Glass fiber reinforced polycarbonate composite material, its manufacturing method and use

A glass fiber reinforced polycarbonate composite material with controlled siloxane and phosphorus-to-silicon ratios addresses the stiffness-toughness trade-off, enhancing fluidity and mechanical properties for applications in automobiles, electronics, and construction.

JP7562643B2Active Publication Date: 2024-10-07KINGFA SCI & TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022513362
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-30
Filing Date
2020-07-24
Publication Date
2024-10-07
Estimated Expiration
2040-07-24

AI Technical Summary

Technical Problem

Traditional glass fiber reinforced polycarbonate composite materials face a trade-off between high stiffness and low toughness, and traditional toughening methods affect fluidity, limiting their application in industries like automobiles, electronics, and construction.

Method used

A glass fiber reinforced polycarbonate composite material comprising specific ratios of polycarbonate, polysiloxane block copolymer, glass fiber, phosphorus-containing compound, and polyolefin compound, with controlled siloxane and phosphorus-to-silicon ratios, processed using a twin-screw extruder.

Benefits of technology

The composite material achieves high elastic modulus, toughness, and excellent fluidity, making it suitable for demanding applications in automobiles, electronics, and construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562643000001
    Figure 0007562643000001
  • Figure 0007562643000002
    Figure 0007562643000002
Patent Text Reader

Abstract

The present invention discloses a glass fiber-reinforced polycarbonate composite, its manufacturing method, and use. The glass fiber-reinforced polycarbonate composite comprises 40 to 90 parts of Component A: polycarbonate, 1.5 to 50 parts of Component B: polysiloxane block copolymer, 5 to 60 parts of Component C: glass fiber, 0.1 to 30 parts of a phosphorus-containing compound, and 0.01 to 30 parts of a polyolefin compound. The present invention adds specific amounts of the polysiloxane block copolymer, phosphorus-containing compound, and polyolefin compound to the glass fiber-reinforced polycarbonate composite formulation, thereby ensuring a specific siloxane content and specific weight ratio of phosphorus to silicon in the final composite. This results in a composite with a high modulus, high toughness, and excellent processability. Compared with conventional reinforcement and modification methods, this composite combines rigidity and toughness, making it particularly suitable for applications in the automotive, electronics / electrical, communications, and construction industries.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of engineering plastics, in particular to glass fiber reinforced polycarbonate composites, their preparation method and use. [Background technology]

[0002] Polycarbonate resin PC is a thermoplastic engineering plastic with excellent comprehensive performance. In recent years, due to its characteristics such as high transparency, good flame retardancy, heat resistance, electrical insulation, dimensional stability, and low water absorption, it has been widely used in the fields of automobiles, electronics and electrical equipment, communication industries, and construction industries. With the development of its application fields, the requirements for the performance of polycarbonate such as impact strength, flexural modulus, tensile strength, fluidity, and dielectric loss are all increasing, and simple polycarbonate or ordinary polycarbonate materials cannot meet the requirements, so it is necessary to carry out modification treatment on polycarbonate materials. In order to improve the performance and grade of the material and meet the needs of the final parts and customers, it is generally necessary to improve the processability and modification by glass fiber reinforcement.

[0003] However, conventional glass fiber reinforced polycarbonate composite materials have a contradiction between high rigidity and low toughness. On the other hand, the usual toughening method is to directly add a toughening agent, which also greatly reduces the fluidity of the composite material. Moreover, the improvement of the rigidity and toughness of the composite material is also very limited, which severely restricts its application in fields such as automobiles, electronics and electrical appliances, communication industries, and construction industries. Summary of the Invention [Problem to be solved by the invention]

[0004] SUMMARY OF THE PRESENT EMBODIMENT In order to overcome the shortcomings and deficiencies of the prior art, the object of the present invention is to provide a glass fiber reinforced polycarbonate composite material that combines stiffness and toughness with high flowability.

[0005] Another object of the present invention is to provide a method for producing the above glass fiber reinforced polycarbonate composite material.

[0006] Yet another object of the present invention is to provide uses of the above glass fiber reinforced polycarbonate composite material. [Means for solving the problem]

[0007] The present invention is achieved by the following technical solutions:

[0008] 1. A glass fiber reinforced polycarbonate composite material, comprising: Component A: 40 parts by weight to 90 parts by weight of polycarbonate, Component B: 1.5 parts by weight to 50 parts by weight of a polysiloxane block copolymer; Component C: 5 parts by weight to 60 parts by weight of glass fiber, Component D: 0.1 parts by weight to 30 parts by weight of a phosphorus-containing compound; Component E: 0.01 to 30 parts by weight of a polyolefin compound; Includes.

[0009] Preferably, the glass fiber reinforced polycarbonate composite material comprises: Component A: 40 parts by weight to 90 parts by weight of polycarbonate, Component B: 3.5 parts by weight to 45 parts by weight of a polysiloxane block copolymer; Component C: 5 parts by weight to 60 parts by weight of glass fiber, Component D: 8 parts by weight to 12 parts by weight of a phosphorus-containing compound; Component E: 6 parts by weight to 10 parts by weight of a polyolefin compound; Includes.

[0010] In the glass fiber reinforced polycarbonate composite material, the percentage of the siloxane content based on the total weight of the composition is 0.6 wt % to 17 wt %, preferably 2.8 wt % to 12 wt %.

[0011] In the glass fiber reinforced polycarbonate composite material, the weight ratio of phosphorus element to silicon element is (1:0.1 to 3.2), and preferably (1:0.6 to 2.5).

[0012] The polycarbonate is one or more selected from aromatic polycarbonates, aliphatic polycarbonates, aromatic-aliphatic polycarbonates, and branched polycarbonates, and is preferably an aromatic polycarbonate; Preferably, the aromatic polycarbonate has a viscosity average molecular weight of 13,000 to 40,000, and more preferably, a viscosity average molecular weight of 18,000 to 28,000. If the viscosity average molecular weight is within the above range, the mechanical strength is good and excellent moldability can be maintained. The viscosity average molecular weight is calculated from the solution viscosity at a test temperature of 25°C using methylene chloride as a solvent.

[0013] The polycarbonate can be produced by interfacial polymerization and transesterification, and the content of terminal hydroxyl groups in the process can be controlled.

[0014] The polysiloxane block copolymer comprises a polydimethylsiloxane block and a polycarbonate block of bisphenol A, and the siloxane content is 0.6 wt% to 36 wt% based on the weight of component B. After adding the siloxane block copolymer, the siloxane content of the glass fiber reinforced polycarbonate composite material can be tested by near infrared analysis, and the test method is to weigh a certain weight of the glass fiber reinforced polycarbonate composite material pellets, uniformly dissolve them in methane, and then detect them in a sheet form.

[0015] The phosphorus-containing compound is selected from oxygen-containing phosphoric acid, phosphates and derivatives thereof, the oxygen-containing phosphoric acid is selected from phosphoric acid and / or hypophosphorous acid, and the phosphates and derivatives thereof are selected from sodium phosphate and / or zinc hypophosphite.

[0016] The polyolefin compound is one or more selected from saturated linear polyolefins, polyolefins containing unsaturated bonds, polyolefins containing partial branched chains, and modified polyolefins, the saturated linear polyolefins are one or more selected from polyethylene, polypropylene, and polybutene, the polyolefins containing unsaturated bonds are selected from polybutadiene and derivatives thereof, the polyolefins containing partial branched chains are selected from polyX-olefins, and the modified polyolefins are one or more selected from epoxy modified polyolefins and maleic anhydride modified polyolefins.

[0017] The glass fiber reinforced polycarbonate composite material of the present invention may further contain Component F: other auxiliary agents in an amount of 0 to 10 parts by weight based on the weight of the glass fiber reinforced polycarbonate composite material, and the other auxiliary agents are one or more selected from stabilizers, flame retardants, drip-proofing agents, lubricants, release agents, plasticizers, fillers, antistatic agents, antibacterial agents, and colorants.

[0018] Suitable stabilizers may include one or more combinations of organic phosphites, such as triphenyl phosphite, tris-(2,6-dimethylphenyl) phosphite, trinonylphenyl phosphite, dimethyl phenylphosphonate, trimethyl phosphate, and the like, organic phosphites, alkylated monohydric or polyhydric phenols, alkylation reaction products of polyhydric phenols and dienes, butylation reaction products of p-cresol or dicyclopentadiene, alkylated hydroquinones, hydroxylated thiodiphenyl ethers, alkylene-bisphenols, benzyl compounds, polyol esters, benzotriazoles, and benzophenones.

[0019] Suitable flame retardants may include phosphate ester flame retardants or sulfonate flame retardants. Suitable phosphate ester flame retardants may include bisphenol A diphosphate tetraphenyl, triphenyl, tritolyl, tolyl diphenyl, bisphenol A diphosphate tetratoly, resorcinol tetrakis(2,6-dimethylphenyl) and tetramethylbenzyl piperidine amide, and the flame retardant may be a sulfonate such as Rimar salt potassium perfluorobutyl sulfonate, KSS potassium diphenyl sulfone sulfonate, sodium benzene sulfonate, etc.

[0020] The method for producing the glass fiber reinforced polycarbonate composite material includes the steps of: Step 1) of weighing polycarbonate, polysiloxane block copolymer, phosphorus-containing compound, polyolefin compound, and other auxiliary agents in a mixing ratio and blending them in a high-speed mixer for 1 to 3 minutes to obtain a premix; The obtained premix is ​​fed into the main feed port of a twin-screw extruder, glass fibers are added to the side feed port, and the mixture is melt-extruded, granulated, and dried to complete step 2. Includes.

[0021] The aspect ratio of the twin-screw extruder is 46:1 to 50:1, and the temperatures of the twin-screw extruder are, in order from the supply section to the head section, 120°C to 160°C in zone 1, 200°C to 230°C in zone 2, 200°C to 230°C in zone 3, 200°C to 220°C in zone 4, 200°C to 220°C in zone 5, 200°C to 220°C in zone 6, 200°C to 220°C in zone 7, 200°C to 220°C in zone 8, 200°C to 220°C in zone 9, 200°C to 220°C in zone 10, and 200°C to 220°C in zone 11; the head temperature is 220°C to 240°C; and the rotation speed of the main body is 350 rpm to 500 rpm.

[0022] The glass fiber reinforced polycarbonate composite material obtained by the above-mentioned production method is used in the automobile, electronics / electrical, communication, and building industries. Effect of the Invention

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention adds specific amounts of polysiloxane block copolymer, phosphorus-containing compound and polyolefin compound to the formulation of glass fiber reinforced polycarbonate composite material, thereby ensuring a specific siloxane content and a specific weight ratio of phosphorus and silicon in the manufactured composite material. The manufactured composite material has excellent high elastic modulus and high toughness, as well as excellent fluidity and processability. Compared with conventional reinforcement and modification means, this composite material has both rigidity and toughness, and is particularly suitable for fields such as automobiles, electronics, electrical equipment, communication industries and construction industries. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The present invention will be further described below with reference to specific embodiments. The following embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the following embodiments.

[0026] Test standards or methods for each performance: Test method for Izod unnotched impact strength: according to ASTM D256-2010 standard. Tensile strength test method: According to ASTM D638-2014 standard, tensile speed is 10mm / min. Flexural modulus test method: According to ASTM D790-2010 standard, bending speed is 2mm / min. Fluidity test method: According to ASTM D1238-2013 standard, melting temperature is 300℃. Polycarbonates used in the present invention: Component A-1: ​​Aromatic polycarbonate with a viscosity average molecular weight of 18,000, manufactured by Idemitsu Co., Ltd. of Japan; Component A-2: Aromatic polycarbonate with a viscosity average molecular weight of 27,000, manufactured by Idemitsu Co., Ltd. of Japan; Polysiloxane block copolymers used in the present invention: Component B-1: Polysiloxane block copolymer with siloxane content of 8 wt%, manufactured by Idemitsu Co., Ltd. of Japan Component B-2: Polysiloxane block copolymer with siloxane content of 34 wt%, manufactured by Idemitsu Co., Ltd. of Japan Glass fibers used in the present invention: Ingredient C-1: Toyobo Co., Ltd., Japan Phosphorus-containing compounds for use in the present invention: Ingredient D-1: Hypophosphorous acid, manufactured by Aladdin Ingredient D-2: Sodium phosphate, manufactured by Hakutoku Chemical Co., Ltd. Polyolefin compounds used in the present invention: Component E-1: Polyethylene, manufactured by Sinopec Component E-2: PolyX-olefin, manufactured by Shinshin Kako Co., Ltd. Other auxiliaries used in the present invention: Ingredient F-1: Stabilizer: 2112, manufactured by Adeka Corporation Component F-2: Lubricant: PETS, manufactured by Lonza

[0027] Examples 1 to 8 and Comparative Examples 1 to 6: Production of glass fiber reinforced polycarbonate composite materials Polycarbonate, polysiloxane block copolymer, phosphorus-containing compound, polyolefin compound, and other auxiliary agents were weighed in the compounding ratio, and blended by stirring for 1 to 3 minutes in a high-speed mixer to obtain a premix. The obtained premix was placed in the main feed port of a twin-screw extruder, glass fiber was added to the side feed port, melt extruded, granulated, and dried to obtain a glass fiber reinforced polycarbonate composite material. The above glass fiber reinforced polycarbonate composite material was tested for Izod notched impact strength, Izod unnotched impact strength, tensile strength, flexural modulus, and fluidity, and the obtained data are shown in Table 1.

[0028] Table 1: Specific compositions (parts by weight) of Examples 1 to 8 and Comparative Examples 1 to 6 and their test results TIFF0007562643000001.tif177136 Continued in Table 1 TIFF0007562643000002.tif177137 Preferred aspects of the invention include the following. [1] A glass fiber reinforced polycarbonate composite material, Component A: 40 parts by weight to 90 parts by weight of polycarbonate, Component B: 1.5 parts by weight to 50 parts by weight of a polysiloxane block copolymer; Component C: 5 parts by weight to 60 parts by weight of glass fiber, Component D: 0.1 parts by weight to 30 parts by weight of a phosphorus-containing compound; Component E: 0.01 to 30 parts by weight of a polyolefin compound Composite materials. [2] Component A: 40 parts by weight to 90 parts by weight of polycarbonate, Component B: 3.5 parts by weight to 45 parts by weight of a polysiloxane block copolymer; Component C: 5 parts by weight to 60 parts by weight of glass fiber, Component D: 8 parts by weight to 12 parts by weight of a phosphorus-containing compound; Component E: 6 parts by weight to 10 parts by weight of a polyolefin compound The glass fiber reinforced polycarbonate composite material according to [1], [3] The glass fiber reinforced polycarbonate composite material according to [1] or [2], characterized in that the percentage of the siloxane content in the total weight of the composition in the glass fiber reinforced polycarbonate composite material is 0.6 wt% to 17 wt%, preferably 2.8 wt% to 12 wt%. [4] The glass fiber reinforced polycarbonate composite material according to [1] or [2], characterized in that the weight ratio of phosphorus element to silicon element in the glass fiber reinforced polycarbonate composite material is 1:0.1-3.2, preferably 1:0.6-2.5. [5] The glass fiber-reinforced polycarbonate composite material according to [1] or [2], characterized in that the polycarbonate is one or more selected from aromatic polycarbonates, aliphatic polycarbonates, aromatic-aliphatic polycarbonates, and branched polycarbonates, preferably aromatic polycarbonates, and the aromatic polycarbonate is an aromatic polycarbonate having a viscosity average molecular weight of 13,000 to 40,000, preferably an aromatic polycarbonate having a viscosity average molecular weight of 18,000 to 28,000. [6] The glass fiber-reinforced polycarbonate composite material according to [1] or [2], characterized in that the polysiloxane block copolymer contains a polydimethylsiloxane block and a bisphenol A polycarbonate block, and has a siloxane content of 0.6 wt% to 36 wt% based on the weight of component B. [7] The glass fiber reinforced polycarbonate composite material according to [1] or [2], characterized in that the phosphorus-containing compound is selected from oxygen-containing phosphoric acid, phosphates and derivatives thereof, the oxygen-containing phosphoric acid is selected from phosphoric acid and / or hypophosphorous acid, and the phosphates and derivatives thereof are selected from sodium phosphate and / or zinc hypophosphite. [8] The glass fiber-reinforced polycarbonate composite material according to [1] or [2], characterized in that the polyolefin compound is one or more selected from saturated linear polyolefins, polyolefins containing unsaturated bonds, polyolefins containing partial branched chains, and modified polyolefins, the saturated linear polyolefins are one or more selected from polyethylene, polypropylene, and polybutene, the polyolefins containing unsaturated bonds are selected from polybutadiene and its derivatives, the polyolefins containing partial branched chains are selected from polyX-olefins, and the modified polyolefins are one or more selected from epoxy-modified polyolefins and maleic anhydride-modified polyolefins. [9] The glass fiber reinforced polycarbonate composite material according to [1] or [2], further comprising 0 to 10 parts by weight of component F: other auxiliary agents relative to the weight of the glass fiber reinforced polycarbonate composite material, the other auxiliary agents being one or more selected from stabilizers, flame retardants, drip-proofing agents, lubricants, release agents, plasticizers, fillers, antistatic agents, antibacterial agents, and colorants.

[10] Step 1) of weighing out polycarbonate, polysiloxane block copolymer, phosphorus-containing compound, polyolefin compound, and other auxiliary agents in a mixing ratio, and blending them by stirring for 1 to 3 minutes in a high-speed mixer to obtain a premix; The obtained premix is ​​fed into the main feed port of a twin-screw extruder, glass fibers are added to the side feed port, and the mixture is melt-extruded, granulated, and dried to complete step 2. The method for producing a glass fiber-reinforced polycarbonate composite material according to any one of [1] to [9], comprising:

[11] The aspect ratio of the twin-screw extruder is 46:1 to 50:1, and the temperatures of the twin-screw extruder are, in order from the supply section to the head section, 120°C to 160°C in zone 1, 200°C to 230°C in zone 2, 200°C to 230°C in zone 3, 200°C to 220°C in zone 4, 200°C to 220°C in zone 5, 200°C to 220°C in zone 6, and 200°C to 220°C in zone 7. the temperature of zone 8 is 200°C to 220°C, the temperature of zone 9 is 200°C to 220°C, the temperature of zone 10 is 200°C to 220°C, the temperature of zone 11 is 200°C to 220°C, the temperature of the head is 220°C to 240°C, and the rotation speed of the main body is 350 rpm to 500 rpm.

[12] Use of a glass fiber reinforced polycarbonate composite material obtained by the production method according to

[10] in the automobile, electronics / electrical, and communications industries, and the construction industry.

Claims

1. 1. A glass fiber reinforced polycarbonate composite material, comprising: Component A: 40 to 90 parts by weight of polycarbonate; Component B: 1.5 parts by weight to 50 parts by weight of a polysiloxane block copolymer; Component C: 5 to 60 parts by weight of glass fiber; Component D: 0.1 to 30 parts by weight of a phosphorus-containing compound; Component E: 0.01 to 30 parts by weight of a polyolefin compound where the polysiloxane block copolymer comprises a polydimethylsiloxane block and a polycarbonate block of bisphenol A, the siloxane content being 0.6 wt % to 36 wt % based on the weight of component B; In the glass fiber reinforced polycarbonate composite material, the percentage of the siloxane content based on the total weight of the composition is 0.6 wt % to 17 wt %; In the glass fiber reinforced polycarbonate composite material, the weight ratio of phosphorus element to silicon element is 1:0.1-3.2; Composite material.

2. Component A: 40 to 65 parts by weight of polycarbonate; Component B: 3.5 parts by weight to 45 parts by weight of a polysiloxane block copolymer; Component C: 5 to 60 parts by weight of glass fiber; Component D: 8 parts by weight to 12 parts by weight of a phosphorus-containing compound; Component E: 6 to 10 parts by weight of a polyolefin compound 2. The glass fiber reinforced polycarbonate composite of claim 1, comprising:

3. 3. The glass fiber reinforced polycarbonate composite material according to claim 1, wherein the percentage of the siloxane content in the glass fiber reinforced polycarbonate composite material is 2.8 wt % to 12 wt % of the total weight of the composition.

4. 3. The glass fiber reinforced polycarbonate composite material according to claim 1, wherein the weight ratio of phosphorus element to silicon element in the glass fiber reinforced polycarbonate composite material is 1:0.6-2.

5.

5. The glass fiber reinforced polycarbonate composite material according to claim 1 or 2, characterized in that the polycarbonate is one or more selected from the group consisting of aromatic polycarbonates, aliphatic polycarbonates, aromatic-aliphatic polycarbonates, and branched polycarbonates, and the aromatic polycarbonate is an aromatic polycarbonate having a viscosity average molecular weight of 13,000 to 40,000.

6. The glass fiber reinforced polycarbonate composite material according to claim 1 or 2, characterized in that the polysiloxane block copolymer comprises a polydimethylsiloxane block and a polycarbonate block of bisphenol A, and the siloxane content is 8 wt% to 34 wt% based on the weight of component B.

7. 3. The glass fiber reinforced polycarbonate composite material according to claim 1, characterized in that the phosphorus-containing compound is selected from oxygen-containing phosphoric acid, phosphates and derivatives thereof, the oxygen-containing phosphoric acid is selected from phosphoric acid and / or hypophosphorous acid, and the phosphates and derivatives thereof are selected from sodium phosphate and / or zinc hypophosphite.

8. 3. The glass fiber reinforced polycarbonate composite material according to claim 1, wherein the polyolefin compound is one or more selected from the group consisting of saturated linear polyolefins, polyolefins containing unsaturated bonds, polyolefins containing partially branched chains, and modified polyolefins, the saturated linear polyolefins are one or more selected from the group consisting of polyethylene, polypropylene, and polybutene, the polyolefins containing unsaturated bonds are selected from polybutadiene and derivatives thereof, and the modified polyolefins are one or more selected from the group consisting of epoxy modified polyolefins and maleic anhydride modified polyolefins.

9. 3. The glass fiber reinforced polycarbonate composite material according to claim 1 or 2, further comprising 0 to 10 parts by weight of component F: other auxiliary agents, based on the weight of the glass fiber reinforced polycarbonate composite material, the other auxiliary agents being one or more selected from the group consisting of stabilizers, flame retardants, drip-proofing agents, lubricants, release agents, plasticizers, fillers, antistatic agents, antibacterial agents, and colorants.

10. Step 1) of weighing out polycarbonate, polysiloxane block copolymer, phosphorus-containing compound, polyolefin compound, and other auxiliary agents in a mixing ratio, and blending them by stirring for 1 to 3 minutes in a high-speed mixer to obtain a premix; The obtained premix is ​​fed into the main feed port of a twin-screw extruder, glass fibers are added to the side feed port, and the mixture is melt-extruded, granulated, and dried to complete the step 2.

10. The method for producing the glass fiber reinforced polycarbonate composite material according to claim 1, comprising:

11. The aspect ratio of the twin-screw extruder is 46:1 to 50:1, and the temperatures of the twin-screw extruder are, in order from the feed section to the head section, 120°C to 160°C for zone 1, 200°C to 230°C for zone 2, 200°C to 230°C for zone 3, 200°C to 220°C for zone 4, 200°C to 220°C for zone 5, 200°C to 220°C for zone 6, 200°C to 220°C for zone 7, 200°C to 220°C for zone 8, 200°C to 220°C for zone 9, 200°C to 220°C for zone 10, 200°C to 220°C for zone 11, 200°C to 220°C for zone 12, 220°C to 240°C for zone 13, and 350 rpm to 500 rpm for the head. The method for producing a glass fiber reinforced polycarbonate composite material according to claim 10.

12. Use of the glass fiber reinforced polycarbonate composite material obtained by the method according to claim 10 in the automotive, electronics / electrical, communication and construction industries.

Citation Information

Patent Citations

  • Resin composition for decorative molding

    JP2014055231A

  • Polycarbonate resin composition and resin metal composite molding formed from the same

    JP2018095669A

  • Impact improved filled polycarbonate or polyester compositions

    US20150353732A1

  • Reinforced polycarbonate composition with improved impact performance

    US20180066133A1