Rubber products and their manufacturing method

By integrating hydrogen-containing fluororubber and polyvinylidene fluoride with a hydrogen site protecting agent, the composition addresses kneading issues in uncrosslinked rubber production, achieving enhanced processability and improved product properties for semiconductor applications.

JP7562465B2Active Publication Date: 2024-10-07MITSUBISHI CABLE INDUSTRIES LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021060302
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-31
Publication Date
2024-10-07
Estimated Expiration
2038-03-29

AI Technical Summary

Technical Problem

The low compatibility of organic peroxide and crosslinking aid with fluororubber results in slippage and embrittlement during kneading, leading to poor processability and potential interruption in the production of uncrosslinked rubber compositions, particularly for sealing materials used in semiconductor processing equipment.

Method used

Incorporating hydrogen-containing fluororubber, polyvinylidene fluoride, and a hydrogen site protecting agent into the rubber composition, along with organic peroxide and a crosslinking aid, enhances compatibility and processability by ensuring smooth kneading and preventing embrittlement.

Benefits of technology

The improved composition allows for efficient kneading and reduces the risk of slippage and embrittlement, resulting in superior processability and enhanced properties of the rubber products, including improved plasma resistance and reduced particle generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562465000001
    Figure 0007562465000001
Patent Text Reader

Abstract

To provide an uncrosslinked rubber composition having excellent mixing workability.SOLUTION: An uncrosslinked rubber composition contains a hydrogen-containing fluorine rubber other than a polyvinylidene fluoride, as the main component of a rubber component, and contains an organic peroxide, a crosslinking aid, PVDF, and a hydrogen site protectant which is a compound that, when irradiated, binds to a radical of carbon derived from cutting of a carbon-hydrogen bond of the rubber component. The content of the organic peroxide is 0.5 pt.mass or more and 2.5 pts.mass or less with respect to 100 pts.mass of the rubber component. The content of the crosslinking aid is 1 pt.mass or more and 10 pts.mass or less with respect to 100 pts.mass of the rubber component. The PVDF is in a powder form and the content of it is 5 pts.mass or more and 30 pts.mass or less with respect to 100 pts.mass of the rubber component. The content of the hydrogen site protectant is 1 pt.mass or more and 20 pts.mass or less with respect to 100 pts.mass of the rubber component.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an uncrosslinked rubber composition, a rubber product produced using the same, and a method for producing the same. [Background technology]

[0002] In the field of semiconductor process equipment and the like, it is known to use sealing materials made of fluororubber (for example, Patent Documents 1 to 5). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 4381087 [Patent Document 2] Patent No. 4628814 [Patent Document 3] Patent No. 4778782 [Patent Document 4] Patent No. 6134391 [Patent Document 5] JP 2001-348462 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the preparation of an uncrosslinked rubber composition for producing rubber products such as fluororubber seals, when an organic peroxide and a crosslinking aid are added to the fluororubber of the rubber component and kneaded with a roll, the organic peroxide and the crosslinking aid become liquid, and since the compatibility of the organic peroxide and the crosslinking aid with the fluororubber is low, if the addition rate of them is not slowed down, the organic peroxide and the crosslinking aid that are not absorbed by the fluororubber adhere to the roll surface and function as a lubricant, causing slippage and preventing smooth kneading. In addition, since the fluororubber becomes brittle by absorbing the liquid organic peroxide and the crosslinking aid, it becomes difficult to keep the uncrosslinked rubber composition wound around the roll, and the uncrosslinked rubber composition may fall off the roll and kneading may be interrupted. Therefore, in the preparation of an uncrosslinked rubber composition for producing a rubber product made of fluororubber, there is a problem of poor kneading processability.

[0005] An object of the present invention is to provide an uncrosslinked rubber composition having excellent kneading processability. [Means for solving the problem]

[0006] The uncrosslinked rubber composition of the present invention contains a hydrogen-containing fluororubber other than polyvinylidene fluoride as a main component of a rubber component, and also contains an organic peroxide, a crosslinking aid, polyvinylidene fluoride, and a hydrogen site protecting agent which is a compound that bonds to a carbon radical generated when a carbon-hydrogen bond of the rubber component is broken when irradiated with radiation, wherein the content of the organic peroxide is 0.5 parts by mass or more and 2.0 parts by mass or less per 100 parts by mass of the rubber component, the content of the crosslinking aid is 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the rubber component, the polyvinylidene fluoride is in a powder form, the content of the polyvinylidene fluoride is 5 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the rubber component, and the content of the hydrogen site protecting agent is 1 part by mass or more and 20 parts by mass or less per 100 parts by mass of the rubber component.

[0007] The rubber product of the present invention is formed by crosslinking the rubber component in the uncrosslinked rubber composition of the present invention, and is formed from a rubber composition in which the hydrogen site protectant is bonded to the carbon of the rubber component.

[0008] The method for producing a rubber product of the present invention comprises heating the uncrosslinked rubber composition of the present invention to a predetermined temperature to crosslink the rubber component with the organic peroxide, and then irradiating the heated product with radiation. Effect of the Invention

[0009] According to the uncrosslinked rubber composition of the present invention, since it contains polyvinylidene fluoride, which has relatively high compatibility with organic peroxides and crosslinking aids, the polyvinylidene fluoride absorbs the organic peroxides and crosslinking aids and is smoothly kneaded with the rubber components, and the polyvinylidene fluoride suppresses embrittlement and provides reinforcement, resulting in excellent kneading processability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The embodiments will be described in detail below.

[0011] The uncrosslinked rubber composition according to the embodiment contains a hydrogen-containing fluororubber other than polyvinylidene fluoride (hereinafter referred to as "PVDF") as the main rubber component, and also contains an organic peroxide, a crosslinking aid, and PVDF. The uncrosslinked rubber composition according to the embodiment is suitably used for the manufacture of rubber products, particularly sealing materials such as O-rings used in semiconductor processing equipment that uses plasma, such as semiconductor etching equipment and plasma CVD equipment.

[0012] According to the uncrosslinked rubber composition of the embodiment, since it contains PVDF which has a relatively high compatibility with organic peroxides and crosslinking aids, the PVDF absorbs the organic peroxides and crosslinking aids and is smoothly kneaded with the rubber component, and the PVDF suppresses embrittlement and reinforces the rubber component, resulting in excellent kneading processability.

[0013] Here, the rubber component mainly contains hydrogen-containing fluororubber other than PVDF. In the present application, the "hydrogen-containing fluororubber" is a fluororubber containing carbon with hydrogen bonded to the main chain of the polymer. The content of the hydrogen-containing fluororubber other than PVDF in the rubber component is more than 50% by mass, and from the viewpoint of obtaining excellent physical properties, is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 100% by mass. In addition to the hydrogen-containing fluororubber other than PVDF, the rubber component may contain a hydrogen-free fluororubber such as a polymer (PTFE) of tetrafluoroethylene (TFE) or a silicone rubber.

[0014] Examples of hydrogen-containing fluororubbers other than PVDF include copolymers of vinylidene fluoride (VDF) and hexafluoropropylene (HFP) (binary FKM), copolymers of vinylidene fluoride (VDF), hexafluoropropylene (HFP), and tetrafluoroethylene (TFE) (ternary FKM), copolymers of tetrafluoroethylene (TFE) and propylene (Pr) (FEP), copolymers of vinylidene fluoride (VDF), propylene (Pr), and tetrafluoroethylene (TFE), copolymers of ethylene (E) and tetrafluoroethylene (TFE) (ETFE), copolymers of ethylene (E), tetrafluoroethylene (TFE), and perfluoromethylvinylether (PMVE), copolymers of vinylidene fluoride (VDF), tetrafluoroethylene (TFE), and perfluoromethylvinylether (PMVE), copolymers of vinylidene fluoride (VDF) and perfluoromethylvinylether (PMVE), and the like. It is preferable to use one or more of these hydrogen-containing fluororubbers other than PVDF, and from the viewpoint of obtaining excellent physical properties, it is more preferable to use one containing vinylidene fluoride (VDF) as a monomer, and it is even more preferable to use a ternary FKM. It is preferable that the hydrogen-containing fluororubber other than PVDF has iodine or bromine in the molecule, from the viewpoint of obtaining excellent physical properties.

[0015] The organic peroxide is a thermal crosslinking agent that crosslinks the rubber component when heated to a predetermined temperature. Examples of the organic peroxide include 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroperoxide, di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, α,α-bis(t-butylperoxy)-p-diisopropylbenzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3, benzoyl peroxide, t-butylperoxybenzene, t-butylperoxymaleic acid, t-butylperoxyisopropylcarbonate, and t-butylperoxybenzoate. It is preferable to use one or more of these organic peroxides, and from the viewpoint of obtaining excellent physical properties, it is more preferable to use 2,5-dimethyl-2,5-di(t-butylperoxy)hexane.

[0016] The content (A) of the organic peroxide is preferably 0.5 parts by mass or more and 2.5 parts by mass or less, and more preferably 0.5 parts by mass or more and 2.0 parts by mass or less, based on 100 parts by mass of the rubber component, in order to obtain excellent physical properties.

[0017] The crosslinking aid is a compound that bonds between the molecules of the rubber component when the rubber component is crosslinked by an organic peroxide. Examples of the crosslinking aid include triallyl cyanurate, trimethallyl isocyanurate, triallyl isocyanurate, triacrylformal, triallyl trimellitate, N,N'-m-phenylene bismaleimide, dipropargyl terephthalate, diallyl phthalate, tetraallyl terephthalate amide, triallyl phosphate, bismaleimide, fluorinated triallyl isocyanurate (1,3,5-tris(2,3,3-trifluoro-2-propenyl)-1,3,5-triazine, etc.). Examples of the crosslinking aid include tris(diallylamine)-S-triazine, triallyl phosphite, N,N-diallylacrylamide, 1,6-divindodecafluorohexane, hexaallyl phosphoramide, N,N,N',N'-tetraallylphthalamide, N,N,N',N'-tetraallylmalonamide, trivinyl isocyanurate, 2,4,6-trivinylmethyltrisiloxane, tri(5-norbornene-2-methylene)cyanurate, and triallyl phosphite. It is preferable to use one or more of these crosslinking aids, and from the viewpoint of obtaining excellent physical properties, it is more preferable to use triallyl isocyanurate.

[0018] The content of the crosslinking aid (B) is preferably 1 part by mass or more and 10 parts by mass or less, more preferably 2 parts by mass or more and 5 parts by mass or less, based on 100 parts by mass of the rubber component, from the viewpoint of obtaining excellent physical properties. The content of the crosslinking aid (B) is preferably more than the content of the organic peroxide (A), from the viewpoint of obtaining excellent physical properties. The ratio (B / A) of the content of the crosslinking aid (B) to the content of the organic peroxide (A) is preferably 1.0 or more and 4.0 or less, more preferably 2.0 or more and 3.0 or less, from the viewpoint of reacting the crosslinking aid without excess or deficiency and obtaining excellent physical properties.

[0019] PVDF may be contained so as to constitute a part of the rubber component, but from the viewpoints of improving the absorbency of organic peroxides and processing aids to obtain excellent kneading processability, and improving the tear strength of a rubber product using the uncrosslinked rubber composition according to the embodiment to obtain excellent crush resistance, it is preferable that PVDF is in a powder form and is dispersed in the rubber component.

[0020] However, for example, in a fluororubber seal material used in a semiconductor processing device, when the rubber component deteriorates due to use in a plasma atmosphere, the powder-like material with high plasma resistance dispersed therein remains, and the particles are released and contaminate the inside of the device. However, since PVDF has plasma resistance equivalent to that of hydrogen-containing fluororubbers other than PVDF in the rubber component, even if powdered PVDF is dispersed and contained in the rubber component, the generation of such particles can be suppressed. The average particle size of the powdered PVDF is preferably 1 μm or more and 100 μm or less from the viewpoint of obtaining excellent crush resistance of the rubber product.

[0021] The PVDF content (C) is 3 parts by mass or more and 9.8 parts by mass or less, preferably 5 parts by mass or more and 9.7 parts by mass or less, based on 100 parts by mass of the rubber component, from the viewpoint of obtaining excellent kneading processability and suppressing sink marks and obtaining excellent physical properties in a rubber product using the uncrosslinked rubber composition according to the embodiment. The PVDF content (C) is preferably equal to or more than the sum of the organic peroxide content (A) and the crosslinking auxiliary content (B) from the viewpoint of obtaining excellent kneading processability. The ratio (C / (A+B)) of the PVDF content (C) to the sum of the organic peroxide content (A) and the crosslinking auxiliary content (B) is preferably 0.5 to 6, more preferably 0.9 to 2.

[0022] The uncrosslinked rubber composition according to the embodiment may further contain a hydrogen site protecting agent. The hydrogen site protecting agent is a compound that bonds to a carbon radical generated when a carbon-hydrogen bond of a rubber component is broken when the rubber component is irradiated with radiation during the production of a rubber product.

[0023] The hydrogen site protective agent preferably contains a perfluoro-skeleton compound having an alkenyl group in the molecule that bonds to a carbon radical of the rubber component, and / or a siloxane-skeleton compound having an alkenyl group in the molecule that bonds to a carbon radical of the rubber component. Examples of the alkenyl group include vinyl, allyl, butenyl, pentenyl, hexenyl, and heptenyl groups. Of these, the alkenyl group is preferably a vinyl group.

[0024] Examples of the perfluoro skeleton compound having an alkenyl group in the molecule include a perfluoropolyether structure compound and a perfluoroalkylene structure compound. Examples of the siloxane skeleton compound having an alkenyl group in the molecule include a methylvinylsiloxane polymer, a dimethylsiloxane polymer, a copolymer of dimethylsiloxane and methylvinylsiloxane, and a copolymer of dimethylsiloxane, methylvinylsiloxane, and methylphenylsiloxane. Other examples include organopolysiloxanes containing an alkenyl group in the molecule, which are liquid silicone rubbers of addition polymerization. It is preferable to use one or more of these hydrogen site protecting agents.

[0025] In order to enhance plasma resistance, the amount of the hydrogen site protective agent is preferably 1 part by mass or more and 20 parts by mass or less, and more preferably 5 parts by mass or more and 15 parts by mass or less, per 100 parts by mass of the rubber component.

[0026] Depending on the rubber product to be manufactured, the uncrosslinked rubber composition according to the embodiment may contain reinforcing materials such as carbon black and silica, plasticizers, processing aids, vulcanization accelerators, antiaging agents, etc. However, when used in the manufacture of rubber products in which generation of particles in a plasma atmosphere is a problem, the content of powdery inorganic fillers such as carbon black, silica, metal oxides, etc. is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and most preferably 0 parts by mass, relative to 100 parts by mass of the hydrogen-containing fluororubber.

[0027] The uncrosslinked rubber composition according to the embodiment can be prepared using an open-type rubber kneader such as an open roll or an enclosed-type rubber kneader such as a kneader. Among these, particularly in an open-type rubber kneader such as an open roll, excellent kneading processability can be obtained.

[0028] Next, a method for producing a rubber product using the uncrosslinked rubber composition according to the embodiment will be described.

[0029] In the method for producing a rubber product, first, a predetermined amount of the uncrosslinked rubber composition according to the embodiment is filled into the cavity of a preheated mold, and then the mold is closed, and in that state, the composition is held at a predetermined molding temperature and a predetermined molding pressure for a predetermined molding time. At this time, the uncrosslinked rubber composition according to the embodiment is molded into the shape of the cavity, and the rubber component is crosslinked by the organic peroxide and loses plasticity. This molding may be press molding or injection molding. The molding temperature is, for example, 150°C or higher and 180°C or lower. The molding pressure is, for example, 0.1 MPa or higher and 25 MPa or lower. The molding time is, for example, 3 minutes or higher and 20 minutes or lower. Then, the mold is opened, and the molded product is taken out from the inside and cooled to obtain a rubber product. The molded product taken out of the mold may be further subjected to a heat treatment at a heating temperature of 150°C or higher and 250°C or lower and for a heating time of 2 hours to 6 hours.

[0030] In order to develop excellent crush resistance when the powdered PVDF is contained in the uncrosslinked rubber composition according to the embodiment, and to suppress cracking in a plasma atmosphere when a rubber product to be used in a plasma atmosphere is manufactured, it is preferable to irradiate the molded product after heating with radiation. In this case, the radiation irradiation causes crosslinking at the interface between the rubber component and PVDF, which are the starting points for cracking, and they are integrated, thereby inhibiting the growth of the crack.

[0031] Examples of radiation include α-rays, β-rays, γ-rays, electron beams, ions, etc. Of these, it is preferable to use electron beams or γ-rays as radiation. From the viewpoint of suppressing particle generation, the radiation exposure dose is preferably 10 kGy to 200 kGy, more preferably 20 kGy to 80 kGy. EXAMPLES

[0032] (Mixing of Uncrosslinked Rubber Composition and Preparation of Crosslinked Rubber Sheet) In each of the following Examples 1 to 6, Comparative Examples, and Reference Examples, an uncrosslinked rubber composition was kneaded and a crosslinked rubber sheet was prepared using the kneaded composition.

[0033] <Example 1> Using an 8-inch open roll, 1.5 parts by mass of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (Perhexa 25B, manufactured by Nippon Oil & Fats Co., Ltd.) as an organic peroxide, 4 parts by mass of triallyl isocyanurate (Taiku, manufactured by Nippon Kasei Co., Ltd.) as a crosslinking aid, 5 parts by mass of powdered PVDF (manufactured by Daikin Industries, Ltd., average particle size: 7 μm), and 10 parts by mass of a perfluoro skeleton compound having a vinyl group in the molecule of the hydrogen site protecting agent (I) (SIFEL3590-N, manufactured by Shin-Etsu Chemical Co., Ltd.) were added to the ternary FKM of the rubber component (Daiel G912, manufactured by Daikin Industries, Ltd.) per 100 parts by mass of the rubber component to prepare an uncrosslinked rubber composition. The kneading time required to obtain 4 kg of a uniform uncrosslinked rubber composition was 2.0 hours.

[0034] Next, this uncrosslinked rubber composition was press-molded at a molding temperature of 165°C, a molding pressure of 5 MPa, and a molding time of 15 minutes, and then heat-treated at a heating temperature of 200°C and a heating time of 4 hours to obtain a sheet-shaped rubber composition.

[0035] This sheet-like rubber composition was then irradiated with γ rays at an exposure dose of 30 kGy to obtain a crosslinked rubber sheet.

[0036] <Example 2> The same operation as in Example 1 was carried out, except that the rubber composition in sheet form obtained by heat treatment was used as a crosslinked rubber sheet without irradiating with gamma rays. The kneading time required to obtain 4 kg of a uniform uncrosslinked rubber composition was 2.0 hours.

[0037] <Example 3> The same operation as in Example 1 was carried out, except that the amount of powdered PVDF added was 10 parts by mass per 100 parts by mass of the rubber component. The kneading time required to obtain 4 kg of a uniform uncrosslinked rubber composition was 1.5 hours.

[0038] <Example 4> The same operation as in Example 1 was carried out, except that the amount of powdered PVDF added was 30 parts by mass per 100 parts by mass of the rubber component. The kneading time required to obtain 4 kg of a uniform uncrosslinked rubber composition was 1.0 hour.

[0039] <Example 5: Reference Example> The rubber component was a blend rubber containing 90% by mass of ternary FKM and 10% by mass of PVDF (manufactured by Daikin Industries, Ltd.), i.e., PVDF was contained so as to constitute a part of the rubber component, but the same operation as in Example 1 was performed. The kneading time required to obtain 4 kg of a uniform uncrosslinked rubber composition was 2.5 hours.

[0040] <Example 6> The same operation as in Example 1 was carried out, except that a siloxane skeleton compound having a vinyl group in the molecule of the hydrogen site protecting agent (II) (KE-1830, manufactured by Shin-Etsu Chemical Co., Ltd.) was added instead of the hydrogen site protecting agent (I). The kneading time required to obtain 4 kg of a uniform uncrosslinked rubber composition was 2.0 hours.

[0041] <Comparative Example> Except for not adding powdery PVDF, the same operation as in Example 1 was carried out. The kneading time required to obtain 4 kg of a uniform uncrosslinked rubber composition was 5.0 hours.

[0042] <Reference example> The same operation as in Example 1 was carried out, except that powdered PTFE (manufactured by Daikin Industries, Ltd., average particle size: 27 μm) was added instead of powdered PVDF. The kneading time required to obtain 4 kg of a uniform uncrosslinked rubber composition was 2.0 hours.

[0043] [Table 1]

[0044] (Test Method) <Plasma resistance> For the crosslinked rubber sheets prepared in each of Examples 1 to 6, Comparative Examples, and Reference Examples, an O2 plasma irradiation test and a CF4 plasma irradiation test were performed using a microwave plasma generator at an elongation rate of 10%, and mass loss, the presence or absence of cracks, and the presence or absence of particle generation were examined. In the tests, O2 and CF4 were used as reaction gases, and the flow rate ratio of the two was 50:1 in the O2 plasma irradiation test and 1:50 in the CF4 plasma irradiation test. The reaction pressure was 100 Pa and the plasma irradiation time was 60 minutes.

[0045] <Tensile properties> The crosslinked rubber sheets prepared in Examples 1 to 6, Comparative Example, and Reference Example were subjected to a tensile test based on JIS K6251, and the 100% modulus (M 100 The tensile strength (TB) and elongation at break (EB) were measured.

[0046] <Compression set> For each of the crosslinked rubber sheets prepared in Examples 1 to 6, Comparative Example, and Reference Example, compression set was measured at a test time of 72 hours and a test temperature of 200° C. according to JIS K6262:2013.

[0047] <40% crushing crack> The crosslinked rubber sheets prepared in each of Examples 1 to 6, Comparative Example, and Reference Example were subjected to a heat treatment at 150° C. for 24 hours, and then compressed by 40% to visually check for the presence or absence of cracks.

[0048] (Test Results) The test results are shown in Table 1.

[0049] According to Table 1, it is seen that in Examples 1 to 6 in which PVDF was added, the kneading time of the uncrosslinked rubber composition was half or less than that of the Comparative Example in which PVDF was not added, and therefore the kneading processability was excellent.

[0050] Comparing Examples 1 and 2, it can be seen that Example 1, which was irradiated with gamma rays after heat molding, has better O2 plasma resistance and crush resistance than Example 2, which was not irradiated with gamma rays. This is presumably because gamma ray irradiation causes crosslinking at the interface between the ternary FKM and PVDF, which are the rubber components that are the starting points for crack generation, and these are integrated, thereby inhibiting the growth of cracks.

[0051] Comparing Examples 1, 3, and 4, it is found that as the powdered PVDF content increases, the O2 plasma resistance tends to decrease, and the compression set also tends to increase.

[0052] Comparing Examples 3 and 5, it can be seen that Example 3, in which powdered PVDF was added, had better kneading processability and crush resistance because the kneading time was shorter than that of Example 5, in which PVDF was contained so as to constitute part of the rubber component.

[0053] Comparing Examples 1 and 6, it can be seen that the addition of either the hydrogen site protection agent (I) or the hydrogen site protection agent (II) does not affect the kneading processability, plasma resistance, physical properties, and crushing resistance, and thus exhibits excellent performance.

[0054] In the reference example in which powdered PTFE was added, excellent kneading processability was obtained, but plasma resistance and crush resistance were poor. This is presumably because PTFE has higher plasma resistance than the rubber component ternary FKM, so when the ternary FKM deteriorates, only the powdered PTFE remains, and even when irradiated with gamma rays, no crosslinking occurs between the rubber component ternary FKM and PTFE that does not contain hydrogen atoms bonded to carbon atoms. [Industrial Applicability]

[0055] INDUSTRIAL APPLICABILITY The present invention is useful in the technical fields of an uncrosslinked rubber composition, a rubber product produced using the same, and a method for producing the same.

Claims

1. A rubber product formed from a rubber composition in which a hydrogen-containing fluororubber other than polyvinylidene fluoride is used as a rubber component, an organic peroxide, a crosslinking aid, powdered polyvinylidene fluoride dispersed in the rubber component, and a perfluoro-skeleton compound having an alkenyl group in its molecule, or a siloxane-skeleton compound having an alkenyl group in its molecule are heated to a predetermined temperature, whereby the rubber component is crosslinked by the organic peroxide, and then irradiated with radiation, whereby carbon-hydrogen bonds in the rubber component are broken to generate carbon radicals to which the alkenyl group of the perfluoro-skeleton compound or the alkenyl group of the siloxane-skeleton compound is bonded, In the uncrosslinked rubber composition, a content of the organic peroxide is 0.5 parts by mass or more and 2.5 parts by mass or less based on 100 parts by mass of the rubber component, the content of the crosslinking aid is 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the rubber component, an amount of the powdered polyvinylidene fluoride per 100 parts by mass of the rubber component is 5 parts by mass or more and 30 parts by mass or less; a ratio of the content of the powdered polyvinylidene fluoride to the sum of the content of the organic peroxide and the content of the crosslinking aid is 0.9 or more and 2 or less, The rubber product has a content of the perfluoro skeleton compound or the siloxane skeleton compound in a range of 1 part by mass to 20 parts by mass per 100 parts by mass of the rubber component.

2. The rubber product according to claim 1, The powdered polyvinylidene fluoride has an average particle size of 1 μm or more and 100 μm or less.

3. The rubber product according to claim 1 or 2, The rubber product is a sealing material.

4. The method for producing a rubber product according to any one of claims 1 to 3, The uncrosslinked rubber composition is heated to a predetermined temperature to crosslink the rubber component with the organic peroxide, and the heated composition is irradiated with radiation to break carbon-hydrogen bonds in the rubber component to generate carbon radicals to which an alkenyl group of the perfluoro skeleton compound or an alkenyl group of the siloxane skeleton compound is bonded to form the rubber composition.

Citation Information

Patent Citations

  • Rotary pump

    JP1986034391A

  • Manufacture of wire and cable covered with elastomer containing fluorine

    JP1986206114A

  • Fluororubber composition

    JP1993117478A

  • Plasma resistant rubber composition and rubber material for plasma processing apparatus

    JP2001348462A

  • Milling method

    JP2014521820A