Metal corrosion inhibitor and method for producing same

A co-condensate of silane coupling agents with epoxy and amino groups, combined with alkali metal silicate, addresses stability and corrosion issues in water-based lubricants, providing effective corrosion inhibition and stability for metals in machining processes.

JP7561345B2Active Publication Date: 2024-10-04CHUBU KIRESUTO +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020172410
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-13
Publication Date
2024-10-04
Estimated Expiration
2040-10-13

AI Technical Summary

Technical Problem

Conventional metal corrosion inhibitors, particularly those used in water-based lubricants for machining, fail to provide sufficient stability and corrosion inhibition due to dilution, alkalinity, and gelation issues, leading to corrosion of metals like aluminum and its alloys.

Method used

A metal corrosion inhibitor composed of a co-condensate of silane coupling agents with epoxy and amino groups, combined with alkali metal silicate, is developed to enhance stability and inhibit corrosion, featuring a pH range of 8 to 13, suppressing insolubility and precipitation.

Benefits of technology

The inhibitor maintains stability and effectively prevents metal corrosion in machining processes such as cutting, drilling, and polishing, ensuring excellent lubricity and corrosion resistance for metals like aluminum and its alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561345000001
    Figure 0007561345000001
  • Figure 0007561345000002
    Figure 0007561345000002
  • Figure 0007561345000003
    Figure 0007561345000003
Patent Text Reader

Abstract

To provide a metal corrosion inhibitor having superior stability and metal corrosion inhibitory effect, and a method for producing the same.SOLUTION: A metal corrosion inhibitor contains a cocondensate having a constitutional unit derived from a silane coupling agent having an epoxy group and a constitutional unit derived from a silane coupling agent having an amino group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metal corrosion inhibitor having excellent stability and metal corrosion inhibiting effect, and a method for producing the same. [Background technology]

[0002] Background Art As rust inhibitors for iron-based metal materials such as steel, and non-ferrous metal materials such as aluminum and titanium, particularly for aluminum and its alloys, phosphorus-based rust inhibitors such as phosphates and phosphoric acid esters, or organic rust inhibitors such as organic acid amine salts and heterocyclic compounds are widely used.

[0003] However, even if these rust inhibitors are mixed into aqueous lubricants for cutting, milling, drilling, polishing, etc. of metals, satisfactory rust prevention effects may not be obtained. The reasons are considered as follows. That is, the above-mentioned aqueous lubricants for processing are usually diluted with water by about 10 to 30 times before use, so that the concentration is insufficient and the rust prevention effect is not fully exerted. In addition, since the dilution liquid is generally alkaline with a pH of 8 or more, the oil-based agent components contained in the aqueous lubricant act as corrosive components, and it is thought that the environment is easily corroded, especially in the case of aluminum and its alloys. In addition, phosphorus-based rust inhibitors also have a major problem of promoting the decay and deterioration of the aqueous lubricant due to bacteria and mold as described above.

[0004] On the other hand, water-soluble alkali silicates, such as sodium silicate, have long been known as rust inhibitors for aluminum alloys, and are very inexpensive and easy to obtain. When mixed in an appropriate amount into an aqueous lubricant, they provide excellent rust prevention effects. Moreover, since they do not contain phosphorus, they do not promote the decay and deterioration of the aqueous lubricant. However, alkali silicates have a serious practical drawback in that they quickly gel in aqueous lubricants, and improvements are required in terms of stability over time.

[0005] On the other hand, Patent Document 1 describes that when a specific silane-based compound is blended into an aqueous lubricant as a metal corrosion inhibitor, corrosion of metal materials such as aluminum alloys can be prevented. Patent Document 2 describes that when an organosilicon compound obtained by hydrolyzing a hydrolyzable silane-based compound or its partial hydrolyzate having an organic group containing a nitrogen atom in its molecule and a hydrolyzable silane-based compound or its partial hydrolyzate is blended into an aqueous lubricant as a metal corrosion inhibitor, it is effective in preventing corrosion of aluminum alloys and the like.

[0006] The present inventors have developed a rust inhibitor composition containing an alkali silicate and a specific silane coupling agent (Patent Documents 3 and 4). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 9-194872 [Patent Document 2] JP 2003-268396 A [Patent Document 3] JP 2006-299356 A [Patent Document 4] JP 2006-299357 A Summary of the Invention [Problem to be solved by the invention]

[0008] As described above, various corrosion inhibitors for aluminum, aluminum alloys, etc. have been developed, but the present inventors have found that some of the conventional metal corrosion inhibitors are insufficient in terms of stability and metal corrosion inhibition effect. SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a metal corrosion inhibitor excellent in stability and metal corrosion inhibitory effect, and a method for producing the same. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that a co-condensate of a specific silane coupling agent can enhance the stability and metal corrosion inhibitory effect of a metal corrosion inhibitor, particularly one containing an alkali metal silicate, and have completed the present invention. The present invention will now be described.

[0010] [1] A metal corrosion inhibitor comprising a co-condensate containing a structural unit derived from a silane coupling agent having an epoxy group and a structural unit derived from a silane coupling agent having an amino group. [2] The metal corrosion inhibitor according to [1], wherein the structural unit derived from a silane coupling agent having an epoxy group is represented by the following formula (I), and the structural unit derived from a silane coupling agent having an amino group is represented by the following formula (II). [ka] [In the formula, R 1 ~R 4 is independently 1-6 represents a divalent hydrocarbon group, R 5 and R 6 are independently H or C 1-6 represents a monovalent hydrocarbon group, m and n each independently represent an integer of 0 to 3, When m and / or n are 2 or 3, there are multiple R 2 and / or R 4 may be the same or different from each other, In the formula (I), R 2 may be bonded to the terminal carbon to form a cyclic hydrocarbon group or a cyclic ether group. [3] The metal corrosion inhibitor according to [1] or [2] above, further comprising a base. [4] The metal corrosion inhibitor according to [3] above, wherein the base is an alkali metal silicate. [5] The metal corrosion inhibitor according to any one of the above [1] to [4], further comprising a solvent and having a pH of 8 or more and 13 or less. [6] The metal corrosion inhibitor according to any one of [1] to [5] above, wherein the metal is aluminum or an aluminum alloy. [7] A method for producing a metal corrosion inhibitor, comprising the step of co-condensing a silane coupling agent having an epoxy group and a silane coupling agent having an amino group in the presence of a base. [8] The method for producing a metal corrosion inhibitor according to the above [7], wherein the silane coupling agent having an epoxy group is represented by the following formula (III), and the silane coupling agent having an amino group is represented by the following formula (IV). [ka] [In the formula, R 1 ~R 4 is independently 1-6 represents a divalent hydrocarbon group, R 5 and R 6 are independently H or C 1-6 represents a monovalent hydrocarbon group, R 7 , R 8 , R 10 and R 11 is independently 1-6 represents an alkoxy group, R 9 and R 12 are independently H, C 1-6 Alkyl group, or C 1-6 represents an alkoxy group, m and n each independently represent an integer of 0 to 3, When m and / or n are 2 or 3, there are multiple R 2 and / or R 4 may be the same or different from each other, In the formula (III), R 2 may be bonded to the terminal carbon to form a cyclic hydrocarbon group or a cyclic ether group.

[0011] "C 1-6 The "divalent hydrocarbon group" is a divalent hydrocarbon group having 1 to 6 carbon atoms, for example, C1-6 Alkanediyl group, C 2-6 Alkenediyl group, C 2-6 Examples include alkynediyl groups, and phenyldiyl (phenylene).

[0012] "C 1-6 The term "alkanediyl group" refers to a linear or branched divalent saturated aliphatic hydrocarbon group having 1 to 6 carbon atoms. Examples include methanediyl, ethanediyl, methylmethanediyl, n-propanediyl, methylethanediyl, n-butanediyl, methylpropanediyl, dimethylethanediyl, n-pentanediyl, and n-hexanediyl. 1-4 Alkanediyl groups, more preferably C 1-3 It is an alkanediyl group.

[0013] "C 2-6 The term "alkenediyl group" refers to a linear or branched divalent unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms and one or more carbon-carbon double bonds. Examples include ethenediyl, n-propenediyl, methylethenediyl, n-butenediyl, methylpropenediyl, dimethylethenediyl, n-pentenediyl, and n-hexenediyl. Preferably, C 1-4 Alkenyl groups are preferred, and C 1-3 It is an alkenediyl group.

[0014] "C 2-6 The term "alkynediyl group" refers to a linear or branched divalent unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms and one or more carbon-carbon triple bonds. Examples of the alkynediyl group include ethynediyl, n-propynediyl, n-butynediyl, methylpropynediyl, n-pentynediyl, and n-hexynediyl. 1-4 Alkynediyl group, more preferably C 1-3 It is an alkynediyl group.

[0015] "C 1-6 The "monovalent hydrocarbon group" is a monovalent hydrocarbon group having 1 to 6 carbon atoms, for example, C 1-6 Alkyl group, C2-6 Alkenyl group, C 2-6 Examples include alkynyl groups, and phenyl groups.

[0016] "C 1-6 The term "alkyl group" refers to a linear or branched monovalent saturated aliphatic hydrocarbon group having 1 to 6 carbon atoms. Examples include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, n-pentyl, and n-hexyl. 1-4 is an alkyl group, more preferably C 1-3 It is an alkyl group.

[0017] "C 2-6 The term "alkenyl group" refers to a linear or branched monovalent unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms and one or more carbon-carbon double bonds. Examples include ethenyl (vinyl), 1-propenyl, 2-propenyl (allyl), isopropenyl, 2-butenyl, 3-butenyl, isobutenyl, pentenyl, and hexenyl. Preferably, C 1-4 alkenyl group, more preferably C 1-3 It is an alkenyl group.

[0018] "C 2-6 The term "alkynyl group" refers to a linear or branched monovalent unsaturated aliphatic hydrocarbon group having 2 to 6 carbon atoms and one or more carbon-carbon triple bonds. Examples include ethynyl, 1-propynyl, 2-propynyl, 2-butynyl, 3-butynyl, pentynyl, and hexynyl. Preferably, C 1-4 Alkynyl groups, more preferably C 1-3 It is an alkynyl group.

[0019] "C 1-6 The term "alkoxy group" refers to a linear or branched saturated aliphatic hydrocarbon oxy group having 1 to 6 carbon atoms. Examples include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, t-butoxy, n-pentoxy, n-hexoxy, and the like, and preferably C 1-4 is an alkoxy group, more preferably C 1-2It is an alkoxy group.

[0020] In the formula (I) and the formula (III), R 2 may be bonded to a terminal carbon to form a cyclic hydrocarbon group or a cyclic ether group, 2 Carbon atoms in the R 2 If there is one R 2 and the carbon atoms in R 2 It indicates that the carbon at the end opposite to the Si in the group containing may be covalently bonded to form a cyclic hydrocarbon group or a cyclic ether group. Examples of the cyclic hydrocarbon group include cyclobutyl, cyclopentyl, and cyclohexyl, and examples of the cyclic ether group include tetrahydrofuranyl and tetrahydropyranyl. For example, the structural unit represented by the formula (I) includes the following structural unit.

[0021] [ka] Effect of the Invention

[0022] The metal corrosion inhibitor according to the present invention is inhibited from insolubilization, precipitation, and sedimentation of insoluble components, and does not contain any components that cause spoilage, so it can be said to have both metal corrosion inhibition and storage stability. In addition, metal corrosion inhibitors are sometimes mixed with processing oils during metal processing, and insoluble components may precipitate at that time, whereas the metal corrosion inhibitor according to the present invention is inhibited from precipitating even when mixed with processing oil. Furthermore, by using the metal corrosion inhibitor according to the present invention as a rust-preventive lubricant in processing such as cutting, cutting, drilling, and polishing of metals, it is possible to enjoy excellent lubricity and effectively prevent corrosion of metal materials after processing. Thus, the metal corrosion inhibitor according to the present invention is very useful industrially because of its excellent stability and metal corrosion inhibition effect. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] First, a method for producing a metal corrosion inhibitor according to the present invention will be described. The method for producing a metal corrosion inhibitor according to the present invention includes a step of co-condensing a silane coupling agent having an epoxy group and a silane coupling agent having an amino group in the presence of a base.

[0024] The silane coupling agent used in the present invention has an epoxy group or an amino group on a silicon atom via a linker group, and has 2 or more C 1-6 It has an alkoxy group.

[0025] The linker group has the effect of facilitating the synthesis of the silane coupling agent and increasing the positional freedom of the epoxy group and the amino group. The linker group is not particularly limited as long as it has such an effect. For example, 1-6 Examples of the linked groups include an alkanediyl group, an ether group (-O-), a thioether group (-S-), a carbonyl group (-C(=O)-), a thionyl group (-C(=S)-), an ester group (-OC(=O)- or -C(=O)-O-), an amide group (-NH-C(=O)- or -C(=O)-NH-), a urea group (-NH-C(=O)-NH-), a thiourea group (-NH-C(=S)-NH-), a polyalkylene glycol group, and a polyvinyl alcohol group; as well as groups in which 2 or more and 5 or less of these groups are linked together. Examples of the linked groups include, for example, C 1-6 Alkanediyl-OC 1-6 Alkanediyl groups and -[C 1-6 Alkanediyl-NH-] m -C 1-6 Examples of the alkyl group include an alkanediyl group (wherein m is an integer of 0 to 3).

[0026] More specifically, the above-mentioned epoxy group-containing silane coupling agent (III) and amino group-containing silane coupling agent (IV) can be used. During co-condensation, the epoxy group of the epoxy group-containing silane coupling agent (III) is cleaved to generate a 1,2-diol structure. The R 7 , R 8 , R10 and R 11 The alkoxy groups of R are hydrolyzed and dehydrated and condensed with each other to form siloxane bonds. 9 and / or R 12 When is an alkoxy group, the cocondensate is extended not only in one dimension but also in two dimensions.

[0027] The ratio of the epoxy group-containing silane coupling agent (III) and the amino group-containing silane coupling agent (IV) may be appropriately adjusted within a range in which good metal corrosion inhibition action is exerted, and for example, the molar ratio of the epoxy group-containing silane coupling agent (III) to the amino group-containing silane coupling agent (IV) can be 1 or more and 20 or less. If the ratio is 1 or more, the stability of the metal corrosion inhibitor according to the present invention when mixed with processing oil can be more reliably maintained, and if the ratio is 20 or less, the rust prevention performance can be more reliably exerted. The molar ratio is preferably 2 or more, more preferably 5 or more, and more preferably 15 or less.

[0028] Examples of the epoxy group-containing silane coupling agent (III) include γ-glycidoxymethyltrimethoxysilane, γ-glycidoxymethyltriethoxysilane, γ-glycidoxymethylmethyldimethoxysilane, γ-glycidoxymethylmethyldiethoxysilane, γ-glycidoxymethylethyldimethoxysilane, γ-glycidoxymethylethyldiethoxysilane, γ-glycidoxymethylpropyldimethoxysilane, γ-glycidoxymethylpropyldiethoxysilane, γ-glycidoxymethylbutyldimethoxysilane, γ-glycidoxymethylbutyl ...ethyldimethoxysilane, γ-glycidoxymethylethyldimethoxysilane, γ-glycidoxymethylethyldiethoxysilane, γ-glycidoxymethylpropyldimethoxysilane, γ-glycidoxymethylpropyldiethoxysilane, γ-glycidoxymethylpropyldimethoxysilane, γ-glycidoxymethylpropyldiethoxysilane, γ-glycidoxymethylbutylbutyldimethoxysilane, γ-glycidoxymethylbutylbutyldimethoxysilane, γ-glycidoxymethylbutylbutyldimethoxysilane, γ-glycidoxymethylbutylbutyldimethoxysilane, γ-glycidoxymethylbutylbutyldimethoxysilane, γ-glycidoxymethylbutylbutyldimethoxysilane, γ-glycidoxymethylbutylbutyldimethoxysilane, γ-glycidoxymethylbutylbutyldimethoxysilane, γ-glycidoxymethylethyldimethoxysilane, γ-glycidoxymethylethyldimethoxysilane, γ-glyc ethyldiethoxysilane, γ-glycidoxyethyltrimethoxysilane, γ-glycidoxyethyltriethoxysilane, γ-glycidoxyethylmethyldimethoxysilane, γ-glycidoxyethylmethyldiethoxysilane, γ-glycidoxyethylethyldimethoxysilane, γ-glycidoxyethylethyldiethoxysilane, γ-glycidoxyethylpropyldimethoxysilane, γ-glycidoxyethylpropyldiethoxysilane, γ-glycidoxyethylbutyldimethoxysilane, γ-glycidoxyethylbutyldiethoxysilane, γ-glycidoxypropyl propyltrimethoxysilane, gamma-glycidoxypropyltriethoxysilane, gamma-glycidoxypropylmethyldimethoxysilane, gamma-glycidoxypropylmethyldiethoxysilane, gamma-glycidoxypropylethyldimethoxysilane, gamma-glycidoxypropylethyldiethoxysilane, gamma-glycidoxypropylpropyldimethoxysilane, gamma-glycidoxypropylpropyldiethoxysilane, gamma-glycidoxypropylbutyldimethoxysilane, gamma-glycidoxypropylbutyldiethoxysilane, gamma-glycidoxybutyltrimethoxysilane , γ-glycidoxybutyltriethoxysilane, γ-glycidoxybutylmethyldimethoxysilane, γ-glycidoxybutylmethyldiethoxysilane, γ-glycidoxybutylethyldimethoxysilane, γ-glycidoxybutylethyldiethoxysilane, γ-glycidoxybutylpropyldimethoxysilane, γ-glycidoxybutylpropyldiethoxysilane, γ-glycidoxybutylbutyldimethoxysilane, γ-glycidoxybutylbutyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, etc. can be used.

[0029] As the amino group-containing silane coupling agent (IV), for example, N-2-aminoethyl-3-aminopropyltrimethoxysilane, N-2-aminoethyl-3-aminopropylmethyldimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, etc. can be used.

[0030] In the present invention, silane coupling agents other than the epoxy group-containing silane coupling agent (III) and the amino group-containing silane coupling agent (IV) may be used. Examples of such silane coupling agents include methyltrimethoxysilane, vinyltrimethoxysilane, N-2-(N-vinylbenzylaminoethyl)-3-aminopropylmethoxysilane, dimethyldimethoxysilane, methyltrimethoxysilane, phenyltriethoxysilane, tetramethylsilicate, and tetraethylsilicate.

[0031] When using silane coupling agents other than epoxy group-containing silane coupling agent (III) and amino group-containing silane coupling agent (IV), the ratio of epoxy group-containing silane coupling agent (III) and amino group-containing silane coupling agent (IV) to the total silane coupling agents is preferably 60 mass% or more or 70 mass% or more, more preferably 80 mass% or more or 90 mass% or more, and even more preferably 95 mass% or more or 98 mass% or more.The above ratio is 100 mass%, that is, as silane coupling agents, only epoxy group-containing silane coupling agent (III) and amino group-containing silane coupling agent (IV) are used substantially, and other coupling agents are not used.

[0032] In the present invention, a base is used as a catalyst for promoting the co-condensation reaction. Examples of the base that can be used include alkali metal silicates such as lithium silicate, sodium silicate, and potassium silicate; alkali metal hydroxides such as sodium hydroxide and potassium hydroxide; Group 2 metal hydroxides such as magnesium hydroxide and calcium hydroxide; alkali metal carbonates such as sodium carbonate and potassium carbonate; and alkali metal hydrogen carbonates such as sodium hydrogen carbonate and potassium hydrogen carbonate. As the base, an alkali metal silicate is preferred because it has a metal corrosion inhibitory effect by itself. The alkali metal silicate is represented by the formula MO·pSiO (M is an alkali metal, and p is a positive number greater than 0 and less than 10).

[0033] The solvent for the co-condensation reaction in the present invention is not particularly limited as long as it can dissolve the base and the silane coupling agent appropriately and does not inhibit the co-condensation reaction, but since the co-condensation reaction of the silane coupling agent involves a hydrolysis reaction, it is preferable to use an aqueous solvent. The aqueous solvent refers to water and a mixed solvent of water and a water-miscible organic solvent. The water-miscible organic solvent refers to an organic solvent that can be mixed with water without any restrictions, and is, for example, a C solvent such as methanol, ethanol, isopropanol, etc. 1-3 Examples of the solvent include alcohol solvents. The water-miscible organic solvent is useful for improving the solubility of a silane coupling agent, which has a relatively low solubility in water, in the solvent. The proportion of water in the mixed solvent is preferably 50% by mass or more or 60% by mass or more, more preferably 70% by mass or more or 80% by mass or more, and even more preferably 90% by mass or more. The upper limit of the proportion is not particularly limited, and may be 100% by mass, i.e., the solvent may be only water, but the proportion may be 98% by mass or less or 95% by mass or less.

[0034] The conditions of the co-condensation reaction may be appropriately adjusted within a range where at least the epoxy group-containing silane coupling agent (III) and the amino group-containing silane coupling agent (IV) are co-condensed well. For example, the ratio of the total amount of the silane coupling agent to the amount of the solvent can be 5% by mass or more and 30% by mass or less, and the ratio of the base to the amount of the solvent can be 10% by mass or more and 40% by mass or less.

[0035] Since the co-condensation reaction according to the present invention involves hydrolysis of the silane coupling agent, it is preferable to heat the reaction solution. The reaction temperature can be, for example, 50°C or higher and 120°C or lower, and the reaction can be carried out under heating and reflux. The reaction time can be, for example, 30 minutes or longer and 10 hours or shorter.

[0036] The reaction liquid after the reaction may be used as a metal corrosion inhibitor as it is, or may be diluted by adding a solvent. As the dilution solvent, an aqueous solvent may be used, and water is preferred. The dilution degree may be appropriately adjusted within a range in which the metal corrosion inhibitory effect is effectively exerted, but it is preferable to adjust, for example, so that the ratio of the co-condensate to the whole is 0.01% by mass or more and 10% by mass or less, and / or the ratio of SiO2 contained in the alkali metal silicate, which is a base having a metal corrosion inhibitory effect, to the whole is 0.01% by mass or more and 10% by mass or less.

[0037] The metal corrosion inhibitor according to the present invention contains a co-condensate comprising a structural unit derived from a silane coupling agent having an epoxy group and a structural unit derived from a silane coupling agent having an amino group.From the above reaction conditions, it is considered that the structural unit derived from a silane coupling agent having an epoxy group and the structural unit derived from a silane coupling agent having an amino group in the co-condensate are arranged randomly, and it is considered that the ratio of the structural unit derived from a silane coupling agent having an epoxy group and the structural unit derived from a silane coupling agent having an amino group in the co-condensate corresponds to the ratio of the structural unit derived from a silane coupling agent having an epoxy group and a silane coupling agent having an amino group used.In addition, it is possible that some of the silane coupling agent having an epoxy group and the silane coupling agent having an amino group remain without co-condensation.

[0038] In conventional metal corrosion inhibitors, for example, there is a problem that alkali metal silicate is easily gelled, and there is also a finding that such gelling is suppressed by condensation of silane coupling agent.On the other hand, the present inventors experimentally found that some silane coupling agents cannot sufficiently suppress such gelling, insolubility, precipitation, etc. in metal corrosion inhibitors, and thus stability is insufficient, while other silane coupling agents do not have sufficient metal corrosion suppression effect, and also found that the co-condensate that contains the structural unit derived from the silane coupling agent having epoxy group and the structural unit derived from the silane coupling agent having amino group can further improve the stability and metal corrosion suppression effect of metal corrosion inhibitors.

[0039] The structural unit derived from a silane coupling agent having an epoxy group that constitutes the co-condensation product of the present invention includes the one represented by the above formula (I), and the structural unit derived from a silane coupling agent having an amino group includes the one represented by the above formula (II).

[0040] The metal corrosion inhibitor according to the present invention may contain a base. In general, the higher the pH of a metal corrosion inhibitor containing a base, the higher the stability and anticorrosive effect. If the base contains an alkali metal silicate which itself exhibits a metal corrosion inhibitory effect, the metal corrosion inhibitory effect is further enhanced. On the other hand, if the pH is excessively high, non-ferrous metals such as aluminum and aluminum alloys are more likely to corrode. Therefore, it is preferable to adjust the pH of the metal corrosion inhibitor according to the present invention to 8 or more and 13 or less. In particular, alkali metal silicate can be made into a stable aqueous solution at a pH of 11 or more, but gels and forms insoluble matter at a pH of less than 11. In contrast, in the present invention, the co-condensate suppresses gelation and the formation of insoluble matter even at a pH of less than 11, and maintains stability.

[0041] The metal corrosion inhibitor according to the present invention is excellent in stability and exhibits excellent corrosion inhibition action against metals. Examples of the target metals include iron-based metals such as steel, non-ferrous metals such as aluminum and titanium, and alloys thereof, and is particularly effective against aluminum and aluminum alloys. The metal corrosion inhibitor according to the present invention is also useful as a lubricant anticorrosive agent when processing metals such as cutting, milling, drilling, and polishing. In particular, when the metal corrosion inhibitor according to the present invention is used for aluminum and its alloys, which are susceptible to corrosion by oily agent components for lubrication in an alkaline environment, its characteristics are more effectively exhibited, and excellent lubricant corrosion inhibition action is exhibited, which is preferable. EXAMPLES

[0042] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and it is possible to carry out the present invention by making appropriate modifications within the scope of the above and below-mentioned aims, and all of these modifications are included in the technical scope of the present invention.

[0043] Example 1: Preparation of metal corrosion inhibitor 350 g of deionized water and 50 g of γ-glycidoxypropyltrimethoxysilane were stirred at room temperature (25° C.) to obtain a transparent solution. Next, 95 g of approximately 50% by mass potassium silicate aqueous solution and 5 g of N-2-(aminoethyl)-3-aminopropyltrimethoxysilane were added and stirred and mixed at 90° C. for 2 hours to obtain a transparent solution that is a metal corrosion inhibitor.

[0044] Comparative Example 1: Preparation of metal corrosion inhibitor 150 g of an aqueous potassium silicate solution was added to 350 g of deionized water and stirred at room temperature for 1 hour to obtain a transparent solution that is a metal corrosion inhibitor.

[0045] Comparative Example 2: Preparation of metal corrosion inhibitor 350g of deionized water and 55g of γ-glycidoxypropyltrimethoxysilane were stirred at room temperature to obtain a transparent solution. Next, 95g of potassium silicate aqueous solution was added and stirred at 90°C for 2 hours to obtain a transparent solution of metal corrosion inhibitor.

[0046] Comparative Example 3: Preparation of metal corrosion inhibitor 350g of deionized water and 55g of N-2-(aminoethyl)-3-aminopropyltrimethoxysilane were stirred at room temperature to obtain a transparent solution. Next, 95g of potassium silicate aqueous solution was added and stirred at 90°C for 2 hours to obtain a transparent solution of metal corrosion inhibitor.

[0047] Test Example 1: Stability evaluation when processing oil is added The metal corrosion inhibitor (5.0 g) of Example 1 or Comparative Examples 1 to 3 and aluminum processing oil (95.0 g) not containing a metal corrosion inhibitor were placed in a transparent 100 mL glass container and thoroughly stirred to prepare a test solution. The appearance of the test solution immediately after preparation and after being left to stand at room temperature for 2 weeks was visually evaluated according to the following criteria. The results are shown in Table 1. ○: No turbidity or precipitation ×: Turbidity or sedimentation present

[0048] [Table 1]

[0049] As shown in Table 1, the metal corrosion inhibitors of Comparative Examples 1 and 3 remained opaque immediately after being mixed with the aluminum processing oil. On the other hand, the metal corrosion inhibitors of Example 1 and Comparative Example 2 were transparent and stable even after being left to stand for 2 weeks after being mixed with the aluminum processing oil.

[0050] Test example 2: Corrosion inhibition test The metal corrosion inhibitors (0.03 g) of Example 1 and Comparative Example 2, water-soluble aluminum processing oil (0.47 g) not containing a metal corrosion inhibitor, and tap water (49.5 g) were added to a 100 mL glass container and thoroughly stirred to prepare a test solution. The pH of the test solution was measured and found to be 10.2 in both cases. Note that, for the metal corrosion inhibitors of Comparative Examples 1 and 3 in Test Example 1, which showed turbidity and precipitation immediately after the end of stirring, this test was not performed. Aluminum test pieces were prepared by wet polishing 60×40×1.0 mm aluminum plates (JIS H 4000 A1050P) with #320 water-resistant emery paper and then washing with deionized water and acetone in that order. After wetting the entire surface of an aluminum test piece with each test liquid once, about half of the piece was immersed in each test liquid and left to stand at room temperature for one week. The test piece was then removed from the test liquid, washed with water and acetone, and dried, after which the degree of discoloration of the test piece was visually evaluated according to the following criteria. ◎: No discoloration ○: Slight discoloration △: Slight discoloration ×: Clear discoloration

[0051] [Table 2]

[0052] As shown in the results in Table 2, the aluminum test piece treated with the composition (Comparative Example 2) prepared by heating an aqueous solution containing γ-glycidoxypropyltrimethoxysilane and potassium silicate did not show any discoloration in the immersed area, but did show discoloration in the non-immersed area. In contrast, the aluminum test piece treated with the composition (Example 1) prepared by heating an aqueous solution containing γ-glycidoxypropyltrimethoxysilane, potassium silicate, and N-2-(aminoethyl)-3-aminopropyltrimethoxysilane did not show any discoloration in the immersed area, non-immersed area, or the interface between them. Thus, the metal corrosion inhibitor according to the present invention clearly had an excellent corrosion inhibitory effect on aluminum.

Claims

1. The composition contains a co-condensate including a structural unit derived from a silane coupling agent having an epoxy group and a structural unit derived from a silane coupling agent having an amino group, and an alkali metal silicate, A metal corrosion inhibitor characterized in that the structural unit derived from a silane coupling agent having an epoxy group is represented by the following formula (I), and the structural unit derived from a silane coupling agent having an amino group is represented by the following formula (II). 【Chemistry 1】 [In the formula, R 1 to R 4 each independently represent a C 1-6 divalent hydrocarbon group; R 5 and R 6 independently represent H or a C 1-6 monovalent hydrocarbon group; m and n each independently represent an integer of 0 to 3, When m and / or n are 2 or 3, multiple R 2 s and / or R 4 s may be the same or different from each other; In the formula (I), R 2 may be bonded to the terminal carbon to form a cyclic hydrocarbon group or a cyclic ether group.

2. A metal corrosion inhibitor as described in claim 1, wherein the molar ratio of the constituent units derived from a silane coupling agent having an epoxy group represented by formula (I) to the constituent units derived from a silane coupling agent having an amino group represented by formula (II) is 1 or more and 20 or less.

3. A metal corrosion inhibitor as described in claim 1 or 2, wherein the proportion of the co-condensate is 0.01 mass% or more and 10 mass% or less.

4. The metal corrosion inhibitor according to claim 1, wherein the proportion of SiO 2 contained in said alkali metal silicate is 0.01 mass % or more and 10 mass % or less.

5. The metal corrosion inhibitor according to any one of claims 1 to 4, further comprising a solvent and having a pH of 8 or more and 13 or less.

6. The metal corrosion inhibitor according to any one of claims 1 to 5, wherein the metal is aluminum or an aluminum alloy.

7. A method for producing a silane coupling agent having an epoxy group and a silane coupling agent having an amino group, comprising the steps of: co-condensing a silane coupling agent having an epoxy group and a silane coupling agent having an amino group in the presence of an alkali metal silicate; The method for producing a metal corrosion inhibitor, characterized in that the silane coupling agent having an epoxy group is represented by the following formula (III), and the silane coupling agent having an amino group is represented by the following formula (IV). 【Chemistry 2】 [In the formula, R 1 to R 4 each independently represent a C 1-6 divalent hydrocarbon group; R 5 and R 6 independently represent H or a C 1-6 monovalent hydrocarbon group; R 7 , R 8 , R 10 and R 11 each independently represent a C 1-6 alkoxy group; R 9 and R 12 independently represent H, a C 1-6 alkyl group, or a C 1-6 alkoxy group; m and n each independently represent an integer of 0 to 3, When m and / or n are 2 or 3, multiple R 2 s and / or R 4 s may be the same or different from each other; In the formula (III), R 2 may be bonded to the terminal carbon to form a cyclic hydrocarbon group or a cyclic ether group.

8. A method for producing a metal corrosion inhibitor as described in claim 7, wherein the molar ratio of the silane coupling agent having an epoxy group represented by formula (III) to the silane coupling agent having an amino group represented by formula (IV) is 1 or more and 20 or less.

Citation Information

Patent Citations

  • Curable composition for coating metal surface

    JP1980133466A

  • Water-soluble lubricant composition and method for inhibiting corrosion of metal

    JP1997194872A

  • Water-base lubricant composition and method for preventing corrosion of metal by using it

    JP2003268396A

  • Composition for rust-preventive agent, aqueous rust-preventive lubricant and working method using the same

    JP2006299356A

  • Rust preventive composition, water base rust preventive lubricant, and method for working metal using the same

    JP2006299357A