Predried polystyrene / alumina composites for foam extrusion.

The introduction of a dry PS/alumina composite in PS compositions significantly enhances blowing agent solubility and retention, leading to improved thermal insulation and mechanical properties in low-density PS foams, addressing the need for environmentally friendly alternatives to HFCs.

JP7562635B2Active Publication Date: 2024-10-07FINA TECH INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022507817
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-08
Filing Date
2020-08-04
Publication Date
2024-10-07
Estimated Expiration
2040-08-04

AI Technical Summary

Technical Problem

There is a need for a simple and economical approach to improve blowing agent solubility and retention in polystyrene (PS) foams, particularly with hydrofluoroolefins (HFOs) and hydrofluorocarbons (HFCs), to achieve superior thermal insulation properties while reducing environmental impact.

Method used

A dry PS/alumina composite is used in PS compositions, with a moisture content of 0.05 weight percent or less, to enhance blowing agent solubility and retention, allowing for higher concentrations of HFOs and HFCs in PS foams, thereby improving thermal insulation and mechanical properties.

Benefits of technology

The use of a dry PS/alumina composite increases blowing agent solubility by up to 30%, enabling the production of low-density PS foams with enhanced thermal insulation and mechanical properties, while reducing the use of high-GWP HFCs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562635000002
    Figure 0007562635000002
  • Figure 0007562635000003
    Figure 0007562635000003
  • Figure 0007562635000004
    Figure 0007562635000004
Patent Text Reader

Abstract

A polystyrene (PS) composition for producing an extruded foam, the PS composition comprising: a dried PS / alumina composite comprising PS and an alumina additive, the dried PS / alumina composite having a moisture content of about 0.05 weight percent (wt%) or less as measured by a coulometer; and a blowing agent.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Patent Application No. 62 / 884,289, filed August 8, 2019, which is incorporated by reference in its entirety for all purposes.

[0002] STATEMENT REGARDING FEDERALLY SPONSORED RESEARCH OR DEVELOPMENT Not applicable.

[0003] References to Microfiche Appendix Not applicable.

[0004] The present disclosure relates to the production of polystyrene (PS) foams. More particularly, the present disclosure provides PS compositions and methods for increasing the solubility of blowing agents during PS foam extrusion. Even more particularly, the present disclosure provides PS compositions and methods for producing PS foams having desirable thermal insulation properties, and the PS foams produced thereby. [Background technology]

[0005] It is well known in the art that polystyrene can be foamed and formed into a variety of articles, such as foam rods, planks, and sheets. Polystyrene (PS) foams formed with hydrofluorocarbon (HFC) blowing agents, such as HFC 134a, can be used in the construction of insulation boards. High HFC blowing agent concentrations are desirable in foam boards due to their superior insulation properties (e.g., as measured by R-value). Commonly used physical blowing agents (e.g., hydrochlorofluorocarbons (HCFCs), hydrofluorocarbons (HFCs), or combinations thereof) can result in the formation of smog, have high ozone depletion potential or global warming potential (GWP), and / or be harmful air pollutants. For example, due to their high GWP (global warming potential), some HFCs, including HFC 134a, will be banned by 2021. Thus, alternatives to HFCs, such as HFC 134a, are needed. Hydrofluoroolefins (HFOs) appear to be one candidate due to their zero GWP. Summary of the Invention [Problem to be solved by the invention]

[0006] Despite advances in foam production, there remains a need for simple and economical approaches to achieve improved blowing agent solubility, including both HFCs and HFOs, in polystyrene compositions for foam extrusion and / or to improve blowing agent retention in polystyrene foams. [Means for solving the problem]

[0007] Disclosed herein is a polystyrene (PS) composition for producing an extruded foam, the PS composition comprising a dry PS / alumina composite comprising PS and an alumina additive, the dry PS / alumina composite having a moisture content of about 0.05 weight percent (wt%) or less as measured by a coulometer, and a blowing agent. Disclosed herein is a low density polystyrene (PS) foam produced by extrusion of the PS composition, the low density PS foam comprising a higher blowing agent concentration than that of an otherwise similar low density PS foam produced by extrusion of a PS composition that does not include the dry PS / alumina composite. Disclosed herein is a low density polystyrene (PS) foam produced by extrusion of the PS composition, the low density PS foam comprising a higher blowing agent concentration than that of an otherwise similar low density PS foam produced by extrusion of a PS composition that does not include the dry PS / alumina composite. The foam exhibits at least one superior thermal insulation property compared to an otherwise similar low density PS foam produced by extrusion of a PS composition that does not include a dry PS / alumina composite. Also disclosed herein is a low density polystyrene (PS) foam produced by extrusion of a PS composition, the low density PS foam exhibiting at least one mechanical property at least equivalent to that of an otherwise similar low density PS foam produced by extrusion of a PS composition that does not include a dry PS / alumina composite. Further disclosed herein is a low density polystyrene (PS) foam produced by extrusion of a PS composition, the blowing agent comprising one or more hydrofluoroolefins (HFOs), the low density PS foam exhibiting at least one thermal insulation property at least equivalent to that of an otherwise similar low density PS foam produced by extrusion of a PS composition that does not include a dry PS / alumina composite and comprises one or more blowing agents selected from the group consisting of hydrofluorocarbons (HFCs).

[0008] Also disclosed herein is a method for producing a low density polystyrene (PS) foam, the method comprising forming a polystyrene (PS) / alumina composite comprising PS and an alumina additive, removing moisture from the PS / alumina composite to form a dry PS / alumina composite, the dry PS / alumina composite having a moisture content of about 0.05 weight percent (wt%) or less as measured by coulometer, blending the dry PS / alumina composite, a blowing agent, and optionally one or more additional additives to form a foamable mixture, and producing a foam by extruding the foamable mixture through a die into a region of reduced pressure. A low density polystyrene (PS) foam produced via this method is also provided. In an embodiment, the low density PS foam comprises a higher blowing agent concentration and / or exhibits at least one superior thermal insulating or mechanical property compared to that of an otherwise similar low density PS foam produced by extrusion of a foamable mixture without the dry PS / alumina composite.

[0009] Also disclosed herein is a dry polystyrene (PS) / alumina composite for producing an extruded foam, the dry PS / alumina composite comprising an extruded mixture of PS and an alumina additive, the extruded mixture being dried to provide a dry PS / alumina composite such that the dry PS / alumina composite has a moisture content of about 0.05 weight percent (wt%) or less as measured by coulometer, the dry PS / alumina composite comprising about 0.01 to about 20.0 weight percent (wt%) of the alumina additive.

[0010] For a more complete understanding of the present disclosure and its advantages, reference is now made to the following brief description, taken in conjunction with the accompanying drawings and detailed description, in which like reference numerals represent like parts. [Brief description of the drawings]

[0011] [Figure 1A] 1 provides an image of a first comparative foam sample C1 of Example 1 containing 7 wt% of blowing agent HFC 134a; [Figure 1B]1 provides an image of a first comparative foam sample C1 of Example 1 containing 8 wt% of blowing agent HFC 134a; [Figure 2A] 1 provides an image of a second comparative foam sample C2 of Example 1 containing 6 wt% of blowing agent HFC 134a; [Figure 2B] 1 provides an image of a second comparative foam sample C2 of Example 1 containing 7 wt% of blowing agent HFC 134a; [Figure 3A] 1 provides an image of inventive foam sample I1 of Example 1 containing 6 wt. % of blowing agent HFC 134a; [Figure 3B] 1 provides an image of inventive foam sample I1 of Example 1 containing 7 wt. % of blowing agent HFC 134a; [Figure 3C] 1 provides an image of inventive foam sample I1 of Example 1 containing 8.5 wt. % of blowing agent HFC 134a; [Figure 4] 1 shows a side-by-side comparison of a second comparative foam sample C2 of Example 1 containing 7 wt. % and 7.5 wt. % HFC 134a with an inventive foam sample I1 of Example 1 containing 9 wt. % HFC 134a; [Diagram 5] 1 is a plot of wet density (g / cc) as a function of concentration (wt %) of blowing agent HFC 134a for the composition of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Detailed Description First, exemplary implementations of one or more aspects are provided below, but it should be understood that the disclosed compositions, methods, and / or products may be implemented using any number of techniques, whether currently known or in existence. The present disclosure should in no way be limited to the exemplary implementations, drawings, and techniques shown below, including the exemplary designs and implementations shown and described herein, and may be amended within the scope of the appended claims, along with their full scope of equivalents. The present disclosure describes a dry polystyrene (PS) / alumina composite for use in polystyrene (PS) compositions containing the dry PS / alumina composite and a blowing agent. It has been unexpectedly discovered that the use of the dry PS / alumina composite and PS compositions containing the same allows PS to retain a higher concentration of blowing agent in the finished PS foam, improves the solubility of physical blowing agents, such as, but not limited to, HFCs (hydrofluorocarbons), HFOs (hydrofluoroolefins), and carbon dioxide (CO2), in polystyrene during foam extrusion, and / or increases the retention of blowing agent in the resulting PS foam. Specifically, the PS composition includes a dry PS / alumina composite comprising PS (e.g., crystal polystyrene) and an alumina additive, the dry PS / alumina composite having a moisture content of about 0.1, 0.05, 0.04, 0.03, 0.02, 0.01, or 0 weight percent (wt %) or less as measured by coulometer; and a blowing agent.

[0013] In an embodiment, the PS composition of the present disclosure has a wider foam extrusion processing window, as indicated by higher blowing agent concentration and / or foamability at a wider range of temperatures. In an embodiment, the PS foam (e.g., low density PS foam) obtained from the extrusion / foaming of the PS composition disclosed herein has a higher blowing agent (e.g., HFC or HFO) concentration (e.g., due to desired high blowing agent solubility during foam extrusion), increased blowing agent retention in the resulting PS foam, and / or improved mechanical properties of the foam (e.g., superior insulation properties). A potential advantage of the PS composition of the present disclosure is that such a composition may enable polystyrene insulation board manufacturers to replace commonly used HFC 134 with low GWP (global warming potential) blowing agents such as HFOs.

[0014] In embodiments, the use of a dried PS / alumina composite to form a PS composition of the present disclosure increases the blowing agent solubility in the PS composition during foam extrusion (and thus the resulting PS foam) by at least 10, 20, or 30%. The alumina additive can be present in the dried PS / alumina composite in an embodiment in a range of about 0.01 to about 20.0 weight percent (wt %). In embodiments, the solubility of the blowing agent in the PS composition is about 6.5, 7, 7.5, or 8 weight percent or greater.

[0015] There are two major challenges with the use of HFOs as blowing agents. First, HFOs are very expensive refrigerants / blowing agents, and second, HFOs have relatively low solubility in polystyrene compared to traditional blowing agents such as HFC 134a, and therefore it can be difficult to achieve the desired insulating properties in the resulting foam product. Furthermore, polystyrene typically does not exhibit favorable foaming behavior when a physical blowing agent such as carbon dioxide is used. In particular, when used as a physical blowing agent in traditional polystyrene foaming processes, carbon dioxide tends to result in featureless clumping or disintegration of the polymer material. Produces poor quality thermoplastic foam. Without being limited by theory, this may be the result of lack of polymer-gas compatibility and limited solubility of carbon dioxide in the molten thermoplastic extrudate, which results in the generation of uncontrollably high levels of open cells in the foam structure as the thermoplastic / blowing agent combination exits the die. Furthermore, even if the resulting foam has a visible foam structure, the foam tends to collapse quickly due to the relatively high permeability of carbon dioxide to air (i.e., the cells may collapse due to partial vacuum caused by rapid escape of carbon dioxide from the cells), making it unsuitable for most practical applications within a few hours of being produced. Through this disclosure, non-HFC blowing agents such as HFOs and CO2 may be used as blowing agents or co-blowing agents in certain low density PS foam applications. In an embodiment, the dried PS / alumina composites including the PS compositions of the present disclosure may enable a transition to non-flammable, inexpensive, and low GWP (global warming potential) blowing agents such as CO2, with improved blowing agent solubility during extrusion and / or improved retention of the blowing agent in the produced foam.

[0016] The present disclosure describes a dry polystyrene (PS) / alumina composite for use in a polystyrene (PS) composition comprising the dry PS / alumina composite and a blowing agent. It has been unexpectedly discovered that the use of the dry PS / alumina composite and the PS composition comprising the same allows the PS to retain a higher concentration of the blowing agent in the finished PS foam, improves the solubility of physical blowing agents such as, but not limited to, HFCs (hydrofluorocarbons), HFOs (hydrofluoroolefins), and carbon dioxide (CO2) in polystyrene during foam extrusion, and / or increases the retention of the blowing agent in the resulting PS foam. Specifically, the PS composition comprises a dry PS / alumina composite comprising PS (e.g., crystal polystyrene) and an alumina additive, the dry PS / alumina composite having a moisture content of about 0.05 weight percent (wt%) or less as measured by coulometer; and a blowing agent.

[0017] In an embodiment, the PS composition of the present disclosure has a wider foam extrusion processing window, as indicated by higher blowing agent concentration and / or foamability at a wider range of temperatures. In an embodiment, the PS foam (e.g., low density PS foam) obtained from the extrusion / foaming of the PS composition disclosed herein has a higher blowing agent (e.g., HFC or HFO) concentration (e.g., due to desired high blowing agent solubility during foam extrusion), increased blowing agent retention in the resulting PS foam, and / or improved mechanical properties of the foam (e.g., superior insulation properties). A potential advantage of the PS composition of the present disclosure is that such a composition may enable polystyrene insulation board manufacturers to replace commonly used HFC 134 with low GWP (global warming potential) blowing agents such as HFOs.

[0018] In embodiments, the use of a dry PS / alumina composite to form a PS composition of the present disclosure increases the blowing agent solubility in the PS composition during foam extrusion (and thus the resulting PS foam) by at least 10, 20, or 30%. The alumina additive can be present in the dry PS / alumina composite in an embodiment in a range of about 0.01 to about 20.0 weight percent (wt %).

[0019] There are two main challenges with the use of HFOs as blowing agents. First, HFOs are very expensive refrigerants / blowing agents, and second, HFOs have relatively low solubility in polystyrene compared to traditional blowing agents such as HFC 134a, and therefore it may be difficult to achieve the desired insulating properties in the resulting foam product. Furthermore, polystyrene typically does not exhibit favorable foaming behavior when a physical blowing agent such as carbon dioxide is used. In particular, when used as a physical blowing agent in traditional polystyrene foaming processes, carbon dioxide produces featureless chunks of polymer material, or poor quality thermoplastic foam that tends to collapse. Without being limited by theory, this is believed to be due to the fact that the foaming agent is not very stable, and therefore the foaming agent is not very stable. , the lack of polymer-gas compatibility, and the limited solubility of carbon dioxide in the molten thermoplastic extrudate, which results in the generation of uncontrollably high levels of open cells in the foam structure as the thermoplastic / blowing agent combination exits the die. Furthermore, even if the resulting foam has a visible foam structure, the foam tends to collapse rapidly due to the relatively high permeability of carbon dioxide to air (i.e., the cells may collapse due to a partial vacuum caused by the rapid escape of carbon dioxide from the cells), making it unsuitable for most practical applications within a few hours of being produced. Through this disclosure, non-HFC blowing agents such as HFOs and CO2 may be used as blowing agents or co-blowing agents in certain low density PS foam applications. In an embodiment, the dried PS / alumina composites including the PS compositions of the present disclosure may enable a transition to non-flammable, inexpensive, and low GWP (global warming potential) blowing agents such as CO2, with improved blowing agent solubility during extrusion and / or improved retention of the blowing agent in the produced foam.

[0020] Although the following terms are believed to be well understood by those of ordinary skill in the art, the following definitions are provided to facilitate the description of the subject matter disclosed herein. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the subject matter disclosed herein belongs.

[0021] Styrene, also known as vinylbenzene, is an aromatic compound produced in industrial quantities from ethylbenzene. The most common method of styrene production involves the dehydrogenation of ethylbenzene, which produces styrene monomer and the crude products unreacted ethylbenzene and hydrogen. Polystyrene is an aromatic polymer produced from styrene monomer. Polystyrene is a widely used polymer found in insulation, packaging, and foam products including disposable cutlery and foam cups.

[0022] Different types of polystyrene materials can include general purpose polystyrene (GPPS) and high impact polystyrene (HIPS). Many conditions affect the properties of the resulting product, including processing time, temperature, pressure, purity of the monomer feedstock, and the presence of additives or other compounds. These and other processing conditions change the physical and chemical properties of the polystyrene product, affecting its suitability for a desired use.

[0023] Expanded polystyrene offers the advantages of low cost, light weight, and high structural strength due to its density. In addition, typical polystyrene foams have relatively high impact resistance and have excellent electrical and thermal insulation properties. Expanded polystyrene is useful in a variety of applications such as insulation, packaging, coolers, food packaging, decorations, and dunnage used to protect and secure cargo during transportation. Furthermore, polystyrene foams are generally classified into three general categories: low density, medium density, and high density. Low density polystyrene foams typically have a strength of about 1 to about 3 lb / ft 3 whereas medium density foam has a density of about 4 to about 19 lb / ft 3 and high density foams often have densities ranging from 20 to about 30 lb / ft 3 It has a density in the range of

[0024] The two main types of polystyrene foam are extruded polystyrene (XPS) foam and expanded polystyrene (EPS) foam. Extruded polystyrene foam is typically formed by mixing polystyrene with additives and blowing agents into an extruder where the mixture is heated. The mixture is then extruded, expanded into the desired shape, and cooled. Expanded polystyrene foam is typically formed by expanding solid polystyrene beads containing a blowing agent such as pentane with steam or hot gas. These pre-expanded beads may then be formed into the desired shape and expanded again with steam or hot gas to fuse the beads together.

[0025] The term "blowing agent," as used herein, refers to any of a wide variety of substances that, alone or in combination with at least one other substance, are capable of producing a cellular structure in a plastic mass. Thus, the term includes, but is not limited to, gases that expand when pressure is released, soluble solids that leave pores when exuded, liquids that generate bubbles when converted to a gas, and / or chemical agents that decompose or react under the influence of heat to form a gas.

[0026] In the production of extruded polystyrene foam, it is common to use blowing agents such as methyl chloride, ethyl chloride, chlorocarbons, fluorocarbons (including HFCs) and chlorofluorocarbons (CFCs). However, such blowing agents have been heavily regulated due to potential environmental impacts, including ozone depletion or global warming. An ongoing trend in extrusion foaming process development is to find environmentally friendly chemicals as blowing agents. Some foaming processes have used hydrofluoroolefins (HFOs) or carbon dioxide (CO2) as blowing agents or co-blowing agents. For the desired thermal insulation properties, HFOs are preferred due to their low thermal conductivity and minimal environmental impact. However, HFO solubility in polystyrene requires further improvement as provided herein to meet the stringent regulatory requirements for structural insulation foam boards.

[0027] The term "thermoplastic foam" refers to a cellular polymer in which a multitude of gas bubbles or cells are distributed in a polymer matrix that can be repeatedly heated, melted, molded, and cooled. As a result, thermoplastic foams can be easily melted and recycled. Polystyrene foams produced according to the present disclosure may be thermoplastic foams.

[0028] Most of the above definitions are as would be substantially understood by one of ordinary skill in the art, however, one or more of the above definitions may be defined above to have a different meaning than would normally be understood by one of ordinary skill in the art, due to the particular description herein of the subject matter disclosed herein.

[0029] Disclosed herein are polystyrene (PS) compositions (also referred to herein as "PS blends," "PS formulations," or "expandable mixtures") for producing polystyrene foams. Disclosed herein are PS compositions comprising a dry PS / alumina composite comprising PS and an alumina additive. The dry PS / alumina composite has a moisture content of about 0.05 weight percent (wt%) or less as measured by coulometer. The dry PS / alumina composite can be produced by forming a polystyrene (PS) / alumina composite comprising PS and an alumina additive, and removing moisture from the PS / alumina composite to form a dry PS / alumina composite, where the dry PS / alumina composite has a moisture content of about 0.05 weight percent (wt%) or less as measured by coulometer. Alternatively, the combination of PS and alumina additive results in a dry PS / alumina composite, i.e., the combination of PS and alumina additive is sufficiently dry (without further moisture removal) to result in a PS / alumina composite having a required moisture content of about 0.05 weight percent (wt%) or less as measured by coulometer, and thus the PS / alumina composite is considered a dry PS / alumina composite. As described in more detail below, the PS composition of the present disclosure can further include a blowing agent (e.g., a blowing agent, or multiple blowing agents). Additional additives described herein below may be included in the PS composition (e.g., incorporated into or combined with the dry PS / alumina composite to form a polystyrene composition). For example, as described further below, such additional additives may include an SRA, an antioxidant, a flame retardant, or a combination thereof.

[0030] The PS composition of the present disclosure includes polystyrene incorporated therein via a dry PS / alumina composite. Various polystyrene homopolymers and copolymers, and polymerization or irradiation High impact polystyrene (HIPS) engineered by technology can be used. In embodiments, PS can include crystal polystyrene (also called general purpose polystyrene (GPPS)), high impact polystyrene (HIPS), PS copolymer, or combinations thereof. In embodiments, the polystyrene copolymer may include a metal monomer. For example, in embodiments, the metal monomer includes zinc dimethylacrylate (ZDMA). Suitable polystyrene copolymers can include a wide variety of polymers, such as, but not limited to, glycidyl methacrylate, 2-hydroxyethyl methacrylate copolymer, acrylonitrile, and the like. In embodiments, suitable polystyrene can be derived from petroleum-based and / or bio-based sources.

[0031] In embodiments, the polystyrene of the dried PS / alumina composites and PS compositions disclosed herein have a melt flow rate (MFR) as measured by D1238 in the range of 0.2 to 30 grams (g) / 10 minutes (min), 1.0 to 20 g / 10 min, or 1.0 to 10.0 g / 10 min.

[0032] In embodiments, the dried PS / alumina composites and PS compositions of the present disclosure include crystalline polystyrene, which has a melt flow rate, as measured in accordance with ASTM D-1238, of 0.2 g / 10 min to 30 g / 10 min, 1.0 g / 10 min to 20 g / 10 min, or 1.0 g / 10 min to 10.0 g / 10 min; a tensile strength, as measured in accordance with ASTM D-1238, of 6,000 psi to 8,000 psi (41.4 to 55.2 MPa), 6,500 psi to 8,000 psi (44.8 to 55.2 MPa), or 7,000 psi to 8,000 psi (48.3 to 55.2 MPa); A tensile modulus of 400,000 psi to 480,000 psi (2.8 to 3.3 GPa), 420,000 psi to 460,000 psi (2.9 to 3.2 GPa), or 430,000 psi to 450,000 psi (3.0 to 3.1 GPa), as measured in accordance with ASTM D-638; a flexural modulus of 400,000 psi to 480,000 psi (2.8 to 3.3 MPa), 420,000 psi to 460,000 psi (2.9 to 3.2 MPa), or 430,000 psi to 450,000 psi (3.0 to 3.1 MPa), as measured in accordance with ASTM D-790; Flexural strength of 10,000 psi to 15,000 psi (68.9 to 103.4 MPa), 12,000 psi to 14,000 psi (82.7 to 96.5 MPa), or 13,000 psi to 14,000 psi (89.6 to 96.5 MPa), as measured in accordance with ASTM D-790; annealing heat strain of 190°F to 220°F (87.8°C to 104.4°C), 200°F to 220°F (93.3°C to 104.4°C), or 210°F to 220°F (98.9°C to 104.4°C), as measured in accordance with ASTM D-648; and / or It may be characterized by a Vicat softening of 200°F to 230°F (93.3°C to 110.0°C), 210°F to 230°F (98.9°C to 110.0°C), or 215°F to 225°F (101.7°C to 107.2°C), as measured in accordance with D-1525.

[0033] In an embodiment, the dried PS / alumina composite and PS composition of the present disclosure comprises HIPS. HIPS refers to any elastomer-reinforced vinyl aromatic polymer. Vinyl aromatic monomers may include, but are not limited to, styrene, α-methylstyrene, and ring-substituted styrenes. HIPS may further include comonomers including methylstyrene; halogenated styrenes; alkylated styrenes; acrylonitrile; esters of (meth)acrylic acid with alcohols having 1 to 8 carbons; N-vinyl compounds such as vinyl-carbazole, maleic anhydride, and the like; compounds containing two polymerizable double bonds such as divinylbenzene or butanediol diacrylate; or combinations thereof. The comonomer may be present in an amount effective to impart one or more properties desired by the user to the polystyrene resin. Such effective amounts may be determined by one of skill in the art with the aid of the present disclosure. For example, the comonomer may be present in an amount of 1% by weight to 1% by weight of the total weight of the reaction mixture from which the polystyrene is formed. It may be present in the styrene polymer composition in an amount of 99.9%, 1% to 90%, or 1% to 50% by weight.

[0034] In HIPS, elastomeric materials are typically embedded in a polystyrene matrix. Examples of elastomeric materials include conjugated diene monomers, including but not limited to 1,3-butadiene, 2-methyl-1,3-butadiene, 2-chloro-1,3-butadiene, 2-methyl-1,3-butadiene, or combinations thereof. In embodiments, HIPS include aliphatic conjugated diene monomers as elastomers. Examples of suitable aliphatic conjugated diene monomers include but are not limited to C4-C9 dienes, such as butadiene monomer. Blends or copolymers of diene monomers may also be used. Similarly, mixtures or blends of one or more elastomers may be used to produce HIPS. In embodiments, the elastomer includes a homopolymer of a diene monomer, and in embodiments, the elastomer includes polybutadiene. The elastomer may be present in the HIPS in an amount effective to produce one or more properties desired by the user. Such effective amounts may be determined by one of skill in the art with the aid of this disclosure. For example, the elastomer may be present in the HIPS product in an amount of from 1% to 20%, from 2% to 15%, or from 5% to 11% by weight based on the total weight of the HIPS.

[0035] In an embodiment, the HIPS used in the dried PS / alumina composite or PS composition of the present disclosure has a melt flow rate of from 1 g / 10 min to 40 g / 10 min, from 1.5 g / 10 min to 20 g / 10 min, or from 2 g / 10 min to 15 g / 10 min, as measured in accordance with ASTM D-1238; a falling dart impact of from 5 in-lb to 200 in-lb (0.6 to 22.6 Nm), from 50 in-lb to 180 in-lb (5.6 to 20.3 Nm), or from 100 in-lb to 150 in-lb (11.3 to 16.9 Nm), as measured in accordance with ASTM D-3029; Izod impact of 0.4 ft-lb / in to 5 ft-lb / in (0.4 to 267 J / m), 1 ft-lbs / in to 4 ft-lbs / in (53 to 213 J / m), or 2 ft-lbs / in to 3.5 ft-lbs / in (107 to 187 J / m), as measured in accordance with ASTM D-256; tensile strength of 2,000 psi to 10,000 psi (13.8 to 68.9 MPa), 2,800 psi to 8,000 psi (19.3 to 55.1 MPa), or 3,000 psi to 5,000 psi (20.7 to 34.5 MPa), as measured in accordance with ASTM D-638; A tensile modulus of 100,000 psi to 400,000 psi (0.7 to 2.7 GPa), 200,000 psi to 400,000 psi (1.4 to 2.7 GPa), or 250,000 psi to 380,000 psi (1.7 to 2.6 GPa), as measured in accordance with ASTM D-638; an elongation of 0.5% to 90%, 5% to 70%, or 35% to 60%, as measured in accordance with ASTM D-638; a flexural strength of 3,000 psi to 15,000 psi (20.7 to 103.4 MPa), 4,000 psi to 10,000 psi (27.6 to 68.9 MPa), or 6,000 psi to 9,000 psi (41.4 to 62.1 MPa), as measured in accordance with ASTM D-790; 200,000 psi to 450,000 psi (1.4 to 3.1 GPa), 230,000 psi to 400,000 psi (1.6 to 2.8 GPa), or 250,000 psi to 350,000 psi (1.7 to 2.4 GPa); an annealing heat distortion of 180°F to 215°F (82°C to 102°C), 185°F to 210°F (85°C to 99°C), or 190°F to 205°F (88°C to 96°C), as measured in accordance with ASTM D-648; a Vicat softening of 195°F to 225°F (91°C to 107°C), 195°F to 220°F (91°C to 104°C), or 200°F to 215°F (93°C to 102°C), as measured in accordance with ASTM D-1525; and / or a gloss 60° of 30 to 100, 40 to 98, or 50 to 95, as measured in accordance with ASTM D-523.

[0036] The dried PS / alumina composites and PS compositions of the present disclosure include an alumina additive. Any suitable alumina known in the art can be used as the alumina additive. In an embodiment, the alumina additive comprises about 64 to about 80, about 72 to about 76, about 72 to about 74, or about 70, 72, or 74 weight percent or more of aluminum oxide (Al2O3). In an embodiment, the alumina additive comprises about 0.002 weight percent or less of sodium oxide (Na2O). In an embodiment, the remainder of the alumina composition (i.e., the remainder including components other than aluminum oxide or sodium oxide) comprises titania (TiO2), silica (SiO2), and iron oxide (e.g., iron(III), Fe2O3). In an embodiment, the alumina additive comprises a diameter in the range of about 5 to about 60, about 26 to about 60, about 35 to about 60, or about 5, 10, 20, 30, 40, 50, or 60 μm or more, below which 50% of the mass of the sample is contained. 50 In an embodiment, the alumina additive has a particle size (or mass average diameter) of about 80 to about 360 μm, as measured by the Brunauer-Emmett-Teller (BET) method. 2 / g, about 35~400m 2 / g, about 150~360m 2 / g, approx. 200~360m 2 / g range, or about 35, 80, 100, 150, or 230 m 2 / g or greater. In an embodiment, the alumina additive has a pore volume in the range of about 0.3 to about 1.5 mL / g, about 0.5 to about 1.3 mL / g, or about 0.5 to about 1.0 mL / g. In an embodiment, the alumina additive has a 120 crystallite size in the range of about 4 to about 50 nm, about 4.5 to about 20 nm, or about 5.5 to about 10 nm, as measured by x-ray diffraction at the (120) diffraction peak. In an embodiment, the alumina additive comprises CATAPAL® available from Sasol, PURAL® available from Sasol, or a combination thereof. For example, in embodiments, the alumina additive includes CATAPAL® A, CATAPAL® B, CATAPAL® C1, CATAPAL® D, CATAPAL® 200, PURAL® SB, PURAL® SCF, PURAL® 200, PURAL® BT, or combinations thereof. Table 1 shows exemplary alumina additives that can be used in the PS / alumina composites of the present disclosure (e.g., PS / alumina composites from which moisture has been removed to form dry PS / alumina composites). This table is not exhaustive, and any suitable alumina additive described herein or known to one of ordinary skill in the art can be used in embodiments with the aid of the present disclosure. Without wishing to be limited by theory, the alumina additive can function as an infrared (IR) attenuator in embodiments.

[0037] [Table 1]

[0038] In an embodiment, the dry PS / alumina composite comprises from about 0.01 to about 20.0 weight percent (wt %), from about 0.1 to about 10 wt %, from about 0.2 to about 1 wt %, up to about 10, 7, or 5 wt %, or more than about 0.1, 0.2, or 0.5 wt % alumina additive.

[0039] As noted above, the PS composition of the present disclosure may further comprise one or more additional additives. In embodiments, the PS composition (e.g., the PS / alumina composite from which water is removed to form the dried PS / alumina composite, the dried PS / alumina composite used to form the PS composition, and / or the PS composition) comprises low levels of one or more solubility and / or retention additives, i.e., "SRA," as described in U.S. Patent Application No. 16 / 014,883, the entirety of which is incorporated herein by reference. In embodiments, the SRA is selected from the group consisting of epoxidized soybean oil (ESO), epoxidized polybutadiene, mineral oil (MO), glycerol monostearate (GMS), glycerol tristearate (GTS), IRGANOX 1, glycerol stearate (GMS), glycerol tristearate (GTS), glycerol ... 010® (pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), or combinations thereof. Without wishing to be bound by theory, it is hypothesized that the presence of an SRA may further increase the solubility of the blowing agent, thereby improving miscibility in PS (e.g., molten PS, such as during extrusion), and that the presence of an SRA may reduce the activation energy for bubble nucleation and growth due to increased polymer chain mobility due to a plasticizing effect. This may result in the generation of a larger number of bubbles, thereby, in embodiments, resulting in a lower foam density.

[0040] In embodiments, the PS composition can include about 0.01-10.0 weight percent (wt%), about 0.01-5.0 wt%, about 0.01-2.0 wt%, about 0.1-1.0 wt%, or about 0.01-0.50 wt% SRA, where the weight percentages are based on the total weight of the PS composition. In embodiments, the dry PS / alumina composition includes about 0.01, 0.05, 0.1, 0.25, 0.5, 0.75, 1.0, 1.25, 1.5, 1.75, 2.0, 2.25, 2.5, 2.75, 3.0, 3.25, 3.5, 3.75, 4.0, 4.25, 4.5, 4.75, or 5.0 wt% SRA, based on the total weight of the dry PS / alumina composition.

[0041] In embodiments, the dried PS / alumina composite and / or PS composition of the present disclosure includes low levels of mineral oil (MO) and / or epoxidized soybean oil (ESO) as SRA. Without wishing to be limited by theory, it is speculated that MO and ESO can plasticize the PS melt to some extent, effectively improving the "free volume" by increasing the mobility of polymer chain segments. The polar species of ESO may promote the diffusivity of polar blowing agent molecules throughout the PS melt. Thus, the addition of ESO to PS to produce the PS composition of the present disclosure may, in embodiments, allow PS to foam at relatively low temperatures with high blowing agent concentrations. Because the presence of MO and / or ESO may adversely affect the mechanical properties of the foam, such as the melt strength of polystyrene, which, if significant, may result in undesirable collapsed cells, PS compositions containing such SRA may be fine-tuned to achieve an optimal balance between improved blowing agent solubility and melt strength. For example, in embodiments, a reinforcing agent such as, but not limited to, high stiffness poly(phenylene oxide) (PPO), polyalphamethylstyrene, or a combination may be added to the PS composition (e.g., incorporated into a PS / alumina composite, incorporated into a dry PS / alumina composite, and / or combined with a dry PS / alumina composite to form a PS composition) to achieve a desired foam compressive strength.

[0042] Although described with reference to epoxidized soybean oil, in embodiments, the SRA of the present disclosure may include any of a wide variety of epoxidized fatty acids and esters. For example, in embodiments, the epoxidized fatty acids may include myristic acid, myristoleic acid, palmitic acid, palmitoleic acid, margaric acid, margaroleic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, arachidic acid, gadoleic acid, eicosadienoic acid, behenic acid, erucic acid, lignoceric acid, or combinations thereof. Such fatty acids may be found in a variety of vegetable oils, including, but not limited to, linseed oil, tung oil, safflower oil, soybean oil, castor oil, cottonseed oil, peanut oil, rapeseed oil, coconut oil, palm oil, olive oil, corn oil, corn germ oil, sesame oil, peach seed oil, peanut oil, soybean lecithin, and egg yolk lecithin. Thus, a variety of epoxidized fatty acids may be used in the PS compositions according to the present disclosure. In embodiments, the SRA comprises an acrylated epoxidized fatty acid, for example, as described in U.S. Pat. No. 8,648,122, the disclosure of which is incorporated herein in its entirety for any purpose not contrary to the present disclosure.

[0043] In an embodiment, the SRA comprises a mineral oil (MO). As used herein, MO may be any light mixture of alkanes from a mineral source, such as a petroleum distillate, including mixtures of mineral oils from different sources or processes. MO may be, for example, a liquid by-product of the refining of crude oil.

[0044] In an embodiment, the SRA comprises an epoxidized polybutadiene. The epoxidized polybutadiene comprises epoxy groups (or "oxirane oxygen" groups) on the polymer backbone. In an embodiment, the epoxidized polybutadiene can comprise from about 0.01% to about 5.0%, from about 0.01% to about 2.0%, or from about 0.01% to about 1.0% oxirane oxygen. In an embodiment, the epoxidized polybutadiene can have an epoxy value ranging from about 0.1 to about 5.0 meq / g, from about 0.5 to about 3.0 meq / g, or from about 1.0 to about 2.0 meq / g, as measured by ASTM D1652. In an embodiment, the molecular weight of the epoxidized polybutadiene ranges from 800 to 10,000.

[0045] In embodiments, the SRA includes glycerol monostearate (GMS). In embodiments, the PS compositions of the present disclosure include glycerol tristearate (GTS), which is bulkier than GMS and may, in embodiments, impart particularly beneficial properties to the PS foam.

[0046] In embodiments, the SRA further enhances the solubility of the blowing agent in PS for foam extrusion, hi embodiments, the SRA enhances the solubility of the blowing agent in the foamable mixture by at least 5, 7, 10, or 20% over the solubility of the blowing agent in the foamable mixture without the additive.

[0047] Without wishing to be limited by theory, the SRA may act as a permeation barrier in the resulting polystyrene foams of the present disclosure, thus reducing the permeability of the blowing agent through the cell walls of the PS foam.

[0048] In an embodiment, the PS of the PS composition of the present disclosure further comprises one or more additional additives used to impart desired physical properties, such as increased gloss or color. Examples of such additives include, but are not limited to, stabilizers, talc, antioxidants, UV stabilizers, lubricants, plasticizers, UV screeners, oxidants, antioxidants, antistatic agents, UV absorbers, flame retardants, processing oils, release agents, colorants, pigments / dyes, fillers, and the like. The aforementioned additives may be used alone or in combination to form the PS of the PS composition, the PS / alumina composite, and / or the dried PS / alumina composite, or may be added to the PS composition of the present disclosure separately from the PS of the PS composition or the dried PS / alumina composite. For example, stabilizers or stabilizers may be used to help protect the polymer composition from degradation due to exposure to excessive temperature and / or UV light during the formation of the PS. Additives may be added after recovery of the PS during compounding, such as pelletization. These additives may be included in an amount effective to impart the desired properties. Effective amounts of additives and processes for including these additives in polymer compositions to produce PS for use in the PS compositions of the present disclosure are known to those of skill in the art. For example, the additives may be present in the PS or PS composition in an amount of 0.1 wt % to 5 wt %, alternatively 0.1 wt % to 2 wt %, or alternatively 0.1 wt % to 1.0 wt %, based on the total weight of the PS composition or the polymer composition from which the PS of the PS composition of the present disclosure is produced, respectively.

[0049] As noted above, various additional additives can be included within the PS composition. In embodiments, the PS composition of the present disclosure further comprises additives in addition to the SRA and PS (i.e., in addition to any additives used during the formation of the polystyrene and introduced separately from the polystyrene and SRA). In embodiments, for example, foam nucleating agents (e.g., chemical blowing agents as foam nucleating agents, zinc oxide, zirconium oxide, silica, talc, etc.) and / or aging modifiers. (e.g., fatty acid esters, fatty acid amides, hydroxylamides, etc.). Other additives that can be used include pigments, colorants, fillers, stability control agents, antioxidants, flame retardants, stabilizers or co-stabilizers (e.g., thioethers, phosphites, light stabilizers and other functional stabilizers), fragrances, odor masking agents, antistatic agents, lubricants, foaming aids, colorants, anti-aging agents, etc. Such additives are well known to those skilled in the art. In an embodiment, the PS composition of the present disclosure includes an additive (in addition to any additives and any SRA in the PS) selected from the group consisting of antioxidants, flame retardants, infrared (IR) attenuators foaming nucleators, and combinations thereof. In an embodiment, the PS composition of the present disclosure includes the antioxidant IRGANOX® 1010 (pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate)). As noted above, in embodiments, one or more additional additives, such as, but not limited to, toughening agents (e.g., PPO, polyalphamethylstyrene, etc.), are used to improve the mechanical properties of the foam. The additives may also be used in embodiments in the form of a masterbatch. As used herein, a "masterbatch" is a concentrated formulation of an additive.

[0050] The PS composition of the present disclosure may further comprise a blowing agent. In embodiments, any chemical or physical blowing agent may be used. Chemical blowing agents typically decompose at polymer melt conditions. For example, a mixture of sodium bicarbonate and citric acid is commonly used to nucleate fine bubbles. Chemical blowing agents typically decompose between about 100°C and about 140°C to produce at least one gas, such as carbon dioxide, and water. Additionally, solid particles can potentially act as nucleation sites. Once the nucleated bubbles reach a critical size, gas diffusion within the bubble causes the bubble to grow continuously until the bubble is stable and reaches an end stage. Suitable chemical blowing agents are known to those skilled in the art. In embodiments, the blowing agent may be a physical blowing agent. Physical blowing agents may be further classified into two categories, including gases and volatile liquids. Gaseous physical blowing agents may include, but are not limited to, carbon dioxide (CO2), nitrogen (N2), argon (Ar), air, helium (He), hydrogen (H2), xenon (Xe), sulfur hexafluoride (SF6), nitrous oxide (NO), ammonia (NH3), silicon tetrafluoride (SiF4), nitrogen tetrafluoride (NF4), boron tetrafluoride (BF4), boron trichloride (BCl3), or combinations thereof. Thus, in an embodiment, the blowing agent may be carbon dioxide (CO2). Volatile liquid physical blowing agents may include, but are not limited to, liquids such as water, and aliphatic or linear hydrocarbons.

[0051] In embodiments, a single blowing agent or class thereof (e.g., HFC, HFO, HFCs, HFOs) is used. In embodiments, multiple blowing agents are used (e.g., one or more HFOs and / or one or more HFCs, optionally in combination with one or more additional blowing agents). In embodiments, the blowing agent is selected from the group consisting of hydrofluorocarbons (HFCs), hydrofluoroolefins (HFOs), and combinations thereof. In embodiments, the blowing agent or one or more additional blowing agents further comprises one or more components selected from the group consisting of hydrocarbons, carbon dioxide, nitrogen, and combinations thereof. As an example, in embodiments, the blowing agent comprises one or more HFOs, optionally in combination with one or more additional blowing agents selected from the group consisting of hydrocarbons, carbon dioxide, nitrogen, HFCs, and combinations thereof. As an alternative example, in embodiments, the blowing agent comprises one or more HFCs, optionally in combination with one or more additional blowing agents selected from the group consisting of hydrocarbons, carbon dioxide, nitrogen, HFOs, and combinations thereof.

[0052] In an embodiment, the use of the dry PS / alumina composite of the present disclosure in a PS composition increases the solubility of a blowing agent in the PS composition or foamable mixture by increasing the solubility of the blowing agent in the dry PS / alumina composite. The solubility of the blowing agent is increased by at least 5, 10, 15, or 20% greater than the solubility of the blowing agent in another similar PS composition or foamable mixture made without the alumina (i.e., PS is present in approximately equal amounts, but no alumina is present).

[0053] The disclosed PS compositions can have a wet density of about 0.09 g / mL (5.6 pounds per cubic foot ("pcf") or less, as measured by ASTM C578. In embodiments, the disclosed PS compositions can have a wet density in the range of about 0.03 to about 0.09 g / mL (about 1.9 to about 5.6 pcf), about 0.03 to about 0.085 g / mL (about 1.9 to about 5.5 pcf), or about 0.03 to about 0.08 g / mL (about 1.9 to about 5.0 pcf).

[0054] Also disclosed herein are low density polystyrene (PS) foams produced by extrusion of the PS compositions of the present disclosure. In embodiments, the low density polystyrene (PS) foams produced by extrusion of the PS compositions of the present disclosure contain a higher blowing agent concentration than that of an otherwise similar low density PS foam produced by extrusion of a PS composition that does not include (e.g., was not produced with) a dry PS / alumina composite (i.e., PS is present in approximately equal amounts, but no alumina is present). For example, in embodiments, the blowing agent solubility in the PS composition used to produce the foam, and / or the blowing agent concentration in the low density PS foam produced by extrusion of the PS composition of the present disclosure is about 6.5, 7, 7.5, or 8 weight percent or greater.

[0055] In an embodiment, the low density PS foam exhibits at least one equivalent or at least one superior thermal insulation property compared to that of an otherwise similar low density PS foam produced by extrusion of a PS composition not including (e.g., not produced with) a dry PS / alumina composite (i.e., PS is present in about equal amounts, but alumina is not present). The at least one superior thermal insulation property can include an R-value as determined by ASTM C518. In an embodiment, the low density PS foam exhibits at least one mechanical property at least equivalent to that of an otherwise similar low density PS foam produced by extrusion of a PS composition not including (e.g., not produced with) a dry PS / alumina composite (i.e., PS is present in about equal amounts, but alumina is not present). In an embodiment, the at least one mechanical property can be compressive strength (measured by ASTM D3574-C). In embodiments, a low density polystyrene (PS) foam produced by extrusion of a PS composition of the present disclosure that includes a blowing agent comprising one or more hydrofluoroolefins exhibits at least one thermal insulating property at least equivalent to that of an otherwise similar low density PS foam produced by extrusion of a PS composition that does not include (e.g., was not produced with) a dry PS / alumina composite and that includes one or more blowing agents selected from the group consisting of hydrofluorocarbons (HFCs) (i.e., PS is present in approximately equal amounts, but alumina is absent).

[0056] In an embodiment, a low density PS foam produced from a PS composition comprising a dry PS / alumina composite as described herein and a blowing agent comprising one or more hydrofluorocarbons (HFCs) or one or more hydrofluoroolefins (HFOs) comprises a higher concentration of blowing agent compared to that of an otherwise similar low density PS foam produced by extrusion of a PS composition not comprising a dry PS / alumina composite (i.e., PS is present in approximately equal amounts, but alumina is absent). Such low density PS foams can be produced from a PS composition further comprising an additional blowing agent. For example, the additional blowing agent can be selected from the group consisting of a hydrocarbon, CO2, N2, and combinations thereof.

[0057] Without wishing to be limited by theory, it is believed that the PS / alumina composite and / or any SRA additives provide a permeation barrier in the resulting polystyrene foam of the present disclosure. and thus may reduce the permeability of the blowing agent through the cell walls of the PS foam. Thus, the (e.g., low density) polystyrene foams of the present disclosure may exhibit increased retention of blowing agent, e.g., 15, 30, or 60 days after foam formation. In embodiments, the low density polystyrene foams of the present disclosure exhibit at least 0, 5, 10, 15, or 20% greater blowing agent retention, as determined, e.g., by GC headspace methods, than an otherwise similar polystyrene foam made in the absence of the PS / alumina composite and / or optional SRA additive (i.e., PS is present in approximately equal amounts, but alumina and / or optional SRA additive are absent).

[0058] The disclosed low density polystyrene foams can have any desired thickness to suit the intended application. For example, in embodiments, the disclosed polystyrene foams can be in the form of sheets or planks having thicknesses ranging from about 1 / 32 inch to about 2.0 inches. However, thinner or thicker foams are also within the scope of the subject matter disclosed herein. The low density polystyrene foams can have any desired density, such as, but not limited to, a wet density of about 0.09 g / mL (5.6 pounds per cubic foot ("pcf")) or less as measured by ASTM C578. In embodiments, the low density polystyrene foams can have a wet density ranging from about 0.02 to about 0.09 g / mL, about 0.03 to about 0.08 g / mL, about 0.04 to about 0.08 g / mL, or about 0.04 to about 0.06 g / mL.

[0059] In embodiments, the disclosed polystyrene foams can have an average cell size of at least about 50 microns. In embodiments, the disclosed foams can have an average cell size of up to about 1000 microns. Average cell size can be measured according to ASTM D3576-98 (Procedure A).

[0060] The disclosed polystyrene foams can be in any of a wide variety of configurations, such as, but not limited to, sheets, planks, slabs, blocks, boards, rods, beads, and molded shapes.

[0061] A method of making a PS foam according to the present disclosure includes forming a dry PS / alumina composite, blending the dry PS / alumina composite, a blowing agent, and optionally one or more additional additives to form a foamable mixture, and producing a PS foam by extruding the foamable mixture through a die into a region of reduced pressure. According to the present disclosure, the PS / alumina composite must be thoroughly dried (i.e., have a moisture content of about 0.05% by weight or less, as measured by a coulometer) to form a dry PS / alumina composite prior to extrusion foaming. According to this disclosure, moisture absorption during foam extrusion is minimized. Forming a dry PS / alumina composite can include combining PS with an alumina additive to form a PS / alumina composite, and optionally removing moisture from the PS / alumina composite to form a dry PS / alumina composite, the dry PS / alumina composite having a moisture content of about 0.05 weight percent (wt%) or less, as measured by a coulometer. In an embodiment, the combination of the PS and the alumina additive results in a dry PS / alumina composite, i.e., the PS and the alumina additive are sufficiently dry prior to combination such that their combination (without further moisture removal) results in a PS / alumina composite having the requisite moisture content (e.g., about 0.05 weight percent (wt %) or less as measured by coulometer), and thus the PS / alumina composite is considered a dry PS / alumina composite.

[0062] To form the PS / alumina composite, the PS and alumina additives can be combined in any suitable manner known to one of ordinary skill in the art. For example, in embodiments, the PS and alumina additives are combined by extrusion to provide the PS / alumina composite. The lumina additive and / or PS may optionally be dried prior to combining the alumina additive with the PS. For example, in embodiments, the alumina additive may be dried by heating the alumina additive to an elevated temperature (e.g., greater than about 120° C., 200° C., or 250° C.) and / or by maintaining the temperature at an elevated temperature for a period of time sufficient to reduce the moisture content of the alumina additive to a moisture content of less than or equal to about 0.05, 0.03, or 0 weight percent (wt%), e.g., as measured by a coulometer (e.g., for a period of about 2, 3, or 4 hours or more).

[0063] Removing moisture from the PS / alumina composite to form a dry PS / alumina composite can be done by any means known to one of skill in the art, and with the aid of the present invention, suitable to reduce the moisture content of the PS / alumina composite to provide a dry PS / alumina composite having a moisture content of about 0.05% by weight or less as measured by coulometer. For example, removing moisture can include heating the PS / alumina composite to an elevated temperature (e.g., about 50, 60, 70, or 80° C. or higher) and / or maintaining the elevated temperature for a sufficient period of time (e.g., about 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12 hours or more) to provide a dry PS / alumina composite.

[0064] The disclosed polystyrene foams can be constructed from the dry PS / alumina composite using any process known in the art. For example, in embodiments, the PS foam is produced by blending the dry PS / alumina composite, a blowing agent, and optionally one or more additional additives (such as, for example, the blowing agents and additives described herein above) to form a foamable mixture, and extruding the foamable mixture through a die into a region of reduced pressure to produce the foam.

[0065] In embodiments, any chemical or physical blowing agent as described above may be used. As will be apparent to one skilled in the art, the blowing agent acts by foaming the thermoplastic resin to produce a porous thermoplastic structure having a density substantially lower than the resin from which the foam is made. Gas bubbles form around "nucleation sites" and expand by heating or vacuum, or by the process of a chemical reaction in which gas is generated. Nucleation sites are small particles or agglomerations of small particles that promote the formation of bubbles in the resin. In embodiments, one or more additives may be incorporated into the resin to promote the nucleation of a particular blowing agent, thereby providing a more uniform pore distribution. In embodiments, alumina serves as the foam nucleating agent for the PS composition of the present disclosure, and no additional nucleating agent is used to form the low density PS foam of the present disclosure.

[0066] The total amount of blowing agent in the PS composition used to prepare the disclosed PS foam structures depends on conditions such as the temperature and pressure at which the blowing agent is dissolved in the polymer, the chemical and thermophysical properties of the blowing agent used, and the desired density and related properties (insulation value, weight-to-strength ratio, compressive strength, etc.) of the resulting foamed article. Thus, in embodiments, the blowing agent can be mixed with the dry PS / alumina composite in an amount suitable to achieve the desired degree of expansion in the resulting PS foam. For example, in embodiments, the blowing agent can be added to the dry PS / alumina composite in an amount ranging from about 0.5 to about 15 parts by weight; in embodiments, from about 2 to 10 parts by weight; and in embodiments, from about 3 to 9 parts by weight, based on 100 parts by weight of the PS composition or foamable mixture.

[0067] In an embodiment, the disclosed polystyrene foam can be constructed using a continuous extrusion process. In this method, the dry PS / alumina composite and any additional additives are blended together and added to an extruder. In an embodiment, one or more additional additives can be added in masterbatch form. Any conventional extruder can be used, for example, single screw, twin screw, and / or tandem extruders. In the extruder, the dry PA / alumina composite and any additional additives are melted and mixed to form the PS / alumina composite. The blowing agent is added to the molten PS / alumina blend through one or more inlets of the extruder. Any additional additives to be used can be added to the molten PS / alumina blend in the extruder and / or with the PS resin pellets and / or dry PS / alumina composite as described herein above. The extruder extrudes the entire molten mixture (molten PS / alumina blend, blowing agent, and any additional additives) through a die at the end of the extruder into a region of reduced temperature and pressure relative to the temperature and pressure within the extruder. Any of a wide variety of dies can be used, including but not limited to strand, annular, flat, coextrusion, and microlayered dies. In embodiments, the region of reduced temperature and pressure may be at ambient atmospheric pressure. The sudden pressure drop with the gas-filled polymer exiting the die results in thermodynamic instability. The nucleating agent (e.g., alumina) creates a large number of bubbles that grow by diffusing the vaporized gas into the growing bubbles. The foam continues to expand until the bubbles grow and stabilize. The foam surface solidifies upon cooling of the polymer mass due to the reduction in temperature, thereby trapping the blowing agent within the cells, thereby forming extruded polystyrene foam.

[0068] Alternatively, in embodiments, the disclosed polystyrene foam can be constructed using a batch process. In such embodiments, the polystyrene blend (i.e., the dry PS / alumina composite and any desired additional additives) is added to a vessel, such as a pressure chamber. The vessel is heated to a specific temperature or temperature range sufficient to plasticize the polystyrene resin. A blowing agent is then added to the vessel to a specific pressure or pressure range, allowing the blowing agent to infiltrate the polystyrene resin for a period of time. The pressure is rapidly released, thereby allowing the resin to expand into PS foam.

[0069] The subject matter disclosed herein also includes additional foaming methods, including, but not limited to, solid phase foaming, integral skin foaming, microcellular foaming, autoclave foaming, and semi-continuous foaming processes. Such methods are well known to those skilled in the art of foaming technology. In embodiments, optional additional additives (e.g., SRA, flame retardants, IR attenuators / suppressants, antioxidants, and / or others) may be added to otherwise conventional polystyrene formulations as masterbatches.

[0070] As described herein, the methods disclosed herein can be used to construct polystyrene foam using physical blowing agents (e.g., one or more HFOs, one or more HFCs, carbon dioxide and / or others). Depending on the materials and processes used, the resulting foam article can be beads, sheets, boards, planks, rods, tubes, profiled members, etc. The disclosed polystyrene foam can be used as is, cut into other shapes, further molded or thermoformed by application of heat or pressure, or otherwise machined or formed into desired sizes and shapes, as is well known to those skilled in the packaging art.

[0071] The disclosed polystyrene foams can be used for any of a wide variety of purposes. For example, in embodiments, the disclosed polystyrene foams can be used in various containers and packaging systems for thermal insulation, and / or as protective or flexible packaging. Thus, in embodiments, the disclosed polystyrene foams can be thermoformed into containers, such as, but not limited to, trays, bowls, and / or plates, used in flexible and rigid packaging, used in a variety of protective packaging applications, used in loose-fill packaging, and / or molded into sheets, planks, boards, or contoured articles for flexible, protective, rigid, and / or thermal insulation applications.

[0072] As described above, the PS compositions and methods for producing PS foams therefrom disclosed herein The process may allow for greater solubility of the blowing agent in the PS during extrusion and / or a higher concentration of the blowing agent in the resulting PS foam. Incorporation of a higher concentration of the blowing agent in the resulting polystyrene foam may provide improved thermal insulation properties thereof.

[0073] Furthermore, it has been found that when a dry PS / alumina composite is used to form a PS composition according to the present disclosure, the PS composition can be foamed in the presence of a physical blowing agent, such as carbon dioxide and / or HFO. In embodiments, the non-flammable and / or low GWP of the blowing agent allows for improved safety and / or environmental friendliness compared to traditional flammable or high GWP hydrocarbons. The use of a physical blowing agent may also help to reduce the cure time of the foam, which may save time, effort, and money. EXAMPLES

[0074] Having generally described the embodiments, the following examples are given as specific embodiments of the disclosure and to demonstrate its practice and advantages. It is understood that the examples are given for illustrative purposes and are not intended to limit the scope of the specification or claims in any way.

[0075] Example 1 In this example, three PS foams were produced and studied, including a first comparative foam C1 made with a PS composition comprising standard polystyrene PS533 and no alumina additive, a second comparative foam C2 made with a PS composition comprising PS533 and a wet PS / alumina composite comprising 1 wt. % alumina additive and water, and a PS foam I1 of the present invention made with a dry PS / alumina composite comprising PS533 and 1 wt. % alumina additive and dried to substantially no moisture, e.g., by drying in a nitrogen purged oven at 250°C for about 2 hours. The alumina additive used in this example was Sasol CATAPAL® C1, whose relevant properties are a particle size distribution of 60 microns, d 50 The results are provided in Table 1 above, including:

[0076] Specifically, the first comparative foam C1 was a standard foam made from polystyrene PS533 dry blended with 0.5% talc masterbatch for foam extrusion. PS533 has an MFR of 4.5 g / 10 min and is available from Total Petrochemicals and Refining USA, Inc. A number of PS / alumina composites containing PS533 and 1 wt. % dry alumina additive were produced in a 1.25" single screw extruder. The PS / alumina composite was dried and then split into two. Drying included drying at 250°C for about 2 hours in a nitrogen purged oven. The first half of the dried PS / alumina composite was used directly for foam extrusion to form the inventive foam I1. Deionized water in an amount of 0.75 wt. % was added to the other half of the PS / alumina composite, which was then left overnight to allow for sufficient moisture absorption before foam extrusion to form the second comparative foam C2.

[0077] The foam extrudates were evaluated on an Applications Laboratory Davis Standard foam line. As described above, Comparative Foam C1 was formed from PS533 dry blended with 0.5% talc masterbatch as a nucleating agent for the foam extrusion. The alumina additive acted as a foam nucleating agent in the PS / alumina composite used to form Second Comparative Foam C2 and Inventive Foam I1, therefore no additional nucleating agent was added to the PS composition used to form Second Comparative Foam C2 and Inventive Foam I1.

[0078] The PS compositions were evaluated for foam extrusion using various amounts of HFC 134a (also known as R134a) as the blowing agent. The PS compositions were foamed in a tandem foam extrusion line containing a 0.75" primary extruder and a 1.5" secondary extruder. Specifically, samples were placed in the hopper of the primary extruder. The blowing agent, HFC 134a, was fed to the primary extruder through a MaxPro fluid pump. The homogenized melt was fed to the secondary extruder through a Nordson Xaloy melt pump. The temperature of the secondary extruder was adjusted to maintain a constant die head pressure of 1100-1200 psi at different HFC 134a blowing agent levels. As the melt exited the die, low density foams were produced. A 5mm rod die was used for extrusion of all samples. A gear pump was used to control the extrusion throughput to 6.5-7 lbs / hr. Maximum HFC 134a solubility was defined as the blowing agent level at which premature foaming became visible (eg, foam density increased).

[0079] First Comparative Example C1 PS foam C1, made with standard PS533 polystyrene, produced foams with consistent cell structure at less than 7% blowing agent HFC 134a. However, at higher HFC 134a blowing agent levels, premature foaming became noticeable and very likely in front of the breaker plate near the die head, resulting in foam defects with inconsistent foam cell structure. Under the foaming conditions established in the small laboratory line, the maximum HFC 134a blowing agent solubility for PS compositions containing standard PS533 and no alumina additive was determined to be about 7 wt% HFC 134a. FIG. 1A provides an image of the first comparative foam sample C1 of this example containing 7 wt% blowing agent HFC 134a, and FIG. 1B provides an image of the first comparative foam sample C1 of this example containing 8 wt% blowing agent HFC 134a.

[0080] Second Comparative Example The wet PS533 / alumina composite was examined for foam extrusion under standard conditions. Similar to what was seen for the first comparative foam C1, the second comparative foam C2 was produced with consistent cell structure when the HFC 134a blowing agent concentration was less than 7 wt%. Due to the presence of abundant moisture, bi-cellular foams could be produced. However, HFC 134a concentrations of 7 wt% or more significantly reduced the quality of the second comparative C2 foam resulting in premature foaming. Thus, moisture is not an effective plasticizer for crystalline PS and did not provide an advantage at high HFC 134a levels compared to the first comparative C1 foam without alumina. Overall, the maximum HFC 134a solubility in the wet PS / alumina composite used to produce the second comparative foam C2 was at most 7%, similar to what was seen for the first comparative C1 foam. FIG. 2A provides an image of a second comparative foam sample C2 of this example containing 6 wt. % of the blowing agent HFC 134a, and FIG. 2B provides an image of a second comparative foam sample C2 of this example containing 7 wt. % of the blowing agent HFC 134a.

[0081] Invention Example Dry PS533 / alumina composites were examined for foam extrusion under standard conditions for producing inventive foam I1. As with the standard PS533 used to produce the first comparative foam C1 and the wet PS / alumina composite used to produce the second comparative foam C2, very good foams (e.g., foams with consistent cell structure) were produced using the dry PS / alumina composites when the HFC 134a blowing agent concentration was less than 7 wt.%. Successful I1 foams were also produced at HFC 134a levels above 8.5 wt.%.

[0082] Figure 3A provides an image of inventive foam sample I1 of this example containing 6 wt% blowing agent HFC 134a, Figure 3B provides an image of inventive foam sample I1 containing 7 wt% blowing agent HFC 134a, and Figure 3C provides an image of inventive foam sample I1 containing 8.5 wt% blowing agent HFC 134a. As can be seen in Figures 3A-3C, expanded foams with consistent cell structure were produced even with 9 wt% blowing agent HFC 134a in the dry PS53 foam. 3 / alumina composite, showing an improvement over the second comparative foam C2 obtained using a wet PS533 / alumina composite with 7.5% 134a. It should also be noted that the relatively low foam density (e.g., of the inventive I1 foam) was produced from the dry PS533 / alumina composite at higher HFC 134a levels. Based on the established protocol, the maximum HFC 134a solubility in the dry PS533 / alumina composite appeared to be about 9 wt%. Figure 4 shows a side-by-side comparison of the second comparative foam sample C2 at 7 wt% and 7.5 wt% HFC 134a blowing agent with the inventive foam sample I1 at 9 wt% HFC 134a blowing agent. Figure 5 is a plot of wet density (g / cc) as a function of blowing agent HFC 134a concentration (wt%) for the first comparative foam C1, second comparative foam C2, and inventive foam I1 of this example. Wet density was measured by ASTM C578. Overall, the use of pre-dried PS533 / 1 wt% alumina composite in the PS composition significantly improved the solubility of the HFC 134a blowing agent. The porosity of the dried alumina additive was expected to facilitate increased absorption of the HFC 134a blowing agent in the PS composite. Although only 1% alumina was used in this example, it was interesting to find that the pre-dried PS / alumina composite could be processed at a maximum HFC 134a blowing agent concentration of more than 9 wt%. This equates to a more than 20% increase in blowing agent solubility in the PS composition containing the dried PS / alumina composite used to make the inventive foam I1 compared to the PS composition containing PS 533 and no alumina additive used to make the first comparative foam C1. Additional alumina can be used to further improve the solubility of the HFC 134a blowing agent in the PS composition used to make the PS foam, and thus the blowing agent concentration in the resulting PS foam.

[0083] Although various embodiments have been shown and described, modifications thereof may be made by one skilled in the art without departing from the spirit and teachings of the present disclosure. The embodiments described herein are illustrative only and are not intended to be limiting. Many variations and modifications of the subject matter disclosed herein are possible and are within the scope of the present disclosure. When a numerical range or limit is explicitly stated, such an explicit range or limit should be understood to include iterative ranges or limits of similar magnitude that are within the explicitly stated range or limit (e.g., about 1 to about 10 includes 2, 3, 4, etc., and greater than 0.10 includes 0.11, 0.12, 0.13, etc.). For example, a lower limit, R L and upper limit, R U Whenever a numerical range having a value of R = R is disclosed, any number falling within that range is specifically disclosed. In particular, numbers within the following ranges are specifically disclosed: R = R L +k * (R U -R L ), where k is a variable ranging from 1 percent to 100 percent in 1 percent increments, i.e., k is 1 percent, 2 percent, 3 percent, 4 percent, 5 percent, ... 50 percent, 51 percent, 52 percent, ..., 95 percent, 96 percent, 97 percent, 98 percent, 99 percent, or 100 percent. Additionally, any numerical range defined by two R numbers defined above is also specifically disclosed. Use of the term "optionally" with respect to any element of a claim is intended to mean that the subject element is required, or alternatively is not required. Both alternatives are intended to be within the scope of the claim. Use of broader terms such as comprise, include, having, etc. should be understood to provide support for narrower terms such as consisting of, consisting essentially of, and consisting essentially of.

[0084] Thus, the scope of protection is not limited by the above description, but only by the following claims, including all equivalents of the subject matter of the claims. Each claim is incorporated herein as an aspect of the disclosure. The claims are thus further explanation and in addition to the aspects of the disclosure. The discussion of a reference is not an admission that it is prior art to the disclosure, especially any reference that may have a publication date after the priority date of this application. All patents cited herein are incorporated by reference in their entirety. The disclosures of the patent applications and publications, to the extent that they provide exemplary, procedural, or other details supplementary to those set forth herein, are incorporated herein by reference.

[0085] Further explanation The particular embodiments disclosed above are illustrative only, as the disclosure may be modified and practiced in different but equivalent manners apparent to those skilled in the art having the benefit of the teachings herein. Moreover, no limitations are intended to the details of construction or design shown herein, other than as described in the claims that follow. It is therefore apparent that the particular exemplary embodiments disclosed above may be altered and modified, and all such variations are deemed to be within the scope and spirit of the disclosure. Alternative embodiments resulting from combining, combining, and / or omitting features of the embodiments are also within the scope of the disclosure. Although the compositions and methods are described in broader terms such as "having," "comprising," "containing," or "including" various components or steps, the compositions and methods can also "consist essentially of" or "consist of" various components and steps. The use of the term "optionally" with respect to any element of a claim means that the element is required, or alternatively, that the element is not required, and both alternatives are within the scope of the claim.

[0086] The numbers and ranges disclosed above may vary by a certain amount. Whenever a numerical range with a lower and upper limit is disclosed, any number falling within that range and any included range is specifically disclosed. In particular, each range of values ​​disclosed herein (in the form of "about a to about b", or equivalently "approximately a to b", or equivalently "approximately a to b") should be understood to represent each number and range encompassed within the broader range of values. Moreover, the terms in the claims have their plain and ordinary meaning unless expressly and unambiguously defined by the patent owner. Moreover, the indefinite article "a" or "an" used in the claims is defined herein to mean one or more of the element it introduces. In the event of any inconsistency in the use of a word or term in this specification and one or more patents or other documents, the non-inconsistent definition in this specification should be adopted.

[0087] Aspects disclosed herein include the following:

[0088] Aspect A: A polystyrene (PS) composition for producing an extruded foam, the PS composition comprising: a dry PS / alumina composite comprising PS and an alumina additive, the dry PS / alumina composite having a moisture content of about 0.05 weight percent (wt%) or less as measured by coulometer; and a blowing agent.

[0089] Aspect B: A low density polystyrene (PS) foam produced by extrusion of the PS composition of Aspect A, wherein the low density PS foam comprises a higher blowing agent concentration than that of an otherwise similar low density PS foam produced by extrusion of a PS composition that does not include the dry PS / alumina composite.

[0090] Aspect C: A low density polystyrene (PS) foam produced by extrusion of the PS composition of Aspect A, wherein the low density PS foam exhibits at least one superior thermal insulation property as compared to that of an otherwise similar low density PS foam produced by extrusion of a PS composition that does not include the dry PS / alumina composite.

[0091] Aspect D: A low density polystyrene (PS) foam produced by extrusion of the PS composition of aspect A, wherein the low density PS foam has a density at least equal to that of an otherwise similar low density PS foam produced by extrusion of a PS composition that does not include a dry PS / alumina composite. A low density polystyrene (PS) foam exhibiting at least one mechanical property.

[0092] Aspect E: A low density polystyrene (PS) foam produced by extrusion of the PS composition of Aspect A, wherein the blowing agent comprises one or more hydrofluoroolefins (HFOs), wherein the low density PS foam does not comprise a dry PS / alumina composite and exhibits at least one thermal insulation property at least similar to that of an otherwise similar low density PS foam produced by extrusion of a PS composition comprising one or more blowing agents selected from the group consisting of hydrofluorocarbons (HFCs).

[0093] Aspect F: A method for making a low density polystyrene (PS) foam comprising: forming a polystyrene (PS) / alumina composite comprising PS and an alumina additive; removing moisture from the PS / alumina composite to form a dry PS / alumina composite, the dry PS / alumina composite having a moisture content of about 0.05 weight percent (wt%) or less as measured by a coulometer; blending the dry PS / alumina composite, a blowing agent, and optionally one or more additional additives to form a foamable mixture; and producing a foam by extruding the foamable mixture through a die into a region of reduced pressure.

[0094] Embodiment G: A low density polystyrene (PS) foam produced by the method of embodiment F.

[0095] Embodiment H: The low density PS foam of embodiment G, wherein the low density PS foam comprises a higher blowing agent concentration and / or exhibits at least one superior thermal insulating or mechanical property as compared to that of an otherwise similar low density PS foam produced by extrusion of a foamable mixture that does not include the dry PS / alumina composite.

[0096] Aspect I: A dried polystyrene (PS) / alumina composite for producing an extruded foam, the dried PS / alumina composite comprising an extruded mixture of PS and an alumina additive, the extruded mixture being dried to provide a dried PS / alumina composite such that the dried PS / alumina composite has a moisture content of about 0.05 weight percent (wt %) or less as measured by coulometer, the dried PS / alumina composite comprising about 0.01 to about 20.0 weight percent (wt %) of the alumina additive.

[0097] J: A low density polystyrene (PS) foam produced by extrusion of a PS composition, comprising: a dry PS / alumina composite comprising PS and an alumina additive, the dry PS / alumina composite having a moisture content of about 0.05 weight percent (wt%) or less as measured by a coulometer; and a blowing agent, the PS composition comprising about 7 weight percent or more of the blowing agent.

[0098] Each of embodiments A, B, C, D, E, F, G, H, I, and J may have one or more of the following additional elements: Element 1: The dry PS / alumina composite includes about 0.01 to about 20.0 weight percent (wt%) of an alumina additive. Element 2: The alumina additive includes Sasol CATAPAL® C1. Element 3: The PS includes crystal polystyrene, high impact polystyrene (HIPS), a PS copolymer, or a combination thereof. Element 4: The PS copolymer includes a metal monomer, glycidyl methacrylate, 2-hydroxyethyl methacrylate, acrylonitrile, or a combination thereof. Element 5: The PS has a melt flow rate (MFR) in the range of 0.2 to 30 grams (g) / 10 minutes (min) as measured by ASTM D-1238. Element 6: Additives including glycerol monostearate (GMS), glycerol tristearate (GTS), mineral oil (MO), epoxidized soybean oil (ESO), epoxidized polybutadiene, or combinations thereof. Element 7: about 0.01 to 10.0 weight percent (wt%) of an additive, the weight percent being based on the total amount of polystyrene and additive in the PS composition. Element 8: further comprising an additive selected from the group consisting of an antioxidant, a flame retardant, and combinations thereof. Element 9: the solubility of the blowing agent in the PS composition is about 7 weight percent or greater. Element 10: the blowing agent is selected from the group consisting of a hydrofluorocarbon (HFC), a hydrofluoroolefin (HFO), carbon dioxide (CO2), and combinations thereof. Element 11: the dry polystyrene (PS) / alumina composite comprises about 0.01 to about 20.0 weight percent (wt%) of an alumina additive. Element 12: the solubility of the blowing agent in the foamable mixture is at least 5, 10, 15, or 20% greater than the solubility of the blowing agent in an otherwise similar foamable mixture produced without the dry PS / alumina composite. Element 13: The one or more additional additives are selected from the group consisting of glycerol monostearate (GMS), glycerol tristearate (GTS), mineral oil (MO), epoxidized soybean oil (ESO), epoxidized polybutadiene, flame retardants, antioxidants, and combinations thereof. Element 14: The blowing agent comprises one or more hydrofluoroolefins, and the low density PS foam exhibits at least one thermal insulation property at least equivalent to an otherwise similar low density PS foam produced by extrusion of a foamable mixture that does not include a dry PS / alumina composite and that includes one or more blowing agents selected from the group consisting of hydrofluorocarbons (HFCs). Element 15: The blowing agent comprises one or more hydrofluorocarbons (HFCs) or one or more hydrofluoroolefins (HFOs), and the low density PS foam comprises a higher concentration of blowing agent compared to that of an otherwise similar low density PS foam produced by extrusion of a foamable mixture that does not include a dry PS / alumina composite. Element 16: Further comprising an additional blowing agent selected from the group consisting of hydrocarbons, CO2, and combinations thereof.

[0099] Although preferred embodiments of the present invention have been shown and described, modifications of the present invention can be made by one skilled in the art without departing from the teachings of the present disclosure. The embodiments described herein are illustrative only and are not intended to be limiting. Many variations and modifications of the invention disclosed herein are possible and are within the scope of the invention.

[0100] Numerous other modifications, equivalents, and alternatives will become apparent to those skilled in the art once the above disclosure is fully appreciated. It is intended that the following claims be interpreted to encompass all such modifications, equivalents, and alternatives, where applicable. Thus, the scope of protection is not limited by the above description, but only by the following claims, including all equivalents of the subject matter of the claims. Each claim is incorporated herein as an embodiment of the present invention. Thus, the claims are further explanation and additions to the detailed description of the present invention. The disclosures of all patents, patent applications, and publications cited herein are incorporated herein by reference.

Claims

1. 1. A polystyrene (PS) composition for producing an extruded foam comprising: a dry PS / alumina composite comprising PS and an alumina additive, the dry PS / alumina composite having a moisture content of 0.05 weight percent (wt%) or less as measured by a coulometer; Foaming agent and A polystyrene (PS) composition comprising:

2. 10. The PS composition of claim 1, wherein the dry PS / alumina composite comprises 0.01 to 20.0 weight percent (wt%) of the alumina additive.

3. 2. The PS composition of claim 1, wherein the alumina additive comprises Sasol CATAPAL® C1.

4. 10. The PS composition of claim 1, wherein the PS comprises crystal polystyrene, high impact polystyrene (HIPS), a PS copolymer, or a combination thereof.

5. The PS composition of claim 4, wherein the PS copolymer comprises a metal monomer, glycidyl methacrylate, 2-hydroxyethyl methacrylate, acrylonitrile, or a combination thereof.

6. 10. The PS composition of claim 1, wherein the PS has a melt flow rate (MFR) in the range of 0.2 to 30 grams (g) / 10 minutes (min), as measured by ASTM D-1238.

7. 10. The PS composition of claim 1, further comprising an additive comprising glycerol monostearate (GMS), glycerol tristearate (GTS), mineral oil (MO), epoxidized soybean oil (ESO), epoxidized polybutadiene, or a combination thereof.

8. The PS composition of claim 7, comprising 0.01 to 10.0 weight percent (wt %) of the additive, the weight percent being based on the total amount of polystyrene and additive in the PS composition.

9. 10. The PS composition of claim 1, wherein the solubility of the blowing agent in the PS composition is 7 weight percent or greater.

10. 10. A low density polystyrene (PS) foam produced by extrusion of the PS composition of claim 1, wherein the low density PS foam comprises a higher blowing agent concentration than that of a low density PS foam produced by extrusion of a PS composition comprising polystyrene (PS) without alumina or comprising a wet PS / alumina composite, and comprising no dry PS / alumina composite.

11. The blowing agent is a hydrofluorocarbon (HFC), a hydrofluoroolefin (HFO), or carbon dioxide (CO 2 11. The low density PS foam of claim 10, wherein the polyvinyl chloride (Pc) is selected from the group consisting of phenyl, ...

12. 1. A method for producing a low density polystyrene (PS) foam comprising the steps of: forming a polystyrene (PS) / alumina composite containing PS and an alumina additive; removing moisture from the PS / alumina composite to form a dry PS / alumina composite, the dry PS / alumina composite having a moisture content of 0.05 weight percent (wt%) or less as measured by a coulometer; blending the dry PS / alumina composite, a blowing agent, and optionally one or more additional additives to form a foamable mixture; generating a foam by extruding the foamable mixture through a die into a region of reduced pressure; A method comprising:

13. The method of claim 12, wherein the dry polystyrene (PS) / alumina composite comprises 0.01 to 20.0 weight percent (wt %) of the alumina additive.

14. 13. The method of claim 12, wherein the solubility of the blowing agent in the foamable mixture is at least 5, 10, 15, or 20% greater than the solubility of the blowing agent in a foamable mixture made with polystyrene (PS) without alumina or with a wet PS / alumina composite and without a dry PS / alumina composite.

15. 13. A low density polystyrene (PS) foam produced by the method of claim 12.

16. 16. The low density PS foam of claim 15, wherein the low density PS foam comprises a higher blowing agent concentration and / or exhibits at least one superior thermal insulating or mechanical property compared to that of a low density PS foam produced by extrusion of a foamable mixture comprising polystyrene (PS) without alumina or comprising a wet PS / alumina composite and not a dry PS / alumina composite.

17. 16. The low density PS foam of claim 15, wherein the blowing agent comprises one or more hydrofluoroolefins, and the low density PS foam exhibits at least one thermal insulation property at least equivalent to that of a low density PS foam produced by extrusion of a foamable mixture comprising polystyrene (PS) without alumina or comprising a wet PS / alumina composite and comprising one or more blowing agents selected from the group consisting of hydrofluorocarbons (HFCs), without a dry PS / alumina composite.

18. 16. The low density PS foam of claim 15, wherein the blowing agent comprises one or more hydrofluorocarbons (HFCs) or one or more hydrofluoroolefins (HFOs), and the low density PS foam comprises a higher concentration of blowing agent compared to that of a low density PS foam produced by extrusion of a foamable mixture comprising polystyrene (PS) without alumina or comprising a wet PS / alumina composite and not a dry PS / alumina composite.

19. Hydrocarbons, CO 2 20. The low density PS foam of claim 18, further comprising an additional blowing agent selected from the group consisting of:

20. 1. A dry polystyrene (PS) / alumina composite for producing an extruded foam, the dry PS / alumina composite comprising an extruded mixture of PS and an alumina additive, the dry PS / alumina composite being dried to provide a dry PS / alumina composite having a moisture content of 0.05 weight percent (wt%) or less as measured by a coulometer, the dry PS / alumina composite comprising 0.01 to 20.0 weight percent (wt%) of the alumina additive.

21. 1. A low density polystyrene (PS) foam produced by extrusion of a PS composition comprising: a dry PS / alumina composite comprising PS and an alumina additive, the dry PS / alumina composite having a moisture content of 0.05 weight percent (wt%) or less as measured by a coulometer; a blowing agent, wherein the PS composition comprises 7 weight percent or more of the blowing agent.

Citation Information

Patent Citations

  • Polymer foam containing alumina bemite

    JP2012522070A

  • Biodegradable resin composition, method of manufacturing biodegradable foamed sheet, biodegradable foamed sheet and biodegradable foamed molded product

    JP2013023576A

  • Foamed product exhibiting improved thermal properties

    JP2013528248A

  • Foamed Articles Exhibiting Improved Thermal Properties

    US20110306691A1

  • Polymeric foam containing alumina boehmite

    US20120025126A1