Manufacturing method of tow prepreg
The grooved roller method with controlled resin application and speed differential stabilizes resin content and width in tow prepreg, addressing production inefficiencies and contamination issues.
Patent Information
- Application Number
- JP2020152695
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-09-11
AI Technical Summary
Existing methods for manufacturing tow prepreg with high-viscosity matrix resin result in unstable resin content and width due to varying fiber bundle widths and resin application issues, leading to contamination and inefficiencies.
A method involving a grooved roller with controlled resin application and speed differential to stabilize resin content and width, using a grooved roller with a resin layer inside the grooves and a speed ratio that matches the fiber direction, ensuring complete resin transfer and uniform application.
Achieves stable resin content and width in tow prepreg, minimizing contamination and improving production quality by ensuring complete resin transfer and uniform application.
Smart Images

Figure 0007563063000004 
Figure 0007563063000005 
Figure 0007563063000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a tow prepreg, and more particularly to a method for uniformly applying a coating liquid to reinforcing fibers even when the matrix resin has a high viscosity. [Background technology]
[0002] Fiber-reinforced composite materials (FRP), which are made by reinforcing matrix resins, including thermoplastic resins and thermosetting resins, with reinforcing fibers, are used in a variety of fields, including aerospace materials, automotive materials, industrial materials, pressure vessels, building materials, housings, medical applications, and sports applications. Carbon fiber-reinforced composite materials (CFRP) are widely and preferably used when high mechanical properties and light weight are required. On the other hand, glass fiber-reinforced composite materials (GFRP) may be used when cost is prioritized over mechanical properties and light weight. FRP is manufactured by obtaining an intermediate substrate (prepreg) in which a matrix resin is impregnated into a bundle of reinforcing fibers, laminating and molding the prepreg, and further heat-curing it when a thermosetting resin is used, to produce a component made of FRP.
[0003] Prepregs include two-dimensional sheet-like objects and narrow tape-like objects, but narrow tape-like prepregs (tow prepregs) are preferably used for spherical components such as pressure vessels and components with complex shapes such as sports goods. The tow prepreg referred to here is a product in which an uncured thermosetting resin composition such as epoxy resin, vinyl ester resin, unsaturated polyester resin, etc. is impregnated in a predetermined composition ratio into a continuous fiber bundle such as a tow, yarn, roving, or multifilament, and is usually once wound up on a bobbin or the like and then commercialized. In addition, FRP using tow prepregs as a starting material is usually formed by loading a predetermined number of bobbins on which tow prepregs are wound onto a creel, and then leading the tow prepregs to a filament winding device, an automatic tape layup device, a drum winding device, etc. while unwinding them, stacking and shaping them into any shape such as a tube, a sphere, or a sheet, and then heating them to harden the matrix resin.
[0004] As a method for manufacturing a tow prepreg, for example, Patent Document 1 discloses a method in which a resin layer of uniform thickness is formed on the entire surface of a cylindrical roller, and then the reinforcing fiber bundle is brought into contact with the resin layer to supply resin to the reinforcing fiber bundle. This method is excellent in workability such as threading the reinforcing fiber bundle, and it is possible to control the thickness of the resin layer by adjusting the clearance between the roller and the blade, thereby adjusting the resin content of the tow prepreg. However, this method has a problem that when the width of the reinforcing fiber bundle changes, the amount of resin in contact with the reinforcing fiber bundle changes, and the resin content of the tow prepreg varies. Patent Document 1 proposes a method for making the resin content uniform by regulating the width of the reinforcing fiber bundle just before the resin layer on the roller surface and the reinforcing fiber bundle come into contact. However, in reality, the width of the reinforcing fiber bundle also expands when it comes into contact with the resin layer on the roller surface, and the extent of the expansion varies depending on the tension applied to the reinforcing fiber bundle, the thickness of the resin layer on the roller surface, and the viscosity of the resin, so it is difficult to strictly control the width of the reinforcing fiber bundle on the roller surface. Furthermore, in the method of Patent Document 1, a resin layer is formed even in the parts where the reinforcing fiber bundles do not run, so that excess resin adheres to the widthwise ends of the reinforcing fiber bundles. This not only makes the resin content of the tow prepreg unstable, but also causes the downstream conveying rollers and the like to be contaminated with resin.
[0005] As another method for manufacturing a tow prepreg, Patent Document 2 discloses a method in which a groove is provided in a cylindrical roller, and the reinforcing fiber bundle is impregnated by contacting the resin supplied to the groove. In this method, the width of the reinforcing fiber bundle on the roller can be regulated by the groove, so that the width of the reinforcing fiber bundle is stabilized and the resin content of the tow prepreg is less likely to fluctuate. In addition, by passing through the groove of the roller, excess resin does not adhere to the width direction end of the reinforcing fiber bundle, and downstream conveying rollers and the like are not contaminated with resin. Here, in the method of Patent Document 2, it is preferable to make the peripheral speed of the surface of the cylindrical roller the same as the running speed of the reinforcing fiber bundle, and it is suggested that the resin is applied to the reinforcing fiber bundle mainly by impregnation. For this reason, when the resin has a high viscosity or when the running speed of the reinforcing fiber bundle is high, the impregnation on the roller surface deteriorates, and the reinforcing fiber bundle leaves the roller surface while leaving an unimpregnated resin layer between the reinforcing fiber bundle and the roller surface. At this time, since the running speed of the reinforcing fiber bundle and the peripheral speed of the roller surface are the same, the unimpregnated resin layer peels off like strings and adheres to both the reinforcing fiber bundle and the roller surface. As a result, not only does the resin content of the tow prepreg become unstable, but the peeled resin scatters and contaminates the surrounding area, and some of the fluff of the reinforcing fiber bundle is taken up by the resin on the roller surface, causing part of the reinforcing fiber bundle to wrap around the roller, making it impossible for it to run. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2014-148573 A [Patent Document 2] Japanese Patent Application Publication No. 9-255799 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a method for producing a tow prepreg which facilitates operations such as threading and which is capable of maintaining uniform width and resin content of the tow prepreg even when a highly viscous resin is used. [Means for solving the problem]
[0008] The method for producing a tow prepreg of the present invention, which solves the above-mentioned problems, comprises the steps of forming a resin layer inside the grooves of a rotating grooved roller, and bringing reinforcing fibers into contact with the resin layer of the grooved roller to transfer the resin layer to the reinforcing fibers and impregnate them with resin, and is characterized in that the rotation direction of the grooved roller coincides with the running direction of the reinforcing fibers, and the peripheral speed at the bottom of the groove is controlled to be slower than the running speed of the reinforcing fibers. Effect of the Invention
[0009] According to the method for producing a tow prepreg of the present invention, the width of the reinforcing fiber is regulated by contacting the reinforcing fiber with the resin layer inside the groove of the grooved roller, and the amount of resin applied to the reinforcing fiber can be stabilized. In addition, by controlling the peripheral speed at the bottom surface of the groove of the grooved roller to be slower than the running speed of the reinforcing fiber, the reinforcing fiber has the effect of scraping off the resin layer inside the groove. Even if there is an unimpregnated resin layer between the reinforcing fiber and the grooved roller, the resin adheres to the reinforcing fiber side and almost no resin remains on the grooved roller side, and the entire amount of resin supplied inside the groove can be applied to the reinforcing fiber. In addition, since there is a speed difference between the bottom surface of the groove of the grooved roller and the reinforcing fiber, the reinforcing fiber opens on the grooved roller and the width of the reinforcing fiber expands to the full width of the groove, so that no resin is left in the corners of the groove. As a result, the width and resin content of the tow prepreg are stabilized, and it is possible to obtain a high-quality tow prepreg. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram showing a method for producing a tow prepreg according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a method for producing a tow prepreg according to another embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing a method for producing a tow prepreg according to another embodiment of the present invention. [Figure 4] 5A to 5C are schematic diagrams showing examples of the shape of a guide roller. [Diagram 5] FIG. 2 is a schematic diagram showing a method for producing a tow prepreg according to another embodiment of the present invention. [Figure 6] FIG. 2 is a schematic diagram showing a method for producing a tow prepreg according to another embodiment of the present invention. [Figure 7] FIG. 2 is a schematic diagram showing a method for producing a tow prepreg according to another embodiment of the present invention. [Figure 8] FIG. 2 is a schematic diagram showing a method for producing a tow prepreg according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] A preferred embodiment of the present invention will be described below. Note that the following description is merely an example of an embodiment of the invention, and the present invention should not be construed as being limited thereto, and various modifications are possible without departing from the object and effect of the present invention. In addition, expressions expressing a numerical range using "from" or "to" include numerical values at both ends.
[0012] FIG. 1 shows a schematic diagram of a method for producing a tow prepreg according to an embodiment of the present invention. FIG. 1 is viewed from the width direction of the reinforcing fiber 1 and the axial direction of the grooved roller 2. The outer solid circle of the grooved roller 2 represents the outer peripheral surface of the roller, and the inner dashed circle represents the bottom surface of the groove. The reinforcing fiber 1 and the grooved roller 2 run and rotate in the direction of the arrow in FIG. 1, and the peripheral speed of the bottom surface of the groove of the grooved roller 2 is controlled to be slower than the running speed of the reinforcing fiber 1. The grooved roller 2 is provided with a nozzle 3 for supplying resin, and a resin layer 4 (not shown) is formed inside the groove of the grooved roller 2. At this time, the moving speed of the resin layer 4 is almost the same as the peripheral speed of the bottom surface of the groove of the grooved roller 2. Next, the reinforcing fiber 1 is transported so as to be guided into the groove of the grooved roller 2, and comes into contact with the resin layer 4 inside the groove. In the section A where the reinforcing fiber 1 and the resin layer 4 are in contact with each other, the reinforcing fiber 1 runs as if sliding on the resin layer 4, and a part of the resin of the resin layer 4 is impregnated into the inside of the reinforcing fiber 1. Furthermore, the unimpregnated resin layer is scraped off by the reinforcing fibers 1 due to the speed difference between the reinforcing fibers 1 and the resin layer 4, and is wound up as a tow prepreg 5 by a downstream winder or the like (not shown).
[0013] Examples of reinforcing fibers include carbon fibers, glass fibers, metal fibers, metal oxide fibers, metal nitride fibers, and organic fibers (aramid fibers, polybenzoxazole fibers, polyvinyl alcohol fibers, polyethylene fibers, etc.). From the viewpoints of the mechanical properties and light weight of FRP, it is preferable to use carbon fibers.
[0014] The form of the reinforcing fibers is not particularly limited, but examples include continuous fiber bundles such as tow, yarn, roving, and multifilament, as well as unidirectional materials (UD substrates) in which these are arranged in one direction on a surface, and reinforcing fiber fabrics in which reinforcing fibers are arranged multiaxially or randomly to form a sheet. The width and thickness of the reinforcing fibers are also not particularly limited, but a width of 3 mm to 30 mm and a thickness of 0.1 mm to 0.5 mm that are easy to handle as a tow prepreg can be used.
[0015] The resin used in the tow prepreg of the present invention (hereinafter sometimes referred to as the matrix resin) can be appropriately selected depending on the application, and may be any resin generally used in FRP, such as a thermoplastic resin, a thermosetting resin, or a photocurable resin. The matrix resin may be a molten resin obtained by heating and melting it, or a liquid resin at room temperature. It may also be a solution or varnish made by using a solvent. Polymer particles or inorganic particles may be added to prevent the tow prepreg from collapsing when wound around a bobbin, to prevent the resin from seeping out, and to improve the strength of the FRP.
[0016] The grooved roller 2 used in the present invention is not particularly limited in shape or material, but for example, a stainless steel roller having grooves formed on its surface by cutting can be used. In this case, the width of the groove is preferably about the same as the width of the reinforcing fiber. Specifically, the width of the reinforcing fiber is preferably ±5 mm, more preferably ±2 mm. The depth of the groove is not particularly limited as long as the reinforcing fiber does not deviate from the groove, but from the viewpoint of ease of processing and cleaning, it is preferably 0.5 mm to 5 mm. In addition, as a method of forming the groove, a plurality of guide members such as set collars may be installed on a smooth roller, and the gap between adjacent guide members may be used as the groove. With this method, the groove width can be changed arbitrarily, but care must be taken because fluff may be caught in the gap between the guide member and the smooth roller, causing the reinforcing fiber to wrap around it. From the viewpoint of preventing the reinforcing fiber from wrapping around it and stably producing tow prepregs, it is preferable to form the groove on the roller surface by cutting.
[0017] If there is concern about fuzzing due to friction between the bottom or wall of the groove and the reinforcing fibers, the roller may be made of a material with a low friction coefficient such as PTFE or high molecular weight polyethylene, or the surface may be subjected to a surface treatment such as DLC coating. It is also preferable that the bottom and wall of the groove are smooth.
[0018] The nozzle 3 used in the present invention is not particularly limited as long as it can form a resin layer inside the groove, but a cylindrical nozzle or a slit die can be used. From the viewpoint of forming a resin layer of uniform thickness inside the groove, the outlet shape of the nozzle is preferably slit-shaped. The width and tip shape of the nozzle may be freely selected according to the width and thickness of the resin layer to be formed. Next, the means for supplying resin to the nozzle 3 is not particularly limited, but it is preferable to use a metering pump such as a single-axis screw pump, a twin-axis extruder, a diaphragm pump, or a syringe pump, since it is possible to control the amount of resin applied to the reinforcing fiber. In the present invention, since the reinforcing fiber scrapes off the resin layer, almost the entire amount of resin supplied to the grooved roller is applied to the reinforcing fiber, it is possible to adjust the resin content of the tow prepreg only by the supply amount of the metering pump, and the controllability of the resin content of the tow prepreg is extremely excellent.
[0019] The width of the resin layer 4 formed in the present invention is not particularly limited, but it is preferable to make the width of the resin layer 4 slightly narrower than the width of the groove of the grooved roller 2. Specifically, it is preferable to make the width of the resin layer 4 0.5 mm to 3 mm narrower than the width of the groove of the grooved roller 2. For example, if the resin layer 4 is formed to the full extent of the groove of the grooved roller, the resin at the corner of the groove may overflow from the widthwise end of the reinforcing fiber, and a part of the resin may wrap around the back surface of the reinforcing fiber, contaminating the downstream conveying rollers and the like with the resin. On the other hand, if the width of the resin layer 4 is made too narrow, the resin may not be applied to the widthwise end of the reinforcing fiber, and unevenness in the resin content may occur in the width direction of the tow prepreg. Therefore, if the width of the resin layer 4 is made 0.5 mm to 3 mm narrower than the width of the groove of the grooved roller 2, the resin will not wrap around the back surface of the reinforcing fiber, and the widthwise end of the reinforcing fiber will be impregnated with resin during the process of transporting the tow prepreg downstream and the process of winding it with a winder, making it possible to minimize unevenness in the resin content.
[0020] In the present invention, the length of section A where the reinforcing fiber 1 and the resin layer 4 contact each other is not particularly limited, and may be freely determined in consideration of the state of scraping off the resin layer by the reinforcing fiber. However, care must be taken because if section A where the reinforcing fiber 1 and the resin layer 4 contact each other is made too long, the reinforcing fiber will be completely impregnated with the resin of the resin layer, and the reinforcing fiber 1 and the bottom surface of the groove of the grooved roller 2 may directly rub against each other, causing fluff.
[0021] In the present invention, the ratio of the circumferential speed of the bottom surface of the groove of the grooved roller 2 to the running speed of the reinforcing fiber 1 (hereinafter referred to as the speed ratio) is preferably determined in consideration of the formation of the resin layer on the surface of the grooved roller and the scraping of the resin by the reinforcing fiber. Specifically, when the speed ratio is set to 3% to 50%, a higher quality tow prepreg can be obtained. The reasons for this are described in detail below.
[0022] First, the thickness T of the resin applied to a general tow prepreg is often 30 μm to 100 μm, including the amount impregnated into the reinforcing fibers. In this case, the thickness H of the resin layer to be formed inside the groove of the grooved roller 2 is calculated as T / speed ratio when the width of the resin layer and the width of the reinforcing fibers are equal. For example, when the thickness T of the resin applied to the tow prepreg is 40 μm and the speed ratio of the reinforcing fibers to the roller is 80%, the thickness H of the resin layer to be formed inside the groove is 50 μm. Here, when a high-viscosity resin layer is formed on the roller using a nozzle, the clearance (gap) between the nozzle and the roller surface needs to be set to 1 to 1.5 times the thickness of the resin layer. If the clearance is larger than this, the width of the resin layer formed will be narrow, air bubbles will be mixed into the resin layer, and in the worst case, it will be impossible to form a continuous resin layer.
[0023] In the above example of a speed ratio of 80%, in order to form a 50 μm thick resin layer inside the groove of the grooved roller, the clearance between the nozzle and the grooved roller needs to be set to 50 μm to 75 μm. However, when the clearance is narrow like this, the influence of the setting error of the operator (about 10 μm to 30 μm) and the eccentricity of the grooved roller (about 10 μm to 50 μm) becomes large, causing unevenness in the thickness of the resin layer formed on the grooved roller. As a result, the resin content of the tow prepreg also becomes uneven in the longitudinal direction, and the quality of the tow prepreg deteriorates. To avoid this, it is necessary to use a device that measures the clearance between the nozzle and the grooved roller and a high-precision grooved roller with small eccentricity, which results in high equipment costs.
[0024] For example, when the speed ratio between the reinforcing fiber and the roller is 20%, when the thickness T of the resin applied to the tow prepreg is 40 μm, the thickness H of the resin layer to be formed inside the groove is 200 μm, and the clearance between the nozzle and the grooved roller can be expanded from 200 μm to 300 μm. When the clearance is wide like this, the influence of the setting error of the operator and the eccentricity of the grooved roller becomes relatively small, and it becomes possible to form a resin layer of uniform thickness on the grooved roller. As a result, it becomes possible to obtain a tow prepreg of higher quality.
[0025] On the other hand, if the speed ratio between the reinforcing fibers and the roller is too small, the thickness H of the resin layer formed on the grooved roller becomes very large, and the resin layer may sag due to gravity, or when the reinforcing fibers run onto the resin layer, the resin may move in the width direction of the reinforcing fibers and seep out from the width direction ends of the reinforcing fibers. Specifically, when the thickness H of the resin layer formed on the grooved roller exceeds 1 mm, the above phenomenon is likely to occur. As a result, excess resin adheres to the width direction ends of the tow prepreg, contaminating the downstream conveying rollers, etc. with resin.
[0026] From the above, the thickness H of the resin layer formed inside the groove of the grooved roller is preferably 200 μm to 1 mm, and considering that the thickness T of the resin contained in a typical tow prepreg is 30 μm to 100 μm, the speed ratio between the reinforcing fiber and the roller is preferably 3% to 50%.
[0027] Furthermore, if the viscosity of the resin supplied from the nozzle 3 is too high, scraping of the resin layer 4 by the reinforcing fibers 1 inside the grooves of the grooved roller 2 may not be completed. In this case, it is preferable to heat the resin layer 4 to reduce the viscosity, which promotes scraping of the resin layer 4 by the reinforcing fibers 1. The method of heating the resin layer 4 is not particularly limited, but the resin layer 4 may be directly heated by blowing hot air onto it, the grooved roller 2 may be heated, or the resin supplied from the nozzle 3 may be preheated.
[0028] FIG. 2 is a schematic diagram showing a method for producing a tow prepreg according to another embodiment of the present invention. In the embodiment of FIG. 2, the residual resin in the groove of the grooved roller is removed by a blade 6 in a section downstream of the position where the grooved roller 2 and the reinforcing fiber 1 are separated and upstream of the nozzle 3 that forms the resin layer 4 on the grooved roller 2. The purpose of the present invention is that the reinforcing fiber 1 scrapes off the entire amount of resin supplied to the grooved roller 2. However, in rare cases, when the width of the reinforcing fiber is significantly narrowed due to the reinforcing fiber 1 being twisted, a part of the resin layer 4 is not scraped off by the reinforcing fiber and remains in the groove of the grooved roller. The residual resin may go around once by the grooved roller and disturb the formation of the next resin layer by the nozzle 3 and the scraping of the resin layer by the next reinforcing fiber. Therefore, it is preferable to remove the residual resin by the blade 6, since it does not hinder the formation of the next resin layer or the scraping of the resin layer by the reinforcing fiber. In addition, when the tow prepreg is produced for a long time, fluff may accumulate in the groove of the grooved roller 2, and it is preferable to install the blade 6 from the viewpoint of removing this fluff. The material of the blade 6 is not particularly limited, and a resin or metal blade can be used.
[0029] FIG. 3 is a schematic diagram showing a method for producing a tow prepreg according to another embodiment of the present invention. In the embodiment of FIG. 3, a guide roller 7 is provided upstream of the grooved roller 2 on the conveying path of the reinforcing fiber to regulate the meandering and width change of the reinforcing fiber 1. In the manufacturing method of the tow prepreg of the present invention, it is important to stably guide the reinforcing fiber 1 to the same position as the resin layer 4 formed inside the groove of the grooved roller 2, and it is preferable to suppress the meandering of the reinforcing fiber upstream of the grooved roller on the conveying path of the reinforcing fiber, as in the embodiment of FIG. 3. In addition, if the width of the reinforcing fiber 1 and the width of the groove of the grooved roller 2 are significantly different, the width direction end of the reinforcing fiber may be folded inside the groove of the grooved roller, or the resin layer 4 may remain unscraped. From the viewpoint of preventing these, it is preferable to control the width of the reinforcing fiber in advance upstream of the grooved roller on the conveying path of the reinforcing fiber, as in the embodiment of FIG. 3. Here, as the shape of the guide roller 7 that regulates the meandering and width change of the reinforcing fiber 1, for example, a flanged roller shown in FIG. 4(A) or a drum roller shown in FIG. 4(B) can be used.
[0030] FIG. 5 is a schematic diagram showing a method for manufacturing a tow prepreg according to another embodiment of the present invention. In the embodiment of FIG. 5, the formation of the resin layer 4 by the grooved roller 2 and the nozzle 3, the transfer of the resin, and the impregnation are performed on one side of the reinforcing fiber 1 (the lower side in FIG. 5), and then the formation of the second resin layer 14 by the second grooved roller 12 and the second nozzle 13, the transfer of the resin, and the impregnation are performed on the other side of the reinforcing fiber 1 (the upper side in FIG. 5). In this way, by transferring the resin from both sides of the reinforcing fiber 1, the distribution of the resin contained in the tow prepreg 5 in the thickness direction becomes uniform, and it becomes possible to obtain a tow prepreg of higher quality. Furthermore, since the amount of resin supplied to the reinforcing fiber 1 from each grooved roller is small, the scraping of the resin by the reinforcing fiber is completed smoothly, no resin is left unscraped on the grooved roller, and the resin content of the tow prepreg 5 can be made more uniform in the longitudinal direction. In addition, by impregnating the reinforcing fibers 1 with the resin from both sides, the reinforcing fibers can be easily impregnated with the resin, and it is possible to obtain a tow prepreg 5 that does not contain air (voids) inside. In the embodiment of FIG. 5, it is preferable to make the amount of resin supplied from the nozzle 3 and the second nozzle 13 equal in order to uniformly distribute the resin contained in the tow prepreg 5 in the thickness direction. However, if it is desired to attach more resin to one side in order to change the characteristics of the tow prepreg between one side and the other side, the amount of resin supplied from one nozzle may be increased. In addition, in order to change the characteristics of the tow prepreg between one side and the other side, resins of different compositions may be supplied from the nozzle 3 and the second nozzle 13, respectively.
[0031] Fig. 6 is a schematic diagram showing a method for producing a tow prepreg according to another embodiment of the present invention. In the embodiment of Fig. 6, a nip roller 8 is provided in the groove of the grooved roller 2 in section A where the reinforcing fiber 1 and the resin layer 4 contact each other. This promotes impregnation of the reinforcing fiber 1 with the resin, and makes it possible to obtain a tow prepreg 5 that does not contain air inside. In addition, the nip roller 8 spreads the reinforcing fiber 1 inside the groove of the grooved roller 2, so that the width of the reinforcing fiber spreads to the full extent of the groove, making it possible to obtain a tow prepreg 5 with a stable width. The nip roller 8 may be provided anywhere in section A where the reinforcing fiber 1 and the resin layer 4 contact each other.
[0032] Fig. 7 is a schematic diagram showing a method for producing a tow prepreg according to another embodiment of the present invention. In the embodiment of Fig. 7, the basis weight of the tow prepreg 5 is measured by a basis weight measuring device 20 downstream of the grooved roller 2. Furthermore, the measured value measured by the basis weight measuring device 20 is fed back to the discharge rate of the pump 22 by the control device 21. In the embodiment of Fig. 7, for example, if the basis weight of the tow prepreg 5 is larger than the standard value, the basis weight measuring device 20 detects this, and feedback control is performed to reduce the discharge rate of the pump 22 and reduce the basis weight of the tow prepreg. This makes it possible to obtain a tow prepreg 5 with a uniform basis weight over its entire length.
[0033] Fig. 8 is a schematic diagram showing a method for producing a tow prepreg according to another embodiment of the present invention. In the embodiment of Fig. 8, a plurality of reinforcing fibers 1 are passed through a multi-grooved roller 9 having a plurality of grooves, and a resin layer 4 is formed inside each groove by a nozzle 3, and the resin is transferred to and impregnated into the reinforcing fibers. This makes it possible to simultaneously produce a plurality of tow prepregs 5, and significantly improves the productivity of the tow prepregs. Here, in Fig. 8, the resin layer is formed in each groove of the multi-grooved roller 9 by a plurality of nozzles 3, but this is not limited thereto, and for example, a resin layer may be formed by supplying resin in a stripe shape from one nozzle 3.
[0034] In addition, if the thickness of the resin layer in each groove of the multiple grooved roller 9 can be controlled independently for each groove, it is possible to obtain a tow prepreg with a uniform basis weight or resin content between bobbins even if there is a variation in the weight of the multiple reinforcing fibers 1, which is preferable. As a method for independently controlling the thickness of the resin layer for each groove, for example, multiple pumps may be used to supply resin to multiple nozzles 3, or one pump may be used to supply resin to multiple nozzles 3 in divided portions while changing the pressure loss of each nozzle 3 to change the resin division ratio. As a method for changing the pressure loss of the nozzle 3, for example, the outlet shape of the nozzle 3 may be deformed, or the piping that communicates the nozzle 3 with the pump may be deformed. EXAMPLES
[0035] Next, specific examples of the present invention will be described. Reference example However, the present invention will be described with reference to the following Reference example It is not to be construed as being limited to the following:
[0036] below Reference example As common implementation conditions to the above and the comparative examples, carbon fiber (Toray Industries, "TORAYCA (registered trademark)" T700SC (24K)) was used as the reinforcing fiber, and epoxy resin (specific gravity 1.2, viscosity 50 Pa s at room temperature of 20°C) was used as the matrix resin. The width of the carbon fiber immediately after being unwound from the bobbin was 10 mm.
[0037] Table 1 shows the present invention Reference example 1 and Comparative Examples 1 to 3, which are different from the present invention, were used to produce tow prepregs, and the state of transfer of the resin to the reinforcing fibers was confirmed.
[0038] [ Reference example 1] The tow prepreg was manufactured using the tow prepreg manufacturing apparatus of the embodiment of FIG. 1. The material of the grooved roller 2 was stainless steel, the diameter of the bottom of the groove was 100 mm, the width of the groove was 11 mm, and the depth of the groove was 2 mm. The outlet shape of the nozzle 3 that supplies the resin to the grooved roller 2 was a slit shape with a width of 8 mm and a height of 2 mm. A "Mono Pump (registered trademark)" (single-axis screw pump) manufactured by Heishin Soubi was used as a metering pump that supplies the resin to the nozzle 3. The conveying speed of the reinforcing fiber 1 was 30 m / min, the rotation direction of the grooved roller 2 was the same as the running direction of the reinforcing fiber 1 (forward rotation), and the peripheral speed of the bottom of the groove of the grooved roller was 3 m / min (speed ratio 10%). The embrace angle between the grooved roller 2 and the reinforcing fiber was 45°. The length of the section A where the reinforcing fiber 1 and the grooved roller 2 contacted each other was about 40 mm. The amount of resin supplied from the metering pump was 16 g / min, and the clearance between the nozzle 3 and the grooved roller 2 was adjusted so that the width of the resin layer 4 formed inside the grooves of the grooved roller 2 was 8 mm. The thickness of the resin layer 4 at this time was calculated to be about 560 μm.
[0039] As an evaluation method, the inside of the groove of the grooved roller 2 after the tow prepreg 5 was released was visually inspected. If no resin layer remained, the total resin transfer was judged as "OK". If some resin layer remained or if the resin overflowed from the groove of the grooved roller and dripped down from the grooved roller during the production of the tow prepreg, the total resin transfer was judged as "NO".
[0040] the result, Reference example In case 1, after the tow prepreg 5 was released, no resin layer remained inside the groove of the grooved roller 2, and the transfer of the entire amount of resin was “OK.” In addition, when the obtained tow prepreg 5 was wound onto a bobbin and then unwound by hand to check its condition, it was found that the entire width of the tow prepreg was impregnated with resin.
[0041] [Comparative Example 1] Reference exampleThe grooved roller was replaced with a non-grooved roller under the same conditions as in 1 to produce tow prepregs. The diameter of the non-grooved roller was 100 mm, and the peripheral speed of the groove surface was 3 m / min (speed ratio 10%). Other conditions and evaluation methods were as follows: Reference example Same as 1.
[0042] As a result, in Comparative Example 1, the reinforcing fibers 1 that had climbed onto the resin layer 4 on the roller meandered in the width direction of the reinforcing fibers in the middle of section A where the reinforcing fibers and the resin layer contacted, and fell off from the resin layer, resulting in a state in which a part of the resin layer was not scraped off by the reinforcing fibers. Since the resin layer remained on the roller after the tow prepreg 5 was released, the transfer of the entire amount of resin was "impossible." In addition, the amount of the resin layer remaining on the roller changed in conjunction with the meandering of the reinforcing fibers 1. In addition, when the state of the obtained tow prepreg 5 was checked, it was found that parts that were impregnated with resin and parts that were not impregnated with resin were mixed in the longitudinal direction.
[0043] [Comparative Example 2] Reference example The rotation direction of the grooved roller 2 was changed from the implementation condition 1 to the opposite (reverse rotation) to the running direction of the reinforcing fiber 1, and a tow prepreg was produced. The peripheral speed of the groove surface was 3 m / min (speed ratio 10%). Other implementation conditions and evaluation methods were Reference example Same as 1.
[0044] As a result, in Comparative Example 2, a resin puddle was formed between the tow prepreg 5 and the grooved roller 2 at the position where the tow prepreg 5 separated from the grooved roller 2. The resin puddle grew over time while generating an internal vortex flow, and overflowed from the groove of the grooved roller, and eventually some of the resin dripped from the grooved roller onto the floor. Although the tow prepreg had taken some of the resin out of the resin puddle, most of the resin supplied to the grooved roller had dripped onto the floor, and transfer of the entire amount of resin was "impossible." In addition, discontinuous lumps of resin were attached to both ends of the width of the traveling tow prepreg 5, contaminating the downstream roller with resin.
[0045] [Comparative Example 3] Reference exampleThe peripheral speed of the groove surface of the grooved roller 2 was changed to 30 m / min (speed ratio 100%) from the implementation condition 1, and the tow prepreg was manufactured. Other implementation conditions and evaluation methods Reference example Same as 1.
[0046] As a result, in Comparative Example 3, when the tow prepreg 5 was separated from the grooved roller 2, stringing of the resin was observed between the tow prepreg and the grooved roller, and part of the resin layer remained inside the grooves of the grooved roller after the tow prepreg was separated, so the transfer of the entire resin was "impossible." Reference example The amount of resin impregnated was less than that of 1.
[0047] [Table 1]
[0048] Table 2 shows the present invention Reference example The results are as follows: tow prepregs were manufactured under each of the implementation conditions 1 to 4, and the state of transfer of the resin to the reinforcing fibers and the width of the resin layer 4 formed inside the grooves of the grooved roller 2 were confirmed. The width of the resin layer 4 was measured by placing a scale on the grooved roller 2 and visually checking the variation in the width of the resin layer during one rotation of the grooved roller.
[0049] [ Reference example 2] Reference example The peripheral speed of the groove surface of the grooved roller 2 was changed to 6 m / min (speed ratio 20%) from the implementation conditions in 1, and the tow prepreg was manufactured. Other implementation conditions and evaluation methods were as follows. Reference example Same as 1.
[0050] the result, Reference example In the test 2, after the tow prepreg 5 was separated from the grooved roller 2, no resin remained inside the grooves of the grooved roller, and the transfer of the entire amount of resin was “OK.” In addition, the width of the resin layer 4 was stable at 8 mm.
[0051] [ Reference example 3] Reference example The peripheral speed of the groove surface of the grooved roller 2 was changed to 15 m / min (speed ratio 50%) from the implementation condition 1, and the tow prepreg was manufactured. Other implementation conditions and evaluation methods were Reference example Same as 1.
[0052] the result, Reference example In the case of 3, after the tow prepreg 5 was separated from the grooved roller 2, no resin remained inside the groove of the grooved roller, and the transfer of the entire amount of resin was “OK.” In addition, the width of the resin layer 4 was stable at 8 mm.
[0053] [ Reference example 4] Reference example The peripheral speed of the groove surface of the grooved roller 2 was changed to 21 m / min (speed ratio 70%) from the implementation conditions in 1, and the tow prepreg was manufactured. Other implementation conditions and evaluation methods were Reference example Same as 1.
[0054] the result, Reference example In case 4, after the tow prepreg 5 was separated from the grooved roller 2, no resin remained inside the grooves of the grooved roller, and the transfer of the entire amount of resin was "OK". However, the width of the resin layer 4 was unstable, varying from 6 mm to 8 mm during one rotation of the grooved roller 2. The thickness of the resin layer 4 at this time was calculated to be about 70 μm to 90 μm.
[0055] [Table 2]
[0056] Table 3 shows the present invention Reference example Tow prepregs were produced under the respective implementation conditions of 1 and 5, and the resin content and the variation in the resin content of the obtained tow prepreg 5 were measured.
[0057] As an evaluation method, first, reinforcing fiber 1 without resin was unwound from a bobbin, cut into 10 pieces every 600 mm in length, and the mass was measured, and the average of the 10 pieces was taken as the average mass Wf of the reinforcing fiber. Next, the obtained tow prepreg 5 was unwound from a bobbin, cut into 10 pieces every 600 mm in length, and the mass Wt of the tow prepreg was measured. The mass Wr of the resin was calculated by subtracting the average mass Wf of the reinforcing fiber from the mass Wt of the tow prepreg 5, which was Wr=Wt-Wf, and the resin content of the tow prepreg was calculated as Wr / Wt (%). Reference example The resin content of 10 tow prepregs was calculated and the average resin content was calculated. The variation in the resin content of the 10 tow prepregs was calculated as (maximum value - minimum value) / 2 (%).
[0058] Reference example The average resin content of the tow prepreg 5 obtained in 1 was 26%, and the variation in the resin content was ±2.5%.
[0059] [ Reference example 5] A tow prepreg was produced using the tow prepreg production apparatus of the embodiment shown in FIG. Reference example In No. 5, the second grooved roller 12 is used to apply resin to both sides of the reinforcing fiber. The total amount of resin supplied to the nozzles 3 and 13 is 16 g / min, and the pressure loss of the resin supply pipes leading to the nozzles 3 and 13 is unified so that the resin is supplied in roughly half the amount. Other implementation conditions are Reference example Same as 1.
[0060] the result, Reference example The average resin content of the tow prepreg 5 obtained in 5 was 25%, and the variation in the resin content was ±1.5%. Reference example The variation in resin content is smaller than in case 1).
[0061] [Table 3] [Industrial Applicability]
[0062] The tow prepreg obtained by the manufacturing method of the present invention can be widely used as FRP, such as CFRP, in aerospace applications, structural and interior materials for automobiles, trains, ships, etc., pressure vessels, industrial materials, sports materials, medical equipment, housings, civil engineering and construction applications, etc. [Explanation of symbols]
[0063] 1 Reinforced Fiber 2 Grooved rollers 3 Nozzles 4 Resin layer 5 Tow prepreg 6 Blades 7 Guide roller 8 Nip roller 9 Multi-grooved roller 12 Second grooved roller 13 Second Nozzle 14 Second resin layer 20. Basis weight measuring device 21 Control device 22 Pump A is the length of the section where the reinforcing fiber and the resin layer are in contact H: the thickness of the resin layer to be formed inside the groove of the grooved roller T Actual thickness of the resin layer applied to the tow prepreg Wf Average mass of reinforcing fibers Wt Mass of tow prepreg Wr Resin mass
Claims
1. A method for producing a tow prepreg in which reinforcing fibers are impregnated with a resin, comprising the steps of: The method includes the steps of forming a resin layer inside the grooves of a rotating grooved roller, and contacting reinforcing fibers with the resin layer of the grooved roller to transfer the resin layer to the reinforcing fibers and impregnate them with resin, The resin layer is transferred to one side of the reinforcing fiber by the grooved roller and the resin is impregnated therewith, and then the resin layer is transferred to the other side of the reinforcing fiber by a second grooved roller and the resin is impregnated therewith; The method for producing a tow prepreg further comprises controlling a rotation direction of the grooved roller to coincide with a running direction of the reinforcing fibers, and a peripheral speed at the bottom of the groove to be slower than a running speed of the reinforcing fibers.
2. 2. The method for producing a tow prepreg according to claim 1, wherein a peripheral speed of the grooved roller at a bottom surface of the groove is 3% to 50% of a running speed of the reinforcing fibers.
3. 3. The method for producing a tow prepreg according to claim 1, further comprising removing resin remaining inside the grooves of the grooved roller in a section of the outer periphery of the grooved roller downstream of a position where the grooved roller and the reinforcing fibers are separated from each other and upstream of a position where a resin layer is formed on the grooved roller.
4. The method for producing a tow prepreg according to any one of claims 1 to 3, wherein a width of the reinforcing fibers is controlled upstream of the grooved roller in a conveying path of the reinforcing fibers.
5. 5. The method for producing a tow prepreg according to claim 1, wherein the reinforcing fibers are pressed against the resin layer by a nip roller in a section of the outer periphery of the grooved roller where the reinforcing fibers and the resin layer are in contact with each other.
6. 6. The method for producing a tow prepreg according to claim 1, wherein the grooved roller has a plurality of grooves in an axial direction, and in each groove, a resin layer is formed inside the groove, the resin layer is transferred to the reinforcing fibers, and the reinforcing fibers are impregnated with the resin.
7. The method for producing a tow prepreg according to claim 6, wherein a thickness of the resin layer formed in each of the grooves of the grooved roller is controlled independently for each groove.
Citation Information
Patent Citations
Production of tow prepreg and sheet like prepreg
JP1996300349A
Process and apparatus for preparing yarn prepreg
JP1997255799A
Yarn prepreg and its production
JP1998081770A
Method for producing narrow prepreg, and fiber-reinforced plastic
JP2012167252A
Method for manufacturing tow prepreg
JP2014148573A