Curable organopolysiloxane composition and cured product thereof

The curable organopolysiloxane composition addresses filler aggregation and fluidity issues by combining specific components, ensuring excellent workability and fluidity for sealing materials.

JP7563337B2Active Publication Date: 2024-10-08SHIN ETSU CHEMICAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021138078
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-26
Publication Date
2024-10-08
Estimated Expiration
2041-08-26

AI Technical Summary

Technical Problem

Flowable organopolysiloxane compositions used as substrate sealing materials face issues with filler aggregation and loss of fluidity due to miniaturization, necessitating improved methods to prevent agglomeration and enhance redispersibility.

Method used

A curable organopolysiloxane composition combining specific components such as organopolysiloxane, organohydrogenpolysiloxane, filler with a defined median diameter and BET specific surface area, and a hydrosilylation reaction catalyst, which suppresses filler aggregation and facilitates easy redispersion.

Benefits of technology

The composition maintains excellent workability and high fluidity, allowing it to flow into complex spaces and protect parts with complex shapes while preventing filler sedimentation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563337000001
    Figure 0007563337000001
  • Figure 0007563337000002
    Figure 0007563337000002
  • Figure 0007563337000003
    Figure 0007563337000003
Patent Text Reader

Abstract

To provide a curable organopolysiloxane composition that suppresses agglomeration of a filler, allows the sedimented filler to be easily redispersed, and has excellent workability.SOLUTION: There is provided a curable organopolysiloxane composition comprising: (A) an organopolysiloxane having at least two alkenyl groups in one molecule and having a viscosity at 25°C of 0.01 to 100 Pa s; (B) an organohydrogenpolysiloxane having at least two SiH groups in one molecule; (C) a filler having a volume median diameter of 0.1 to 100 μm; (D) silica having a BET specific surface area of 50 m2 / g or more; and (E) a hydrosilylation reaction catalyst.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable organopolysiloxane composition and a cured product thereof. [Background technology]

[0002] Organopolysiloxane compositions having flowability are widely used as sealing materials for substrates of automobile parts and various electric products. However, in recent years, with the miniaturization of devices and the miniaturization of parts, it has become necessary to lower the viscosity of sealing materials, and as a result, as a drawback, when an organopolysiloxane composition is stored for a long period of time, the filler contained in the composition separates from the organopolysiloxane, aggregates, and loses fluidity, which is a frequent phenomenon that occurs. For this reason, polyether compounds, typified by polypropylene glycol, and ester compounds are generally used as aggregation prevention additives, but their effect of suppressing aggregation in low-viscosity organopolysiloxane compositions is insufficient. On the other hand, Patent Document 1 reports that aggregation can be suppressed by surface treating the filler with a silane coupling agent having a hydrolyzable group. However, the technology of Patent Document 1 requires a surface treatment step of the filler, and a simpler method for suppressing aggregation has been desired. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 3904469 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a curable organopolysiloxane composition that suppresses aggregation of the filler contained therein, allows any settled filler to be easily redispersed, and has excellent workability. [Means for solving the problem]

[0005]

[0005] As a result of extensive investigations in order to achieve the above-mentioned object, the present inventors have discovered that by combining a filler having a specific volume median diameter with silica having a specific BET specific surface area, it is possible to obtain a curable organopolysiloxane composition that is easy to redisperse without the blended filler agglomerating even after long-term storage and that has excellent workability, thereby completing the present invention.

[0006] That is, the present invention provides 1. (A) 100 parts by mass of an organopolysiloxane having at least two alkenyl groups per molecule and having a viscosity at 25°C of 0.01 to 100 Pa s, (B) an organohydrogenpolysiloxane having at least two SiH groups per molecule: 0.1 to 100 parts by mass, (C) a filler having a volume median diameter of 0.1 to 100 μm (excluding component (D)): 30 to 4,000 parts by mass, (D) BET specific surface area is 50m 2 / g or more of silica: 0.01 to 1 part by mass, and (E) Hydrosilylation reaction catalyst A curable organopolysiloxane composition comprising: 2. The curable organopolysiloxane composition according to 1, wherein the filler (C) is alumina, crystalline silica or both of them. 3. The curable organopolysiloxane composition according to 1 or 2, which has a viscosity of 0.1 to 100 Pa s. 4. A cured product obtained by curing the curable organopolysiloxane composition according to any one of 1 to 3. to provide. Effect of the Invention

[0007] The curable organopolysiloxane composition of the present invention not only has excellent workability because aggregation of the filler is suppressed and settled filler can be easily redispersed, but also has high fluidity, which enables it to flow into minute spaces and protect parts with complex shapes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will be described in further detail below. The curable organopolysiloxane composition according to the present invention contains the following components (A) to (E): (A) Alkenyl-containing organopolysiloxane (B) Organohydrogenpolysiloxane (C) Filler with a volume median diameter of 0.1 to 100 μm (D)BET specific surface area 50m 2 / g or more of silica (E) Hydrosilylation reaction catalyst

[0009] [Component (A)] Component (A) is an organopolysiloxane having a viscosity at 25° C. of 0.01 to 100 Pa·s, and preferably 0.06 to 10 Pa·s, and containing at least two alkenyl groups bonded to silicon atoms in each molecule. If the viscosity at 25°C is less than 0.01 Pa·s, the storage stability of the composition will deteriorate, and if it exceeds 100 Pa·s, high fluidity cannot be ensured. Note that the above viscosity is measured using a B-type rotational viscometer. Such organopolysiloxane is not particularly limited as long as it satisfies the above-mentioned viscosity and alkenyl group content, and any known organopolysiloxane can be used. The structure thereof may be linear or branched, and may also be a mixture of two or more organopolysiloxanes having different viscosities.

[0010] The alkenyl group bonded to the silicon atom is not particularly limited, but is preferably an alkenyl group having 2 to 10 carbon atoms, and more preferably an alkenyl group having 2 to 8 carbon atoms. Specific examples thereof include vinyl, allyl, 1-butenyl, 1-hexenyl groups, etc. Among these, those having 2 to 4 carbon atoms are preferred, and from the standpoint of ease of synthesis and cost, the vinyl group is preferred. The number of alkenyl groups is preferably 2 to 10, and they may be present either at the ends (both ends or one end) or along the middle of the molecular chain of the organopolysiloxane, but from the standpoint of flexibility, it is preferable for them to be present only at both ends.

[0011] The group bonded to the silicon atom other than the alkenyl group is not particularly limited, but is preferably a monovalent hydrocarbon group having 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms. Specific examples thereof include alkyl groups such as methyl, ethyl, n-propyl, n-butyl, n-hexyl, and n-dodecyl groups; aryl groups such as phenyl group; and aralkyl groups such as 2-phenylethyl and 2-phenylpropyl groups. In addition, some or all of the hydrogen atoms bonded to the carbon atoms of these monovalent hydrocarbon groups may be substituted with halogen atoms such as chlorine, fluorine, bromine, etc., and specific examples thereof include halogen-substituted monovalent hydrocarbon groups such as fluoromethyl, bromoethyl, chloromethyl, and 3,3,3-trifluoropropyl groups. Among these, alkyl groups having 1 to 5 carbon atoms are preferred, and from the standpoint of ease of synthesis and cost, it is more preferred that 90 mol % or more of them are methyl groups.

[0012] Examples of such organopolysiloxanes include dimethylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxy groups, dimethylpolysiloxanes capped at both molecular chain terminals with methyldivinylsiloxy groups, dimethylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxy groups, and dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxy groups, with dimethylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxy groups being particularly preferred. The component (A) may use one type alone, or two or more types in combination.

[0013] [(B) Component] The component (B) is an organohydrogenpolysiloxane having at least 2, and preferably 2 to 100, SiH groups in one molecule. The molecular structure of the organohydrogensiloxane of component (B) may be linear, branched or network, and multiple organohydrogensiloxane chains may be linked together via linking groups. Silicon-bonded hydrogen atoms may be present either at the molecular chain terminal portions (both terminals or one terminal) or at non-terminal portions of the molecular chain, or may be present at both.

[0014] Examples of groups other than hydrogen atoms bonded to silicon atoms in component (B) include monovalent hydrocarbon groups having 1 to 10 carbon atoms, excluding alkenyl groups. Specific examples of such groups include alkyl groups such as methyl, ethyl, n-propyl, and n-butyl; aryl groups such as phenyl and tolyl; aralkyl groups such as 2-phenylethyl and 2-phenylpropyl; and halogenated alkyl groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with halogen atoms such as chlorine, fluorine, and bromine.

[0015] The kinetic viscosity of component (B) at 25°C is not particularly limited, but is preferably 1 to 10,000 mm 2 / s is preferable, and 1 to 1,000 mm 2 The kinematic viscosity is a value measured at 25° C. using an Ostwald viscometer.

[0016] Furthermore, component (B) may be a cyclic organohydrogensiloxane represented by the following general formula (1): This compound has the role of crosslinking components (A) and (B) and of imparting adhesiveness.

[0017] [ka] (In the formula, R 1 each independently represents an alkyl group having 1 to 6 carbon atoms; R 2each independently represents a hydrogen atom, an epoxy group bonded to a silicon atom via a carbon atom or a carbon atom and an oxygen atom, an acryloyl group, a methacryloyl group, or a trialkoxysilyl group, an ether bond-containing monovalent organic group, or an aryl group-containing monovalent organic group, 2 At least two of the groups represented by the formula (I) are hydrogen atoms. m is an integer of 2 to 10.

[0018] R 1 Examples of the alkyl group having 1 to 6 carbon atoms include methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, etc. Among these, it is preferable that 90 mol % or more of the alkyl group is a methyl group from the viewpoints of ease of synthesis and cost.

[0019] As mentioned above, R 2 Of the groups represented by the formula (I), two or more are hydrogen atoms. If two or more are not hydrogen atoms, they will not be able to react with the alkenyl groups of component (A) etc. to form a crosslinked structure. Also, R 2 Specific examples of the group other than a hydrogen atom in the formula include epoxy group-containing monovalent organic groups such as 3-glycidoxypropyl, 3-glycidoxypropylmethyl, 2-glycidoxyethyl, and 3,4-epoxycyclohexylethyl groups; (meth)acryloyl group-containing monovalent organic groups such as methacryloxypropyl, methacryloxypropylmethyl, methacryloxyethyl, acryloxypropyl, acryloxypropylmethyl, and acryloxyethyl groups; trialkoxysilyl group-containing monovalent organic groups such as trimethoxysilylpropyl, trimethoxysilylpropylmethyl, trimethoxysilylethyl, triethoxysilylpropyl, triethoxysilylpropylmethyl, and triethoxysilylethyl groups; ether bond-containing monovalent organic groups such as oxyalkyl groups and alkyloxyalkyl groups; aryl group-containing monovalent organic groups such as phenyl, diphenyl, and bisphenol A residues; and ether bond-containing halogen-substituted monovalent organic groups such as perfluorooxyalkyl groups and perfluoroalkyloxyalkyl groups in which the hydrogen atoms bonded to the carbon atoms of these groups are substituted with halogen atoms such as fluorine atoms. m is an integer of 2 to 10, preferably an integer of 2 to 6, more preferably an integer of 2 to 4, and even more preferably 2.

[0020] Among the components (B) represented by formula (1), organohydrogensiloxanes represented by the following general formula (2) are particularly preferred.

[0021] [ka] (In the formula, R 1 and R 2 has the same meaning as above.)

[0022] Specific examples of the component (B) include organohydrogensiloxanes represented by the following formula, but are not limited to these. The component (B) may use one type alone, or two or more types in combination.

[0023] [ka] (In the formula, q and p+r are numbers that result in the above viscosity range, and are preferably integers from 2 to 100, and more preferably from 5 to 50.)

[0024] The blending amount of component (B) is 0.1 to 100 parts by mass, and preferably 2 to 30 parts by mass, per 100 parts by mass of component (A). If it is less than 0.1 part by mass, the hardness becomes insufficient, and if it exceeds 100 parts by mass, the physical properties after curing become poor.

[0025] [(C) component] The component (C) is a filler other than the component (D) described below, and has a volume median diameter of 0.1 to 100 μm, preferably 0.1 to 70 μm. If the volume median diameter is less than 0.1 μm, the particles tend to aggregate and the fluidity becomes poor, whereas if it exceeds 100 μm, the fluidity of the particles themselves becomes low. The shape of component (C) is arbitrary and may be either amorphous or spherical. In the present invention, the volume median diameter is the 50% cumulative diameter (D 50 ) shall be measured.

[0026] Examples of fillers for component (C) include metal-based powders such as aluminum powder, copper powder, and nickel powder; metal oxide-based powders such as silicon oxide powder (crystalline silica powder) other than component (D), alumina powder, magnesium oxide powder, beryllium oxide powder, chromium oxide powder, and titanium oxide powder; metal nitride-based powders such as boron nitride powder and aluminum nitride powder; and metal carbide-based powders such as boron carbide powder, titanium carbide powder, and silicon carbide powder. Of these, when electrical insulation properties are required for the resulting silicone rubber, metal oxide powders, metal nitride powders, and metal carbide powders are preferred, metal oxide powders are more preferred, and alumina powder and crystalline silica powder are even more preferred. The component (C) may use one type alone, or two or more types in combination.

[0027] The blend amount of the component (C) is 30 to 4,000 parts by mass, preferably 100 to 3,000 parts by mass, and more preferably 200 to 2,000 parts by mass, per 100 parts by mass of the component (A).

[0028] [(D) component] Component (D) has a BET specific surface area of ​​50 m 2 / g or more, preferably 100m 2 / g or more. BET specific surface area is 50m 2 If the specific surface area is less than 400 m / g, the effect of facilitating redispersion of the settled filler cannot be obtained. 2 / g or less is preferable, and 300m 2 / g or less is more preferable.

[0029] Examples of silica as component (D) include fumed silica, precipitated silica, calcined silica, quartz powder (excluding crystalline silica powder), and diatomaceous earth. These silicas may be used as they are, or may be used after having been subjected to a surface hydrophobization treatment with a surface treatment agent in advance, or after the silica surface is hydrophobized by adding a surface treatment agent when it is mixed with component (A). Examples of the surface treatment agent include methylchlorosilanes such as trimethylchlorosilane, dimethyldichlorosilane, and methyltrichlorosilane; dimethylpolysiloxane; and organosilicon compounds such as hexamethyldisilazane, divinyltetramethyldisilazane, and dimethyltetravinyldisilazane. As component (D), fumed silica is preferred, and fumed silica the surface of which has been hydrophobized with the above-mentioned organosilicon compounds is particularly preferred.

[0030] The component (D) is available as a commercially available product. Specific examples thereof include Aerosil (registered trademark) R8200, R972, R972V, R972CF, R974, R202, R805, R812, R812S, RY200, RY200S, and RX200 manufactured by Nippon Aerosil Co., Ltd.; Reolosil (registered trademark) DM-10, DM-20, DM-20S, DM-30, and DM-30S manufactured by Tokuyama Corporation; and Musil 120A and Musil 130A manufactured by Shin-Etsu Chemical Co., Ltd. The component (D) may use one type alone, or two or more types in combination.

[0031] The amount of component (D) is 0.01 to 1 part by mass, and preferably 0.05 to 0.1 part by mass, per 100 parts by mass of component (A). If it is less than 0.01 part by mass, the effect of facilitating redispersion of the settled filler is inferior, and if it exceeds 1 part by mass, the fluidity of the composition is reduced.

[0032] [(E) component] Component (E) is a hydrosilylation catalyst. Any hydrosilylation catalyst that can promote the addition reaction between the alkenyl group of component (A) and the SiH group of component (B) can be used, and any conventionally known catalyst can be used. Specifically, it is preferable to use a platinum group metal catalyst. Specific examples of the catalyst include platinum group metals such as platinum (including platinum black), rhodium, and palladium; platinum chlorides such as H2PtCl4·nH2O, H2PtCl6·H2O, NaHPtCl6·nH2O, KHPtCl6·nH2O, Na2PtCl6·nH2O, K2PtCl4·nH2O, PtCl4·nH2O, PtCl2, and Na2HPtCl4·nH2O (wherein n is an integer of 0 to 6, preferably 0 or 6), chloroplatinic acid, platinum chloride, etc. Examples of suitable catalysts include gold salts; alcohol-modified chloroplatinic acid; complexes of chloroplatinic acid and olefins; platinum black, platinum group metals such as palladium supported on supports such as alumina, silica, and carbon; rhodium-olefin complexes; chlorotris(triphenylphosphine)rhodium (Wilkinson's catalyst); complexes of platinum chloride, chloroplatinic acid or chloroplatinate with vinyl group-containing siloxanes, and the like. These may be used alone or in combination of two or more. Among these, a catalyst selected from platinum and platinum compounds is preferred.

[0033] The amount of component (E) added should be an effective amount as a catalyst that can promote the reaction between components (A) and (B), and may be adjusted appropriately depending on the desired curing rate. In particular, the amount of component (E) is preferably 0.1 to 7,000 ppm, and more preferably 1 to 6,000 ppm, calculated as platinum group metal atoms relative to the mass of component (A).When the amount of component (E) is within the above range, a more efficient catalytic action can be expected.

[0034] [Other ingredients] In addition to the above components (A) to (E), known additives may be added to the curable organopolysiloxane composition of the present invention, provided the addition does not impair the object of the present invention. Reaction control agent For example, a reaction inhibitor may be added to suppress the curing reaction of the composition at room temperature and to extend the shelf life and pot life. The reaction inhibitor may be any that is capable of suppressing the catalytic activity of the component (E), and any reaction inhibitor known in the art can be used. Specific examples thereof include acetylene alcohol compounds such as 1-ethynyl-1-cyclohexanol and 3-butyn-1-ol, various nitrogen compounds such as triallyl isocyanurate, organic phosphorus compounds, oxime compounds, and organic chloro compounds, and these may be used alone or in combination of two or more. Among these, 1-ethynyl-1-cyclohexanol and triallyl isocyanurate are preferred.

[0035] When a reaction inhibitor is used, the amount thereof is preferably 0.01 to 5 parts by mass, and more preferably 0.05 to 1 part by mass, per 100 parts by mass of component (A), taking into consideration the shelf life and pot life of the composition, and the curability of the composition. The reaction inhibitor may be diluted with an organic solvent such as toluene, xylene, or isopropyl alcohol in order to improve dispersibility in the composition.

[0036] · Trialkoxysilyl-blocked organopolysiloxane Furthermore, for the purpose of lowering the viscosity of the curable organopolysiloxane composition of the present invention and imparting fluidity, an organopolysiloxane in which one molecular chain end is capped with a trialkoxysilyl group, an organopolysiloxane in which both molecular chain ends are capped with trialkoxysilyl groups, or both of these may be added. The viscosity at 25° C. of the organopolysiloxane having one or both molecular chain ends capped with a trialkoxysilyl group is preferably 0.01 to 100 Pa s, more preferably 0.03 to 10 Pa s, and even more preferably 0.05 to 5 Pa s. The above viscosity is measured using a B-type rotational viscometer. Each alkoxy group constituting the terminal trialkoxysilyl group preferably has, independently of one another, 1 to 6 carbon atoms, more preferably 1 to 4 carbon atoms, and examples thereof include a trimethoxysilyl group and a triethoxysilyl group. Examples of substituents bonded to silicon atoms other than terminal trialkoxysilyl groups include monovalent hydrocarbon groups having 1 to 8 carbon atoms, such as alkyl groups, such as methyl, ethyl, n-propyl, n-butyl, n-pentyl, and n-hexyl groups; cycloalkyl groups, such as cyclohexyl groups; alkenyl groups, such as vinyl and allyl groups; and aryl groups, such as phenyl and tolyl groups, as well as halogenated monovalent hydrocarbon groups, such as chloromethyl and trifluoromethyl groups, in which some or all of the hydrogen atoms bonded to the carbon atoms of these monovalent hydrocarbon groups have been substituted with halogen atoms, such as chlorine, fluorine, and bromine.

[0037] Examples of such organopolysiloxanes include those represented by the following general formulas (3) and (4).

[0038] [ka]

[0039] In the above formulas (3) and (4), R 3 are each independently an alkyl group having 1 to 4 carbon atoms, specific examples of which include methyl, ethyl, n-propyl, n-butyl, etc. Among these, a methyl group and an ethyl group are preferred. R 4 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 8 carbon atoms, and specific examples thereof include alkyl groups such as methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, and n-heptyl; aryl groups such as phenyl and tolyl; and halogenated monovalent hydrocarbon groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these monovalent hydrocarbon groups have been substituted with halogen atoms such as chlorine, fluorine, and bromine, such as chloromethyl, 3-chloropropyl, and trifluoromethyl. Among these, alkyl groups having 1 to 3 carbon atoms are preferred, and a methyl group and an ethyl group are more preferred. Furthermore, s is preferably an integer of 1-100, and more preferably 5-50.

[0040] When using an organopolysiloxane having one molecular chain end blocked with a trialkoxysilyl group, an organopolysiloxane having both molecular chain ends blocked with trialkoxysilyl groups, or both of them, the amount blended is preferably 1 to 100 parts by mass, and more preferably 2 to 50 parts by mass, per 100 parts by mass of component (A).

[0041] Other Ingredients In addition, hindered phenol-based antioxidants; and colorants such as pigments and dyes may also be added.

[0042] [Method of producing the curable organopolysiloxane composition] There are no particular limitations on the method for producing the curable organopolysiloxane composition of the present invention, and it may be in accordance with a conventionally known method, for example, by mixing the components (A) to (E) and, if necessary, other components, and the composition may be in the form of either a one-component type or a two-component type. In addition, if it is a one-component type, it can be stored for a long time by refrigerating or freezing, and if it is a two-component type, it can be stored for a long time at room temperature.

[0043] A one-liquid type composition can be obtained by, for example, putting components (A) and (C) into a Gate Mixer (product name: Planetary Mixer, manufactured by Inoue Seisakusho Co., Ltd.), heating and mixing at 150°C for 1 hour, and then cooling. Then, component (E) and a reaction inhibitor are added and mixed at room temperature for 30 minutes. Furthermore, components (B) and (D) are added and mixed at room temperature for 30 minutes until uniform.

[0044] On the other hand, a two-liquid type composition can be composed of any combination, so long as the combination of components (A), (B), and (E) does not coexist. For example, components (A) and (C) are placed in a gate mixer, heated and mixed at 150°C for 1 hour, and cooled. Then, component (E) is added and mixed at 25°C for 30 minutes to obtain a composition called agent A. Next, components (A), (C), and (D) are placed in a gate mixer, heated and mixed at 150°C for 1 hour, and cooled. Then, a reaction inhibitor is added and mixed at room temperature for 30 minutes, and further component (B) is added and mixed at 25°C for 30 minutes to obtain a composition called agent B. This allows a two-liquid type composition of agents A and B to be obtained.

[0045] The curable organopolysiloxane composition of the present invention has a viscosity at 25°C of preferably 0.1 to 100 Pa·s, more preferably 1 to 50 Pa·s, even more preferably 2 to 30 Pa·s, and particularly preferably 3 to 20 Pa·s. Within such ranges, settling of the filler can be suppressed, resulting in a composition with superior fluidity. The above viscosity is measured using a B-type rotational viscometer.

[0046] The curing conditions for the curable organopolysiloxane composition of the present invention are not particularly limited, but for example, after pouring the composition, it may be left at room temperature (25°C) or actively cured by heating. The heat curing conditions are preferably at a temperature of 50 to 200°C, more preferably 80 to 150°C, for preferably 0.1 to 3 hours, more preferably 0.5 to 2 hours.

[0047] The properties of the cured product thus obtained are not particularly limited, but may be, for example, a rubber-like material with high hardness to a rubber-like material with low hardness, i.e., a gel-like material. The cured product thus obtained can be sufficiently adhered to a member, and is easy to handle. Therefore, it is preferable that the type A durometer hardness defined in JIS K6253 is 5 to 90, or that the Asker C hardness defined in the Society of Rubber Industry, Japan Standards (SRIS) is 5 to 60. EXAMPLES

[0048] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0049] The components used in the examples and comparative examples are shown below. Component (A) A-1: Dimethylpolysiloxane with both ends capped with dimethylvinylsilyl groups and a viscosity of 0.06 Pa s at 25°C A-2: Dimethylpolysiloxane with both ends capped with dimethylvinylsilyl groups and a viscosity of 0.4 Pa s at 25°C A-3: Dimethylpolysiloxane with both ends capped with dimethylvinylsilyl groups and a viscosity of 0.6 Pa s at 25°C

[0050] (B) Component B-1: Organohydrogenpolysiloxane represented by the following formula (kinematic viscosity at 25°C: 18 mm 2 / s) [ka] B-2: Organohydrogenpolysiloxane represented by the following formula (kinematic viscosity at 25°C: 100 mm 2 / s) [ka] (In the formula, the order of the siloxane units in parentheses is not specified.) B-3: Organohydrogenpolysiloxane represented by the following formula (kinematic viscosity at 25°C: 10 mm 2 / s) [ka] B-4: Organohydrogenpolysiloxane represented by the following formula (kinematic viscosity at 25°C: 800 mm 2 / s) [ka] B-5: Organohydrogenpolysiloxane represented by the following formula (kinematic viscosity at 25°C: 15 mm 2 / s) [ka]

[0051] (C) Component C-1: Alumina powder with a volume median diameter of 10 μm C-2: Alumina powder with a volume median diameter of 1 μm C-3: Alumina powder with a volume median diameter of 10 μm C-4: Alumina powder with a volume median diameter of 45 μm C-5: Alumina powder with a volume median diameter of 70 μm C-6: Crystalline silica powder with a volume median diameter of 5 μm

[0052] (D) Component ·D-1:BET specific surface area 200m 2 / g of fumed silica (Musil 120A, Shin-Etsu Chemical Co., Ltd.)

[0053] (E) Component E-1: Dimethylpolysiloxane solution of platinum-divinyltetramethyldisiloxane complex (dissolved in the same dimethylpolysiloxane as A-3 above. Contains 1% by mass of platinum atoms.)

[0054] Other Ingredients F-1: 1-ethynyl-1-cyclohexanol F-2: Triallyl isocyanurate

[0055] G-1: Dimethylpolysiloxane with both ends capped with trimethoxysilyl groups and a viscosity of 1 Pa·s at 25°C G-2: Organopolysiloxane represented by the following formula: [ka]

[0056] [Examples 1 to 4, Comparative Examples 1 to 4] Components (A) to (E) and other components were mixed as follows to obtain a curable organopolysiloxane composition. Components (A), (C), (G-1) and (G-2) were added to a 5L gate mixer (product name: 5L Planetary Mixer, manufactured by Inoue Seisakusho Co., Ltd.) in the amounts shown in Table 1, and mixed at 150°C for 2 hours with heating. After cooling the mixture, component (E) was added and mixed at 25°C for 30 minutes. Next, reaction inhibitors (F-1) and (F-2) were added and mixed at 25°C for 30 minutes. Finally, components (B) and (D) were added and mixed at 25°C for 30 minutes.

[0057] [Table 1]

[0058] The following physical properties of the resulting composition were measured, and the results are shown in Table 2. [1] Viscosity The viscosity of the curable organopolysiloxane composition at 25° C. was measured using a Brookfield type rotational viscometer at 20 rpm. [2] Storage stability The compositions were sealed in glass containers and allowed to stand in a thermostatic chamber at 23°C for 3 days, 15 days, 30 days, and 60 days, after which the presence or absence of aggregation was visually observed, and the composition was rated as ◯ when no aggregation was observed, and as × when aggregation was observed. [3] Redispersibility The composition was placed in a centrifuge and centrifuged at 1000 rpm for 1 minute, after which the filler that had settled to the bottom was evaluated for redispersibility by shaking. If it was easily redispersible by shaking, it was marked as ◯, and if it was not redispersible, it was marked as ×. [4]Hardness The curable organopolysiloxane composition was press-cured at 120° C. for 10 minutes to a thickness of 2.0 mm, and then heated in an oven at 120° C. for 50 minutes. Three of the obtained silicone sheets were stacked, and the hardness was measured using a Type A durometer or an Asker C durometer as specified in JIS K 6253:2012.

[0059] [Table 2]

[0060] As shown in Table 2, the compositions of Examples 1 to 4 had excellent storage stability and the filler could be easily redispersed. On the other hand, the compositions of Comparative Examples 1 to 4, which did not contain component (D), showed poor redispersibility due to the filler agglomeration caused by long-term storage.

Claims

1. (A) an organopolysiloxane having at least two alkenyl groups in one molecule and a viscosity at 25° C. of 0.01 to 100 Pa s: 100 parts by mass, (B) organohydrogenpolysiloxane having at least two SiH groups per molecule: 0.1 to 100 parts by mass, (C) a filler having a volume median diameter of 0.1 to 100 μm (excluding component (D)): 30 to 4,000 parts by mass, (D) BET specific surface area is 200 to 400 m 2 / g silica: 0.01 to 0.36 parts by weight, and (E) Hydrosilylation reaction catalyst 1. A curable organopolysiloxane composition comprising:

2. 2. The curable organopolysiloxane composition of claim 1, wherein (C) the filler is alumina, crystalline silica, or both.

3. 3. The curable organopolysiloxane composition according to claim 1, which has a viscosity of 0.1 to 100 Pa·s.

4. A cured product obtained by curing the curable organopolysiloxane composition according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Fixing belt and silicone rubber composition for it

    JP2004138764A

  • Heat-curing type liquid silicone rubber composition for fixing roll or fixing belt and fixing roll and fixing belt

    JP2006052254A

  • Fluid curable organopolysiloxane composition

    JP3904469B2