Method and apparatus for manufacturing plastic elements

The method uses thermal expansion molds to enhance transfer accuracy of plastic elements by compressing thermosetting resins during curing, addressing the shrinkage issue with a simple setup and improving shape accuracy.

JP7563265B2Active Publication Date: 2024-10-08RICOH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021048733
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-23
Publication Date
2024-10-08
Estimated Expiration
2041-03-23

AI Technical Summary

Technical Problem

Conventional methods for manufacturing plastic elements with micro- and nano-order fine structures face challenges in transfer accuracy due to volumetric shrinkage during the curing process of thermosetting resins, requiring complex sensors and control mechanisms, and the increased heating rate complicates control, leading to decreased accuracy.

Method used

A method involving a pair of molds where at least one mold is made of a high thermal expansion material, expanding to compress the thermosetting resin during heating to counteract curing shrinkage, ensuring the pattern transfer accuracy by maintaining compressive stress.

Benefits of technology

Improves transfer accuracy of plastic elements with a simple configuration by using thermal expansion to counteract curing shrinkage, reducing sink marks and enhancing shape accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563265000001
    Figure 0007563265000001
  • Figure 0007563265000002
    Figure 0007563265000002
  • Figure 0007563265000003
    Figure 0007563265000003
Patent Text Reader

Abstract

To provide a method for manufacturing a plastic element capable of improving a transfer accuracy of the plastic element with a simple configuration.SOLUTION: There is provided a method for manufacturing a plastic element, in which a plastic element is molded by heating and curing a thermosetting resin having a predetermined pattern transferred thereon. The method includes the steps of: fixing a pair of molds by sandwiching a thermosetting resin between the pair of molds; and heating the pair of molds to cure the thermosetting resin. At least one of the pair of molds includes: a transfer unit that transfers the pattern in contact with the thermosetting resin; and an expansion unit that expands in a compression direction in which the transfer unit compresses the thermosetting resin by heating. An expansion amount of the expansion unit is greater than or equal to an amount of curing shrinkage of the thermosetting resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a plastic element and to an apparatus for producing a plastic element. [Background technology]

[0002] In recent years, optical elements with fine structures on the micro- and nano-order, such as microlens arrays and diffractive optical elements, have been used to improve the uniformity of illumination in 3D sensing using Tof (Time of Flight) and thereby enhance distance measurement accuracy.

[0003] A known method for manufacturing such optical elements involves sandwiching a liquid thermosetting resin between flat upper and lower molds, on which the inverted shape of the desired optical surface has been formed in advance, and heating the resin to transfer the inverted shape to the resin and harden it.

[0004] In addition, thermosetting resins that are liquid at room temperature undergo volumetric shrinkage during the process of hardening due to a crosslinking reaction caused by heating, which can lead to poor transfer such as sink marks and reduced shape accuracy. To address this issue, a system is known that detects the negative pressure that occurs due to hardening shrinkage at the gel point where the viscosity of the thermosetting resin increases, and applies pressure accordingly (for example, Patent Document 1). Summary of the Invention [Problem to be solved by the invention]

[0005] However, conventional techniques require highly accurate sensors and complex control mechanisms to detect the gel point and provide feedback, etc. In addition, the faster the heating speed is increased to increase productivity, the more difficult it becomes to control, resulting in a problem of reduced transfer accuracy of the plastic elements.

[0006] An object of the present invention is to provide a method for manufacturing a plastic element that can improve the transfer accuracy of the plastic element with a simple configuration. [Means for solving the problem]

[0007] One aspect of the present invention is a manufacturing method for a plastic element in which a thermosetting resin to which a predetermined pattern has been transferred is hardened by heating to form a plastic element, the method comprising the steps of: sandwiching thermosetting resin between a pair of molds and fixing the pair of molds; and heating the pair of molds to harden the thermosetting resin, wherein at least one of the pair of molds has a transfer portion that contacts the thermosetting resin to transfer the pattern, and an expansion portion that expands in a compression direction in which the transfer portion compresses the thermosetting resin upon heating, and the amount of expansion of the expansion portion is equal to or greater than the amount of cure contraction of the thermosetting resin. Effect of the Invention

[0008] According to one aspect of the present invention, it is possible to improve the transfer accuracy of a plastic element with a simple configuration. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a schematic diagram showing a manufacturing apparatus for a plastic element. [Diagram 2] 4 is a flow chart showing a method for manufacturing a plastic element. [Diagram 3] 4 is a flow chart showing a method for manufacturing a plastic element. [Figure 4] 4 is a flow chart showing a method for manufacturing a plastic element. [Diagram 5] 4 is a flow chart showing a method for manufacturing a plastic element. [Figure 6] FIG. 2 is a schematic diagram showing a manufacturing apparatus (manufacturing process) according to the first embodiment. [Figure 7] Schematic diagram showing a manufacturing process of the first embodiment. [Figure 8] Schematic diagram showing a manufacturing process of the first embodiment. [Figure 9] Schematic diagram showing a manufacturing process of the first embodiment. [Figure 10] Schematic diagram showing a manufacturing process of the first embodiment. [Figure 11]5A to 5C are diagrams showing the relationship between the manufacturing process of a plastic element and pressure due to thermal expansion. [Figure 12] These are images showing the transfer surface of the mold, where (a) is a laser microscope image and (b) is a 3D display image of (a). [Figure 13] 1A and 1B are images showing a lens surface of a plastic element according to an embodiment, where (a) is a laser microscope image and (b) is a three-dimensional display image of (a). [Figure 14] These are images showing the lens surface of a conventional plastic element, where (a) is a laser microscope image and (b) is a 3D display image of (a). [Figure 15] FIG. 6 is a schematic diagram showing a manufacturing apparatus (manufacturing process) according to a second embodiment. [Figure 16] Schematic diagram showing a manufacturing process of the second embodiment. [Figure 17] Schematic diagram showing a manufacturing process of the second embodiment. [Figure 18] Schematic diagram showing a manufacturing process of the second embodiment. [Figure 19] Schematic diagram showing a manufacturing process of the second embodiment. [Figure 20] Schematic diagram showing a manufacturing process of the second embodiment. [Figure 21] FIG. 13 is a schematic diagram showing a manufacturing apparatus according to a third embodiment. [Figure 22] FIG. 13 is a diagram showing a state before heating of an upper mold constituting the manufacturing apparatus according to the third embodiment. [Figure 23] FIG. 13 is a diagram showing a state in which an upper mold constituting the manufacturing apparatus according to the third embodiment is being heated. [Figure 24] 11A to 11C are schematic diagrams showing a manufacturing process of the third embodiment. [Diagram 25] 11A to 11C are schematic diagrams showing a manufacturing process of the third embodiment. [Figure 26] 13A to 13C are views showing a plastic element obtained by a manufacturing process according to a third embodiment. [Figure 27] FIG. 13 is a schematic diagram showing a manufacturing apparatus according to a fourth embodiment. [Figure 28] 13A to 13C are schematic diagrams showing a manufacturing process of the fourth embodiment. [Figure 29] 13A to 13C are schematic diagrams showing a manufacturing process of the fourth embodiment. [Diagram 30]13A to 13C are schematic diagrams showing a manufacturing process of the fourth embodiment. [Diagram 31] 13A to 13C are schematic diagrams showing a manufacturing process of the fourth embodiment. [Diagram 32] 13A to 13C are schematic diagrams showing a manufacturing process of the fourth embodiment. [Diagram 33] FIG. 13 is a diagram showing an example of a lower mold that constitutes a manufacturing apparatus according to a fourth embodiment. [Diagram 34] FIG. 13 is a diagram showing an example of a lower mold that constitutes a manufacturing apparatus according to a fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described.

[0011] <Manufacturing method of plastic elements> In the method for producing a plastic element according to this embodiment, the thermosetting resin to which a predetermined pattern has been transferred is hardened by heating to form a plastic element.

[0012] The method for manufacturing a plastic element of this embodiment includes the steps of: fixing a pair of molds by sandwiching a thermosetting resin between the pair of molds using the liquid composition of this embodiment; and heating the pair of molds to harden the thermosetting resin.

[0013] At least one of the pair of molds has a transfer portion that comes into contact with the thermosetting resin to transfer a pattern, and an expansion portion that expands in a compression direction in which the transfer portion compresses the thermosetting resin when heated, and the amount of expansion of the expansion portion is equal to or greater than the amount of cure contraction of the thermosetting resin.

[0014] The method for producing a plastic element of this embodiment is specifically realized by the apparatus shown in Fig. 1. Fig. 1 is a schematic diagram showing the apparatus for producing a plastic element.

[0015] The plastic element manufacturing apparatus 100 shown in Figure 1 has an upper die plate 10, a lower die plate 20, a drive unit having guides 70 and 80, a temperature control unit 30 formed on the upper die plate 10 and having a heat transfer unit 31, a heating unit 32, and a cooling unit 33, and a temperature control unit 40 formed on the lower die plate 20 and having a heat transfer unit 41, a heating unit 42, and a cooling unit 43.

[0016] The plastic element manufacturing apparatus 100 further has a control unit (not shown), which controls the drive unit and the temperature adjustment units 30, 40. The control unit has a central processing unit (CPU) and a memory, and is connected to the drive unit and the temperature adjustment units 30, 40 in a wired or wireless manner so as to be able to communicate with them.

[0017] An upper mold 50 is formed on the upper die plate 10 via a temperature control unit 30. The upper mold 50 has an expansion unit 51 that thermally expands when heated, and a transfer unit 52. In the first embodiment, the transfer unit 52 constitutes the transfer surface of the upper mold 50, and a predetermined pattern shape to be transferred to a plastic element is formed in the transfer unit 52. In the upper mold 50, the expansion unit 51 and the transfer unit 52 are integrally formed.

[0018] A lower mold 60 is formed on the lower die plate 20 via a temperature control unit 40. The lower mold 60 has an expansion unit 61 that thermally expands when heated, and a transfer unit 62. In the first embodiment, the transfer unit 62 constitutes the transfer surface of the lower mold 60, and is configured with a predetermined mirror shape that is transferred to a plastic element. In the lower mold 60, the expansion unit 61 and the transfer unit 62 are integrally formed.

[0019] In this specification, the upper mold 50 and the lower mold 60 are an example of a pair of molds of this embodiment, and the upper mold 50 is an example of at least one of the pair of molds of this embodiment.

[0020] Note that the transfer portion 62 may be formed with a predetermined pattern shape to be transferred to the plastic element, similar to the transfer portion 52 of the upper mold 50. Alternatively, instead of the transfer portion 52, the transfer portion 62 may be formed with a predetermined pattern shape to be transferred to the plastic element.

[0021] Thermosetting resin 90 is disposed between upper mold 50 and lower mold 60. In this embodiment, as the drive unit operates, upper mold 50 moves toward fixed lower mold 60, and transfer unit 52 comes into contact with thermosetting resin 90, thereby deforming the shape of thermosetting resin 90. In addition, the temperatures of upper and lower molds 50, 60 are controlled by the temperatures of temperature adjustment units 30, 40, and the thermosetting resin 90 is heated, hardened, and cooled.

[0022] In this specification, a thermosetting resin refers to a synthetic resin having thermosetting properties, which does not dissolve in a solvent after curing, and does not soften even when reheated. The thermosetting resin is not particularly limited, and examples thereof include epoxy resin, urethane resin, acrylic resin, urea resin, melamine resin, phenol resin, and resin.

[0023] The expansion portion 51 of the upper mold 50 is made of a high thermal expansion material. The high thermal expansion material has a linear expansion coefficient of 10×10 -6 / ℃ or more 50×10 -6 / ℃ or less, and more preferably 15×10 -6 / ℃ or more 45×10 -6 / ℃ or less, and more preferably 20×10 -6 / ℃ or more 35×10 -6 / ℃ or less. Examples of such high thermal expansion materials include aluminum (linear expansion coefficient: 27×10 -6 / °C) can be used.

[0024] The thickness of the upper mold 50 is arbitrary, but when the expansion portion 51 of the upper mold 50 is made of a high thermal expansion material, taking into consideration thermal conduction, the thickness is preferably, for example, 20 mm or more and 60 mm or less, more preferably 30 mm or more and 50 mm or less, and even more preferably 35 mm or more and 45 mm or less.

[0025] The expansion section 61 of the lower mold 60 is made of a low thermal expansion material. -6 / ℃, and more preferably 8×10 -6 / ℃ or less, and more preferably 5×10 -6 / °C or less. The lower limit of the linear expansion coefficient of the low thermal expansion material is not limited, and is usually 0.1×10 -6 / °C. An example of such a low thermal expansion material is silicon (linear expansion coefficient: 3.9×10 -6 / °C) can be used.

[0026] In this embodiment, the upper side is a high thermal expansion member and the lower side is a low thermal expansion member, but as long as compressive stress is applied to the transfer surface by heating, the upper side may be a low thermal expansion member and the lower side a high thermal expansion member, or both the upper and lower sides may be high thermal expansion members. This allows the high thermal expansion member to thermally expand in response to the temperatures of the temperature adjustment units 30 and 40, creating an action mechanism in which compressive stress is applied in the transfer direction.

[0027] Here, the steps of the process for carrying out the manufacturing method of the plastic element of this embodiment will be described. Figures 2 to 5 are flowcharts showing the manufacturing method of the plastic element. Figures 6 to 10 show the manufacturing steps of the first embodiment. Figure 11 shows the relationship between the manufacturing steps of the plastic element and pressure due to thermal expansion.

[0028] The method for producing a plastic element of this embodiment includes a resin application step, a mold closing step, a heating step, a cooling step, and a mold opening step (FIG. 2, steps S1 to S5).

[0029] In the resin application process (FIG. 2, step S1), the upper die plate 10 and the lower die plate 20 wait in separate positions (FIG. 3, step S11). At this time, the transfer unit 52 of the upper mold 50 waits in a position separated from the thermosetting resin 90 (FIG. 6). The temperature adjustment units 30 and 40 are maintained in a preheated state at a constant temperature (FIG. 4, step S21). Liquid thermosetting resin 90 is applied to the lower mold 60 (FIG. 5, step S31).

[0030] In the mold closing process (FIG. 2, step S2), upper die plate 10 is lowered and stopped at a position distance D1 from the standby position (FIG. 3, steps S12 and S13). As a result, upper mold 50 is fixed to lower mold 60. Transfer part 52 of upper mold 50 also stops at a position distance D1 below the standby position and comes into contact with thermosetting resin 90 (FIG. 7).

[0031] At this time, the pressure behavior is close to zero (to the left of the solid line in Fig. 11). Note that a slight positive pressure is generated by contact with the resin material, but since it is a liquid, it can be considered to be almost zero.

[0032] The mold closing step (FIG. 2, step S2) is an example of a step in this embodiment in which a pair of molds is fixed together by sandwiching a thermosetting resin between the pair of molds.

[0033] In the heating step (FIG. 2, step S3), heating is started by temperature adjustment units 30, 40 (FIG. 4, step S22). This also heats upper mold 50 and lower mold 60. At this time, upper mold 50, which is made of a high thermal expansion material, thermally expands.

[0034] Therefore, even though the driving part (upper die plate 10) is not moving, the transfer part 52 of the upper mold 50 further descends by a distance D2 (FIG. 8). As a result, even if the thermosetting resin 90 cures and shrinks, a compressive stress is applied in the transfer direction (points (A) and (B) in FIG. 11).

[0035] Furthermore, when the heating is maintained by the temperature adjustment units 30, 40 (FIG. 4, step S23), the heating temperature by the temperature adjustment units 30, 40 becomes constant, and the amount of thermal expansion also settles at a constant value, so that the pressure becomes constant (point (C) in FIG. 11). At this time, the descent of the transfer unit 52 of the upper mold 50 stops (FIG. 8).

[0036] Furthermore, the thermosetting resin 90 becomes a gelled thermosetting resin 91 and undergoes volumetric shrinkage (curing shrinkage), but remains in close contact with the transfer portion 52 due to the compressive stress from the expanded upper mold 50 (FIG. 8).

[0037] On the other hand, in the case of a normal molding method (upper mold 150 and lower mold 160) that does not use a high thermal expansion material, when heating is started and the thermosetting resin 190 gels, volumetric shrinkage (curing shrinkage) occurs (point (E) in Figure 11).

[0038] At this time, negative pressure is generated due to tensile stress while there is intimate contact between the transfer surface of upper mold 150 and gelled thermosetting resin 191. When the contraction further progresses and the resin can no longer withstand the pressure, gelled thermosetting resin 191 peels off from the transfer surface of upper mold 150, and the pressure becomes zero (FIG. 11(F)).

[0039] Furthermore, in the case of the prior art (Patent Document 1), complex feedback control is implemented in this process in which the negative pressure is detected and the drive unit is controlled to fine-tune the die plate position. However, in this embodiment, the transferability can be improved simply by heating without using such complex configurations or controls.

[0040] In this specification, the heating step is an example of a step of heating the pair of molds in this embodiment to harden the thermosetting resin.

[0041] In the cooling step (FIG. 2, step S4), cooling by temperature adjustment units 30, 40 is started (FIG. 4, step S24). As a result, upper mold 50 in an expanded state contracts and returns to its original state. Accordingly, transfer unit 52 of upper mold 50 rises and returns to its original position (position at a distance D1 from the standby position). Thereafter, cooling by temperature adjustment units 30, 40 is terminated (FIG. 4, step S25).

[0042] In addition, since the hardened and solidified thermosetting resin (molded product) 92 also thermally shrinks when cooled, a force acts in the direction in which the upper mold 50 and the molded product peel off from each other (FIG. 9). As a result, the pressure approaches zero (point (D) in FIG. 11). At this point, the molded product 92 has hardened sufficiently and is solid, so even if it peels off from the mold, the transfer accuracy is maintained as a plastic element.

[0043] In the mold opening process (FIG. 2, step S5), the upper die plate 10 is raised and placed on standby, and the transfer part 52 of the upper mold 50 is raised and returns to the standby state (FIG. 3, steps S14 and S15). This allows the molded product 92 to be taken out as a plastic element (FIG. 5, step S32).

[0044] If steps S1 to S5 are to be repeated after the mold opening step (FIG. 2, step S5), the process returns to the resin application step (FIG. 2, step S1) and steps S1 to S5 are executed. If steps S1 to S5 are not to be repeated, the process ends.

[0045] When steps S1 to S5 are repeated (FIG. 2, step S6), the upper die plate 10 remains elevated and waits (FIG. 3, steps S15 and S16). At this time, the temperature adjustment units 30 and 40 are maintained in a preheated state at a constant temperature in preparation for the next molding (FIG. 4, steps S26 and S27), and liquid thermosetting resin 90 is applied to the lower mold 60 again (FIG. 5, step S33).

[0046] In the case of a molding method that does not use a high thermal expansion material, the thermosetting resin peels off from the transfer surface during the heating process, and the pressure becomes zero, as shown in Figure 11. Because the peeling occurs when the thermosetting resin is still uncured, sink marks may appear in the molded product, and the shape accuracy may deteriorate (Figures 12 and 14).

[0047] In contrast, in this embodiment, a high thermal expansion material is used, and therefore, even if the thermosetting resin cures and shrinks in the heating process, a compressive stress is applied in the transfer direction due to the thermal expansion of the upper mold 50 (expansion portion 51). This makes it possible to suppress sink marks in the molded product 92 and improve the shape accuracy (FIGS. 12 and 13).

[0048] In addition, if the amount of movement of the transfer portion 52 due to the thermal expansion of the upper mold 50 (distance D2 in FIG. 11), i.e., the amount of expansion of the expansion portion 51, is equal to or greater than the amount of hardening and shrinkage of the resin, the resin will not separate from the transfer surface. In this case, the pattern of the transfer portion 52 can be reliably transferred to the thermosetting resin 90.

[0049] For example, the preheating temperature is 100° C., the heating temperature is 150° C., the cure shrinkage of the thermosetting resin is 5%, and the thickness of the molded product is 1 mm. As described above, the material of the upper mold 50 is aluminum (linear expansion coefficient: 27×10 -6 / °C) and a thickness of 40 mm, the following relationship is established in which the amount of thermal expansion is greater than or equal to the amount of curing shrinkage (amount of thermal expansion ≧ amount of curing shrinkage), and the pattern shape of the transfer portion 52 can be reliably transferred to the thermosetting resin 90.

[0050] Thermal expansion of upper mold: 27 x 10 -6 / ℃×(150℃-100℃)×40mm=54um Amount of shrinkage of thermosetting resin during hardening: 1mm x 5% = 50um

[0051] Furthermore, if both the upper mold 50 and the lower mold 60 are made of aluminum, even if the thickness of each mold 50, 60 is half that of the upper mold 50, 60 at 20 mm, the combined expansion of the upper and lower molds 50, 60 can exceed the amount of hardening shrinkage.

[0052] On the other hand, the upper mold 50 and the lower mold 60 are both made of silicon (linear expansion coefficient: 3.9×10 -6 / ℃) Thermal expansion of upper mold: 3.9×10 -6 / ℃×(150℃-100℃)×40mm=7.8um This is significantly less than the amount of cure shrinkage.

[0053] To exceed the amount of cure shrinkage (50 um) of the thermosetting resin, the thickness of both the upper and lower molds must be 128 mm or more. A mold with a thickness of more than 100 mm is not practical because it takes too long for heat conduction and significantly extends the tact time. From this perspective, it is preferable to use a high thermal expansion material such as aluminum for at least one of the upper mold 50 and the lower mold 60.

[0054] In this way, according to the first embodiment, it is possible to improve the transfer accuracy of the plastic element with a simple configuration.

[0055] Fig. 15 shows a manufacturing apparatus of the second embodiment. Fig. 16 to Fig. 20 show the manufacturing process of the second embodiment. Note that the same reference numerals are used for the parts of the second embodiment that are common to the first embodiment, and the description thereof will be omitted.

[0056] In the manufacturing apparatus of the second embodiment, the expansion section 51 and the transfer section 52 of the upper mold 50 are configured as separate members. Specifically, the expansion section 51 is disposed between the transfer section 52 and the temperature adjustment section 30, and expands when heated, thereby configuring a pressure adjustment section for the transfer section 52.

[0057] In the second embodiment, the material of the transfer part 52 is selected so that the amount of expansion of the transfer part 52 is smaller than the amount of expansion of the expansion part 51. Specifically, the material of the transfer part 52 of the upper mold 50 is made of the same low thermal expansion material as the lower mold 60.

[0058] For example, in the case of a microlens array in which the pattern to be transferred to a plastic element is an array of tens of thousands of microlenses with a diameter of about 100 μm, it is difficult to machine the shape into aluminum, which is a material with high thermal expansion. In this case, silicon (linear expansion coefficient: 3.9×10 -6 / ℃) and glass substrate (linear expansion coefficient: 0.6×10 -6 / ℃), it is preferable to process it using a semiconductor process. However, silicon and glass have an extremely small linear expansion coefficient.

[0059] Therefore, in the second embodiment, a low thermal expansion material such as silicon is used for the transfer portion 52 of the upper mold 50, and a high thermal expansion material such as aluminum is used for the expansion portion 51 of the upper mold 50, thereby achieving both workability and transferability of the transfer surface. Also, it is possible to adjust the thickness of the expansion portion 51 according to the amount of cure shrinkage of the resin material to be transferred, and to change the material of the expansion portion 51 to accommodate various resin materials.

[0060] For example, the expansion portion 51 is made of aluminum (linear expansion coefficient: 27×10 -6 / °C), the thickness is 40 mm, the preheating temperature is 100°C, the heating temperature is 150°C, the cure shrinkage amount of the thermosetting resin is 5%, and the thickness of the molded product 92 is 1 mm. In this case, as in the first embodiment, a relationship is established in which the amount of thermal expansion is equal to or greater than the amount of cure shrinkage (amount of thermal expansion ≧ amount of cure shrinkage), and the pattern shape of the transfer portion 52 can be reliably transferred to the thermosetting resin 90.

[0061] When forming a pattern shape in the silicon or glass transfer portion 52 of the upper mold 50, the wafer process is used as described above, but the thickness of the transfer portion 52 is 1 mm or less, so there is no problem with thermal conductivity.

[0062] The mechanism by which transferability is improved in the second embodiment is the same as in the first embodiment. During the heating process, the expansion portion 51 of the upper mold 50 thermally expands, causing the transfer portion 52 to descend by a distance D4, thereby applying pressure according to the heating temperature (Figures 17 to 18).

[0063] Although the expansion section 61 and the transfer section 62 of the lower mold 60 in the second embodiment are integrally formed, the expansion section 61 and the transfer section 62 may be formed of separate members, as in the upper mold 50. In that case, the expansion section 61 is disposed between the transfer section 62 and the temperature adjustment section 40, and can configure a pressure adjustment section for the transfer section 62 by expanding when heated.

[0064] In the second embodiment, the amount of expansion of transfer section 52 is smaller than the amount of expansion of expansion section 51, so the shape of transfer section 52 is less likely to change not only in the compression direction in which the thermosetting resin is compressed, but also in a direction perpendicular to the compression direction. This makes it possible to improve the transfer accuracy of the pattern shape by transfer section 52 not only against the cure shrinkage of the thermosetting resin in the compression direction, but also against the cure shrinkage in the direction perpendicular to the compression direction.

[0065] Furthermore, in the second embodiment, by constructing the transfer portion 52 of the upper mold 50 from a low thermal expansion material separate from the expansion portion 51, it is possible to suppress a decrease in the transfer accuracy of the pattern shape even if the upper mold 50 itself undergoes thermal expansion.

[0066] Fig. 21 shows a manufacturing apparatus of the third embodiment. Fig. 22 shows the state of an upper mold constituting the manufacturing apparatus of the third embodiment before heating, and Fig. 23 shows the state of the upper mold constituting the manufacturing apparatus of the third embodiment during heating. Figs. 24 to 25 show the manufacturing process of the third embodiment. Fig. 26 shows a plastic element obtained by the manufacturing process of the third embodiment. Note that parts of the third embodiment that are common to the second embodiment are given the same reference numerals and description thereof will be omitted.

[0067] In the manufacturing apparatus of the third embodiment, upper mold 50 has non-expansion portion 53 adjacent to expansion portion 51 in a direction perpendicular to the compression direction. Non-expansion portion 53 is disposed around expansion portion 51. In the third embodiment, expansion portion 51 has a rectangular shape in a plan view, and non-expansion portion 53 has a shape surrounding expansion portion 51, which is rectangular in plan view (FIG. 22).

[0068] There is no particular limitation on the shape of the non-inflatable portion 53. In this embodiment, the non-inflatable portion 53 has an annular shape with a rectangular outline in a plan view.

[0069] The non-expandable portion 53 is a portion that does not expand due to heat, or expands only slightly even if it does. The material of the non-expandable portion 53 is not particularly limited, but for example, a low thermal expansion material such as silicon can be used, similar to the lower mold 60.

[0070] Moreover, in the third embodiment, transfer portion 52 is provided in the compression direction of expansion portion 51. As a result, when upper mold 50 is heated, expansion portion 51 expands, transfer portion 52 descends, and non-expansion portion 53 does not descend. Transfer portion 52 that descends due to heating becomes effective region 92A of hardened thermosetting resin (molded product) 92, and non-expansion portion 53 that does not descend even when heated constitutes non-effective region 92B of molded product 92.

[0071] Here, the effective area is the area in the plastic element where a desired pattern shape (or mirror surface) is desired to be formed. For example, in the case of an optical element, it refers to the area that performs functions such as transmitting and reflecting light. Also, in the case of an exterior part, it refers to the area where a desired appearance is desired to be ensured. On the other hand, the non-effective area does not necessarily need to have the desired pattern shape (or mirror surface). In other words, it refers to the area where the occurrence of transfer defects such as sink marks will not cause any problems for the element.

[0072] In the third embodiment, the transfer portion 52 of the upper mold 50 is provided only on the portion where the effective area 92A of the molded product 92 is projected, so that the effective area 92A is pressed against the non-effective area 92B in a convex manner when heated (FIG. 23). On the other hand, the non-effective area 92B is not subjected to the pressurizing effect due to thermal expansion, so that the thermosetting resin 90 is weakly constrained against the effective area 92A.

[0073] As a result, since the thermosetting resin 90 can shrink inward, the transferability is improved in the effective area 92A on the inside of the hardened thermosetting resin 92, and shrinkage occurs in the non-effective area 92B on the outside. In other words, by allowing the sink marks to escape to the non-effective area 92B, the transferability of the thermosetting resin 90 can be improved.

[0074] In addition, after the thermosetting resin 90 hardens, the outer periphery (non-effective area 92B) of the solidified thermosetting resin (molded product) 92 peels off from the non-expanding portion 53 of the upper mold 50, making it easier to release the molded product 92 during processes after the mold is opened.

[0075] Furthermore, in the third embodiment, since the expanding portion 51 is restricted by the surrounding non-expanding portion 53, the amount of movement of the transfer portion 52 due to thermal expansion can be increased.

[0076] Fig. 27 shows a manufacturing apparatus of the fourth embodiment. Figs. 28 to 32 show the manufacturing process of the fourth embodiment. Fig. 33 shows an example of a lower mold constituting the manufacturing apparatus of the fourth embodiment. Fig. 34 shows an example of a lower mold constituting the manufacturing apparatus of the fourth embodiment. Note that parts of the fourth embodiment that are common to the second embodiment are given the same reference numerals and descriptions thereof will be omitted.

[0077] In the manufacturing apparatus of the fourth embodiment, a spacer portion 63 that regulates the distance between the upper mold 50 and the lower mold 60 is formed between the upper mold 50 and the lower mold 60 (FIG. 27).

[0078] Since the manufacture of plastic elements includes a heating process, heat accumulates throughout the device when the device is operated continuously, and in the case of the second embodiment described above, the amount of thermal expansion of expansion portion 51 of upper mold 50 also changes slightly, causing dimensional variation in the molded product. Furthermore, if there is temperature unevenness in temperature adjustment portions 30 and 40, pressure unevenness also occurs within transfer portion 52 of upper mold 50, which may result in a decrease in the parallelism of transfer portion 52.

[0079] In contrast, in the fourth embodiment, a spacer portion 63 is provided between the upper mold 50 and the lower mold 60. This regulates the distance between the upper mold 50 and the lower mold 60 and makes it possible to adjust the distance at which the thermosetting resin is compressed, thereby improving the shape accuracy in the thickness direction of the molded product.

[0080] Specifically, the spacer portion 63 is provided in a ring shape in a plan view on the outer periphery of the surface of the lower mold 60 (FIG. 33). During the heating step in FIG. 30, the transfer portion 52 of the upper mold 50 abuts against the spacer portion 63 provided on the lower mold 60 as it descends. This fixes the distance between the transfer portion 52 of the upper mold 50 and the transfer portion 62 of the lower mold 60 at a constant value.

[0081] In the fourth embodiment, the parallelism of the transfer surface is improved by hitting against the spacer portion 63 provided on the outer periphery of the lower mold 60. This provides the effect of further improving the shape accuracy of the molded product in the thickness direction.

[0082] In the fourth embodiment, the height of the spacer portion 63 in the compression direction is preferably smaller than the thickness of the thermosetting resin 90 in the compression direction before heating (FIGS. 28 and 29). By making the height of the spacer portion 63 in the compression direction smaller than the thickness of the thermosetting resin 90 in the compression direction before heating, it is possible to prevent insufficient pressurization by the upper mold 50.

[0083] The material of the spacer portion 63 is not particularly limited, but is preferably a material that has a linear expansion coefficient smaller than that of the expansion portion 51 and is not easily broken. For example, the lower mold 60 and the spacer portion 63 may be made of a nickel-phosphorus alloy (linear expansion coefficient: 12×10 -6 / ℃), the shape precision of the molded product in the thickness direction is further improved.

[0084] In the example of Fig. 33, spacer portion 63 is configured with one spacer around the entire outer periphery of lower mold 60, but the shape of spacer portion 63 is not limited to this. For example, as shown in Fig. 34, multiple spacer portions 63 may be formed at the four corners of lower mold 60. By partially providing multiple spacer portions 63 in this manner, spacer portion 63 is less likely to get in the way when molded product 92 is released in the process after mold opening.

[0085] In the fourth embodiment, the spacer portion that regulates the distance between the upper mold 50 and the lower mold 60 is provided on the lower mold 60, but the location where the spacer is provided is not limited to this. For example, the spacer portion may be formed on the upper mold 50, or the spacer portion may be formed on both the upper mold 50 and the lower mold 60.

[0086] Although an embodiment of the present invention has been described above, the present invention is not limited to a specific embodiment, and various modifications and changes are possible within the scope of the invention described in the claims.

[0087] <Plastic elements> The plastic element of this embodiment is manufactured by the above-mentioned manufacturing method for a plastic element. Specifically, by using the above-mentioned manufacturing apparatus 100 for a plastic element, a cured body (molded product) of a thermosetting resin obtained can become the plastic element of this embodiment.

[0088] As mentioned above, the plastic element obtained in this way has excellent shape precision and suppresses sink marks in the molded product, which is a hardened body of thermosetting resin (Fig. 13). Therefore, such plastic elements can be used for optical elements with fine structures on the micro- and nano-order, such as microlens arrays and diffractive optical elements.

[0089] <Plastic element manufacturing equipment> The plastic element manufacturing apparatus of this embodiment is a plastic element manufacturing apparatus that heats and hardens thermosetting resin to which a predetermined pattern has been transferred to form a plastic element, and has a pair of molds, a drive unit that moves at least one of the pair of molds to a position where the thermosetting resin is sandwiched between the pair of molds, and a heating unit that heats the pair of molds to harden the thermosetting resin, and at least one of the pair of molds has a transfer unit that contacts the thermosetting resin to transfer the pattern, and an expansion unit that expands in a compression direction in which the transfer unit compresses the thermosetting resin due to heating, and the amount of expansion of the expansion unit is greater than or equal to the amount of cure contraction of the thermosetting resin.

[0090] Specifically, the manufacturing apparatus for the plastic element of this embodiment can use the manufacturing apparatus 100 that realizes the above-mentioned manufacturing method for the plastic element (FIGS. 1 to 10).

[0091] In the manufacturing apparatus for plastic elements of this embodiment, as described above, a high thermal expansion member is used, so that even if the thermosetting resin cures and shrinks in the heating process, a compressive stress is applied in the transfer direction due to the thermal expansion of the upper mold 50 (expansion portion 51). Therefore, it is possible to suppress sink marks in the molded product 92 and improve the shape accuracy (FIGS. 12 and 13). [Explanation of symbols]

[0092] 100 Manufacturing equipment 10 Upper die plate 20 Lower die plate 30 Temperature control section 31 Heat transfer section 32 Heating section 33 Cooling section 40 Temperature control section 41 Heat transfer section 42 Heating section 43 Cooling section 50 Upper mold 51 Expansion section 52 Transcription section 53 Non-expandable section 60 Lower mold 61 Expansion section 62 Transcription section 63 Spacer part 70 Guide 80 Guide 90 Thermosetting resin 91 Gelled thermosetting resin 92 Solidified thermosetting resin (molded product) 92A Effective Area 92B Non-validated area [Prior art documents] [Patent documents]

[0093] [Patent Document 1] JP 2013-75499 A

Claims

1. A method for manufacturing a plastic element, comprising the steps of: curing a thermosetting resin onto which a predetermined pattern has been transferred by heating to form a plastic element, the method comprising the steps of: a step of fixing the pair of molds by sandwiching a thermosetting resin between the pair of molds; and heating the pair of molds to harden the thermosetting resin. At least one of the pair of molds is a transfer unit that contacts the thermosetting resin and transfers the pattern; an expansion portion that expands in a compression direction in which the transfer portion compresses the thermosetting resin by heating; A method for manufacturing a plastic element, wherein an amount of expansion of the expansion portion is equal to or greater than an amount of cure contraction of the thermosetting resin.

2. The method for producing a plastic element according to claim 1 , wherein an amount of expansion of the transfer portion is smaller than an amount of expansion of the expansion portion.

3. The method for producing a plastic element according to claim 1 or 2, wherein at least one of the pair of molds has a non-expanded portion adjacent to the expanded portion in a direction perpendicular to the compression direction.

4. The method for producing a plastic element according to claim 3 , wherein the non-expanding portion is arranged around the expanding portion.

5. The method for producing a plastic element according to claim 1 , further comprising forming a spacer portion between the pair of molds to regulate a distance between the pair of molds.

6. The method for producing a plastic element according to claim 5 , wherein a height of the spacer portion in the compression direction is smaller than a thickness of the thermosetting resin in the compression direction before heating.

7. A plastic element produced by the method according to any one of claims 1 to 6.

8. A manufacturing apparatus for a plastic element, which molds a plastic element by heating and curing a thermosetting resin to which a predetermined pattern has been transferred, comprising: A pair of molds; a drive unit that moves at least one of the pair of molds to a position where the thermosetting resin is sandwiched between the pair of molds; a heating unit that heats the pair of molds to harden the thermosetting resin, At least one of the pair of molds is a transfer unit that contacts the thermosetting resin and transfers the pattern; an expansion portion that expands in a compression direction in which the transfer portion compresses the thermosetting resin by heating; An apparatus for manufacturing a plastic element, wherein an amount of expansion of the expansion section is equal to or greater than an amount of cure contraction of the thermosetting resin.

Citation Information

Patent Citations

  • Methods of manufacturing panels of composite material reinforced with closed-section stringers

    EP3112116A1

  • Optical element producing method, optical element produced by the method, display element and display device having the optical element, and imaging element and imaging device having the optical element

    JP2001315217A

  • Manufacturing method for optical element

    JP2009083268A

  • Manufacturing method of mold for forming fine structure and optical element

    JP2013064836A

  • Optical element producing device, optical element producing method, and controlling program

    JP2013075499A