Organic electroluminescence device
By using multiple organic layers with distinct p-type dopants in OLEDs, the hole injection ability is better controlled, balancing carriers and enhancing device performance in terms of efficiency and longevity.
Patent Information
- Application Number
- JP2023105803
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-06-28
- Filing Date
- 2023-06-28
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2043-06-28
AI Technical Summary
Existing OLED devices face challenges in balancing hole and electron concentrations due to the limited adjustability of hole injection ability in single-layer hole injection layers, leading to unbalanced carrier concentrations that accelerate device aging and reduce efficiency.
Incorporating multiple organic layers with different p-type dopants having lower than -4.35 eV LUMO energy levels, allowing for enhanced control over hole injection and carrier balance through varying doping rates.
This approach improves the overall performance of OLED devices by extending service life and maintaining efficiency, as demonstrated by improved EQE and reduced voltage.
Smart Images

Figure 0007562176000032 
Figure 0007562176000033 
Figure 0007562176000034
Abstract
Description
[Technical field]
[0001] The present application relates to an organic electroluminescent device, more particularly to an organic electroluminescent device having at least two contacted organic layers containing a specific p-type dopant, and an electronic assembly including the organic electroluminescent device. [Background technology]
[0002] Organic electronic devices include, but are not limited to, organic light emitting diodes (OLEDs), organic field effect transistors (O-FETs), organic light emitting transistors (OLETs), organic photovoltaic cells (OPVs), dye-sensitized solar cells (DSSCs), organic photodetectors, organic photosensitive devices, organic field effect devices (OFQDs), light emitting electrochemical cells (LECs), organic laser diodes, and organic plasma light emitting devices.
[0003] Organic electroluminescent devices (OLEDs) are stacked with a cathode, an anode, and a series of organic layers between the cathode and the anode. By applying a voltage across the cathode and the anode of the device, electrical energy is converted into light, and the device has the advantages of a wide viewing angle, high contrast, and faster response time. In 1987, Tang and Van Slyke of Eastman Kodak reported an organic light-emitting device with an arylamine hole-transporting layer and a tris-8-hydroxyquinoline-aluminum layer as an electron-transporting layer and a light-emitting layer (Applied Physics Letters, 1987, 51(12):913-915). When a voltage is applied across the device, green light is emitted from the device. This invention laid the foundation for the development of modern organic light-emitting diodes (OLEDs). OLEDs are self-luminous solid-state devices, offering enormous potential for display and lighting applications. In addition, the inherent properties of organic materials, such as their flexibility, make them suitable for special applications, such as manufacturing flexible displays or lighting on flexible substrates. OLEDs have the advantages of low cost, low power consumption, high brightness, wide viewing angle, thin thickness, etc., and have been widely applied in the fields of display and lighting after decades of development.
[0004] OLED devices are generally composed of organic functional layers stacked in multiple layers, and in addition to the cathode, anode, and emitting layer (EML), they further include a hole transport region and an electron transport region. The hole transport region is located between the anode and the emitting layer, and generally includes functional layers such as a hole injection layer (HIL), a hole transport layer (HTL), and an electron blocking layer (EBL), while the electron transport region is located between the cathode and the emitting layer, and generally includes functional layers such as a hole blocking layer (HBL), an electron transport layer (ETL), and an electron injection layer (EIL). These functional layers may be provided in one or more layers selectively, or may not be present, as required. In the hole injection layer and the electron injection layer, holes and electrons are injected into the device from the anode terminal and the cathode terminal, respectively, and the two types of carriers transition to the emitting layer via the transport layer, and are combined in the emitting layer to form excitons, which emit light as they fall from the excited state to the ground state. The electron blocking layer and the hole blocking layer are usually selective layers. The hole injection layer may be a functional layer containing a single material or a functional layer containing multiple materials. The most common type of multiple materials is a hole transport material (HTM) doped with a certain percentage of a p-type dopant. The strong electron trapping ability of the p-type dopant can greatly increase the concentration of holes in the hole transport substrate by trapping electrons from the hole transport material to the p-type doped material. This allows the energy levels of the anode and the organic layer to match to form good hole injection and transport.
[0005] Effective combination of electrons and holes is an important factor that affects the luminescence quantum efficiency of a device. Currently, there are three main ways to improve the carrier balance of an OLED device. One is to balance the carrier concentration by using a suitable electron and hole injection material. The second is to improve the suitable electron and hole transport material to change the transport ability of the carrier in the organic transport material and achieve the balance. The third is to achieve the carrier balance by adjusting the transport performance of the host material and / or the light-emitting material in the light-emitting layer. Most of the hole transport materials (HTM) in existing OLED devices are arylamine-based compounds, which have strong electron supplying ability and can achieve good hole conduction. Assuming that the concentrations of electrons and holes injected from the cathode and anode are the same, due to the difference in the performance of the organic materials themselves, the hole mobility in the OLED structure is 1 to 3 orders of magnitude higher than the electron mobility, i.e., the hole concentration transported to the light-emitting layer is much larger than the electron concentration, resulting in an unbalanced carrier concentration and forming a hole-rich device. Carrier imbalance is likely to cause carriers to accumulate at the film layer boundary and generate heat, which not only accelerates the aging of the device and reduces its service life, but also reduces the exciton complex probability and reduces the efficiency of the device. Carriers can be balanced by improving the electron injection and transport performance, but the types of organic materials that can be selected are relatively small. Therefore, effectively reducing the number of holes that reach the light-emitting region is an effective way to improve the carrier balance and improve the performance of the device.
[0006] In OLEDs, the HIL generally adjusts and controls the hole injection ability by doping the HTM with an appropriate amount of p-type dopant to achieve ohmic contact between the anode and the HIL, thereby achieving a good hole injection effect. At present, a single-layer HIL is generally used in commercial structures, but there is a problem that the adjustment and control ability of the single-layer HIL for hole injection is very limited. If the concentration of the p-type doping material is low, the ohmic contact cannot be formed, and both the voltage and the service life of the device are affected. If the concentration of the p-type doping material is high, the ohmic contact can be ensured, but due to the injection of a large amount of holes, the concentration of holes in the light-emitting layer will accelerate to be greater than the concentration of electrons, which may cause carrier imbalance.
[0007] In order to balance electrons and holes in OLED, the prior art usually increases the thickness of the hole transport layer, so that electrons and holes can effectively combine in the organic layer within the same time, and do not cause hole accumulation.However, the increase in the thickness of the hole transport layer may bring about negative effects such as increased voltage, decreased efficiency, and thus shortened service life.
[0008] Patent CN100373656C discloses an organic light-emitting display device with a combination of a hole injection layer and a first hole transport layer. The hole injection layer uses a fluorocarbon compound, and the first hole transport layer uses a p-type dopant. The hole injection layer promotes hole injection, and the first hole transport layer containing a p-type dopant improves the structure of the device. The patent introduces a p-type doped first hole transport layer to reduce the voltage. However, the patent discloses a device containing only one p-type doped organic layer, but does not disclose a device containing p-type dopant in multiple organic layers, and does not disclose or teach the effect on the performance of the device when there are multiple organic layers containing p-type dopant.
[0009] In the prior art, some of the structures of devices in which the organic layers all contain p-type dopant are disclosed, but the organic layers all contain the same kind of p-type dopant material. For example, patent CN109216565B discloses an organic electroluminescence device. Its hole injection layer is composed of a first doping layer and a second doping layer, and the first doping layer is composed of a p-type dopant and is used to inject a large amount of holes. The second doping layer contains a p-type dopant and a hole transport material, and the doping rate is adjusted to adjust the amount of hole injection, thereby adjusting the balance between electrons and holes, and achieving the purpose of improving the service life of the device. The p-type dopants in the first doping layer and the second doping layer are the same kind of p-type dopant material. In addition, for example, patent application CN107112437A also discloses a similar device structure. The application discloses in the examples a device structure including two p-type doped organic layers, but the p-type dopants used are the same. In the above patent (application), the p-type dopants in the multiple p-type doped layers are all the same type of material, and the effect of the inclusion of different p-type dopants in the multiple organic layers on the performance of the device is not disclosed or taught.
[0010] In short, the prior art discloses some organic electroluminescence devices having multiple p-type doping layers, and the multiple p-type doping layers all contain the same type of p-type dopant material. However, when a single p-type dopant material is used in the device, the hole injection ability can only be adjusted by adjusting the doping rate of the p-type dopant, and generally, after the doping rate of the p-type dopant reaches a certain concentration, the hole injection cannot be continuously adjusted and controlled, so the adjustment and control ability of the single p-type dopant for the hole injection is relatively limited. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] CN100373656C [Patent Document 2] CN109216565B [Patent Document 3] CN107112437A [Non-patent literature]
[0012] [Non-Patent Document 1] (Applied Letter Physics, 1987, 51(12):913~915) Summary of the Invention [Problem to be solved by the invention]
[0013] In view of the above-mentioned problems, the present invention aims to provide a novel organic electroluminescent device, which comprises an anode, a cathode and an organic layer disposed between the anode and the cathode, the organic layer comprising a first organic layer and a second organic layer in direct contact with each other, the first organic layer containing a first p-type dopant, the second organic layer containing a second p-type dopant, the first p-type dopant and the second p-type dopant being different, and both of the LUMO energy levels being lower than -4.35 eV. By introducing at least two p-type doping layers in the organic electroluminescent device and using different p-type dopants in the two layers, the adjustment and control of the hole injection ability of the device can be improved, and more space can be provided for adjusting the hole injection ability of the device. For example, by selecting and combining different p-type dopants rationally, and further adjusting the concentration of p-type dopants in multiple p-doped layers, the hole injection ability can be better adjusted and controlled, carriers can be balanced, and the overall performance of the device can be improved. [Means for solving the problem]
[0014] According to one embodiment of the present invention, there is provided an organic electroluminescence device including an anode, a cathode, a first organic layer and a second organic layer disposed between the anode and the cathode, the first organic layer contains a first p-type dopant; the second organic layer contains a second p-type dopant; the first p-type dopant and the second p-type dopant are different; the LUMO energy levels of the first p-type dopant and the second p-type dopant are both less than −4.35 eV; An organic electroluminescent device is disclosed, wherein the first organic layer is in contact with a second organic layer.
[0015] According to an embodiment of the present invention, there is further disclosed an electronic assembly including the organic electroluminescent device described in the above embodiments.
[0016] The present invention aims to provide a novel organic electroluminescence device, which comprises an anode, a cathode and an organic layer disposed between the anode and the cathode, the organic layer comprising a first organic layer and a second organic layer in direct contact with each other, the first organic layer containing a first p-type dopant, the second organic layer containing a second p-type dopant, the first p-type dopant and the second p-type dopant being different, and both of the LUMO energy levels being lower than -4.35 eV. By introducing at least two p-type doping layers in the organic electroluminescence device and using different p-type dopants in the two layers, the adjustment and control of the hole injection ability of the device can be improved, more space can be provided for adjusting the hole injection ability of the device, and the overall performance of the device, especially the service life of the device, can be significantly improved. For example, by selecting and combining different p-type dopants rationally, and further adjusting the concentration of p-type dopants in multiple p-doped layers, the hole injection ability can be better adjusted and controlled, carriers can be balanced, and the overall performance of the device can be improved. [Brief description of the drawings]
[0017] [Figure 1] 1 is a schematic diagram of an organic light-emitting device 100. FIG. [Diagram 2] 2 is a schematic diagram of an organic light-emitting device 200. FIG. [Diagram 3] 1 is a schematic diagram of an organic electroluminescence element 300. FIG. [Figure 4] FIG. 4 is a schematic diagram of a laminated organic electroluminescence element 400. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] OLEDs can be fabricated on various substrates, such as glass, plastic, and metal. FIG. 1 shows an organic light-emitting device 100 by way of example and without limitation. The drawings are not necessarily drawn to scale, and some layer structures may be omitted in the drawings as necessary. The device 100 may include a substrate 101, an anode 110, a hole injection layer 120, a hole transport layer 130, an electron blocking layer 140 (optional layer), an emissive layer 150, a hole blocking layer 160 (optional layer), an electron transport layer 170, an electron injection layer 180, and a cathode 190. The device 100 may be fabricated by depositing the layers described in order. In some applications, the hole injection layer 120 and the hole transport layer 130 are collectively referred to as a hole transport layer, or a first hole transport layer, a second hole transport layer, but the two have a major difference in that the hole injection layer is usually in direct contact with the anode and has a smaller thickness than the hole transport layer. The properties, functions and exemplary materials of each layer are described in more detail in columns 6-10 of US Pat. No. 7,279,704 B2, the contents of which are incorporated herein in their entirety by reference.
[0019] There are many examples of each of these layers. Illustratively, in U.S. Patent Application Publication No. 5,844,363, which is incorporated herein by reference in its entirety, a flexible and transparent substrate-anode combination is disclosed. For example, in U.S. Patent Application Publication No. 2003 / 0230980, which is incorporated herein by reference in its entirety, an example of a p-doped hole transport layer is m-MTDATA doped with F4-TCNQ at a molar ratio of 1:50. An example of a host material is disclosed in U.S. Patent Application Publication No. 6,303,238 by Thompson et al., which is incorporated herein by reference in its entirety. For example, in U.S. Patent Application Publication No. 2003 / 0230980, which is incorporated herein by reference in its entirety, an example of an n-doped electron transport layer is BPhen doped with Li at a molar ratio of 1:1. Examples of cathodes are disclosed in U.S. Patent Nos. 5,703,436 and 5,707,745, which are incorporated by reference in their entirety, including composite cathodes having a thin metal layer, such as Mg:Ag, and a sputter-deposited transparent conductive ITO layer coated thereon. The principles and uses of blocking layers are described in more detail in U.S. Patent No. 6,097,147 and U.S. Patent Application Publication No. 2003 / 0230980, which are incorporated by reference in their entirety. Examples of injection layers are provided in U.S. Patent Application Publication No. 2004 / 0174116, which is incorporated by reference in its entirety. Protective layers are described in U.S. Patent Application Publication No. 2004 / 0174116, which is incorporated by reference in its entirety.
[0020] The above-mentioned split-layer structures are provided by way of non-limiting examples. The functions of the OLED can be realized by combining the various layers described above, or some layers can be omitted entirely. For example, the hole blocking layer is not a necessary layer and can be omitted in some structures. It may include other layers not explicitly described. Within each layer, a single material or a mixture of multiple materials can be used to achieve optimal performance. Any of the functional layers may include multiple sub-layers, for example, an emitting layer may have two layers of different emitting materials to achieve a desired emission spectrum.
[0021] In one embodiment, an OLED may be described as having an "organic layer" disposed between a cathode and an anode. The organic layer may include one or more layers.
[0022] An OLED also requires an encapsulation layer, and as shown in FIG. 2, an organic light-emitting device 200 is shown by way of example and not by way of limitation. The difference from FIG. 1 is that it may include an encapsulation layer 102 on the cathode 190 to prevent harmful substances from the outside, such as moisture and oxygen. Any material that can provide an encapsulation function, such as glass or an organic-inorganic mixed layer, may be used as the encapsulation layer. The encapsulation layer should be disposed directly or indirectly on the outside of the OLED element. A multi-layer thin-film encapsulation is described in U.S. Pat. No. US7968146B2, the entire contents of which are incorporated herein by reference.
[0023] Devices manufactured according to embodiments of the invention may be incorporated into a variety of consumer products having one or more electronic modules (or units) of the device, including, for example, flat panel displays, monitors, medical monitors, televisions, billboards, indoor or outdoor lighting and / or signaling lamps, heads-up displays, fully or partially transparent displays, flexible displays, smart phones, flat panel computers, flat panel mobile phones, wearable devices, smart watches, laptop computers, digital cameras, handheld video cameras, viewfinders, microdisplays, 3-D displays, in-vehicle displays, and tail lights.
[0024] The materials and structures described herein may also be used in the other organic electronic devices listed above.
[0025] Various OLED manufacturing methods are known. Small molecule OLEDs are generally manufactured by vacuum thermal evaporation. Polymer OLEDs are manufactured by solution processes, such as spin coating, inkjet printing, and nozzle printing. If the material can be dissolved or dispersed in a solvent, small molecule OLEDs can also be manufactured by solution processes. Each organic layer in the organic electroluminescent device according to the present application can be manufactured by deposition or solution processes. For example, the first organic layer and the second organic layer in the present application can be manufactured by deposition or solution processes as necessary.
[0026] In this specification, the energy levels of a compound (LUMO energy level: lowest unoccupied molecular orbital, HOMO energy level: highest occupied molecular orbital) are measured by cyclic voltammetry. For example, the compound HATCN measured by the test method of the present application [ka] The LUMO energy level of is -4.33 eV. In this specification, all "LUMO energy levels" and "HOMO energy levels" are expressed as negative values, and the smaller the numerical value (i.e., the larger the absolute value), the deeper the energy level. In this specification, a statement that an energy level is smaller than a certain value indicates that the energy level is numerically smaller than this value, i.e., has a more negative value. For example, the LUMO energy level of an organic material being -4.5 eV or less indicates that the LUMO energy level of the organic material is numerically -4.5 eV or more negative than -4.5 eV.
[0027] The term "doping ratio" refers to the percentage of one material of an organic layer to the total mass of the organic layer. For example, the doping ratio of the first p-type dopant in the first organic layer referred to in this application refers to the percentage of the first p-type dopant to the total mass of the first organic layer. When the first organic layer is composed of the first organic material and the first p-type dopant, the total mass of the first organic layer is the sum of the mass of the first organic material and the first p-type dopant.
[0028] When the first organic layer is composed only of the first p-type dopant, the doping rate of the first p-type dopant in the first organic layer is 100%. When the second organic layer is composed only of the second p-type dopant, the doping rate of the second p-type dopant in the second organic layer is 100%.
[0029] In this application, the term "same" or "different" materials refers to, for example, "a first p-type dopant and a second p-type dopant are different" and "a first organic material and a second organic material are the same or different." In this context, "same" refers to two or more materials having the same chemical structure, or the difference between the two or more materials is only that some or all of the hydrogens in the chemical structure are replaced with deuterium. Conversely, "different" refers to the chemical structure of the organic materials used being different (i.e., the difference between the chemical structure formulas is not only that some or all of the hydrogens in the molecular formula are replaced with deuterium).
[0030] In the present application, the organic layers being "different" means that if the organic layers are layers containing only a single material, the organic layers contain different materials. If the organic layers are composite materials / layers containing at least two materials, at least one of the materials contained in the organic layers is different, or the composite materials / layers formed by the organic layers are different (the materials in the composite materials / layers are different and / or the doping rates are different). The organic layers being "same" means that the materials in the organic layers are the same and the doping rates are also the same.
[0031] As used herein, the term "p-type dopant" refers to a dopant that has oxidizing ability, has strong electron-withdrawing ability, and is an electron acceptor. In this specification, it refers to a molecular type p-type dopant.
[0032] As used herein, the "molecular p-type dopant" refers to an organic compound consisting of 6 or more atoms in a dopant molecule. Preferably, the number of atoms forming the dopant molecule is greater than 10. More preferably, the number of atoms forming the dopant molecule is greater than 20. Preferably, the molar mass of the "molecular p-type organic dopant" is 200 g / mol to 2000 g / mol. Preferably, it is 300 g / mol to 1800 g / mol. More preferably, it is 400 g / mol to 1500 g / mol.
[0033] As used herein, "top" means furthest from the anode and "bottom" means closest to the anode. When a second layer is described as being "on" a first layer, the first layer is relatively close to the anode. Conversely, when a second layer is described as being "on" a first layer, the second layer is relatively close to the anode. Other layers may be present between the first layer and the second layer, unless it is specified that the first layer is "in contact with" the second layer. Illustratively, the cathode may still be described as being "on" the anode, even if there are various organic layers between the cathode and the anode.
[0034] As used herein, an "emitting unit" is an organic material layer that emits light by applying a voltage or current. One "emitting unit" includes at least one emitting layer. The emitting layer further contains a host material and a light-emitting material. The "emitting unit" further includes at least one pair of hole and electron injection / transport layers, such as a hole injection layer, a hole transport layer, an electron blocking layer, a hole blocking layer, an electron transport layer and an electron injection layer.
[0035] As used herein, a "charge generation layer (CGL)" is a layer for providing electrons and holes between two light-emitting units, and is composed of an n-type charge generation layer and a p-type charge generation layer. The n-type charge generation layer contacts the electron transport layer or electron injection layer of one light-emitting unit, and the p-type charge generation layer usually contacts the hole injection layer or hole transport layer of the adjacent light-emitting unit and provides holes to the latter. The p-type charge generation layer may be composed of a single material p-type dopant, or may be a composite layer in which a hole transport material is doped with a p-type dopant.
[0036] Definitions of Substituent Terminology
[0037] Halogen or halide, as used herein, includes fluorine, chlorine, bromine and iodine.
[0038] As used herein, alkyl groups include straight and branched chain alkyl groups. The alkyl groups may be alkyl groups having 1 to 20 carbon atoms, preferably alkyl groups having 1 to 12 carbon atoms, and more preferably alkyl groups having 1 to 6 carbon atoms. Examples of alkyl groups include methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-pentadecyl, n-hexadecyl, n-heptadecyl, n-octadecyl, neopentyl, 1-methylpentyl, 2-methylpentyl, 1-pentylhexyl, 1-butylpentyl, 1-heptyloctyl, and 3-methylpentyl. Of these, methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl and n-hexane are preferred. The alkyl group may be optionally substituted.
[0039] As used herein, the cycloalkyl group includes cyclic alkyl groups. The cycloalkyl group may be a cycloalkyl group having 3 to 20 ring carbon atoms, and is preferably a cycloalkyl group having 4 to 10 carbon atoms. Examples of the cycloalkyl group include cyclobutyl, cyclopentyl, cyclohexyl, 4-methylcyclohexyl, 4,4-dimethylcyclohexyl, 1-adamantyl, 2-adamantyl, 1-norbornyl group, and 2-norbornyl group. Of these, cyclopentyl, cyclohexyl, 4-methylcyclohexyl, and 4,4-dimethylcyclohexyl are preferred. The cycloalkyl group may be substituted.
[0040] As used herein, a heteroalkyl group is one in which one or more carbons in an alkyl chain are replaced with a heteroatom selected from the group consisting of a nitrogen atom, an oxygen atom, a sulfur atom, a selenium atom, a phosphorus atom, a silicon atom, a germanium atom, and a boron atom. The heteroalkyl group may be a heteroalkyl group having 1 to 20 carbon atoms, preferably a heteroalkyl group having 1 to 10 carbon atoms, and more preferably a heteroalkyl group having 1 to 6 carbon atoms. Illustrative examples of heteroalkyl groups are methoxymethyl, ethoxymethyl, ethoxyethyl, methylthiomethyl, ethylthiomethyl, ethylthioethyl, methoxymethoxymethyl, ethoxymethoxymethyl, ethoxyethoxyethyl, hydroxymethyl, hydroxyethyl, hydroxypropyl, mercaptomethyl, mercaptoethyl, mercaptopropyl, aminomethyl, aminoethyl, aminopropyl, dimethylaminomethyl, trimethylgermaniummethyl, trimethylgermaniumethyl, trimethylgermaniumisopropyl, dimethylethylgermaniummethyl, dimethylisopropylgermaniummethyl, tert-butyldimethylgermaniummethyl, triethylgermaniummethyl, triethylgermaniumethyl, triisopropylgermaniummethyl, triisopropylgermaniumethyl, trimethylsilylmethyl, trimethylsilylethyl, trimethylsilylisopropyl, trimethylsilylisopropyl, triisopropylsilylmethyl, and triisopropyloylsilylethyl. Heteroalkyl groups may also be substituted.
[0041] As used herein, alkenyl groups include linear, branched and cyclic olefin groups. The linear alkenyl group may be an alkenyl group having 2 to 20 carbon atoms, and is preferably an alkenyl group having 2 to 10 carbon atoms. Examples of alkenyl groups include vinyl, propylene, 1-butenyl, 2-butenyl, 3-butenyl, 1,3-butadienyl, 1-methylvinyl, styryl, 2,2-diphenylvinyl, 1,2-diphenylvinyl, 1-methylallyl, 1,1-dimethylallyl, 2-methylallyl, 1-phenylallyl, 2-phenylallyl, 3-phenylallyl, 3,3-diphenylallyl, 1,2-dimethylallyl, 1-phenyl-1-butenyl, 3-phenyl-1-butenyl, cyclopentenyl, cyclopentadienyl, cyclohexenyl, cycloheptenyl, cycloheptatrienyl, cyclooctenyl, cyclooctatetraenyl and norbornylalkenyl groups. The alkenyl group may be substituted.
[0042] As used herein, the term "alkynyl group" includes linear alkynyl groups. The alkynyl group may be an alkynyl group having 2 to 20 carbon atoms, and is preferably an alkynyl group having 2 to 10 carbon atoms. Examples of the alkynyl group include an ethynyl group, a propynyl group, a propargyl group, a 1-butynyl group, a 2-butynyl group, a 3-butynyl group, a 1-pentynyl group, a 2-pentynyl group, a 3,3-dimethyl-1-butynyl group, a 3-ethyl-3-methyl-1-pentynyl group, a 3,3-diisopropyl-1-pentynyl group, a phenylethynyl group, and a phenylpropynyl group. Among these, an ethynyl group, a propynyl group, a propargyl group, a 1-butynyl group, a 2-butynyl group, a 3-butynyl group, a 1-pentynyl group, and a phenylethynyl group are preferred. The alkynyl group may be substituted.
[0043] As used herein, aryl or aromatic groups contemplate non-condensed and condensed systems. The aryl group may be an aryl group having 6 to 30 carbon atoms, preferably an aryl group having 6 to 20 carbon atoms, and more preferably an aryl group having 6 to 12 carbon atoms. Examples of aryl groups include phenyl, biphenyl, terphenyl, triphenylene, tetraphenylene, naphthalene, anthracene, phenalene, phenanthrene, fluorene, pyrene, chrysene, perylene, and azulene, and are preferably phenyl, biphenyl, terphenyl, triphenylene, fluorene, and naphthalene. Examples of non-fused aryl groups include phenyl, biphenyl-2-yl, biphenyl-3-yl, biphenyl-4-yl, p-terphenyl-4-yl, p-terphenyl-3-yl, p-tribiphenyl-2-yl, m-terphenyl-4-yl, m-terphenyl-3-yl, m-terphenyl-2-yl, o-tolyl, m-tolyl, p-tolyl, p-(2-phenylpropyl)phenyl, 4'-methylbiphenyl, 4''-tert-butyl-p-terphenyl-4-yl, o-cumyl, m-cumyl, p-cumyl, 2,3-xylyl, 3,4-xylyl, 2,5-dimethylphenyl, mesitylene and m-tetraphenyl. The aryl group may also be substituted.
[0044] Heterocyclic group or heterocycle, as used herein, refers to a non-aromatic cyclic group. Non-aromatic heterocyclic groups include saturated heterocyclic groups having 3 to 20 ring atoms and unsaturated non-aromatic heterocyclic groups having 3 to 20 ring atoms, at least one ring atom of which is selected from the group consisting of nitrogen, oxygen, sulfur, selenium, silicon, phosphorus, germanium and boron atoms, and non-aromatic heterocyclic groups preferably have 3 to 7 ring atoms and contain at least one heteroatom such as nitrogen, oxygen, silicon or sulfur. Examples of non-aromatic heterocyclic groups include oxiranyl, oxetanyl, tetrahydrofuranyl, tetrahydropyranyl, dioxopentyl, dioxanyl, aziridinyl, dihydropyrrole, tetrahydropyrrolyl, piperidinyl, oxazolidinyl, morpholinyl, piperazinyl, oxacycloheptatrienyl, thiacycloheptatrienyl, azacycloheptatrienyl, and tetrahydrosilole. Heterocyclic groups may also be substituted.
[0045] Heteroaryl groups, as used herein, may include non-fused and fused heteroaromatic groups having 1 to 5 heteroatoms, at least one of which is selected from the group consisting of nitrogen, oxygen, sulfur, selenium, silicon, phosphorus, germanium, and boron. Isoaryl groups also refer to heteroaryl groups. Heteroaryl groups may be heteroaryl groups having 3 to 30 carbon atoms, preferably heteroaryl groups having 3 to 20 carbon atoms, and more preferably heteroaryl groups having 3 to 12 carbon atoms. Suitable heteroaryl groups are dibenzothiophene, dibenzofuran, dibenzoselenophene, furan, thiophene, benzofuran, benzothiophene, benzoselenophene, carbazole, indolocarbazole, pyridoindole, pyrrolopyridine, pyrazole, imidazole, triazole, oxazole, thiazole, oxadiazole, oxatriazole, dioxazole, thiadiazole, pyridine, pyridazine, pyrimidine, pyrazine, triazine, oxazine, oxathiazine, oxadiazine, indole, benzimidazole, indazole, indenoazine, benzoxazole, benzisoxazole, Heteroaryl groups include benzothiazole, quinoline, isoquinoline, cinnoline, quinazoline, quinoxaline, naphthyridine, phthalazine, pteridine, xanthene, acridine, phenazine, phenothiazine, benzofuranpyridine, frangipyridine, benzothienopyridine, thienobipyridine, benzoselenopyridine, and selenobenzopyridine, and preferably include dibenzothiophene, dibenzofuran, dibenzoselenophene, carbazole, indolocarbazole, imidazole, pyridine, triazine, benzimidazole, 1,2-azaborane, 1,3-azaborane, 1,4-azaborane, borazole, and their aza analogues. Heteroaryl groups may also be substituted.
[0046] As used herein, the alkoxy group is represented by -O-alkyl group, -O-cycloalkyl group, -O-heteroalkyl group, or -O-heterocyclic group. Examples and preferred examples of the alkyl group, cycloalkyl group, heteroalkyl group, and heterocyclic group are the same as those mentioned above. The alkoxy group may be an alkoxy group having 1 to 20 carbon atoms, and is preferably an alkoxy group having 1 to 6 carbon atoms. Examples of the alkoxy group include methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy, cyclopropyloxy, cyclobutyloxy, cyclopentyloxy, cyclohexyloxy, tetrahydrofuranyloxy, tetrahydropyranyloxy, methoxypropyloxy, ethoxyethyloxy, methoxymethyloxy, and ethoxymethyloxy. The alkoxy group may be substituted.
[0047] As used herein, the aryloxy group is represented by -O-aryl group or -O-heteroaryl group. Examples and preferred examples of the aryl group and the heteroaryl group are the same as those mentioned above. The aryloxy group may be an aryloxy group having 6 to 30 carbon atoms, and is preferably an aryloxy group having 6 to 20 carbon atoms. Examples of the aryloxy group include phenoxy and biphenoxy. The aryloxy group may be substituted.
[0048] As used herein, the term "aralkyl group" includes an alkyl group substituted with an aryl group. The aralkyl group may be an aralkyl group having 7 to 30 carbon atoms, preferably an aralkyl group having 7 to 20 carbon atoms, and more preferably an aralkyl group having 7 to 13 carbon atoms. Examples of the aralkyl group include benzyl, 1-phenylethyl, 2-phenylethyl, 1-phenylisopropyl, 2-phenylisopropyl, phenyl-tert-butyl, α-naphthylmethyl, 1-α-naphthylethyl, 2-α-naphthylethyl, 1-α-naphthylisopropyl, 2-α-naphthylisopropyl, β-naphthylmethyl, 1-β-naphthyl-ethyl, 2-β-naphthyl-ethyl, 1-β-naphthylisopropyl, 2-β-naphthylisopropyl, p-methylbenzyl, m-methylbenzyl, o-methylbenzyl, p-chlorobenzyl, m-chlorobenzyl, o ... Aralkyl groups include chlorobenzyl, o-chlorobenzyl, p-bromobenzyl, m-bromobenzyl, o-bromobenzyl, p-iodobenzyl, m-iodobenzyl, o-iodobenzyl, p-hydroxybenzyl, m-hydroxybenzyl, o-hydroxybenzyl, p-aminobenzyl, m-aminobenzyl, o-aminobenzyl, p-nitrobenzyl, m-nitrobenzyl, o-nitrobenzyl, p-cyanobenzyl, m-cyanobenzyl, o-cyanobenzyl, 1-hydroxy-2-phenylisopropyl and 1-chloro-2-phenylisopropyl. Among them, benzyl, p-cyanobenzyl, m-cyanobenzyl, o-cyanobenzyl, 1-phenylethyl, 2-phenylethyl, 1-phenylisopropyl and 2-phenylisopropyl are preferred. The aralkyl group may also be substituted.
[0049] As used herein, the term "alkylsilyl group" includes silyl groups substituted with an alkyl group. The alkylsilyl group may be an alkylsilyl group having 3 to 20 carbon atoms, and is preferably an alkylsilyl group having 3 to 10 carbon atoms. Examples of the alkylsilyl group include trimethylsilyl, triethylsilyl, methyldiethylsilyl, ethyldimethylsilyl, tripropylsilyl, tributylsilyl, triisopropylsilyl, methyldiisopropylsilyl, dimethylisopropylsilyl, tri-tert-butylsilyl, triisobutylsilyl, dimethyl-tert-butylsilyl, and methyldi-tert-butylsilyl. The alkylsilyl group may also be substituted.
[0050] As used herein, the term "arylsilyl group" includes a silyl group substituted with at least one aryl group. The arylsilyl group may be an arylsilyl group having 6 to 30 carbon atoms, and is preferably an arylsilyl group having 8 to 20 carbon atoms. Examples of the arylsilyl group include triphenylsilyl, phenyl dibiphenylsilyl, diphenyl biphenylsilyl, phenyl diethylsilyl, diphenyl ethylsilyl, phenyl dimethylsilyl, diphenyl methylsilyl, phenyl diisopropylsilyl, diphenyl isopropylsilyl, diphenyl butylsilyl, diphenyl isobutylsilyl, and diphenyl-tert-butylsilyl. The arylsilyl group may be substituted.
[0051] As used herein, the term "alkyl germanium group" includes a germanium group substituted with an alkyl group. The alkyl germanium group may be an alkyl germanium group having 3 to 20 carbon atoms, and is preferably an alkyl germanium group having 3 to 10 carbon atoms. Examples of the alkyl germanium group include a trimethyl germanium group, a triethyl germanium group, a methyldiethyl germanium group, an ethyldimethyl germanium group, a tripropyl germanium group, a tributyl germanium group, a triisopropyl germanium group, a methyldiisopropyl germanium group, a dimethylisopropyl germanium group, a tri-tert-butyl germanium group, a triisobutyl germanium group, a dimethyl-tert-butyl germanium group, and a methyldi-tert-butyl germanium group. The alkyl germanium group may be substituted.
[0052] As used herein, the term "arylgermanium group" includes a germanium group substituted with at least one aryl group or heteroaryl group. The arylgermanium group may be an aryl group germanium group having 6 to 30 carbon atoms, and is preferably an arylgermanium group having 8 to 20 carbon atoms. Examples of the arylgermanium group include a triphenylgermanium group, a phenyldibiphenylgermanium group, a diphenylbiphenylgermanium group, a phenyldiethylgermanium group, a diphenylethylgermanium group, a phenyldimethylgermanium group, a diphenylmethylgermanium group, a phenyldiisopropylgermanium group, a diphenylisopropylgermanium group, a diphenylbutylgermanium group, a diphenylisobutylgermanium group, and a diphenyl-tert-butylgermanium group. The arylgermanium group may also be substituted.
[0053] The "aza" in azadibenzofuran, azadibenzothiophene, etc. refers to the replacement of one or more CH groups in the corresponding aromatic fragment with a nitrogen atom. For example, azatriphenylene includes dibenzo[f,h]quinoxaline, dibenzo[f,h]quinoline, and other analogs having two or more nitrogens in the ring system. Those skilled in the art can easily imagine other nitrogen analogs of the above-mentioned aza derivatives, and all of these analogs are defined as being included in the terminology described herein.
[0054] In the present invention, unless otherwise specified, the following groups are included: a substituted alkyl group, a substituted cycloalkyl group, a substituted heteroalkyl group, a substituted heterocyclic group, a substituted aralkyl group, a substituted alkoxy group, a substituted aryloxy group, a substituted alkenyl group, a substituted alkynyl group, a substituted aryl group, a substituted heteroaryl group, a substituted alkylsilyl group, a substituted arylsilyl group, a substituted alkylgermanium group, a substituted arylgermanium group, a substituted amino group, a substituted acyl group, a substituted carbonyl group, a substituted carboxyl group, a substituted ester group, a substituted sulfur group, a substituted aryl ... When any of the terms from the group consisting of alkyl, cycloalkyl, heteroalkyl, heterocyclyl, aralkyl, alkoxy, aryloxy, alkenyl, alkynyl, aryl, heteroaryl, alkylsilyl, arylsilyl, alkylgermanium, arylgermanium, amino, acyl, carbonyl, carboxyl, ester, sulfinyl, sulfonyl, and phosphino groups is used, any one of the following groups is included: alkyl, cycloalkyl, heteroalkyl, heterocyclyl, aralkyl, alkoxy, aryloxy, alkenyl, alkynyl, aryl, heteroaryl, alkylsilyl, arylsilyl, alkylgermanium, arylgermanium, amino, acyl, carbonyl, carboxyl, ester, sulfinyl, sulfonyl, and phosphino. The group is selected from the group consisting of deuterium, halogen, an unsubstituted alkyl group having 1 to 20 carbon atoms, an unsubstituted cycloalkyl group having 3 to 20 ring carbon atoms, an unsubstituted heteroalkyl group having 1 to 20 carbon atoms, an unsubstituted heterocyclic group having 3 to 20 ring atoms, an unsubstituted aralkyl group having 7 to 30 carbon atoms, an unsubstituted alkoxy group having 1 to 20 carbon atoms, an unsubstituted aryloxy group having 6 to 30 carbon atoms, an unsubstituted alkenyl group having 2 to 20 carbon atoms, an unsubstituted alkynyl group having 2 to 20 carbon atoms, an unsubstituted aryl group having 6 to 30 carbon atoms, an unsubstituted heptyl group having 3 to 30 carbon atoms, an unsubstituted aryl ... It means that the aryl group may be substituted with one or more selected from a heteroaryl group, an unsubstituted alkylsilyl group having 3 to 20 carbon atoms, an unsubstituted arylsilyl group having 6 to 20 carbon atoms, an unsubstituted alkylgermanium group having 3 to 20 carbon atoms, an unsubstituted arylgermanium group having 6 to 20 carbon atoms, an unsubstituted amino group, acyl group, carbonyl group, carboxyl group, ester group, cyano group, isocyano group, hydroxyl group, mercapto group, sulfinyl group, sulfonyl group, phosphino group, and combinations thereof.
[0055] When describing a molecular fragment as being attached to another moiety by a substituent or otherwise, it should be understood that the designation can be defined as to whether it is a fragment (e.g., a phenyl group, a phenylene group, a naphthyl group, a dibenzofuranyl group) or an entire molecule (e.g., benzene, naphthalene, dibenzofuran). As used herein, the designations of the substituents or different modes of attachment of the fragment are recognized as equivalents.
[0056] In the compounds mentioned herein, hydrogen atoms may be partially or completely replaced by deuterium.Other atoms, such as carbon and nitrogen, may also be replaced by their other stable isotopes.In order to improve the efficiency and stability of the device, the replacement of other stable isotopes in the compounds may be preferred.
[0057] In the compounds referred to herein, multiple substitution refers to the range up to the most available substitution, including double substitution.When a substituent in a compound referred to herein means multiple substitution (including double substitution, triple substitution, quadruple substitution, etc.), it means that the substituent can be present at multiple available substitution positions on the bond structure, and the substituents present at multiple available substitution positions can be the same structure or different structures.
[0058] Unless otherwise specifically limited, adjacent substituents in the compounds mentioned herein may be bonded to form a ring, adjacent substituents in the compounds may not be bonded to form a ring. In the compounds mentioned herein, adjacent substituents may be bonded to form a ring, including not only the situation where adjacent substituents may be bonded to form a ring, but also the situation where adjacent substituents do not bond to form a ring. When adjacent substituents may be bonded to form a ring, the ring formed may be a monocyclic or polycyclic ring, and an alicyclic ring, a heteroalicyclic ring, an aryl ring, or a heteroaryl ring. In such a description, adjacent substituents may refer to substituents bonded to the same atom, substituents bonded to carbon atoms directly bonded to each other, or substituents bonded to carbon atoms further apart. Preferably, adjacent substituents refer to substituents bonded to the same carbon atom and substituents bonded to carbon atoms directly bonded to each other.
[0059] The statement that adjacent substituents may be bonded to form a ring is also understood to mean that two substituents bonded to the same carbon atom are bonded to each other by a chemical bond to form a ring, which can be exemplified by the following formula: [ka]
[0060] The statement that adjacent substituents may be bonded to form a ring is also understood to mean that two substituents bonded to carbon atoms that are directly bonded to each other are bonded to each other by a chemical bond to form a ring, which can be exemplified by the following formula: [ka]
[0061] The statement that adjacent substituents may be bonded to form a ring is also understood to mean that two substituents bonded to carbon atoms further apart are bonded to each other by a chemical bond to form a ring, which can be exemplified by the following formula: [ka]
[0062] In addition, the statement that adjacent substituents may be bonded to form a ring is also recognized as meaning that when one of the two substituents bonded to carbon atoms directly bonded to each other represents hydrogen, the second substituent is bonded to the position to which the hydrogen atom is bonded to form a ring. The following formula is an example. [ka]
[0063] According to one embodiment of the present invention, there is provided an organic electroluminescent device including an anode, a cathode, and a hole transport region disposed between the anode and the cathode, the hole transport region includes a first organic layer and a second organic layer; the first organic layer contains a first p-type dopant; the second organic layer contains a second p-type dopant; the first p-type dopant and the second p-type dopant are different; the LUMO energy levels of the first p-type dopant and the second p-type dopant are both less than −4.35 eV; An organic electroluminescent device is disclosed, wherein the first organic layer is in contact with a second organic layer.
[0064] According to an embodiment of the present invention, the sum of the thicknesses of the first and second organic layers is not greater than 100 nm.
[0065] According to an embodiment of the present invention, the sum of the thicknesses of the first and second organic layers is not greater than 50 nm.
[0066] According to an embodiment of the present invention, the sum of the thicknesses of the first and second organic layers is not greater than 30 nm.
[0067] According to an embodiment of the present invention, the sum of the thicknesses of the first and second organic layers is not greater than 20 nm.
[0068] According to an embodiment of the present invention, the first p-type dopant and the second p-type dopant are molecular type p-type dopants.
[0069] According to one embodiment of the present invention, the sum of the thicknesses of the first organic layer and the second organic layer is equal to or greater than 5 nm.
[0070] According to one embodiment of the present invention, the sum of the thicknesses of the first organic layer and the second organic layer is greater than or equal to 10 nm.
[0071] According to an embodiment of the present invention, the LUMO energy level of the first p-type dopant and / or the second p-type dopant is less than or equal to −4.4 eV.
[0072] According to an embodiment of the present invention, the LUMO energy level of the first p-type dopant and / or the second p-type dopant is less than or equal to -4.5 eV.
[0073] According to an embodiment of the present invention, the LUMO energy level of the first p-type dopant and / or the second p-type dopant is less than or equal to -4.6 eV.
[0074] According to an embodiment of the present invention, the LUMO energy level of the first p-type dopant and / or the second p-type dopant is less than or equal to -4.8 eV.
[0075] According to one embodiment of the present invention, the first organic layer is in contact with an anode.
[0076] According to an embodiment of the present invention, the doping rate of the first p-type dopant in the first organic layer is equal to or greater than the doping rate of the second p-type dopant in the second organic layer.
[0077] According to an embodiment of the present invention, the doping rate of the first p-type dopant in the first organic layer is smaller than the doping rate of the second p-type dopant in the second organic layer.
[0078] According to an embodiment of the present invention, the doping rate of the first p-type dopant in the first organic layer is ≧0.1% and ≦60%.
[0079] According to an embodiment of the present invention, the doping rate of the first p-type dopant in the first organic layer is ≧0.5% and ≦50%.
[0080] According to an embodiment of the present invention, the doping rate of the first p-type dopant in the first organic layer is ≧1% and ≦30%.
[0081] According to an embodiment of the present invention, the doping rate of the second p-type dopant in the second organic layer is ≧0.1% and ≦60%.
[0082] According to an embodiment of the present invention, the doping rate of the second p-type dopant in the second organic layer is ≧0.5% and ≦50%.
[0083] According to an embodiment of the present invention, the doping rate of the second p-type dopant in the second organic layer is ≧1% and ≦30%.
[0084] According to one embodiment of the present invention, the second organic layer is located above the first organic layer.
[0085] According to one embodiment of the present invention, the LUMO energy level of the first p-type dopant is greater than or equal to the LUMO energy level of the second p-type dopant.
[0086] According to one embodiment of the present invention, the LUMO energy level of the first p-type dopant is lower than or equal to the LUMO energy level of the second p-type dopant.
[0087] According to one embodiment of the present invention, the doping rate of the first p-type dopant in the first organic layer is less than or equal to the doping rate of the second p-type dopant in the second organic layer.
[0088] A lightly doped p-type dopant in the first organic layer (i.e., the bottom layer closer to the anode) can be used to control the number of hole injections, while a heavy p-type dopant in the second organic layer (i.e., the top layer closer to the cathode) can be used to balance the number of hole injections.
[0089] According to one embodiment of the present invention, the doping rate of the first p-type dopant in the first organic layer is equal to or greater than the doping rate of the second p-type dopant in the second organic layer.
[0090] According to one embodiment of the present invention, the LUMO of the first p-type dopant is greater than −5.2 eV.
[0091] According to one embodiment of the present invention, the LUMO of the first p-type dopant is greater than or equal to −5.1 eV.
[0092] According to one embodiment of the present invention, the LUMO of the first p-type dopant is greater than or equal to −5.0 eV.
[0093] According to one embodiment of the present invention, the LUMO of the second p-type dopant is greater than −5.2 eV.
[0094] According to one embodiment of the present invention, the LUMO of the second p-type dopant is greater than or equal to −5.1 eV.
[0095] According to one embodiment of the present invention, the LUMO of the second p-type dopant is greater than or equal to −5.0 eV.
[0096] According to an embodiment of the present invention, the LUMO of the first p-type dopant and / or the second p-type dopant is less than or equal to −4.35 eV.
[0097] According to an embodiment of the present invention, the LUMO of the first p-type dopant and / or the second p-type dopant is less than or equal to -4.5 eV.
[0098] According to an embodiment of the present invention, the first organic layer further comprises a first organic material.
[0099] According to an embodiment of the present invention, the second organic layer further comprises a second organic material.
[0100] According to one embodiment of the present invention, the HOMO energy level of the first organic material and / or the second organic material is greater than or equal to −4.5 eV.
[0101] According to one embodiment of the present invention, the HOMO energy level of the first organic material and / or the second organic material is greater than or equal to −4.8 eV.
[0102] According to an embodiment of the present invention, the doping rate of the first p-type dopant in the first organic layer is ≧0.01% and ≦99.9%.
[0103] According to an embodiment of the present invention, the doping rate of the first p-type dopant in the first organic layer is ≧0.1% and ≦99.9%.
[0104] According to one embodiment of the present invention, the doping rate of the first p-type dopant in the first organic layer is 0.5% to 50%.
[0105] According to an embodiment of the present invention, the doping rate of the second p-type dopant in the second organic layer is ≧0.01% and ≦99.9%.
[0106] According to an embodiment of the present invention, the doping rate of the second p-type dopant in the second organic layer is ≧0.1% and ≦99.9%.
[0107] According to an embodiment of the present invention, the doping rate of the second p-type dopant in the second organic layer is ≧0.5% and ≦50%.
[0108] According to an embodiment of the present invention, the electroluminescent device further includes a light-emitting layer disposed between the hole transport region and the cathode.
[0109] According to one embodiment of the present invention, the light-emitting layer contains a light-emitting material, which is a phosphorescent material, a fluorescent material or a delayed fluorescent material.
[0110] According to an embodiment of the present invention, the device further includes a third organic layer between the anode and the light emitting layer, the third organic layer containing a third p-type dopant.
[0111] According to an embodiment of the present invention, the third organic layer further comprises a third organic material.
[0112] According to an embodiment of the present invention, the third p-type dopant and the first p-type dopant are the same or different.
[0113] According to an embodiment of the present invention, the third p-type dopant and the second p-type dopant are the same or different.
[0114] According to an embodiment of the present invention, the third organic material and the first organic material are the same or different.
[0115] According to an embodiment of the present invention, the third organic material and the second organic material are the same or different.
[0116] According to an embodiment of the present invention, the organic electroluminescent device has two or more organic layers containing p-type dopant, for example, three, four or five organic layers containing p-type dopant. When the organic electroluminescent device has two or more organic layers containing p-type dopant, for example, a third organic layer is further included on the second organic layer. The third organic layer contains a third organic material and a third p-type dopant. The doping rate of the p-type dopant in the two or more organic layers may increase with a gradient along the direction from the anode to the cathode, may decrease with a gradient along the direction from the anode to the cathode, or may change parabolically (i.e., the doping rate increases and then decreases, or decreases and then increases). If necessary, the doping rates may be consistent.
[0117] According to an embodiment of the present invention, the organic electroluminescence device further includes a charge generating layer including a p-type charge generating layer.
[0118] According to one embodiment of the present invention, the p-type charge generating layer contains a first p-type dopant or a second p-type dopant.
[0119] According to one embodiment of the present invention, the first organic layer or the second organic layer is in contact with a p-type charge generating layer.
[0120] According to an embodiment of the present invention, in the charge generating layer, the doping rate of the first p-type dopant or the second p-type dopant in the p-type charge generating layer is 0.01% or more and 100% or less.
[0121] According to one embodiment of the present invention, the first organic material and the second organic material are identical.
[0122] According to one embodiment of the present invention, the first organic material and the second organic material are different.
[0123] According to one embodiment of the present invention, the organic electroluminescence device has a single-layer device structure of anode / first organic layer / second organic layer / hole transport layer / electron blocking layer / light-emitting layer / hole blocking layer / electron transport layer / electron injection layer / cathode. The organic layer structure may or may not be added as needed. For example, the electron blocking layer and the hole blocking layer are optional layers and can be selected as needed. The layer structure is not limited to a single-layer structure, for example, the light-emitting layer may be a two-layer structure, i.e., it may include two light-emitting layers. Between the second organic layer and the hole transport layer, the third organic layer of the present invention is further included.
[0124] According to one embodiment of the present invention, the organic electroluminescent device has a laminated element structure of anode / first light-emitting unit / charge generation layer / second light-emitting unit / cathode. Wherein, the first light-emitting unit and the second light-emitting unit may be the same or different, and each independently has an organic layer structure between the anode and the cathode in the above single-layer device structure. Between the second light-emitting unit and the cathode, a first charge generation layer and a third light-emitting unit, that is, an element structure of anode / first light-emitting unit / charge generation layer / second light-emitting unit / first charge generation layer / third light-emitting unit / cathode may be further included. Wherein, the third light-emitting unit and the first light-emitting unit may be the same or different, and the third light-emitting unit and the second light-emitting unit may also be the same or different.
[0125] According to one embodiment of the present invention, there is disclosed an electronic assembly including an organic electroluminescent device as described in any one of the above embodiments.
[0126] According to one embodiment of the present invention, the p-type dopant has a structure represented by Formula 1: [ka] (n is an integer selected from 1 to 5, Ring A is the same or different at each occurrence and is selected from conjugated rings having 3 to 30 ring atoms; R3 represents mono-, poly- or no substitution; R1, R2 and R3 are the same or different at each occurrence and are selected from hydrogen, deuterium or a substituent; Adjacent substituents R1, R2, and R3 may be bonded to form a ring.
[0127] In the present specification, "ring A is a conjugated ring having 3 to 30 ring atoms" means that ring A is a cyclic structure having 3 to 30 ring atoms, and ring A has a conjugated structural feature. Exemplarily, ring A includes, but is not limited to, structures represented by formulas 2 to 14 in the present application. The ring A may be a monocyclic structure or a polycyclic structure. Among them, the polycyclic ring may be a bonded ring structure or a condensed ring structure, or may be a totally conjugated structure formed by bonding two conjugated rings with a double bond, for example, a structure represented by formula 13 in the present application. The ring A may be a carbon ring or a hetero ring.
[0128] In this specification, "adjacent substituents R1, R2, and R3 may be bonded to form a ring" means that any one or more of adjacent substituent groups, such as the substituents R3, the substituents R1 and R2, the substituents R1 and R3, and the substituents R2 and R3, may be bonded to form a ring. Obviously, none of these substituents may be bonded to form a ring.
[0129] According to one embodiment of the present invention, the substituent is an electron-withdrawing group.
[0130] According to one embodiment of the present invention, n is selected from 1, 2 or 3.
[0131] According to one embodiment of the present invention, n is selected from 1 or 2.
[0132] According to one embodiment of the present invention, ring A is identical or different at each occurrence and is selected from conjugated rings having 3 to 20 ring atoms.
[0133] According to one embodiment of the present invention, ring A is identical or different at each occurrence and is selected from conjugated rings having 4 to 20 ring atoms.
[0134] According to one embodiment of the present invention, R1 and / or R2 are substituents comprising at least one electron-withdrawing group.
[0135] According to one embodiment of the present invention, the Hammett constant of the electron-withdrawing group is 0.05 or more, preferably 0.3 or more, more preferably 0.5 or more.
[0136] The electron-withdrawing group in the present invention has a Hammett substituent constant value of 0.05 or more, for example, 0.1 or more or 0.2 or more, preferably 0.3 or more, and more preferably 0.5 or more. Since the electron-withdrawing ability is strong, the LUMO energy level of the compound can be significantly lowered and the effect of improving the charge mobility can be achieved.
[0137] The Hammett substituent constant value includes a Hammett substituent para-position constant and / or a Hammett substituent meta-position constant. If both the para-position constant and the meta-position constant are greater than 0, and one of them is 0.05 or greater, the group can be selected in the present invention.
[0138] According to one embodiment of the present invention, the electron-withdrawing group is a C1-C20 substituted with one or more of halogen, nitroso, nitro, acyl, carbonyl, carboxyl, ester, cyano, isocyano, SCN, OCN, SF5, boranyl, sulfinyl, sulfonyl, phosphonoxy, or aza aromatic ring group, or a C1-C20 substituted with one or more of halogen, nitroso, nitro, acyl, carbonyl, carboxyl, ester, cyano, isocyano, SCN, OCN, SF5, boranyl, sulfinyl, sulfonyl, phosphonoxy, or aza aromatic ring group. the alkyl group having from 3 to 20 ring atoms, the cycloalkyl group having from 3 to 20 ring atoms, the heteroalkyl group having from 1 to 20 carbon atoms, the heterocyclic group having from 3 to 20 ring atoms, the aralkyl group having from 7 to 30 carbon atoms, the alkoxy group having from 1 to 20 carbon atoms, the aryloxy group having from 6 to 30 carbon atoms, the alkenyl group having from 2 to 20 carbon atoms, the alkynyl group having from 2 to 20 carbon atoms, the aryl group having from 6 to 30 carbon atoms, the heteroaryl group having from 3 to 30 carbon atoms, the alkylsilyl group having from 3 to 20 carbon atoms, and the arylsilyl group having from 6 to 20 carbon atoms, as well as any one of these groups and combinations thereof.
[0139] According to one embodiment of the present invention, the electron-withdrawing group is a halogen, a nitroso group, a nitro group, an acyl group, a carbonyl group, a carboxyl group, an ester group, SF5, a boranyl group, a sulfinyl group, a sulfonyl group, a phosphonoxy group, an aza aromatic ring group, or an aryl group having 1 to 20 carbon atoms substituted with one or more of a halogen, a nitroso group, a nitro group, an acyl group, a carbonyl group, a carboxyl group, an ester group, a cyano group, an isocyano group, SCN, OCN, SF5, a boranyl group, a sulfinyl group, a sulfonyl group, a phosphonoxy group, an aza aromatic ring group. and combinations thereof.
[0140] According to one embodiment of the present invention, the electron-withdrawing group is selected from the group consisting of fluorine, an acyl group, a carbonyl group, an ester group, SF5, a boranyl group, an azaaromatic ring group, and any one of an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 20 ring carbon atoms, a heteroalkyl group having 1 to 20 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an aryloxy group having 6 to 30 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, a heteroaryl group having 3 to 30 carbon atoms, an alkylsilyl group having 3 to 20 carbon atoms, and an arylsilyl group having 6 to 20 carbon atoms, each of which is substituted with one or more of fluorine, cyano, isocyano, SCN, OCN, SF5, CF3, OCF3, SCF3, and an azaaromatic ring group, and combinations thereof.
[0141] According to one embodiment of the present invention, ring A is selected from the group consisting of formulae 2 to 14, each occurrence being the same or different. [ka] X is, at each occurrence, identically or differently selected from the group consisting of N and CR3; W at each occurrence is identically or differently selected from the group consisting of O, S, Se, and NR3; R3 represents mono-, poly- or no substitution; R1, R2 and R3 are the same or different at each occurrence and are selected from hydrogen, deuterium or a substituent; Adjacent substituents R1, R2, and R3 may be bonded to form a ring; [ka] represents the bonding site between the double bond in Formula 2 to Formula 14 and Formula 1.
[0142] According to one embodiment of the present invention, the p-type dopant has a structure represented by the following formula: [ka] (X1, X2, X3 and X4 are identically or differently selected from the group consisting of N and CR3 at each occurrence; W at each occurrence is identically or differently selected from the group consisting of O, S, Se, and NR3; R1, R2 and R3 are the same or different at each occurrence and are selected from hydrogen, deuterium or a substituent; Adjacent substituents R1, R2, and R3 may be bonded to form a ring.
[0143] According to one embodiment of the present invention, the substituent is selected from the group consisting of halogen, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 ring carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted heterocyclic group having 3 to 20 ring atoms, a substituted or unsubstituted aralkyl group having 7 to 30 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted aryloxy group having 6 to 30 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted carbonyl group having 2 to 20 ring ... a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, a substituted or unsubstituted heteroaryl group having 3 to 30 carbon atoms, a substituted or unsubstituted alkylsilyl group having 3 to 20 carbon atoms, a substituted or unsubstituted arylsilyl group having 6 to 20 carbon atoms, a substituted or unsubstituted alkylgermanium group having 3 to 20 carbon atoms, a substituted or unsubstituted arylgermanium group having 6 to 20 carbon atoms, a substituted or unsubstituted amino group, acyl group, carbonyl group, carboxyl group, ester group, cyano group, isocyano group, hydroxy group, sulfanyl group, sulfinyl group, sulfonyl group, phosphino group, or a combination thereof, each having 0 to 20 carbon atoms.
[0144] According to one embodiment of the present invention, W, at each occurrence, is identical or different and is selected from O, S or Se.
[0145] According to one embodiment of the invention, W is selected from O or S, identically or differently at each occurrence.
[0146] According to one embodiment of the present invention, W is selected from O.
[0147] According to one embodiment of the present invention, W is selected from NR3, and R3 is selected from the group consisting of substituted or unsubstituted alkyl groups having 1 to 20 carbon atoms, substituted or unsubstituted cycloalkyl groups having 3 to 20 ring carbon atoms, substituted or unsubstituted heteroalkyl groups having 1 to 20 carbon atoms, substituted or unsubstituted aralkyl groups having 7 to 30 carbon atoms, substituted or unsubstituted alkoxy groups having 1 to 20 carbon atoms, substituted or unsubstituted aryloxy groups having 6 to 30 carbon atoms, substituted or unsubstituted alkenyl groups having 2 to 20 carbon atoms, substituted or unsubstituted alkynyl groups having 2 to 20 carbon atoms, substituted or unsubstituted aryl groups having 6 to 30 carbon atoms, substituted or unsubstituted heteroaryl groups having 3 to 30 carbon atoms, substituted or unsubstituted alkylsilyl groups having 3 to 20 carbon atoms, substituted or unsubstituted arylsilyl groups having 6 to 20 carbon atoms, and combinations thereof.
[0148] According to one embodiment of the present invention, W at each occurrence is the same or different and is selected from NR3, and R3 at each occurrence is the same or different and is selected from the group consisting of substituted or unsubstituted alkyl groups having 1 to 20 carbon atoms, substituted or unsubstituted cycloalkyl groups having 3 to 20 ring carbon atoms, substituted or unsubstituted aryl groups having 6 to 30 carbon atoms, substituted or unsubstituted heteroaryl groups having 3 to 30 carbon atoms, and combinations thereof.
[0149] According to one embodiment of the present invention, the p-type dopant is selected from the group consisting of, but not limited to, the following structures: [ka] [ka] [ka] [ka] [ka] [ka]
[0150] According to one embodiment of the present invention, the first organic material and / or the second organic material is selected from the group consisting of compounds having triarylamine units, spirobifluorene-based compounds, pentacene-based compounds, oligothiophene-based compounds, oligophenyl compounds, oligophenyleneethylene compounds, oligofluorene-based compounds, porphyrin complexes, or metal phthalocyanine complexes.
[0151] According to one embodiment of the present invention, the first organic material, the second organic material and the third organic material are all hole transport materials.
[0152] According to one embodiment of the present invention, the first organic material and / or the second organic material includes one or more chemical structural units selected from the group consisting of triarylamine, carbazole, fluorene, spirobifluorene, thiophene, furan, phenyl, oligophenyleneethylene, oligofluorene, and combinations thereof.
[0153] According to one embodiment of the present invention, the first organic material and / or the second organic material comprises monotriarylamine structural units or bistriarylamine structural units.
[0154] According to one embodiment of the present invention, the first organic material and / or the second organic material includes one or more chemical structural units selected from the group consisting of a monotriarylamine-carbazole structural unit, a monotriarylamine-thiophene structural unit, a monotriarylamine-furan structural unit, a monotriarylamine-fluorene structural unit, a bistriarylamine-carbazole structural unit, a bistriarylamine-thiophene structural unit, a bistriarylamine-furan structural unit, and a bistriarylamine-fluorene structural unit.
[0155] According to an embodiment of the present invention, the first organic material and / or the second organic material is a monotriarylamine compound or a bistriarylamine compound.
[0156] According to an embodiment of the present invention, the first organic material and / or the second organic material is selected from monotriarylamine-carbazole compounds, monotriarylamine-thiophene compounds, monotriarylamine-furan compounds, monotriarylamine-fluorene compounds, bistriarylamine-carbazole compounds, bistriarylamine-thiophene compounds, bistriarylamine-furan compounds, and bistriarylamine-fluorene compounds.
[0157] According to one embodiment of the present invention, the first organic material and / or the second organic material containing the monotriarylamine structural unit has a structure represented by Formula 20 or Formula 21. [ka] (Ar1, Ar2, Ar3, Ar4, Ar5 and Ar6 each occurrence may be the same or different and each occurrence may be selected from a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted heteroaryl group having 3 to 30 carbon atoms, and the structures of Ar1, Ar2, Ar3, Ar4, Ar5 and Ar6 do not include carbazole, L1, L2, L3 and L4 each appearing are the same or different and are selected from a single bond, a substituted or unsubstituted arylene group having 6 to 30 carbon atoms, a substituted or unsubstituted heteroarylene group having 3 to 30 carbon atoms, or a combination thereof, and the structures of L1, L2, L3 and L4 do not include carbazole; R, when present, is the same or different and represents mono-, multi- or no substitution; R each occurrence may be the same or different and is hydrogen, deuterium, a halogen, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 ring carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted heterocyclic group having 3 to 20 ring atoms, a substituted or unsubstituted aralkyl group having 7 to 30 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted aryloxy group having 6 to 30 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted carbon selected from the group consisting of an aryl group having 6 to 30 atoms, a substituted or unsubstituted heteroaryl group having 3 to 30 carbon atoms, a substituted or unsubstituted alkylsilyl group having 3 to 20 carbon atoms, a substituted or unsubstituted arylsilyl group having 6 to 20 carbon atoms, a substituted or unsubstituted alkylgermanium group having 3 to 20 carbon atoms, a substituted or unsubstituted arylgermanium group having 6 to 20 carbon atoms, an acyl group, a carbonyl group, a carboxyl group, an ester group, a cyano group, an isocyano group, a hydroxy group, a sulfanyl group, a sulfinyl group, a sulfonyl group, a phosphino group, and combinations thereof, wherein the structure of R does not include carbazole, Adjacent substituents may be bonded to form a ring.
[0158] According to one embodiment of the present invention, Ar1, Ar2, Ar3, Ar4, Ar5 and Ar6, each occurrence being the same or different, are selected from substituted or unsubstituted phenyl group, substituted or unsubstituted biphenyl group, substituted or unsubstituted terphenyl group, substituted or unsubstituted naphthalene group, substituted or unsubstituted dibenzofuran group, substituted or unsubstituted dibenzothiophene group, substituted or unsubstituted dibenzoselenophene group, substituted or unsubstituted phenanthrene group, substituted or unsubstituted triphenylene group, substituted or unsubstituted pyridine group, substituted or unsubstituted anthracene group, substituted or unsubstituted pyrene group, substituted or unsubstituted fluorene group, or combinations thereof.
[0159] According to one embodiment of the present invention, L1, L2, L3 and L4, each occurrence being the same or different, are selected from a single bond, a substituted or unsubstituted phenylene group, a substituted or unsubstituted biphenylene group, a substituted or unsubstituted terphenylene group, a substituted or unsubstituted naphthylene group, a substituted or unsubstituted dibenzofuranylene group, a substituted or unsubstituted dibenzothienylene group, a substituted or unsubstituted dibenzoselenophene group, a substituted or unsubstituted phenanthrylene group, a substituted or unsubstituted triphenylenylene group, a substituted or unsubstituted pyridinylene group, a substituted or unsubstituted anthracenylene group, a substituted or unsubstituted pyrenylene group, a substituted or unsubstituted fluorenylene group, or a combination thereof.
[0160] According to one embodiment of the present invention, the first organic material and / or the second organic material containing a bistriarylamine structural unit has a structure represented by Formula 22: [ka] (Ar7, Ar8, Ar9 and Ar 10 is selected from a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted heteroaryl group having 3 to 30 carbon atoms; Adjacent substituents Ar7 and Ar8 do not bond to form a ring, or adjacent substituents Ar9 and Ar 10 does not bond to form a ring, L5 is selected from a substituted or unsubstituted arylene group having 6 to 30 carbon atoms, or a substituted or unsubstituted heteroarylene group having 3 to 30 carbon atoms.
[0161] According to one embodiment of the present invention, Ar7, Ar8, Ar9 and Ar 10are the same or different at each occurrence and are selected from a substituted or unsubstituted phenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted terphenyl group, a substituted or unsubstituted naphthalene group, a substituted or unsubstituted carbazole group, a substituted or unsubstituted dibenzofuran group, a substituted or unsubstituted dibenzothiophene group, a substituted or unsubstituted dibenzoselenophene group, a substituted or unsubstituted phenanthrene group, a substituted or unsubstituted triphenylene group, a substituted or unsubstituted pyridine group, a substituted or unsubstituted anthracene group, a substituted or unsubstituted pyrene group, a substituted or unsubstituted fluorene group, or a combination thereof. Among them, adjacent substituents Ar7 and Ar8 do not bond to form a ring, or adjacent substituents Ar9 and Ar 10 do not bond to form a ring.
[0162] According to one embodiment of the present invention, L5 is selected from a single bond, a substituted or unsubstituted phenylene group, a substituted or unsubstituted biphenylene group, a substituted or unsubstituted terphenylene group, a substituted or unsubstituted naphthylene group, a substituted or unsubstituted carbazolylene group, a substituted or unsubstituted dibenzofuranylene group, a substituted or unsubstituted dibenzothienylene group, a substituted or unsubstituted dibenzoselenophene group, a substituted or unsubstituted phenanthrylene group, a substituted or unsubstituted triphenylenylene group, a substituted or unsubstituted pyridinylene group, a substituted or unsubstituted anthracenylene group, a substituted or unsubstituted pyrenylene group, a substituted or unsubstituted fluorenylene group, or a combination thereof.
[0163] According to one embodiment of the present invention, the first organic material and / or the second organic material includes one or more chemical structural units selected from the group consisting of triarylamine, carbazole, fluorene, spirobifluorene, thiophene, furan, phenyl, oligophenyleneethylene, oligofluorene, and combinations thereof.
[0164] According to one embodiment of the present invention, the first organic material and / or the second organic material is selected from the group consisting of, but not limited to, the following structures:
change
change
change
change
[0165] In terms of the device structure, OLEDs can be divided into a normal single-layer structure and a tandem structure (also called a stacked structure). A normal single-layer OLED contains only one light-emitting unit between a cathode and an anode, while a tandem OLED is composed of a plurality of light-emitting units stacked together. A light-emitting unit generally contains at least one light-emitting layer, one hole transport layer and one electron transport layer. The light-emitting unit may further contain a hole injection layer, an electron injection layer, a hole blocking layer and an electron blocking layer. It should be noted that a normal single-layer OLED contains only one light-emitting unit, but the light-emitting unit may contain multiple light-emitting layers, for example, the light-emitting unit may contain one yellow light-emitting layer and one blue light-emitting layer. However, each light-emitting unit can only contain one pair of hole transport layers and electron transport layers. A tandem OLED contains at least two or more light-emitting units, that is, it contains at least two pairs and more than two pairs of hole transport layers and electron transport layers. Here, the light-emitting units are arranged in a physical form of vertical stacking, thereby realizing the feature of series connection on a circuit, so it may be called a series-connected OLED (from circuit connection) or a stacked OLED (from physical form). At the same brightness, the current density required for the tandem OLED is smaller than that of a normal single-layer OLED, so the effect of improving the service life can be achieved. Conversely, at a constant current density, the brightness of the tandem OLED may be higher than that of a normal single-layer OLED, and the voltage may be improved accordingly. In the tandem OLED, adjacent light-emitting units are connected by a charge generation layer, and the quality of the charge generation layer directly affects the parameters such as the voltage, service life and efficiency of the tandem OLED. Therefore, the charge generation layer region needs to effectively generate holes and electrons and smoothly inject them into the corresponding light-emitting units, and the larger the transmittance in the visible light range, the more stable the performance and easy to manufacture.
[0166] In this specification, the LUMO energy level (lowest unoccupied molecular orbital) and HOMO energy level (highest occupied molecular orbital) of a compound are measured by cyclic voltammetry. A specific method is to use an electrochemical station, model number CorrTestCS120, manufactured by Wuhan Science Instrument Co., Ltd., and a three-electrode working system is used, with a platinum disk electrode as the working electrode, an Ag / AgNO3 electrode as the reference electrode, and a platinum wire electrode as the auxiliary electrode. Anhydrous DCM is used as the solvent and 0.1 mol / L tetrabutylammonium hexafluorophosphate is used as the supporting electrolyte, and the target compound is dissolved in 10 -3 mol / L solution, and before testing, nitrogen gas was introduced into the solution for 10 min to remove oxygen. The instrument parameters were set as follows: scan rate 100 mV / s, potential interval 0.5 mV, test window 1 V to -0.5 V. The LUMO energy levels of some p-type dopants and HOMO energy levels of organic materials in this application measured according to the above test method are listed in Table 1 below. Among them, the LUMOs of the p-type dopants are all smaller than -4.35 eV.
[0167] [Table 1]
[0168] The HOMO energy level of commonly used HTMs is generally less than -4.5 eV, but the present application uses a p-type dopant with a LUMO energy level less than -4.35 eV to reduce the energy difference with the HOMO of the HTM, ensure hole injection, and help stabilize the device voltage. By applying this p-type dopant with a LUMO energy level less than -4.35 eV to a device with a specific structure of the present application, the overall performance of the device can be further improved.
[0169] It is stated herein that the materials of specific layers used in the organic light-emitting device can be used in combination with multiple other materials present in the device. Illustratively, the compounds disclosed herein can be used in combination with multiple emitting dopants, hosts, transport layers, blocking layers, injection layers, electrodes and other possible layers. These combinations of materials are described in detail in paragraphs 0080-0101 of US Patent Application US2015 / 0349273A1, the contents of which are incorporated herein by reference in their entirety. The materials described or mentioned are non-limiting examples of materials that can be used in combination with the compounds disclosed herein, and those skilled in the art can easily refer to the literature to identify other materials that can be used in combination.
[0170] In the device examples, the characteristics of the devices were also tested using equipment common in the art (including but not limited to an evaporation machine manufactured by Angstrom Engineering, an optical test system and a service life test system manufactured by Suzhou Fusida, an ellipsometer manufactured by Beijing Liangtuo, etc.) in a manner familiar to those skilled in the art. Those skilled in the art are familiar with the use of the above-mentioned equipment, the test methods, and other related content, and can reliably and unaffectedly obtain the specific data of the samples, so the above-mentioned related content will not be repeated in this specification. EXAMPLES
[0171] The following will be described in detail with some examples to illustrate the working principle of the organic electroluminescence device. Obviously, the following examples are only for illustrative purposes, and are not intended to limit the scope of the present invention. Based on the following examples, those skilled in the art can obtain other embodiments of the present invention through modification.
[0172] Example 1-1
[0173] An organic electroluminescence device 300 shown in FIG. 3 was manufactured. (While the hole blocking layer 160 is omitted in this embodiment, those skilled in the art can add a hole blocking layer as necessary). The specific method is as follows. First, a glass substrate 101 having an indium tin oxide (ITO) anode 110 with a thickness of 1200 Å was cleaned and then treated with UV ozone and oxygen plasma. After treatment, the substrate was dried in a glove box filled with nitrogen gas to remove water. Then, the substrate was mounted on a substrate holder and placed in a vacuum chamber. The vacuum level was about 10. -6In the case of Torr, the organic layers were deposited on the ITO anode 110 in sequence by hot vacuum deposition at a rate of 0.01 to 10 Å / s. First, HT-18 and the first p-type dopant, compound 5-1, were co-deposited to form the first organic layer 120a. The doping rate of compound 5-1 was 0.5%, and the thickness of the first organic layer 120a was 50 Å. Then, HT-18 and compound 3-1 were co-deposited on the first organic layer to form the second organic layer 120b. The doping rate of compound 3-1 was 0.5%, and the thickness of the second organic layer 120b was 50 Å. The first organic layer 120a and the second organic layer 120b were both used as the hole injection layer 120, and the total thickness was 100 Å. Then, compound HT-18 is evaporated to be used as hole transport layer (HTL) 130, and the thickness of the hole transport layer (HTL) 130 is 400 Å. Compound EB is evaporated to be used as electron blocking layer (EBL) 140, and the thickness of the electron blocking layer (EBL) 140 is 50 Å. Next, compound D-1, which is a red light emitting dopant, is doped into host compound RH to form red light emitting layer (EML) 150. Among them, the doping rate of compound D-1 is 3%, and the thickness of the red light emitting layer (EML) 150 is 400 Å. Then, compounds ET and LiQ are co-evaporated to be used as electron transport layer (ETL) 170, and the thickness of the electron transport layer (ETL) 170 is 350 Å, and the doping rate of LiQ is 60%. On the ETL, 10 Å of LiQ is evaporated to be used as electron injection layer (EIL) 180. Finally, 1200 Å of Al was evaporated to serve as the cathode 190. The evaporated device was transferred to a glove box, and a glass cover was used as the sealing layer 102 to encapsulate and complete the device.
[0174] Example 1-2
[0175] The preparation process of Example 1-2 is similar to that of Example 1-1, except that the doping rate of the compound 5-1 in the first organic layer 120a is 1%.
[0176] Examples 1-3
[0177] The manufacturing process of Example 1-3 is the same as that of Example 1-1, except that the first organic layer 120a is made of the compound HT-18 and the compound 3-1, and the doping rate of the compound 3-1 is 2%, and the second organic layer 120b is made of the compound HT-18 and the compound 5-1, and the doping rate of the compound 5-1 is 0.5%.
[0178] Examples 1-4
[0179] The manufacturing process of Example 1-4 is similar to that of Example 1-1, except that the first organic layer 120a is composed of compound HT-18 and compound 1-2, the doping rate of compound 1-2 is 16%, and the thickness of the first organic layer 120a is 80 Å, the second organic layer 120b is composed of compound HT-18 and compound 3-1, the doping rate of compound 3-1 is 2%, and the thickness of the second organic layer 120b is 20 Å.
[0180] Examples 1-5
[0181] The manufacturing process of Example 1-5 is similar to that of Example 1-1, except that the first organic layer 120a is composed of compound HT-18 and compound 1-2, the doping rate of compound 1-2 is 16%, and the thickness of the first organic layer 120a is 80 Å, the second organic layer 120b is composed of compound HT-18 and compound 4-5, the doping rate of compound 4-5 is 3%, and the thickness of the second organic layer 120b is 20 Å.
[0182] Examples 1-6
[0183] The manufacturing process of Example 1-6 is the same as that of Example 1-1, except that the first organic layer 120a is composed of the compound HT-18 and the compound 1-2, and the doping rate of the compound 1-2 is 16%, and the second organic layer 120b is composed of the compound HT-18 and the compound 4-19, and the doping rate of the compound 4-19 is 2%.
[0184] Examples 1-7
[0185] The manufacturing process of Example 1-7 is the same as that of Example 1-1, except that the first organic layer 120a is made of the compound HT-18 and the compound 1-2, and the doping rate of the compound 1-2 is 16%, and the second organic layer 120b is made of the compound HT-18 and the compound 5-1, and the doping rate of the compound 5-1 is 2%.
[0186] Comparative Example 1-1
[0187] The manufacturing process of Comparative Example 1-1 is similar to that of Example 1-1, except that the first organic layer 120a is composed of compounds HT-18 and 5-1, the doping rate of compound 5-1 is 0.5%, and the thickness of the first organic layer 120a is 50 Å, the second organic layer 120b is composed of compounds HT-18 and 5-1, the doping rate of compound 5-1 is 0.5%, and the thickness of the second organic layer 120b is 50 Å.
[0188] Comparative Example 1-2
[0189] The manufacturing process of Comparative Example 1-2 is similar to that of Example 1-1, except that the first organic layer 120a is composed of compounds HT-18 and 3-1, the doping rate of compound 3-1 is 0.5%, and the thickness of the first organic layer 120a is 50 Å, the second organic layer 120b is composed of compounds HT-18 and 3-1, the doping rate of compound 3-1 is 0.5%, and the thickness of the second organic layer 120b is 50 Å.
[0190] Comparative Example 1-3
[0191] The manufacturing process of Comparative Example 1-3 is similar to that of Example 1-1, except that the first organic layer 120a is composed of compounds HT-18 and 5-1, the doping rate of compound 5-1 is 1%, and the thickness of the first organic layer 120a is 50 Å, the second organic layer 120b is composed of compounds HT-18 and 5-1, the doping rate of compound 5-1 is 1%, and the thickness of the second organic layer 120b is 50 Å.
[0192] Comparative Example 1-4
[0193] The manufacturing process of Comparative Example 1-4 is similar to that of Example 1-1, except that the first organic layer 120a is composed of the compound HT-18 and the compound 3-1, the doping rate of the compound 3-1 is 2%, and the thickness of the first organic layer 120a is 50 Å, the second organic layer 120b is composed of the compound HT-18 and the compound 3-1, the doping rate of the compound 3-1 is 2%, and the thickness of the second organic layer 120b is 50 Å.
[0194] Comparative Examples 1-5
[0195] The manufacturing process of Comparative Example 1-5 is similar to that of Example 1-1, except that the first organic layer 120a is composed of the compound HT-18 and the compound 1-2, the doping rate of the compound 1-2 is 16%, and the thickness of the first organic layer 120a is 50 Å, the second organic layer 120b is composed of the compound HT-18 and the compound 1-2, the doping rate of the compound 1-2 is 16%, and the thickness of the second organic layer 120b is 50 Å.
[0196] Comparative Examples 1-6
[0197] The manufacturing process of Comparative Example 1-6 is similar to that of Example 1-1, except that the first organic layer 120a is composed of the compound HT-18 and the compound 4-5, the doping rate of the compound 4-5 is 3%, and the thickness of the first organic layer 120a is 50 Å, the second organic layer 120b is composed of the compound HT-18 and the compound 4-5, the doping rate of the compound 4-5 is 3%, and the thickness of the second organic layer 120b is 50 Å.
[0198] Comparative Examples 1-7
[0199] The manufacturing process of Comparative Example 1-7 is similar to that of Example 1-1, except that the first organic layer 120a is composed of compounds HT-18 and 4-19, the doping rate of compound 4-19 is 2%, and the thickness of the first organic layer 120a is 50 Å, the second organic layer 120b is composed of compounds HT-18 and 4-19, the doping rate of compound 4-19 is 2%, and the thickness of the second organic layer 120b is 50 Å.
[0200] Comparative Example 1-8
[0201] The manufacturing process of Comparative Example 1-8 is similar to that of Example 1-1, except that the first organic layer 120a is composed of compounds HT-18 and 5-1, the doping rate of compound 5-1 is 2%, and the thickness of the first organic layer 120a is 50 Å, the second organic layer 120b is composed of compounds HT-18 and 5-1, the doping rate of compound 5-1 is 2%, and the thickness of the second organic layer 120b is 50 Å.
[0202] The details of the structures of some of the elements in Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-8 are shown in Table 2. Layers using more than one material are obtained by doping different compounds in the weight ratios mentioned above.
[0203] [Table 2]
[0204] The structure of the compound used in the device is shown below. [ka]
[0205] The performance of the elements in Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-8 was measured. Among them, the color coordinate (CIE), voltage and external quantum efficiency (EQE) were measured at a current density of 10 mA / cm 2 The element service life (LT97) was measured under the conditions of 80mA / cm 2 This is the actual measured time for the luminance to decay to 97% of the initial luminance under driving at a constant current density of 1000 Hz. These data are shown in Table 3.
[0206] [Table 3]
[0207] As can be seen from the color coordinates, the color coordinates in the above Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-8 were almost the same.
[0208] An OLED with high EQE, low voltage and long service life is a desirable good device, but if both cannot be achieved at the same time, the overall performance of the device must be considered. In Example 1-1, a device structure including the first and second organic layers in the present invention is used, the first organic layer and the second organic layer are in contact with each other, and the first p-type dopant in the first organic layer and the second p-type dopant in the second organic layer are different. The first p-type dopant, compound 5-1, has a LUMO energy level of -5.04 eV, and the second p-type dopant, compound 3-1, has a LUMO energy level of -4.91 eV, both of which are smaller than -4.35 eV. As shown in Table 3, Example 1 achieved a high EQE of 29.1%, a long service life of 200 h and a low driving voltage of 3.2 V. The results of comparing and analyzing Example 1-1 with Comparative Example 1-1 and Comparative Example 1-2, respectively, are as follows. (1) The first p-type dopant and the second p-type dopant in Comparative Example 1-1 are both compound 5-1, which are the same as the first dopant in Example 1-1, and the doping rate of compound 5-1 is also the same as the first organic layer in Example 1-1. Example 1-1 has a service life improved by 1.1 times compared to Comparative Example 1-1, and the voltage was equivalent. (2) The first p-type dopant and the second p-type dopant in Comparative Example 1-2 are both compound 3-1, which are the same as the second dopant in Example 1-1, and the doping rate of compound 3-1 is also the same as the second organic layer in Example 1-1. Example 1-1 has a service life improved by 42.8% and a driving voltage reduced by 0.4V compared to Comparative Example 1-2. Although the EQE of Example 1-1 was reduced by about 8% compared to Comparative Examples 1-1 and 1-2, it achieved a high EQE level of 29.1%, and more importantly, the improvement in service life in Example 1-1 was very significant, making the overall performance of Example 1-1 even more superior.
[0209] Example 1-2 is different from Example 1-1 in that the doping rate of the first p-type dopant in the first organic layer is improved from 0.5% in Example 1-1 to 1%. As shown in Table 3, Example 1-2 further improves the life of the device while achieving a high EQE of 27.6%, achieving an ultra-long life of 260h and a lower driving voltage. The results of comparing and analyzing Example 1-2 with Comparative Example 1-3 and Comparative Example 1-2 are as follows. The first p-type dopant and the second p-type dopant in Comparative Example 1-3 are both compound 5-1, which is the same as the first dopant in Example 1-2, and the doping rate of compound 5-1 is also the same as the first organic layer in Example 1-2. The first p-type dopant and the second p-type dopant in Comparative Example 1-2 are both compound 3-1, which is the same as the second dopant in Example 1-2, and the doping rate of compound 3-1 is also the same as the second organic layer in Example 1-2. Example 1-2 has an improved service life of 85.7% and 116.7% compared to Comparative Examples 1-2 and 1-3, respectively. At the same time, Example 1-2 has a reduced driving voltage of 0.6V compared to Comparative Example 1-2. Although the EQE in Example 1-2 is slightly lower than Comparative Examples 1-2 and 1-3, it achieves a relatively high EQE level of 27.6%, and more importantly, the improvement in service life in Example 1-2 is very significant, so that the overall performance of Example 1-2 is more excellent.
[0210] In Example 1-3, the first p-type dopant in the first organic layer is compound 3-1 with a doping rate of 2%, and the second p-type dopant in the second organic layer is compound 5-1 with a doping rate of 0.5%, and the first organic layer and the second organic layer contact each other. In Comparative Example 1-4, the first p-type dopant and the second p-type dopant are both compound 3-1, which are the same as the first dopant in Example 1-3, and the doping rate of compound 3-1 is also the same as the first organic layer in Example 1-3. In Comparative Example 1-1, the first p-type dopant and the second p-type dopant are both compound 5-1, which are the same as the second dopant in Example 1-3, and the doping rate of compound 5-1 is also the same as the second organic layer in Example 1-3. Compared with Comparative Examples 1-1 and 1-4, Example 1-3 has a comparable voltage and a service life of 163.1% and 15.7%, respectively, and Comparative Example 1-4 in particular has a longer service life and is therefore further improved. Although the EQE in Example 1-3 is slightly lower than that in Comparative Example 1-1, it achieves a relatively high EQE level of 28%, and more importantly, the service life improvement in Example 1-3 is very significant, so that the overall performance of Example 1-3 is even better.
[0211] In Example 1-4, the structure of the device including the first and second organic layers according to the present invention is used, the first organic layer and the second organic layer are in contact with each other, and the first p-type dopant in the first organic layer and the second p-type dopant in the second organic layer are different. The first p-type dopant, compound 1-2, has a LUMO energy level of -4.63 eV, and the second p-type dopant, compound 3-1, has a LUMO energy level of -4.91 eV, both of which are smaller than -4.35 eV. Compared with Comparative Example 1-5, in which the first p-type dopant and the second p-type dopant are both compound 1-2, Example 1-4 has a voltage lowered by 0.7 V, a service life significantly increased by 342%, and a slightly lower EQE, but an ultra-high EQE level of 31.5% is achieved, making it an element with excellent overall performance. Compared with Comparative Example 1-4 in which the first p-type dopant and the second p-type dopant are both compound 3-1, Example 1-4 has a 16% improvement in EQE, a slight 2% improvement in service life, and a slight 0.3V increase in voltage, so the overall performance of the device of Example 1-4 is better.
[0212] In Examples 1-5, the structure of the device including the first and second organic layers according to the present invention is used, the first organic layer and the second organic layer are in contact with each other, and the first p-type dopant in the first organic layer and the second p-type dopant in the second organic layer are different. The first p-type dopant, compound 1-2, has a LUMO energy level of -4.63 eV, and the second p-type dopant, compound 4-5, has a LUMO energy level of -5.17 eV, both of which are smaller than -4.35 eV. Compared with Comparative Example 1-5, in which both the first p-type dopant and the second p-type dopant are compound 1-2, Example 1-5 has a voltage lowered by 1 V, a service life significantly improved by 282%, and a slightly lower EQE of 28.8%, making it a device with very excellent overall performance. Compared with Comparative Example 1-6, in which the first p-type dopant and the second p-type dopant are both compounds 4-5, Examples 1-5 have an 11% improvement in EQE, and the voltage and service life are comparable, so the overall performance of the devices in Examples 1-5 is better.
[0213] In Examples 1-6, the structure of the device including the first and second organic layers according to the present invention is used, the first organic layer and the second organic layer are in contact with each other, and the first p-type dopant in the first organic layer and the second p-type dopant in the second organic layer are different. The first p-type dopant, compound 1-2, has a LUMO energy level of -4.63 eV, and the second p-type dopant, compound 4-19, has a LUMO energy level of -5.12 eV, both of which are smaller than -4.35 eV. Compared with Comparative Example 1-5, in which the first p-type dopant and the second p-type dopant are both compound 1-2, Example 1-6 has a voltage lowered by 0.8 V, a service life significantly improved by 340%, and a slightly lower EQE of 30.6%, making it a device with excellent overall performance. Compared with Comparative Example 1-7 in which the first p-type dopant and the second p-type dopant are both compound 4-19, the EQE of Example 1-6 is improved by 9%, the service life is significantly improved by 106%, and the voltage is slightly improved by 0.2V, so that the overall performance of the device of Example 1-6 is more excellent.
[0214] In Example 1-7, the first p-type dopant in the first organic layer is compound 1-2, and the second p-type dopant in the second organic layer is compound 5-1, the first organic layer and the second organic layer are in contact with each other, and the LUMO energy levels of the first p-type dopant and the second p-type dopant are both less than -4.35 eV. Compared with Comparative Example 1-5, in which the first p-type dopant and the second p-type dopant are compound 1-2, Example 1-7 has a voltage lowered by 1V, a service life significantly improved by 320%, and a slightly lower EQE of 29.2%, making it an element with very good overall performance. Compared with Comparative Example 1-8, in which the first p-type dopant and the second p-type dopant are both compound 5-1, Example 1-7 has a 9% improvement in EQE, a significantly improved service life of 75%, and a voltage that is almost the same.
[0215] From the above comparison, it was found that an OLED having excellent overall performance can be obtained by using an organic electroluminescence device including the specific first organic layer and second organic layer according to the present invention.
[0216] Example 2-1
[0217] A stacked organic electroluminescence device 400 shown in FIG. 4 was manufactured (wherein, in this embodiment, the hole blocking layers 160a and 160b are omitted, but those skilled in the art can add hole blocking layers as necessary). The specific method is as follows. First, a glass substrate 101 having a pre-patterned indium tin oxide (ITO) anode 110 with a thickness of 1200 Å was washed with ultrapure water, and the ITO surface was treated with UV ozone and oxygen plasma. Then, the substrate was dried in a glove box filled with nitrogen gas to remove water, and then mounted on a holder and placed in a deposition chamber. Hereinafter, for the specified organic layer, the vacuum degree was about 1*10 -6In the case of 3000 Å, deposition was performed on the ITO anode 110 in sequence by hot vacuum deposition at a rate of 0.01 to 10 Å / s. First, the first light-emitting unit 1101 was deposited. First, HT-18 and compound 1-2 were co-deposited to be used as the first organic layer (121a). Among them, the doping rate of compound 1-2 was 16%, and the thickness of the first organic layer (121a) was 80 Å. Then, HT-18 and compound 3-1 were co-deposited on the first organic layer 121a to be used as the second organic layer (122a). Among them, the doping rate of compound 3-1 was 3%, and the thickness of the second organic layer (122a) was 20 Å. The first organic layer 121a and the second organic layer 122a were both used as the hole injection layer 220a, and the total thickness was 100 Å. Then, compound HT-18 is evaporated to form hole transport layer (HTL) 130a, and the thickness of hole transport layer (HTL) 130a is 400 Å. On HTL, compound EB is evaporated to form electron blocking layer (EBL) 140a, and the thickness of electron blocking layer (EBL) 140a is 50 Å. Next, compound D-1, which is a red light emitting dopant, is doped into host compound RH to form red light emitting layer (EML) 150a. Among them, the doping rate of compound D-1 is 3%, and the thickness of red light emitting layer (EML) 150a is 400 Å. Then, compound ET and LiQ are co-evaporated to form electron transport layer (ETL) 170a, and the thickness of electron transport layer (ETL) 170a is 350 Å, and the doping rate of LiQ is 60%. A charge generation layer 1102 was deposited on the ETL, and then 15 Å of Yb metal was deposited to form an n-type charge generation layer 210. Then, 30 Å of compound 1-2 was deposited to form a p-type charge generation layer 310. Then, a second light-emitting unit 1103 was deposited. HT-18 and compound 1-2 were co-deposited to form a first organic layer (121b). The doping rate of compound 1-2 was 16%, and the thickness of the first organic layer (121b) was 80 Å. Then, HT-18 and compound 3-1 were co-deposited on the first organic layer 121b to form a second organic layer (122b). The doping rate of compound 3-1 was 3%, and the thickness of the second organic layer (122b) was 20 Å.The first organic layer 121b and the second organic layer 122b are both used as the hole injection layer 220b, and have a total thickness of 100 Å. Then, the compound HT-18 is evaporated to be used as the hole injection layer (HTL) 130b, and the thickness of the hole transport layer (HTL) 130b is 400 Å. The compound EB is evaporated to be used as the electron blocking layer (EBL) 140b, and the thickness of the electron blocking layer (EBL) 140b is 50 Å. Next, the compound D-1, which is a red light emitting dopant, is doped into the host compound RH to form the red light emitting layer (EML) 150b. The doping rate of the compound D-1 is 3%, and the thickness of the red light emitting layer (EML) 150b is 400 Å. Then, the compounds ET and LiQ are co-evaporated to form the electron transport layer (ETL) 170b, the thickness of the electron transport layer (ETL) 170b is 350 Å, and the doping rate of LiQ is 60%. Finally, the compound LiQ is evaporated to a thickness of 10 Å to form the electron injection layer (EIL) 180, and aluminum is evaporated to a thickness of 1200 Å to form the cathode 190. After the device is fabricated, it is transferred from the evaporation chamber to a glove box, and a glass cover is used as the sealing layer 102 to complete the encapsulation. It should be noted that the structure of the device is merely illustrative and is not limited to those described in the present invention. For example, the hole injection layer 220a in the first light-emitting unit 1101 may have a different structure from that of the hole injection layer 220b in the second light-emitting unit 1103. Furthermore, for example, the second light-emitting unit 1103 may use other color light-emitting materials and host compounds, and a corresponding set of transport materials and device structures.
[0218] Comparative Example 2-1
[0219] The manufacturing method of Comparative Example 2-1 is identical to that of Example 2-1, except that the first organic layer 121a in the first light-emitting unit and the first organic layer 121b in the second light-emitting unit are both composed of HT-18 and compound 3-1, the doping rate of compound 3-1 is both 3%, and the thickness is 80 Å, and the second organic layer 122a in the first light-emitting unit and 122b in the second light-emitting unit are both composed of HT-18 and compound 3-1, the doping rate of compound 3-1 is both 3%, and the thickness is 20 Å.
[0220] Comparative Example 2-2
[0221] The manufacturing method of Comparative Example 2-2 is identical to that of Example 2-1, except that the first organic layer 121a in the first light-emitting unit and the first organic layer 121b in the second light-emitting unit are both composed of HT-18 and compound 1-2, the doping rate of compound 1-2 is both 16%, and the thickness is 80 Å, and the second organic layer 122a in the first light-emitting unit and the second organic layer 122b in the second light-emitting unit are both composed of HT-18 and compound 1-2, the doping rate of compound 1-2 is both 16%, and the thickness is 20 Å.
[0222] The detailed structures of some of the elements in Example 2-1 and Comparative Examples 2-1 to 2-2 are shown in Table 4. Layers using more than one material are obtained by doping different compounds in the weight ratios mentioned above.
[0223] [Table 4]
[0224] The performance of the elements in Example 2-1 and Comparative Examples 2-1 and 2-2 was measured. Among them, the color coordinate (CIE), voltage and external quantum efficiency (EQE) were 2 The device's service life is 2000cd / m 2 The time it takes for the light to decay to 97% of its initial brightness under these conditions is shown in Table 5.
[0225] [Table 5]
[0226] Example 2-1 is a stacked OLED connected by a charge generating layer. The first light-emitting unit and the second light-emitting unit connected to the charge generating layer both include the same first organic layer and second organic layer, and the first p-type dopant contained in the first organic layer and the second p-type dopant contained in the second organic layer are different, and are compound 1-2 and compound 3-1, respectively. Comparative Examples 2-1 and 2-2 are also stacked OLEDs having a similar device structure, but the first organic layer and the second organic layer in the first light-emitting unit and the second light-emitting unit both contain the same p-type dopant. In Comparative Example 2-1, compound 3-1 is used as the p-type dopant, and in Comparative Example 2-2, compound 1-2 is used as the p-type dopant.
[0227] As can be seen from the device performance data in Table 5 above, Example 2-1, which includes the specific first and second organic layers according to the present application, has a luminance of 2000 cd / m 2 A high EQE of 61.7%, a low voltage of 5.7V, and a long service life of 25300h were achieved under the same temperature range, and the service life was 4% longer, the voltage was kept at the same level, and the EQE was 22% higher than that of Comparative Example 2-1, in which both the first and second organic layers contained compound 3-1. At the same time, Example 2-1 showed a voltage 0.2V lower and an efficiency 6% higher than that of Comparative Example 2-2, in which both the first and second organic layers contained compound 1-2, and the improvement in service life was more significant, increasing by 17%.
[0228] As can be seen from this, the laminated element including the specific first organic layer and second organic layer according to the present invention can also significantly improve the overall performance of the laminated element.
[0229] Example 3-1
[0230] The organic electroluminescence device 300 shown in FIG. 3 was manufactured by the following specific method. First, a glass substrate 101 having an indium tin oxide (ITO) anode 110 with a thickness of 800 Å was cleaned and then treated with UV ozone and oxygen plasma. The substrate was then dried in a glove box filled with nitrogen gas to remove water. The vacuum degree was about 10. -6 In the case of Torr, the organic layers were deposited on the ITO anode 110 in sequence by host vacuum deposition at a rate of 0.01 to 10 Å / s. First, HT-18 and a compound 1-2, which is a first p-type dopant, were co-deposited to form a first organic layer 120a. The doping rate of the compound 1-2 was 16%, and the thickness of the first organic layer 120a was 80 Å. Then, HT-18 and a compound 3-1 were co-deposited on the first organic layer 120a to form a second organic layer 120b. The doping rate of the compound 3-1 was 3%, and the thickness of the second organic layer 120b was 20 Å. The first organic layer 120a and the second organic layer 120b were both used as the hole injection layer 120, and the total thickness was 100 Å. Then, compound HT-18 is evaporated to be used as hole transport layer (HTL) 130, and the thickness of the hole transport layer (HTL) 130 is 250 Å. Compound HT-1 is used as electron blocking layer (EBL) 140, and the thickness of the electron blocking layer (EBL) 140 is 50 Å. Then, compound D-2, which is a blue light dopant, and blue light host compound BH are co-evaporated to be used as blue light emitting layer (EML) 150, and the doping rate of compound D-2 is 4% and the total thickness is 250 Å. Then, compound HB is evaporated to be used as hole blocking layer (HBL) 160, and the thickness of the hole blocking layer (HBL) 160 is 50 Å. On the HBL, compound ET1 and LiQ are co-evaporated to be used as electron transport layer (ETL) 170, and the thickness of the electron transport layer (ETL) 170 is 300 Å and the doping rate of LiQ is 60%. On the ETL, 10 Å of LiQ was evaporated to serve as an electron injection layer (EIL). Finally, 1200 Å of Al was evaporated to serve as a cathode 190. The evaporated device was transferred to a glove box and a glass cover was used as an encapsulation layer 102 to encapsulate and complete the device.
[0231] Comparative Example 3-1
[0232] The manufacturing process of Comparative Example 3-1 is the same as that of Example 3-1, except that the first organic layer 120a is composed of HT-18 and compound 3-1, the doping rate of compound 3-1 is 3%, and the thickness of the first organic layer 120a is 80 Å, the second organic layer is composed of compound HT-18 and compound 3-1, the doping rate of compound 3-1 is 3%, and the thickness of the second organic layer is 20 Å.
[0233] The structural details of some elements in Example 3-1 and Comparative Example 3-1 are shown in Table 6. Layers using more than one material are obtained by doping different compounds in the weight ratios mentioned above.
[0234] [Table 6]
[0235] The structure of the compound newly used in the device is shown below. [ka]
[0236] The performance of the elements in Example 3-1 and Comparative Example 3-1 was measured. The color coordinates (CIE), voltage and external quantum efficiency (EQE) were measured at a current density of 10 mA / cm 2 The element service life (LT97) was measured under the conditions of 80mA / cm 2 This is the actual measured time for the luminance to decay to 97% of the initial luminance under driving at a constant current density of 1000 Hz. These data are shown in Table 7.
[0237] [Table 7]
[0238] Example 3-1 and Comparative Example 3-1 are blue fluorescent devices, and the color coordinates of Example 3-1 and Comparative Example 3-1 shown in Table 7 are almost the same. In Example 3-1, the device includes a first organic layer and a second organic layer, and the first p-type dopant and the second p-type dopant contained in the first organic layer and the second organic layer are different, while the p-type dopant contained in the first organic layer and the second organic layer in Comparative Example 3-1 is the same. As can be seen from the comparison of the device data in Table 7, the voltages of the devices in Example 3-1 and Comparative Example 3-1 are almost equivalent, but the service life in Example 3-1 is significantly improved by 20% and the EQE is improved by 8.6%. It is shown that the first organic layer and the second organic layer containing a specific structure in the present invention also have a remarkable effect in terms of improving the overall performance of the blue light device.
[0239] In summary, this application discloses a novel organic electroluminescent device, which relates to a first organic layer and a second organic layer having a specific structure, in which the first organic layer contains a first p-type dopant, the second organic layer contains a second p-type dopant, the first p-type dopant and the second p-type dopant are different, and the first organic layer and the second organic layer are in contact with each other. The organic electroluminescent device having such a specific structure achieves a remarkable effect in terms of improving the overall performance of the device.
[0240] It should be understood that the various embodiments described herein are merely illustrative and are not intended to limit the scope of the present invention. Thus, it will be apparent to those skilled in the art that the invention sought to be protected includes variations of the specific and preferred embodiments described herein. Many of the materials and structures described herein can be substituted with other materials and structures without departing from the concept of the present invention. It should be understood that the various theories as to why the present invention works are not limiting.
Claims
1. An organic electroluminescent device comprising an anode, a cathode, and a hole transport region disposed between the anode and the cathode, the hole transport region includes a first organic layer and a second organic layer; the first organic layer contains a first p-type dopant; the second organic layer contains a second p-type dopant; the first p-type dopant and the second p-type dopant are different; the LUMO energy levels of the first p-type dopant and the second p-type dopant are both −4.35 eV or less; the first organic layer is in contact with the second organic layer; the second organic layer overlies the first organic layer; An organic electroluminescent device, wherein a doping rate of the first p-type dopant in the first organic layer is greater than a doping rate of the second p-type dopant in the second organic layer.
2. 2. The organic electroluminescence device according to claim 1, wherein the sum of the thicknesses of the first and second organic layers is not greater than 100 nm.
3. The organic electroluminescent element as described in claim 1, characterized in that the sum of the thicknesses of the first organic layer and the second organic layer is not greater than 20 nm.
4. 2. The organic electroluminescence device according to claim 1, wherein the first p-type dopant and the second p-type dopant are molecular type p-type dopants, and the p-type dopants have the following structure: 【Chemistry 1】 wherein X 1 , X 2 , X 3 and X 4 at each occurrence are the same or different and are selected from the group consisting of N and CR 3 ; W at each occurrence is the same or different and is selected from the group consisting of O, S, Se and NR 3 ; R 1 , R 2 and R 3 at each occurrence are the same or different and are selected from hydrogen, deuterium or a substituent; adjacent substituents R 1 , R 2 and R 3 may be bonded to form a ring; The substituents include halogen, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 ring carbon atoms, a substituted or unsubstituted heteroalkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted heterocyclic group having 3 to 20 ring atoms, a substituted or unsubstituted aralkyl group having 7 to 30 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 20 carbon atoms, a substituted or unsubstituted aryloxy group having 6 to 30 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a substituted or unsubstituted aryloxy group having 6 to 3 ... aryl group having 0 carbon atoms, a substituted or unsubstituted heteroaryl group having 3 to 30 carbon atoms, a substituted or unsubstituted alkylsilyl group having 3 to 20 carbon atoms, a substituted or unsubstituted arylsilyl group having 6 to 20 carbon atoms, a substituted or unsubstituted alkylgermanium group having 3 to 20 carbon atoms, a substituted or unsubstituted arylgermanium group having 6 to 20 carbon atoms, a substituted or unsubstituted amino group, acyl group, carbonyl group, carboxyl group, ester group, cyano group, isocyano group, hydroxy group, sulfanyl group, sulfinyl group, sulfonyl group, phosphino group, or a combination thereof having 0 to 20 carbon atoms.
5. 2. The organic electroluminescence device according to claim 1, wherein the LUMO energy level of the first p-type dopant and / or the second p-type dopant is −4.5 eV or less.
6. The organic electroluminescent element of claim 5, wherein the LUMO energy level of the first p-type dopant and / or the second p-type dopant is greater than −5.2 eV.
7. The organic electroluminescence device according to claim 1 , wherein the first organic layer is in contact with an anode.
8. 8. The organic electroluminescence device according to claim 1, wherein a LUMO energy level of the first p-type dopant is greater than a LUMO energy level of the second p-type dopant.
9. 8. The organic electroluminescence device according to claim 1, wherein a LUMO energy level of the first p-type dopant is equal to or lower than a LUMO energy level of the second p-type dopant.
10. 2. The organic electroluminescence device according to claim 1, further comprising a light-emitting layer provided between the anode and the cathode.
11. 11. The organic electroluminescence device according to claim 10, wherein the light-emitting layer contains a light-emitting material which is a phosphorescent material, a fluorescent material, or a delayed fluorescent material.
12. 2. The organic electroluminescent device according to claim 1, wherein the hole transport region further comprises a third organic layer containing a third p-type dopant.
13. An organic electroluminescent element as described in claim 12, characterized in that the third p-type dopant and the first p-type dopant are the same or different, and / or the third p-type dopant and the second p-type dopant are the same or different.
14. 2. The organic electroluminescence device according to claim 1, further comprising a charge generating layer comprising a p-type charge generating layer.
15. 15. The organic electroluminescence device according to claim 14, wherein the p-type charge generating layer contains a first p-type dopant or a second p-type dopant.
16. 15. The organic electroluminescence device according to claim 14, wherein the first organic layer or the second organic layer is in contact with a p-type charge generating layer.
17. the first organic layer further comprises a first organic material, and the second organic layer further comprises a second organic material; 2. The organic electroluminescence device according to claim 1, wherein the first organic material and the second organic material are the same or different.
18. 18. The organic electroluminescence device according to claim 17, wherein the HOMO energy level of the first organic material and / or the second organic material is smaller than −4.5 eV.
19. The organic electroluminescent element of claim 17, wherein the HOMO energy level of the first organic material and / or the second organic material is smaller than −4.8 eV.
20. 18. The organic electroluminescence device according to claim 17, wherein the first organic material and / or the second organic material contains a monotriarylamine structural unit or a bistriarylamine structural unit.
21. The organic electroluminescence element of claim 17, wherein the first organic material and / or the second organic material includes one or more chemical structural units selected from the group consisting of a monotriarylamine-carbazole structural unit, a monotriarylamine-thiophene structural unit, a monotriarylamine-furan structural unit, a monotriarylamine-fluorene structural unit, a bistriarylamine-carbazole structural unit, a bistriarylamine-thiophene structural unit, a bistriarylamine-furan structural unit, and a bistriarylamine-fluorene structural unit.
22. An electronic assembly comprising the organic electroluminescent device of claim 1 .
Citation Information
Patent Citations
Organic luminous display element and its producing method
CN100373656C
Materials for electronic devices
CN107112437A
Organic electroluminescent devices and their fabrication methods
CN109216565B
Organic electric field light emitting element
JP2001223084A
Organic electroluminescence element
JP2006024711A