Resin composition, resin film and molded article

The resin composition combining alicyclic structure-containing polymers with thermoplastic polyurethane addresses issues of deformation and transparency, achieving enhanced tensile elongation and impact resistance.

JP7563172B2Active Publication Date: 2024-10-08MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020217805
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-25
Publication Date
2024-10-08
Estimated Expiration
2040-12-25

AI Technical Summary

Technical Problem

Existing resin compositions containing alicyclic structure-containing polymers suffer from poor deformation resistance, bending resistance, and transparency when blended with soft polymers, necessitating further improvements.

Method used

A resin composition comprising an alicyclic structure-containing polymer blended with thermoplastic polyurethane, specifically carbonate, lactone, or ester thermoplastic polyurethane, in a ratio of 95:5 to 50:50, with a glass transition temperature of 30°C or lower, enhancing tensile elongation, impact resistance, and transparency.

Benefits of technology

The composition achieves excellent tensile elongation, impact resistance, deformation resistance, and transparency, maintaining optical properties and durability under various conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563172000001
    Figure 0007563172000001
  • Figure 0007563172000002
    Figure 0007563172000002
Patent Text Reader

Abstract

To provide a resin composition having excellent tensile elongation, impact resistance, deformation resistance and transparency, and provide a resin film and a molding.SOLUTION: A resin composition contains an alicyclic structure-containing polymer, and at least one thermoplastic polyurethane selected from the group consisting of a carbonate thermoplastic polyurethane, a lactone thermoplastic polyurethane and an ester thermoplastic polyurethane.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a resin film, and a molded article. [Background technology]

[0002] Alicyclic structure-containing polymers are often amorphous resins due to their bulky structure, and are excellent in transparency, optical properties, and heat resistance, and therefore are used in various applications such as replacement for glass windows, optical films, automobile headlamp covers, etc. Among them, carbonate-based polymers containing alicyclic dihydroxy compounds are excellent in weather resistance and are therefore used in applications requiring long-term outdoor use, such as automobile parts and building materials such as carports, but may have poor impact resistance.

[0003] Patent Document 1 proposes a resin composition comprising a specific alicyclic structure-containing polymer blended with a flexible polymer as a resin composition having low dielectric properties, excellent heat resistance, and excellent crack resistance in specified reliability tests and against solvents. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-098130 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the technology described in Patent Document 1, the addition of a soft polymer may result in poor resistance to deformation due to stretching, bending, and the like, or poor transparency, and further improvements were necessary.

[0006] Therefore, an object of the present invention is to provide a resin composition, a resin film, and a molded article that are excellent in tensile elongation, impact resistance, deformation resistance, and transparency. [Means for solving the problem]

[0007] In view of the above circumstances, the present inventors have conducted intensive research and have found that the above-mentioned problems can be solved, thereby completing the present invention. [1] A resin composition comprising an alicyclic structure-containing polymer and at least one thermoplastic polyurethane selected from the group consisting of carbonate-based thermoplastic polyurethanes, lactone-based thermoplastic polyurethanes, and ester-based thermoplastic polyurethanes. [2] The resin composition according to [1], wherein the mass ratio of the alicyclic structure-containing polymer to the thermoplastic polyurethane is alicyclic structure-containing polymer:thermoplastic polyurethane=95:5 to 50:50. [3] The resin composition according to [1] or [2], wherein the thermoplastic polyurethane has a glass transition temperature of 30°C or lower. [4] The resin composition according to any one of [1] to [3], wherein the alicyclic structure-containing polymer is a polycarbonate-based polymer. [5] The resin composition according to any one of [1] to [4], wherein the alicyclic structure-containing polymer is a copolymer of a cyclic ether (a) and an alicyclic dihydroxy compound (b). [6] The resin composition according to [5], wherein the cyclic ether (a) is isosorbide. [7] The resin composition according to [5] or [6], wherein the alicyclic dihydroxy compound (b) is cyclohexanedimethanol or tricyclodecanedimethanol. [8] A resin film or molded article comprising the resin composition according to any one of [1] to [7], and having a tensile elongation at 23° C. of 100% or more. [9] A resin film or molded article comprising the resin composition according to any one of [1] to [7], the resin film or molded article having a light transmittance of 85% or more at a thickness of 100 μm and a haze of 10% or less.

[10] A resin film or molded article comprising the resin composition according to any one of [1] to [7], which does not whiten even when cut into a 5 cm square and folded perpendicularly to both the MD and TD directions.

[11] A resin film or molded article comprising the resin composition according to any one of [1] to [7], the resin film or molded article having a breaking point displacement of 9.0 mm or more in a Hydroshot high-speed impact test at -20°C.

[12] A resin film or molded article comprising the resin composition according to any one of [1] to [7], the resin film or molded article having a breaking point displacement of 15.0 mm or more in a Hydroshot high-speed impact test at 23°C.

[13] A resin film or molded article comprising the resin composition according to any one of [1] to [7], which has a YI value of less than 10.0 after 200 hours of exposure to an accelerated weather resistance test under the following conditions: Accelerated weathering test conditions: Black panel temperature 63°C, humidity 50% (relative humidity), illuminance 255W / m 2 , Continuous irradiation, Water spray time 12 minutes / 60 minutes irradiation Effect of the Invention

[0008] According to the present invention, it is possible to provide a resin composition, a film, and a molded article which are excellent in tensile elongation, impact resistance, deformation resistance, and transparency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described in detail. However, the content of the present invention is not limited to the embodiment described below.

[0010] <Resin composition> The resin composition of the present invention contains an alicyclic structure-containing polymer and at least one thermoplastic polyurethane selected from the group consisting of carbonate-based thermoplastic polyurethanes, lactone-based thermoplastic polyurethanes, and ester-based thermoplastic polyurethanes.

[0011] [Alicyclic structure-containing polymer] The alicyclic structure-containing polymer of the present invention is a polymer having an alicyclic structure in the repeating unit of the polymer. In the present invention, both a polymer having an alicyclic structure in the main chain and a polymer having an alicyclic structure in the side chain can be used. In addition, as the polymer having an alicyclic structure in the repeating unit, a crystalline polymer or an amorphous polymer can be obtained depending on the structure of the repeating unit, and in the present invention, an amorphous resin having excellent transparency is preferable.

[0012] Examples of the alicyclic structure include a cycloalkane structure and a cycloalkene structure, and the cycloalkane structure is preferred from the viewpoint of thermal stability, etc. The number of carbon atoms constituting the alicyclic structure is not particularly limited, but is usually 4 to 30, preferably 5 to 20, and more preferably 6 to 15. The type of the polymer is not particularly limited as long as it has an alicyclic structure in the repeating unit of the polymer. For example, polycarbonate-based polymers having carbonate bonds in the main chain, polyester-based polymers having ester bonds in the main chain, addition-based polymers, etc. are listed, and polycarbonate-based polymers are preferred.

[0013] Specific examples of the alicyclic structure-containing polymer include (1) copolymers of cyclic ethers and alicyclic dihydroxy compounds, (2) norbornene polymers, (3) monocyclic olefin polymers, (4) cyclic conjugated diene polymers, (5) vinyl alicyclic hydrocarbon polymers, and hydrogenated products thereof. Among these, from the viewpoints of transparency and moldability, (1) copolymers of cyclic ethers and alicyclic dihydroxy compounds are more preferred.

[0014] In the copolymer of a cyclic ether (a) and an alicyclic dihydroxy compound (b), examples of the cyclic ether (a) include isosorbide, isomannide, and isoidet. Here, isosorbide can be produced inexpensively by hydrogenating and then dehydrating D-glucose obtained from starch, and is an abundantly available resource. Examples of the alicyclic dihydroxy compound (b) include alicyclic dihydroxy compounds described in International Publication No. 2007 / 148604. In the present invention, compounds containing a 5-membered ring structure or a 6-membered ring structure are preferred in terms of heat resistance and optical properties. The 6-membered ring structure may be fixed in a chair or boat shape by a covalent bond. Among these, preferred examples include cyclohexane dimethanol, tricyclodecane dimethanol, adamantane diol, and pentacyclopentadecane dimethanol. Among these, cyclohexane dimethanol or tricyclodecane dimethanol is more preferred in terms of economy and heat resistance.

[0015] As the copolymer of the cyclic ethers (a) and the alicyclic dihydroxy compound (b), commercially available products can be used, specifically, polycarbonate manufactured by Mitsubishi Chemical Corporation, under the trade name "DURABIO (registered trademark)".

[0016] The molar ratio of the cyclic ether (a) to the alicyclic dihydroxy compound (b) in the alicyclic structure polymer of the present invention is preferably (a):(b)=95:5 to 30:70, more preferably 80:20 to 40:60. By setting the molar ratio within the above range, coloration due to heat retention is unlikely to occur, the glass transition temperature can be maintained, and heat resistance is improved.

[0017] (glass transition temperature) The glass transition temperature of the alicyclic structure-containing polymer of the present invention is preferably 80° C. or higher and 200° C. or lower, more preferably 90° C. or higher and 180° C. or lower. By setting the glass transition temperature at 80° C. or higher, the polymer has excellent durability against deformation and stress during use at high temperatures, which is preferable. On the other hand, by setting the glass transition temperature at 200° C. or lower, moldability can be ensured. The glass transition temperature of the alicyclic structure-containing polymer can be measured by differential scanning calorimetry (DSC).

[0018] (Melt Flow Rate (MFR)) The melt flow rate (MFR) of the alicyclic structure-containing material of the present invention at 230° C. is preferably 0.1 g / 10 min or more. By having an MFR of 0.1 g / 10 min or more, the melt viscosity of the resin composition during molding is unlikely to become high, and productivity is excellent. In addition, from the viewpoint of film formability, the MFR of the alicyclic structure-containing material in the present invention is preferably 100 g / 10 min or less. From this viewpoint, the MFR at 230° C. of the alicyclic structure-containing material in the present invention is more preferably 0.5 to 80 g / 10 min, and further preferably 0.6 to 70 g / 10 min. The MFR is based on JIS K7210-1999 and is a value measured under conditions of a temperature of 230°C and a load of 2.16 kg.

[0019] The alicyclic structure-containing polymer of the present invention can be produced by a known method, or a commercially available product may be used.

[0020] [Thermoplastic polyurethane] The resin composition of the present invention contains at least one thermoplastic polyurethane selected from the group consisting of carbonate-based thermoplastic polyurethanes, lactone-based thermoplastic polyurethanes, and ester-based thermoplastic polyurethanes. The resin composition of the present invention preferably contains the above thermoplastic polyurethane as a main component as the thermoplastic polyurethane. The content of the above thermoplastic polyurethane is preferably 60 mass% or more, more preferably 80 mass% or more, and even more preferably 100 mass% of the total amount of thermoplastic polyurethane. That is, the resin composition of the present invention preferably contains only the above thermoplastic polyurethane as the thermoplastic polyurethane. Polyurethane is a general term for compounds that have a urethane bond (-NHCOO-) and are obtained by the polyaddition reaction (urethanization reaction) of isocyanate (-NCO) and alcohol (-OH). The thermoplastic polyurethane (TPU) of the present invention is a resin having a urethane bond in the main chain of a polymer molecule having repeating units derived from a diisocyanate component, repeating units derived from a polyol component, and, as necessary, repeating units derived from a chain extender.

[0021] The diisocyanate component in the thermoplastic polyurethane of the present invention may be an aromatic diisocyanate component or an aliphatic diisocyanate component. Examples of the aromatic diisocyanate component include tolylene diisocyanate, 4,4-diphenylmethane diisocyanate, xylylene diisocyanate, naphthylene diisocyanate, and paraphenylene diisocyanate, while examples of the aliphatic diisocyanate component include hexamethylene diisocyanate, hydrogenated 4,4-diphenylmethane diisocyanate, 1,4-bis(isocyanatomethyl)cyclohexane, hydrogenated xylylene diisocyanate, lysine diisocyanate, and isophorone diisocyanate. The diisocyanate component in the thermoplastic polyurethane of the present invention is not particularly limited, but from the viewpoint of the weather resistance of the resin composition, an aliphatic diisocyanate component is preferred, and an alicyclic diisocyanate such as hydrogenated 4,4-diphenylmethane diisocyanate, 1,4-bis(isocyanatomethyl)cyclohexane, hydrogenated xylylene diisocyanate, or isophorone diisocyanate is more preferred.

[0022] The polyol component in the thermoplastic polyurethane of the present invention is a polycarbonate-based polyol in the case of a carbonate-based thermoplastic polyurethane, a polylactone-based polyol in the case of a lactone-based thermoplastic polyurethane, and a polyester-based polyol in the case of an ester-based thermoplastic polyurethane.

[0023] Examples of the polycarbonate-based polyol include polyols obtained by dealcoholization reaction between low molecular weight polyols such as ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, octanediol, nonanediol, 1,4-cyclohexanedimethanol, and neopentyl glycol and carbonate compounds such as diethylene carbonate, dipropylene carbonate, and diphenyl carbonate.

[0024] Examples of the polylactone polyol include polycaprolactone diol, polymethylvalerolactone diol, and other polylactone diols obtained by ring-opening polymerization of lactone using, as an initiator, the low molecular weight polyols exemplified above for the polycarbonate polyols.

[0025] Examples of the polyester-based polyol include condensation polymers of low-molecular-weight polyols exemplified above as the polycarbonate-based polyols and polyvalent carboxylic acids. Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids such as malonic acid, maleic acid, fumaric acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid; and aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, 2,6-naphthalenedicarboxylic acid, paraphenylenedicarboxylic acid, and trimellitic acid.

[0026] The chain extender is not particularly limited, but examples thereof include aliphatic glycols, aromatic glycols, low molecular weight diols such as 1,4-butanediol and 1,6-hexanediol, and bis(hydroxyethyl)hydroquinone.

[0027] (hardness) The hardness (Shore A) of the thermoplastic polyurethane in the present invention is not particularly limited, but is preferably 80A or more and 98A or less, more preferably 85A or more, and even more preferably 87A or more, from the viewpoint of general-purpose availability. By making the hardness 80A or more, blocking during raw material supply is unlikely to occur, and productivity is improved. In addition, by making the hardness 98A or less, flexibility and impact resistance are improved. The hardness of the thermoplastic polyurethane can be measured by a method based on JIS K7311-1995 (Shore A).

[0028] (Glass transition temperature and melting point) The glass transition temperature (Tg) of the thermoplastic polyurethane in the present invention is preferably 30° C. or lower. The thermoplastic polyurethane of the present invention has a Tg of 30° C. or less, which can impart flexibility and impact resistance. The thermoplastic polyurethane of the present invention has a Tg of more preferably 25° C. or less, and even more preferably 20° C. or less. The lower limit of the Tg of the thermoplastic polyurethane is not particularly limited, but from the viewpoint of easy availability as a general-purpose product, it is preferably −100° C. or higher. Furthermore, the thermoplastic polyurethane in the present invention does not necessarily have a melting point (Tm), but if it does have a melting point (Tm), it is preferably 60 to 200°C. When the Tm of the thermoplastic polyurethane of the present invention is 60° C. or higher, the heat resistance is good, and when it is 200° C. or lower, the film formability is good. The Tm of the thermoplastic polyurethane of the present invention is more preferably 70 to 195° C., and further preferably 75 to 190° C. The Tg and Tm of a thermoplastic polyurethane can be measured by differential scanning calorimetry (DSC).

[0029] (Melt Flow Rate (MFR)) The thermoplastic polyurethane of the present invention preferably has a melt flow rate (MFR) at 220° C. of 0.1 g / 10 min or more. When the MFR is 0.1 g / 10 min or more, the melt viscosity of the resin composition during molding is unlikely to become high, and productivity is excellent. From the viewpoint of film formability, the MFR of the polyurethane in the present invention is preferably 100 g / 10 min or less. From this viewpoint, the MFR at 220° C. of the thermoplastic polyurethane of the present invention is more preferably from 0.5 to 80 g / 10 min, and further preferably from 0.6 to 70 g / 10 min. The MFR is based on JIS K7210-1999 and is a value measured under conditions of a temperature of 220°C and a load of 2.16 kg.

[0030] The thermoplastic polyurethane of the present invention can be produced by a known method, or a commercially available product may be used.

[0031] [Content of each ingredient] The content mass ratio of the alicyclic structure-containing polymer to the thermoplastic polyurethane in the resin composition of the present invention is preferably alicyclic structure-containing polymer:thermoplastic polyurethane=95:5 to 50:50, more preferably 90:10 to 60:40. By containing 5% by mass or more of thermoplastic polyurethane, flexibility and impact resistance can be imparted, and by containing 50% by mass or less, heat resistance and weather resistance can be maintained, and whitening during deformation is less likely to occur.

[0032] [Optional ingredients] The resin composition of the present invention may contain additives as optional components. Examples of additives include lubricants, colorants, flame retardants, antioxidants, UV absorbers, light stabilizers, conductive materials, antibacterial agents, etc. The additives may be used in amounts that are normally used.

[0033] <Resin films and molded articles> The resin film and molded article using the resin composition of the present invention can be produced by known methods. Examples of methods for producing resin films include an extrusion molding method in which an alicyclic structure-containing polymer, a thermoplastic polyurethane, and, if necessary, additives are melt-kneaded in a single-screw or twin-screw extruder, extruded into a film shape from a T-die, and cooled and solidified by a casting roll to obtain a non-oriented film. Examples of methods for producing molded articles include, for example, an injection molding method in which the resin is melt-kneaded in the same manner as in the case of the resin film, the resin is filled into a mold of a predetermined shape, and the mold is cooled and solidified to obtain a molded article.

[0034] (Thickness) The thickness of the resin film and molded article using the resin composition of the present invention is not particularly limited, but is preferably from 0.03 mm to 10 mm, for example, in consideration of processability and practicality.

[0035] (shock resistance) From the viewpoint of impact resistance, the resin film and molded article using the resin composition of the present invention preferably have a breaking point displacement of 9.0 mm or more, more preferably 10.0 mm or more, in a Hydroshot high-speed impact test at −20° C. The upper limit is not particularly limited, but is usually 20.0 mm or less. The displacement at break in the test at 23° C. is preferably 15.0 mm or more, more preferably 10 mm or more. There is no particular upper limit, but it is usually 30.0 mm or less. The fracture energy in this test is preferably 0.4 J or more at both -20°C and 23°C. The Hydroshot high-velocity impact test can be performed according to a method in accordance with ASTM D3763.

[0036] (Tensile elongation) From the viewpoint of flexibility, the resin film and molded article using the resin composition of the present invention preferably have a tensile elongation of 100% or more, more preferably 120% or more at 23° C. The upper limit is not particularly limited, but is usually 500% or less. The tensile elongation can be measured using a tensile tester according to a method in accordance with JIS K7161-1-2014.

[0037] (Deformation resistance) It is preferable that the resin film and molded article using the resin composition of the present invention have practical transparency such that they do not turn white when deformed by stretching, bending, or the like. More specifically, for example, it is preferable that the resin film or molded product does not whiten even when cut into a 5 cm square and folded in directions perpendicular to both the MD and TD.

[0038] (Light transmittance and haze) From the viewpoint of transparency, a resin film and a molded article using the resin composition of the present invention preferably have a light transmittance (total light transmittance) at a thickness of 100 μm of 85% or more, and more preferably 87% or more. Furthermore, the haze (internal haze) at a thickness of 100 μm is preferably 10% or less, more preferably 8% or less, and even more preferably 5% or less. The light transmittance can be measured by a method conforming to JIS K 7361-1-2008, and the haze can be measured by a method conforming to JIS K 7136-2000.

[0039] (YI value) From the viewpoints of weather resistance and transparency, the resin film and molded article using the resin composition of the present invention preferably have a YI value at a thickness of 100 μm of less than 5.0, more preferably less than 4.0, and even more preferably less than 3.0. Furthermore, the YI value after exposure for 200 hours to an accelerated weather resistance test under the following conditions is preferably less than 10.0, more preferably less than 8.0, and even more preferably less than 6.0. Accelerated weathering test conditions Black panel temperature 63℃, humidity 50% (relative humidity), illuminance 255W / m 2 , Continuous irradiation, Water spray time 12 minutes / 60 minutes irradiation The above-mentioned "water spray time 12 minutes / irradiation time 60 minutes" means that, when irradiation time is 60 minutes, one cycle is water sprayed for 12 minutes and no water spray is performed for 48 minutes. The YI value can be measured by a method in accordance with JIS K7373-2006. EXAMPLES

[0040] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited by these in any way.

[0041] <Raw materials> The raw materials used in the examples and comparative examples are listed below.

[0042] [Alicyclic structure-containing polymer] A-1: Polycarbonate resin with a molar ratio of cyclic ethers (structural units derived from isosorbide):alicyclic hydroxy compounds (structural units derived from 1,4-cyclohexanedimethanol) = 70:30, MFR (230℃) = 10.0g / 10min, glass transition temperature 120℃ A-2: Polycarbonate resin with a molar ratio of cyclic ethers (structural units derived from isosorbide):alicyclic hydroxy compounds (structural units derived from 1,4-cyclohexanedimethanol) = 50:50, MFR (230℃) = 5.0g / 10min, glass transition temperature 100℃

[0043] [Aromatic polycarbonate resin] A-101: "Iupilon H3000" (manufactured by Mitsubishi Engineering Plastics Corporation, polycarbonate resin with a structure derived from bisphenol A, MFR (230℃) = 3.6g / 10min, glass transition temperature 140℃)

[0044] [Thermoplastic polyurethane] B-1: Carbonate-based thermoplastic polyurethane containing an aliphatic diisocyanate component (1,4-bis(isocyanatomethyl)cyclohexane 30.2 wt%), MFR (220℃) = 2.7g / 10min, hardness 95A, melting point 182℃, glass transition temperature -3℃ B-2: Carbonate-based thermoplastic polyurethane containing an aliphatic diisocyanate component (hydrogenated 4,4-diphenylmethane diisocyanate 34.9 wt%), MFR (220℃) = 12g / 10min, hardness 95A, melting point 131℃, glass transition temperature -9.8℃ B-3: Caprolactone-based thermoplastic polyurethane containing an aliphatic diisocyanate component (hydrogenated 4,4-diphenylmethane diisocyanate 42.1 wt%), MFR (220℃) = 4.5g / 10min, hardness 90A, glass transition temperature -1.8℃ B-4: Ester-based thermoplastic polyurethane containing an aliphatic diisocyanate component (hydrogenated 4,4-diphenylmethane diisocyanate 41.6 wt%), MFR (220℃) = 1.0g / 10min, hardness 90A, melting point 93℃, glass transition temperature -6℃ B-101: Ether-based thermoplastic polyurethane containing an aliphatic diisocyanate component (1,4-bis(isocyanatomethyl)cyclohexane 24.7 wt%), MFR (220℃) = 3.0g / 10min, hardness 95A, glass transition temperature -12.8℃

[0045] The physical properties of the alicyclic structure-containing polymer, aromatic polycarbonate resin, and thermoplastic polyurethane were measured by the following methods.

[0046] (Thermoplastic polyurethane composition) The components of the thermoplastic polyurethane were qualitatively analyzed by H-NMR analysis using a nuclear magnetic resonance apparatus (manufactured by BRUKER, product name "Ultrashield", 400 MHz). Then, CHN analysis was performed using an elemental analyzer (manufactured by Elemental, product name "Vario EL cube") to calculate the weight ratio of the diisocyanate component.

[0047] (Hardness of Thermoplastic Polyurethane) The hardness (A hardness) of the thermoplastic polyurethane was measured according to JIS K 7311-1995 (Testing method for polyurethane-based thermoplastic elastomers).

[0048] (MFR) In accordance with JIS K7210-1999 (Method of testing melt mass-flow rate (MFR) and melt volume-flow rate (MVR) of plastics-thermoplastics), the MFR of each raw material was measured under conditions of a temperature of 220°C or 230°C and a load of 2.16 kg.

[0049] (Glass transition temperature and melting point) Using a differential scanning calorimeter (manufactured by PerkinElmer, product name "DSC8000"), the temperature of each raw material was raised at 10°C / min to measure Tg and Tm.

[0050] <Examples 1 to 8 and Comparative Examples 1 to 4> Each raw material was melt-kneaded to prepare a resin composition having the composition shown in Tables 1 and 2, and the resin composition was melt-extruded to produce a resin film having a thickness of 100 μm.

[0051] 〔evaluation〕 The resin films of Examples 1 to 8 and Comparative Examples 1 to 4 were evaluated for impact resistance, tensile elongation, deformation resistance, transparency and color difference.

[0052] (Impact resistance: Hydroshot high-speed impact test) The resin film was measured for displacement and energy at the breaking point using a method based on ASTM D3763 under conditions of a speed of 3 m / sec, height of 200 mm, striker φ12.7 mm, and test atmosphere temperatures of -20°C and 23°C, and evaluated according to the following criteria. Test atmosphere temperature: -20℃ A (good): The breaking point energy is 0.4 J or more, and the breaking point displacement is 9.0 mm or more. B (poor): The breaking point energy is less than 0.4 J or the breaking point displacement is less than 9.0 mm. Test atmosphere temperature: 23℃ A (good): The breaking point energy is 0.4 J or more, and the breaking point displacement is 15.0 mm or more. B (poor): The breaking point energy is less than 0.4 J or the breaking point displacement is less than 15.0 mm.

[0053] (Tensile elongation) The resin film was cut into a strip (test piece: width 10 mm, initial length 40 mm), and a tensile test was performed in the MD direction (machine direction) and TD direction (direction perpendicular to the machine direction (including a range approximately perpendicular to the machine direction); transverse direction) at a tensile speed of 200 mm / min in an atmosphere of 23°C using a tensile tester (Shimadzu Corporation, precision universal testing machine AG-XPlus). The breaking elongation was measured and evaluated according to the following criteria. A (good): The tensile elongation at break in both the MD and TD directions is 100% or more. B (poor): The tensile elongation at break in the MD or TD direction is less than 100%.

[0054] (Deformation resistance) The resin film was cut into a 5 cm square and completely folded in a direction perpendicular to both the MD and TD directions, and the appearance change of the fold was visually evaluated. Here, the evaluation result MD indicates the case where the material is folded perpendicular to the MD direction, and the fold is assumed to be horizontal to the MD direction. A (good): The crease does not turn white. B(poor): The crease is whitened

[0055] (transparency) The resin film surface was irradiated with light using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH 5000"), and the light transmittance and haze were measured in accordance with JIS K-7136-2008 and evaluated according to the following criteria. A (good): Light transmittance is 85% or more and internal haze is less than 10%. B(poor): Light transmittance is less than 85% or internal haze is 10% or more

[0056] (color difference) The resin film was subjected to an accelerated weathering test using a weathering tester (manufactured by Suga Test Instruments Co., Ltd., product name "Sunshine Weather Meter") at a BPT (black panel temperature) of 63°C, humidity of 50% RH, and illuminance of 255 W / m 2 The samples were exposed to accelerated weathering tests for 200 hours under the conditions of continuous irradiation and water spray time of 12 minutes / 60 minutes. The yellowing index (YI value) was measured before and after the accelerated weathering tests and evaluated according to the following criteria. A (good): YI value before the test is less than 5.0 and YI value after the test is less than 10.0 B (poor): YI value before the test is 5.0 or more, or YI value after the test is 10.0 or more.

[0057] [Table 1]

[0058] [Table 2]

[0059] The resin films described in Examples 1 to 8 were excellent in impact resistance and tensile elongation at low temperature and room temperature. They were also excellent in transparency and weather resistance, and did not whiten when folded, maintaining their appearance. On the other hand, Comparative Examples 1 and 2 did not contain the thermoplastic polyurethane according to the present invention, and therefore were inferior in impact resistance and tensile elongation. Comparative Example 3 did not contain the alicyclic structure-containing polymer according to the present invention, and therefore were inferior in tensile elongation and transparency. Comparative Example 4 contained an ether-type thermoplastic polyurethane as the thermoplastic polyurethane, and therefore the film whitened when folded, resulting in poor appearance.

[0060] The resin film of the present invention can be suitably used for, but is not particularly limited to, optical films, automobile parts such as automobile headlamp covers, building materials such as replacements for glass windows and carports, home appliance materials, office automation equipment materials, card materials, films for various moldings (vacuum, compressed air, TOM, heat press), and the like.

Claims

1. The thermoplastic polyurethane composition comprises an alicyclic structure-containing polymer and at least one thermoplastic polyurethane selected from the group consisting of a carbonate-based thermoplastic polyurethane, a lactone-based thermoplastic polyurethane, and an ester-based thermoplastic polyurethane, a mass ratio of the alicyclic structure-containing polymer to the thermoplastic polyurethane (alicyclic structure-containing polymer:thermoplastic polyurethane) is 95:5 to 50:50; the alicyclic structure-containing polymer is a polycarbonate-based polymer, the polycarbonate-based polymer is a copolymer of a cyclic ether (a) and an alicyclic dihydroxy compound (b); The cyclic ether (a) is isosorbide, The resin composition, wherein the alicyclic dihydroxy compound (b) is cyclohexanedimethanol or tricyclodecanedimethanol.

2. The resin composition according to claim 1, wherein the thermoplastic polyurethane has a glass transition temperature of 30°C or lower.

3. A resin film or molded article comprising the resin composition according to claim 1 or 2, and having a tensile elongation at 23° C. of 100% or more.

4. 3. A resin film or molded article comprising the resin composition according to claim 1 or 2, the resin film or molded article having a light transmittance of 85% or more at a thickness of 100 μm and a haze of 10% or less.

5. 3. A resin film or molded article comprising the resin composition according to claim 1 or 2, which does not whiten even when cut into a 5 cm square and folded perpendicularly to both the MD and TD directions.

6. A resin film or molded article comprising the resin composition according to claim 1 or 2, the resin film or molded article having a breaking point displacement of 9.0 mm or more in a Hydroshot high-speed impact test at -20°C.

7. 3. A resin film or molded article comprising the resin composition according to claim 1 or 2, the resin film or molded article having a breaking point displacement of 15.0 mm or more in a Hydroshot high-speed impact test at 23°C.

8. 3. A resin film or molded article comprising the resin composition according to claim 1 or 2, which has a YI value of less than 10.0 after being exposed for 200 hours to an accelerated weather resistance test under the following conditions. Accelerated weather resistance test conditions: Black panel temperature 63°C, humidity 50% (relative humidity), illuminance 255W / m 2 , Continuous irradiation, Water spray time 12 minutes / 60 minutes irradiation

Citation Information

Patent Citations

  • Three-component thermoplastic mixture

    JP1991070770A

  • Polymer blend composition

    JP1992213351A

  • Resin composition formulated with non-rigid polymer

    JP2001098130A

  • Thermoplastic resin composition and molded article thereof

    JP2009197092A

  • Polycarbonate resin composition

    JP2016121275A