Manufacturing method of Sn particles
The method of forming an oxide film on a substrate and irradiating it with hydrogen radical-containing plasma allows for the efficient production of spherical Sn particles, addressing the complexity and inefficiency of conventional methods.
Patent Information
- Application Number
- JP2020115248
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-02
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-07-02
AI Technical Summary
Conventional methods for producing Sn particles are complex and inefficient, particularly in producing spherical Sn particles with a diameter of several μm.
A method involving the formation of an oxide film on a substrate, followed by irradiation with plasma containing hydrogen radicals to reduce the oxide film and generate spherical Sn particles, utilizing a floating wire plasma generation device to stabilize plasma irradiation.
Enables the easy and efficient production of spherical Sn particles with diameters ranging from 0.5 to 5 μm, facilitating easy detachment from the substrate.
Smart Images

Figure 0007562110000001 
Figure 0007562110000002 
Figure 0007562110000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing Sn particles using plasma. [Background technology]
[0002] Known conventional methods for producing metal particles include centrifugal atomization, dispersion methods using ultrasonic vibration or ultrasonic cavitation, etc. Patent Document 1 describes a method for producing Sn particles with a diameter of 1 to 10 μm by supplying a liquid metal composition that has been heated and melted into a solvent, irradiating the liquid metal composition with ultrasonic waves to generate droplets, transferring the solvent and the droplets to another location, further irradiating the droplets with ultrasonic waves to break them into fine droplets, and then cooling and solidifying the droplets. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-66789 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, conventional methods for producing Sn particles are complicated and not simple, and it has been particularly difficult to efficiently produce spherical Sn particles with a diameter of several micrometers.
[0005] Therefore, the present disclosure provides a method for easily producing Sn particles. [Means for solving the problem]
[0006] The present disclosure relates to a method for producing Sn particles made of spherical Sn, the method comprising the steps of forming an oxide film made of SnO2 on a substrate made of glass, and irradiating the oxide film with plasma containing hydrogen radicals to remove the oxide film from the substrate, thereby generating Sn particles on the substrate. Effect of the Invention
[0007] According to the present disclosure, spherical Sn particles can be easily produced. [Brief description of the drawings]
[0008] [Figure 1] 3 is a flowchart of a method for producing Sn particles according to an embodiment. [Diagram 2] A schematic diagram showing the mechanism by which Sn particles are generated. [Diagram 3] FIG. 1 is a diagram showing the configuration of a floating wire plasma generation device. [Figure 4] Photographs of the top surface and cross section of substrate 2. [Diagram 5] 1 is a graph showing the temperature dependence of the coverage of Sn particles in a region where Sn particles are present and the average diameter of the Sn particles on the temperature of substrate 2. [Figure 6] 1 is a graph showing the temperature dependence of the rate of increase in the area where Sn particles are generated on the substrate 2. [Figure 7] Graph showing the relationship between plasma exposure time and the area where Sn particles are generated. [Figure 8] Photographs of Sn particles taken at each irradiation time. [Figure 9] Photographs of the top surface of substrate 2 taken at furnace pressures of 0.1 atm and 0.7 atm. [Figure 10] A photograph of the top surface of substrate 2 when irradiated with a mixture of hydrogen and argon gas instead of plasma. [Figure 11] Photographs of the top surface of board 2 before and after wiping. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] 1 is a diagram showing a flow chart of steps in the method for producing Sn particles according to the present embodiment. Hereinafter, the method for producing Sn particles according to the present embodiment will be described with reference to FIG.
[0010] First, an oxide film 1 made of SnO2 is formed on a substrate 2 made of glass (Step S1 in FIG. 1). The oxide film 1 is formed on the substrate 2 by, for example, sputtering, vapor deposition or the like.
[0011] In the method for producing Sn particles according to the present embodiment, the diameter of the Sn particles can be controlled by the thickness of the oxide film 1. Here, the diameter of the Sn particles is defined as the diameter of a circumscribed sphere. The diameter of the Sn particles can be 0.1 to 10 times the thickness of the oxide film 1, and can be larger than the thickness of the oxide film 1. The thickness of the oxide film 1 is preferably 10 nm to 10 μm. Within this range, Sn particles can be efficiently produced. For example, it is 500 nm. It is more preferably 50 nm to 5 μm, and further preferably 100 nm to 1 μm.
[0012] The substrate 2 may be made of any material as long as it is glass. Since glass has poor wettability with Sn, the shape of the Sn particles can be made spherical. For example, quartz glass, soda glass, borosilicate glass, lead glass, etc. can be used.
[0013] Next, the oxide film 1 is irradiated with plasma made of a mixed gas of hydrogen and argon (step S2 in FIG. 1). The oxide film 1 is reduced by hydrogen radicals to become Sn, and when the oxide film 1 on the substrate 2 disappears, the Sn becomes spherical due to surface tension, and Sn particles are generated. The diameter of the Sn particles becomes larger than the thickness of the oxide film 1, and can be 2 to 10 times the thickness of the oxide film 1. For example, Sn particles with a diameter of 0.5 to 5 μm can be produced. Since the Sn particles are spherical, the contact area with the substrate 2 is very small. Therefore, the Sn particles can be easily peeled off from the substrate 2. For example, the Sn particles can be easily peeled off by applying a light physical force to the substrate 2, such as by applying a brush to the substrate 2 or wiping the substrate 2 with paper or cloth.
[0014] Any gas may be used for generating the plasma as long as it can generate plasma containing hydrogen radicals, but a mixed gas of hydrogen and a rare gas is preferred. This facilitates the generation of hydrogen radicals, and allows Sn particles to be produced efficiently. The rare gas is preferably argon. The hydrogen concentration in the mixed gas is preferably 0.001 to 10 vol%. By setting the hydrogen concentration within this range, hydrogen radicals can be generated efficiently. The hydrogen concentration is more preferably 0.05 to 1 vol%, and even more preferably 0.1 to 0.5 vol%.
[0015] During plasma irradiation, the substrate 2 may be heated. The diameter of the Sn particles can be controlled by controlling the temperature of the substrate 2, and the higher the temperature of the substrate 2, the larger the diameter of the Sn particles can be. Furthermore, the higher the temperature of the substrate 2, the wider the range in which Sn particles are generated in the substrate 2. The temperature of the substrate 2 is preferably 100 to 500°C. This is because if the temperature exceeds 500°C, the surface of the Sn particles may be etched by hydrogen radicals. Note that when the substrate 2 is irradiated with plasma without being heated, the temperature of the substrate 2 rises to about 100 to 160°C.
[0016] The pressure in the furnace in which the substrate 2 is placed may be normal pressure or reduced pressure. By irradiating plasma under reduced pressure, the time required for Sn particle generation can be shortened and the range of Sn particle generation on the substrate 2 can be expanded. This is believed to be because the reduced pressure lengthens the mean free path of hydrogen radicals, making it easier for the hydrogen radicals to reach the oxide film 1. The pressure is preferably 0.001 to 1 atm, more preferably 0.01 to 0.9 atm, and even more preferably 0.05 to 0.1 atm.
[0017] The plasma irradiation time can be any time as long as it is longer than the time when the oxide film 1 on the substrate 2 is removed. The longer the plasma irradiation time, the wider the region where Sn particles are generated. However, if the irradiation time is too long, the surface of the Sn particles may be etched, causing unevenness on the surface. The irradiation time also depends on the density of the hydrogen radicals, and the higher the density of the hydrogen radicals, the shorter the time can be. The irradiation time is, for example, 2 to 10 minutes.
[0018] In order to efficiently produce Sn particles, the following ranges are preferable for the plasma electron density, hydrogen radical density, and gas temperature. The plasma electron density is 1×10 14 ~1×10 15 cm -3 The density of hydrogen radicals is preferably 1×10 13 ~1×10 15 cm -3 The gas temperature is preferably 300 to 1000K.
[0019] The detailed mechanism by which Sn particles are generated is as follows. In the early stages of plasma irradiation, the oxide film 1 is reduced and etched by hydrogen radicals in the plasma, generating Sn and water. A large number of hemispherical liquid Sn (hereafter referred to as hemispheres 3) are generated in islands on the oxide film 1 (see Figure 2(a)). The water also evaporates and is removed from the substrate 2.
[0020] As etching continues, the oxide film 1 becomes thinner, the number of island-like hemispheres 3 increases, adjacent island-like hemispheres 3 merge, and the hemispheres 3 gradually become larger (see Figure 2(b)). In addition, the contact angle of the hemispheres 3 increases, and they become closer to a sphere.
[0021] When the oxide film 1 on the substrate 2 is completely reduced and disappears, the island-like hemispheres 3 change into spherical liquid Sn particles 4 due to surface tension (see Fig. 2(c)). Adjacent Sn particles 4 then coalesce to form larger Sn particles 4 (see Fig. 2(d)). When the distance between adjacent Sn particles 4 becomes sufficiently wide, the coalescence stops and the diameter of the Sn particle becomes constant.
[0022] As described above, according to the method for producing Sn particles of this embodiment, Sn particles can be produced simply and easily.
[0023] A floating wire plasma generating device is preferably used as the plasma generating device used in the Sn particle manufacturing method of this embodiment, because the floating wire plasma generating device can stably radiate high-density plasma over a wide range.
[0024] 3 is a diagram showing the configuration of a floating wire plasma generating apparatus. As shown in FIG. 3, the floating wire plasma generating apparatus is composed of a quartz tube 10, a floating wire 11, a coil 12, and a high frequency power supply 13.
[0025] As shown in FIG. 3, the quartz tube 10 is a tube made of quartz, with one end open and the other end closed. Gas for plasma generation is supplied into the tube from the opening of the quartz tube 10. The end opposite to the gas supply side is bent in two stages, and is composed of a main part 10A of a predetermined length from the opening on the gas supply side, a first bent part 10B connected to the rear of the main part 10A and bent at about 45° to the main part 10A, and a second bent part 10C connected to the rear of the first bent part 10B and bent at about 135°. The second bent part 10C forms an angle of about 90° with respect to the main part 10A. The length of the quartz tube 10 is 200 mm, and the outer diameter is 6 mm.
[0026] The second bent portion 10C has a slit 14 extending in the axial direction of the second bent portion 10C. The plasma generated inside the quartz tube 10 is extracted and radiated to the outside of the quartz tube 10 through the slit 14. The slit 14 is, for example, 2×20 mm.
[0027] The floating wire 11 is a metal wire disposed inside the quartz tube 10 and extending from the center of the main portion 10A to the slit in the second bent portion 10C. This floating wire 11 makes it possible to generate plasma with low power, and further allows the plasma generated in the center of the main portion 10A to stably extend to the slit 14. The material of the floating wire 11 is W (tungsten). The floating wire 11 has a diameter of 0.5 mm and a length of 170 mm.
[0028] The coil 12 is wound three times around the center of the main portion 10A of the quartz tube 10 along the outer wall of the quartz tube 10. The material of the coil 12 is, for example, Cu. The coil 12 is a hollow wire, and is cooled by running water through the tube.
[0029] The high frequency power supply 13 is connected to the coil 12 via a matching circuit (not shown). The high frequency power supply 13 is a 100 MHz high frequency power supply. The temperature, electron density, and hydrogen radical density of the plasma gas can be controlled by the power of the high frequency power supply 13.
[0030] In the floating wire plasma generator, a mixed gas of hydrogen and argon is flowed inside the quartz tube 10, and a high frequency voltage is applied to the coil 12 to generate an inductively coupled plasma inside the tube at the center of the main part 10A of the quartz tube 10. The plasma is guided to the slit 14 by the floating wire 11, and is radiated to the outside from the slit 14. In this way, the floating wire plasma generator of the first embodiment can stably irradiate the plasma over a wide area. EXAMPLES
[0031] Using a floating wire plasma generator, plasma was irradiated onto a substrate 2 made of quartz glass on which an oxide film 1 made of SnO2 was laminated, to produce Sn particles. The oxide film 1 was 500 nm. The gas used to generate the plasma was a mixed gas of hydrogen and argon, with a hydrogen concentration of 0.05 vol%. The gas flow rate was 6 slm. The power of the high-frequency power supply 13 was 150 W, and the plasma irradiation time was 5 minutes. The pressure inside the furnace was normal pressure. The substrate 2 was not heated.
[0032] Figure 4 shows the top and cross-sections of the substrate 2. Figure 4(a) shows the state before plasma irradiation. Before plasma irradiation, an oxide film 1 was formed on the substrate 2 with a thickness of 500 nm, and it was found that no Sn particles were present on the oxide film 1. Figure 4(b) shows the state at which the oxide film 1 was etched by about half after plasma irradiation. As shown in Figure 4(b), it was found that hemispherical Sn islands were formed on the oxide film 1. Figure 4(c) shows the state at which the oxide film 1 was completely etched. As shown in Figure 4(c), it was found that the island-shaped Sn became closer to a sphere. Figure 4(d) shows the state after 5 minutes of plasma irradiation. As shown in Figure 4(d), the Sn became almost spherical, with a diameter of approximately 2.3 μm. It was thus found that plasma irradiation can generate Sn particles.
[0033] Next, the plasma exposure time was set to 2 minutes, and the effect of varying the temperature of substrate 2 was investigated. Figure 5 is a graph showing the dependence of the Sn particle coverage in the region where Sn particles exist, and the average diameter of the Sn particles, on the temperature of substrate 2. As shown in Figure 5, it was found that the higher the temperature of substrate 2, the fewer the number of Sn particles and the larger their diameter. In addition, Figure 6 is a graph showing the dependence of the rate of increase in the area where Sn particles are generated, on the temperature of substrate 2. It was found that the higher the temperature of substrate 2, the more efficiently the oxide film 1 can be reduced in a short period of time, and the larger the area where Sn particles are generated.
[0034] Next, the effect of changing the plasma exposure time was investigated. Figure 7 is a graph showing the relationship between the plasma exposure time and the area where Sn particles were generated. The graph also shows photographs of the top surface of the substrate 2 taken at each exposure time. Also, Figure 8 is a photograph of the Sn particles taken at each exposure time. In the photograph of the top surface of the substrate 2 in Figure 7, the gray area surrounded by the black curved line is the area where Sn particles were generated. As shown in Figure 7, it was found that the longer the plasma exposure time, the larger the area where Sn particles were generated. In addition, the temperature of the substrate 2 rose slightly as the exposure time became longer. Also, as shown in Figure 8, the diameter of the Sn particles did not change much when the plasma exposure time was 2 minutes or more.
[0035] Next, the Sn particle generation area was compared when the furnace pressure was set to 0.1 atm and 0.7 atm. Figure 9 is a photograph of the upper surface of the substrate 2. In Figure 9, the gray area surrounded by the black curved line is the area where Sn particles were generated. As shown in Figure 9, when comparing at the same plasma exposure time, it was found that the Sn particle generation area was wider when the pressure was lower.
[0036] Next, instead of irradiating the plasma, the substrate 2 was irradiated with a mixed gas of hydrogen and argon. The temperature of the substrate 2 was set to 460°C. Figure 10 shows photographs of the top surface of the substrate 2, with Fig. 10(a) being before irradiation, Fig. 10(b) being 2 minutes after irradiation, and Fig. 10(c) being 20 minutes after irradiation. As shown in Fig. 10, almost no Sn particles were generated on the substrate 2. This revealed that hydrogen radicals are necessary for the generation of Sn particles.
[0037] Next, the surface of substrate 2 on which the Sn particles had been generated was wiped with a wet tissue, and the Sn particles on substrate 2 could be easily removed. Figure 11(a) is a photograph of the top surface of substrate 2 before wiping, and Figure 11(b) is a photograph after half of substrate 2 had been wiped with a wet tissue. As shown in Figure 11, before wiping, the surface of substrate 2 was gray with a whitish metallic luster and contained Sn particles, but after wiping, substrate 2 itself was exposed and transparent, indicating that the Sn particles had been removed. [Industrial Applicability]
[0038] The Sn particles produced according to the present disclosure can be used as a raw material for conductive materials such as conductive pastes. [Explanation of symbols]
[0039] 1: Oxide film 2: Substrate 3: Hemisphere 4: Sn particles 10:Quartz tube 10A: Main part 10B: Second bend 10C: Second folding section 10D: Slit 11: Floating wire 12: Coil 13:High frequency power supply 14: Slit
Claims
1. A method for producing Sn particles comprising producing spherical Sn particles, comprising the steps of: On a glass substrate, SnO 2 forming an oxide film comprising: a step of irradiating the oxide film with a plasma containing hydrogen radicals to remove the oxide film from the substrate and generate the Sn particles on the substrate; A method for producing Sn particles, comprising the steps of:
2. A method for producing Sn particles comprising producing spherical Sn particles, comprising the steps of: On a glass substrate, SnO 2 forming an oxide film consisting of the above by sputtering or vapor deposition; a step of irradiating the oxide film with a plasma containing hydrogen radicals to reduce and etch the oxide film, generating hemispherical Sn on the oxide film, combining the hemispherical Sn particles together, further reducing and etching the oxide film to remove the oxide film from the substrate, and bringing the hemispherical Sn particles into contact with the substrate to change the hemispherical Sn particles into spherical shapes due to surface tension, thereby generating the Sn particles on the substrate; A method for producing Sn particles, comprising the steps of:
3. 3. The method for producing Sn particles according to claim 1, wherein the plasma gas is a mixed gas of hydrogen and a rare gas.
4. 4. The method for producing Sn particles according to claim 3, wherein the concentration of hydrogen is 0.001 to 10 vol %.
5. The method for producing Sn particles according to any one of claims 1 to 4, characterized in that the diameter of the Sn particles is larger than the thickness of the oxide film.
6. The method for producing Sn particles according to claim 4, characterized in that the diameter of the Sn particles is 0.1 to 10 times the thickness of the oxide film.
7. The method for producing Sn particles according to any one of claims 1 to 6, characterized in that the substrate is heated during plasma irradiation.
8. The method for producing Sn particles according to any one of claims 1 to 7, characterized in that the temperature of the substrate is 100 to 500°C.
9. The method for producing Sn particles according to any one of claims 1 to 8, characterized in that the plasma irradiation is performed under reduced pressure.
10. The method for producing Sn particles according to any one of claims 1 to 8, characterized in that the plasma is irradiated at a pressure of 0.001 to 1 atm.
11. The density of hydrogen radicals in the plasma is 1×10 13 ~1×10 15 cm -3 The method for producing Sn particles according to any one of claims 1 to 10, characterized in that
12. The method for producing Sn particles according to any one of claims 1 to 11, characterized in that the plasma is generated and irradiated using a floating wire plasma generating device.
Citation Information
Patent Citations
Production of hyperfine metallic particles
JP1987070505A
Forming of ultrafine particle construction
JP2000133794A
Production method of particulate
JP2005097684A
Inductively-coupled micro plasma source having floating electrode
JP2011249289A
Conductive substrate
JP2012104857A