight of one or more condensation products of melamine, As component E), 0 to 50% by weight of fillers and / or reinforcing materials, As component F), 0 to 2% by weight of a phosphite or phosphonite or a mixture thereof, and as component G), 0 to 2% by weight of typically C 14 ~C 40 Esters or salts of long chain aliphatic carboxylic acids (fatty acids) having a chain length of wherein the sum of said components is always 100% by weight. 2.15 to 89.9% by weight of component A), 5 to 20% by weight of component B), 2 to 10% by weight of component C), 2 to 10% by weight of component D), 1 to 50% by weight of component E), 0 to 2% by weight of component F) and 0.1 to 1% by weight of component G) 2. The flame retardant polyamide composition according to claim 1, comprising: 3.15 to 75.8% by weight of component A), 5 to 20% by weight of component B), 2 to 10% by weight of component C), 2 to 10% by weight of component D), 15 to 35% by weight of component E), 0.1 to 1% by weight of component F), and 0.1 to 1% by weight of component G) 3. The flame-retardant polyamide composition according to claim 1 or 2, comprising: 4.35 to 65.8% by weight of component A), 5 to 20% by weight of component B), 2 to 7% by weight of component C), 2 to 7% by weight of component D), 25 to 35% by weight of component E), 0.1 to 0.5% by weight of component F), and 0.1 to 0.5% by weight of component G) 4. The flame-retardant polyamide composition according to any one of 1 to 3 above, comprising: 5.35 to 96% by weight of component A), 2 to 25% by weight of component B), 1 to 20% by weight of component C), 1 to 20% by weight of component D), 0 to 50% by weight of component E), 0 to 2% by weight of component F) and 0 to 2% by weight of component G) 2. The flame retardant polyamide composition according to claim 1, comprising: 6. The flame-retardant polyamide composition according to any one of 1 to 5 above, characterized in that it has a comparative tracking index (CTI) of more than 500 volts measured in accordance with the International Electrotechnical Commission standard IEC-60112 / 3. 7. A flame-retardant polyamide composition according to any one of 1 to 6 above, characterized in that it achieves a rating of V-0 according to UL-94 at a test specimen thickness of 3.2 mm to 0.4 mm. 8. The flame-retardant polyamide composition according to any one of 1 to 7 above, characterized in that it has a glow-wire flammability index (GWFI) of 850°C or more according to IEC-60695-2-12 in a test specimen thickness of 0.4 to 3 mm. 9. The flame-retardant polyamide composition according to any one of 1 to 7 above, characterized in that it has a glow wire ignition temperature index (GWIT) of 750°C or more according to IEC-60695-2-13 in a test piece thickness of 0.4 to 3 mm. 10. The flame retardant polyamide composition according to any one of 1 to 9 above, characterized in that the polyamide (PA) is selected from the group consisting of PA6, PA6,6, PA4,6, PA12, PA6,10, PA6T / 66, PA6T / 6, PA4T, PA9T, PA10T, polyamide copolymers, polyamide blends and combinations thereof. 11. The flame-retardant polyamide composition according to any one of 1 to 10 above, characterized in that component A) is polyamide 66 or a copolymer or polymer blend of polyamide 66 and polyamide 6. 12. The flame-retardant polyamide composition according to any one of 1 to 10 above, characterized in that component A) is polyamide PA6T / 66, PA6T / 6, PA4T, PA9T and / or PA10T. 13. The flame-retardant polyamide composition according to any one of 1 to 12 above, characterized in that component D) is melam, melem and / or melon. 14. The flame-retardant polyamide composition according to any one of 1 to 13 above, characterized in that component D) is melem. 15. In component B), R 1 and R 2 15. The flame-retardant polyamide composition according to any one of 1 to 14 above, wherein are the same or different and represent methyl, ethyl, n-propyl, isopropyl, n-butyl, tert.-butyl, n-pentyl and / or phenyl. 16. The above-mentioned phosphorous acid salt (component (C)) is represented by the general formula (II) [HP(=O)O 2 ] 2- M m+ (II) is equivalent to 16. The flame-retardant polyamide composition according to any one of 1 to 15 above, characterized in that in the formula, M means Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na and / or K. 17. The above-mentioned phosphorous acid salt (component (C)) is aluminum phosphite Al(H 2 PO 3 ) 3 , secondary aluminum phosphite Al 2 (HPO 3 ) 3 , Aluminum phosphite tetrahydrate Al 2 (HPO 3 ) 3 *4aq, Aluminum Phosphonate, Basic Aluminum Phosphite Al(OH)(H 2 PO 3 ) 2 *2aq, Al7 (HPO 3 ) 9 (OH) 6 (1,6-Hexanediamine) 1.5 *12H 2 O, Al 2 (HPO 3 ) 3 *xAl 2 O 3 *nH 2 O (x=1 to 2.27, n=1 to 50) and / or Al 4 H 6 P 16 O 18 16. The flame-retardant polyamide composition according to any one of the above 1 to 15, 18. The salt of phosphorous acid is an aluminum phosphite of formula (III), (IV) and / or (V) Formula (III): Al 2 (HPO 3 ) 3 x (H 2 O) q (q means 0-4); Formula (IV) Al 2.00 M z (HPO 3 ) y (OH) v x (H 2 O) w (M represents an alkali metal ion, z is between 0.01 and 1.5. y means 2.63 to 3.5, v ranges from 0 to 2, and w means 0 to 4); Formula (V) Al 2.00 (HPO 3 ) u (H 2 PO 3 ) t x (H 2 O) s (u means 2 to 2.99, t means 2 to 0.01, and s means 0 to 4), and / or a mixture of the aluminum phosphite of the formula (VII) with a sparingly soluble aluminum salt and a nitrogen-free foreign ion, a mixture of the aluminum phosphite of the formula (IX) with an aluminum salt, a mixture of the aluminum phosphite of the formulas (VII) to (IX) with an aluminum phosphite [Al(H 2 PO 3 ) 3 ], secondary aluminum phosphite [Al 2 (HPO 3 ) 3 ], basic aluminum phosphite [Al(OH)(H 2 PO 3 ) 2 *2aq], Aluminum Phosphite Tetrahydrate [Al 2 (HPO 3 ) 3 *4aq], aluminum phosphonate, Al 7 (HPO 3 ) 9 (OH) 6 (1,6-Hexanediamine) 1.5 *12H 2 O, Al 2 (HPO 3 ) 3 *xAl 2 O 3 *nH 2 O (x=1-2.27 and n=1-50) and / or Al 4 H 6 P 16 O 18 16. The flame-retardant polyamide composition according to any one of 1 to 15 above, which is a mixture of 19. The flame-retardant polyamide composition according to any one of the above 1 to 18, characterized in that component C) has an average particle size of 0.2 to 100 μm. 20. The flame-retardant polyamide composition according to any one of 1 to 19 above, characterized in that the reinforcing filler or reinforcing material (component E)) is a glass fiber. 21. The flame-retardant polyamide composition according to any one of 1 to 20 above, characterized in that the phosphonite (component F)) has the following general structure: R-[P(OR 5 ) 2 ] m (VI) [In the formula, R is a monovalent or polyvalent aliphatic, aromatic or heteroaromatic organic group, and R 5 Structure (VII)
change
change
Claims
1. As component A), 15 to 89.9% by weight of one or more thermoplastic polyamides, As component B), 5 to 20% by weight of a dialkylphosphinic acid salt of the formula (I) 【Chemistry 1】 [In the formula, R 1 and R 2 are the same or different and are linear, branched or cyclic C 1 -C 18 -Alkyl, C 6 -C 18 -Aryl, C 7 -C 18 -arylalkyl or C 7 -C 18 - alkylaryl, M means Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K or a protonated nitrogen base; m is 1 to 4; as component C) 2 to 10% by weight of a salt of phosphorous acid, as component D) 2 to 10% by weight of one or more condensation products of melamine, as component E) 1 to 50% by weight of reinforcing fillers and / or reinforcing materials, As component F), 0 to 2% by weight of a phosphite or phosphonite or a mixture thereof, and As component G), typically 0.1 to 1% by weight of C 14 ~C 40 esters or salts of long chain aliphatic carboxylic acids (fatty acids) having a chain length of wherein the sum of said components is always 100% by weight, Component A) is a polyamide PA6T / 66, PA6T / 6, PA4T, PA9T and / or PA10T, and said flame retardant polyamide composition has the following characteristics: Comparative Tracking Index (CTI) of greater than 500 volts measured according to International Electrotechnical Commission standard IEC-60112 / 3; A rating of V-0 according to UL-94 for specimen thicknesses of 3.2 mm to 0.4 mm; and A Glow Wire Ignition Temperature Index (GWIT) of 750°C or higher according to IEC-60695-2-13 for test specimen thicknesses of 0.4 to 3 mm; The flame-retardant polyamide composition satisfies the above requirements at the same time.
2. 35 to 65.8% by weight of component A; 5 to 20% by weight of component B); 2 to 7% by weight of component C); 2 to 7% by weight of component D); 25 to 35% by weight of component E); 0.1 to 0.5% by weight of component F), and 0.1 to 0.5% by weight of component G) 2. The flame retardant polyamide composition of claim 1, comprising:
3. As component A), 35 to 96% by weight of one or more thermoplastic polyamides, As component B), 2 to 25% by weight of a dialkylphosphinic acid salt of the formula (I) 【Chemistry 2】 [In the formula, R 1 and R 2 are the same or different and are linear, branched or cyclic C 1 -C 18 -Alkyl, C 6 -C 18 -Aryl, C 7 -C 18 -arylalkyl or C 7 -C 18 - alkylaryl, M means Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K or a protonated nitrogen base; m is 1 to 4; as component C) 1 to 20% by weight of a salt of phosphorous acid, as component D) 1 to 20% by weight of one or more condensation products of melamine, as component E) 0 to 50% by weight of reinforcing fillers and / or reinforcing materials, As component F), 0 to 2% by weight of a phosphite or phosphonite or a mixture thereof, and As component G), typically 0 to 2% by weight of C 14 ~C 40 esters or salts of long chain aliphatic carboxylic acids (fatty acids) having a chain length of wherein the sum of said components is always 100% by weight, Component A) is a polyamide PA6T / 66, PA6T / 6, PA4T, PA9T and / or PA10T, and said flame retardant polyamide composition has the following characteristics: Comparative Tracking Index (CTI) of greater than 500 volts measured according to International Electrotechnical Commission standard IEC-60112 / 3; A rating of V-0 according to UL-94 for specimen thicknesses of 3.2 mm to 0.4 mm; and A Glow Wire Ignition Temperature Index (GWIT) of 750°C or higher according to IEC-60695-2-13 for test specimen thicknesses of 0.4 to 3 mm; The flame-retardant polyamide composition satisfies the above requirements at the same time.
4. 4. The flame-retardant polyamide composition according to claim 1, characterized in that it has a Glow Wire Flammability Index (GWFI) of 850° C. or more according to IEC-60695-2-12 at a test specimen thickness of 0.4 to 3 mm.
5. The flame retardant polyamide composition according to any one of claims 1 to 4, which does not exhibit blooming after storage for 14 days under conditions of 100% humidity and 70°C.
6. 6. The flame-retardant polyamide composition according to claim 1, wherein component D) is melam, melem and / or melon.
7. 7. The flame retardant polyamide composition according to claim 1, wherein component D) is melem.
8. In component B), R 1 and R 2 The flame-retardant polyamide composition according to any one of claims 1 to 7, characterized in that: are identical or different and denote methyl, ethyl, n-propyl, isopropyl, n-butyl, tert.-butyl, n-pentyl or phenyl.
9. The phosphorous acid salt (component (C)) is aluminum phosphite Al(H 2 P.O. 3 ) 3 , secondary aluminum phosphite Al 2 (H.P.O. 3 ) 3 , Aluminum phosphite tetrahydrate Al 2 (H.P.O. 3 ) 3 *4H 2 O, aluminum phosphonate, basic aluminum phosphite Al(OH)(H 2 P.O. 3 ) 2 *2H 2 O, Al 7 (H.P.O. 3 ) 9 (OH) 6 (1,6-Hexanediamine) 1.5 *12H 2 O, Al 2 (H.P.O. 3 ) 3 *xAl 2 O 3 *nH 2 O (x=1 to 2.27, n=1 to 50) and / or Al 4 H 6 P 16 O 18 The flame-retardant polyamide composition according to any one of claims 1 to 8,
10. The salt of phosphorous acid is an aluminum phosphite of the formula (III), (IV) and / or (V) Formula (III): Al 2 (HPO 3 ) 3 *(H 2 O) q (q is 0 to 4); Formula (IV) Al 2.00 M z (HPO 3 ) y (OH) v * (H 2 O) w (M represents an alkali metal ion, z is 0.01 to 1.5, y means 2.63 to 3.5, v ranges from 0 to 2, and w is 0 to 4; Formula (V) Al 2.00 (HPO 3 ) u (H 2 PO 3 ) t * (H 2 O) s (u means 2 to 2.99, t is between 2 and 0.01, and s is 0 to 4; The flame-retardant polyamide composition according to any one of claims 1 to 8,
11. 11. The flame-retardant polyamide composition according to claim 1, characterized in that component C) has an average particle size of 0.2 to 100 μm.
12. 12. The flame-retardant polyamide composition according to claim 1, characterized in that the reinforcing filler or reinforcement (component E)) is glass fibre.
13. 13. The flame-retardant polyamide composition according to claim 1, wherein the phosphonite (component F)) is of the following general structure: R-[P(OR 5 ) 2 ] m (VI) [In the formula, R is a monovalent or polyvalent aliphatic, aromatic or heteroaromatic organic group; and R 5 has the structure (VII) 【Chemistry 3】 or a compound of the formula: 5 forms a bridging group of structure (VIII) 【Chemistry 4】 Where: A is a direct bond, O, S, C 1-18 - alkylene (linear or branched), or C 1-18 - alkylidene (linear or branched), in which R 6 are, independently of each other, C 1-12 -Alkyl (linear or branched), C 1-12 -Alkoxy or C 5-12 - means cycloalkyl, and n is an integer from 0 to 5; m is an integer of 1 to 4.
14. 14. The flame-retardant polyamide composition according to claim 1, characterized in that component G) is an alkali metal, alkaline earth metal, aluminium and / or zinc salt of a long-chain fatty acid having 14 to 40 C atoms and / or a reaction product of a long-chain fatty acid having 14 to 40 C atoms with a polyhydric alcohol.
15. 15. The flame retardant polyamide composition of claim 14, wherein the polyhydric alcohol is selected from the group consisting of ethylene glycol, glycerol, trimethylolpropane and pentaerythritol.
16. 16. The flame retardant polyamide composition according to any one of claims 1 to 15, further comprising a telomer, said telomer being ethylbutylphosphinic acid, dibutylphosphinic acid, ethylhexylphosphinic acid, butylhexylphosphinic acid, ethyloctylphosphinic acid, sec-butylethylphosphinic acid, 1-ethylbutyl-butyl-phosphinic acid, ethyl-1-methylpentyl-phosphinic acid, di-sec-butylphosphinic acid (di-1-methyl-propylphosphinic acid), propyl-hexylphosphinic acid, dihexylphosphinic acid, hexyl-nonylphosphinic acid, dinonylphosphinic acid and / or their salts with the metals Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K.
17. A three-dimensional article comprising a composition according to any one of claims 1 to 16, characterized in that it is a moulded body, an injection moulded part, an extruded material or an extruded part.
18. 17. Use of the flame-retardant polyamide composition according to any one of claims 1 to 16 in or for plug connectors, current contact parts in power distribution equipment (earth leakage interruption), printed circuit boards, seals, power plugs, circuit breakers, lamp housings (LED housings), capacitor housings, coil components in or on circuit boards and ventilators for ground wires, plugs; housings for plugs, for cables, for flexible printed circuit boards, for mobile phone charging cables, engine covers, textile coatings or other products.
Citation Information
Patent Citations
synergistic flame retardant combination for polymers
DE19734437A1
synergistic flame retardant combination for plastics
DE19737727A1
flame retardant THERMOPLASTIC POLYESTER
DE2252258A1
Flame-retardant polyamide molding compounds
DE2447727A1
Method and apparatus for speckle pattern interferometric determination of point displacements
EP0024167A2