Polyolefin resin composition and molded article thereof
The polyolefin resin composition with fibrous basic magnesium sulfate and cellulose nanofibers addresses deformation and impact resistance, achieving high flexural modulus and Charpy impact strength with enhanced surface hardness.
Patent Information
- Application Number
- JP2022015040
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-02-02
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2042-02-02
AI Technical Summary
Molded articles made of resin compositions require improved resistance to deformation under bending and impact, along with enhanced surface hardness and scratch resistance.
A polyolefin resin composition containing an olefin polymer, fibrous basic magnesium sulfate, and cellulose nanofibers is developed, with specific ratios and treatments to enhance flexural modulus, Charpy impact strength, and surface hardness.
The composition results in molded articles with high flexural modulus, Charpy impact strength, and excellent surface hardness, maintaining integrity under bending and impact.
Smart Images

Figure 0007562584000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyolefin resin composition and a molded article thereof. [Background technology]
[0002] Cellulose fibers are attracting attention as a reinforcing material for resins because they are lightweight, have a high modulus of elasticity, and are strong. A resin composition has been proposed in which cellulose fibers with an average fiber diameter of 3 nm to 50 μm are dispersed in a thermoplastic resin (see, for example, Patent Document 1). It is described that by using this resin composition, a molded article with high mechanical properties can be produced.
[0003] Also, a composite resin composition has been proposed that contains cellulose nanofibers having a fiber diameter of 2 to 10 μm, a fiber length of 200 to 1000 μm, and an aspect ratio of about 100 to 200 (see, for example, Patent Document 2). It is described that a resin molded product made from this composite resin composition has high elastic modulus and impact resistance.
[0004] Furthermore, the fiber diameter distribution D 90 The fiber diameter is 5 μm or more, and D 10 A melt-kneaded product containing a cellulose fiber filler having a fiber diameter of 500 nm or less has been proposed (see, for example, Patent Document 3). It is described that the use of this melt-kneaded product allows the production of a composite resin molding having excellent mechanical strength and appearance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-143016 A [Patent Document 2] JP 2019-85529 A [Patent Document 3] Patent No. 6545145 Summary of the Invention [Problem to be solved by the invention]
[0006] A molded article made of a resin composition is required to have both resistance to deformation when bent and resistance to cracking when impacted. Furthermore, it is desirable for such a molded article to have excellent surface hardness and be resistant to scratches.
[0007] An object of the present invention is to provide a polyolefin resin composition which can give a molded article having high flexural modulus and Charpy impact strength and excellent surface hardness, and a molded article having high flexural modulus and Charpy impact strength and excellent surface hardness. [Means for solving the problem]
[0008] The polyolefin resin composition according to the present invention contains an olefin polymer, fibrous basic magnesium sulfate, and cellulose nanofibers in an amount 0.01 to 1.00 times the blend amount of the fibrous basic magnesium sulfate.
[0009] The molded article according to the present invention is a molded product of the above-mentioned polyolefin resin composition. Effect of the Invention
[0010] According to the present invention, it is possible to provide a polyolefin resin composition which can give a molded article having high flexural modulus and Charpy impact strength and excellent surface hardness, and a molded article having high flexural modulus and Charpy impact strength and excellent surface hardness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Through intensive research, the present inventors have discovered that by blending a predetermined amount of cellulose nanofibers with a polyolefin resin composition containing fibrous basic magnesium sulfate and an olefin polymer, it is possible to obtain a molded article having improved flexural modulus and Charpy impact strength without impairing surface hardness. Hereinafter, an embodiment of the present invention will be described in detail.
[0012] <Olefin polymer> Examples of the olefin polymer include ethylene polymer, propylene polymer, ethylene-propylene random copolymer, ethylene-propylene block copolymer, etc., and propylene polymer (polypropylene) is particularly preferred. As the propylene polymer, a propylene homopolymer or a propylene copolymer can be used. In terms of high impact resistance, a propylene block copolymer is more preferred as the propylene polymer.
[0013] The olefin polymer may be used alone or in combination of two or more. The melt flow rate (MFR) of the olefin polymer is usually in the range of 3 to 300 g / 10 min, and preferably in the range of 6 to 100 g / 10 min.
[0014] To prepare the resin composition, the blending amount of the olefin polymer is preferably in the range of 20 to 99 parts by mass, and more preferably in the range of 30 to 90 parts by mass, based on 100 parts by mass of the entire polyolefin resin composition.
[0015] <Fiber-like basic magnesium sulfate> Fibrous basic magnesium sulfate can be obtained by hydrothermal synthesis using alkaline substances such as sodium hydroxide, magnesium hydroxide, magnesium oxide, and calcium hydroxide and magnesium sulfate as raw materials. Basic magnesium sulfate is expressed as MgSO4·5Mg(OH)2·3H2O, and acts as a filler to improve the physical properties of the resulting molded body, such as FM (flexural modulus) and impact strength.
[0016] The fibrous basic magnesium sulfate has an average fiber length of generally 2 to 100 μm, preferably 5 to 50 μm, and an average fiber diameter of generally 0.1 to 2.0 μm, preferably 0.1 to 1.0 μm. The fibrous basic magnesium sulfate has an average aspect ratio (average fiber length / average fiber diameter) of generally 2 or more, preferably 3 to 1000, more preferably 3 to 100, and particularly preferably 5 to 50. The average fiber length and average fiber diameter of the fibrous basic magnesium sulfate can be calculated from the number average values of the fiber length and fiber diameter measured by image analysis of an enlarged image taken with a scanning electron microscope (SEM). In this specification, a fibrous basic magnesium sulfate is exemplified, but it may be in a shape other than the fibrous shape, such as a fan shape or other shapes.
[0017] The blending amount of the fibrous basic magnesium sulfate is preferably 1 to 50 parts by mass, and more preferably 3 to 30 parts by mass, based on 100 parts by mass of the entire polyolefin resin composition.
[0018] <Cellulose nanofiber> The cellulose nanofiber is a fibrous cellulose, and when added to an olefin polymer together with fibrous basic magnesium sulfate, it imparts excellent strength to a molded article. The cellulose nanofiber is not particularly limited, and commercially available products or those produced by a known production method can be used.
[0019] The fiber diameter of the cellulose nanofiber is preferably 1 to 500 nm, and more preferably 10 to 100 nm. If the fiber diameter is 1 nm or more, the manufacturing cost is low. On the other hand, if the fiber diameter is 500 nm or less, the aspect ratio is less likely to decrease, and as a result, a sufficient reinforcing effect can be obtained at low cost. The fiber diameter of the cellulose nanofiber can be measured, for example, by dropping a drop of 0.001 wt % cellulose fiber aqueous dispersion on a mica substrate, drying it, and using the resulting sample.
[0020] The specific surface area of cellulose nanofiber is 50 to 200 m 2 / g, and 70 to 150m 2 The specific surface area of the cellulose nanofiber can be determined, for example, by the BET method.
[0021] The surface of the cellulose nanofiber is preferably hydrophobized so that the cellulose nanofiber can be uniformly dispersed in a highly hydrophobic olefin polymer such as polypropylene. For example, the hydrophobization can be performed by reacting cellulose with acetic anhydride in a solvent containing cellulose and acetic acid to acetylate the cellulose.
[0022] The average degree of polymerization of the cellulose nanofiber is preferably 600 to 30,000, more preferably 600 to 5,000, and even more preferably 800 to 5,000. If the average degree of polymerization is 600 or more, a sufficient reinforcing effect can be obtained. On the other hand, if the average degree of polymerization is 30,000 or less, the viscosity does not increase during kneading, and problems such as difficulty in kneading with the olefin polymer are unlikely to occur.
[0023] The aspect ratio of the cellulose nanofiber is preferably 20 to 10,000, and more preferably 20 to 2,000. When the aspect ratio is 20 or more, a sufficient reinforcing effect is obtained. On the other hand, when the aspect ratio is 10,000 or less, a resin composition with good moldability is obtained. Furthermore, when the aspect ratio is within the above range, the cellulose nanofiber has strong molecular entanglements and a strong network structure, and the strength of the molded article is further improved. In the present invention, the term "aspect ratio" refers to the ratio of the average fiber length to the average diameter of the cellulose nanofibers (average fiber length / fiber diameter).
[0024] The fiber diameter and average fiber length of cellulose nanofibers can be determined based on measurements using a scanning electron microscope (SEM). For example, a dispersion liquid in which cellulose nanofibers are dispersed is cast onto a substrate and observed with an SEM. The diameter and length values are read for 20 or more fibers per image obtained. This is performed for at least three images of non-overlapping areas to obtain diameter and length information for at least 30 fibers. The fiber diameter can be calculated from the obtained fiber diameter data, and the average fiber length can be calculated from the length data. The aspect ratio can be calculated from the ratio of the number average fiber length to the fiber diameter.
[0025] The cellulose nanofibers are preferably modified with hydroxyl groups (hydrogen atoms of hydroxyl groups are replaced with modifying groups). Hydroxyl-modified cellulose nanofibers have fewer hydroxyl groups on the cellulose nanofiber surface than unmodified cellulose nanofibers, and therefore strong adhesion due to hydrogen bonds between the cellulose nanofibers is suppressed. This improves the uniformity of dispersion of the cellulose nanofibers in the resin composition, resulting in a more excellent reinforcing effect. In addition, due to the synergistic effect of the dispersibility caused by the hydroxyl group modification of the cellulose nanofibers described above, the dispersibility of the fibrous basic magnesium sulfate in the resin composition is also improved. Therefore, the resin composition of the present invention can improve the dispersibility of the fibrous basic magnesium sulfate without adding fatty acid metal salts such as magnesium stearate or fatty acids that have been conventionally used to improve the dispersibility of the fibrous basic magnesium sulfate.
[0026] The modification rate of cellulose nanofibers, that is, the proportion of modified hydroxyl groups among all hydroxyl groups in the cellulose nanofibers (the sum of modified and unmodified hydroxyl groups), is preferably 0.01 to 50%, and more preferably 10 to 20%. The modification rate can be calculated from the elemental proportions of carbon, hydrogen, and oxygen obtained by elemental analysis.
[0027] The hydroxyl groups of cellulose nanofibers can be modified by reacting the cellulose nanofibers with a modifying agent. The modifying agent may be any agent capable of reacting with hydroxyl groups, and may be appropriately selected from among the modifying agents proposed thus far. From the viewpoints of simplicity and efficiency, the modifying agent is preferably an etherifying agent or an esterifying agent.
[0028] Examples of the etherifying agent include alkyl etherifying agents, silyl etherifying agents, and aromatic ring-containing etherifying agents. Preferred examples of the alkyl etherifying agent include alkyl halides such as methyl chloride and ethyl chloride; dialkyl carbonates such as dimethyl carbonate and diethyl carbonate; dialkyl sulfates such as dimethyl sulfate and diethyl sulfate; and alkylene oxides such as ethylene oxide and propylene oxide.
[0029] Examples of the silyl etherifying agent include alkoxysilanes such as n-butoxytrimethylsilane, tert-butoxytrimethylsilane, sec-butoxytrimethylsilane, isobutoxytrimethylsilane, ethoxytriethylsilane, octyldimethylethoxysilane, and cyclohexyloxytrimethylsilane; alkoxysiloxanes such as butoxypolydimethylsiloxane; disilazanes such as hexamethyldisilazane, tetramethyldisilazane, and diphenyltetramethyldisilazane; silyl halides such as trimethylsilyl chloride and diphenylbutyl chloride; and silyl trifluoromethanesulfonates such as tert-butyldimethylsilyl trifluoromethanesulfonate. Of the above silyl etherifying agents, alkylsilyl etherifying agents having an alkyl group bonded to a silicon atom are preferred. An example of the aromatic ring-containing etherifying agent is benzyl bromide.
[0030] Examples of the esterifying agent include carboxylic acids, carboxylic anhydrides, and carboxylic acid halides, each of which may contain a heteroatom. More specifically, examples of the esterifying agent include acetic acid, propionic acid, butyric acid, acrylic acid, methacrylic acid, and derivatives thereof. The esterifying agent is preferably an alkyl esterifying agent, and more preferably acetic acid, acetic anhydride, or butyric anhydride.
[0031] Among the above-mentioned modifying agents, alkyl etherifying agents, alkyl silyl etherifying agents, and alkyl esterifying agents are preferred because they have an excellent effect of improving dispersibility. With the alkyl etherifying agent, an alkyl group is introduced as a modifying group. With the silyl etherifying agent, a silyl group is introduced as a modifying group. With the alkyl esterifying agent, an alkylcarbonyl group is introduced as a modifying group.
[0032] The amount of the cellulose nanofiber is preferably 0.01 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, when the entire polyolefin resin composition is taken as 100 parts by mass. However, the amount of the cellulose nanofiber is specified to be 0.01 to 1.00 times the amount of the fibrous basic magnesium sulfate. If the amount of the cellulose nanofiber is too small relative to the fibrous basic magnesium, a synergistic effect of mechanical properties cannot be obtained, while if the amount of the cellulose nanofiber is too large relative to the fibrous basic magnesium, dispersion of the filler in the resin composition becomes difficult, causing poor mechanical properties. The amount of the cellulose nanofiber is preferably 0.001 to 5.0 times the amount of the fibrous basic magnesium sulfate, and more preferably 0.01 to 1.00 times.
[0033] Furthermore, the polyolefin resin composition of the present invention may contain a non-fibrous filler, such as talc, mica, calcium carbonate, barium sulfate, magnesium carbonate, clay, alumina, silica, calcium sulfate, silica sand, carbon black, titanium oxide, magnesium hydroxide, zeolite, molybdenum, diatomaceous earth, sericite, shirasu, calcium hydroxide, calcium sulfite, sodium sulfate, bentonite, and graphite.
[0034] Furthermore, the polyolefin resin composition of the present invention may contain other components within the range that does not impair the effects of the present invention, such as antioxidants, ultraviolet absorbers, pigments, antistatic agents, copper inhibitors, flame retardants, neutralizing agents, foaming agents, plasticizers, nucleating agents, bubble inhibitors, crosslinking agents, etc.
[0035] The polyolefin resin composition of the present invention can be produced by mixing each component and then melt-kneading. Specifically, first, an olefin polymer, fibrous basic magnesium sulfate, and cellulose nanofibers are mixed in a predetermined blending amount. For example, the polyolefin polymer is 50 to 99 parts by mass, the basic magnesium sulfate is 1 to 50 parts by mass, and the cellulose nanofiber is 0.01 to 10 parts by mass. However, the blending amount of the cellulose nanofiber is within a range of 0.01 to 1.00 times that of the fibrous basic magnesium sulfate. A tumbler, a blender, a Henschel mixer, or the like can be used for mixing.
[0036] The resulting mixture is melt-kneaded at 180 to 250° C. using a twin-screw extruder or the like to obtain the polyolefin resin composition of the present invention.
[0037] <Molded body> The molded article of the present invention can be produced by molding the polyolefin resin composition of the present invention. For molding, a molding machine such as a rolling molding machine (such as a calendar molding machine), a vacuum molding machine, an extrusion molding machine, an injection molding machine, a blow molding machine, or a press molding machine can be used.
[0038] As described above, the polyolefin resin composition of the present invention contains a predetermined blend amount of cellulose nanofibers in addition to fibrous basic magnesium sulfate, and therefore it is possible to obtain a molded article having high flexural modulus and Charpy impact strength as well as excellent surface hardness. EXAMPLES
[0039] Specific examples of the present invention will be described below, but the present invention is not limited to these.
[0040] The raw materials used are summarized below. <Raw materials> Propylene polymer (A): Propylene homopolymer, Prime Polypro, J-700GP, manufactured by Prime Polymer Co., Ltd. Fibrous basic magnesium sulfate (B): Mos-Hige A-1, manufactured by Ube Material Industries, Ltd., average major axis 15 μm, average minor axis 0.5 μm Cellulose nanofiber (C): Polypropylene masterbatch containing cellulose nanofiber, PP-CNFC-40, manufactured by Mori Machinery Co., Ltd., containing 40% cellulose nanofiber Talc (D): average particle size 5 μm Magnesium stearate (E): Reagent
[0041] <Example 1> 92.5 parts by mass of polypropylene (A), 5 parts by mass of basic magnesium sulfate (B), and 2.5 parts by mass of cellulose nanofiber master batch (C) were mixed so that the composition of the resin composition was polypropylene (A): fibrous basic magnesium sulfate (B): cellulose nanofiber (C) 94: 5: 1. The resulting mixture was melt-kneaded at 200 ° C. using a twin-screw melt-kneading extruder (L / D = 25, manufactured by Imoto Machinery Co., Ltd.) to obtain the resin composition of Example 1.
[0042] <Example 2> The resin composition of Example 2 was obtained in the same manner as in Example 1, except that the amount of the propylene polymer (A) was changed to 87.5 parts by mass and the amount of the fibrous basic magnesium sulfate (B) was changed to 10 parts by mass.
[0043] <Example 3> The resin composition of Example 3 was obtained in the same manner as in Example 1, except that the amount of the propylene polymer (A) was changed to 82.5 parts by mass and the amount of the fibrous basic magnesium sulfate (B) was changed to 15 parts by mass.
[0044] <Comparative Example 1> A resin composition of Comparative Example 1 was obtained in the same manner as in Example 1, except that the fibrous basic magnesium sulfate (B) was not blended and the blending amount of the propylene polymer (A) was changed to 97.5 parts by mass.
[0045] <Comparative Example 2> A resin composition of Comparative Example 2 was obtained in the same manner as in Example 1, except that the fibrous basic magnesium sulfate (B) was changed to the same amount of talc (D).
[0046] <Comparative Example 3> A resin composition of Comparative Example 3 was obtained in the same manner as in Example 2, except that the fibrous basic magnesium sulfate (B) was changed to the same amount of talc (D).
[0047] <Comparative Example 4> A resin composition of Comparative Example 4 was obtained in the same manner as in Example 3, except that the fibrous basic magnesium sulfate (B) was changed to the same amount of talc (D).
[0048] <Comparative Example 5> A resin composition of Comparative Example 5 was obtained in the same manner as in Example 1, except that the cellulose nanofibers (C) were not blended and the blending amount of the propylene polymer (A) was changed to 95 parts by mass.
[0049] <Comparative Example 6> A resin composition of Comparative Example 6 was obtained in the same manner as in Example 2, except that the cellulose nanofibers (C) were not blended and the blending amount of the propylene polymer (A) was changed to 90 parts by mass.
[0050] <Comparative Example 7> A resin composition of Comparative Example 7 was obtained in the same manner as in Example 3, except that the cellulose nanofibers (C) were not blended and the blending amount of the propylene polymer (A) was changed to 85 parts by mass.
[0051] <Comparative Example 8> The resin composition of Comparative Example 8 was obtained by melt-kneading the propylene polymer (A) alone.
[0052] <Comparative Example 9> A resin composition of Comparative Example 9 was obtained in the same manner as in Example 1, except that 0.15 parts by mass of magnesium stearate was added.
[0053] <Comparative Example 10> A resin composition of Comparative Example 10 was obtained in the same manner as in Example 2, except that 0.30 parts by mass of magnesium stearate was added.
[0054] <Comparative Example 11> A resin composition of Comparative Example 11 was obtained in the same manner as in Example 3, except that 0.45 parts by mass of magnesium stearate was added.
[0055] <Preparation of test specimen> Each resin composition was molded to a predetermined size using an electric injection molding machine (C,Mobile0813, manufactured by Shinko Selvic Co., Ltd.) to obtain a test piece for each evaluation. The test pieces for the mechanical property evaluation and the Vickers hardness test were rectangular (length 50 mm, width 5 mm, thickness 2 mm).
[0056] <Evaluation of physical properties> Using rectangular test pieces for evaluating physical properties, the flexural modulus, Charpy impact strength, and surface hardness were measured by the following methods. <Flexural modulus> A three-point bending test was performed using a universal mechanical testing machine (Imada Co., Ltd.), and the bending modulus was evaluated from the obtained load deflection curve using a method conforming to JIS K 7171. The support distance was 40 mm, the load speed was 10 mm / min, and the measurement temperature was 23°C. <Charpy impact strength> The notched impact strength was evaluated using a Charpy impact tester (manufactured by Mize Testing Instruments Co., Ltd.) according to a method conforming to JIS K7111. The hammer was 2.75 J and the measurement temperature was 23°C. <Surface hardness> The test was performed using a micro Vickers hardness tester (manufactured by Mitutoyo Corporation) in accordance with JIS Z2244, and the Vickers hardness was calculated. The measurement conditions were a load of 1 kgf and a load time of 15 seconds.
[0057] The evaluation results of the molded articles of the examples and comparative examples are summarized in the table below, together with the components of the resin compositions.
[0058] [Table 1]
[0059] Comparison of Examples 1 to 3 with Comparative Examples 1 and 8 shows that by blending a certain amount of cellulose nanofibers in addition to fibrous basic magnesium sulfate, the flexural modulus and Charpy impact strength of the resulting molded article are improved without impairing the surface hardness of the molded article.
[0060] When the fibrous basic magnesium sulfate in the resin compositions of the examples was replaced with talc, the surface hardness could not be increased and the Charpy impact strength also decreased (Comparative Examples 2 to 4). When the cellulose nanofibers were omitted from the resin compositions of the examples, the Charpy impact strength and surface hardness decreased (Comparative Examples 5 to 7). When magnesium stearate was blended into the resin compositions of the examples, the Charpy impact strength decreased (Comparative Examples 9 to 11).
Claims
1. Olefin polymers, Fibrous basic magnesium sulfate, and The amount of cellulose nanofibers is 0.01 to 1.00 times the amount of the fibrous basic magnesium sulfate. A polyolefin resin composition (excluding those containing a fatty acid metal salt or a fatty acid) comprising the above compound.
2. The cellulose nanofiber has a fiber diameter of 1 to 500 nm and a specific surface area of 50 to 200 m 2 The polyolefin resin composition according to claim 1, wherein the molecular weight of the polyolefin resin composition is 1 / g.
3. 3. The polyolefin resin composition according to claim 1, wherein the fibrous basic magnesium sulfate has an average fiber length of 2 to 100 μm and an average fiber diameter of 0.1 to 2.0 μm.
4. The polyolefin resin composition according to any one of claims 1 to 3, wherein the olefin polymer is polypropylene.
5. The polyolefin resin composition according to any one of claims 1 to 4, wherein the cellulose nanofibers are hydrophobized by acetylation.
6. A molded article which is a molded product of the polyolefin resin composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Propylene resin composition and molded product thereof
JP2011144278A
Molded article with excellent mechanical characteristic, and method and apparatus for manufacturing the same
JP2012207100A
Composite resin molded body
JP2017210595A
Composite resin molding
JP2019085529A
Cellulose fiber dispersant, resin composition, method for producing resin composition and molding
JP2019143016A