Towpreg and method for manufacturing filament-wound product using towpreg
The use of a thermosetting resin composition with controlled particle components and properties in tow preg enhances expandability and winding tightness, addressing uneven thickness issues and improving the formability and productivity of filament winding processes.
Patent Information
- Application Number
- JP2020204686
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-30
- Filing Date
- 2020-12-10
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-12-10
AI Technical Summary
Existing tow preg impregnated with thermosetting resin compositions exhibit poor expandability and winding tightness, leading to uneven thickness and reduced pressure resistance due to yarn width fluctuations during filament winding, which affects the formability and mass productivity of molded products.
The tow preg is formulated with a thermosetting resin composition containing specific particle components like silica, kaolin, or mica with an angle of repose of 47° or less, and controlled viscosity and hardness to achieve a widening ratio of 0.8 to 1.0 and tightening speed of 9.0 to 12.5 mm/s, enhancing expandability and winding tightness.
This formulation improves filament winding moldability, resulting in higher mass productivity, quality, and cost competitiveness by ensuring uniform thickness and strength of the reinforcing fiber layer.
Smart Images

Figure 0007563150000002 
Figure 0007563150000003 
Figure 0007563150000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a towpreg having excellent filament winding (hereinafter sometimes referred to as "FW") moldability and handling properties, in which a reinforcing fiber bundle is previously impregnated with a thermosetting resin. In particular, the present invention relates to a towpreg having improved FW moldability, such as improved spreadability and tightening properties of the towpreg, when the towpreg impregnated with a thermosetting resin composition is unwound and wound around a liner while being impregnated with the resin. [Background technology]
[0002] Conventionally, the FW molding method has been widely used for pressure vessels, rolls, propeller shafts, flywheels, fishing rods, golf club shafts, aerospace applications, leisure applications, and general industrial applications, and has been recognized for its excellent moldability and high mechanical properties of the molded products. In particular, in recent years, attention has been focused on pressure vessel applications that are expected to be filled with fuel for natural gas vehicles and fuel cell vehicles. As such, the demand for pressure vessels is increasing year by year, and there is a strong demand for mass production and quality improvements by improving FW moldability compared to the past.
[0003] In many cases of FW molding, a process is provided in which a liquid thermosetting resin composition is supplied to the fiber bundle before it is wound around the liner to impregnate it. However, there are technical issues such as the deterioration of the working environment due to the handling of a liquid thermosetting resin composition in the manufacturing process, and the inability to increase the process speed of the FW molding process due to the impregnation process. Therefore, instead of supplying a liquid thermosetting resin composition in the FW process, a FW molding method using a towpreg in which a reinforcing fiber bundle is previously impregnated with a thermosetting resin composition has been attracting attention in recent years. The reason for this is thought to be that the use of a towpreg eliminates the need for a resin impregnation process in the process, and therefore has the advantage of being able to increase the FW process speed.
[0004] However, towpregs (Figure 1), in which reinforcing fiber bundles are impregnated with a thermosetting resin composition that uses a solid curing agent that has excellent resin curing properties and pot life, have poor spreadability when wound around a liner 101, and fluctuations in the yarn width cause uneven thickness of the reinforcing fiber layer, resulting in reduced pressure resistance. In addition, the winding pressure caused by tension causes the reinforcing fiber bundles in the inner layer to escape laterally, resulting in bobbin winding tightening 201 (Figure 2). These are some of the technical issues that remain with regard to FW moldability, and each company is actively studying ways to solve these issues.
[0005] For example, the following Patent Document 1 (JP Patent Publication No. 2015-98584) is known as a tow prepreg impregnated with a thermosetting resin with improved FW moldability. Patent Document 1 discloses a tow prepreg made of reinforcing fiber bundles impregnated with a matrix resin composition containing a particulate component made of a thermoplastic resin, the average maximum stress value of which is in the range of 5,000 to 55,000 Pa in the results of a tack test. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-98584 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the invention described in the above Patent Document 1 improves the spreadability when the towpreg is wound around a liner during FW molding, but the yarn width varies greatly, which is not satisfactory for practical use, and the invention makes no mention of a towpreg containing particulate components having an angle of repose of 47° or less according to the present invention.
[0008] Therefore, an object of the present invention is to provide a towpreg that has excellent FW formability (towpreg expandability and winding tightening ability) and bobbin handleability. [Means for solving the problem]
[0009] In order to solve the above problems, a towpreg impregnated with a liquid thermosetting resin composition has any one of the following configurations: The thermosetting resin composition (A) comprises At least one of silica, kaolin, mica, and talc is selected. It does not contain particle components (B) with an angle of repose of 47° or less. The towpreg width expansion ratio is 0.8 to 1, and the towpreg winding speed is 9.0 mm / s to 12.5 mm / s. The towpreg is characterized in that
[0011] The particulate component (B) contained in the thermosetting resin composition (A) used in the towpreg of the present invention preferably has a volume average particle size of 1 μm or more and 35 μm or less.
[0012] The particulate component (B) contained in the thermosetting resin composition (A) used in the towpreg of the present invention preferably has a Mohs hardness of 7 or less.
[0013] The complex viscosity of the thermosetting resin composition (A) (rheometer method: measurement frequency 10 Hz, measurement strain 10%, measurement temperature 25° C.) is preferably 0.01 Pa·s or more and 60 Pa·s or less.
[0014] The fiber bundles used in the towpreg of the present invention are preferably made of carbon fibers or glass fibers.
[0015] The prepreg laminate using the towpreg of the present invention preferably has a Rockwell hardness (R scale) of 115 or more and 130 or less, measured based on JIS Z 2245 (2016).
[0016] In addition, the method for producing a molded product using a towpreg of the present invention has the following configuration. That is, The method for producing a filament winding molded product comprises the steps of: (a) preparing a molded product intermediate by winding a towpreg impregnated with a thermosetting resin composition (A) around a liner to form a fiber-reinforced resin layer; (b) maintaining the molded product intermediate at a temperature of 5 to 35°C to cause the thermosetting resin composition (A) to flow; and (c) heating the molded product intermediate to thermally cure the thermosetting resin composition (A). Effect of the Invention
[0017] According to the present invention, by using a towpreg with improved towpreg spreadability and winding tightening properties, FW formability and bobbin handleability are improved, and a FW molded product with excellent mass productivity, quality, and cost competitiveness can be obtained. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a schematic diagram illustrating an example of a bobbin wound with a towpreg. [Diagram 2] FIG. 1 is a schematic diagram showing an example of a bobbin in which the towpreg is tightened and deformed due to tension when the towpreg is unwound from the bobbin during FW molding. [Diagram 3] FIG. 1 is a schematic diagram showing an example of a towpreg manufacturing process. [Figure 4] FIG. 2 is a schematic diagram of an evaluation device for evaluating towpreg spreadability. [Diagram 5] FIG. 2 is a schematic diagram of an evaluation device for evaluating towpreg winding tightening property. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an embodiment of the present invention will be described in detail.
[0020] The towpreg according to the present invention is a towpreg in which reinforcing fiber bundles are previously impregnated with the thermosetting resin composition (A).
[0021] <Thermosetting resin> The thermosetting resin used in the thermosetting resin composition (A) of the present invention is not particularly limited as long as it is liquid, and examples of the thermosetting resin include epoxy resins, unsaturated polyester resins, phenolic resins, urea resins, and melamine resins. In particular, from the viewpoint of high adhesive strength, epoxy resins having precursors such as compounds of phenols, amines, carboxylic acids, and intramolecular unsaturated carbon are preferred.
[0022] Examples of glycidyl ether type epoxy resins that use phenols as precursors include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, epoxy resins with a biphenyl skeleton, phenol novolac type epoxy resins, cresol novolac type epoxy resins, resorcinol type epoxy resins, epoxy resins with a naphthalene skeleton, trisphenylmethane type epoxy resins, phenol aralkyl type epoxy resins, dicyclopentadiene type epoxy resins, diphenylfluorene type epoxy resins, and various isomers, alkyl, and halogen-substituted derivatives of each of these. Compounds in which epoxy resins made of phenols are modified with urethane or isocyanate are also included in this type.
[0023] Examples of glycidylamine type epoxy resins using amines as precursors include tetraglycidyldiaminodiphenylmethane, glycidyl compounds of xylylenediamine, triglycidylaminophenol, and positional isomers of glycidylaniline, and alkyl or halogen-substituted products.
[0024] Examples of epoxy resins that have a carboxylic acid as a precursor include glycidyl compounds of phthalic acid, and various isomers of glycidyl compounds of hexahydrophthalic acid and dimer acid.
[0025] Examples of epoxy resins having an intramolecularly unsaturated carbon as a precursor include alicyclic epoxy resins.
[0026] The curing agent used in the thermosetting resin composition (A) of the present invention is not particularly limited as long as it cures the thermosetting resin. It may be a curing agent that undergoes an addition reaction such as amines and anhydrides, or a curing catalyst that induces addition polymerization such as cationic polymerization and anionic polymerization, and two or more types of curing agents may be used in combination. As the curing agent, a compound having an amino group, an acid anhydride group, or an azide group is preferably suitable. For example, phenolic compounds such as dicyandiamide, alicyclic amines, aliphatic amines, aromatic amines, aminobenzoic acid esters, various acid anhydrides, phenol novolac resins, cresol novolac resins, imidazole derivatives, and t-butylcatechol, as well as Lewis acid complexes such as boron trifluoride complexes and boron trichloride complexes, may be mentioned.
[0027] <Particle components with repose angle of 47° or less (B)> It is important that the thermosetting resin composition (A) of the present invention contains a particle component (B) having an angle of repose of 47° or less. If the angle of repose of the particle component (B) used in the present invention is greater than 47°, the towpreg is not sufficiently widened when wound around the liner during FW molding, resulting in large yarn width fluctuations, which is undesirable because of the risk of uneven thickness in the reinforcing fiber layer and reduced tank strength. If the lower limit of the angle of repose is less than 20°, the towpreg is tightened due to the tension when unwinding the towpreg from the bobbin during FW molding, which is undesirable because the bobbin is prone to losing its shape.
[0028] The angle of repose in the present invention is measured in accordance with JIS R9301-1-2 (2013) and means the maximum angle between the horizontal plane at which the surface layer of powder particles can remain stationary due to friction between the powder particles. The more cohesive the particle component, the larger the angle of repose, and the worse the towpreg spreadability when winding the liner. A specific method for measuring the angle of repose in the present invention is exemplified below.
[0029] First, the powder sample to be measured is adjusted to a temperature of 22°C ± 4°C, and then a fixed amount of the sample (usually 200g) is transferred to a glass beaker. Then, while being careful not to vibrate the main body of the device, the sample is fed at a constant speed of 20g to 60g per minute from a height of about 40mm above the upper edge of the stainless steel funnel around the circumference of the stainless steel funnel, and dropped onto a horizontal base prepared in advance. The base angle is calculated from the diameter and height of the cone-shaped deposit that is generated, and this base angle is taken as the angle of repose. The measuring device is composed of the following instruments. (1) Stainless steel funnel In the middle is a sieve with 1 mm openings sandwiched between two plates, and below that is a nozzle with an inner diameter of 6 mm. The funnel is screwed into the support. (2) Circuit Board A polished plate made of stainless steel or other rigid corrosion-resistant metal, at least 270 mm long and 200 mm wide. The surface of the plate is engraved with four radial lines that intersect at 45° to each other, and at the intersections are positioning pins to which the height block can be fixed. The plate is equipped with three leveling feet. (3) Funnel holder It is made of stainless steel and has a robust structure, and is designed so that the central axis of the funnel nozzle is vertically above the positioning pin. (4) Height block It is a 40 mm high metal cylinder with a polished surface and a hole in the bottom for inserting a positioning pin.
[0030] The particulate component (B) having an angle of repose of 47° or less used in the thermosetting resin composition (A) of the present invention is not particularly limited, but is preferably at least one selected from silica, kaolin, mica, and talc, and silica is particularly preferably used because it contains less metal impurities.
[0031] The silica used in the embodiment of the present invention is a raw material obtained by separating the quartz component from a mineral called begmatite, which is composed of quartz, feldspar, and mica, by flotation. Alternatively, silica powder synthesized by a direct method, a soot remelting method, a plasma method, a sol-gel method, an LPD method, or the like may also be used as the raw material.
[0032] The silica manufacturing method used in the present invention can be roughly divided into an electric melting method and a fire melting method. The electric melting method includes a method of melting in a crucible in a vacuum or inert gas atmosphere, a melting method using arc plasma, and a continuous melting tube drawing method in which quartz powder is melted and directly drawn into a tube. The fire melting method is a method in which quartz powder is dropped from the center of an oxyhydrogen burner to melt it, and includes a column type that produces silica without contact and a slab type that produces large silica using a mold.
[0033] In an embodiment of the present invention, in order to improve the adhesion between the particulate component (B) in the thermosetting resin composition (A) and the reinforcing fiber, the surface of the particulate component (B) may be treated with a silane coupling agent, etc. Also, silica that has been heat-treated to remove impurities and harden the silica may be used.
[0034] From the viewpoint of imparting excellent resin impregnation property and FW moldability, the particle component (B) used in the present invention preferably has a volume average particle size in the range of 1 μm to 35 μm, with the upper limit being more preferably 30 μm, and even more preferably 20 μm, and the lower limit being more preferably 2 μm, and even more preferably 3 μm.
[0035] Here, the "volume average particle size" of the particle component (B) means the average particle size weighted by the volume of each particle in a certain particle group, and specifically, 100 mg of a measurement sample is weighed out and dispersed in water, and then the volume average particle size is measured using a laser diffraction / scattering type particle size distribution measuring device (LA-30 manufactured by HORIBA). The shape of the particle component used in the present invention is preferably spherical, since crushed, fibrous, or plate-shaped particles cannot penetrate between the fibers of the reinforcing fiber bundles of the towpreg and do not sufficiently improve the FW moldability.
[0036] In order to reduce wear on the conveying roller during towpreg production and FW molding, the particle component (B) used in the present invention preferably has a Mohs hardness of 7 or less, more preferably a Mohs hardness of 5 or less, and even more preferably a Mohs hardness of 3 or less. The lower limit of the Mohs hardness of the particle component (B) used in the present invention is 1 or more, which is the measurable limit. Here, the Mohs hardness of the particle component (B) is a method in which standard minerals with hardnesses of 1 to 10 are set, the standard material and the measured material are rubbed, and the hardness is measured based on the presence or absence of scratches. In addition, as standard materials for Mohs hardness, talc is used for Mohs hardness 1, gypsum is used for Mohs hardness 2, calcite is used for Mohs hardness 3, fluorite is used for Mohs hardness 4, apatite is used for Mohs hardness 5, orthoclase is used for Mohs hardness 6, quartz is used for Mohs hardness 7, topaz is used for Mohs hardness 8, corundum is used for Mohs hardness 9, and diamond is used for Mohs hardness 10.
[0037] The complex viscosity of the thermosetting resin composition (A) used in the present invention is preferably in the range of 0.1 Pa·s or more and 60 Pa·s or less, from the viewpoint of imparting excellent resin impregnation ability, with the upper limit being more preferably 40 Pa·s and even more preferably 20 Pa·s, and the lower limit being preferably 0.5 Pa·s or more and even more preferably 1 Pa·s.
[0038] Here, the "complex viscosity" of the thermoplastic resin composition (A) means the viscosity measured using a DMA (ARES manufactured by TA Instruments) at 25°C, a frequency of 10 Hz, and a strain of 10%. If the upper limit of the complex viscosity of the thermosetting resin composition (A) is greater than 60 Pa s, unimpregnated parts will appear in the reinforcing fiber bundle, while if the lower limit is less than 0.1 Pa s, there will be a lot of scattering during resin impregnation, which will deteriorate the working environment, and this is not preferable.
[0039] The Rockwell hardness of the prepreg laminate using the towpreg of the present invention is correlated with the disturbance of the reinforcing fiber alignment during FW molding. If the Rockwell hardness is low, the alignment of the reinforcing fibers will be large, which will have a negative effect on the strength of the molded product. Therefore, the Rockwell hardness is preferably 115 or more, and the upper limit is more preferably 130. If the thickness of the prepreg laminate is less than 6 mm, the measured value of the Rockwell hardness will vary greatly, which is undesirable because the data will not be reliable. If the thickness of the prepreg laminate is 6 mm or more, the Rockwell hardness will be stable and the value will not change. The upper limit of the measurable thickness is 300 mm, but considering the thickness limit when creating the prepreg laminate, it is actually 10 mm. Here, the "Rockwell hardness" of the present invention is measured in accordance with JIS Z 2245 (2016), and the measurement conditions mean the Rockwell hardness at the R scale using a 1 / 2 inch steel ball (test load 60 kg) as the indenter.
[0040] The width expansion ratio of the towpreg of the present invention (towpreg yarn width in the head portion of the liner during helical winding / towpreg yarn width in the body portion of the liner) is preferably in the range of 0.8 to 1 inclusive, with the lower limit being more preferably 0.85, and even more preferably 0.90, in order to impart excellent FW formability.
[0041] The "widening ratio" of the towpreg of the present invention referred to here means that a single-filament towpreg is helically wound around a liner during FW molding, the yarn widths of the trunk and mirror parts are measured and recorded a total of seven times with a vernier caliper, and the ratio of each yarn width of the mirror part to the trunk part is calculated as the average value, as shown in Fig. 4. In particular, during helical winding, the towpreg yarn width tends to be narrower in the mirror part of the liner than in the trunk part, and a towpreg with a widening ratio of less than 0.8 is undesirable because it is prone to uneven thickness of the reinforcing fiber layer due to the generation of gaps, which may reduce the strength of the tank.
[0042] In addition, examples of the fibers constituting the reinforcing fiber bundles used in the towpreg of the present invention include glass fibers, carbon fibers, graphite fibers, aramid fibers, boron fibers, alumina fibers, and silicon carbide fibers. Various reinforcing fibers can be used alone or in combination of multiple types. Glass fibers and carbon fibers are preferably used due to the requirements for strength and rigidity. Although any type of reinforcing fiber can be used depending on the application, carbon fibers having a tensile strength of 3 to 30 GPa in a strand tensile test according to the method described in JIS R 7601 (1986) are preferably used because they can produce molded products with high strength.
[0043] The form of the reinforcing fibers is not particularly limited as long as they can be pulled out from the package, and cloth or roving is preferably used. In particular, for applications requiring high strength, it is particularly preferable to use roving in which the reinforcing fibers are aligned in a single direction.
[0044] <Towpreg manufacturing method of the present invention> A method for producing a towpreg according to the present invention will be described with reference to FIG. A reinforcing fiber bundle 302 is unwound from a reinforcing fiber bundle winding bobbin 301 installed on a creel stand 305 equipped with a tension control mechanism, and is guided to a resin attachment process 314 via an induction guide 303 and a dancer roll 304. Thereafter, a towpreg 321, which is resin-impregnated reinforcing fiber, is sent to a bobbin winding process 323, and a towpreg-wound bobbin 322 is obtained.
[0045] The tension control method of the creel stand 305 can be various types, such as a magnetic torque type using a permanent torque, a computer control type using a powder brake, or a servo control type using a servo motor, as long as the tension of the reinforcing fiber bundle 302 can be controlled by the creel stand.
[0046] It is preferable to provide a dancer roll 304 to absorb slack in the reinforcing fiber bundle 302 during the production of the towpreg. Furthermore, in order to improve the response accuracy of the tension control, it is preferable to feed back data acquired by the dancer roll 304 to the creel stand 305 via the control unit 330. There is no limit to the type of data acquired by the dancer roll 304, as long as the data is used for the tension control of the creel stand 305, such as dancer position information and tension information. The data sent to the control unit 330 may be acquired by the induction guide 303 or other sensors (not shown).
[0047] The illustrated guide is merely one example, and there are no limitations on the number of guides, the material of the guides, or the locations where the guides are installed, so long as the guides are intended to guide the unwound reinforcing fiber bundle 302 and towpreg 321 to the resin attachment process 314 or the bobbin winding process 323. The guides may be fixed, rotating, or a combination of both. The rotating type is preferable to avoid damage to the towpreg.
[0048] The resin attachment step 314 is a process for attaching resin 312 to the reinforcing fiber bundle 302. The illustrated resin attachment step 314 using an impregnation roller is merely one example, and various other resin attachment means can be applied as long as the purpose is to attach and impregnate a predetermined amount of resin to the reinforcing fiber bundle, such as a dip method in which the reinforcing fiber bundle is directly passed through the resin, or a fixed-quantity discharge method in which the reinforcing fiber bundle is drawn into an impregnation die and a separately measured amount of resin is discharged into the die.
[0049] In the impregnation roller type shown in the figure, the reinforcing fiber bundle 302 passes through an induction guide 303, then passes over an impregnation roller 310, and passes through another induction guide 303 to send the towpreg 321 to a bobbin winding process 323. A resin bath 313 containing the impregnation roller 310 is filled with resin 312, and the impregnation roller 310 is disposed so that the lower part thereof passes through the resin 312, so that the resin adheres to the surface of the impregnation roller 310. After the excess resin on the impregnation roller 310 is scraped off by a scraping member 311 to appropriately control the amount of resin on the roller, the reinforcing fiber bundle passes over the impregnation roller 310, so that an appropriate amount of resin 312 can be adhered to the reinforcing fiber bundle 302.
[0050] The bobbin winding process 323 is a process for winding the towpreg 321 around a bobbin to obtain a towpreg-wound bobbin 322. There are no limitations on the package shape of the towpreg-wound bobbin 322, but square end winding is preferred, which allows for a high winding density of the towpreg.
[0051] <Manufacturing method for filament winding molded products using towpregs> The method for producing a filament winding molded product of the present invention includes the steps of: (a) preparing a molded intermediate formed of a plurality of fiber-reinforced resin layers by winding a towpreg impregnated with a liquid thermosetting resin composition (A) around a liner; (b) holding the molded intermediate at room temperature to cause the thermosetting resin composition (A) to flow; and (c) heating the molded intermediate after step (b) to thermally cure the thermosetting resin composition (A). In the present invention, room temperature refers to a temperature in the range of 5°C to 35°C.
[0052] In the step (a) of preparing a molded intermediate, a reinforcing fiber bundle is drawn out, impregnated with a thermosetting resin composition (A), and then wound around a liner. The liner can be freely selected depending on the application of the FW molded product. For example, in the production of a hollow pipe member, a cylindrical liner that can be de-cored after the molded product is cured, or a liner of various shapes that can be de-cored by melting it by heating or the like can be used. In the production of a pressure vessel, a metal or resin liner that ensures sealing properties for a predetermined content can be used. As a method of winding a towpreg around a liner, from the viewpoint of moldability and mechanical properties of the molded product, it is preferable to supply the towpreg from a head portion that can be freely moved relative to the liner, and arrange the towpreg so as to satisfy the required performance of the FW molded product.
[0053] In the step (b) of holding the intermediate molded article at room temperature, the intermediate molded article is held at room temperature, so that the thermosetting resin composition (A) is kept in a state of having fluidity in at least a part of the step. In a state in which the thermosetting resin composition (A) is capable of flowing, the air bubbles that have entered the fiber-reinforced resin layer obtained in the step (a) are exposed to the surface layer of the fiber-reinforced resin layer due to the buoyancy acting on the air bubbles and the tightening caused by the tension remaining in the fiber when the fiber is wound around the winding core. Therefore, by holding the intermediate molded article at room temperature, at least a part of the air bubbles in the fiber-reinforced resin layer can be removed, and the voids remaining in the filament winding molded article can be reduced. The intermediate molded article can be held while rotating the liner of the intermediate molded article as the center of rotation. This prevents the thermosetting resin composition (A) having fluidity from dripping and falling off due to gravity. The falling off of the thermosetting resin composition (A) increases the fiber volume content (Vf:%) of the filament winding molded product, which may deteriorate the product performance. In addition, the fallen thermosetting resin composition (A) is often discarded, which deteriorates the product yield. By rotating the intermediate molded product while it is being held, the influence of the falling off of the thermosetting resin composition (A) can be eliminated.
[0054] In the retention of the intermediate molded article, the retention temperature is room temperature, but preferably within the range of room temperature, and can be any temperature ±5°C determined according to the type and use conditions of the thermosetting resin composition (A). When this range of any temperature ±5°C exceeds the range of room temperature, the excess is to be rounded down. Depending on the type and use conditions of the thermosetting resin composition (A), if the temperature is high, the gelation of the thermosetting resin composition (A) may proceed quickly, and sufficient resin flow time may not be ensured. In addition, if the temperature is low, the viscosity of the thermosetting resin composition (A) may decrease, and it may take a long time to achieve the same degree of void reduction effect compared to when the temperature is high. Therefore, the retention temperature is not particularly limited as long as it is room temperature, but it is preferable that it is in a range determined according to the type and use conditions of the thermosetting resin composition (A) used.
[0055] In the step (c) of thermally curing the thermosetting resin composition (A), the molded intermediate body after being kept at room temperature is heated to thermally cure the thermosetting resin composition (A), but the method is not limited, and heating can be performed using any method such as a heater or an induction heating coil. During heating, the molded intermediate body can be held while rotating. By rotating and holding the molded intermediate body, it is possible to prevent the thermosetting resin composition (A) from falling off.
[0056] The step (a) of preparing a molded intermediate, the step (b) of holding the molded intermediate at room temperature, and the step (c) of thermally curing the thermosetting resin composition (A) are not limited to a specific location. That is, the molded intermediate may be moved between steps (a) and (b), or the steps may be performed consecutively without moving. The molded intermediate may be moved between steps (b) and (c), or the steps may be performed consecutively without moving. Furthermore, when the molded intermediate is moved between steps (b) and (c), the location of the movement may be the location where step (a) was performed.
[0057] The filament winding molded product obtained by the present invention can be widely used for aerospace applications, leisure applications, and general industrial applications, including pressure vessels, rolls, propeller shafts, flywheels, fishing rods, and golf club shafts. In particular, it can be suitably used for pressure vessels and the like that require strength. The pressure vessels produced by the present invention are not limited to hydrogen gas vehicles and natural gas vehicles, but are also suitably used for ships and aircraft, stationary types that are fixed to the ground and used, and air respirators used by hospitals and firefighters. The substances stored in the pressure vessels may be gases such as nitrogen, oxygen, argon, liquefied petroleum gas, and hydrogen, or liquefied versions of the above substances. EXAMPLES
[0058] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the descriptions of these examples. Physical properties in each example and comparative example were evaluated according to the following methods.
[0059] [Complex viscosity (resin impregnation)] The viscosity of the thermosetting resin composition (uncured) obtained in each Example and Comparative Example was measured at 25°C, a frequency of 10 Hz, and a strain of 10% using a DMA (ARES manufactured by TA Instruments). The smaller this value, the better the resin impregnation into the reinforcing fiber bundle.
[0060] [Angle of repose (powder slipperiness)] The angle of repose of the particulate components and solid curing agents used in each Example and Comparative Example was measured in accordance with JIS R9301-1-2 (2013). The smaller this value, the better the powder slipperiness and the easier it is to improve the towpreg spreadability.
[0061] [Mohs hardness (hardness of particle component (B))] For the particulate components and solid hardeners used in each Example and Comparative Example, the Mohs hardness was measured based on the presence or absence of scratches caused by rubbing against the standard substance, using a standard substance with a Mohs hardness of 1 to 10. The smaller this value, the softer the material is, and the better the durability (aggression against the transport rollers) of the towpreg equipment and FW molding equipment is.
[0062] [Method for producing prepreg laminate using towpreg] The towpregs obtained in each of the Examples and Comparative Examples were arranged in one direction on a drum winder for a winding roll to form sheet-like prepregs, which were then laminated in an autoclave and heated at 150°C for 1 hour while being degassed under reduced pressure to obtain a unidirectional laminate with a fiber content Wf of 76%. [Rockwell hardness (hardness of prepreg laminate using towpreg)] The prepreg laminate obtained by the above method was measured for Rockwell hardness (R scale, indenter: 1 / 2 inch steel ball, test load: 60 kg) based on the JIS Z 2245 (2016) standard. Note that the larger this value, the smaller the alignment disorder of the reinforcing fiber bundles.
[0063] [Volume average particle size] For the particle components and solid curing agents used in each of the Examples and Comparative Examples, 100 mg of a measurement sample was weighed out and dispersed in water, and then the average particle size was measured using a laser diffraction / scattering type particle size distribution measuring device (LA-30 manufactured by HORIBA Corporation).
[0064] [Rc (resin content)] The resin content was calculated from the following formula (1). Weight of thermosetting resin composition attached in the towpreg (g) / Total weight of the towpreg (g) × 100 (wt%) (1)
[0065] [Resin application property (adhered to impregnated roller)] Using the towpreg manufacturing apparatus shown in FIG. 3, the thermosetting resin compositions of the examples and comparative examples were impregnated into the reinforcing fiber bundles. The resin adhesion states of the impregnation roller 310 and the scraping member 311 were visually inspected, and the resin applicability was evaluated according to the following criteria.
[0066] Good: No solid matter adheres to the impregnated roller, and resin feed is excellent. Possible: Some solid components adhere to the impregnated roller, occasionally causing clogging of the scraping member. Defective: Solid components adhere to the entire impregnated roller, causing clogging at the scraping member.
[0067] [Towpreg spreadability (spread ratio)] A bobbin with a length of 280 mm, an outer diameter of 82.5 mm, and an inner diameter of 76.5 mm was installed in the towpreg manufacturing apparatus shown in FIG. 3, and a towpreg (thread width 10±2 mm, thickness 0.08 mm, resin content 24%, 300 m winding) of the example and comparative example was prototyped. Next, as shown in FIG. 4, a cylindrical liner (made of aluminum) with an outer diameter of 146 mm and a total length of 250 mm was installed, and a helical layer (±45°) was wound around the liner with one combined thread (creel tension 30 N), and the towpreg thread width of the trunk and head parts after the second helical layer was measured with a vernier caliper (n=7). The towpreg width expansion ratio was calculated using the following formula (2), and the standard deviation and coefficient of variation (CV) were also calculated by calculating the average value. It can be said that the closer this average value is to 1.0, the better the towpreg width expansion property is, and the smaller the standard deviation and coefficient of variation are, the less the thread width variation is. Towpreg width ratio = Towpreg thread width in the head part of the helical layer / Towpreg thread width in the body part of the helical layer (2)
[0068] [Towpreg winding tightening property (initial winding tightening speed)] A bobbin having a length of 280 mm, an outer diameter of 82.5 mm, and an inner diameter of 76.5 mm was installed in the towpreg manufacturing apparatus shown in FIG. 3, and a towpreg (thread width 10±2 mm, thickness 0.08 mm, resin content 24%, 300 m winding) of the embodiment and the comparative example was prototyped. Next, the obtained towpreg was rewound with a tension of 7 N to make the winding tension constant, and then the displacement amount when the weight was hung down using the apparatus shown in FIG. 5 was recorded with a displacement meter (laser reading type) to create a displacement curve (displacement amount vs. elapsed time), and the average value of the initial winding tightening speed (mm / s) was calculated from the slope of the displacement curve (n=4). In addition, the standard deviation and the coefficient of variation (CV) were also calculated. It can be said that the smaller this average value, the more difficult it is for the towpreg to be wound, and the smaller the standard deviation and the coefficient of variation, the smaller the influence of individual differences in the bobbin.
[0069] [Raw materials] In the examples and comparative examples, the following raw materials were used. <Reference example 1> Thermosetting resin Bisphenol A type epoxy resin ("jER" (registered trademark) 828 (manufactured by Mitsubishi Chemical Corporation) <Reference Example 2> Solid hardener Dicyandiamide (DICY-1) (volume average particle size 3 μm, angle of repose 52°) Dicyandiamide (DICY-2) (volume average particle size 40 μm, angle of repose 44°) Dicyandiamide (DICY-3) (volume average particle size 15 μm, angle of repose 47°) <Reference Example 3> Particle components with repose angle of 47° or less (B) Fused silica (silica-1) (volume average particle size 3 μm, angle of repose 43°) Fused silica (silica-2) (volume average particle size 35 μm, angle of repose 30°) Synthetic mica (volume average particle size 3 μm, angle of repose 42°) Talc (volume average particle size 3μm, angle of repose 42°) Kaolin (volume average particle size 3 μm, angle of repose 43°) <Reference Example 4> Particle components (B´) with an angle of repose greater than 47° Heavy calcium carbonate (Ca carbonate) (volume average particle size 3 μm, angle of repose 50°) Alumina oxide (alumina) (volume average particle size 3 μm, angle of repose 50°) <Reference Example 5> Reinforced fiber bundle Carbon fiber (Toray Industries, Inc., "TORAYCA" (registered trademark) T700SC-24K)
[0070] [Table 1]
[0071] As described above, by comparing the Examples and Comparative Examples, it can be seen that the towpreg impregnated with the thermosetting resin composition (A) of the present invention can simultaneously achieve high levels of resin impregnation, resin coatability, and FW moldability (expandability, tightening ability) in a well-balanced manner. [Explanation of symbols]
[0072] 101 Liner 102 Bobbin 201 Bobbin winding tightening 301 Reinforced fiber bundle winding bobbin 302 Reinforced fiber bundle 303 Guidance Guide 304 Dancer Roll 305 Creel Stand 310 Impregnated roller 311 Scraping member 312 Resin 313 Resin Bath 314 Resin adhesion process 321 Towpreg 322 Towpreg Wrapped Bobbin 323 Winding process 330 Control Unit
Claims
1. A towpreg having a reinforcing fiber bundle previously impregnated with a thermosetting resin composition (A), wherein the thermosetting resin composition (A) contains a particulate component (B) selected from at least one of silica, kaolin, mica, and talc and having an angle of repose of 47° or less, the towpreg widening ratio being 0.8 or more and 1 or less, and the towpreg winding speed being 9.0 mm / s or more and 12.5 mm / s or less.
2. 2. The towpreg according to claim 1, wherein the particulate component (B) has a volume average particle diameter of 1 μm or more and 35 μm or less.
3. 3. The towpreg according to claim 1, wherein the particulate component (B) has a Mohs hardness of 7 or less.
4. The towpreg according to any one of claims 1 to 3, characterized in that the complex viscosity of the thermosetting resin composition (A) (rheometer method: measurement frequency 10 Hz, measurement strain 10%, measurement temperature 25°C) is 0.01 Pa s or more and 60 Pa s or less.
5. The towpreg according to any one of claims 1 to 4, wherein the reinforcing fiber bundles are made of carbon fibers or glass fibers.
6. A towpreg laminate using the towpreg according to any one of claims 1 to 5, characterized in that the Rockwell hardness (R scale) measured based on JIS Z 2245 (2016) is 115 or more and 130 or less.
7. A method for producing a filament winding molded product, comprising: a step (a) of preparing a molded product intermediate formed of a plurality of fiber reinforced resin layers by winding a towpreg impregnated with the thermosetting resin composition (A) according to any one of claims 1 to 6 around a liner; a step (b) of maintaining the molded product intermediate at a temperature of 5°C to 35°C to cause the thermosetting resin composition (A) to flow; and a step (c) of heating the molded product intermediate to thermally cure the thermosetting resin composition (A).
Citation Information
Patent Citations
Curable composition
JP2009518465A
Thermally conductive composition
JP2012082295A
Tow prepreg
JP2015098584A
Coil for rotary electric machines, prepreg mica tape, method for producing prepreg mica tape, cured product of prepreg mica tape, article with insulating layer, and method for producing coil for rotary electric machines
JP2018170252A
Fiber-reinforced molded article and method for producing same
WO2019151174A1