Manufacturing method of thermoelectric conversion module

The method of thermal spraying an electrode bonding layer on magnesium antimony thermoelectric materials addresses the connectivity and performance issues, facilitating the assembly of thermoelectric conversion modules with improved bonding and thermoelectric performance.

JP7562115B2Active Publication Date: 2024-10-07TEX E G CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023039160
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-03-13
Publication Date
2024-10-07
Estimated Expiration
2043-03-13

AI Technical Summary

Technical Problem

Magnesium antimony thermoelectric materials are difficult to braze or plate, and their properties change at high temperatures, making it challenging to maintain thermoelectric performance and connect them effectively in thermoelectric conversion modules.

Method used

A method involving thermal spraying of an electrode bonding layer on the end surface of a sintered magnesium antimony-based thermoelectric material to facilitate bonding with electrodes, using metals like copper, nickel, or molybdenum, and assembling the thermoelectric elements with insulating substrates to form a thermoelectric conversion module.

Benefits of technology

Enables effective bonding and connection of magnesium antimony thermoelectric elements, simplifying the manufacturing process and maintaining thermoelectric performance across varying temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562115000001
    Figure 0007562115000001
  • Figure 0007562115000002
    Figure 0007562115000002
  • Figure 0007562115000003
    Figure 0007562115000003
Patent Text Reader

Abstract

To provide a novel manufacturing method for a thermoelectric conversion module equipped with a magnesium antimony-based thermoelectric element.SOLUTION: An electrode junction layer 320 for joining electrodes is formed by thermal spraying on the end faces of a sintered body 310 obtained by sintering a magnesium antimony-based thermoelectric material, and the sintered body 310 with an electrode junction layer 320 formed thereon is processed to form a thermoelectric element 110 having the electrode junction layer 320 on the end face, and electrodes for electrically connecting the thermoelectric elements to each other are joined to the electrode junction layer 320 of the obtained thermoelectric element 110.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a thermoelectric conversion module. [Background technology]

[0002] Thermoelectric conversion modules for thermoelectric power generation and electronic cooling have been known. Such thermoelectric conversion modules are generally composed of a plurality of thermoelectric elements (n-type semiconductor elements and p-type semiconductor elements), a plurality of metal electrodes for electrically connecting the plurality of thermoelectric elements, and a pair of insulating substrates (e.g., ceramic substrates) that sandwich the plurality of thermoelectric elements and the plurality of metal electrodes.

[0003] Meanwhile, magnesium antimony-based thermoelectric materials, whose main components are magnesium (Mg) and antimony (Sb), have been known for some time, and thermoelectric elements using magnesium antimony-based thermoelectric materials (magnesium antimony-based thermoelectric elements) are known to have relatively high thermoelectric performance (power generation performance) around room temperature.

[0004] However, magnesium (Mg), the raw material for magnesium antimony-based thermoelectric materials, is generally difficult to braze or plate, and joining to metal electrodes is an issue for magnesium antimony-based thermoelectric elements that contain such magnesium (Mg) as their main component.

[0005] In addition, it has been reported that MgAgSb-based thermoelectric materials, which are a type of magnesium antimony-based thermoelectric material, change in characteristics in the temperature range above 400°C and are unable to maintain their thermoelectric performance. For this reason, they generally cannot be used for brazing using filler metals with a melting point of 450°C or higher.

[0006] In addition, JP 2017-11109 A discloses a method for manufacturing a thermoelectric conversion module including a plurality of thermoelectric elements, a plurality of electrodes for electrically connecting the plurality of thermoelectric elements, and a pair of insulating substrates arranged to sandwich the plurality of thermoelectric elements and the plurality of electrodes, the method comprising: an electrode pattern forming process for forming a pattern for the electrodes on a surface of the insulating substrate using active metal solder; an assembly process for assembling the plurality of thermoelectric elements and the pair of insulating substrates on which the pattern for the electrodes is formed; and a brazing process for heating and brazing the thermoelectric conversion module assembled in the assembly process. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2017-11109 A Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a novel method for producing a thermoelectric conversion module including a magnesium antimony-based thermoelectric element. [Means for solving the problem]

[0009] The manufacturing method of a thermoelectric conversion module according to the present invention is a manufacturing method of a thermoelectric conversion module including a plurality of thermoelectric elements, a plurality of electrodes for electrically connecting the plurality of thermoelectric elements, and a pair of insulating substrates arranged to sandwich the plurality of thermoelectric elements and the plurality of electrodes, and is characterized by comprising an electrode junction layer forming step of forming an electrode junction layer by thermal spraying on an end face of a sintered body of a magnesium antimony-based thermoelectric material, an element forming step of obtaining a thermoelectric element having an electrode junction layer on an end face thereof from the sintered body on which the electrode junction layer has been formed, and a joining step of joining the electrode junction layer of the thermoelectric element obtained in the element forming step to the electrode.

[0010] In this case, the electrode junction layer may be formed by spraying a metal (for example, copper) in the electrode junction layer forming step. The electrode junction layer may have a thickness of about 100 to 200 μm.

[0011] In the above case, the method may further include an electrode formation process for forming the electrode on one side of the insulating substrate, and the joining process may join the electrode formed on the insulating substrate to an electrode joining layer of the thermoelectric element.

[0012] In this case, the method may further include an assembly process of assembling a plurality of thermoelectric elements having the electrode junction layers on both end surfaces and a pair of insulating substrates on which the electrodes are formed, and the joining process may simultaneously join the electrodes formed on the pair of insulating substrates to the electrode junction layers on both ends of the thermoelectric elements.

[0013] In the above cases, the sintered body may have a size that allows a plurality of thermoelectric elements to be cut out, and the element formation process may involve cutting the sintered body on which the electrode junction layer is formed to obtain a plurality of thermoelectric elements having the electrode junction layer on their end faces.

[0014] In the above case, the electrode junction layer forming step may include forming an electrode junction layer for each of the n-type sintered body made of an Mg3Sb2-based thermoelectric material and the p-type sintered body made of an MgAgSb-based thermoelectric material, and the element forming step may include obtaining an n-type thermoelectric element having an electrode junction layer on an end surface from the n-type sintered body on which the electrode junction layer is formed, and obtaining a p-type thermoelectric element having an electrode junction layer on an end surface from the p-type sintered body on which the electrode junction layer is formed. Effect of the Invention

[0015] According to the present invention, a novel method for producing a thermoelectric conversion module including a magnesium antimony-based thermoelectric element can be provided. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a diagram for explaining a configuration example of a thermoelectric conversion module. [Diagram 2] FIG. 1 is a diagram (part 1) for explaining a method for producing a magnesium antimony-based thermoelectric element according to the present invention. [Diagram 3] FIG. 2 is a diagram (part 2) for explaining the method for producing a magnesium antimony-based thermoelectric element according to the present invention. [Figure 4] FIG. 1 is a diagram (part 1) for explaining a method for manufacturing a thermoelectric conversion module according to the present invention. [Diagram 5] FIG. 2 is a diagram (part 2) for explaining the manufacturing method of the thermoelectric conversion module according to the present invention. [Figure 6] FIG. 2 is a cross-sectional view for explaining the configuration of a sintering jig used in the sintering step of the embodiment. [Figure 7] FIG. 2 is a diagram showing an X-ray diffraction pattern of an n-type sintered body. [Figure 8] FIG. 2 is a diagram showing an X-ray diffraction pattern of a p-type sintered body. [Figure 9] FIG. 2 is a diagram for explaining the configuration of electrodes formed on an alumina substrate in an embodiment. [Figure 10] FIG. 4 is a diagram showing the measurement results of the voltage-current characteristics of Example 1. [Figure 11] FIG. 13 is a diagram showing the measurement results of the voltage-current characteristics of Example 2. [Figure 12] FIG. 13 is a diagram showing the measurement results of the voltage-current characteristics of Example 3. [Figure 13] 2 is a scanning electron microscope photograph (a photograph substituting a drawing) of a cross section of an n-type sintered body of Example 1. [Figure 14] 1 is a scanning electron microscope photograph (a photograph substituting a drawing) of a cross section of an n-type sintered body of Example 2. [Figure 15] 1 is a scanning electron microscope photograph (drawing substitute photograph) of a cross section of an n-type sintered body of Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.

[0018] The manufacturing method for a thermoelectric conversion module according to the present invention manufactures a thermoelectric conversion module equipped with a thermoelectric element (magnesium antimony-based thermoelectric element) constituted by a sintered body of a magnesium antimony-based thermoelectric material, and enables bonding between the thermoelectric element and the electrode by forming a layer (electrode bonding layer) on the end face of the thermoelectric element (sintered body) by thermal spraying to enable bonding with an electrode.

[0019] The magnesium antimony-based thermoelectric materials referred to here include both Mg3Sb2-based thermoelectric materials whose main components are magnesium (Mg) and antimony (Sb), and MgAgSb-based thermoelectric materials whose main components are magnesium (Mg), silver (Ag), and antimony (Sb).

[0020] First, the configuration of a thermoelectric conversion module manufactured by the manufacturing method according to the present invention will be described.

[0021] 1 is a diagram for explaining an example of the configuration of a thermoelectric conversion module manufactured by a manufacturing method according to the present invention, in which (a) is a plan view, (b) is a front view, and (c) is a right side view.

[0022] As shown in the figure, a thermoelectric conversion module 100 manufactured by the manufacturing method of the present invention comprises a plurality of thermoelectric elements 110 (111, 112), a plurality of electrodes 120 (121, 122) for electrically connecting the plurality of thermoelectric elements 110, and a pair of insulating substrates 131, 132 arranged to sandwich the plurality of thermoelectric elements 110 and the plurality of electrodes 120.

[0023] The thermoelectric conversion module 100 shown in the figure is used as a thermoelectric conversion module for thermoelectric power generation that generates an electromotive force due to the Seebeck effect when a temperature difference is applied between a pair of insulating substrates 131, 132, for example.

[0024] The multiple thermoelectric elements 110 are composed of multiple n-type thermoelectric elements (n-type semiconductor elements) 111 and multiple p-type thermoelectric elements (p-type semiconductor elements) 112, and multiple π-type thermoelectric elements are configured by electrically connecting one end of a pair of adjacent n-type thermoelectric elements 111 and p-type thermoelectric elements 112 with an electrode 121 on one side (the left side in FIG. 1C).The multiple π-type thermoelectric elements arranged in a plate shape are electrically connected in series and thermally in parallel with an electrode 122 on the other side (the right side in FIG. 1C).

[0025] In this embodiment, the n-type thermoelectric element 111 is made of a sintered body of a Mg3Sb2-based thermoelectric material, and the p-type thermoelectric element 112 is made of a sintered body of a MgAgSb-based thermoelectric material.

[0026] Moreover, an electrode junction layer (metal layer) having a predetermined thickness (for example, 100 to 200 μm) is formed on both end surfaces of the thermoelectric elements 111 and 112. Note that the electrode junction layer is omitted from the drawing.

[0027] The multiple electrodes 120 electrically connect the multiple thermoelectric elements 110 in series and are made of metal (nickel in this embodiment). In this embodiment, the multiple electrodes 120 are formed on the inner surfaces (surfaces facing the thermoelectric elements 110) of the pair of insulating substrates 131, 132 by electroless nickel plating.

[0028] The pair of insulating substrates 131, 132 are arranged to sandwich the multiple thermoelectric elements 110 and the multiple electrodes 120, and constitute the high-temperature surface (heating surface) and the low-temperature surface (heat dissipation surface) of the thermoelectric conversion module. In this embodiment, the insulating substrates 131, 132 are made of ceramics, more specifically, aluminum oxide (Al2O3). As described above, the multiple electrodes 120 are formed on the inner surfaces of the pair of insulating substrates 131, 132 by electroless nickel plating.

[0029] Next, a method for manufacturing the thermoelectric conversion module 100 having the above-mentioned configuration will be described.

[0030] First, a method for manufacturing the thermoelectric elements 110 included in the thermoelectric conversion module 100 will be described.

[0031] Figures 2 and 3 are diagrams for explaining the manufacturing method of a magnesium antimony-based thermoelectric element according to the present invention. Figure 2 is a flow chart for explaining the flow of the manufacturing process, and Figure 3 is a diagram for explaining the electrode junction layer forming process (spraying process) and the element forming process (machining process).

[0032] As shown in Fig. 2, first, the raw materials are weighed (S1). For example, when manufacturing an Mg3Sb2-based thermoelectric element, magnesium (Mg) powder and antimony (Sb) powder, which are the main raw materials, are weighed, and when manufacturing an MgAgSb-based thermoelectric element, magnesium (Mg) powder, silver (Ag) powder, and antimony (Sb) powder, which are the main raw materials, are weighed. When a dopant is added, the dopant is also weighed.

[0033] Next, the raw material powders are mixed so that the raw material powders weighed in the weighing step S1 become uniform (S2). For example, the raw material powders are mixed using a mixer or the like.

[0034] Next, the raw material powders uniformly mixed in the mixing step S2 are subjected to heat treatment to synthesize a magnesium antimony-based thermoelectric material (S3). For example, the raw material powders are placed in a semi-sealable container (e.g., a carbon container) and then placed in an electric furnace, and kept in an argon (Ar) atmosphere at a temperature of about 900°C for about 30 minutes in the case of Mg3Sb2-based thermoelectric materials, and for about 6 hours in the case of MgAgSb-based thermoelectric materials, to synthesize the magnesium antimony-based thermoelectric material.

[0035] Next, the magnesium antimony-based thermoelectric material synthesized in the synthesis step S3 is pulverized (S4) to a desired particle size (for example, 90 μm or less) using, for example, an automatic mortar or a ball mill.

[0036] Next, the magnesium antimony based thermoelectric material pulverized in the pulverization step S4 is sintered (S5). In this embodiment, pressure sintering is performed by spark plasma sintering (SPS). For example, -5 Pressure sintering is performed by SPS under conditions of approximately 50 MPa sintering pressure, approximately 850°C sintering temperature, and approximately 10 minutes for Mg3Sb2-based thermoelectric materials, and approximately 50 MPa sintering pressure, approximately 450°C sintering temperature, and approximately 10 minutes for MgAgSb-based thermoelectric materials.

[0037] Next, an electrode junction layer for joining electrodes is formed by thermal spraying on the end faces (surfaces to which electrodes are joined) of the sintered body obtained in the sintering step S5 (S6). For example, as shown in Fig. 3(a), a metal (e.g., copper, nickel, molybdenum, etc.) is thermally sprayed on both end faces (top and bottom) of the sintered body 310 by a flame spraying method to form an electrode junction layer (metal layer) 320 having a thickness of about 100 to 200 µm.

[0038] Next, the sintered body having the electrode junction layer formed on its end surface in the electrode junction layer forming step S6 is processed to form a thermoelectric element having a desired shape (S7). For example, as shown in Fig. 3(b), the sintered body 310 having the electrode junction layer 320 formed thereon is cut by a cutting device such as a wire cutter to form a plurality of rectangular parallelepiped elements 330. At this time, the cutting process is performed so that each thermoelectric element 330 has the electrode junction layer 320 on both end surfaces.

[0039] In the manner described above, the thermoelectric elements used in the method for manufacturing a thermoelectric conversion module according to the present invention are manufactured. Note that the above steps S1 to S7 are performed for each of the n-type thermoelectric elements and the p-type thermoelectric elements.

[0040] Next, a method for producing a thermoelectric conversion module using the thermoelectric element produced as described above will be described.

[0041] 4 and 5 are diagrams for explaining a method for manufacturing a thermoelectric conversion module according to the present invention, in which Fig. 4(a) and Fig. 5(a) show plan views, and Fig. 4(b) and Fig. 5(b) show front views.

[0042] First, a pair of insulating substrates 131, 132 constituting the high-temperature surface and the low-temperature surface of the thermoelectric conversion module 100 are prepared, and electrodes 120 for electrically connecting the thermoelectric elements to each other are formed on one surface (the surface facing the thermoelectric element 110 when assembled) of each insulating substrate 131, 132 as shown in Fig. 4 (electrode formation process). The electrodes are formed, for example, by masking areas other than the electrode formation area and then performing electroless nickel plating.

[0043] Next, as shown in Fig. 5, a plurality of thermoelectric elements 330 having electrode junction layers 320 on both end surfaces are placed at predetermined positions on one insulating substrate 132 on which electrodes 120 are formed, and the other insulating substrate 131 on which electrodes 120 are formed is placed thereon as shown in Fig. 1, to assemble the thermoelectric conversion module 100 (assembly process). Note that, before placing each member, solder paste is applied to the contact surfaces between the thermoelectric elements 330 and the electrodes 120 (for example, the electrode portions to which the thermoelectric elements 330 are joined).

[0044] Next, in a state in which the thermoelectric conversion module 100 is assembled, the thermoelectric element and the electrodes are joined (joining process). In this embodiment, both ends (electrode joining layer 320) of the thermoelectric element 330 are joined to the upper and lower electrodes 120 simultaneously by reflow soldering.

[0045] Through the steps described above, the thermoelectric conversion module 100 as shown in FIG. 1 is manufactured.

[0046] As described above, in the manufacturing method of a thermoelectric conversion module according to the present invention, an electrode junction layer is formed on the end face of a magnesium antimony-based thermoelectric element by a thermal spraying method, so that the magnesium antimony-based thermoelectric element can be easily joined to the electrode.

[0047] Furthermore, in the above-described embodiment, a sintered body having a size from which a plurality of thermoelectric elements can be cut out is produced, and then an electrode junction layer is formed on an end face of the sintered body by a thermal spraying method, and then a plurality of thermoelectric elements are cut out. This makes it possible to easily form the electrode junction layer by thermal spraying.

[0048] In addition, in the above-described embodiment, an electrode is formed on one surface (the surface facing the thermoelectric element) of each of a pair of insulating substrates, and then the thermoelectric element and the electrode are joined together at once, thereby simplifying the manufacturing process.

[0049] Although the embodiments of the present invention have been described above, it is needless to say that the embodiments of the present invention are not limited to those described above. For example, in the above-mentioned embodiment, the magnesium antimony-based thermoelectric material is synthesized by heat treatment (liquid-solid reaction method) in the synthesis step S3, but it is also possible to perform synthesis by other synthesis methods, for example, solid-solid reaction method or mechanical alloying method.

[0050] In the above-described embodiment, pressure sintering is performed by spark plasma sintering (SPS) in the sintering step S5. However, it is also possible to perform other sintering methods, such as pressure sintering by hot pressing (HP) or hot isostatic pressing (HIP), or atmospheric sintering.

[0051] In the above-described embodiment, the electrodes are formed on the insulating substrate by electroless nickel plating, but it is also possible to use a strip-shaped metal plate as the electrodes.

[0052] Furthermore, in the above-described embodiment, the thermoelectric conversion module 100 is a thermoelectric conversion module for thermoelectric power generation, but the manufacturing method for a thermoelectric conversion module according to the present invention can also be used to manufacture a thermoelectric conversion module (Peltier module) for electronic cooling. EXAMPLES

[0053] Next, an embodiment of the method for manufacturing a thermoelectric conversion module according to the present invention will be described.

[0054] First, an n-type sintered body and a p-type sintered body made of a magnesium antimony-based thermoelectric material were prepared as follows.

[0055] <N-type sintered body> First, the composition of the feed is Mg 3.2 Sb 1.5 Bi 0.49 Te 0.01 Cu 0.01 Magnesium (Mg) powder (manufactured by High Purity Chemical Laboratory Co., Ltd.) with a purity of 99.5% and an average particle size of 180 μm, antimony (Sb) powder (manufactured by Shanghai Chung Fu Nam Technology Co., Ltd.) with a purity of 99.9% and an average particle size of 180 μm, bismuth (Bi) powder (manufactured by High Purity Chemical Laboratory Co., Ltd.) with a purity of 99.9% and an average particle size of 180 μm, tellurium (Te) powder (manufactured by High Purity Chemical Laboratory Co., Ltd.) with a purity of 99.9% and an average particle size of 45 μm, and copper (Cu) powder (manufactured by High Purity Chemical Laboratory Co., Ltd.) with a purity of 5 μm were weighed out so that the total weight was 46.744 g, specifically, Mg: 10 g, Sb: 23.5 g, Bi: 13 g, Te: 0.164 g, Cu: 0.08 g.

[0056] In this case, bismuth (Bi) and tellurium (Te) are added as dopants, and copper (Cu) is added as a component for improving characteristics.

[0057] Next, the raw material powders were mixed in a mortar until they were uniform. The uniformly mixed raw material powders were then placed in a semi-sealable carbon container with a lid, which was then placed in an electric furnace and kept at 900°C in an argon atmosphere for 30 minutes to obtain an Mg3Sb2-based thermoelectric material (ingot of Mg3Sb2 alloy).

[0058] Next, the obtained ingot was coarsely crushed in a mortar to a size of 1 mm or less, and then finely crushed in an automatic mortar (manufactured by Changzhou Zhongshi Sanshui Machinery Technology Co., Ltd., TYM120) to a particle size of 90 μm or less.

[0059] Next, the obtained Mg3Sb2-based thermoelectric material powder was filled into a sintering jig as shown in FIG.

[0060] More specifically, a carbon sheet (manufactured by NJS Co., Ltd.) having a thickness of 0.2 mm was cut into a predetermined shape to prepare a cylindrical carbon paper 621 and upper and lower disk-shaped carbon papers (30φ) 622, 623. Next, the cylindrical carbon paper 621 was placed in a carbon die 611 having a diameter of 30.4φ, and then the lower carbon punch 613 was inserted. Next, the lower disk-shaped carbon paper 623 was placed on the lower carbon punch 613, and then the Mg3Sb2-based thermoelectric material powder 601 was filled in. Next, the upper disk-shaped carbon paper 622 was placed on the Mg3Sb2-based thermoelectric material 601, and then the upper carbon punch 612 was inserted.

[0061] The sintering jig 600 prepared as described above was placed in a spark plasma sintering apparatus (LABOX-1575, manufactured by Sinterland Co., Ltd.) and sintered for 10 -5 Sintering was carried out in a vacuum of 10 Pa under conditions of a sintering temperature of 850°C, a sintering pressure of 50 MPa, and a sintering time of 10 minutes to obtain a disk-shaped (30φ, 3 mm thick) n-type sintered body.

[0062] {p-type sintered body} First, the composition of the mixture is MgAg 0.97 Sb 0.99 Magnesium (Mg) powder (manufactured by High Purity Chemical Laboratory Co., Ltd.) with a purity of 99.5% and an average particle size of 180 μm, silver (Ag) powder (manufactured by High Purity Chemical Laboratory Co., Ltd.) with a purity of 99.9% and an average particle size of 75 to 150 μm, and antimony (Sb) powder (manufactured by Shanghai Chung-Fu Nam Technology Co., Ltd.) with a purity of 99.9% and an average particle size of 180 μm were weighed out so that the total weight was 47.68 g, specifically, Mg: 4.64 g, Sb: 23.04 g, Ag: 20 g.

[0063] Next, the raw material powders were mixed in a mortar until they were uniform. The uniformly mixed raw material powders were then placed in a semi-sealable carbon container with a lid, which was then placed in an electric furnace and kept at 900°C for 6 hours in an argon atmosphere to obtain an MgAgSb-based thermoelectric material (ingot of MgAgSb alloy).

[0064] Next, the obtained ingot was coarsely crushed in a mortar to a size of 1 mm or less, and then finely crushed in an automatic mortar (manufactured by Changzhou Zhongshi Sanshui Machinery Technology Co., Ltd., TYM120) to a particle size of 90 μm or less.

[0065] Next, the obtained MgAgSb-based thermoelectric material powder was packed into a sintering jig in the same manner as in the case of the n-type sintered body described above, and then placed in a spark plasma sintering device (LABOX-1575, manufactured by Sinterland Co., Ltd.) and sintered for 10 -5 Sintering was carried out in a vacuum of 10 Pa under the conditions of a sintering temperature of 450°C, a sintering pressure of 50 MPa, and a sintering time of 10 minutes.

[0066] After that, the material was cooled to room temperature in the furnace, and then annealed in air at 300°C for 336 hours to change the crystal structure to a low-temperature phase with high thermoelectric properties. After that, the material was cooled in the furnace to obtain a disk-shaped (30φ, 3mm thick) p-type sintered body.

[0067] Next, the n-type sintered body and the p-type sintered body obtained as described above were subjected to XRD analysis using an X-ray diffractometer (MiniFlex, manufactured by Rigaku Corporation).

[0068] Figures 7 and 8 are diagrams showing the X-ray diffraction patterns of the n-type sintered body and the p-type sintered body, respectively. Note that Figure 7 also shows the X-ray diffraction pattern of Mg3Sb2 transcribed from the JCPDS card data, and Figure 8 also shows the X-ray diffraction pattern of α-MgAgSb transcribed from the JCPDS card data.

[0069] As shown in Figures 7 and 8, the peak positions of the n-type sintered body and the p-type sintered body roughly correspond to those in the JCPDS card data, and it was confirmed that the n-type sintered body and the p-type sintered body are roughly single phases of Mg3Sb2 and MgAgSb, respectively.

[0070] Next, n-type thermoelectric elements and p-type thermoelectric elements were produced using the n-type sintered body and the p-type sintered body obtained as described above, and then a thermoelectric conversion module including the n-type thermoelectric elements and the p-type thermoelectric elements was produced.

[0071] Specifically, multiple types of n-type thermoelectric elements and p-type thermoelectric elements composed of the above-mentioned n-type sintered body and p-type sintered body were produced by changing the material constituting the electrode junction layer, and then multiple types of thermoelectric conversion modules equipped with these n-type thermoelectric elements and p-type thermoelectric elements were produced as follows.

[0072] Example 1 First, copper (Cu) was sprayed onto both end faces (top and bottom) of each of the n-type sintered body and the p-type sintered body by a flame spraying method to form a copper layer (electrode contact layer) having a thickness of 100 μm.

[0073] Next, the n-type sintered body and the p-type sintered body having the copper layers formed on both end surfaces were cut using a wire saw (DWS3400, manufactured by Meiwa Force Systems Co., Ltd.) to cut out multiple rectangular sintered body pieces of 2.5 mm x 2.5 mm x 3 mm, which were used as n-type thermoelectric elements and p-type thermoelectric elements, respectively.

[0074] Next, a thermoelectric conversion module was produced using two each of the obtained n-type thermoelectric elements and p-type thermoelectric elements as described below.

[0075] First, an electrode having a thickness of 10 μm was formed by electroless nickel plating on one surface (the surface facing the thermoelectric element) of an alumina substrate (18 mm×20 mm×1 mm) serving as an insulating substrate.

[0076] 9 is a diagram for explaining the configuration of electrodes formed on an alumina substrate. In the figure, a two-dot chain line 901 indicates the position (thermoelectric element mounting position) where a thermoelectric element is mounted (joined).

[0077] As shown in the figure, electrodes 920 for electrically connecting the thermoelectric elements to each other were formed on one surface (the surface facing the thermoelectric element when assembled) of each of the alumina substrates 931 and 932. The electrodes were formed by masking areas other than the electrode formation area and then performing electroless nickel plating.

[0078] Next, solder paste (SN97C, manufactured by Nihon Superior Co., Ltd.) was applied to a predetermined position (thermoelectric element mounting position) on one of the alumina substrates on which the electrodes were formed, and the n-type thermoelectric element and p-type thermoelectric element were then mounted thereon.

[0079] Next, the alumina substrate on which the n-type and p-type thermoelectric elements were placed was placed on a hot plate and heated to 214°C. When this temperature was reached, heating was stopped, thereby bonding one end of each thermoelectric element (electrode bonding layer) to the electrode.

[0080] Subsequently, the other end of each thermoelectric element was joined to an electrode formed on the other alumina substrate in the same manner as above.

[0081] Finally, a copper lead wire was soldered to the electrode part, which serves as the output end, to complete the thermoelectric conversion module.

[0082] Example 2 First, nickel (Ni) was sprayed onto both end faces (top and bottom) of each of the n-type sintered body and the p-type sintered body by a flame spraying method to form a nickel layer (electrode contact layer) having a thickness of 100 μm.

[0083] Thereafter, a thermoelectric conversion module was produced in the same manner as in Example 1 described above.

[0084] Example 3 First, molybdenum (Mo) was sprayed onto both end faces (top and bottom) of each of the n-type sintered body and the p-type sintered body by a flame spraying method to form a molybdenum layer (electrode contact layer) having a thickness of 100 μm.

[0085] Thereafter, a thermoelectric conversion module was produced in the same manner as in Example 1 described above.

[0086] Next, each of the produced thermoelectric conversion modules was evaluated as follows.

[0087] First, a variable resistor was connected to each of the prepared thermoelectric conversion modules, and one side (the high-temperature side) of the thermoelectric conversion module was placed on a hot plate and heated to temperatures of 60, 100, and 150°C. The voltage-current characteristics (VI) were then measured using a nanovoltmeter while appropriately changing the resistance value of the variable resistor.

[0088] 10 to 12 are diagrams showing the measurement results of the voltage-current characteristics. FIG. 10 shows the measurement results of Example 1, FIG. 11 shows the measurement results of Example 2, and FIG. 12 shows the measurement results of Example 3. In each figure, a triangle (▲) indicates a measured value when the heating temperature was 60°C, a square (■) indicates a measured value when the heating temperature was 100°C, and a circle (●) indicates a measured value when the heating temperature was 150°C. In each figure, the power values ​​calculated from the measurement results are also plotted, and the temperature difference (ΔT), internal resistance (R), and maximum output power (P max )

[0089] 10 to 12, in a comparison of Examples 1 to 3, it was confirmed that the thermoelectric conversion module of Example 1 had the lowest internal resistance and good bonding. In other words, it was confirmed that the internal resistance of the electrode bonding layer is lower when it is made of copper than when it is made of nickel or molybdenum.

[0090] The maximum output power was also the largest in the thermoelectric conversion module of Example 1. That is, it was confirmed that the maximum output power was greater when the electrode junction layer was made of copper than when it was made of nickel or molybdenum.

[0091] In addition, in the process of producing each of the above thermoelectric conversion modules, the cross section (the boundary between the electrode junction layer and the sintered body) of each n-type sintered body on which the electrode junction layer was formed by thermal spraying was observed and subjected to elemental analysis using a scanning electron microscope (SEM) and an energy dispersive X-ray analyzer (EDX) (Hitachi High-Technologies Corporation, TM3030Plus).

[0092] 13 to 15 are scanning electron microscope photographs of the cross sections of the n-type sintered bodies of Examples 1 to 3, respectively.

[0093] As shown in FIGS. 13 to 15, in all of the n-type sintered bodies of Examples 1 to 3, it was confirmed that the electrode contact layer and the sintered body were well contacted.

[0094] In addition, according to the results of the EDX analysis, the concentration of each material element in the electrode contact layer at a position 20 μm toward the sintered body from the boundary between the electrode contact layer and the sintered body was 20% for copper in Example 1, 2% for nickel in Example 2, and 0% for molybdenum in Example 3, and it was confirmed that no more diffusion than necessary occurred for any of the materials.

[0095] Furthermore, a peeling test was carried out on the sintered body of Example 1 in which the material of the electrode contact layer was relatively most diffused.

[0096] Specifically, a peel test was performed in which the bottom surface of the sintered body was fixed to a lower tensile jig, and an upper tensile jig was fixed to the top surface of the electrode junction layer via an attachment, and the upper tensile jig was then pulled upward. As a result, the average peel strength for five tests was 11.6 MPa for the n-type sintered body and 11.7 MPa for the p-type sintered body, confirming that they had a strength of 10 MPa or more.

[0097] In this way, it was confirmed that the electrode contact layer (copper layer) of Example 1, in which the material of the electrode contact layer was relatively most diffused, also had sufficient contact strength.

[0098] From the above results, it was found that a thermoelectric conversion module including a magnesium antimony-based thermoelectric element having an electrode junction layer formed of copper exhibits high thermoelectric conversion performance and can be used satisfactorily. [Explanation of symbols]

[0099] 100 Thermoelectric conversion module 110 Thermoelectric element 111 n-type thermoelectric element 112 p-type thermoelectric element 120,121,122 electrode 131,132 Insulating substrate 310 Sintered body 320 Electrode bonding layer 330 Thermoelectric elements 600 Sintering fixture 601 Magnesium antimony based thermoelectric materials 611 Dice 612,613 punch 621 Cylindrical carbon paper 622,623 Carbon paper disc 901 Thermoelectric element placement position 920 electrode 931,932 Alumina substrate S1 Weighing process S2 mixing process S3 synthesis process S4 Grinding process S5 Sintering process S6 Electrode bonding layer formation process S7 Element formation process

Claims

1. A method for manufacturing a thermoelectric conversion module including a plurality of thermoelectric elements, a plurality of electrodes for electrically connecting the plurality of thermoelectric elements, and a pair of insulating substrates arranged to sandwich the plurality of thermoelectric elements and the plurality of electrodes, comprising: an electrode contact layer forming step of forming an electrode contact layer on an end surface of the sintered body of the magnesium antimony-based thermoelectric material by thermal spraying; an element forming step of obtaining a thermoelectric element having an electrode junction layer on an end surface from the sintered body on which the electrode junction layer is formed; a bonding step of bonding the electrode bonding layer of the thermoelectric element obtained in the element forming step to the electrode; Equipped with The electrode junction layer forming step forms the electrode junction layer by thermal spraying copper, The thickness of the electrode contact layer is 100 to 200 μm. A method for manufacturing a thermoelectric conversion module comprising the steps of:

2. The method further includes forming the electrode on one surface of the insulating substrate, The bonding step bonds an electrode formed on the insulating substrate to an electrode bonding layer of the thermoelectric element. The method for manufacturing a thermoelectric conversion module according to claim 1 .

3. The method further includes an assembly step of assembling a plurality of thermoelectric elements having the electrode junction layers on both end surfaces and a pair of insulating substrates on which the electrodes are formed, The bonding step simultaneously bonds electrodes formed on the pair of insulating substrates to electrode bonding layers on both ends of the thermoelectric element. The method for manufacturing a thermoelectric conversion module according to claim 2 .

4. The sintered body has a size that allows a plurality of thermoelectric elements to be cut out, The element forming step includes cutting the sintered body on which the electrode junction layer is formed to obtain a plurality of thermoelectric elements having the electrode junction layer on an end surface thereof. The method for manufacturing the thermoelectric conversion module according to any one of claims 1 to 3.

5. The electrode contact layer forming step includes: 3 Sb 2 forming an electrode junction layer on each of the n-type sintered body made of the MgAgSb-based thermoelectric material and the p-type sintered body made of the MgAgSb-based thermoelectric material; The element forming step obtains an n-type thermoelectric element having an electrode junction layer on an end surface from the n-type sintered body on which the electrode junction layer is formed, and obtains a p-type thermoelectric element having an electrode junction layer on an end surface from the p-type sintered body on which the electrode junction layer is formed. The method for manufacturing the thermoelectric conversion module according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Thermoelectric conversion module and its manufacturing method

    JP2005277120A

  • Thermoelectric power generation module and manufacturing method thereof

    JP2010157643A

  • Magnesium silicide, thermoelectric conversion material, sintered body, sintered body for thermoelectric conversion element, thermoelectric conversion element, and thermoelectric conversion module

    JP2013073960A

  • Thermoelectric conversion module and manufacturing method therefor

    JP2017011109A

  • Thermoelectric module and method for manufacturing thermoelectric module

    JP2022156629A