Emulsion composition for wood boards

By combining EVA, SBR, and acrylic emulsions with fillers, the adhesive composition achieves durability in low-temperature environments, passing structural laminated wood tests and suitable for laminated wood and wood boards.

JP7562356B2Inactive Publication Date: 2024-10-07AICA KOGYO CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020162953
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-29
Publication Date
2024-10-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Water-based vinyl urethane compositions fail to demonstrate good durability in low-temperature environments, such as 5°C, when used in laminated wood applications.

Method used

Incorporating specific ratios of EVA, SBR, and acrylic emulsions, along with fillers and additives, to enhance adhesive performance and stability in low-temperature conditions.

Benefits of technology

The emulsion composition ensures passing the vacuum pressure peeling test at low temperatures, enabling its use in laminated wood and various wood boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562356000001
    Figure 0007562356000001
  • Figure 0007562356000002
    Figure 0007562356000002
  • Figure 0007562356000003
    Figure 0007562356000003
Patent Text Reader

Abstract

To provide an emulsion composition that can give a good result when a water-based vinyl urethane (water vinyl) is prepared finally and even when a durability test is performed on the material of Japanese cypress, Scotch pine or the like using a test piece prepared in a low temperature environment such as 5°C or the like.SOLUTION: The problem is solved by obtaining an emulsion composition for wooden board that is characterized by containing, of 100 pts.mass of solid content, EVA emulsion (A) by 0.5 to 50 pts.mass in terms of solid content, SBR emulsion (B) by 0.5 to 33 pts.mass in terms of solid content, and acryl-based emulsion (C) by 0.5 to 50 pts.mass in terms of solid content.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an emulsion composition which, when a water-based vinyl urethane (WAU) composition is finally produced, can give good results even when a durability test is carried out using test pieces made of materials such as Japanese cypress and Scots pine at a low temperature environment such as 5°C. [Background technology]

[0002] The wooden materials used in buildings include solid wood and laminated wood. Laminated wood is made by gluing together small pieces of wood, and because of this manufacturing method, it has the advantage of being less prone to warping compared to solid wood. It is also sold at a lower price than solid wood, and is widely used in various buildings. Examples of laminated timber include structural laminated timber, joinery laminated timber, decorative joinery laminated timber, and decorative structural laminated columns.

[0003] Laminated wood is bonded with various compositions, some of which use water-based vinyl urethane (aqueous vinyl urethane). Water-based vinyl urethane is a composition that has been developed by mixing an emulsion with hydroxyl-containing molecules with an isocyanate compound, evaporating the water and solidifying it, while at the same time reacting the hydroxyl-containing molecules with the isocyanate compound, increasing the molecular weight from the original and obtaining a stronger van der Waals force. Compared to non-reactive types, this composition has higher adhesive strength and does not peel off even when subjected to various durability tests, resulting in improved adhesive performance.

[0004] Since the water is evaporated and solidified, and at the same time the molecules containing hydroxyl groups react with the isocyanate compound, the evaporation of water is faster and the reaction between the molecules containing hydroxyl groups and the isocyanate compound is also faster if the test specimen is obtained at room temperature such as 23°C or at a higher temperature. However, although the environment in which laminated timber is produced is kept relatively clean, it is rare for the temperature to be kept constant all year round. Generally, laminated timber is produced in a high temperature environment of around 30°C in summer and a low temperature environment of around 5°C in winter. In particular, laminated timber is required to exhibit stable adhesive performance even when produced in a low temperature environment of around 5°C in winter, when evaporation of water and reaction between molecules containing hydroxyl groups and isocyanate compounds are slow.

[0005] Patent Document 1 is a publication about a resin emulsion and adhesive applications that does not contain plasticizers suspected of being environmental hormones, does not emit formaldehyde or styrene, which are pointed out as volatile chemical substances (hereinafter abbreviated as VOCs), has excellent adhesive strength, water resistance, heat resistance, and storage stability, and can be used for bonding woodwork, plywood, laminated lumber, etc., or for secondary processing such as bonding veneer, decorative paper, etc. to various substrates such as plywood and particle board. There was room for improvement regarding the types of emulsions.

[0006] Patent Document 2 is a publication that describes how the use time of an aqueous emulsion-isocyanate compound or an isocyanate polymer can be significantly extended by using a surfactant. Patent Document 3 is a publication about a bulky and elastic adhesive material made of a water-containing polyurethane containing an adhesive component. Both publications list various emulsions in the specification, but do not show examples of combining these emulsions.

[0007] Patent Document 4 relates to a lightweight elastic composition, and more specifically, to a lightweight elastic composition that can be used as a repair material for concrete structures or a cushioning joint material for the joints of concrete structures, and Patent Document 5 is a publication on a two-liquid separately applied water-based adhesive and adhesion method that allows for short-time adhesion and also has excellent water resistance, which is required for structural members. In both publications, various emulsions are used in the examples, but there is room for improvement in the combinations. Aqueous emulsion-isocyanate-based compound or isocyanate-based polymer that can significantly extend the use time of the aqueous emulsion-isocyanate-based compound or isocyanate-based polymer that can significantly extend the use time of the aqueous emulsion-isocyanate-based compound or isocyanate-based polymer [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent Publication No. 2006-273889 [Patent Document 2] Patent Publication 50-069134 [Patent Document 3] Patent Publication 51-131546 [Patent Document 4] Patent Publication No. 2001-89678 [Patent Document 5] Patent Publication No. 2010-229397 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0009] The object of the present invention is to provide an emulsion composition which, when a water-based vinyl urethane (WV) composition is finally produced, can give good results even when a durability test is carried out using test pieces made of materials such as Japanese cypress and Scots pine in a low-temperature environment such as 5°C. [Means for solving the problem]

[0010] The present inventors have succeeded in obtaining an emulsion composition for wood boards, characterized in that, per 100 parts by mass of solid content, the composition contains 0.5 to 50 parts by mass of EVA emulsion (A), 0.5 to 33 parts by mass of SBR emulsion (B), and 0.5 to 50 parts by mass of acrylic emulsion (C). Effect of the Invention

[0011] The adhesive composition of the present invention is an emulsion composition that, when the final aqueous vinyl urethane (APU) composition is prepared, passes the reduced pressure and pressure peel test (usage environment B) of the JAS standard for structural laminated lumber using test specimens made from materials such as cypress and Scots pine at a low temperature environment of, for example, 5°C. Therefore, the adhesive composition can be used as an adhesive emulsion composition for various types of wood boards, as well as for laminated lumber. BEST MODE FOR CARRYING OUT THEINVENTION

[0012] The present invention will be described in detail below.

[0013] As the ethylene vinyl acetate (EVA) emulsion (A), a commercially available product can be used. The amount of the EVA emulsion (A) added is 0.5 to 50 parts by mass, more preferably 1 to 40 parts by mass, of 100 parts by mass of solid content.

[0014] As the styrene-butadiene rubber (SBR) emulsion (B), commercially available products can be used. The amount of the SBR emulsion (B) added is 0.5 to 33 parts by mass, more preferably 1 to 20 parts by mass, of 100 parts by mass of solid content.

[0015] The acrylic emulsion (C) may be a commercially available product. In addition to (meth)acrylic acid (ester), a component that can be copolymerized with (meth)acrylic acid (ester) may be included. The amount of the acrylic emulsion (C) added is 0.5 to 50 parts by mass, more preferably 1 to 40 parts by mass, of 100 parts by mass of solid content.

[0016] Polyvinyl alcohol (PVA) can be added as a moisturizing agent to the emulsion composition for wooden boards of the present invention. Commercially available PVA can be used. When PVA is added, the amount of PVA added is 0.5 to 20 parts by mass, more preferably 1 to 7 parts by mass, per 100 parts by mass of solid content.

[0017] The emulsion composition for wood boards of the present invention can contain inorganic fillers such as calcium carbonate, talc, silica, kaolin, calcined kaolin, clay, calcium silicate, calcium sulfate, aluminum oxide (alumina), aluminum hydroxide, aluminum silicate, titanium oxide, zinc oxide, magnesium carbonate, magnesium silicate, zeolite, glass beads, and shirasu balloons. In addition, organic fillers such as polyethylene, polypropylene, polymethyl methacrylate, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, ethylene-vinyl acetate copolymer, nylon, polyethylene terephthalate, polybutylene terephthalate, polystyrene, ABS resin, acrylonitrile-styrene copolymer, and polycarbonate can also be added. A more preferred filler is calcium carbonate, and commercially available calcium carbonate can be used. Commercially available products include Softon 1200 White, Hakuenka CC, and Lighton A from Shiraishi Calcium Co., Ltd., and Super S, Super SS, and Super SSS from Maruo Calcium Co., Ltd. The amount of calcium carbonate to be added is 30 to 70 parts by mass, more preferably 35 to 65 parts by mass, per 100 parts by mass of solid content.

[0018] A dispersant can be added to the emulsion composition for wood boards of the present application in order to improve the dispersibility of the filler. A commercially available dispersant can be added, and examples of commercially available dispersants include SN Dispersant 2060, Nopco Sant R, and Nopco Sperse 6150 sold by San Nopco Ltd. The amount of dispersant added is 0.05 to 1 part by mass, more preferably 0.2 to 0.8 parts by mass, per 100 parts by mass of solid content.

[0019] A defoaming agent can be added to the emulsion composition for wooden boards of the present application. A commercially available defoaming agent can be used. Commercially available defoaming agents are sold by San Nopco under the trade names SN Deformer AP, SN Deformer S, and Nopco 267-A. The amount of defoaming agent added is 0.05 to 0.5 parts by mass, more preferably 0.1 to 0.3 parts by mass, relative to a total of about 164 parts by mass of the emulsion composition for wooden boards. The defoaming agent is not counted as a solid content.

[0020] A preservative can be added to the emulsion composition for wood boards of the present application. A commercially available preservative can be used. Commercially available products include those sold by Saw Japan under the trade names ACTICIDE MV4, ACTICIDE MBS, and ACTICIDE MBZ. The amount of preservative added is 0.05 to 0.5 parts by mass, and more preferably 0.1 to 0.3 parts by mass, relative to a total of about 164 parts by mass of the emulsion composition for wood boards. The preservative is not included in the solid content.

[0021] The order of addition for obtaining the emulsion composition for wood boards is as follows: PVA is dissolved in water for dissolving PVA, and the filler is dispersed, then EVA emulsion (A), SBR emulsion (B), and acrylic emulsion (C) are added and stirred. Then, the defoamer, preservative, and water for viscosity adjustment are added and stirred to obtain the emulsion composition for wood boards.

[0022] Finally, an isocyanate component is added to the emulsion composition for wood boards and stirred to produce a laminated lumber as an aqueous vinyl urethane. The isocyanate component can be a commercially available isocyanate compound. Any isocyanate compound can be used, but from the viewpoint of availability, it is more preferable to use crude MDI. The amount of the emulsion composition for wood boards and the isocyanate compound is 10 to 20 parts by mass, more preferably 12 to 18 parts by mass, per 100 parts by mass of the solid content of the emulsion composition for wood boards.

[0023] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples. EXAMPLES

[0024] As an ethylene vinyl acetate (EVA) emulsion (A), a commercially available EVA emulsion 1 with a solid content of 65% was prepared. As styrene-butadiene rubber (SBR) emulsions (B), commercially available SBR emulsion 1 with a solid content of 50% and commercially available SBR emulsion 2 with a solid content of 50% were prepared. As the acrylic emulsion (C), commercially available acrylic emulsion 1 with a solid content of 50% and commercially available acrylic emulsion 2 with a solid content of 50% were prepared. In addition, commercially available PVA and commercially available crude MDI were prepared.

[0025] Preparation of emulsion composition for wood board according to Example 1 25.69g of water for dissolving PVA and 5.37g of PVA were weighed into a container, and the PVA was dissolved by stirring with a stirring motor. Next, 50.81g of Softon 1200 white calcium carbonate was weighed and stirred to disperse uniformly. Next, 51.02g of EVA emulsion 1 of ethylene vinyl acetate copolymer resin emulsion (A), 17.07g of SBR emulsion 1 of SBR emulsion (B), and 5.30g of acrylic emulsion 1 of acrylic emulsion (C) were added and stirred to make uniform. Next, 0.17g of SN DEFOAMER S as a defoamer, 0.17g of ACTICIDE MV4 as a preservative, and 5.52g of water for viscosity adjustment were added and stirred to make uniform, to obtain an emulsion composition for wooden boards of Example 1.

[0026] Preparation of Emulsion Compositions for Wood Boards of Examples 2 to 6 and Comparative Examples 1 to 3 Emulsion compositions for wood boards of Examples 2 to 6 and Comparative Examples 1 to 3 were obtained according to the procedure of Example 1 using the ratios shown in Tables 1 and 2. The values ​​in parentheses are solid contents, and the total is set to 100 parts by mass.

[0027] Preparation of aqueous vinyl urethane compositions 1 to 9 As shown in Tables 3 and 4, the emulsions for wooden boards in Examples 1 to 6 and Comparative Examples 1 to 3 with a solid content of 100 parts by mass and 15 g of crude MDI were mixed and homogenized with a stirring motor equipped with a stirring blade to prepare aqueous vinyl urethane compositions, which were then subjected to a reduced pressure and pressure peeling test according to the JAS standard for structural laminated lumber. This adjustment was made immediately before preparing the test specimens after the temperature adjustment of the wood was completed, as shown in the test specimen preparation method below.

[0028] Test piece preparation method Five pieces of Scots pine and Japanese cypress wood measuring 110mm x 300mm x 30mm were prepared and conditioned to 5℃. The test pieces were taken out to room temperature of 23℃, and four of the test pieces were coated with each water-based vinyl urethane at 250g / m2. The four pieces were then stacked, and finally a test piece that had not been coated with the water-based vinyl urethane was stacked on top of the other, pressed at 1MPa for 20 minutes, and removed. The test pieces were then placed again in a constant temperature bath at 5℃ and cured for 7 days. After curing, the test pieces were cut at a position 75 mm from the end of the long side, and used as test pieces for the reduced pressure peel test of the JAS standard for structural laminated timber.

[0029] Decompression and pressure peeling test for structural laminated timber (usage environment B) The test piece was immersed in water at about 23°C, decompressed to 0.085 MPa for 5 minutes, and then pressurized to 0.51±0.03 MPa for 1 hour. This treatment was repeated twice, and then the test piece was taken out of the water. The specimen was placed in a thermostatic oven at 70±3℃, and dried to a mass of 100-110% of the mass before the test, while being careful not to trap moisture in the oven. This operation is performed only once, as is the test method for the reduced pressure and pressure test (usage environment B) of the JAS standard for structural laminated timber.

[0030] JAS standard for structural laminated timber: Decompression and pressure peeling test criteria Five sheets of board material are stacked and glued together, so eight 110 mm adhesive layers of cured water-based vinyl urethane are observed. If peeling of 5% or more is not observed out of the total 880mm of the 110mm cured line, it is a pass, and if peeling of 5% or more is observed, it is a fail. Perform the test on three test pieces (n=3), and if peeling of 5% or more is not observed in any of them, it is a pass, and if peeling of 5% or more is observed in even one, it is a fail.

[0031] Between Scots pine and Japanese cypress, the test results tend to be worse for Scots pine and Japanese cypress. However, in Examples 1 to 6, which are emulsion compositions for wood boards characterized by containing 0.5 to 50 parts by solid mass of EVA emulsion (A), 0.5 to 33 parts by solid mass of SBR emulsion (B), and 0.5 to 50 parts by solid mass of acrylic emulsion (C) out of 100 parts by solid mass, when the aqueous vinyl urethane (A) compositions were finally prepared, all of them passed the reduced pressure and pressure peeling test (usage environment B) of the JAS standard for structural laminated lumber using test pieces made of materials such as cypress and Scots pine in a low temperature environment such as 5°C.

[0032] Of the EVA emulsion (A), SBR emulsion (B), and acrylic emulsion (C), Comparative Example 1, in which no acrylic emulsion (C) was added, Comparative Example 2, in which no SBR emulsion (B) was added, (A), and Comparative Example 3, in which no SBR emulsion was added, all failed the reduced pressure and pressure peeling test (usage environment B) of the JAS standard for structural laminated timber when the final aqueous vinyl urethane (AVI) compositions were prepared using test pieces made of materials such as cypress and Scots pine in a low temperature environment such as 5°C.

[0033] [Table 1]

[0034] [Table 2]

[0035] [Table 3]

[0036] [Table 4]

[0037] [Table 5]

[0038] [Table 6]

Claims

1. The aqueous vinyl urethane composition contains 5 to 25 parts by mass of crude MDI per 100 parts by mass of the solid content of an emulsion composition for wood board, the emulsion composition containing 0.5 to 50 parts by mass of EVA emulsion (A), 0.5 to 33 parts by mass of SBR emulsion (B), 0.5 to 50 parts by mass of acrylic emulsion (C), and 0.5 to 10 parts by mass of PVA as a moisturizing agent, out of 100 parts by mass of solid content.

2. The aqueous vinyl urethane composition according to claim 1, comprising 30 to 70 parts by mass of a filler and 0.05 to 1 part by mass of a dispersant, based on 100 parts by mass of the solid content of the emulsion composition for wood boards.

3. 3. The aqueous vinyl urethane composition of claim 2, wherein the filler is calcium carbonate.

Citation Information

Patent Citations

  • JP1975069134A

  • Adhesive materials with bulkiness and improved elasticity

    JP1976131546A

  • Adhesive composition

    JP1985055071A

  • Adhesive for decorative processing of veneer

    JP1993306383A

  • Adhesive for producing plywood and production of plywood by using the same

    JP1998121021A