Thermoplastic resin composition and cushioning material
A thermoplastic resin composition with a specific blend of elastomers and plasticizers addresses moldability and adhesion issues, ensuring high transparency and flexibility in cushioning members without protective layers, thereby improving production efficiency and product quality.
Patent Information
- Application Number
- JP2020050153
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-19
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2040-03-19
AI Technical Summary
Existing thermoplastic resin compositions used for cushioning members in footwear and other applications face issues with moldability, surface roughness, and loss of transparency during molding, along with challenges in maintaining adhesion without the need for protective layers.
A thermoplastic resin composition comprising a styrene-based thermoplastic elastomer, urethane-based thermoplastic elastomer, paraffin oil as a first plasticizer, and glycerin fatty acid ester as a second plasticizer, with specific blending ratios and a sea-island structure, to enhance mold releasability, transparency, and adhesion without a protective layer.
The composition achieves high transparency, flexibility, and adhesion with improved mold releasability, reducing production costs and enhancing the quality of cushioning members by eliminating the need for surface treatments and protective layers.
Smart Images

Figure 0007561303000006 
Figure 0007561303000007 
Figure 0007561303000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic resin composition that can be used for, for example, cushioning materials for footwear such as shoe soles and insoles, protective cases for mobile information terminal devices such as smartphones, and grips and shoulder pads for bags, and to a cushioning material obtained by molding the same. [Background technology]
[0002] In recent years, cushioning materials with excellent design are being used to provide a cushioning effect to parts that are visible from the outside, such as the soles of footwear, protective cases for smartphones, grips and shoulder pads for bags, etc. For example, in shoe design for fields requiring functionality, such as sports shoes, walking shoes, and comfort shoes, the cushioning materials incorporated into the soles are required to be lightweight so as not to hinder the movement of the user, and further, to have high design properties such as a transparent appearance in order to incorporate the cushioning materials into the soles in a manner that is visible from the outside so that the functionality can be appealed to consumers. Therefore, various cushioning materials made of styrene-based thermoplastic elastomers that have low specific gravity and transparency have been proposed (Patent Documents 1 and 2).
[0003] For example, when applied to footwear, the cushioning material is bonded to a sole member having rubber elasticity made of EVA or the like and assembled into the sole, and both the cushioning material and the sole member are deformed by the impact and stress applied during exercise. At that time, the adhesive surface between the cushioning material and the sole member also expands and contracts, so it is important to maintain the adhesive state at the adhesive surface between the two. However, the adhesive between the cushioning material and the sole member must be bonded without impairing the transparency of the cushioning material, and the adhesive, primer, and adhesive method used are limited. Furthermore, the cushioning material is assembled into the sole in a partially exposed state so that it can be seen from the outside, so the adhesive area between the cushioning material and the sole member is also limited. Therefore, peeling of the adhesive state is likely to occur at the boundary between the exposed part that is not bonded and the inside of the sole that is bonded, that is, from the periphery of the exposed part. Since this peeling of the periphery of the exposed part is directly visible even if it is slight, extremely reliable adhesion is required while ensuring the function and quality of the product. In response to this demand, the present applicant has proposed a styrene-based thermoplastic resin composition that is excellent in transparency and flexibility (shock-absorbing properties) as well as adhesiveness (Patent Document 1).
[0004] The thermoplastic resin composition of Patent Document 1 contains a styrene-based thermoplastic elastomer (A), a urethane-based thermoplastic elastomer (B), a first plasticizer (C1) and a second plasticizer (C2) in order to improve all of the transparency, flexibility (shock-absorbing properties) and adhesion, and the blending ratio of the styrene-based thermoplastic elastomer (A) to the urethane-based thermoplastic elastomer (B) is (A):(B)=25:75 to 70:30 in mass ratio, the blending ratio of the first plasticizer (C1) is 85 to 135 parts by mass per 100 parts by mass of the styrene-based thermoplastic elastomer (A), and the blending ratio of the second plasticizer (C2) is 3.5 to 18 parts by mass per 100 parts by mass of the urethane-based thermoplastic elastomer (B), the first plasticizer (C1) is paraffin oil, and the second plasticizer (C2) is composed of a carboxylic acid ester. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent application 2019-058627 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the thermoplastic resin composition of Patent Document 1 has a problem that the molded article is difficult to release from the mold during molding, and the surface of the molded article becomes rough when the molded article is removed from the mold, causing a loss of transparency, and there is room for further improvement in terms of moldability. To address this problem, a method of performing a surface treatment process to improve the mold releasability on the mold surface is effective, but since the surface treatment process is expensive, it has been desired to improve the moldability of the thermoplastic resin composition from the viewpoint of production costs.
[0007] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a thermoplastic resin composition which has excellent transparency and flexibility (cushioning properties), is capable of forming a cushioning member with excellent adhesion even without forming a protective layer such as a urethane-based coating agent on the adherend surface, and further has excellent releasability from a molding die, reduces surface roughness of a molded article, and gives a molded article with a smooth surface and excellent surface transparency, and a cushioning member using the same.
[0008] Another object of the present invention is to provide a method for producing a thermoplastic resin composition which has excellent transparency and flexibility (shock-absorbing properties), can form a shock-absorbing member with excellent adhesion even without forming a protective layer such as a urethane-based coating agent on the bonding surface with other members, and further has excellent releasability from a molding die, reduces surface roughness of a molded article, and produces a smooth surface and excellent surface transparency of the molded article.
[0009] In order to solve the above problems, the thermoplastic resin composition of the present invention contains a styrene-based thermoplastic elastomer (A), a urethane-based thermoplastic elastomer (B), a first plasticizer (C1) and a second plasticizer (C2), and the blending ratio of the styrene-based thermoplastic elastomer (A) to the urethane-based thermoplastic elastomer (B) is (A):(B)=30:70 to 40:60 in mass ratio, the blending ratio of the first plasticizer (C1) is 85 to 135 parts by mass per 100 parts by mass of the styrene-based thermoplastic elastomer (A), and the blending ratio of the second plasticizer (C2) is 40 to 50 parts by mass per 100 parts by mass of the urethane-based thermoplastic elastomer (B), the first plasticizer (C1) is paraffin oil, and the second plasticizer (C2) is a glycerin fatty acid ester.
[0010] The thermoplastic resin composition of the present invention contains a styrene-based thermoplastic elastomer (A), a urethane-based thermoplastic elastomer (B), a first plasticizer (C1) and a second plasticizer (C2) in a predetermined blending ratio, whereby a two-phase sea-island structure is formed in which the styrene-based thermoplastic elastomer (A) is an island phase and the urethane-based thermoplastic elastomer (B) is a sea phase, and the functionality of the styrene-based thermoplastic elastomer, such as transparency and flexibility, and the adhesiveness of the urethane-based thermoplastic elastomer are both achieved. Specifically, by blending the styrene-based thermoplastic elastomer (A) and the urethane-based thermoplastic elastomer (B) in a mass ratio of (A):(B)=30:70 to 40:60, a composition is obtained that has flexibility and mechanical strength, has excellent adhesiveness even without a protective layer such as a urethane-based coating agent, and can sufficiently maintain the adhesive state with other members via the adhesive, and can form a molded product that is unlikely to peel off in the adhesive state. In addition, by setting the blending ratio of the first plasticizer (C1) to 85 to 135 parts by mass per 100 parts by mass of the styrene-based thermoplastic elastomer (A), and the blending ratio of the second plasticizer (C2) to 40 to 50 parts by mass per 100 parts by mass of the urethane-based thermoplastic elastomer (B), the refractive index of the styrene-based thermoplastic elastomer containing the first plasticizer (C1) and the refractive index of the urethane-based thermoplastic elastomer containing the second plasticizer (C2) are adjusted to be close to each other, thereby obtaining a composition that can form a molded product that has adhesion, flexibility, and mechanical strength while maintaining transparency. Furthermore, by selecting paraffin oil as the first plasticizer (C1) and glycerin fatty acid ester as the second plasticizer (C2), respectively, plasticity is preferentially imparted to the styrene-based thermoplastic elastomer (A) and the urethane-based thermoplastic elastomer (B), respectively. As a result, a composition is obtained that can form a molded article having a smooth molded surface and surface transparency (referred to as surface transparency) with excellent flexibility and adhesiveness that contribute to cushioning performance, excellent flowability during injection molding, and improved releasability from the molding die, thereby reducing surface roughness of the molded article.
[0011] It is also preferred that the first plasticizer (C1) and the second plasticizer (C2) in the thermoplastic resin composition of the present invention are blended in such a ratio that the difference between the refractive index of the mixture in a state where the first plasticizer (C1) is mixed with the styrene-based thermoplastic elastomer (A) and the refractive index of the mixture in a state where the second plasticizer is mixed with the urethane-based thermoplastic elastomer (B) is 0.003 or less. This provides a composition that has excellent releasability from a molding die, suppresses the loss of transparency caused by mixing two different types of elastomers, and forms a molded product with high transparency.
[0012] The first plasticizer (C1) of the thermoplastic resin composition of the present invention is also preferably paraffin oil having a weight average molecular weight of 400 to 1200. This allows the selection of suitable components capable of improving the transparency and mechanical strength of the molded article and the flowability during injection molding.
[0013] The thermoplastic resin composition of the present invention preferably further contains one or more compatibilizers selected from the group consisting of acid-modified styrene-based elastomers, polyurethane-based block copolymers, and acid-modified polyolefins, thereby improving the compatibility between the styrene-based thermoplastic elastomer (A) and the urethane-based thermoplastic elastomer (B), and selecting suitable components capable of improving the mechanical strength and peel adhesion strength of the molded article.
[0014] It is also preferred that the compatibilizer of the thermoplastic resin composition of the present invention is a maleic anhydride-modified styrene-based elastomer, which allows a particularly preferred component to be selected as the compatibilizer, and allows the transparency and flexibility of the molded article to be maintained while improving the tensile strength and peel adhesion strength.
[0015] The cushioning material of the present invention is a cushioning material obtained by molding the above-mentioned thermoplastic resin composition, and has a haze value (based on JIS K7135:2000) of 30% or less and a hardness of less than Asker C55 (SRIS 0101 standard). This results in a cushioning material that is transparent in appearance, has excellent design, and has excellent flexibility that contributes to cushioning performance.
[0016] The method for producing a thermoplastic resin composition of the present invention is a method for producing a thermoplastic resin composition as described above, and includes a premixing step of mixing a styrene-based thermoplastic elastomer (A) and a urethane-based thermoplastic elastomer (B) with paraffin oil as a first plasticizer (C1) and a glycerin fatty acid ester as a second plasticizer (C2) to obtain a first mixture (I) and a second mixture (II), respectively, and a kneading step of mixing and kneading the first mixture (I) and the second mixture (II) that have been through the premixing step. By providing the premixing step of mixing the first plasticizer (C1) with the styrene-based thermoplastic elastomer (A) to obtain the first mixture (I) and mixing the second plasticizer (C2) with the urethane-based thermoplastic elastomer (B) to obtain the second mixture (II), the components are easily uniformly dispersed in the kneading step. Therefore, a composition can be obtained which forms a molded article having high transparency, excellent flexibility which contributes to cushioning performance, and excellent releasability from a molding die resulting in a smooth molded surface with high surface transparency, as well as adhesion and mechanical strength.
[0017] In the method for producing a thermoplastic resin composition of the present invention, it is also preferable to mix the first plasticizer (C1) and the compatibilizer with the styrene-based thermoplastic elastomer (A) in the above-mentioned premixing step to obtain the first mixture (I). This improves the compatibility between the above-mentioned styrene-based thermoplastic elastomer (A) and the urethane-based thermoplastic elastomer (B), and provides a composition that forms a molded product with more stable adhesiveness and mechanical strength.
[0018] In the method for producing a thermoplastic resin composition of the present invention, it is also preferable that the amounts of the first plasticizer (C1) and the second plasticizer (C2) are adjusted in the premixing step so that the difference between the refractive index of the first mixture (I) and the refractive index of the second mixture (II) is 0.003 or less. This prevents a decrease in transparency due to kneading of the first mixture (I) and the second mixture (II), each of which contains a different type of elastomer, and provides a composition that forms a molded product with high transparency.
[0019] The method for producing the thermoplastic resin composition of the present invention preferably includes a kneading step of mixing and kneading the styrene-based thermoplastic elastomer (A), the urethane-based thermoplastic elastomer (B), paraffin oil as the first plasticizer (C1), and a glycerin fatty acid ester as the second plasticizer (C2). This allows suitable components to be selected as the first plasticizer (C1) and the second plasticizer (C2), and a composition suitable for mass production can be obtained, which forms a molded product having high transparency, excellent flexibility, adhesion, surface transparency, and mechanical strength that contribute to cushioning performance.
[0020] In the method for producing the thermoplastic resin composition of the present invention, it is also preferable to further mix and knead a compatibilizer in the kneading step. This improves the compatibility between the above-mentioned styrene-based thermoplastic elastomer (A) and the urethane-based thermoplastic elastomer (B), thereby improving the adhesiveness. 、 A composition that forms moldable products having more stable surface transparency and mechanical strength can be obtained. Effect of the Invention
[0021] According to the present invention, it is possible to provide a thermoplastic resin composition and a method for producing the same, which have the following excellent effects. (1) While possessing excellent transparency and flexibility (shock-absorbing properties), it also has excellent adhesion even when a protective layer such as a urethane-based coating agent is not formed on the adherend surface of the molded article, and it also has excellent releasability from the molding die. Therefore, it is possible to form a molded article with a smooth molded surface, excellent surface transparency, and mechanical strength. (2) Since the step of forming a protective layer on the surface to be adhered of the molded body can be omitted, the productivity of the cushioning material and the like can be improved and the manufacturing costs can be reduced. (3) The molded body has excellent releasability from the molding die, so no special surface treatment is required for the molding die and general mold materials can be used, further reducing manufacturing costs. [Brief description of the drawings]
[0022] [Figure 1] 1A and 1B are a plan view and a front view, respectively, each showing a schematic configuration of a test piece prepared for a peel adhesion strength test of a molded body (cushion member) in an example and a comparative example. [Diagram 2] FIG. 2 is a diagram illustrating a method for a peel adhesion strength test performed using the test piece of FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The thermoplastic resin composition of the present invention is a thermoplastic resin composition containing a styrene-based thermoplastic elastomer (A), a urethane-based thermoplastic elastomer (B), a first plasticizer (C1), and a second plasticizer (C2) in a predetermined blending ratio, among which the styrene-based thermoplastic elastomer (A) forms an island phase and the urethane-based thermoplastic elastomer (B) forms a sea phase, thereby achieving both the functionality of the styrene-based thermoplastic elastomer and the adhesiveness of the urethane-based thermoplastic elastomer. In addition, the first plasticizer (C1) (paraffin oil) preferentially plasticizes the styrene-based thermoplastic elastomer (A), and the second plasticizer (C2) (glycerin fatty acid ester) preferentially plasticizes the urethane-based thermoplastic elastomer (B), respectively, so that the refractive index of the styrene-based thermoplastic elastomer and the refractive index of the urethane-based thermoplastic elastomer are adjusted to be close to each other, thereby obtaining a composition that forms a molded product having high transparency and flexibility while also having excellent peel adhesion strength and mechanical strength. Each component will be described below.
[0024] The styrene-based thermoplastic elastomer (A) constituting the thermoplastic resin composition of the present invention will be described first. The styrene-based thermoplastic elastomer (A) refers to a styrene-based block copolymer (TPS), and is not particularly limited. Examples include modified SEBS such as styrene-ethylene-butylene-styrene block copolymer (SEBS), amine-modified styrene-ethylene-butylene-styrene block copolymer (amine-modified SEBS), and acid-modified styrene-ethylene-butylene-styrene block copolymer (acid-modified SEBS), or styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS). SEBS also includes hydrogenated block copolymers obtained by hydrogenating styrene-butadiene-styrene block copolymers, and amine-modified SEBS also includes hydrogenated block copolymers obtained by hydrogenating amine-modified styrene-butadiene-styrene block copolymers. SEEPS also includes hydrogenated block copolymers obtained by hydrogenating styrene-ethylene-isoprene-styrene block copolymers. As the styrene-based thermoplastic elastomer (A) of the present invention, it is possible to use only one of the above-mentioned styrene-based block copolymers or to use a combination of multiple types. However, from the viewpoint of excellent transparency and flexibility (shock-absorbing properties) of the molded product, styrene-ethylene-butylene-styrene block copolymer (SEBS) is preferably used. The weight-average molecular weight Mw of the styrene-based block copolymer used as the styrene-based thermoplastic elastomer (A) of the present invention is preferably 50,000 or more from the viewpoint of mechanical strength, and is preferably less than 200,000 from the viewpoint of adhesiveness and fluidity during molding, that is, 50,000 to 200,000 is preferred. By adopting a styrene-based block copolymer having a weight-average molecular weight Mw in the range of 50,000 to 200,000, excellent peel adhesion strength, mechanical strength, and good fluidity during molding can be obtained. The molecular weight in the present invention refers to the weight-average molecular weight Mw, which is a value measured by gel permeation chromatography (GPC).
[0025] The urethane-based thermoplastic elastomer (B) constituting the thermoplastic resin of the present invention refers to a urethane-based block copolymer (TPU), which is composed of a hard segment mainly composed of a diisocyanate and a short-chain diol, and a soft segment mainly composed of a diisocyanate and a long-chain polyol. Specific examples of the short-chain diol constituting the hard segment include, but are not limited to, ethylene glycol, propylene glycol, 1,4-butanediol, etc., and examples of the long-chain polyol constituting the soft segment include, for example, polyether polyol, polyester polyol, or polycarbonate polyol, and polyether polyol is preferred from the viewpoint of improving the mechanical strength and durability of the obtained molded body. In addition, examples of the isocyanate include, but are not limited to, aromatic isocyanates, aliphatic isocyanates, or alicyclic isocyanates. Among these, from the viewpoints of flexibility, mechanical strength, and production costs, a specific example of the urethane-based thermoplastic elastomer (B) is preferably a urethane-based block copolymer whose main raw materials are diphenylmethane diisocyanate (MDI), which is an aromatic isocyanate, and polytetramethylene ether glycol (PTMEG), which is a polyether-based polyol, and more preferably has a hardness of ASKER A65 or less (in accordance with JIS K 7215).
[0026] The thermoplastic resin composition of the present invention contains two kinds of plasticizers, a first plasticizer (C1) acting mainly on the styrene-based thermoplastic elastomer (A) and a second plasticizer (C2) acting mainly on the urethane-based thermoplastic elastomer (B). Note that this does not exclude the first plasticizer (C1) acting on the urethane-based thermoplastic elastomer (B) and the second plasticizer (C2) acting on the styrene-based thermoplastic elastomer (A) within a range that does not impair the effects of the present invention.
[0027] As the first plasticizer (C1) constituting the thermoplastic resin composition of the present invention, paraffin oil is used from the viewpoint of excellent transparency in appearance. The weight average molecular weight of the paraffin oil is preferably 400 or more from the viewpoint of peel adhesion strength and mechanical strength, and the weight average molecular weight is preferably 1200 or less from the viewpoint of fluidity during molding. Therefore, paraffin-based oils having a weight average molecular weight of 400 to 1200 are preferably used. This makes it possible to obtain a thermoplastic resin composition having excellent transparency and good peel adhesion strength, mechanical strength, and fluidity during molding.
[0028] On the other hand, the second plasticizer (C2) constituting the thermoplastic resin composition of the present invention is a glycerin fatty acid ester. The glycerin fatty acid ester used in the present invention can be selected from glycerin and / or its dehydration condensate and fatty acids having 12 or more carbon atoms, and can be used alone or in combination. Among them, in the present invention, it is preferable to use glycerin diacetomonolaurate, particularly from the viewpoint of adjusting the refractive index and improving fluidity. This makes it possible to obtain a composition that is excellent in transparency and has good flexibility, peel adhesion strength, adhesive strength, and surface transparency of molded products.
[0029] The blending ratio of the styrene-based thermoplastic elastomer (A) and the urethane-based thermoplastic elastomer (B) constituting the thermoplastic resin composition of the present invention is preferably (A):(B)=30:70-40:60 in terms of mass ratio, from the viewpoint of obtaining a molded product having flexibility and mechanical strength and excellent adhesiveness even without a protective layer such as a urethane-based coating agent. This forms a two-phase sea-island structure in which the styrene-based thermoplastic elastomer (A) is an island phase and the urethane-based thermoplastic elastomer (B) is a sea phase, and the functionality of the styrene-based thermoplastic elastomer and the adhesiveness of the urethane-based thermoplastic elastomer are both achieved. In addition, the blending ratio of the first plasticizer (C1) is preferably 85-135 parts by mass per 100 parts by mass of the styrene-based thermoplastic elastomer (A) from the viewpoint of improving the transparency, adhesiveness, mechanical strength, and fluidity during molding of the molded product. Furthermore, the blending ratio of the second plasticizer (C2) is preferably 40 to 50 parts by mass per 100 parts by mass of the urethane-based thermoplastic elastomer (B) from the viewpoint of improving the transparency, adhesion, flexibility, and releasability of the molded article from the molding die. By setting the blending ratio of the components of the thermoplastic resin composition within the above-mentioned range, the refractive index of the styrene-based thermoplastic elastomer material and the refractive index of the urethane-based thermoplastic elastomer material are close to each other, ensuring transparency, and improving the flexibility of both materials. As a result, a composition is obtained that forms a molded article that has flexibility, transparency, and light weight, and has excellent adhesion, surface transparency, and mechanical strength of the molded article even in the absence of a protective layer.
[0030] The thermoplastic resin composition of the present invention may further contain a compatibilizer. As the compatibilizer, from the viewpoint of improving the compatibility and mechanical strength between the styrene-based thermoplastic elastomer (A) and the urethane-based thermoplastic elastomer (B), for example, an acid-modified styrene-based elastomer, a polyurethane-based block copolymer, or an acid-modified polyolefin is preferably used. Among these, from the viewpoint of excellent transparency and compatibility, an acid-modified styrene-based elastomer is more preferably used, and a maleic acid-modified styrene-based elastomer is particularly preferably used. This makes it possible to obtain a composition that forms a molded product having improved peel adhesion strength and mechanical strength while maintaining excellent transparency and flexibility of the molded product. The blending ratio of the compatibilizer is preferably 3 to 15 parts by mass, more preferably 5 to 10 parts by mass, from the viewpoint of maintaining excellent adhesion and mechanical strength, relative to 100 parts by mass of the total amount (A+B+C1+C2) of the styrene-based thermoplastic elastomer (A), the urethane-based thermoplastic elastomer (B), the first plasticizer (C1), and the second plasticizer (C2).
[0031] Furthermore, the thermoplastic resin composition of the present invention may contain other additives within the range that does not impair the effects of the present invention. Examples of additives include pigments, colorants, lubricants, release agents, antioxidants, antibacterial agents, UV absorbers, light stabilizers, and heat resistance agents. These may be used alone or in combination.
[0032] By adjusting the blending ratio of each component in the thermoplastic resin composition of the present invention within the above-mentioned range, the molded product exhibits physical properties such as a haze value (in accordance with JIS K7136:2000) of 30% or less and a hardness of Asker C (SRIS 0101 standard) of less than 55. Therefore, the composition of the present invention is useful as a composition for forming a cushioning member having high transparency in appearance and sufficient flexibility that contributes to cushioning properties.
[0033] The thermoplastic resin composition of the present invention is produced by a known method for producing a resin composition. Specifically, for example, the composition is obtained by adding the blending components in a predetermined ratio using a melt kneader such as a single screw extruder, a twin screw extruder, a kneader, a Banbury mixer, or a heating roll, heating the blending components, and uniformly kneading each component in a molten state. The specific production process is not particularly limited, but it is preferable to have a premixing process in which a first plasticizer (C1) is mixed with a styrene-based thermoplastic elastomer (A) to obtain a first mixture (I), and a second plasticizer (C2) is mixed with a urethane-based thermoplastic elastomer (B) to obtain a second mixture (II), and a kneading process in which the first mixture (I) obtained in the premixing process and the second mixture (II) are mixed and kneaded. By having the pre-mixing step, a suitable plasticizer is mixed in advance for each elastomer, so that even if the first mixture (I) and the second mixture (II) are kneaded later, the styrene-based thermoplastic elastomer (A) is preferentially plasticized by the first plasticizer (C1), and the urethane-based thermoplastic elastomer (B) is preferentially plasticized by the second plasticizer (C2), so that a composition can be obtained that has better flexibility, adhesion, and mechanical strength, and also has better releasability from a molding die, resulting in a smooth molded surface and a molded product with excellent surface transparency. In addition, in the pre-mixing step, a mixing method such as a method of mixing each plasticizer into each thermoplastic elastomer and allowing it to absorb, a method of mixing each plasticizer into each thermoplastic elastomer and kneading, a method of mixing each plasticizer into each thermoplastic elastomer and allowing it to absorb, and then kneading can be used. Furthermore, in this premixing step, the blending ratios of the components are preferably adjusted so that the difference in refractive index between the first mixture (I) and the second mixture (II) is 0.003 or less, and more preferably adjusted so that the difference in refractive index is 0.001 or less. This adjusts the refractive index of the styrene-based thermoplastic elastomer material and the refractive index of the urethane-based thermoplastic elastomer material to be approximately the same, thereby obtaining a composition that forms a molded product with even better transparency.
[0034] In addition, when a compatibilizer is contained in the thermoplastic resin composition, it may be mixed and kneaded in either the above-mentioned preliminary dispersion step or the kneading step, but it is also preferable to add the compatibilizer to the styrene-based thermoplastic elastomer (A) in the preliminary mixing step and mix it with the first plasticizer (C1) to obtain the first mixture (I). This improves the compatibility between the first mixture (I) and the second mixture (II), and obtains a composition that forms a molded product with more stable adhesiveness and mechanical strength.
[0035] The thermoplastic resin composition of the present invention can also be produced by mixing each component at once. Specifically, the thermoplastic resin composition of the present invention can be produced by mixing and kneading the styrene-based thermoplastic elastomer (A), the urethane-based thermoplastic elastomer (B), the first plasticizer (C1), and the second plasticizer (C2), etc. As a result, the thermoplastic resin composition of the present invention can be obtained by a production method with better productivity while maintaining the above-mentioned characteristics of the thermoplastic resin composition (excellent transparency, flexibility and adhesion, releasability from a molding die, and the associated surface transparency). In addition, when a compatibilizer is contained as a component of the thermoplastic resin composition of the present invention, the compatibilizer may be mixed and kneaded together when the components are mixed at once.
[0036] The thermoplastic resin composition of the present invention can be formed into pellets, sheets, chips, etc. by known methods such as injection molding, extrusion molding, blow molding, compression molding, calendar molding, etc. Of course, it can also be molded into various molded articles, as described in detail below.
[0037] The cushioning member of the present invention is obtained by molding the thermoplastic resin composition into a predetermined shape by the above-mentioned injection molding method or the like. The cushioning member obtained from the composition of the present invention has a haze value (based on JIS K7136:2000) of 30% or less and a hardness of less than 55 Asker C (SRIS 0101 standard). Therefore, it is useful as a cushioning member with a transparent appearance and sufficient flexibility that contributes to cushioning properties. And, since it has excellent adhesion via an adhesive even without forming a protective layer such as a urethane-based coating agent on the bonding surface with other members, it is useful as a cushioning member that is highly productive and easy to incorporate. In addition, when bonding to other members, it is possible to bond by directly applying an adhesive to the surface of the molded body, etc., or to apply an adhesive or the like to the surface of the molded body after primer treatment with a primer agent or the like.
[0038] The cushioning material of the present invention is used as a cushioning material for footwear such as an insole, midsole or outsole, or an insole for a shoe, as well as a protective case for a mobile information terminal device such as a smartphone or tablet terminal, a grip for a bag, a shoulder pad, etc. Furthermore, since the cushioning material of the present invention is transparent, has excellent design, is lightweight and has excellent adhesiveness, it can be widely used in the fields of daily necessities, home appliances, furniture, apparel, and automobile parts, etc. EXAMPLES
[0039] The present invention will be described in detail below with reference to examples. The methods for measuring and evaluating the physical properties of the thermoplastic resin composition in the following examples and comparative examples are as follows.
[0040] (1) Haze value (transparency) According to JIS K7136:2000, the haze of each test piece was measured using a spectroscopic haze meter (Haze Meter SH 7000, manufactured by Nippon Denshoku Industries Co., Ltd.). The test pieces were each molded from each thermoplastic resin composition in the Examples and Comparative Examples to a size of 50 mm length x 50 mm width x 3 mm thickness. A haze value of 30% or less was rated as excellent (◯), and a haze value of more than 30% was rated as poor (×).
[0041] (2) Hardness (C hardness) The hardness of each test piece was measured using an Asker C durometer (SRIS 0101 standard) conforming to JIS K6253. The test pieces were each molded from each thermoplastic resin composition in the examples and comparative examples to a size of 60 mm length x 60 mm width x 12 mm thickness. The flexibility (shock-absorbing properties) was evaluated as good (○) when Asker C was less than 55, and poor (×) when it was 55 or more.
[0042] (3) Peel adhesion strength (referred to as "adhesive strength" in Tables 2 to 5) The peel adhesion strength of each test piece was measured in accordance with JIS K6854-3. The test method for peel adhesion strength will be specifically described with reference to FIG. 1 and FIG. 2. FIG. 1 shows a schematic configuration of the test piece 1, and FIG. 2 shows a test method for peel adhesion strength of the test piece. The test piece 1 shown in FIG. 1 was prepared as follows. Each thermoplastic resin composition in the examples and comparative examples was molded into a strip shape (width 20 mm × length 60 mm × thickness 3 mm) to prepare the test piece 2. This test piece 2 was bonded to a urethane piece 3 (Kuraray Co., Ltd., Kuramilon U2195, width 20 mm × length 60 mm × thickness 3 mm) similarly prepared into a strip shape with an adhesive 4 to obtain the test piece 1. More specifically, the surfaces of the test piece 2 and the urethane piece 3 were wiped with Kimwipe (registered trademark) soaked in acetone, and then dried at 60°C for 5 minutes. An adhesive (LOCTITE (registered trademark) BONDACE 812TF, manufactured by Henkel) was applied to one side of each of the test piece 2 and the urethane piece 3, and the process of drying at 60°C for 5 minutes was repeated twice, after which the test piece 2 and the urethane piece 3 were quickly bonded together. The test piece 2 was placed with the side facing up, and the test piece 2 was pressed with a hand roller at 2 to 3 kgf / cm. 2A pressure of 1000 MPa was applied to the specimen 1 to press the specimen 1 against the urethane piece 3, thereby obtaining a specimen 1. After the specimen 1 was cured for 12 hours, the specimen 2 and the urethane piece 3 of the specimen 1 were peeled off from each other by a tensile tester (Autograph (registered trademark), AT-100N, manufactured by Shimadzu Corporation) as shown in Fig. 2(A) and (B), and the peel adhesive strength was measured. In Fig. 2, 51 is a fixed-side tensile jig and 52 is a movable-side tensile jig. The load cell was 1 kN (100 kgf), the test speed was 50 mm / min, and the initial gap between the fixed-side tensile jig 51 and the movable-side tensile jig 52 was 20 mm. In Fig. 2, the adhesive 4 is omitted from the specimen.
[0043] In assessing adhesion, test pieces with a peel strength of 1.5 kgf / 20 mm or more and which underwent material failure were rated as having excellent adhesion (○), and test pieces with a peel strength of less than 1.5 kgf / 20 mm or which underwent interfacial peeling were rated as having poor adhesion (×).
[0044] (4)Surface transparency To evaluate surface transparency (moldability), a flat plate with a width of 120 mm, length of 80 mm, and thickness of 3 mm was injection molded at a molding temperature of 150°C to 200°C, while adjusting the conditions so as to avoid molding defects such as shorts and jetting. The molded product was then cut into approximately two equal parts in the thickness direction, and the transparency of the cut surface and the surface was visually confirmed. If there was no difference in transparency, it was rated as excellent (○), and if there was obvious cloudiness on the surface, it was rated as poor (×).
[0045] Table 1 shows the specifications of each component used in the following examples and comparative examples. The refractive index in Table 1 was measured using a refractometer (Atago Co., Ltd., DR-M2) in accordance with JIS K7105. Specifically, it is a value measured using a polarizing filter with a wavelength of 589 nm, and the samples of the styrene-based thermoplastic elastomer (A) and the urethane-based thermoplastic elastomer (B) were measured as 15 mm x 10 mm x 6 mm thick, and the first plasticizer (C1) and the second plasticizer (C2), which are liquid, were filled in a liquid sample measurement cell and measured. The A hardness in Table 1 is a value measured using a test piece (length 65 mm x width 65 mm x thickness 12 mm) with an A hardness durometer (Kobunshi Keiki Co., Ltd., Asker rubber hardness meter type A) in accordance with JIS K6253-2. On the other hand, the value of C hardness is a value obtained by measuring the hardness of a test piece molded to a length of 60 mm, a width of 60 mm, and a thickness of 12 mm using an Asker C durometer (SRIS 0101 standard) conforming to JIS K6253. Furthermore, the molecular weight Mw in Table 1 is a weight average molecular weight measured by gel permeation chromatography (GPC). Specifically, the molecular weight Mw was measured using a measuring device SHODEX (registered trademark) GPC-104 (product of Showa Denko K.K.) [separation column LF-404 (three columns connected), guard column LF-G, RI detector RI-74S (all products of Showa Denko K.K.)], with tetrahydrofuran as the eluent, under the conditions of a sample concentration of 10 mg / 4 ml, an eluent flow rate of 0.3 ml / min, and a column temperature of 40°C.
[0046] [Table 1]
[0047] [Example 1] The thermoplastic resin composition of this example was produced by the following procedure, and its effects were evaluated. Using the components shown in Table 1, 31.27 g of styrene-based thermoplastic elastomer (A), 72.96 g of urethane-based thermoplastic elastomer (B), 26.58 g of paraffin oil with a molecular weight of 1200 as the first plasticizer (C1), and 29.19 g of glycerin fatty acid ester as the second plasticizer (C2) were weighed out individually. Next, the styrene-based thermoplastic elastomer (A) and the first plasticizer (C1) were mixed at room temperature, and then heated at 100°C for 12 hours to thoroughly absorb and disperse the first plasticizer (C1) in the styrene-based thermoplastic elastomer (A), thereby obtaining a first mixture (I) (pre-mixing step). On the other hand, the urethane-based thermoplastic elastomer (B) and the second plasticizer (C2) were mixed at room temperature, and then heated at 100°C for 36 hours to thoroughly absorb and disperse the second plasticizer (C2) in the urethane-based thermoplastic elastomer (B), thereby obtaining a second mixture (II) (pre-mixing step). The refractive indices of the first mixture (I) and the second mixture (II) were measured in accordance with JIS K7105 using a refractometer (Atago Co., Ltd., DR-M2) with a polarizing filter at a wavelength of 589 nm. The difference between the refractive index of the first mixture (I) and the refractive index of the second mixture was 0.003 or less, and the refractive indices of both were approximately the same and close to each other. The first mixture (I) and the second mixture (II) obtained were dry-blended by manual stirring, and then kneaded for 25 minutes at 160 to 190 ° C and 40 rpm in a batch-type twin-screw kneader (TD3-10MDX type, manufactured by Toshin Co., Ltd.) (kneading step) to obtain 160 g of a thermoplastic resin composition. This composition was hot-press molded for 10 minutes under conditions of 170 ° C and a total load of 5 tonf (surface pressure of 13.9 MPa) into a predetermined test piece shape used in each evaluation method of the thermoplastic resin composition described above, and the obtained test piece was used to evaluate physical properties, etc. The samples of the first mixture (I) and the second mixture (II) used in the refractive index measurement were prepared separately from the preparation of the thermoplastic resin composition, by preparing 160 g each of the first mixture (I) and the second mixture (II) using the same compounding ratio and procedure for the refractive index measurement. Each was kneaded for 25 minutes at 160 to 210°C and a rotation speed of 40 rpm in a batch-type twin-screw kneader (TD3-10MDX type, manufactured by Toshin Corporation), and then hot-press molded into 15 mm x 10 mm x 6 mm thick test pieces.
[0048] [Examples 2 to 9] The thermoplastic resin compositions of each Example were obtained in the same manner as in Example 1, except that the compounding ratios of the components of the thermoplastic resin composition, ie, the styrene-based thermoplastic elastomer (A), the urethane-based thermoplastic elastomer (B), the first plasticizer (C1) and the second plasticizer (C2), were changed as shown in Table 2. Test pieces for evaluating physical properties were molded using the obtained thermoplastic resin compositions in the same manner as in Example 1, and the physical properties and the like were evaluated.
[0049] [Example 10] Using the components shown in Table 1, 30 g of styrene-based thermoplastic elastomer (A), 56 g of urethane-based thermoplastic elastomer (B), 40 g of first plasticizer (C1), 24 g of second plasticizer (C2), and 10 g of maleic anhydride-modified SEBS as compatibilizer (D) were individually weighed as shown in the blending ratio in Table 3 below. Next, the styrene-based thermoplastic elastomer (A), the first plasticizer (C1), and the compatibilizer (D) were mixed at room temperature, and then heated at 100°C for 12 hours to thoroughly absorb and disperse the first plasticizer (C1) and the compatibilizer (D) in the styrene-based thermoplastic elastomer (A), thereby obtaining a first mixture (I) (pre-mixing step). On the other hand, the urethane-based thermoplastic elastomer (B) and the second plasticizer (C2) were mixed at room temperature, and then heated at 100°C for 36 hours to allow the second plasticizer (C2) to be well absorbed and dispersed in the urethane-based thermoplastic elastomer (B), thereby obtaining a second mixture (II) (pre-mixing step). The refractive indexes of the first mixture (I) and the second mixture (II) were measured, respectively, and the difference between the two was calculated as an absolute value. The difference between the refractive index of the first mixture (I) and the refractive index of the second mixture was 0.003 or less, and the refractive indexes of the two were approximately the same and close to each other. The obtained first mixture (I) and second mixture (II) were kneaded in the same manner as in Example 1 to obtain 160 g of a thermoplastic resin composition. As in Example 1, a test piece for evaluating physical properties was molded using the obtained thermoplastic resin composition, and the physical properties and the like were evaluated.
[0050] The results of Examples 1 to 6 are shown in Table 2, and the results of Examples 7 to 10 are shown in Table 3. Here, the "refractive index difference" in Tables 2 and 3 refers to the difference (absolute value) between the refractive index value of a mixture (first mixture (I)) in a state in which a first plasticizer (C1) is mixed and dispersed in a styrene-based thermoplastic elastomer (A) and the refractive index value of a mixture (second mixture (II)) in a state in which a second plasticizer (C2) is mixed and dispersed in a urethane-based thermoplastic elastomer (B) (the same applies to the following Tables 3 to 6).
[0051] [Table 2]
[0052] [Table 3]
[0053] [Comparative Examples 1 to 4] The compositions of each comparative example were obtained in the same manner as in Example 1, except that the compounding ratios of the styrene-based thermoplastic elastomer (A), the urethane-based thermoplastic elastomer (B), the first plasticizer (C1) and the second plasticizer (C2) were changed as shown in Table 4 below. Test pieces for evaluating physical properties were molded using the obtained compositions in the same manner as in Example 1, and the physical properties were evaluated. The results of Comparative Examples 1 to 4 are shown in Table 4.
[0054] [Table 4]
[0055] [Comparative Examples 5 to 8] The compositions of each comparative example were obtained in the same manner as in Example 1, except that the compounding ratios of the styrene-based thermoplastic elastomer (A), the urethane-based thermoplastic elastomer (B), the first plasticizer (C1) and the second plasticizer (C2) were changed as shown in Table 5 below. Test pieces for evaluating physical properties were molded using the obtained compositions in the same manner as in Example 1, and the physical properties were evaluated. The results of Comparative Examples 5 to 8 are shown in Table 5.
[0056] [Table 5]
[0057] From the results of Examples 1 to 10 shown in Tables 2 and 3, it was found that by using the thermoplastic resin composition of the present invention, a thermoplastic resin composition that forms a molded article excellent in transparency, flexibility, adhesion, and surface transparency can be obtained. This molded article exhibits high adhesive strength even without a protective layer such as a urethane-based coating agent on the adherend surface, and is strongly bonded directly to other members via an adhesive. It was also found that the excellent surface transparency provides excellent releasability from a molding die during molding.
[0058] On the other hand, when the results of Examples 1 to 10 and Comparative Examples 1 and 2 are compared, it was found that when the blending ratio of the styrene-based thermoplastic elastomer (A) to the urethane-based thermoplastic elastomer (B) is out of the range of (A):(B)=30:70 to 40:60 in terms of mass ratio, the adhesiveness or surface transparency is reduced. In addition, it was confirmed from the results of Examples 1 to 10 and Comparative Examples 3 to 6 that when the blending ratio of the first plasticizer (C1) is out of the range of 85 to 135 parts by mass relative to 100 parts by mass of the styrene-based thermoplastic elastomer (A), at least one of the physical properties of transparency, flexibility, adhesiveness, or surface transparency is reduced. Furthermore, it was confirmed from the results of Examples 1 to 10 and Comparative Examples 3 to 4 and 7 to 8 that when the blending ratio of the second plasticizer (C2) is out of the range of 40 to 50 parts by mass relative to 100 parts by mass of the urethane-based thermoplastic elastomer (B), at least one of the physical properties of transparency, flexibility, adhesiveness, or surface transparency is reduced.
[0059] From these findings, it was confirmed that by setting the blending ratio of the styrene-based thermoplastic elastomer (A) and the urethane-based thermoplastic elastomer (B) at a mass ratio of (A):(B) = 30:70 to 40:60, the blending ratio of the first plasticizer (C1) at 85 to 135 parts by mass per 100 parts by mass of the styrene-based thermoplastic elastomer (A), and the blending ratio of the second plasticizer (C2) at 40 to 50 parts by mass per 100 parts by mass of the urethane-based thermoplastic elastomer (B), a thermoplastic resin composition was obtained that was excellent in transparency, flexibility (shock-absorbing properties), adhesion, and good releasability from a molding die, and that formed a molded product with excellent surface transparency.
[0060] The present invention is not limited to the above-described embodiments or examples, and various modified forms of design are also included in the technical scope within the scope that does not deviate from the gist of the invention described in the claims. [Explanation of symbols]
[0061] 1 Sample piece 2 Test piece (cushioning material of the embodiment or comparative example) 3 Urethane pieces 4. Glue 51 Fixed side tension jig 52 Movable side tension jig
Claims
1. A thermoplastic resin composition comprising a styrene-based thermoplastic elastomer (A), a urethane-based thermoplastic elastomer (B), a first plasticizer (C1), and a second plasticizer (C2), a blending ratio of the styrene-based thermoplastic elastomer (A) to the urethane-based thermoplastic elastomer (B) is (A):(B)=30:70 to 40:60 by mass ratio, the mixing ratio of the first plasticizer (C1) is 85 to 135 parts by mass per 100 parts by mass of the styrene-based thermoplastic elastomer (A), the mixing ratio of the second plasticizer (C2) is 40 to 50 parts by mass per 100 parts by mass of the urethane-based thermoplastic elastomer (B); The styrene-based thermoplastic elastomer (A) is a styrene-ethylene-butylene-styrene block copolymer (SEBS), The urethane-based thermoplastic elastomer (B) has a hard segment composed of a diisocyanate and a short-chain diol, and a soft segment composed of a diisocyanate and a long-chain polyol, the short-chain diol is at least one diol selected from the group consisting of ethylene glycol, propylene glycol, and 1,4-butanediol; the long-chain polyol is at least one polyol selected from the group consisting of polyether polyols, polyester polyols, and polycarbonate polyols; The first plasticizer (C1) is paraffin oil, A thermoplastic resin composition, wherein the second plasticizer (C2) is glycerin diacetomonolaurate.
2. The first plasticizer (C1) and the second plasticizer (C2) are The thermoplastic resin composition according to claim 1, characterized in that the first plasticizer (C1) is blended in such a ratio that the difference between the refractive index of the mixture in a state in which the first plasticizer is mixed with the styrene-based thermoplastic elastomer (A) and the refractive index of the mixture in a state in which the second plasticizer is mixed with the urethane-based thermoplastic elastomer (B) is 0.003 or less.
3. 3. The thermoplastic resin composition according to claim 1, wherein the first plasticizer (C1) is paraffin oil having a weight average molecular weight of 400 to 1,200.
4. The thermoplastic resin composition according to any one of claims 1 to 3, further comprising one or more compatibilizers selected from the group consisting of acid-modified styrene-based elastomers, polyurethane-based block copolymers, and acid-modified polyolefins.
5. 5. The thermoplastic resin composition according to claim 4, wherein the compatibilizer is a maleic anhydride-modified styrene-based elastomer.
6. A cushioning material obtained by molding the thermoplastic resin composition according to any one of claims 1 to 5, A cushioning material having a haze value (in accordance with JIS K7136:2000) of 30% or less and a hardness of less than Asker C55 (SRIS 0101 standard).
7. A method for producing the thermoplastic resin composition according to any one of claims 1 to 5, a pre-mixing step of previously mixing the styrene-based thermoplastic elastomer (A) and the urethane-based thermoplastic elastomer (B) with paraffin oil as the first plasticizer (C1) and glycerin diacetomonolaurate as the second plasticizer (C2) to obtain a first mixture (I) and a second mixture (II), respectively; a kneading step of mixing and kneading the first mixture (I) that has been subjected to the premixing step with the second mixture (II).
8. The method for producing a thermoplastic resin composition according to claim 7, characterized in that in the pre-mixing step, the first plasticizer (C1) and a compatibilizer are mixed with the styrene-based thermoplastic elastomer (A) to obtain a first mixture (I).
9. 9. The method for producing a thermoplastic resin composition according to claim 7 or 8, characterized in that, in the pre-mixing step, the amounts of the first plasticizer (C1) and the second plasticizer (C2) are adjusted so that a difference between a refractive index of the first mixture (I) and a refractive index of the second mixture (II) is 0.003 or less.
10. A method for producing the thermoplastic resin composition according to any one of claims 1 to 5, A method for producing a thermoplastic resin composition, comprising a kneading step of mixing and kneading the styrene-based thermoplastic elastomer (A), the urethane-based thermoplastic elastomer (B), paraffin oil as the first plasticizer (C1), and glycerin diacetomonolaurate as the second plasticizer (C2).
11. The method for producing a thermoplastic resin composition according to any one of claims 7 to 10, characterized in that in the kneading step, a compatibilizer is further mixed and kneaded.
Citation Information
Patent Citations
Thermoplastic resin composition and buffer member
JP2020158610A