Polymer composite material and its manufacturing method

By integrating polyhydric alcohol and kaolinite with a polymer compound, the polymer composite material addresses issues of thermal fluidity and dispersion, achieving improved melt tension and mechanical strength while promoting sustainable waste utilization.

JP7562199B2Active Publication Date: 2024-10-07大野 孝
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024532383
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-08-29
Publication Date
2024-10-07
Estimated Expiration
2042-08-29

AI Technical Summary

Technical Problem

Existing polymer composite materials face limitations such as reliance on starch-based fillers competing with food resources, low thermal fluidity, poor interfacial adhesion, decreased manufacturing efficiency due to increased liquid medium, and low melt tension, along with molding defects and poor physical properties.

Method used

Incorporating polyhydric alcohol and a thickener like kaolinite into a polymer compound to enhance viscosity, followed by mixing with a filler, forming a melt-kneaded body to create a polymer composite material with improved melt tension and uniform dispersion.

Benefits of technology

The resulting polymer composite material effectively utilizes waste plastics and other fillers, enhancing functionality, improving melt tension and mechanical strength, and contributing to sustainable development goals by reducing fossil resource use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562199000001
    Figure 0007562199000001
  • Figure 0007562199000002
    Figure 0007562199000002
  • Figure 0007562199000003
    Figure 0007562199000003
Patent Text Reader

Abstract

Provided are: a polymer composite material that has excellent functionality, makes effective use of previously unused waste plastics and waste products as a filler, and contributes to achieving the SDGs; and technology for producing the polymer composite material. A method for producing the polymer composite material includes: a step in which a polyalcohol (25), a thickener (26) for increasing the viscosity of the polyalcohol (25), a polymer compound (27), and in some cases a filler (28) are mixed to obtain a mixture (22); and a step in which the mixture (22) is loaded into a sealed container (30), heated, and kneaded to obtain a melt-kneaded body (23).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a manufacturing technology for polymer composite materials that contributes to the realization of the Sustainable Development Goals (SDGs). [Background technology]

[0002] In order to make effective use of biomass and other underutilized resources, it is being considered to disperse and compound them in polymer compounds as fillers. Furthermore, the development of polymer composite materials that contribute to the realization of the SDGs by reducing the amount of polymer compounds produced from fossil resources is being promoted.

[0003] A technology has been disclosed in which starch-based materials are gelatinized by adding moisture while still in granular form, without being subjected to processes such as starch extraction or pulverization, and then heated and kneaded together with a polymer compound and a compatibilizer (Patent Document 1).

[0004] Also, a technology has been disclosed in which powders such as crushed shells and fly ash are heated and kneaded with a polymer compound together with a liquid medium to finely disperse the powder in the continuous phase of the polymer compound (Patent Documents 2 and 3). This allows the proportion of the polymer compound used in the polymer composite material to be sufficiently reduced without impairing its practicality. Furthermore, a solute contained in the liquid medium may function as a compatibilizer between the filler and the polymer compound.

[0005] Furthermore, a technology has been disclosed in which waste with a high moisture content (water-containing material) is treated without drying by adding a hygroscopic substance, and then heated and kneaded with a polymer compound to produce a thin film-like polymer composite material (Patent Document 4). This allows the filler to be finely dispersed in the continuous phase of the polymer compound through a process of hydrogen bonding between the moisture in the water-containing material and the water-absorbing substance, improving the physical properties and imparting functionality to the polymer composite material. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 3878623 [Patent Document 2] Patent No. 5097191 [Patent Document 3] Patent No. 5584807 [Patent Document 4] Patent No. 7061239 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the polymer composite material according to Patent Document 1 is limited to fillers that gelatinize when heated and kneaded. Fillers with such functionality are limited to starch-based materials, which poses a problem of conflict with food issues. In addition, thermoplastic resins with gelatinized starch-based materials dispersed therein have low thermal fluidity. For this reason, it was necessary to add a large amount of a compatibilizer to improve the interfacial adhesion between the starch-based material and the polymer compound.

[0008] In the manufacturing methods of Patent Documents 2 and 3, increasing the amount of liquid medium to finely disperse the powder leads to a decrease in manufacturing efficiency. In addition, when the interfacial adhesion between the filler and the polymer compound is poor, it is necessary to increase the amount of compatibilizer. However, it can be difficult to incorporate a sufficient amount of compatibilizer, and there is a problem that as the proportion of the filler increases, the physical properties of the polymer composite material are significantly reduced compared to the physical properties of the polymer compound that constitutes the continuous phase.

[0009] In the manufacturing method of Patent Document 4, in order to prevent molding defects, it is necessary to adjust the moisture content of the polymer composite material at the thermal flow temperature to 1% or less. For this purpose, it is necessary to use a specially designed device that can remove moisture from the kneaded body. In terms of physical properties, the polymer composite material has a problem of having a lower melt tension than the polymer compound that constitutes the continuous phase.

[0010] The present invention has been made in consideration of the above circumstances, and aims to provide a polymer composite material and its manufacturing technology that has excellent functionality, makes effective use of previously unused waste plastics and other waste materials as fillers, and contributes to the realization of the SDGs. [Means for solving the problem]

[0011] The method for producing a polymer composite material according to the present invention includes the steps of: adding and mixing a polyhydric alcohol into a polymer compound, then adding and mixing a thickener that increases the viscosity of the polyhydric alcohol to form a mixture in which the polyhydric alcohol with increased viscosity is spread on the polymer compound; and putting the mixture into a sealed container and kneading it by heating to form a molten mixture. the polymer compound is a thermoplastic resin, the polyhydric alcohol is ethylene glycol, and the thickener is kaolinite. It is characterized by: Effect of the Invention

[0012] The present invention provides a polymer composite material and a manufacturing technology thereof that has excellent functionality and enables previously unused waste plastics and other waste materials to be effectively utilized as fillers, thereby contributing to the realization of the SDGs. [Brief description of the drawings]

[0013] [Figure 1] 1 is a side view of a production system for a resin composite material according to a first embodiment of the present invention. [Diagram 2] FIG. 4 is a side view of a production system for a resin composite material according to a second embodiment of the present invention. [Diagram 3] 1 is a table showing Example 1 and Comparative Example 1 in which the effect of the first embodiment was confirmed using melt tension as an index. [Figure 4] 13 is a table showing Example 2 and Comparative Example 2 in which the effects of the second embodiment were confirmed using mechanical strength characteristics as an index. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] (First embodiment) Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. Fig. 1 is a side view of a resin composite material manufacturing system 10A (10) according to a first embodiment of the present invention. This manufacturing system 10A is composed of a raw material mixing device 20A, a raw material supplying device 19, and a kneading device 30. The raw material supplying device 19 supplies the mixture 22 mixed in the raw material mixing device 20 to the kneading device 30, and is appropriately selected to suit the properties of the mixture 22.

[0015] The kneading device 30 is preferably a continuous extruder equipped with a cylinder 33 forming a sealed container with a hopper 31 for introducing the mixture 22 provided on the upstream side and a die section 35 for extruding the molten kneaded body 23 provided on the downstream side, and a drive section 32 for extruding the heated mixture 22 from upstream to downstream by rotating a screw around the axis inside the sealed container of the cylinder 33 to form the molten kneaded body 23. Either a single-screw extruder or a twin-screw extruder can be used, but a twin-screw extruder is more preferably used in a method for producing a polymer composite material including a step of mixing a filler 28 (FIG. 2) (second embodiment described later).

[0016] The raw material mixing device 20A includes a first container 15 for accommodating a polyhydric alcohol 25, a second container 16 for accommodating a thickener 26 for increasing the viscosity of the polyhydric alcohol 25, a third container 17 for accommodating a polymer compound 27, and a mixing tank 12 for mixing the polyhydric alcohol 25, the thickener 26, and the polymer compound 27 to obtain a mixture 22A. Then, the first container 15 and the third container 17 are each opened and the mixture is stirred in the mixing tank 12, and the surface of the polymer compound 27 is sufficiently wetted with the polyhydric alcohol 25. After that, the second container 16 is opened and the mixture is stirred in the mixing tank 12, and the thickener 26 is added to obtain a mixture 22A.

[0017] This suppresses gravity separation between the low-viscosity liquid polyhydric alcohol 25 and the solid polymer compound 27, producing a uniform mixture 22A. Note that, as an example of the order of addition for producing the mixture 22A, first, the polyhydric alcohol 25 is added to the polymer compound 27 and mixed, and then the thickener 26 is added and mixed, but there is no particular limitation on the order of addition, and they may be added simultaneously.

[0018] The amount of polyhydric alcohol 25 to be blended must be 5 to 50 parts by weight per 100 parts by weight of polymer compound 27. The amount of thickener 26 to be blended must be 50 to 200 parts by weight per 100 parts by weight of polyhydric alcohol 25. This allows the thickened polyhydric alcohol 25 to spread onto the surface of polymer compound 27, making the two difficult to separate. Here, the reason why polyhydric alcohol 25 thickens is that thickener 26 and polyhydric alcohol 25 form hydrogen bonds.

[0019] The amounts of polyhydric alcohol 25 and thickener 26 to be mixed are not particularly limited as long as the polyhydric alcohol 25 wets the entire surface of the pellets of polymer compound 27 when mixture 22A is fed into kneading device 30 and no gravity separation is caused.

[0020] As the polyhydric alcohol 25, glycols such as ethylene glycol and 1,4-butanediol are preferably used. Two or more kinds of these polyhydric alcohols 25 can be used. However, one or more kinds of the blended polyhydric alcohols 25 are selected that have a boiling point higher than the heating and kneading temperature of the polymer compound 27 so that the molded product of the melt of the composed polymer composite material does not have molding defects.

[0021] The thickener 26 is preferably a clay mineral-based substance that exfoliates into a single layer and disperses in the liquid when added to the polyhydric alcohol 25, and kaolinite in particular can provide a high thickening effect. Other examples of the thickener 26 that can be used include pectin, carrageenan, xanthan gum, galactomannans, gum arabic, methylcellulose, hydroxypropylmethylcellulose (HPMC), carboxymethylcellulose (CMC), and gelatin. Furthermore, the thickener 26 is not limited to one type, and two or more types may be mixed and used.

[0022] The polymer compound 27 may be either a thermoplastic resin that melts when heated or a thermosetting resin that hardens when heated. Thermoplastic resins include polyolefin resins such as low-density polyethylene (LDPE), high-density polyethylene (HDPE), and polypropylene (PP) that are molded into pellets, polycarbonate resin (PC), polyethylene terephthalate resin (PET), acrylic-butylene-styrene (ABS), polyvinyl chloride (PVC), polystyrene (PS), and polyamide (PA), as well as biodegradable plastics such as polybutylene adipate-butylene terephthalate copolymer (PBAT) and polylactic acid (PLA), which are decomposed into water and carbon dioxide by the power of microorganisms in the soil. Any thermoplastic resin that has the property of being thermo-flowable when heated and can generally be extruded may be used without any particular limitation. In addition, two or more of these thermoplastic resins may be mixed and used.

[0023] Furthermore, it can be used to recycle waste plastics that have been degraded by heat history or ultraviolet rays, which were previously difficult to recycle. In addition, it can be used to recycle waste plastics that contain thermoplastic resins, such as laminated films, composite films, and scraps of laminated composite films that were previously discarded without being recycled.

[0024] In addition, synthetic polymer compounds made from substances that fix carbon dioxide in the atmosphere can be used as the polymer compounds 27. Molded products of the melt of polymer composite materials composed of these polymer compounds 27 have zero carbon dioxide emissions, which contributes greatly to reducing carbon dioxide emissions from plastic products.

[0025] Furthermore, the polymer compound can be a natural polymer compound. In particular, whey protein or casein protein contained in by-products and waste products of dairy products, or / and soy protein contained in by-products and waste products of soy products are preferably used. When these natural polymer compounds are used in combination with a polymer compound, a polymer alloy with excellent moldability and high elasticity is composed. This makes it possible to significantly reduce the amount of thermoplastic resin derived from fossil resources, which contributes greatly to reducing carbon dioxide emissions from plastic products.

[0026] The mixture 22 delivered from the raw material mixer 20A is fed into the kneader 30 by the raw material feeder 19. The fed mixture 22 is heated to a temperature equal to or higher than the thermal flow temperature of the polymer compound 27, becomes a molten kneaded body 23, and is removed from the kneader 30. The removed molten kneaded body 23 is cooled and solidified into a polymer composite material in which the polyhydric alcohol 25 hydrogen-bonded with the thickener 26 forms a continuous phase together with the polymer compound 27. This gives the polymer composite material a higher melt tension than the polymer compound 27.

[0027] Second embodiment Next, a second embodiment of the present invention will be described with reference to Fig. 2. Fig. 2 is a side view of a production system 10B for a resin composite material according to the second embodiment of the present invention. The production system 10B of the second embodiment has a configuration in which a fourth container 18 for accommodating a filler 28 is further added to the configuration of the first embodiment described above in a raw material mixing device 20B. In Fig. 2, parts having the same configuration or function as Fig. 1 are indicated by the same reference numerals, and duplicated explanations will be omitted.

[0028] The filler 28 is added after the polymer compound 27, the polyhydric alcohol 25, and the thickener 26 are mixed in the mixing tank 12, and mixed to form a mixture 22B. The amount of the filler 28 added is an amount that allows the thickened polyhydric alcohol 25 to sufficiently wet the surface of the filler 28. The mixture 22B is then added to the kneading device 30 by the raw material supply device 19, heated to a temperature equal to or higher than the thermal flow temperature of the polymer compound 27, and taken out as a molten kneaded body 23. The polymer composite material obtained by cooling and solidifying the taken-out molten kneaded body 23 has the polyhydric alcohol 25 and the polymer compound 27 forming a continuous phase. Furthermore, a dispersed phase of the filler 28 strongly bonded to the polyhydric alcohol 25 contained in the continuous phase is formed in this polymer composite material.

[0029] A hydrophobic powder or fibrous material can be suitably used as the filler 28. This is because a hydrophobic powder or fibrous material requires a smaller amount of thickened polyhydric alcohol 25 to sufficiently wet the surface of the filler 28, compared to a hydrophilic one. Also, as the filler 28, a coarsely ground material of about 2 to 3 cm or a bulk solid material can be used as long as it can be pulverized in the kneading process.

[0030] Furthermore, the filler 28 can be made of underutilized resources such as dried waste. The combustion residue is preferably ash generated during the use of energy such as coal-fired power generation, wood biomass power generation, and solid fuels (RDF and RPF). Also, cinders such as coal husks, ash dregs, waste incineration ash, furnace cleaning emissions, coke ash, and heavy oil combustion ash can be used. Also, soot dust such as dust collected by an electric dust collector, dust collected by a bag filter, and dust collected by a cyclone can be used. Furthermore, soot dust collected from automobile air filters can be used. At this time, the polymer compounds used in the filters can be recycled at the same time.

[0031] Other waste materials include metal scrap such as scrap iron, empty cans, scrap, tinplate, galvanized iron, foil, lead pipes, copper wire, iron powder, burrs, cutting waste, grinding waste, turning powder, solder sludge, and welding waste; slag from blast furnaces, open hearths, converters, and electric furnaces; slag such as cupola smelting furnace slag, dross, slag, spices, defective ore, powdered coal sludge, waste casting sand, waste sand from sandblasting, and molten and solidified incineration ash; debris such as concrete fragments, asphalt fragments, and other similar waste materials; glass waste such as empty bottles, scrap plate glass, ampoule loss, broken glass, glass fiber scrap, cullet scrap, and glass powder; concrete waste such as concrete block scrap and interlocking scrap generated during the manufacturing process; earthenware scrap, ceramic scrap, stoneware scrap, porcelain scrap, and plasterwork scrap. Ceramic waste such as gypsum waste, insulating brick waste, gypsum molds, brick fragments, and tile fragments, gypsum boats, cotton waste, wool waste, hemp waste, thread waste, cloth waste, cotton waste, waste, fallen hair, fine dust, kudzu cocoons, rayon waste, etc., fiber waste from construction sites, fiber waste such as rope, cutting waste, shredded waste, rubber waste such as rubber-coated cloth waste, printing waste, bookbinding waste, shredded waste, old carbonless paper, etc. Materials that can be used include: wrapping paper for building materials, paperboard, paper waste such as waste paper generated from construction sites, waste wood from buildings, bridges, utility poles, construction sites, and boarding houses related to the construction industry (including felled timber and roots generated at construction sites), waste wood from the lumber and wood product manufacturing industries, sawdust, bark, packaging waste, scrap boards, waste chips, waste wooden furniture related to the goods rental business, and wood waste such as wooden pallets related to cargo distribution.

[0032] Even if these fillers 28 contain harmful substances, the dispersed phase of the filler 28 is strongly bound to the polyhydric alcohol 25 which forms a continuous phase together with the polymer compound 27, so that the harmful substances will not elute from the molded product of the polymer composite material. Furthermore, waste materials containing polymer compounds with poor thermal fluidity, such as waste urethane, waste bakelite (printed circuit boards, etc.), waste synthetic building materials (tiles, heat insulation materials, synthetic wood, soundproofing materials, etc.), and waste FRP, can be used as the filler 28. Note that these fillers 28 are preferably used as powder or fibrous bodies by appropriately pulverizing or other processing depending on their shape and properties.

[0033] Furthermore, a layered compound can be used as the filler 28. As the layered compound, graphite, in which the layers are bonded by weak van der Waals forces, transition metal sulfides such as TiS2·TaS2·MoS2·WS2, and selenium compounds are preferably used. Furthermore, as the layered compound, an ion-exchangeable layered oxyacid salt in which exchangeable ions exist between the layers can be used. As the ion-exchangeable layered oxyacid salt, in addition to silicates such as montmorillonite, vermiculite, and beidellite, phosphates, titanates, niobates, titanoniobates, vanadates, tungstates, molybdate layered perovskites, and the like can be used. A molded product in which the layered compound (filler 28) is two-dimensionally dispersed in a continuous phase formed by the polymer compound 27 and the polyhydric alcohol 25 becomes a nanocomposite with improved rigidity, gas barrier properties, electrical conductivity, and heat resistance depending on the properties of the layered compound (filler 28).

[0034] The mixture 22B sent from the raw material mixer 20B is fed into the kneader 30 by the raw material feeder 19. The fed mixture 22B is heated to a temperature equal to or higher than the thermal flow temperature of the polymer compound 27, becomes a molten kneaded body 23, and is taken out of the kneader 30. The polymer composite material is cooled and solidified into pellets, and after being distributed on the market, it is heated and remelted in an injection molding machine (extruder) and then injected into a mold to form a bulk molded product, or stretched (for example, an inflation method, a calendar processing method, a T-die method, a blowing method, etc.) to form a sheet or film molded product, or foamed to form a foam molded product, and thus serves as a raw material for producing general polymer processing moldings.

[0035] According to the first embodiment of the invention, it is possible to recycle polymer compounds that have been considered difficult to recycle, such as degraded waste plastics and scraps of multi-layer composite films. It also makes it possible to turn multiple polymer compounds that undergo phase separation into polymer alloys.

[0036] According to the invention of the second embodiment, by further including a step of mixing a filler in addition to the first embodiment, a polymer composite material in which the filler is finely and uniformly dispersed by the action of the polyhydric alcohol can be obtained. This provides a manufacturing technology for a polymer composite material that promotes the utilization of waste, which is an underutilized resource, and highly expresses the function of the filler. EXAMPLES

[0037] 3 is a table showing Example 1 and Comparative Example 1 in which the effect of the first embodiment was confirmed using melt tension as an index. Here, melt tension is the tension generated when a heated and molten resin is pulled, and is used to evaluate molding processes such as spinnability and blow moldability. The measurement device used was a Capillograph ID PMD-C manufactured by Toyo Seiki Seisakusho Co., Ltd., and melt tension (mN) was measured for the Examples and Comparative Examples under conditions of capillary shape (L / D=20, φ1), test temperature of 190° C., and extrusion speed of 10 mm / min, while keeping the pulling speed constant at 5 m / min, 10 m / min, and 20 m / min.

[0038] Here, Example 1 is a polymer composite material produced by the manufacturing method of the first embodiment, and Comparative Example 1 is the polyethylene used in Example 1. The polymer composite material of Example 1 is a mixture of a polymer compound (polyethylene): a polyhydric alcohol (ethylene glycol): and a thickener (kaolinite) in a weight ratio of 80:10:10.

[0039] Thus, the polymer composite material of Example 1, in which the polyhydric alcohol thickened with a thickener and the polymer compound form a continuous phase, has an increased melt tension compared to Comparative Example 1, in which the polymer compound is 100%, despite the fact that the blending ratio of the polymer compound is 80%. Also, a tendency was observed in which the rate of increase in melt tension increased as the take-up speed increased, and it is clear that Example 1 has improved moldability compared to Comparative Example 1.

[0040] 4 is a table showing Example 2 and Comparative Example 2, in which the effects of the second embodiment were confirmed using mechanical strength characteristics as an index. Here, Example 2 is a polymer composite material produced by the manufacturing method of the second embodiment, and Comparative Example 2 is a repelletized version of the polyethylene used in Example 2. This polymer composite material of Example 2 is a blend of polymer compound (polyethylene): polyhydric alcohol (ethylene glycol): thickener (kaolinite): and wood biomass ash in a weight ratio of 50:5:5:40. The wood biomass ash is ash generated from wood biomass power generation.

[0041] The polymer composite material of Example 2, in which the filler was dispersed in the presence of a polyhydric alcohol, had improved mechanical strength properties even though the blending ratio of the polymer compound was 50%, compared to Comparative Example 1, in which the blending ratio was 100%. This is believed to be due to the synergistic effect of the continuous phase with increased melt tension and the dispersed phase formed of wood biomass ash with a large aspect ratio.

[0042] However, when waste materials such as incineration ash are used as fillers, there is a concern that harmful substances contained therein may leach out from the polymer composite material. The table below shows the results of the leach test of the polymer composite material of Example 2. The method for preparing the test solution is in accordance with "H3 Environmental Notification No. 46, Environmental Standards for Soil Contamination, Appendix." ND indicates that the content is below the lower limit of quantification.

[0043] As shown by these results, no elution of harmful components contained in wood biomass ash was detected. Thus, in the polymer composite material according to the second embodiment, the polyhydric alcohol adheres closely to the interface of the filler, and further, this polyhydric alcohol forms a continuous phase with the polymer compound, which is thought to suppress the elution of trace components of the filler.

[0044] (No.; Analysis date; Analysis result; Reference value; Analysis method) 1;Chloroethylene;ND(less than 0.0002mg / L);0.002mg / L or less;Appendix to H9 Environmental Notification No. 10 2; Carbon tetrachloride; ND (less than 0.0002 mg / L); 0.002 mg / L or less; JIS K 0125 5.2 3;1.2-Dichloroethane;ND(less than 0.0004mg / L);0.004mg / L or less;JIS K 0125 5.2 4;1,1-Dichloroethylene;ND(less than 0.01mg / L);0.1mg / L or less;JIS K 0125 5.2 5;1,2-Dichloroethylene;ND(less than 0.004mg / L);0.04mg / L or less;JIS K 0125 5.2 6;1,3-Dichloropropene;ND(less than 0.0002mg / L);0.002mg / L or less;JIS K 0125 5.2 7;Dichloromethane;ND(less than 0.002mg / L);0.02mg / L or less;JIS K 0125 5.2 8;Tetrachloroethylene;ND(less than 0.001mg / L);0.01mg / L or less;JIS K 0125 5.2 9; 1,1,1-trichloroethane; ND (less than 0.01 mg / L); 1 mg / L or less; JIS K 0125 5.2 10;1,1,2-trichloroethane;ND(less than 0.0006mg / L);0.006mg / L or less;JIS K 0125 5.2 11;Trichloroethylene;ND(less than 0.001mg / L);0.01mg / L or less;JIS K 0125 5.2 12;Benzene;ND(less than 0.001mg / L);0.01mg / L or less;JIS K 0125 5.2 13;Cadmium and its compounds;ND (less than 0.0003mg / L);0.003mg / L or less;JIS K 0102 55.3 14;Hexavalent chromium compounds;ND(less than 0.005mg / L);0.05mg / L or less;JIS K 0102 65.2.4 15; Cyanide compounds; Not detectable (less than 0.1 mg / L); Not detectable; JIS K 0102 38.5 16; Mercury and its compounds; ND (less than 0.0005mg / L); 0.0005mg / L or less; S46 Environmental Notification No. 59, Appendix 2 17; Alkyl mercury compounds; Not detected (less than 0.0005mg / L); Not detected; S46 Environmental Notification No. 59, Appendix 3 18; Selenium and its compounds; ND (less than 0.001 mg / L); 0.01 mg / L or less; JIS K 0102 67.3 19; Lead and its compounds; 0.003mg / L; 0.01mg / L or less; JIS K 0102 54.2 20;Arsenic and its compounds;ND (less than 0.001mg / L);0.01mg / L or less;JIS K 0102 61.3 21;Fluorine and its compounds;0.18mg / L;0.8mg / L or less;JIS K 0102 34.4 22;Boron and its compounds;ND (less than 0.1mg / L);1mg / L or less;JIS K 0102 47.3 23; Simazine; ND (less than 0.0003 mg / L); 0.003 mg / L or less; S46 Environmental Notification No. 59, Appendix 6, No. 1 24; Thiobencarb; ND (less than 0.002 mg / L); 0.02 mg / L or less; S46 Environmental Notification No. 59, Appendix 6, No. 1 25; Thiuram; ND (less than 0.0006mg / L); 0.006mg / L or less; S46 Environmental Notification No. 59, Appendix 5 26; Polychlorinated biphenyls (PCBs); Not detected (less than 0.0005 mg / L); Not detected; S46 Environmental Notification No. 59, Appendix 4 27;Organophosphorus compounds;Not detected (less than 0.1mg / L);Not detected;S49 Environmental Notification No.64 Appendix 1 28;1,4-Dioxane;ND(less than 0.005mg / L);0.05mg / L or less;S46 Environmental Notification No.59 Appendix 8

[0045] (No.; Analysis date; Analysis result; Reference value; Analysis method) 1;Cadmium and its compounds;ND (less than 4.5mg / kg);45mg / kg or less;JIS K 0102 55.3 2;Hexavalent chromium oxide;ND(less than 25mg / kg);250mg / kg or less;JIS K 0102 65.2.4 3; Cyanide compounds g; ND (less than 5.0 mg / kg); 50 mg / kg or less; JIS K 0102 38.3 4; Mercury and its compounds; ND (less than 1.5mg / kg); 15mg / kg or less; S46 Environmental Notification No. 59, Appendix 2 5; Selenium and its compounds; ND (less than 15mg / kg); 150mg / kg or less; JIS K 0102 67.3 6; Lead and its compounds; ND (less than 15mg / kg); 150mg / kg or less; JIS K 0102 54.3 7;Arsenic and its compounds;ND (less than 15mg / kg);150mg / kg or less;JIS K 0102 61.3 8;Fluorine and its compounds;ND (less than 400mg / kg);4000mg / kg or less;JIS K 0102 34.4 9;Boron and its compounds;ND (less than 400mg / kg);4000mg / kg or less;JIS K 0102 47.3 [Explanation of symbols]

[0046] Reference Signs List 10A... manufacturing system, 10B... manufacturing system, 12... mixing tank, 15... first container, 16... second container, 17... third container, 18... fourth container, 19... raw material supply device, 20 (20A, 20B)... raw material mixing device, 22 (22A, 22B)... mixture, 23... molten kneaded body, 25... polyhydric alcohol, 26... thickener, 27... polymer compound, 28... filler, 30... kneading device, 31... hopper, 32... drive unit, 33... cylinder, 35... die unit.

Claims

1. a step of adding and mixing a polyhydric alcohol into a polymer compound, and then adding and mixing a thickener that increases the viscosity of the polyhydric alcohol to form a mixture in which the polyhydric alcohol with increased viscosity is spread over the polymer compound; The mixture is put into a sealed container and heated and kneaded to form a molten kneaded body, The polymer compound is a thermoplastic resin, The polyhydric alcohol is ethylene glycol, The method for producing a polymer composite material, wherein the thickening agent is kaolinite.

2. The method for producing a polymer composite material according to claim 1, A method for producing a polymer composite material, comprising the step of further mixing a filler with the mixture.

3. The method for producing a polymer composite material according to claim 1 or 2, A method for producing a polymer composite material, wherein the heating and kneading temperature is set lower than the boiling point of the polyhydric alcohol.

4. A polymer composite material comprising a polyhydric alcohol, a thickener for increasing the viscosity of the polyhydric alcohol, and a polymer compound, a dispersed phase of the thickener bound to the polyhydric alcohol is formed in a continuous phase formed of the polymer compound and the polyhydric alcohol; The polymer compound is a thermoplastic resin, The polyhydric alcohol is ethylene glycol, The polymeric composite, wherein the thickening agent is kaolinite.

Citation Information

Patent Citations

  • Preparation method for regenerated nanometer flame retardant plastic

    CN103483623A

  • Plastic film for food packaging bags

    CN106243450A

  • JP1975097191A

  • Arrangement for valve used in internallcombustion engine

    JP1980084807A

  • Dispersion, production method, rubber composition and pneumatic tire

    JP2020012069A