Resin composition, modifier and composition containing the modifier

A resin composition with ethylene-vinyl acetate copolymers and ethylene-acrylic or ethylene-methacrylic acid copolymers addresses the recyclability issues of multilayer plastics by enhancing impact resistance and elongation, facilitating the recycling of mixed resin waste.

JP7563039B2Active Publication Date: 2024-10-08TOSOH CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020137634
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-17
Publication Date
2024-10-08
Estimated Expiration
2040-08-17

AI Technical Summary

Technical Problem

Multilayer films and containers made of different types of plastics are difficult to recycle due to poor compatibility, leading to deterioration of physical properties and limitations in recyclability, including brittleness, low impact resistance, and increased viscosity, which results in disposal in landfills or incineration.

Method used

A resin composition containing at least two types of ethylene-vinyl acetate copolymers with different vinyl acetate contents and an ethylene-acrylic or ethylene-methacrylic acid copolymer is used as a modifier to improve the impact resistance and elongation at break of brittle materials composed of multiple resin components.

Benefits of technology

The resin composition enhances the impact resistance and elongation at break of recycled plastics, enabling effective material recycling of mixed resin waste by improving compatibility and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563039000001
    Figure 0007563039000001
  • Figure 0007563039000002
    Figure 0007563039000002
  • Figure 0007563039000003
    Figure 0007563039000003
Patent Text Reader

Abstract

To provide a resin composition capable of improving impact resistance and fracture elongation, and using as a modifier by overcoming brittleness of a plastic material containing a plurality of resins such as laminates of dissimilar materials recovered for recycling.SOLUTION: A resin composition (A) contains the following components (1) and (2): (1) a composition (a1) containing at least two kinds of ethylene-vinyl acetate copolymers having different vinyl acetate contents; and (2) any copolymer (a2) of ethylene-acrylic acid copolymer or ethylene-(meth)acrylic acid copolymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the resin composition and to a molded article made from the composition. [Background technology]

[0002] In recent years, interest in the problem of environmental pollution caused by plastics has been growing, and material recycling of plastic products has been promoted. In material recycling of plastics, collected plastic waste is often melted and returned to raw material pellets, or recycled into consumable materials such as pallets. In this case, if different types of plastics are mixed in the collected plastic waste and recycled, there is a problem that the physical properties of the recycled plastic deteriorate due to poor compatibility with each other. For this reason, the currently used process is to separate the collected plastic waste by material and then recycle it into products.

[0003] However, in the case of multi-layer films and containers in which different types of plastics are layered, it is difficult to separate the materials, so they cannot be recycled and are currently landfilled or incinerated.

[0004] In this context, the addition of a compatibilizer has been considered as a means of recycling composite resins in a laminated state. For example, composite recycling of PE-PET and PP-ABS has been considered using an ionomer resin as a compatibilizer (Patent Document 1). In addition, composite recycling of PE-PET, etc. has been considered using an oxazoline-based compatibilizer (Patent Document 2). Furthermore, composite recycling of PE-EVOH has also been considered (Patent Document 3). According to these documents, it has been shown that the physical properties of composites of PE and PET or EVOH can be improved by adding a compatibilizer. However, the mechanical properties of the recycled resins obtained by these methods are insufficient, so it is necessary to develop a technology that can further improve the mechanical properties. In addition, there are problems such as increased viscosity, yellowing, and odor, which make it difficult to repeatedly recycle, and there are limitations on the uses of the recycled resin. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2001-220473 A [Patent Document 2] JP 2004-182957 A [Patent Document 3] Special Publication No. 2009-535452 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a resin composition that can be used as a modifier that can overcome the brittleness of plastic materials containing multiple resins, such as laminates of recycled heterogeneous materials, and improve the impact resistance and breaking elongation. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems and have found that a resin composition containing two types of ethylene-vinyl acetate copolymers differing in vinyl acetate content and either an ethylene-acrylic acid copolymer or an ethylene-methacrylic acid copolymer can be suitably used as a resin modifier capable of improving the impact resistance and breaking elongation of a brittle material composed of multiple resin components, thereby completing the present invention.

[0008] That is, the present invention relates to a resin composition (A) containing the following components (1) and (2): (1) Composition (a1) containing at least two ethylene-vinyl acetate copolymers having different vinyl acetate contents (2) Resin (a2) of either ethylene-acrylic acid copolymer or ethylene-methacrylic acid copolymer Effect of the Invention

[0009] According to the present invention, a resin composition having excellent effects of modifying impact resistance and elongation at break and useful as a modifier for resin molded products requiring these physical properties can be provided. In particular, by using the resin composition, it is possible to effectively carry out material recycling of plastic waste containing multiple resins. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The resin composition (A) which is one embodiment of the present invention will be described in detail below.

[0011] The resin composition (A) of the present invention includes a composition (a1) containing at least two kinds of ethylene-vinyl acetate copolymers having different vinyl acetate contents (hereinafter referred to as "EVA composition (a1)").

[0012] The vinyl acetate content of each ethylene-vinyl acetate copolymer in the EVA composition (a1) is preferably 5% by weight or more and 85% by weight or less. The vinyl acetate content can be measured by the method of JIS K6924-1.

[0013] Examples of methods for producing ethylene-vinyl acetate copolymers include known production methods such as high-pressure radical polymerization, solution polymerization, and emulsion polymerization. Such resins can be conveniently selected from commercially available products. Ethylene-vinyl acetate copolymers are commercially available from Tosoh Corporation under the product name Ultrathene, and from Lanxess KK under the product names Levaprene and Levamelt.

[0014] In the EVA composition (a1), the difference in vinyl acetate content is preferably 1% by weight or more, more preferably 5% by weight or more, which improves compatibility when the resin composition (A) is blended as a modifier with the thermoplastic resin (B), and improves the impact resistance and breaking elongation of the resulting composition.

[0015] In the EVA composition (a1), when the difference in vinyl acetate content of each copolymer is taken, it is preferable that the difference in vinyl acetate content of at least one set of copolymers is 40% by weight or less. This improves the compatibility between the ethylene-vinyl acetate copolymers constituting the resin composition (A), and when the ethylene-vinyl acetate copolymers are blended as a modifier with a thermoplastic resin, the impact resistance and breaking elongation of the resin are improved. The difference in vinyl acetate content of at least one set of copolymers is preferably 30% by weight or less, more preferably 20% by weight or less, and most preferably 15% by weight or less.

[0016] Here, in the EVA composition (a1), the difference in vinyl acetate content of each copolymer can be calculated as follows, for example, in a composition containing three types of ethylene-vinyl acetate copolymers having vinyl acetate contents of 25 wt%, 50 wt%, and 80 wt% (hereinafter, the vinyl acetate contents will be denoted as VAc25, VAc50, and VAc80, respectively). VAc50 - VAc25 = 25% by weight VAc80 - VAc50 = 30% by weight VAc80 - VAc25 = 55% by weight

[0017] The EVA composition (a1) preferably contains at least three kinds of ethylene-vinyl acetate copolymers having different vinyl acetate contents.

[0018] In order to satisfy these requirements, the EVA composition (a1) can be adjusted by blending two or more, preferably three or more, types of ethylene-vinyl acetate copolymers. If an ethylene-vinyl acetate copolymer with a vinyl acetate content of 25% by weight is represented as VAc25 and the composition of the components is represented by (+), examples include (VAc15+VAc25), (VAc25+VAc40), (VAc25+VAc50), (VAc50+VAc80), (VAc15+VAc25+VAc50), (VAc25+VAc50+VAc80), (VAc15+VAc25+VAc50+VAc70), (VAc15+VAc25+VAc50+VAc80), (VAc15+VAc25+VAc50+VAc70+VAc80), and the like.

[0019] The resin composition (A) of the present invention contains a copolymer (a2) (hereinafter referred to as "copolymer (a2)") which is either an ethylene-acrylic acid copolymer or an ethylene-methacrylic acid copolymer.

[0020] The acrylic acid content or methacrylic acid content of the copolymer (a2) is preferably from 3 mol % to 15 mol %.

[0021] The copolymer (a2) may contain one type or two or more types.

[0022] In the resin composition (A) of the present invention, it is preferable that the absolute value of the difference in solubility parameter (hereinafter, SP value) calculated by the Fedors method (Polym. Eng. Sci., 14, 147 (1974)) between at least one ethylene-vinyl acetate copolymer having a vinyl acetate content constituting the EVA composition (a1) and the copolymer (a2) is 0.3 MPa or less. This improves the compatibility of the ethylene-vinyl acetate copolymer composition (a1) and the copolymer (a2) in the resin composition (A), and improves the impact resistance and breaking elongation of the resulting composition.

[0023] Here, when the SP value of each component is calculated by the Fedors method, for example, the SP values ​​of four types of ethylene-vinyl acetate copolymers having vinyl acetate contents of 15 wt%, 25 wt%, 50 wt%, and 80 wt%, an ethylene-acrylic acid copolymer having an acrylic acid content of 20 wt%, and an ethylene-methacrylic acid copolymer having a methacrylic acid content of 11 wt%, can be calculated as follows. Ethylene-vinyl acetate copolymer with vinyl acetate content of 15% by weight = 18.0 MPa Ethylene-vinyl acetate copolymer with vinyl acetate content of 25% by weight = 18.3 MPa Ethylene-vinyl acetate copolymer with 50% vinyl acetate content by weight = 19.3 MPa Ethylene-vinyl acetate copolymer with 80% vinyl acetate content by weight = 20.6 MPa Ethylene-methacrylic acid copolymer with 4 mol% methacrylic acid content = 18.2 MPa Ethylene-acrylic acid copolymer with 9 mol% acrylic acid content = 19.2 MPa

[0024] For example, when the resin composition (A) contains an ethylene-methacrylic acid copolymer having a methacrylic acid content of 4 mol% (SP value = 18.2 MPa), an ethylene-vinyl acetate copolymer having a vinyl acetate content of 25 wt% (18.3 MPa) and an ethylene-acrylic acid copolymer having an acrylic acid content of 9 mol% (19.2 MPa), by using an ethylene-vinyl acetate copolymer having a vinyl acetate content of 50 wt% (19.3 MPa), the absolute value of the difference in SP value from the copolymer (a2) can be 0.3 MPa or less.

[0025] In the resin composition (A) of the present invention, the mixing ratio of the EVA composition (a1) and the copolymer (a2) is preferably 50% by weight or more and 99% by weight or less of the EVA composition (a1) and 1% by weight or more and 50% by weight or less of the copolymer (a2) (where the total of (a1) and (a2) is 100% by weight), and more preferably 70% by weight or more and 90% by weight or less of the EVA composition (a1) and 10% by weight or more and 30% by weight or less of the copolymer (a2) (where the total of (a1) and (a2) is 100% by weight). By including 50% by weight or more and 99% by weight or less of the EVA composition (a1), the compatibility and impact resistance of the blended resin are further improved. On the other hand, by including 1% by weight or more and 50% by weight or less of the copolymer (a2), the compatibility of the blended resin is further improved.

[0026] The modifier according to one embodiment of the present invention will be described in detail below.

[0027] The present invention is a modifier containing a resin composition (A) (hereinafter referred to as "the modifier of the present invention").

[0028] The resin composition (A) of the present invention can be blended as a modifier into a base resin to enhance the impact resistance of the resin. In addition, when the base resin is composed of multiple resin components, the compatibility between the components can be enhanced.

[0029] The modifier of the present invention can be used in any form, such as pellets or powder.

[0030] The base material (hereinafter referred to as "thermoplastic resin (B)") to be mixed with the modifier of the present invention is preferably at least one selected from the group consisting of polyolefin resins, acrylic acid resins, polyamide resins, polyester resins, polycarbonate resins, polystyrene resins, and styrene-acrylonitrile copolymers, and more preferably a composition containing at least two of them, because they have excellent compatibility with the modifier. Here, the components of the thermoplastic resin (B) exclude the EVA composition (a1) and the copolymer (a2).

[0031] Examples of polyolefin resins include high density polyethylene, low density polyethylene, linear low density polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl alcohol copolymer, ethylene-acrylic acid ester copolymer, ethylene-methacrylic acid ester copolymer, polybutadiene, and polyisoprene.

[0032] Examples of the acrylic acid resin include polyacrylic acid, polymethyl acrylate, polyethyl acrylate, polybutyl acrylate, polyoctyl acrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, and polyoctyl methacrylate.

[0033] Examples of polyamide resins include nylon 6, nylon 6,6, nylon 11, and nylon 12.

[0034] Examples of polyester resins include polyethylene terephthalate, glycol-modified polyethylene terephthalate resin (PETG resin), polybutylene terephthalate, polylactic acid (including poly-L-lactic acid, poly-D-lactic acid, copolymers of L-lactic acid and D-lactic acid, and stereocomplexes of poly-L-lactic acid and poly-D-lactic acid), polybutylene succinate, poly(butylene succinate / adipate), polyethylene succinate, poly(butylene succinate / terephthalate), poly(butylene adipate / terephthalate), poly(hydroxybutyrate / hydroxyhexanoate), polyglycolic acid, poly 3-hydroxybutyrate, and polycaprolactone.

[0035] Among these, the thermoplastic resin constituting the thermoplastic resin (B) is preferably at least one selected from the group consisting of high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl alcohol copolymer, nylon 6, nylon 6,6, nylon 11, nylon 12, polyethylene terephthalate, glycol-modified polyethylene terephthalate resin (PETG resin), polybutylene terephthalate, polylactic acid (including poly-L-lactic acid, poly-D-lactic acid, copolymer of L-lactic acid and D-lactic acid, and stereocomplex of poly-L-lactic acid and poly-D-lactic acid), and polybutylene succinate, because it exhibits great improvement in impact resistance and elongation at break when blended with the resin composition (A).

[0036] More preferably, it is at least one member selected from the group consisting of high-density polyethylene, low-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl alcohol copolymer, nylon 6, nylon 6,6, nylon 11, nylon 12, polyethylene terephthalate, glycol-modified polyethylene terephthalate resin (PETG resin), and polybutylene terephthalate.

[0037] The thermoplastic resin (B) may be an unused virgin resin or a resin obtained by recovering a used molded body. That is, the form in which all of the one or more types of resins are unused resins, the form in which at least one of the one or more types of resins is a used resin, and the form in which all of the one or more types of resins are used resins are also included.

[0038] When the thermoplastic resin (B) is a resin obtained by recovering used molded bodies, it may contain multiple types of resins. In this case, it may contain organic impurities such as PVC resin, wax, adhesives, plasticizers, and antioxidants. On the other hand, it may also contain inorganic impurities such as fillers.

[0039] The mixing ratio of the resin composition (A) and the thermoplastic resin (B) is preferably 50% by weight or more and 99% by weight or less of the thermoplastic resin (B) and 1% by weight or more and 50% by weight or less of the resin composition (A). The resin composition obtained by containing 99% by weight or less of the thermoplastic resin (B) has excellent impact resistance. On the other hand, the resin composition obtained by containing 50% by weight or more of the thermoplastic resin (B) has excellent rigidity. More preferably, the resin composition contains 60% by weight or more and 95% by weight or less of the thermoplastic resin (B) and 5% by weight or more and 40% by weight of the resin composition (A), and even more preferably, the resin composition contains 70% by weight or more and 95% by weight or less of the thermoplastic resin (B) and 5% by weight or more and 30% by weight of the resin composition (A).

[0040] When the modifier of the present invention is blended with the thermoplastic resin (B), the composition can be produced by a production method having a kneading step of kneading the modifier with the thermoplastic resin (B).

[0041] The kneading method includes a method in which the modifier and various materials constituting the thermoplastic resin (B) are kneaded simultaneously in a kneading device, and a method in which only the modifier is kneaded in advance, and then the kneaded modifier is blended with the thermoplastic resin (B) and further kneaded. The latter method is preferable because the modifier is mixed more uniformly and the desired physical properties can be stably obtained.

[0042] The kneading device is not particularly limited as long as it can uniformly disperse each component, and can be produced by a commonly used resin kneading device. For example, kneading devices such as a single screw extruder, a twin screw extruder, a multi-screw extruder, a Banbury mixer, a pressure kneader, a rotating roll, and an internal mixer can be mentioned. Among these, a twin screw extruder is more preferable because of its excellent dispersibility and continuous productivity.

[0043] When kneading with a twin-screw extruder, the screw rotation speed is not particularly limited, but kneading is preferably performed at 50 rpm to 3000 rpm, more preferably 300 rpm to 3000 rpm. A screw rotation speed of 50 rpm or more is preferable because the dispersibility of each mixed component is improved and the physical properties of the resulting resin are excellent, while a screw rotation speed of 3000 rpm or less is preferable because the deterioration of the resin due to excessive shear heat does not occur and the physical properties of the resulting resin are excellent.

[0044] When an extruder is used in the kneading step, the resin composition kneaded in the extruder, preferably the resin composition kneaded under the high-speed shear condition of 50 rpm to 3000 rpm, can be used as a raw material. In addition, a molded body obtained by extrusion molding in the extruder as it is can be used as a molded product.

[0045] The kneading temperature is preferably from the melting point of the component with the lowest melting point among the thermoplastic resins (B) or from the glass transition temperature to about 300° C. in the case of an amorphous resin.

[0046] The resin composition (A) and the composition containing the thermoplastic resin (B) according to one embodiment of the present invention will be described in detail below.

[0047] The composition of the present invention contains a resin composition (A) and a thermoplastic resin (B). That is, it is synonymous with a composition obtained by blending the modifier of the present invention with a thermoplastic resin (B).

[0048] The composition of the present invention may contain antistatic agents, light stabilizers, ultraviolet absorbers, nucleating agents, lubricants, antioxidants, antiblocking agents, flow improvers, release agents, flame retardants, colorants, inorganic neutralizing agents, hydrochloric acid absorbers, filler conductive agents, chain extenders, hydrolysis inhibitors, and the like, as long as the effects of the present invention are not impaired.

[0049] When the composition of the present invention contains components other than the resin composition (A) and the thermoplastic resin (B), the content can be expressed as the amount added relative to 100 parts by weight of the total of (A) and (B). In other words, the expression "~% by weight" of (A) and (B) above refers to the ratio of (A) and (B), and the ratio of other components can be defined separately.

[0050] The composition of the present invention may be used in any form, such as pellets or powder.

[0051] The composition of the present invention may be molded by any method, including, for example, profile extrusion, film, sheet, blow molding, injection molding, foaming, extrusion coating, and rotational molding.

[0052] Molded articles made from the composition of the present invention can be used for a variety of purposes, such as automobile parts, housings for electric and electronic parts, building materials, civil engineering materials, agricultural materials, containers, packaging materials, adhesives, and daily necessities. EXAMPLES

[0053] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0054] (1) Melt mass flow rate (MFR) The MFR of the ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, and thermoplastic resin (B) was measured using a melt indexer (manufactured by Takara Kogyo Co., Ltd.) at 190° C. and a load of 2.16 kg. (2) Vinyl acetate content The vinyl acetate content was measured in accordance with JIS K6924-1. (3) SP value The SP values ​​of ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, and ethylene-methacrylic acid copolymer were calculated by the Fedors method. (4) Impact strength The impact strength was measured in accordance with JIS P 8134. A press-molded sheet having a thickness of 0.1 mm was measured using a film impact tester (FT-M type, manufactured by Toyo Seiki Seisakusho Co., Ltd.) under the conditions of a test capacity of 3 J and a hemispherical hammer for piercing. (5) Tensile test The press-molded sheet with a thickness of 0.1 mm was punched out into an ASTM D-1822-L dumbbell-shaped test piece. The size of the test piece was 63.5 mm in total length, 9.53 mm in parallel length, 3.18 mm in parallel width, 0.1 mm in thickness, and 9.53 mm in grip width. The test piece was measured using a Tensilon tensile tester (Orientec, RTE-1210) under conditions of a chuck distance of 30 mm and a tensile speed of 200 mm / min. The point at which the sample broke was taken as the breaking elongation (breaking elongation [%] = tensile length required to break [mm] / chuck distance 30 mm), and the stress at the time of break was taken as the breaking stress.

[0055] Example 1 As the resin composition (A), a resin composition having the following composition was used. [Resin composition (A)] 65% by weight of ethylene-vinyl acetate copolymer (a1-25) (Ultrathene 640, manufactured by Tosoh Corporation) with a vinyl acetate content of 25% by weight and a melt mass flow rate of 3 g / 10 min 10% by weight of ethylene-vinyl acetate copolymer (a1-50) (manufactured by LANXESS AG, product name: Levaprene 500) with a vinyl acetate content of 50% by weight and a melt mass flow rate of 3 g / 10 min 25% by weight of ethylene-acrylic acid copolymer (a2-9) (SK Sogo Chemicals, product name SK Primacor 5980I) with an acrylic acid content of 9 mol% and a melt mass flow rate of 300 g / 10 min The above resin compositions were dry blended and melt-kneaded using a twin-screw extruder (manufactured by Technovel, product name ULTnano25TW) with a screw diameter of 25 mm at a resin temperature of 160° C. and a screw rotation speed of 150 rpm to obtain pellets of resin composition (A).

[0056] As the thermoplastic resin (B), a thermoplastic resin composition having the following composition was used. [Thermoplastic resin (B) composition] 70% by weight of low-density polyethylene (B-1) (manufactured by Tosoh Corporation, product name Petrothene 205) with a melt mass flow rate of 3 g / 10 min and a melting point of 111°C 30% by weight of ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by Kuraray Co., Ltd., product name EVAL C109B) 80% by weight of the thermoplastic resin (B) composition and 20% by weight of the resin composition (A) were dry blended, and melt-kneaded using a twin-screw extruder (manufactured by Technovel, product name ULTnano25TW) with a screw diameter of 25 mm under conditions of a resin temperature of 200°C and a screw rotation speed of 300 rpm to obtain a composition. The obtained composition was press molded using a press molding machine (AWFA-50 model manufactured by Shinto Metal Industry Co., Ltd.) under conditions of a pressure of 10 MPa, a heating temperature of 200°C (primary pressurization x 3 minutes, secondary pressurization x 3 minutes), and a cooling temperature of 25°C (4 minutes) to obtain a pressed sheet with a thickness of 0.1 mm. The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 1.

[0057] Example 2 As the thermoplastic resin (B), a thermoplastic resin composition having the following composition was used. [Thermoplastic resin (B) composition] 70% by weight of low-density polyethylene (B-1) (manufactured by Tosoh Corporation, product name Petrothene 205) with a melt mass flow rate of 3 g / 10 min and a melting point of 111°C 30% by weight of nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd., product name UBE Nylon 1022D) 80% by weight of the thermoplastic resin (B) composition and 20% by weight of the resin composition (A) described in Example 1 were dry blended, and melt-kneaded using a twin-screw extruder (manufactured by Technovel, product name ULTnano25TW) with a screw diameter of 25 mm under conditions of a resin temperature of 230°C and a screw rotation speed of 300 rpm to obtain a composition. The obtained composition was press molded using a press molding machine (AWFA-50 model manufactured by Shinto Metal Industry Co., Ltd.) under conditions of a pressure of 10 MPa, a heating temperature of 230°C (primary pressurization x 3 minutes, secondary pressurization x 3 minutes), and a cooling temperature of 25°C (4 minutes) to obtain a pressed sheet with a thickness of 0.1 mm. The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 1.

[0058] Example 3 As the thermoplastic resin (B), a thermoplastic resin composition having the following composition was used. [Thermoplastic resin (B) composition] 70% by weight of low-density polyethylene (B-1) (manufactured by Tosoh Corporation, product name Petrothene 205) with a melt mass flow rate of 3 g / 10 min and a melting point of 111°C 30% by weight of polyethylene terephthalate (B-6) (MA-2103, manufactured by Unitika Ltd.) with a melting point of 255°C The composition of thermoplastic resin (B) was dry blended and melt-kneaded using a twin-screw extruder (manufactured by Technovel, product name ULTnano25TW) with a screw diameter of 25 mm at a resin temperature of 270°C and a screw rotation speed of 150 rpm to obtain pellets of thermoplastic resin (B). 80% by weight of the obtained thermoplastic resin (B) and 20% by weight of the resin composition (A) described in Example 1 were dry blended, and melt-kneaded using a twin-screw extruder (manufactured by Technovel, product name ULTnano25TW) with a screw diameter of 25 mm under conditions of a resin temperature of 230°C and a screw rotation speed of 300 rpm to obtain a composition. The obtained composition was press molded using a press molding machine (AWFA-50 model manufactured by Shinto Metal Industry Co., Ltd.) under conditions of a pressure of 10 MPa, a heating temperature of 230°C (primary pressurization x 3 minutes, secondary pressurization x 3 minutes), and a cooling temperature of 25°C (4 minutes) to obtain a pressed sheet with a thickness of 0.1 mm. The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 1.

[0059] Example 4 A press sheet was obtained in the same manner as in Example 3, except that a thermoplastic resin composition having the following composition was used as the thermoplastic resin (B). [Thermoplastic resin (B) composition] 70% by weight of low-density polyethylene (B-1) (manufactured by Tosoh Corporation, product name Petrothene 205) with a melt mass flow rate of 3 g / 10 min and a melting point of 111°C 10% by weight of ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by Kuraray Co., Ltd., product name EVAL C109B) 10% by weight of nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd., product name UBE Nylon 1022D) 10% by weight of polyethylene terephthalate (B-6) (MA-2103, manufactured by Unitika Ltd.) with a melting point of 255°C The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 1.

[0060] Example 5 A press sheet was obtained in the same manner as in Example 1, except that a resin composition having the following composition was used as the resin composition (A). [Composition of resin composition (A)] 33% by weight of ethylene-vinyl acetate copolymer (a1-15) (Ultrathene 626, manufactured by Tosoh Corporation) with a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min 32% by weight of ethylene-vinyl acetate copolymer (a1-25) (Ultrathene 640, manufactured by Tosoh Corporation) with a vinyl acetate content of 25% by weight and a melt mass flow rate of 3 g / 10 min 10% by weight of ethylene-vinyl acetate copolymer (a1-50) (manufactured by LANXESS AG, product name: Levaprene 500) with a vinyl acetate content of 50% by weight and a melt mass flow rate of 3 g / 10 min 25% by weight of ethylene-acrylic acid copolymer (a2-9) (SK Sogo Chemicals, product name SK Primacor 5980I) with an acrylic acid content of 9 mol% and a melt mass flow rate of 300 g / 10 min The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 1.

[0061] Example 6 A press sheet was obtained in the same manner as in Example 2, except that the resin composition described in Example 5 was used as the resin composition (A). The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 1.

[0062] Example 7 A press sheet was obtained in the same manner as in Example 3, except that the resin composition described in Example 5 was used as the resin composition (A). The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 1.

[0063] Example 8 A press sheet was obtained in the same manner as in Example 4, except that the resin composition described in Example 5 was used as the resin composition (A). The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 1.

[0064] [Table 1]

[0065] Example 9 A press sheet was obtained in the same manner as in Example 8, except that the thermoplastic resin (B) was 90% by weight and the resin composition (A) was 10% by weight. The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 2.

[0066] Example 10 A press sheet was obtained in the same manner as in Example 8, except that the thermoplastic resin (B) was 95% by weight and the resin composition (A) was 5% by weight. The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 2.

[0067] Example 11 A press sheet was obtained in the same manner as in Example 4, except that a resin composition having the following composition was used as the resin composition (A). [Composition of resin composition (A)] 25% by weight of ethylene-vinyl acetate copolymer (a1-15) (Ultrathene 626, manufactured by Tosoh Corporation) with a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min 25% by weight of ethylene-vinyl acetate copolymer (a1-25) (Ultrathene 640, manufactured by Tosoh Corporation) with a vinyl acetate content of 25% by weight and a melt mass flow rate of 3 g / 10 min 10% by weight of ethylene-vinyl acetate copolymer (a1-50) (manufactured by LANXESS AG, product name: Levaprene 500) with a vinyl acetate content of 50% by weight and a melt mass flow rate of 3 g / 10 min 40% by weight of ethylene-acrylic acid copolymer (a2-9) (SK Sogo Chemicals, product name SK Primacor 5980I) with an acrylic acid content of 9 mol% and a melt mass flow rate of 300 g / 10 min The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 2.

[0068] Example 12 A press sheet was obtained in the same manner as in Example 4, except that a resin composition having the following composition was used as the resin composition (A). [Composition of resin composition (A)] 33% by weight of ethylene-vinyl acetate copolymer (a1-15) (Ultrathene 626, manufactured by Tosoh Corporation) with a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min 32% by weight of ethylene-vinyl acetate copolymer (a1-25) (Ultrathene 640, manufactured by Tosoh Corporation) with a vinyl acetate content of 25% by weight and a melt mass flow rate of 3 g / 10 min 10% by weight of ethylene-vinyl acetate copolymer (a1-50) (manufactured by LANXESS AG, product name: Levaprene 500) with a vinyl acetate content of 50% by weight and a melt mass flow rate of 3 g / 10 min 25% by weight of ethylene-methacrylic acid copolymer (a2-4) (manufactured by Mitsui Dow Chemical, product name Nucrel 1108C) with a methacrylic acid content of 4 mol% and a melt mass flow rate of 10 g / 10 min The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 2.

[0069] Example 13 A press sheet was obtained in the same manner as in Example 4, except that a resin composition having the following composition was used as the resin composition (A). [Composition of resin composition (A)] 23% by weight of ethylene-vinyl acetate copolymer (a1-15) (Ultrathene 626, manufactured by Tosoh Corporation) with a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min 22% by weight of ethylene-vinyl acetate copolymer (a1-25) (Ultrathene 640, manufactured by Tosoh Corporation) with a vinyl acetate content of 25% by weight and a melt mass flow rate of 3 g / 10 min 10% by weight of ethylene-vinyl acetate copolymer (a1-50) (manufactured by LANXESS AG, product name: Levaprene 500) with a vinyl acetate content of 50% by weight and a melt mass flow rate of 3 g / 10 min 20% by weight of ethylene-vinyl acetate copolymer (a1-80) (manufactured by LANXESS AG, product name Levaprene 800) with a vinyl acetate content of 80% by weight and a melt mass flow rate of 5 g / 10 min 25% by weight of ethylene-acrylic acid copolymer (a2-9) (SK Sogo Chemicals, product name SK Primacor 5980I) with an acrylic acid content of 9 mol% and a melt mass flow rate of 300 g / 10 min The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 2.

[0070] Example 14 A press sheet was obtained in the same manner as in Example 8, except that a thermoplastic resin composition having the following composition was used as the thermoplastic resin (B). [Thermoplastic resin (B) composition] 70% by weight of linear low-density polyethylene (B-2) (manufactured by Tosoh Corporation, product name Nipolon-L F15R) with a melt mass-flow rate of 0.8 g / 10 min and a melting point of 122°C 10% by weight of ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by Kuraray Co., Ltd., product name EVAL C109B) 10% by weight of nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd., product name UBE Nylon 1022D) 10% by weight of polyethylene terephthalate (B-6) (MA-2103, manufactured by Unitika Ltd.) with a melting point of 255°C The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 2.

[0071] Example 15 A press sheet was obtained in the same manner as in Example 8, except that a thermoplastic resin composition having the following composition was used as the thermoplastic resin (B). [Thermoplastic resin (B) composition] 70% by weight of high-density polyethylene (B-3) (manufactured by Tosoh Corporation, product name Nipolon Hard 4020) with a melt mass flow rate of 5.5 g / 10 min and a melting point of 133°C 10% by weight of ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by Kuraray Co., Ltd., product name EVAL C109B) 10% by weight of nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd., product name UBE Nylon 1022D) 10% by weight of polyethylene terephthalate (B-6) (MA-2103, manufactured by Unitika Ltd.) with a melting point of 255°C The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 2.

[0072] [Table 2]

[0073] Comparative Example 1 A press sheet was obtained in the same manner as in Example 1, except that the resin composition (A) was not blended and only the composition of the thermoplastic resin (B) described below was used. [Thermoplastic resin (B) composition] 70% by weight of low-density polyethylene (B-1) (manufactured by Tosoh Corporation, product name Petrothene 205) with a melt mass flow rate of 3 g / 10 min and a melting point of 111°C 30% by weight of ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by Kuraray Co., Ltd., product name EVAL C109B) The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 3.

[0074] Comparative Example 2 A press sheet was obtained in the same manner as in Example 2, except that the resin composition (A) was not blended and only the composition of the thermoplastic resin (B) described below was used. [Thermoplastic resin (B) composition] 70% by weight of low-density polyethylene (B-1) (manufactured by Tosoh Corporation, product name Petrothene 205) with a melt mass flow rate of 3 g / 10 min and a melting point of 111°C 30% by weight of nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd., product name UBE Nylon 1022D) The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 3.

[0075] Comparative Example 3 A press sheet was obtained in the same manner as in Example 3, except that the resin composition (A) was not blended and only the thermoplastic resin (B) composition described below was used. [Thermoplastic resin (B) composition] 70% by weight of low-density polyethylene (B-1) (manufactured by Tosoh Corporation, product name Petrothene 205) with a melt mass flow rate of 3 g / 10 min and a melting point of 111°C 30% by weight of polyethylene terephthalate (B-6) (MA-2103, manufactured by Unitika Ltd.) with a melting point of 255°C The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 3.

[0076] Comparative Example 4 A press sheet was obtained in the same manner as in Example 4, except that the resin composition (A) was not blended and only the composition of the thermoplastic resin (B) described below was used. [Thermoplastic resin (B) composition] 70% by weight of low-density polyethylene (B-1) (manufactured by Tosoh Corporation, product name Petrothene 205) with a melt mass flow rate of 3 g / 10 min and a melting point of 111°C 10% by weight of ethylene-vinyl alcohol copolymer (B-4) having an ethylene content of 35 mol% and a melting point of 177°C (manufactured by Kuraray Co., Ltd., product name EVAL C109B) 10% by weight of nylon 6 (B-5) with a melting point of 220°C (manufactured by Ube Industries, Ltd., product name UBE Nylon 1022D) 10% by weight of polyethylene terephthalate (B-6) (MA-2103, manufactured by Unitika Ltd.) with a melting point of 255°C The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 3.

[0077] Comparative Example 5 A press sheet was obtained in the same manner as in Example 4, except that a resin composition having the following composition was used as the resin composition (A). [Composition of resin composition (A)] 65% by weight of ethylene-vinyl acetate copolymer (a1-15) (Ultrathene 626, manufactured by Tosoh Corporation) with a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min 35% by weight of ethylene-vinyl acetate copolymer (a1-80) (manufactured by LANXESS AG, product name Levaprene 800) with a vinyl acetate content of 80% by weight and a melt mass flow rate of 5 g / 10 min The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 3.

[0078] Comparative Example 6 A press sheet was obtained in the same manner as in Example 4, except that a resin composition having the following composition was used as the resin composition (A). [Composition of resin composition (A)] 75% by weight of ethylene-vinyl acetate copolymer (a1-15) (Ultrathene 626, manufactured by Tosoh Corporation) with a vinyl acetate content of 15% by weight and a melt mass flow rate of 3 g / 10 min 25% by weight of ethylene-acrylic acid copolymer (a2-9) (SK Sogo Chemicals, product name SK Primacor 5980I) with an acrylic acid content of 9 mol% and a melt mass flow rate of 300 g / 10 min The obtained pressed sheets were subjected to impact tests and tensile tests. The evaluation results are shown in Table 3.

[0079] [Table 3]

Claims

1. A modifier for compatibilizing at least two types of resins, comprising a resin composition (A) which comprises the following components (1) and (2), in which the absolute value of the difference between the solubility parameter (SP value) calculated by the Fedors method of any ethylene-vinyl acetate copolymer constituting the ethylene-vinyl acetate copolymer (a1) and the SP value calculated by the Fedors method of any ethylene-acrylic acid copolymer or ethylene-methacrylic acid copolymer (a2) is 0.3 (MPa) 1 / 2 or less. (1) A copolymer containing at least two types of ethylene-vinyl acetate copolymers having different vinyl acetate contents. Composition (a1) (2) Either an ethylene-acrylic acid copolymer or an ethylene-methacrylic acid copolymer Resin (a2)

2. The modifier according to claim 1, wherein the resin composition (A) contains 50% by weight or more and 99% by weight or less of a composition (a1) containing an ethylene-vinyl acetate copolymer, and 1% by weight or more and 50% by weight or less of a copolymer (a2) of either an ethylene-acrylic acid copolymer or an ethylene-methacrylic acid copolymer, (wherein the sum of (a1) and (a2) is 100% by weight).

3. The modifier according to claim 1 or 2, wherein the resin composition (A) is an ethylene-acrylic acid copolymer or an ethylene-methacrylic acid copolymer, and the acrylic acid or methacrylic acid content in the copolymer (a2) is 3 mol% or more and 15 mol% or less.

4. The modifier described in any one of claims 1 to 3, wherein the resin composition (A) contains an ethylene-vinyl acetate copolymer, and the composition (a1) contains three or more types of ethylene-vinyl acetate copolymers having different vinyl acetate contents.

5. The modifier according to any one of claims 1 to 4, wherein in the ethylene-vinyl acetate copolymer composition (a1) of the resin composition (A), when the difference in the vinyl acetate content of each copolymer is taken, the difference in the vinyl acetate content of at least one pair of copolymers is 40 weight % or less.

6. A resin composition comprising 1% by weight or more and 50% by weight or less of the modifier according to any one of claims 1 to 5 and 50% by weight or more and 99% by weight or less of two or more thermoplastic resins (B) (wherein the total of (A) and (B) is 100% by weight).

7. The thermoplastic resin (B) is polyolefin, polyester, acrylic resin, polyamide, A small part of the group consisting of polycarbonate, polystyrene, and styrene-acrylonitrile copolymer. The resin composition according to claim 6, comprising at least one type of copolymer.

8. The thermoplastic resin (B) is high-density polyethylene, low-density polyethylene, linear low-density polyethylene, Styrene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl alcohol Copolymer, nylon 6, nylon 6,6, nylon 11, nylon 12, polyethylene terephthalate Polyethylene terephthalate, glycol modified polyethylene terephthalate resin, polybutylene terephthalate lactic acid (poly-L-lactic acid, poly-D-lactic acid, copolymer of L-lactic acid and D-lactic acid, Poly(L-lactic acid) and poly(D-lactic acid) stereocomplexes, polybutylene succinate 8. The resin composition according to claim 6, wherein the resin composition is at least one member selected from the group consisting of olefins.

9. The thermoplastic resin (B) is high-density polyethylene, low-density polyethylene, linear low-density polyethylene, Styrene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl alcohol Copolymer, nylon 6, nylon 6,6, nylon 11, nylon 12, polyethylene terephthalate Polyethylene terephthalate, glycol modified polyethylene terephthalate resin, polybutylene terephthalate The resin composition according to claim 8, which is at least one member selected from the group consisting of olefins.

10. The resin composition according to any one of claims 6 to 9, wherein the thermoplastic resin (B) is a used molded article.

11. A method for producing the resin composition according to any one of claims 6 to 10, comprising a kneading step of kneading a thermoplastic resin (B) and the modifier according to any one of claims 1 to 5 in a twin-screw extruder.

12. The kneading process is carried out under the condition of a screw rotation speed of 50 rpm to 3000 rpm of the twin screw extruder. The method for producing the resin composition according to claim 11 .

13. A molded article obtained by molding the resin composition according to any one of claims 6 to 10.

Citation Information

Patent Citations

  • Manufacture of sound insulating carpet

    JP1989241422A

  • Thermoplastic resin composition

    JP1990255846A

  • Compatibilizing agent, modifier for plastic recycling use, recycling plastic material and molded form therefrom

    JP2001220473A

  • Plastic material, recycling plastic material, and molded product

    JP2004182957A

  • Resin composition

    JP2005200509A