Methacrylic resin composition

The methacrylic resin composition addresses issues of transparency, surface hardness, and moldability by incorporating specific rubbery elastic bodies, resulting in improved performance for decorative and building material applications.

JP7561768B2Active Publication Date: 2024-10-04KURARAY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021567666
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-12-25
Publication Date
2024-10-04
Estimated Expiration
2040-12-25

AI Technical Summary

Technical Problem

Existing methacrylic resin compositions face challenges in achieving excellent transparency, surface hardness, moldability, and appearance while minimizing stress whitening, cracking, and maintaining surface smoothness during three-dimensional molding.

Method used

A methacrylic resin composition comprising a matrix of methacrylic resin with dispersed rubbery elastic bodies, including multilayer structure polymer particles and block copolymers, where specific particle sizes and content ratios enhance transparency, surface hardness, and moldability, while reducing stress whitening and cracking.

Benefits of technology

The composition achieves excellent transparency, surface smoothness, flex whitening resistance, surface hardness, and cracking resistance, making it suitable for decorative and building material applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561768000001
    Figure 0007561768000001
  • Figure 0007561768000002
    Figure 0007561768000002
  • Figure 0007561768000003
    Figure 0007561768000003
Patent Text Reader

Abstract

The present invention provides a methacrylic resin composition comprising: a methacrylic resin (A) which forms a matrix; and a rubber-like elastic body (B) which is dispersed, wherein when the total amount of the methacrylic resin (A) and the rubber-like elastic body (B) is 100 mass%, the methacrylic resin composition has the following characteristics: (1) the rubber-like elastic body (B) contains multilayer structure polymer particles (b1), multilayer structure polymer particles (b2), and a block copolymer (c); (2) the multilayer structure polymer particles (b1) each have at least one rubber component layer (core part) (b1-1), and a hard resin component layer (b1-2) at an outermost part (shell part), wherein the number-average particle diameter of the rubber component layer closest to the shell part is in the range of 0.05-0.16 μm (exclusive of 0.16), and the content of the multilayer structure polymer particles (b1) in the resin composition is 7.5-42.5 mass% (exclusive of 7.5); (3) the multilayer structure polymer particles (b2) each have at least one rubber component layer (core part) (b2-1), and a hard resin component layer (b2-2) at an outermost part (shell part), wherein the number-average particle diameter of the rubber component layer closest to the shell part is in the range of 0.16-0.3 μm, and the content of the multilayer structure polymer particles (b2) in the resin composition is 0.1-7.5 mass%; (4) the acetone-insoluble content of the methacrylic resin composition is 20-45% (exclusive of 20); (5) the block copolymer (c) contains a methacrylic polymer block (c1) and an acrylic polymer block (c2); and (6) the content of the block copolymer (c) in the methacrylic resin composition is in the range of 0.1-5.0 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a methacrylic resin composition. More specifically, the present invention relates to a methacrylic resin composition having excellent transparency, surface hardness, moldability and appearance after molding. [Background technology]

[0002] Methacrylic resin molded bodies have excellent optical properties such as transparency and weather resistance, and have a beautiful appearance, so they have been used for decorative purposes such as automobile interiors and exteriors and building materials. Methacrylic resin films, which have excellent weather resistance, transparency, surface hardness, and surface smoothness, have been used as surface protective films for the purpose of protecting decorative layers such as printed layers and imparting design properties such as a sense of luxury and depth. In recent years, they have also been increasingly used for components molded into three-dimensional shapes. Problems encountered during three-dimensional molding include stress whitening during molding, increased surface haze, and cracking, and the surface protective layer is required to have stress whitening resistance, surface smoothness, flexibility, and bending resistance in addition to the above properties.

[0003] As a resin molding having excellent whitening properties during molding, a method using crosslinked rubber polymer particles having a particle size of 0.1 μm or less (Patent Document 1) and a method using a block copolymer as the rubber particles (Patent Document 2) have been proposed. However, it has been difficult to suppress cracking during molding while maintaining high surface hardness using only small crosslinked polymer particles or block copolymers.

[0004] A method of using two types of elastomer particles with different particle sizes, namely crosslinked elastomer particles with a large particle size of 0.2 to 0.4 μm and crosslinked elastomer particles with a small particle size of 0.02 to 0.15 μm, has been disclosed to produce a film with excellent surface hardness, stress whitening resistance, and crack resistance (Patent Document 3). However, it is known that adding even a small amount of elastomer particles with a large particle size of 0.2 μm or more impairs surface smoothness and worsens the haze of a resin molded product, and has not yet achieved excellent surface hardness and moldability while suppressing appearance abnormalities such as whitening during molding and maintaining transparency. In addition, a method of using a multilayered polymer particle with a small particle size of 0.18 μm or less and a block copolymer in combination has been disclosed (Patent Document 4). However, there is a problem that the surface hardness is impaired and blocking occurs between films due to the addition of a large amount of block copolymer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2001-316557 A [Patent Document 2] WO2016 / 157908 [Patent Document 3] JP 2000-290397 A [Patent Document 4] WO2013-051239 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a methacrylic resin composition and a molded article which are excellent in transparency, surface hardness, slipperiness, moldability and appearance after molding and are suitable for decorative applications. [Means for solving the problem]

[0007] As a result of investigations aimed at solving the above problems, the present invention has been completed, including the following aspects. [1] A methacrylic resin composition in which a methacrylic resin (A) forms a matrix and a rubber-like elastomer (B) is dispersed, the methacrylic resin composition having the following characteristics when the total of the methacrylic resin (A) and the rubber-like elastomer (B) is 100 mass%: (1) The rubber-like elastomer (B) contains multilayer structure polymer particles (b1), multilayer structure polymer particles (b2) and a block copolymer (c). (2) The multilayer structure polymer particle (b1) has at least one rubber component layer (core portion) (b1-1) and a hard resin component layer (b1-2) in the outermost portion (shell portion), the number average particle diameter of the rubber component layer closest to the shell portion is in the range of 0.05 μm or more and less than 0.16 μm, and the content of the multilayer structure polymer particle (b1) in the resin composition is more than 7.5 mass% and not more than 42.5 mass%. (3) The multilayer structure polymer particle (b2) has at least one rubber component layer (core portion) (b2-1) and a hard resin component layer (b2-2) in the outermost portion (shell portion), the number average particle diameter of the rubber component layer closest to the shell portion is in the range of 0.16 μm or more and 0.3 μm or less, and the content of the multilayer structure polymer particle (b2) in the resin composition is 0.1 mass % or more and 7.5 mass % or less. (4) The acetone insoluble content of the methacrylic resin composition is more than 20% by mass and not more than 45% by mass. (5) The block copolymer (c) contains a methacrylic polymer block (c1) and an acrylic polymer block (c2). (6) The content of the block copolymer (c) in the methacrylic resin composition is in the range of 0.1% by mass or more and 5.0% by mass or less. [2] The methacrylic resin composition according to [1], characterized in that the multilayered polymer particle (b1) has at least one rubber component layer (b1-1) between an innermost layer and an outermost layer, the rubber component layer (b1-1) being made of a copolymer consisting of 50 to 98.99 mass% of acrylic acid ester monomer units, 1 to 44.99 mass% of other monofunctional monomer units, and 0.01 to 10 mass% of a polyfunctional monomer, and the innermost layer and the outermost layer are at least one hard resin component layer (b1-2) consisting of 40 to 100 mass% of methacrylic acid ester monomer units and 60 to 0 mass% of other monomer units. [3] The methacrylic resin composition according to [1], characterized in that the multilayered polymer particle (b2) has at least one rubber component layer (b2-1) between an innermost layer and an outermost layer, the rubber component layer (b2-1) being made of a copolymer containing 50 to 98.99% by mass of acrylic acid ester monomer units, 1 to 44.99% by mass of other monofunctional monomer units, and 0.01 to 10% by mass of a polyfunctional monomer, and the innermost layer and the outermost layer are at least one hard resin component layer (b2-2) containing 40 to 100% by mass of methacrylic acid ester monomer units and 60 to 0% by mass of other monomer units. [4] The methacrylic resin composition according to any one of [1] to [3], characterized in that the block copolymer (c) comprises at least one methacrylic polymer block (c1) and at least one acrylic polymer block (c2), and the block copolymer (c) contains 30 to 60 mass% of the methacrylic polymer block (c1) and 70 to 40 mass% of the acrylic polymer block (c2). [5] A molded article comprising the methacrylic resin composition according to any one of [1] to [4]. [6] The molded article according to [5], which is a film. [7] A method for producing a film, comprising melt-extruding or solution-casting the methacrylic resin composition according to any one of [1] to [4]. Effect of the Invention

[0008] A molded article comprising the methacrylic resin composition of the present invention, preferably a methacrylic melt extrusion molded article, is excellent in transparency, surface smoothness, resistance to whitening due to bending, surface hardness, cracking resistance and slipperiness, and is suitable for decorative applications and building material applications. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] "Methacrylic resin composition" A methacrylic resin composition in which a methacrylic resin (A) forms a matrix and a rubber-like elastomer (B) is dispersed, the methacrylic resin composition having the following characteristics when the total of the methacrylic resin (A) and the rubber-like elastomer (B) is taken as 100% by mass: (1) The rubber-like elastomer (B) contains multilayer structure polymer particles (b1), multilayer structure polymer particles (b2) and a block copolymer (c). (2) The multilayer structure polymer particle (b1) has at least one rubber component layer (core portion) (b1-1) and a hard resin component layer (b1-2) in the outermost portion (shell portion), the number average particle diameter of the rubber component layer closest to the shell portion is in the range of 0.05 μm or more and less than 0.16 μm, and the content of the multilayer structure polymer particle (b1) in the resin composition is more than 7.5 mass% and not more than 42.5 mass%. (3) The multilayer structure polymer particle (b2) has at least one rubber component layer (core portion) (b2-1) and a hard resin component layer (b2-2) in the outermost portion (shell portion), the number average particle diameter of the rubber component layer closest to the shell portion is in the range of 0.16 μm or more and 0.3 μm or less, and the content of the multilayer structure polymer particle (b2) in the resin composition is 0.1 mass % or more and 7.5 mass % or less. (4) The acetone insoluble content of the methacrylic resin composition is more than 20% by mass and not more than 45% by mass. (5) The block copolymer (c) contains a methacrylic polymer block (c1) and an acrylic polymer block (c2). (6) The content of the block copolymer (c) in the methacrylic resin composition is in the range of 0.1% by mass or more and 5.0% by mass or less.

[0010] The multilayered polymer particle (b1) is a core-shell particle having a core and a shell. The core has a rubber component layer (b1-1) at the outermost part (or the part closest to the shell), and the shell has a hard resin component layer (b1-2) at the outermost part. The core may be one rubber component layer (b1-1), or the core may be at least one rubber component layer (b1-1) + at least one hard resin component layer (b1-2). The shell includes one or more hard resin component layers (b1-2). The shell does not include a rubber component layer (b1-1). For example, when the shell is made of two hard resin component layers (b1-2), it is made of the outermost hard resin component layer (b1-2) and the hard resin component layer (b1-2) in contact with the rubber component layer (b1-1) of the core. When the shell portion is composed of one hard resin component layer (b1-2), the outermost hard resin component layer (b1-2) contacts the rubber component layer (b1-1) of the core portion.

[0011] The multilayered polymer particle (b2) is a core-shell particle having a core and a shell. The core has a rubber component layer (b2-1) at the outermost part (or the part closest to the shell), and the shell has a hard resin component layer (b2-2) at the outermost part. The core may be one rubber component layer (b2-1), or may be at least one rubber component layer (b2-1) + at least one hard resin component layer (b2-2). The shell includes one or more hard resin component layers (b2-2). The shell does not include a rubber component layer (b1-1). For example, when the shell is made of two hard resin component layers (b2-2), it is made of the outermost hard resin component layer (b2-2) and the hard resin component layer (b2-2) in contact with the rubber component layer (b2-1) of the core. When the shell portion is composed of one hard resin component layer (b2-2), the outermost hard resin component layer (b2-2) comes into contact with the rubber component layer (b2-1) of the core portion.

[0012] The acetone insoluble content of the methacrylic resin composition of the present invention is more than 20% by mass and not more than 45% by mass, preferably more than 27% by mass and not more than 44% by mass, more preferably more than 30% by mass and not more than 43% by mass. The methacrylic resin molded product is preferably cut into small pieces and used for measuring the acetone insoluble content.

[0013] The acetone insoluble matter can be calculated according to the following formula by using 25 mL of acetone per 1 g of the methacrylic resin composition, stirring at room temperature for 24 hours, centrifuging to separate the precipitate as the acetone insoluble matter, drying it, and measuring the mass.

[0014]

number

[0015] (Methacrylic resin (A)) The methacrylic resin (A) used in the present invention has a ratio of structural units derived from methyl methacrylate of 80% by mass or more, preferably 90% by mass or more, and a ratio of structural units derived from monomers other than methyl methacrylate of 20% by mass or less, preferably 10% by mass or less.

[0016] Examples of such monomers other than methyl methacrylate include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, s-butyl acrylate, t-butyl acrylate, amyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, pentadecyl acrylate, dodecyl acrylate; phenyl acrylate, benzyl acrylate, phenoxyethyl acrylate, 2-hydroxyethyl acrylate, ... acrylate, cyclohexyl acrylate, norbornenyl acrylate, isobornyl acrylate, and other acrylic esters; ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, s-butyl methacrylate, t-butyl methacrylate, amyl methacrylate, isoamyl methacrylate, n-hexyl methacrylate, 2- Ethylhexyl, pentadecyl methacrylate, dodecyl methacrylate; phenyl methacrylate, benzyl methacrylate, phenoxyethyl methacrylate, 2-hydroxyethyl methacrylate, 2-ethoxyethyl methacrylate, glycidyl methacrylate, allyl methacrylate, cyclohexyl methacrylate, norbornenyl methacrylate, isobornyl methacrylate and other methacrylic acid esters other than methyl methacrylate; acrylic acid, methacrylic acid, maleic anhydride, maleic acid, itaconic acid unsaturated carboxylic acids or their anhydrides such as carboxylic acid; olefins such as ethylene, propylene, 1-butene, isobutylene, 1-octene; conjugated dienes such as butadiene, isoprene, myrcene; aromatic vinyl compounds such as styrene, α-methylstyrene, p-methylstyrene, m-methylstyrene; acrylamide, methacrylamide, acrylonitrile, methacrylonitrile, vinyl acetate, vinylpyridine, vinyl ketone, vinyl chloride, vinylidene chloride, vinylidene fluoride, and the like.

[0017] The stereoregularity of the methacrylic resin (A) is not particularly limited, and for example, those having stereoregularity such as isotactic, heterotactic, or syndiotactic may be used.

[0018] The weight average molecular weight (hereinafter referred to as Mw(A)) of the methacrylic resin (A) is preferably 50,000 or more and 500,000 or less, more preferably 80,000 or more and 200,000 or less. If Mw(A) is too small, the impact resistance and toughness of the molded article obtained from the obtained methacrylic resin composition tend to decrease. If Mw(A) is too large, the flowability of the methacrylic resin composition tends to decrease, and the moldability tends to decrease.

[0019] The ratio of the weight average molecular weight Mw(A) to the number average molecular weight Mn(A) of the methacrylic resin (A), Mw(A) / Mn(A) (hereinafter, the ratio of the weight average molecular weight to the number average molecular weight (weight average molecular weight / number average molecular weight) may be referred to as the "molecular weight distribution") is preferably 1.03 or more and 2.6 or less, more preferably 1.05 or more and 2.3 or less, and particularly preferably 1.2 or more and 2.0 or less. If the molecular weight distribution is too small, the molding processability of the methacrylic resin composition tends to decrease. If the molecular weight distribution is too large, the impact resistance of a molded article obtained from the methacrylic resin composition tends to decrease and become brittle.

[0020] It should be noted that Mw(A) and Mn(A) are values ​​calculated as standard polystyrene measured by GPC (gel permeation chromatography).

[0021] The molecular weight and molecular weight distribution of the methacrylic resin can be controlled by adjusting the type and amount of the polymerization initiator and chain transfer agent.

[0022] The methacrylic resin (A) is obtained by polymerizing a monomer or a monomer mixture containing 80% by mass or more of methyl methacrylate.

[0023] In the present invention, a commercially available product may be used as the methacrylic resin (A). Examples of such commercially available methacrylic resins include "PARAPET H1000B" (MFR: 22 g / 10 min (230° C., 37.3 N)), "PARAPET GF" (MFR: 15 g / 10 min (230° C., 37.3 N)), "PARAPET EH" (MFR: 1.3 g / 10 min (230° C., 37.3 N)), "PARAPET HRL" (MFR: 2.0 g / 10 min (230° C., 37.3 N)), and "PARAPET G" (MFR: 8.0 g / 10 min (230° C., 37.3 N)) [all trade names, manufactured by Kuraray Co., Ltd.]. (Acrylic multi-layered polymer particles (b1)) The multilayered polymer particle (b1) is a core-shell particle having at least one rubber component layer (b1-1) (hereinafter sometimes simply abbreviated as "(b1-1)") and at least one hard resin component layer (b1-2) (hereinafter sometimes simply abbreviated as "(b1-2)"). The core of the multilayered polymer particle (b1) is considered to be a "layer". The number of layers of the multilayered polymer particle (b1) may be two or more, and may be three, four or more. Examples of the layer structure include, from the center, a two-layer structure of (b1-1)-(b1-2); a three-layer structure of (b1-1)-(b1-1)-(b1-2), (b1-1)-(b1-2)-(b1-2), or (b1-2)-(b1-1)-(b1-2); and a four-layer structure such as (b1-1)-(b1-2)-(b1-1)-(b1-2). Among them, from the viewpoint of handling, a three-layer structure of (b1-2)-(b1-1)-(b1-2) is preferred. In this specification, the core part may be described as the innermost layer, the shell part may be described as the outermost or outermost layer, and the layer (preferably a rubber component layer) sandwiched between the innermost layer and the outermost layer may be described as the intermediate layer.

[0024] The mass ratio ((b1-1) / (b1-2)) of the total amount of the rubber component layer (b1-1) to the total amount of the hard resin component layer (b1-2) is 30 / 70 to 90 / 10. If the ratio of (b1-1) is less than the above range, the impact strength of the molded article of the resin composition of the present invention may be insufficient. If the ratio of (b1-1) is more than the above range, it may be difficult to form a particle structure, and the melt fluidity may decrease, making it difficult to knead with other components and mold the resin composition of the present invention. The mass ratio ((b1-1) / (b1-2)) is preferably 30 / 70 to 80 / 20, more preferably 40 / 60 to 70 / 30. When the resin composition of the present invention has two or more rubber component layers (b1-1), the mass ratio is calculated based on the total amount thereof, and when the resin composition of the present invention has two or more hard resin component layers (b1-2), the mass ratio is calculated based on the total amount thereof.

[0025] The rubber component layer (b1-1) preferably contains a copolymer containing 50 to 98.99 mass% of acrylic acid ester monomer units, 44.99 to 1 mass% of other monofunctional monomer units, and 0.01 to 10 mass% of polyfunctional monomer units. The content of the acrylic acid ester monomer units is more preferably 55 to 89.9 mass%, the content of the monofunctional monomer units is more preferably 44.9 to 10 mass%, and the content of the polyfunctional monomer units is more preferably 0.1 to 5 mass%.

[0026] If the content of the acrylic acid ester monomer unit is less than 50% by mass, the rubber elasticity of the multilayered polymer particles (b1) may be insufficient, and the impact strength of the molded article of the resin composition of the present invention may be insufficient, and if it exceeds 98.99% by mass, it may be difficult to form a particle structure. If the content of other monofunctional monomer units is less than 1% by mass, the optical performance of the multilayered polymer particles may be insufficient, and if it exceeds 44.99% by mass, the weather resistance of the multilayered polymer particles (b1) may be insufficient. If the content of polyfunctional monomer units is more than 10% by mass, the rubber elasticity of the multilayered polymer particles (b1) may be insufficient, and the impact strength of the molded article of the methacrylic resin composition of the present invention may be insufficient, and if it is less than 0.01% by mass, it may be difficult to form a particle structure.

[0027] The raw material monomers for the rubber component layer (b1-1) will be described below.

[0028] Examples of the acrylic acid ester include acrylic acids such as methyl acrylate (MA), ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate (BA), isobutyl acrylate, s-butyl acrylate, t-butyl acrylate, pentyl acrylate, hexyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, and octadecyl acrylate, and saturated aliphatic alcohols (preferably C1 to C6 18 Examples of the acrylic acid ester include esters of acrylic acid and C5 or C6 alicyclic alcohols such as cyclohexyl acrylate, esters of acrylic acid and phenols such as phenyl acrylate, and esters of acrylic acid and aromatic alcohols such as benzyl acrylate. One or more types of acrylic acid esters can be used.

[0029] Other monofunctional monomers include methacrylic acid and saturated aliphatic alcohols (preferably C1 to C6), such as methyl methacrylate (MMA), ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, pentyl methacrylate, hexyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, myristyl methacrylate, palmityl methacrylate, stearyl methacrylate, and behenyl methacrylate. 22esters of methacrylic acid and C5 or C6 alicyclic alcohols, such as cyclohexyl methacrylate; esters of methacrylic acid and phenols, such as phenyl methacrylate, and esters of methacrylic acid and aromatic alcohols, such as benzyl methacrylate; aromatic vinyl monomers, such as styrene (St), α-methylstyrene, 1-vinylnaphthalene, 3-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, and halogenated styrene; cyanide vinyl monomers, such as acrylonitrile and methacrylonitrile. Among these, styrene is preferred. One or more of the other monofunctional monomers can be used.

[0030] The polyfunctional monomer is a monomer having two or more carbon-carbon double bonds in the molecule. Examples of the polyfunctional monomer include esters of unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, and cinnamic acid with unsaturated alcohols such as allyl alcohol and methallyl alcohol; diesters of the above unsaturated monocarboxylic acids with glycols such as ethylene glycol, butanediol, and hexanediol; diesters of dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, and maleic acid with the above unsaturated alcohols, and the like. Specific examples include allyl acrylate, methallyl acrylate, allyl methacrylate (ALMA), methallyl methacrylate, allyl cinnamate, methallyl cinnamate, diallyl maleate, diallyl phthalate, diallyl terephthalate, diallyl isophthalate, divinylbenzene, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, and hexanediol di(meth)acrylate. Among them, allyl methacrylate (ALMA) is preferable. One or more types of polyfunctional monomers can be used.

[0031] The layer (b1-2) preferably contains a copolymer consisting of 40 to 100% by mass of methacrylic acid ester monomer units and 60 to 0% by mass of other monomer units. The content of the methacrylic acid ester monomer units is more preferably 50 to 99% by mass, further preferably 60 to 99% by mass, particularly preferably 80 to 99% by mass, and the content of the other monomer units is more preferably 50 to 1% by mass, further preferably 40 to 1% by mass, and further preferably 20 to 1% by mass. If the content of the methacrylic acid ester monomer units is less than 40% by mass, the weather resistance of the multilayered polymer particles (b1) may be insufficient.

[0032] The raw material monomers for the hard resin component layer (b1-2) will be described below.

[0033] Examples of methacrylic acid esters include methyl methacrylate (MMA), ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, pentyl methacrylate, hexyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, dodecyl methacrylate, myristyl methacrylate, palmityl methacrylate, stearyl methacrylate, behenyl methacrylate, octadecyl methacrylate, phenyl methacrylate, and benzyl methacrylate. Among these, methyl methacrylate (MMA) is preferred.

[0034] Other monomers include acrylic acids and saturated aliphatic alcohols (preferably C1 to C6) such as methyl acrylate (MA), ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate (BA), isobutyl acrylate, s-butyl acrylate, t-butyl acrylate, pentyl acrylate, hexyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, and octadecyl acrylate. 18esters of acrylic acid with C5 or C6 alicyclic alcohols, such as cyclohexyl acrylate; aromatic vinyl monomers, such as styrene (St), α-methylstyrene, 1-vinylnaphthalene, 3-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, and halogenated styrenes; cyanide vinyl monomers, such as acrylonitrile and methacrylonitrile; maleimide monomers, such as maleimide, N-methylmaleimide, N-ethylmaleimide, N-propylmaleimide, N-isopropylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-(p-bromophenyl)maleimide, and N-(chlorophenyl)maleimide; and the polyfunctional monomers exemplified for layer (b1-1). Among these, alkyl acrylates such as methyl acrylate (MA), ethyl acrylate, and n-butyl acrylate (BA) are preferred.

[0035] In the multilayered polymer particles (b1), the weight average molecular weight (Mw) of the constituent copolymer of the outermost layer (b1-2) measured by GPC is preferably in the range of 20,000 to 100,000, more preferably in the range of 30,000 to 90,000, and particularly preferably in the range of 40,000 to 80,000. If Mw is less than 20,000, the rubber elasticity of the multilayered polymer particles (b1) may be insufficient, making it difficult to mold the resin composition of the present invention into a molded article. If Mw is more than 100,000, the impact strength of the molded article may be reduced.

[0036] The number average particle diameter of the rubber component layer (b1-1) of the multilayered polymer particle (b1) closest to the outermost layer (preferably in contact with the outermost layer) is in the range of 0.05 μm or more and less than 0.16 μm. If the number average particle diameter is less than 0.05 μm, the stress concentration on the multilayered polymer particle (b1) is insufficient, and the impact strength of the molded product may decrease. If the number average particle diameter is 0.16 μm or more, voids are generated in the multilayered polymer particle (b1) due to stress, and the multilayered polymer particle (b1) becomes white. In addition, when the rubber content in the resin composition is constant, if the particle diameter is increased to a certain degree or more, the number of particles decreases, so the surface distance between the particles tends to increase, and the probability of cracks occurring in the continuous phase increases, and the impact strength of the molded product may decrease. The voids referred to here are destruction that occurs only inside the particles, and the amount of energy absorbed is very small, so they do not contribute much to the development of impact resistance.

[0037] From the viewpoint of stress concentration on the multilayered polymer particles (b1), the number average particle size of the rubber component layer of the multilayered polymer particles (b1) is preferably 0.05 μm or more and less than 0.16 μm, more preferably 0.07 to 0.12 μm.

[0038] The average particle diameter of the rubber component layer (b1-1) of the multilayered polymer particle (b1) can be determined by a method of measuring the resin composition with an electron microscope or a method of measuring the latex with a light scattering method. In the method using an electron microscope, the average particle diameter is the average value of the major axis diameter and minor axis diameter of the rubber component layer (b1-1) of the dyed multilayered polymer particle (b1) constituting the outermost part when the resin composition of the present invention is electronically dyed with phosphotungstic acid or ruthenium tetroxide and observed with a transmission electron microscope. In the method using the light scattering method, the latex polymerized up to the rubber component layer during polymerization of the multilayered polymer particles is sampled, and the volume average particle diameter can be measured using a laser diffraction / scattering type particle size distribution measuring device LA-950V2 manufactured by Horiba, Ltd.

[0039] In a preferred embodiment of the present invention, the method for producing the multilayered polymer particle (b1) according to the present invention is not particularly limited as long as it is a method capable of producing the multilayered polymer particle (b1) having the rubber component layer (b1-1) / hard resin component layer (b1-2) as described above. A preferred method for producing the multilayered polymer particle (b1) having a three-layer structure (core-intermediate layer-outermost layer) according to the present invention includes the steps of emulsion polymerizing a monomer for obtaining a polymer constituting the center core to obtain a seed particle (b1-i), seed emulsion polymerizing a monomer for obtaining a polymer constituting the intermediate layer in the presence of the seed particle (b1-i) to obtain a seed particle (b1-ii), and seed emulsion polymerizing a monomer for obtaining a polymer constituting the outermost layer in the presence of the seed particle (b1-ii) to obtain a seed particle (b1-iii). A multilayered polymer (b1) having a two-layer structure or a four-layer or more layer structure can be easily produced by a person skilled in the art by referring to the above-mentioned description of the method for producing the multilayered polymer (b1) having a three-layer structure. The emulsion polymerization method or the seed emulsion polymerization method is a well-known technique in the art for obtaining general multilayered polymer particles, so other documents can be referred to for detailed explanation.In the above preferred example, the seed particle (b1-i) is a particle with a single layer structure consisting of a hard resin component layer (b1-2, core), the seed particle (b1-ii) is a particle with a two-layer structure consisting of a hard resin component layer (b1-2, core) + a rubber component layer (b1-1, intermediate layer), and the seed particle (b1-iii) is a particle with a three-layer structure consisting of a hard resin component layer (b1-2, core) + a rubber component layer (b1-1, intermediate layer) + a hard resin component layer (b1-2, outermost layer).

[0040] In the polymerization reaction step, the polymerization conditions are adjusted so that the Mw of the constituent copolymer of at least the outermost hard resin component layer (b1-2) is 20,000 to 100,000. The polymerization conditions are adjusted mainly by the amount of a molecular weight regulator such as an alkyl mercaptan. The polymerization conditions, such as the type and amount of emulsifier used in the entire polymerization reaction step, are adjusted so that the volume average particle size up to the outermost hard resin component layer (b1-2) in the finally obtained multilayer structure polymer particle (b1) is in the range of 0.05 μm or more and less than 0.16 μm.

[0041] The volume average particle diameter up to the outermost hard resin component layer (b1-2) in the multilayered polymer particle (b1) can be measured by a light scattering method using a laser diffraction / scattering type particle size distribution measuring device LA-950V2 manufactured by HORIBA, Ltd., by sampling the polymerized latex during polymerization of the multilayered polymer particle.

[0042] (Multilayer structure polymer particles (b2)) The multilayered polymer particle (b2) is a core-shell particle having at least one rubber component layer (b2-1) (hereinafter sometimes simply abbreviated as "(b2-1)") and at least one hard resin component layer (b2-2) (hereinafter sometimes simply abbreviated as "(b2-2)"). The core of the multilayered polymer particle (b2) is considered to be a "layer". The number of layers of the multilayered polymer particle (b2) may be two or more, and may be three, four or more. Examples of the layer structure include, from the center, a two-layer structure of (b2-1)-(b2-2); a three-layer structure of (b2-1)-(b2-1)-(b2-2), (b2-1)-(b2-2)-(b2-2), or (b2-2)-(b2-1)-(b2-2); and a four-layer structure such as (b2-1)-(b2-2)-(b2-1)-(b2-2). Among them, from the viewpoint of handling, a three-layer structure of (b2-2)-(b2-1)-(b2-2) is preferred. In this specification, the core part may be described as the innermost layer, the shell part may be described as the outermost or outermost layer, and the layer (preferably a rubber component layer) sandwiched between the innermost layer and the outermost layer may be described as the intermediate layer.

[0043] The mass ratio ((b2-1) / (b2-2)) of the total amount of the rubber component layer (b2-1) to the total amount of the hard resin component layer (b2-2) is 30 / 70 to 90 / 10. If the ratio of (b2-1) is less than the above range, the impact strength of the molded product of the resin composition of the present invention may be insufficient. If the ratio of (b2-1) is more than the above range, it may be difficult to form a particle structure, and the melt fluidity may decrease, making it difficult to knead with other components and mold the resin composition of the present invention. The mass ratio ((b2-1) / (b2-2)) is preferably 30 / 70 to 80 / 20, more preferably 40 / 60 to 70 / 30. When the resin composition of the present invention has two or more rubber component layers (b2-1), the mass ratio is calculated based on the total amount thereof, and when the hard resin composition of the present invention has two or more hard resin component layers (b2-2), the mass ratio is calculated based on the total amount thereof.

[0044] (b2-1) preferably contains a copolymer containing 50 to 98.99% by mass of acrylic acid ester monomer units, 44.99 to 10% by mass of other monofunctional monomer units, and 0.01 to 10% by mass of polyfunctional monomer units. The content of the acrylic acid ester monomer units is more preferably 55 to 89.9% by mass, the content of the monofunctional monomer units is more preferably 44.9 to 10% by mass, and the content of the polyfunctional monomer units is more preferably 0.1 to 5% by mass.

[0045] If the content of the acrylic acid ester monomer unit is less than 50% by mass, the rubber elasticity of the multilayer structure polymer particle (b2) may be insufficient, and the impact strength of the molded product of the resin composition of the present invention may be insufficient, and if it exceeds 98.99% by mass, it may be difficult to form a particle structure. If the content of other monofunctional monomer units is less than 10% by mass, the optical performance of the multilayer structure polymer particle may be insufficient, and if it exceeds 44.99% by mass, the weather resistance of the multilayer structure polymer particle (b2) may be insufficient. If the content of polyfunctional monomer units is more than 10% by mass, the rubber elasticity of the multilayer structure polymer particle (b2) may be insufficient, and the impact strength of the molded product of the methacrylic resin composition of the present invention may be insufficient, and if it is less than 0.01% by mass, it may be difficult to form a particle structure.

[0046] As the raw material monomer for the rubber component layer (b2-1), those described for the rubber component layer (b1-1) can be used.

[0047] The layer (b2-2) preferably contains a copolymer consisting of 50 to 100% by mass of methacrylic acid ester monomer units and 50 to 0% by mass of other monomer units. The content of the methacrylic acid ester monomer units is more preferably 60 to 99% by mass, and even more preferably 80 to 99% by mass, and the content of the other monomer units is more preferably 40 to 1% by mass, and even more preferably 20 to 1% by mass. If the content of the methacrylic acid ester monomer units is less than 50% by mass, the weather resistance of the multilayered polymer particles (b2) may be insufficient.

[0048] As the raw material monomer for the hard resin component layer (b2-2), those described for the hard resin component layer (b1-2) can be used.

[0049] In the multilayered polymer particles (b2), the weight average molecular weight (Mw) of the constituent copolymer of the outermost layer (b2-2) measured by GPC is preferably in the range of 20,000 to 100,000, more preferably in the range of 30,000 to 90,000, and particularly preferably in the range of 40,000 to 80,000. If Mw is less than 20,000, the rubber elasticity of the multilayered polymer particles (b2) may be insufficient, making it difficult to mold the resin composition of the present invention into a molded article. If Mw is more than 100,000, the impact strength of the molded article may be reduced.

[0050] The number average particle diameter of the rubber component layer of the multilayered polymer particles (b2) closest to the outermost layer (preferably in contact with the outermost layer) is in the range of 0.16 μm to 0.3 μm, which is larger than the number average particle diameter of the rubber component layer of the multilayered polymer particles (b1). Therefore, the multilayered polymer particles (b2) increase the surface roughness of the resin molded product and inhibit blocking. If the number average particle diameter of the multilayered polymer particles (b2) is less than 0.16 μm, the increase in surface roughness is insufficient, and blocking of the resin molded product is likely to occur. If the number average particle diameter exceeds 0.3 μm, the surface roughness increases too much, resulting in poor appearance after molding.

[0051] From the viewpoint of preventing blocking and imparting slipping property, the number average particle size of the rubber component layer of the multilayered polymer particles (b2) is preferably 0.195 to 0.25 μm, more preferably 0.20 to 0.23 μm.

[0052] The average particle size of the rubber component layer (b2-1) of the multilayered polymer particle (b2) can be measured in the same manner as the average particle size of the rubber component layer (b1-1).

[0053] In a preferred embodiment of the present invention, the method for producing the multi-layered polymer particles (b2) according to the present invention is the same as the method for producing the multi-layered polymer particles (b1).

[0054] In the polymerization reaction step, the polymerization conditions are adjusted so that the Mw of the constituent copolymer of at least the outermost hard resin component layer (b2-2) is 20,000 to 100,000. The polymerization conditions are adjusted mainly by the amount of a molecular weight regulator such as an alkyl mercaptan. The polymerization conditions, such as the type and amount of emulsifier used in the entire polymerization reaction step, are adjusted so that the volume average particle size up to the outermost hard resin component layer (b2-2) in the finally obtained multilayer structure polymer particle (b2) is in the range of 0.2 to 0.35 μm.

[0055] The volume average particle diameter up to the outermost hard resin component layer (b2-2) in the multilayered polymer particle (b2) can be measured by a light scattering method using a laser diffraction / scattering type particle size distribution measuring device LA-950V2 manufactured by HORIBA, Ltd., by sampling the polymerized latex during polymerization of the multilayered polymer particle.

[0056] (Block copolymer (c)) The block copolymer (c) used in the present invention has a methacrylic polymer block (c1) and an acrylic polymer block (c2). The block copolymer (c) may have only one methacrylic polymer block (c1) or a plurality of methacrylic polymer blocks (c1). The block copolymer (c) may have only one acrylic polymer block (c2) or a plurality of acrylic polymer blocks (c2). Such a block copolymer (c) has good compatibility with the methacrylic resin (A), the multilayered polymer particles (b1) and the multilayered polymer particles (b2).

[0057] From the viewpoint of the compatibility, the block copolymer (c) is preferably a block copolymer containing 10 to 80 mass% of a polymer block (c1) mainly having methacrylic acid ester monomer units and 90 to 20 mass% of a polymer block (c2) mainly having acrylic acid ester monomer units (wherein the total amount of the polymer block (c1) and the polymer block (c2) is 100 mass%). In the block copolymer (c), the content of the polymer block (c1) is more preferably 20 to 70 mass%, and even more preferably 30 to 60 mass%, and the content of the polymer block (c2) is more preferably 80 to 30 mass%, and even more preferably 70 to 40 mass%.

[0058] The number of polymer blocks (c1) in one molecule may be single or multiple. When the number of polymer blocks (c1) in one molecule is multiple, the composition and molecular weight of the structural units of the multiple polymer blocks (c1) may be the same or different. Similarly, the number of polymer blocks (c2) in one molecule may be single or multiple. When the number of polymer blocks (c2) in one molecule is multiple, the composition and molecular weight of the structural units of the multiple polymer blocks (c2) may be the same or different.

[0059] The polymer block (c1) mainly contains methacrylic acid ester monomer units. The content of the methacrylic acid ester monomer units in the polymer block (c1) is preferably 80% by mass or more, more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably 98% by mass or more, and may be composed of only methacrylic acid ester monomer units.

[0060] The raw material monomers for the methacrylic polymer block (c1) will be described below.

[0061] Examples of methacrylic acid esters include methyl methacrylate (MMA), ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, s-butyl methacrylate, t-butyl methacrylate, amyl methacrylate, isoamyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, pentadecyl methacrylate, dodecyl methacrylate, isobornyl methacrylate, phenyl methacrylate, benzyl methacrylate, phenoxyethyl methacrylate, 2-hydroxyethyl methacrylate, 2-methoxyethyl methacrylate, glycidyl methacrylate, and allyl methacrylate (ALMA). Among these, methyl methacrylate (MMA) is preferred from the viewpoint of improving the transparency and heat resistance of the methacrylic resin composition of the present invention. One or more types of methacrylic acid esters can be used.

[0062] The weight average molecular weight (Mw(c1)) of the methacrylic polymer block (c1) has a lower limit of preferably 5,000, more preferably 8,000, even more preferably 12,000, particularly preferably 15,000, and most preferably 20,000, and an upper limit of preferably 150,000, more preferably 120,000, and particularly preferably 100,000. When the block copolymer (c) has a plurality of polymer blocks (c1), the weight average molecular weight (Mw(c1)) is the total amount of Mw of the plurality of polymer blocks (c1).

[0063] In a preferred embodiment of the present invention, the weight average molecular weight Mw(c1) of the methacrylic polymer block (c1) of the block copolymer (c) and the weight average molecular weight Mw(A) of the methacrylic resin (A) satisfy the following formula (Y):

[0064]

number

[0065] The ratio of the weight average molecular weight Mw(A) of the methacrylic resin (A) to Mw(c1), i.e., Mw(A) / Mw(c1), is 0.5 to 2.5, preferably 0.6 to 2.3, more preferably 0.7 to 2.2. If Mw(A) / Mw(c1) is outside the above range, the dispersed particle size of the block copolymer (C) in the methacrylic resin (A) becomes large, and whitening occurs when stress is applied. If Mw(A) / Mw(c1) is within the above range, the dispersed particle size of the block copolymer (C) in the methacrylic resin (A) becomes small, and therefore the stress whitening resistance is excellent.

[0066] The content of the methacrylic polymer block (c1) in the block copolymer (c) is preferably 10 to 80 mass%, more preferably 20 to 70 mass%, from the viewpoints of transparency, softness, flexibility, bending resistance, impact resistance, moldability, and surface smoothness of a molded article of the methacrylic resin composition of the present invention. When the block copolymer (c) has a plurality of polymer blocks (c1), the content of the polymer block (c1) is the total content of the plurality of polymer blocks (c1).

[0067] In a preferred embodiment of the present invention, the acrylic polymer block (c2) mainly contains acrylic acid ester monomer units. The content of the acrylic acid ester monomer units in the acrylic polymer block (c2) is preferably 45% by mass or more, more preferably 50% by mass or more, further preferably 60% by mass or more, and particularly preferably 90% by mass or more.

[0068] The raw material monomers for the acrylic polymer block (c2) will be described below.

[0069] Examples of acrylic acid esters include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate (BA), isobutyl acrylate, s-butyl acrylate, t-butyl acrylate, amyl acrylate, isoamyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, pentadecyl acrylate, dodecyl acrylate, isobornyl acrylate, phenyl acrylate, benzyl acrylate, phenoxyethyl acrylate, 2-hydroxyethyl acrylate, 2-methoxyethyl acrylate, glycidyl acrylate, and allyl acrylate. One or more types of acrylic acid esters can be used.

[0070] In another preferred embodiment of the present invention, from the viewpoint of transparency of the resin composition of the present invention, the acrylic polymer block (c2) is preferably an acrylic polymer block (c2-p) containing an acrylic acid alkyl ester monomer unit and a (meth)acrylic acid aromatic hydrocarbon ester monomer unit. Here, the content of the acrylic acid alkyl ester monomer unit in the acrylic polymer block (c2) is preferably 50 to 90 mass%, more preferably 60 to 80 mass%, and the content of the (meth)acrylic acid aromatic hydrocarbon ester monomer unit is preferably 50 to 10 mass%, more preferably 40 to 20 mass%. Examples of the (meth)acrylic acid aromatic hydrocarbon ester include phenyl (meth)acrylate, benzyl (meth)acrylate, and phenoxyethyl acrylate.

[0071] In a preferred embodiment of the present invention, the weight average molecular weight Mw(c2) of the acrylic polymer block (c2) satisfies the following formula (Z), more preferably the following formula (Z1).

[0072] 5,000≦Mw(c2)≦120,000 (Z) 40,000≦Mw(c2)≦120,000 (Z1) The weight average molecular weight Mw(c2) of the acrylic polymer block (c2) is preferably 5,000, more preferably 15,000, even more preferably 20,000, particularly preferably 30,000, and most preferably 40,000, and is preferably 120,000, more preferably 110,000, and particularly preferably 100,000. If Mw(c2) is too small, the impact resistance of the molded article of the methacrylic resin composition of the present invention may decrease. On the other hand, if Mw(c2) is too large, the surface smoothness of the molded article of the resin composition of the present invention may decrease. When the block copolymer (c) has a plurality of acrylic polymer blocks (c2), the weight average molecular weight Mw(c2) is the total amount of Mw of the plurality of acrylic polymer blocks (c2).

[0073] The content of the acrylic polymer block (c2) in the block copolymer (c) is preferably 10 to 90% by mass, more preferably 20 to 80% by mass, from the viewpoints of transparency, softness, flexibility, bending resistance, impact resistance, moldability, and surface smoothness of the molded article of the methacrylic resin composition of the present invention. When the block copolymer (c) has a plurality of acrylic polymer blocks (c2), the content of the polymer block (c2) is the total content of the plurality of acrylic polymer blocks (c2).

[0074] The bond form between the methacrylic polymer block (c1) and the acrylic polymer block (c2) in the block copolymer (c) is not particularly limited. Among them, a diblock copolymer having a (c1)-(c2) structure and a triblock copolymer having a (c1)-(c2)-(c1) structure are preferred.

[0075] The block copolymer (c) may have functional groups such as hydroxyl groups, carboxyl groups, acid anhydride groups, and amino groups in the molecular chain and / or at the molecular chain terminals, if necessary.

[0076] The block copolymer (c) has a weight average molecular weight (Mw(c)) of 32,000 to 300,000, preferably 40,000 to 250,000, more preferably 45,000 to 230,000, and particularly preferably 50,000 to 200,000. By having Mw(c) within the above range, the amount of unmelted material during melt-kneading of the raw materials in the production of the resin composition, which causes the generation of bumps in the molded product, can be made extremely small.

[0077] The ratio (Mw(c) / Mn(c)) of the weight average molecular weight (Mw(c)) to the number average molecular weight (Mn(c)) of the block copolymer (c) is preferably 1.0 to 2.0, more preferably 1.0 to 1.6. When Mw(c) / Mn(c) is within the above range, the amount of unmelted material during melt-kneading of the raw materials in the production of the resin composition, which causes lumps in the molded product, can be made extremely small.

[0078] The refractive index of the block copolymer (c) is not particularly limited, and is preferably 1.485 to 1.495, more preferably 1.487 to 1.493. When the refractive index is within the above range, the transparency of the thermoplastic resin composition of the present invention is high. In this specification, the "refractive index" means a value measured at a wavelength of 587.6 nm (D line).

[0079] The method for producing the block copolymer (c) is not particularly limited, and a method of living polymerization of each polymer block is generally used. As the living polymerization method, a method of anion polymerization in the presence of an organic aluminum compound using an organic alkali metal compound as a polymerization initiator is particularly preferred, because the block copolymer (c) can be obtained with high purity, the composition and molecular weight of each block can be easily controlled, and it is economical.

[0080] By adding the acrylic multilayer structure polymer particles (b1) and the acrylic multilayer structure polymer (b2) according to the present invention to a mixing step of a methacrylic resin (A) and a block copolymer (c) and kneading them, it is possible to obtain a methacrylic resin composition for producing a methacrylic melt extrusion molded product having excellent transparency, surface smoothness, resistance to whitening upon bending, surface hardness, bending property and slipperiness.

[0081] The order of mixing the methacrylic resin (A) and the multilayered polymer particles (b1), and the order of mixing the multilayered polymer particles (b2) and the block copolymer (c) may be selected in any order.

[0082] The kneading method can be a known method, such as kneading using a batch kneader such as a Banbury mixer, a pressure kneader, or a Prabender Plastograph, or a continuous kneader such as a single-screw, twin-screw, or multi-screw extruder. Alternatively, a method may be used in which high-concentration master pellets are first prepared by the above method, and then the diluted pellets are melt-kneaded. From the viewpoint of productivity, a single-screw or twin-screw method is preferred. In particular, a single-screw extruder is preferred because it imparts less shear energy to the resin composition.

[0083] In the methacrylic resin composition of the present invention, the total amount of the multilayered polymer particles (b1), the multilayered polymer particles (b2) and the block copolymer (c) (total amount of the rubber-like elastomer (B)) is 15 to 55 mass%, preferably 20 to 50 mass%, and more preferably 25 to 45 mass%. If the total amount of the multilayered polymer particles (b1), the multilayered polymer particles (b2) and the block copolymer (c) is less than 15 mass%, the impact strength is deteriorated, and if it exceeds 55 mass%, the rigidity is deteriorated.

[0084] The content of the multilayered polymer particles (b2) is 0.1 to 7.5% by mass, more preferably 0.5 to 7.0% by mass, based on the methacrylic resin composition. If it is less than 0.1% by mass, slipping properties are not exhibited, and if it exceeds 7.5% by mass, the number of cracks caused by stress concentration around the multilayered polymer particles (b2) increases, causing stress whitening.

[0085] The content of the block copolymer (c) is 0.1% by mass or more and less than 5% by mass, more preferably 0.5 to 4.5% by mass, based on the methacrylic resin composition. If it is less than 0.1% by mass, bending resistance is not achieved, whereas if it is 5% by mass or more, the dispersed particle size of the block copolymer (c) becomes large, causing an increase in haze and whitening on bending.

[0086] In the methacrylic resin composition of the present invention, the content ratio of the acrylic polymer block (c2) to the total rubber content of the rubber component layer (b1-1) of the multilayered polymer particle (b1), the rubber component layer (b2-1) of the multilayered polymer particle (b2), and the acrylic polymer block (c2) is in the range of 1 to 25 mass%, preferably in the range of 3 to 23 mass%, and more preferably in the range of 5 to 20 mass%. When the content ratio of the acrylic polymer block (c2) to the rubber content is in the range of 1 to 25 mass%, a synergistic effect between the multilayered polymer particle and the block copolymer is produced, resulting in excellent impact resistance.

[0087] The methacrylic resin composition of the present invention may contain other polymers as necessary in addition to the methacrylic resin (A), the multilayered polymer particles (b1), the multilayered polymer particles (b2), and the block copolymer (c) within a range that does not impair the effects of the present invention. Examples of other polymers include olefin resins such as polyethylene, polypropylene, polybutene-1, poly-4-methylpentene-1, and polynorbornene; ethylene ionomers; styrene resins such as polystyrene, styrene-maleic anhydride copolymer, high impact polystyrene, AS resin, ABS resin, AES resin, AAS resin, ACS resin, and MBS resin; methyl methacrylate-styrene copolymer; ester resins such as polyethylene terephthalate and polybutylene terephthalate; amide resins such as nylon 6, nylon 66, and polyamide elastomer; polyphenylene sulfide, polyether ether ketone, Examples of the other thermoplastic resins include polysulfone, polyphenylene oxide, polyimide, polyetherimide, polycarbonate, polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyacetal, and phenoxy resins; thermosetting resins such as phenolic resins, melamine resins, silicone resins, and epoxy resins; polyurethane; modified polyphenylene ether; silicone modified resins; acrylic rubber, silicone rubber; styrene-based thermoplastic elastomers such as SEPS, SEBS, and SIS; and olefin-based rubbers such as IR, EPR, and EPDM. One or more of the other polymers can be used.

[0088] The methacrylic resin composition and molded article of the present invention may contain various additives as necessary. Examples of additives include antioxidants, heat deterioration inhibitors, ultraviolet absorbers, light stabilizers, lubricants, mold release agents, polymer processing aids, antistatic agents, flame retardants, dyes and pigments, matting agents, anti-sticking agents, impact resistance modifiers, and phosphors. The content of these additives can be appropriately set within a range that does not impair the effects of the present invention, and it is preferable that, for example, the content of the antioxidant is 0.01 to 1 part by mass, the content of the ultraviolet absorber is 0.01 to 3 parts by mass, the content of the light stabilizer is 0.01 to 3 parts by mass, the content of the lubricant is 0.01 to 3 parts by mass, the content of the dyes and pigments is 0.01 to 3 parts by mass, and the anti-sticking agent is 0.001 to 1 part by mass, relative to 100 parts by mass of the methacrylic resin composition. Other additives can also be added in the range of 0.01 to 3 parts by mass.

[0089] The antioxidant is effective in preventing the oxidation degradation of the resin by itself in the presence of oxygen. Examples of the antioxidant include phosphorus-based antioxidants, phenol-based antioxidants, sulfur-based antioxidants, and amine-based antioxidants. Among them, from the viewpoint of the effect of preventing the degradation of optical properties due to coloring, phosphorus-based antioxidants and phenol-based antioxidants are preferred, and it is more preferred to use a phenol-based antioxidant alone or in combination with a phosphorus-based antioxidant and a phenol-based antioxidant. When a phosphorus-based antioxidant and a phenol-based antioxidant are used in combination, it is preferred to use the phosphorus-based antioxidant / phenol-based antioxidant in a mass ratio of 0.2 / 1 to 2 / 1, and more preferably 0.5 / 1 to 1 / 1.

[0090] Preferred examples of the phosphorus-based antioxidant include 2,2-methylenebis(4,6-di-t-butylphenyl)octylphosphite (ADEKA CORPORATION, "ADEKA STAB HP-10"), tris(2,4-di-t-butylphenyl)phosphite (BASF Japan Ltd., "IRGAFOS168"), and 3,9-bis(2,6-di-t-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane (ADEKA CORPORATION, "ADEKA STAB PEP-36")).

[0091] Preferred phenol-based antioxidants include pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (BASF Japan Ltd., "IRGANOX1010") and octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate (BASF Japan Ltd., "IRGANOX1076"), etc.

[0092] As the sulfur-based antioxidant, dilauryl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, pentaerythritol tetrakis(3-laurylthiopropionate), and the like are preferred.

[0093] As the amine-based antioxidant, octylated diphenylamine and the like are preferred.

[0094] The heat deterioration inhibitor can prevent the heat deterioration of the resin by capturing the polymer radicals generated when exposed to high temperatures under substantially oxygen-free conditions. Preferred heat deterioration inhibitors include 2-t-butyl-6-(3'-t-butyl-5'-methyl-hydroxybenzyl)-4-methylphenyl acrylate (Sumitomo Chemical Co., Ltd.'s "Sumilizer GM") and 2,4-di-t-amyl-6-(3',5'-di-t-amyl-2'-hydroxy-α-methylbenzyl)phenyl acrylate (Sumitomo Chemical Co., Ltd.'s "Sumilizer GS"), etc.

[0095] The ultraviolet absorbent is a compound that has ultraviolet absorbing ability and is said to have the function of converting light energy into heat energy.The ultraviolet absorbent includes benzophenones, benzotriazoles, triazines, benzoates, salicylates, cyanoacrylates, oxalic acid anilides, malonic acid esters, and formamidines.Among them, benzotriazoles and triazines are preferred.The ultraviolet absorbent can be used alone or in combination of two or more kinds.

[0096] Benzotriazoles are highly effective in suppressing the deterioration of optical properties such as coloration caused by exposure to ultraviolet light, and are therefore suitable for use in optical applications of the methacrylic resin composition of the present invention. As benzotriazoles, 4-methyl-2-(2H-benzotriazol-2-yl)phenol (manufactured by Johoku Chemical Industry Co., Ltd. under the trade name JF-77), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (manufactured by BASF Japan Ltd. under the trade name TINUVIN329), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (manufactured by BASF Japan Ltd. under the trade name TINUVIN234), and 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-t-octylphenol] (manufactured by ADEKA Corporation under the trade name Adeka STAB LA-31) are preferred.

[0097] In addition, when it is desired to efficiently absorb wavelengths around 380 nm, triazine ultraviolet absorbers are preferably used. Examples of such ultraviolet absorbers include 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine (ADEKA CORPORATION's "ADEKA STAB LA-F70") and its analogue, hydroxyphenyltriazine ultraviolet absorbers (BASF Japan Ltd.'s "TINUVIN477" and "TINUVIN460"), etc.

[0098] A light stabilizer is a compound that is said to have the function of capturing radicals generated mainly by oxidation due to light. Suitable light stabilizers include hindered amines such as compounds having a 2,2,6,6-tetraalkylpiperidine skeleton. For example, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate ("Adeka STAB LA-77Y" manufactured by ADEKA CORPORATION) can be mentioned.

[0099] A lubricant is a compound that is said to have the effect of improving releasability and processability by adjusting the slip between the resin and the metal surface and preventing adhesion or sticking. Examples of lubricants include higher alcohols, hydrocarbons, fatty acids, fatty acid metal salts, aliphatic amides, and fatty acid esters. Among them, from the viewpoint of compatibility with the methacrylic resin composition of the present invention, aliphatic monohydric alcohols and aliphatic amides having 12 to 18 carbon atoms are preferred, and aliphatic amides are more preferred. Aliphatic amides are classified into saturated aliphatic amides and unsaturated aliphatic amides, and unsaturated aliphatic amides are more preferred because they are expected to have a slip effect due to anti-adhesion. Examples of unsaturated aliphatic amides include N,N'-ethylenebisoleic acid amide ("Slipax O" manufactured by Nippon Kasei Co., Ltd.) and N,N'-dioleyl adipic acid amide ("Slipax ZOA" manufactured by Nippon Kasei Co., Ltd.).

[0100] Examples of the release agent include higher alcohols such as cetyl alcohol and stearyl alcohol; and higher fatty acid esters of glycerin such as monoglyceride stearate and diglyceride stearate. In the present invention, it is preferable to use higher alcohols and glycerin fatty acid monoesters in combination as the release agent. When higher alcohols and glycerin fatty acid monoesters are used in combination, the ratio is not particularly limited, but the amount of higher alcohols used: the amount of glycerin fatty acid monoester used is preferably 2.5:1 to 3.5:1, more preferably 2.8:1 to 3.2:1, by mass ratio.

[0101] The polymer processing aid is a compound that is effective in achieving thickness accuracy and thinning when molding a methacrylic resin composition. The polymer processing aid is usually a polymer particle having a particle size of 0.05 to 0.5 μm, which can be produced by emulsion polymerization.

[0102] Examples of the antistatic agent include alkylsulfonates such as sodium heptyl sulfonate, sodium octyl sulfonate, sodium nonyl sulfonate, sodium decyl sulfonate, sodium dodecyl sulfonate, sodium cetyl sulfonate, sodium octadecyl sulfonate, sodium diheptyl sulfonate, potassium heptyl sulfonate, potassium octyl sulfonate, potassium nonyl sulfonate, potassium decyl sulfonate, potassium dodecyl sulfonate, potassium cetyl sulfonate, potassium octadecyl sulfonate, potassium diheptyl sulfonate, lithium heptyl sulfonate, lithium octyl sulfonate, lithium nonyl sulfonate, lithium decyl sulfonate, lithium dodecyl sulfonate, lithium cetyl sulfonate, lithium octadecyl sulfonate, and lithium diheptyl sulfonate.

[0103] Examples of the flame retardant include metal hydrates having a hydroxyl group or crystal water, such as magnesium hydroxide, aluminum hydroxide, hydrated aluminum silicate, hydrated magnesium silicate, and hydrotalcite; phosphate compounds, such as polyamine phosphoric acid esters; and silicon compounds. Of these, preferred are phosphate ester-based flame retardants, such as trimethyl phosphate, triethyl phosphate, tripropyl phosphate, tributyl phosphate, tripentyl phosphate, trihexyl phosphate, tricyclohexyl phosphate, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, dimethylethyl phosphate, methyl dibutyl phosphate, ethyl dipropyl phosphate, and hydroxyphenyl diphenyl phosphate.

[0104] Examples of dyes and pigments include red organic pigments such as para red, fire red, pyrazolone red, thioindigo red, and perylene red; blue organic pigments such as cyanine blue and indanthrene blue; and green organic pigments such as cyanine green and naphthol green. One or more of these may be used.

[0105] The matting agent includes glass particles, polysiloxane-based crosslinked particles, crosslinked polymer particles, mica, talc, calcium carbonate, barium sulfate, etc. The copolymer of the present invention preferably does not contain an acid generator.

[0106] Examples of the anti-sticking agent include fatty acids such as stearic acid and palmitic acid; fatty acid metal salts such as calcium stearate, zinc stearate, magnesium stearate, potassium palmitate, and sodium palmitate; waxes such as polyethylene wax, polypropylene wax, and montanic acid wax; low molecular weight polyolefins such as low molecular weight polyethylene and low molecular weight polypropylene; acrylic resin powder; polyorganosiloxane such as dimethylpolysiloxane; amide resin powders such as octadecylamine, alkyl phosphate, fatty acid ester, and ethylene bisstearylamide, fluororesin powders such as tetrafluoroethylene resin, molybdenum disulfide powder, silicone resin powder, silicone rubber powder, and silica.

[0107] Examples of fluorescent substances include fluorescent pigments, fluorescent dyes, fluorescent white dyes, fluorescent brighteners, and fluorescent bleaches.

[0108] When other polymers and / or additives are contained in the methacrylic resin composition of the present invention, they may be added during polymerization of the methacrylic resin (A) and / or the multilayer structure polymer particles (b1) and / or the multilayer structure polymer particles (b2) and / or the block copolymer (c), or they may be added during mixing with the methacrylic resin (A) and / or the multilayer structure polymer particles (b1) and / or the multilayer structure polymer particles (b2) and / or the block copolymer (c), or they may be added after mixing of the methacrylic resin (A) and / or the multilayer structure polymer particles (b1) and / or the multilayer structure polymer particles (b2) and / or the block copolymer (c).

[0109] The molded article containing the methacrylic resin composition of the present invention can be molded using a molding method and molding device generally used for thermoplastic polymers. For example, the molded article can be produced by a molding method involving heating and melting, such as injection molding, extrusion molding, compression molding, blow molding, calendar molding, and vacuum molding, or a solution casting method. Among these, the melt extrusion molding method is preferred in terms of controlling the dispersed phase of the block copolymer (c) of the present invention.

[0110] The molded article containing the methacrylic resin composition of the present invention is also useful as a film, and can be well processed by, for example, the inflation method or T-die extrusion method, which are common melt extrusion methods, or the calendar method, or further the solution casting method. If necessary, it is also possible to obtain a film with better surface properties by simultaneously contacting both sides of the film with a roll or a metal belt, particularly by simultaneously contacting with a roll or a metal belt heated to a temperature equal to or higher than the glass transition temperature. Depending on the purpose, it is also possible to modify the film by lamination molding or biaxial stretching. Among these, the T-die extrusion method is particularly preferred. The thickness of the film is preferably 20 to 200 μm, more preferably 30 to 100 μm.

[0111] In the film, the acrylic polymer block (c2) in the block copolymer (c) in the amount specified in the present invention is controlled to a specific dispersed phase, thereby improving the resistance to cracking due to bending. For example, in order to disperse into a columnar phase with a short major axis, the ratio Dr / Dt of the die lip opening (Dr) to the thickness (Dt) of the molded body in the T-die extrusion method is preferably in the range of 1≦Dr / Dt≦20, more preferably 3≦Dr / Dt≦10. If Dr / Dt is less than 1, the block copolymer (c) becomes a spherical phase with a large dispersed particle size, which whitens when stress is applied. On the other hand, if Dr / Dt exceeds 20, it becomes a columnar phase with a large major axis, which whitens when stress is applied, and the anisotropy becomes large.

[0112] When a T-die is used for production, the shear rate applied during die extrusion is preferably in the range of 200 to 650 / s, more preferably in the range of 300 to 550 / s. If the shear rate is less than 200 / s, the shear applied to the block copolymer is small, the dispersed particle size becomes large, and whitening occurs. On the other hand, if the shear rate exceeds 650 / s, the block copolymer is subjected to strong shear, the dispersed particle size becomes 1 nm or less, and the molded article does not exhibit flexibility.

[0113] Methacrylic resin molded products, particularly films, can be used by laminating them to metals, plastics, etc. Examples of lamination methods include wet lamination, in which an adhesive is applied to a metal plate such as a steel plate, and then a film is placed on the metal plate and dried to bond them together, dry lamination, extrusion lamination, hot melt lamination, etc.

[0114] Methods for laminating a film onto a plastic part include film insert molding, in which the film is placed in a mold and then filled with resin by injection molding, and laminate injection press molding, as well as film in-mold molding, in which the film is preformed, then placed in a mold and then filled with resin by injection molding.

[0115] The melt-extruded film containing the methacrylic resin composition of the present invention can be further laminated with a functional layer or a thermoplastic resin film to form a laminate film.

[0116] When the molded article of the present invention is a methacrylic melt-extruded film, the methacrylic melt-extruded film and a functional layer can be laminated to form a laminated film. The functional layer can be formed on one or both sides of the film. Examples of the functional layer include a hard coat layer, an antiglare layer, an antireflection layer, an antistatic layer, etc., and the film can include at least one of these layers.

[0117] When the methacrylic melt-extruded film containing the methacrylic resin composition of the present invention is a laminated film in which a functional layer and a film are laminated together, the thickness of the functional layer is preferably 0.1 to 20 μm, more preferably 1 to 10 μm, and the thickness of the laminated film is preferably 20 to 220 μm, more preferably 30 to 110 μm.

[0118] When the molded article of the present invention is a methacrylic melt-extruded film, the methacrylic melt-extruded film and a thermoplastic resin film can be laminated to form a laminated film. The thermoplastic resin film can be formed on one side or both sides of the methacrylic melt-extruded film. Examples of the thermoplastic resin of the thermoplastic resin film include various thermoplastic resins such as polyolefin (polyethylene, polypropylene, polymethylpentene, etc.), polystyrene, polycarbonate, polyvinyl chloride, methacrylic resin, nylon, polyethylene terephthalate, and copolymers having multiple types of monomer units constituting these thermoplastic resins. The thermoplastic resin film may contain only one type of thermoplastic resin, or two or more types of thermoplastic resins.

[0119] In the case of the laminated film of the present invention containing the methacrylic melt-extruded film and a thermoplastic resin film, the thickness of the thermoplastic resin film is preferably 20 to 200 μm, more preferably 30 to 100 μm, and the thickness of the methacrylic melt-extruded film is preferably 5 to 100 μm, more preferably 10 to 15 μm.

[0120] The methacrylic resin molded article containing the methacrylic resin composition of the present invention can be used as a member for various applications. Specific applications include, for example, signboard parts and marking films such as advertising towers, stand signs, side signs, transom signs, and rooftop signs; display parts such as showcases, partitions, and store displays; lighting parts such as fluorescent lamp covers, mood lighting covers, lampshades, light ceilings, light walls, and chandeliers; interior parts such as furniture, pendants, and mirrors; architectural parts such as doors, domes, safety window glass, partitions, staircase wainscoting, balcony wainscoting, and leisure building roofs; transportation-related parts such as aircraft windshields, pilot visors, motorcycle and motorboat windshields, bus visors, automobile side visors, rear visors, head wings, headlight covers, sunroofs, glazing, automobile interior parts, and automobile exterior parts such as bumpers; and audio-visual equipment. electronic equipment parts such as image nameplates, stereo covers, television protective masks, vending machines, mobile phones, and personal computers; medical equipment parts such as incubators and X-ray parts; equipment-related parts such as machine covers, instrument covers, laboratory equipment, rulers, dials, and observation windows; optical parts such as liquid crystal protection plates, light guide plates, light guide films, Fresnel lenses, lenticular lenses, front panels of various displays, and diffusion plates; traffic-related parts such as road signs, information boards, convex mirrors, and soundproof walls; and other materials used in greenhouses, large aquariums, box aquariums, bathroom components, clock panels, bathtubs, sanitary products, desk mats, game parts, toys, face protection masks during welding, back sheets for solar cells, and front sheets for flexible solar cells; and surface materials used in personal computers, mobile phones, furniture, vending machines, bathroom components, etc.

[0121] On the other hand, the methacrylic resin molded article of the present invention, particularly a laminated film, can be used for automobile interior and exterior materials, daily necessities, wallpaper, paint replacement applications, housings for furniture and electrical equipment, housings for office automation equipment such as facsimiles, flooring materials, parts for electrical or electronic devices, bathroom equipment, etc.

[0122] As described above, the methacrylic resin molded article of the present invention contains the methacrylic resin (A), the multilayered polymer particles (b1), the multilayered polymer particles (b2), and the block copolymer (c), and by controlling the dispersion state of these particles within a specific range, the methacrylic resin molded article has excellent transparency, surface smoothness, resistance to whitening due to bending, surface hardness, and flexibility, and is suitable for decorative applications and building material applications. EXAMPLES

[0123] Next, the effects of the present invention will be described with reference to examples and comparative examples. The present invention is not limited to the following examples. In the following description, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0124] The methacrylic resin molded article (film) made of the methacrylic resin composition of the present invention was evaluated by the following methods. [Number average particle diameter of rubber component layer (b1-1) and rubber component layer (b2-1)] Using the films (thickness 75 μm) produced in the examples and comparative examples described below, cross-sectional slices parallel to the extrusion direction were prepared with a thickness of 50 nm using an ultramicrotome (Leica EM UC7rt manufactured by JEOL Ltd.). The prepared slices were stained with a 10% aqueous solution of phosphotungstic acid, and the shape (morphology) of the stained parts was observed using an electron microscope (main body: JSM-7600F, detector: SM-74240RTED manufactured by JEOL Ltd.). The particle diameters of 30 stained parts were measured for each of the observed spherical stained parts, and the number average particle diameter of the rubber component layer (b1) was determined.

[0125] [Acetone insolubles] 2 g (mass of solid content before separation) of the formed film (thickness 75 μm) was placed in 50 mL of acetone and stirred at room temperature for 24 hours. The entire amount of the obtained liquid was centrifuged using a centrifuge (manufactured by Hitachi Koki Co., Ltd., CR20GIII) at a rotation speed of 20,000 rpm, a temperature of 0° C., and for 180 minutes. The supernatant liquid and the precipitate were separated and dried under vacuum at 50° C. for 8 hours to obtain an acetone-soluble fraction and an acetone-insoluble fraction. The mass of the obtained precipitate was measured, and the proportion of the acetone-insoluble fraction was calculated based on the following formula.

[0126]

number

[0127] [Haze] A resin film (thickness 75 μm) was cut into a size of 50 mm×50 mm to prepare a test piece, and the haze was measured at 23° C. in accordance with JIS K7105 and evaluated according to the following criteria. ◎: 0.5% or less 〇: 0.5%~1.0% ×: 1.0% or more

[0128] [Δ haze before and after heating] A resin film (thickness 75 μm) was cut into a size of 100 mm × 100 mm to prepare a test piece, which was then heated for 10 seconds in a tabletop molding machine set at 140° C. The haze of the sample immediately after heating was measured, and the difference from the haze value before heating was calculated as Δhaze, and the result was evaluated according to the following criteria. ○: 0.5% or less △: More than 0.5% and less than 1.0% ×: 1.0% or more

[0129] [Film surface hardness] The resin film (75 μm) was cut into a 10 cm×10 cm test piece, and the pencil hardness was measured in accordance with JIS-K5600-5-4 and evaluated according to the following criteria. 〇: HB or more ×:B or less

[0130] [Film crack resistance] A resin film (75 μm) was cut into a size of 12 cm × 1.5 cm to prepare a test piece, and the MIT flexion count was measured in accordance with JIS-P-8115 and evaluated according to the following criteria. ◎: > 100 ○: 40~100 ×:<40

[0131] [Slipperiness] The multilayer films obtained in the examples and comparative examples were cut into 50 mm x 50 mm test pieces. Two such test pieces were prepared, and the two test pieces were rubbed together by hand so that the thermoplastic resin layer of one test piece was in contact with the easy-slip layer of the other test piece, and the feel was evaluated as follows. If the evaluation criteria below are ◯ or higher, the test pieces can be used in practice. ◎: Slips without getting caught. ○: Slight grip but slippery. ×: No grip or slippage.

[0132] (Production example 1) Multilayer structure polymer particles (b1) 100 parts of ion-exchanged water was placed in a glass-lined reaction vessel equipped with a condenser, a thermometer, and a stirrer, and then 0.019 parts of a surfactant (polyoxyethylene alkyl ether sodium acetate (NIKKOL-ECT-3NEX)) and 0.10 parts of sodium carbonate were added and dissolved. The atmosphere in the reaction vessel was replaced with nitrogen gas to make it substantially oxygen-free. The reaction vessel was then heated to bring the aqueous solution to 80°C.

[0133] To the aqueous solution, 0.04 parts of potassium persulfate was added, and further, a mixture c consisting of 32.6 parts of methyl methacrylate, 2.1 parts of methyl acrylate, and 0.07 parts of allyl methacrylate was added continuously over 50 minutes. After the addition of the mixture c was completed, the mixture was held for 40 minutes and emulsion polymerization was carried out to obtain latex c.

[0134] Next, 0.05 parts of potassium persulfate was added to the latex c, and further, a mixture i consisting of 36.6 parts of butyl acrylate, 7.9 parts of styrene, and 0.89 parts of allyl methacrylate was added continuously over 60 minutes. After the addition of the mixture i was completed, the mixture was held for 90 minutes, and seed emulsion polymerization was carried out to obtain the latex i.

[0135] Next, 0.02 parts of potassium persulfate was added to this latex i, and further, a mixture o consisting of 18.6 parts of methyl methacrylate, 1.2 parts of methyl acrylate, and 0.04 parts of n-octyl mercaptan was added continuously over 30 minutes. After the addition of the mixture o was completed, the mixture was held for 60 minutes and seed emulsion polymerization was carried out to obtain latex I-1. After the latex I-1 was placed in a vessel equipped with a stirrer and mixed, an aqueous magnesium sulfate solution was added to cause salting out and coagulation. The coagulated product was washed with water, dehydrated, and dried to obtain multilayer structure polymer particles (b1). The physical properties of the multilayer structure polymer particles (b1) are shown in Table 1.

[0136] (Production example 2) Multilayer structure polymer particles (b2) 100 parts of ion-exchanged water was placed in a glass-lined reaction vessel equipped with a condenser, a thermometer, and a stirrer, and then 0.019 parts of a surfactant ("Pelex SS-H" manufactured by Kao Corporation) and 0.5 parts of sodium carbonate were added and dissolved. The atmosphere in the reaction vessel was replaced with nitrogen gas to make it substantially oxygen-free. The reaction vessel was then heated to bring the aqueous solution to 80°C.

[0137] To the aqueous solution, 0.02 parts of potassium persulfate was added, and further, a mixture c consisting of 9.4 parts of methyl methacrylate, 0.6 parts of methyl acrylate, and 0.02 parts of allyl methacrylate was added continuously over a period of 20 minutes. After the addition of the mixture c was completed, the mixture was held for 30 minutes and emulsion polymerization was carried out to obtain latex c.

[0138] Next, 0.07 parts of potassium persulfate was added to the latex c, and further, a mixture i consisting of 41.1 parts of butyl acrylate, 8.9 parts of styrene, and 2.0 parts of allyl methacrylate was added continuously over 80 minutes. After the addition of the mixture i was completed, the mixture was held for 60 minutes, and seed emulsion polymerization was carried out to obtain the latex i.

[0139] Next, a mixture o consisting of 37.6 parts of methyl methacrylate, 2.4 parts of methyl acrylate, and 0.12 parts of n-octyl mercaptan was added continuously to the latex i over a period of 60 minutes. After the addition of the mixture o was completed, the mixture was held for 60 minutes and seed emulsion polymerization was carried out to obtain latex I-2. After the latex I-2 was mixed in a vessel equipped with a stirrer, an aqueous magnesium sulfate solution was added to cause salting out and coagulation. The coagulated product was washed with water, dehydrated, and dried to obtain multilayer structure polymer particles (b2). The physical properties of the multilayer structure polymer particles (b2) are shown in Table 1.

[0140] [Table 1]

[0141] (Production Example 3) Methacrylic resin (A1) Methacrylic resin (A1): A methacrylic copolymer consisting of methyl methacrylate (MMA) units (content 99.3% by mass) and methyl acrylate (MA) units (content 0.7% by mass) with Mw=84,000 and Mw / Mn=2.1 was produced according to a conventional method.

[0142] (Production Example 4) Methacrylic resin (A2) Methacrylic resin (A2): A methacrylic copolymer consisting of methyl methacrylate (MMA) units (content 93.6% by mass) and methyl acrylate (MA) units (6.4% by mass) and having Mw=120,000 and Mw / Mn=2.1 was produced according to a conventional method.

[0143] (Production Example 5) Block copolymer (C1) Block copolymer (C1): A triblock copolymer consisting of [methyl methacrylate (MMA) polymer block (c1-1)]-[n-butyl acrylate (BA) polymer block (c2)]-[methyl methacrylate (MMA) polymer block (c1-2)], having a weight average molecular weight (Mw) of 70,000, a mass ratio of the polymer blocks (c1-1):(c2):(c1-2) of 14.3:50.0:35.7, and a total mass ratio of the monomers (MMA:BA)=(50:50) was produced according to a conventional method.

[0144] (Production Example 6) Block copolymer (C2) Block copolymer (C2): A triblock copolymer consisting of [methyl methacrylate (MMA) polymer block (c1-1)]-[n-butyl acrylate (BA) polymer block (c2)]-[methyl methacrylate (MMA) polymer block (c1-2)], having a weight average molecular weight (Mw) of 65,000, a total mass ratio of the polymer blocks (c1-1):(c2):(c1-2) of 15:70:15, and a mass ratio of each monomer (MMA:BA)=(30:70) was produced according to a conventional method.

[0145] (Production Example 7) Block copolymer (C3) Block copolymer (C3): A diblock copolymer consisting of [methyl methacrylate (MMA) polymer block (c1)]-[n-butyl acrylate (BA)) copolymer block (c2)], having a weight average molecular weight (Mw) of 120,000, a mass ratio of the polymer blocks (c1):(c2) of 50:50, a mass ratio of each monomer (MMA:BA)=(50:50), Mw(c1)=60,000, Mw(c2)=60,000, was produced according to a conventional method.

[0146] Example 1 56.2 parts of pellets of methacrylic resin (A2), 42.3 parts of pellets of multilayer structure polymer particles (b1), 0.5 parts of pellets of multilayer structure polymer particles (b2), and 1 part of pellets of block copolymer (C1) were kneaded using a twin-screw extruder and pelletized using a pelletizer to obtain a methacrylic resin composition (R1).

[0147] Using a single-screw vent extruder with a screw diameter of 50 mm and a T-die with a width of 500 mm and a lip opening of 0.8 mm, the methacrylic resin composition (R1) was melt-extruded at a discharge rate of 10 kg / h and a resin temperature of 260°C to obtain a film-like melt, which was then sandwiched between a first nip roll having a gap of 50 μm and consisting of a mirror-finished elastic metal roll whose temperature was adjusted to 85°C and a mirror-finished rigid metal roll whose temperature was adjusted to 90°C at a linear pressure of 30 kg / cm, and then sandwiched between a second nip roll having a gap of 50 μm and consisting of a mirror-finished rigid metal roll whose temperature was adjusted to 90°C and a mirror-finished rigid metal roll whose temperature was adjusted to 85°C at a linear pressure of 30 kg / cm to obtain a single-layer resin film (1) having a thickness of 75 μm. The number average particle diameters of the rubber component layers of the multilayered polymer particles measured by electron microscopy were b1: 0.09 μm and b2: 0.21 μm.

[0148] The evaluation results of the obtained resin film (1) are shown in Table 2. Although the resin film (1) was slightly inferior in crack resistance and slipperiness, it was excellent in transparency and surface hardness.

[0149] Example 2 A resin film (2) was obtained in the same manner as in Example 1, except that 56.2 parts of methacrylic resin (A1) was used instead of methacrylic resin (A2), and 37.8 parts of pellets of multilayer structure polymer particles (b), 2 parts of pellets of multilayer structure polymer particles (b2), and 4 parts of pellets of block copolymer (C1) were used. The evaluation results are shown in Table 2. The resin film (2) was excellent in transparency, surface hardness, crack resistance, and slipperiness.

[0150] Example 3 A resin film (3) was obtained in the same manner as in Example 1, except that the pellets of the methacrylic resin (A2) were changed to 56.2 parts, the pellets of the multilayer structure polymer particles (b1) to 37.8 parts, the pellets of the multilayer structure polymer particles (b2) to 2 parts, and the pellets of the block copolymer (C1) to 4 parts. The evaluation results are shown in Table 2. The resin film (3) was excellent in transparency, surface hardness, crack resistance, and slipperiness.

[0151] Example 4 A resin film (4) was obtained in the same manner as in Example 1, except that the pellets of the multilayered polymer particles (b1) were changed to 37.8 parts, the pellets of the multilayered polymer particles (b2) to 2 parts, and the pellets of the block copolymer (C2) to 4 parts, were changed. The evaluation results are shown in Table 2. The resin film (4) was excellent in transparency, surface hardness, crack resistance, and slipperiness.

[0152] Example 5 A resin film (5) was obtained in the same manner as in Example 1, except that the pellets of the multilayered polymer particles (b1) were changed to 37.8 parts, the pellets of the multilayered polymer particles (b2) to 2 parts, and the pellets of the block copolymer (C3) to 4 parts, were changed. The evaluation results are shown in Table 2. The resin film (5) was excellent in transparency, surface hardness, crack resistance, and slipperiness.

[0153] Example 6 A resin film (6) was obtained in the same manner as in Example 1, except that the pellets of the multilayered polymer particles (b1) were changed to 39.8 parts, the pellets of the multilayered polymer particles (b2) to 4.5 parts, and the pellets of the block copolymer (C1) to 4.5 parts. The evaluation results are shown in Table 2. The resin film (6) was excellent in transparency, surface hardness, crack resistance, and slipperiness.

[0154] Example 7 A resin film (7) was obtained in the same manner as in Example 1, except that the pellets of the methacrylic resin (A2) were changed to 64 parts, the pellets of the multilayer structure polymer particles (b1) to 30 parts, the pellets of the multilayer structure polymer particles (b2) to 2 parts, and the pellets of the block copolymer (C1) to 4 parts. The evaluation results are shown in Table 2. The resin film (7) was excellent in transparency, surface hardness, crack resistance, and slipperiness.

[0155] Example 8 A resin film (8) was obtained in the same manner as in Example 1, except that the pellets were changed to 70 parts of the methacrylic resin (A2), 24 parts of the multilayer structure polymer particles (b1), 2 parts of the multilayer structure polymer particles (b2), and 4 parts of the block copolymer (C1). The evaluation results are shown in Table 2. The resin film (8) was slightly inferior in crack resistance, but was excellent in transparency, surface hardness, and slipperiness.

[0156] Comparative Example 1 A resin film (9) was obtained in the same manner as in Example 1, except that the pellets of the multilayered polymer particles (b1) were changed to 39.75 parts, the pellets of the multilayered polymer particles (b2) to 0.05 parts, and the pellets of the block copolymer (C1) to 4 parts were changed to 4 parts. The evaluation results are shown in Table 2. The resin film (9) had decreased crack resistance and slipperiness.

[0157] Comparative Example 2 A resin film (10) was obtained in the same manner as in Example 1, except that the pellets of the multilayered polymer particles (b1) were changed to 31.8 parts, the pellets of the multilayered polymer particles (b2) to 8 parts, and the pellets of the block copolymer (C1) to 4 parts, were changed to 2. The evaluation results are shown in Table 2. The resin film (10) had a high haze and was whitened when bent.

[0158] Comparative Example 3 A resin film (11) was obtained in the same manner as in Example 1, except that the pellets of the multilayered polymer particles (b1) were changed to 41.75 parts, the pellets of the multilayered polymer particles (b2) to 2 parts, and the pellets of the block copolymer (C1) to 0.05 parts, were changed to 0.05 parts. The evaluation results are shown in Table 2. The resin film (11) was excellent in crack resistance and slipperiness, but the crack resistance was reduced.

[0159] Comparative Example 4 A resin film (12) was obtained in the same manner as in Example 1, except that the pellets of the multilayered polymer particles (b1) were changed to 33.8 parts, the pellets of the multilayered polymer particles (b2) to 2 parts, and the pellets of the block copolymer (C1) to 8 parts. The evaluation results are shown in Table 2. The pencil hardness of the resin film (12) was reduced.

[0160] Comparative Example 5 A resin film (13) was obtained in the same manner as in Example 1, except that the pellets of the methacrylic resin (A2) were changed to 44 parts, the pellets of the multilayered polymer particles (b1) to 50 parts, the pellets of the multilayered polymer particles (b2) to 2 parts, and the pellets of the block copolymer (C1) to 4 parts. The evaluation results are shown in Table 2. The resin film (13) was excellent in crack resistance and slipperiness, but had a high haze and showed whitening when bent.

[0161] Comparative Example 6 A resin film (14) was obtained in the same manner as in Example 1, except that the pellets were changed to 79 parts of methacrylic resin (A2), 15 parts of multilayer structure polymer particles (b1), 2 parts of multilayer structure polymer particles (b2), and 4 parts of block copolymer (C1). The evaluation results are shown in Table 2. The crack resistance of the resin film (14) was reduced.

[0162] Comparative Example 7 A resin film (15) was obtained in the same manner as in Example 1, except that the pellets of the methacrylic resin (A2) were changed to 54.8 parts, the pellets of the multilayer structure polymer particles (b1) to 37.2 parts, the pellets of the multilayer structure polymer particles (b2) to 0 parts, and the pellets of the block copolymer (C2) to 8 parts were changed. The evaluation results are shown in Table 2. The resin film (15) exhibited reduced slippage and whitening upon bending.

[0163] Comparative Example 8 A resin film (16) was obtained in the same manner as in Example 1, except that the pellets of the methacrylic resin (A2) were changed to 52.8 parts, the pellets of the multilayer structure polymer particles (b1) to 37.2 parts, the pellets of the multilayer structure polymer particles (b2) to 10 parts, and the pellets of the block copolymer (C2) to 0 parts. The evaluation results are shown in Table 2. The resin film (16) was found to be whitened when folded.

[0164] [Table 2]

[0165] The above results demonstrate that the acrylic resin composition of the present invention is excellent in transparency, surface hardness, slipperiness, moldability and appearance after molding, and is suitable for decorative applications.

Claims

1. A methacrylic resin composition in which a methacrylic resin (A) forms a matrix and a rubber-like elastomer (B) is dispersed, the methacrylic resin composition having the following characteristics when the total of the methacrylic resin (A) and the rubber-like elastomer (B) is 100 mass%: (1) The rubber-like elastomer (B) contains multilayer structure polymer particles (b1), multilayer structure polymer particles (b2) and a block copolymer (c). (2) The multilayered polymer particle (b1) has at least one rubber component layer (core portion) (b1-1) and a hard resin component layer (b1-2) in the outermost portion (shell portion), the number average particle diameter of the rubber component layer closest to the shell portion is in the range of 0.05 μm or more and less than 0.16 μm, and the content of the multilayered polymer particle (b1) in the resin composition is more than 7.5 mass% and not more than 42.5 mass%. (3) The multilayered polymer particle (b2) has at least one rubber component layer (core portion) (b2-1) and a hard resin component layer (b2-2) in the outermost portion (shell portion), the number average particle diameter of the rubber component layer closest to the shell portion is in the range of 0.16 μm or more and 0.3 μm or less, and the content of the multilayered polymer particle (b2) in the resin composition is 0.1 mass % or more and 7.5 mass % or less. (4) The acetone insoluble content of the methacrylic resin composition is more than 20% by mass and not more than 45% by mass. (5) The block copolymer (c) contains a methacrylic polymer block (c1) and an acrylic polymer block (c2). (6) The content of the block copolymer (c) in the methacrylic resin composition is in the range of 0.1% by mass or more and 5.0% by mass or less. (7) The multilayered polymer particle (b1) has at least one rubber component layer (b1-1) between an innermost layer and an outermost layer, the rubber component layer (b1-1) being made of a copolymer containing 50 to 98.99% by mass of an acrylic acid ester monomer unit, 1 to 44.99% by mass of other monofunctional monomer units, and 0.01 to 10% by mass of a polyfunctional monomer, and the innermost layer and the outermost layer are at least one hard resin component layer (b1-2) containing 40 to 100% by mass of a methacrylic acid ester monomer unit and 60 to 0% by mass of other monomer units. (8) The multilayered polymer particle (b2) has at least one rubber component layer (b2-1) between an innermost layer and an outermost layer, the rubber component layer (b2-1) being made of a copolymer containing 50 to 98.99% by mass of an acrylic acid ester monomer unit, 1 to 44.99% by mass of other monofunctional monomer units, and 0.01 to 10% by mass of a polyfunctional monomer, and the innermost layer and the outermost layer are at least one hard resin component layer (b2-2) containing 40 to 100% by mass of a methacrylic acid ester monomer unit and 60 to 0% by mass of other monomer units. (9) The total amount of the multilayered polymer particles (b1), the multilayered polymer particles (b2) and the block copolymer (c) is 25 to 45% by mass.

2. The methacrylic resin composition according to claim 1, characterized in that the block copolymer (c) comprises at least one methacrylic polymer block (c1) and at least one acrylic polymer block (c2), and the block copolymer (c) contains 30 to 60 mass% of the methacrylic polymer block (c1) and 70 to 40 mass% of the acrylic polymer block (c2).

3. A molded article comprising the methacrylic resin composition according to claim 1 or 2.

4. The molded article according to claim 3, which is a film.

5. A method for producing a film, comprising melt-extruding or solution-casting the methacrylic resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Film for floor material surfacing and floor material prepared by using same

    JP2000290397A

  • Laminating acrylic resin film and acrylic laminated molding using the same

    JP2001316557A

  • Styrene-based thermoplastic resin composition and molded article comprising the same

    JP2012062409A

  • Supporting structure for member, exposure apparatus, method for manufacturing flat panel display, and device manufacturing method

    JP2013051239A

  • Resin composition and production method therefor, molded body, film, and article

    WO2016157908A1