Manufacturing method of H-beam

By controlling the composition and cooling processes of H-beam steel, the challenges of achieving consistent high strength and low yield ratio are addressed, resulting in improved mechanical properties and seismic resistance.

JP7563433B2Active Publication Date: 2024-10-08JFE STEEL CORP
View PDF 21 Cites 0 Cited by

Patent Information

Application Number
JP2022143899
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-11-26
Filing Date
2022-09-09
Publication Date
2024-10-08
Estimated Expiration
2042-09-09

AI Technical Summary

Technical Problem

Existing H-beam steels face challenges in achieving stable high strength and low yield ratio due to variations in cooling processes, leading to inconsistent mechanical properties, and low-temperature steels may suffer from decreased tensile strength and yield ratio issues due to precipitate variations.

Method used

Control the composition of H-beam steel with specific ranges of C, Si, Mn, P, S, V, Ti, and N, and perform intermediate cooling and finish rolling to manage VN precipitation, ensuring a microstructure with controlled ferrite grain sizes and cooling rates to achieve high tensile and yield strengths with a low yield ratio.

Benefits of technology

Stable production of H-section steel with tensile strength of 520 MPa or more, yield strength of 355 MPa or more, and impact absorption energy of 70 J or more at 0°C, while maintaining a yield ratio of 80% or less, enhancing seismic resistance and structural safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563433000003
    Figure 0007563433000003
  • Figure 0007563433000001
    Figure 0007563433000001
  • Figure 0007563433000002
    Figure 0007563433000002
Patent Text Reader

Abstract

To provide an H-section steel and a method of manufacturing the same.SOLUTION: An H-section steel according to the present invention includes a steel composition consisting of a specific component composition and Ceq according to formula (1) in a range satisfying 0.44% or less, with the remainder consisting of Fe and unavoidable impurities, and a microstructure component with an average ferrite grain size of 6 to 30 μm and a maximum ferrite grain size of 70 μm or less from an inner flange surface at 1 / 6 of a flange width to 1 / 2 of a flange thickness, wherein the tensile strength is 520 MPa or higher, the yield strength is 355 MPa or higher, the impact absorption energy vE0 at 0°C is 70 J or higher, and the yield ratio is 80% or lower. Ceq=C+Mn / 6+Si / 24+Ni / 40+Cr / 5+Mo / 4+V / 14(1)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to hot-rolled H-shaped steel beams that are widely used in building structures, and more particularly to H-shaped steel beams intended to improve earthquake resistance and a manufacturing method thereof. [Background technology]

[0002] In light of the serious damage caused to building structures by recent major earthquakes, there is a demand for further improvements in the safety and earthquake resistance of structures.

[0003] From the viewpoint of improving the earthquake resistance of structures by making structural members plastic to absorb earthquake energy, steel materials with low yield ratios are required. Also, for example, if the yield strength of steel applied to beams in architectural structures varies widely, the beams must be thicker than necessary, which is disadvantageous from the viewpoints of safety and economy. For this reason, from the viewpoint of improving the safety and economy of structures, steel materials with a narrower range of variation in yield strength are required.

[0004] In light of this situation, in 1998, JIS standards were established for steel materials for architectural structures with narrow yield strength and low yield ratio, with a narrow variation range of yield strength of 120 MPa or less and a yield ratio of 80% or less. Rolled H-section steel (hot-rolled H-section steel) is used primarily as a structural material for welded structures, particularly as beam material for architectural structures. For this reason, rolled H-section steel is also required to have a narrow variation range of yield strength and a low yield ratio.

[0005] Furthermore, in recent years, there has been a trend for steel-framed building structures to become taller, have larger spans, and are more composite in style. From the standpoint of improving cross-sectional performance such as bending strength and bending rigidity, there is a strong demand for not only narrow yield strength and low yield ratio, but also high strength.

[0006] To satisfy these demands, there are techniques described, for example, in Patent Documents 1 to 3. Patent Document 1 discloses a hot-rolled H-section steel with improved earthquake resistance and high strength and a low yield ratio of 80% or less, which is achieved by optimizing the cooling of the inner and outer surfaces of the flange and generating a hard layer made of bainite and / or tempered martensite with an average volume fraction of 20 to 80% in the flange thickness direction, and a soft layer made of ferrite with an average volume fraction of 50% or more.

[0007] Patent Document 2 discloses a manufacturing technology for thin-walled, high-strength H-shaped steel with a web that combines high strength with good shape by rolling the web at a temperature of Ar3 or lower with a cumulative reduction of 20 to 80% and the flanges at a temperature of Ar3 or higher, and then forming them by finish rolling, and then water cooling from the outer surface side of the flanges.

[0008] Furthermore, Patent Document 3 discloses an H-shaped steel for low temperature use that has high strength and improved low-temperature toughness even when air-cooled, by adding V and Ti in combination, properly controlling the V / N ratio, and performing hot rolling at a cumulative reduction rate of 10% or more at 900°C or less. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 4329583 [Patent Document 2] Patent No. 4581645 [Patent Document 3] Patent No. 6354572 Summary of the Invention [Problem to be solved by the invention]

[0010] However, while the H-shaped steels described in Patent Documents 1 and 2 described above aim to achieve both high strength and a low yield ratio by making maximum use of accelerated cooling after finish rolling, there was a problem in that it was difficult to stably obtain the desired characteristics when cooling variations occurred.

[0011] In addition, the low-temperature H-section steel described in Patent Document 3, which is characterized by its air-cooling manufacturing process, still has problems that, depending on the size and amount of precipitates consisting of V, Ti, and N, the tensile strength decreases or the yield ratio exceeds 80%.

[0012] The present invention has been made to advantageously solve the above-mentioned problems, and has an object to provide an H-shaped steel that can stably achieve a yield ratio of 80% or less while ensuring a tensile strength of 520 MPa or more, a yield strength of 355 MPa or more, and an impact absorption energy vE0 at 0°C of 70 J or more, and a manufacturing method thereof. [Means for solving the problem]

[0013] The inventors produced H-shaped steels with different contents of C, Si, Mn, P, S, V, Ti, Al and N, and thoroughly investigated the tensile strength, yield strength and yield ratio. As a result, they discovered that by controlling the components of the H-shaped steels within appropriate ranges and performing intermediate cooling and finish rolling in hot rolling according to the amounts of V and N, it becomes possible to control the amount of fine VN that contributes to precipitation strengthening and the amount of relatively coarse VN that contributes to ferrite grain refinement, and that H-shaped steels with high strength and low yield ratios can be stably obtained over a wide cooling range.

[0014] The present invention is based on the above findings, and has the following gist and configuration. [1] In weight percent: C: 0.13-0.20%, Si: 0.05 to 0.60%, Mn: 0.80-1.80%, P: 0.025% or less, S: 0.030% or less, V: 0.010~0.100%, Ti: 0.005 to 0.030%, Al: 0.080% or less, and N: 0.0020~0.0100% and a composition in which Ceq according to the following formula (1) is contained in a range satisfying 0.44% or less, with the balance being Fe and unavoidable impurities; A microstructure in which the average ferrite grain size at the 1 / 6 flange width position from the inner surface of the flange to the 1 / 2 flange thickness position is 6 to 30 μm and the maximum ferrite grain size is 70 μm or less; having An H-shaped steel characterized by having a tensile strength of 520 MPa or more, a yield strength of 355 MPa or more, an impact absorption energy vE0 at 0°C of 70 J or more, and a yield ratio of 80% or less. Ceq=C+Mn / 6+Si / 24+Ni / 40+Cr / 5+Mo / 4+V / 14 (1) Here, the element notation in formula (1) indicates the content (mass%) of each element, and the content of elements that are not included is set to 0. [2] The composition further comprises, in mass%, Cr: 1.0% or less, Cu: 1.0% or less, Ni: 1.0% or less, Mo: 1.0% or less Nb: 0.10% or less, B: 0.010% or less, Ca: 0.10% or less, Mg: 0.10% or less, and REM: 0.10% or less The H-shaped steel according to [1], characterized in that it contains one or more selected from the following: [3] A method for manufacturing an H-shaped steel according to [1] or [2], When a steel material having the above-mentioned composition is heated to 1100 to 1350 ° C. and then hot-rolled to form an H-shaped steel, The method for producing H-shaped steel is characterized in that, in the hot rolling, before finish rolling, the outer surface of the flange is cooled at least once to a temperature equal to or lower than T°C calculated by the following formula (2), and then, during reheating, finish rolling is performed at a temperature equal to or lower than (T+130)°C, and then, the outer surface of the flange is cooled at an average cooling rate of 0.10°C / sec or more. T[℃]=-8700 / {log(V N)-3.63}-423 ···(2) Here, the elemental notation in formula (2) indicates the content (mass%) of each element.

[0015] In the present invention, "high strength" refers to a tensile strength of 520 MPa or more, a yield strength of 355 MPa or more, and an impact absorption energy vE0 at 0°C of 70 J or more, as measured by the method described in the examples below. In addition, in the present invention, the term "low yield ratio" refers to a yield ratio of 80% or less, as determined by the method described in the examples below. Effect of the Invention

[0016] According to the present invention, it is possible to stably manufacture H-shaped steel with high strength and low yield ratio even if a relatively inexpensive component system is used, which brings about an industrially beneficial effect. In addition, according to the present invention, it is possible to improve safety and earthquake resistance, and there is also an effect that the reliability of structures is significantly improved. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a cross-sectional view showing an example of an H-section steel according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will be specifically described below, but the present invention is not limited to the embodiment.

[0019] First, the reason why the composition of the H-section steel in the present invention is limited to the above range will be explained. In the following explanation, "%" means "mass %" unless otherwise specified.

[0020] C: 0.13 to 0.20% C is an element necessary for ensuring the strength of the base material, and in order to obtain such an effect, it is necessary that the C content is at least 0.13%. However, if the C content exceeds 0.20%, not only does it reduce the base material toughness, but it also reduces the weldability. Therefore, in the present invention, the C content is set to 0.13 to 0.20%. The C content is preferably 0.14% or more, and 0.19% or less.

[0021] Silicon: 0.05 to 0.60% Silicon must be contained at 0.05% or more to ensure the strength of the base metal and as a deoxidizer. However, if the silicon content exceeds 0.60%, not only does the toughness decrease, but the weldability also deteriorates due to the high bonding strength of silicon with oxygen. Therefore, in the present invention, the silicon content is set to 0.05 to 0.60%. The silicon content is preferably set to 0.20% or more, and 0.50% or less.

[0022] Mn: 0.80 to 1.80% Mn, like Si, is a relatively inexpensive element that has the effect of increasing the strength of the base material, and is therefore an important element for increasing strength. However, if the Mn content is less than 0.80%, the effect of including it is small, while if the Mn content exceeds 1.80%, it is undesirable because it promotes upper bainite transformation and reduces toughness. Therefore, in the present invention, the Mn content is set to 0.80 to 1.80%. The Mn content is preferably set to 1.20% or more, and 1.60% or less.

[0023] P:0.025% or less If the P content exceeds 0.025%, the ductility and toughness of the base material deteriorate. Therefore, in the present invention, the P content in the steel is set to 0.025% or less, and preferably 0.020% or less. On the other hand, since the less P, the better, the lower limit of the P content is not particularly limited and may be 0%. However, since P is usually an element that is inevitably contained in steel as an impurity, and excessively reducing the P content leads to an increase in refining time and an increase in costs, the P content is preferably 0.005% or more.

[0024] S: 0.030% or less When S is contained in steel, it exists in the steel mainly in the form of A-type inclusions. When the S content exceeds 0.030%, the amount of these inclusions increases significantly, and at the same time, coarse inclusions are generated, which greatly reduces the toughness of the base material. Therefore, in the present invention, the S content in steel is set to 0.030% or less. It is preferably 0.020% or less. On the other hand, since the less S, the better, the lower limit of the S content is not particularly limited and may be 0%. Note that S is usually an element that is inevitably contained in steel as an impurity, and excessively reducing the S content leads to an increase in refining time and an increase in costs, so the S content is preferably 0.002% or more.

[0025] V: 0.010~0.100% V is an important element that precipitates in austenite as VN during hot rolling or cooling after hot rolling, becomes a ferrite transformation nucleus, and has the effect of refining crystal grains. V also plays a role in increasing the strength of the base material by precipitation strengthening, and is an essential element for ensuring high tensile strength, high yield strength, and excellent toughness. In order to obtain the above effect, the V content needs to be 0.010% or more. On the other hand, if the V content exceeds 0.100%, not only does the microstructure become significantly finer, making it difficult to ensure a low yield ratio, but it also promotes precipitation embrittlement and significantly impairs the toughness of the base material, which is not preferable. Therefore, in the present invention, the V content is set to 0.010 to 0.100%. The V content is preferably set to 0.015% or more, and preferably 0.070% or less.

[0026] Ti: 0.005 to 0.030% Ti forms TiN in steel to refine austenite grains, and further refines the microstructure by promoting intragranular ferrite transformation with TiN as a nucleus, and is an element effective in improving toughness. In order to obtain the above effect, the Ti content needs to be 0.005% or more. On the other hand, if the Ti content exceeds 0.030%, coarse TiN is generated, which reduces the toughness of the base material, and this is not preferable. Therefore, in the present invention, the Ti content is 0.005 to 0.030%. The Ti content is preferably 0.010% or more, and 0.020% or less.

[0027] Al: 0.080% or less Al is added to steel as a deoxidizing agent, and the effect of the deoxidizing agent saturates when the content exceeds 0.080%, so the upper limit of the Al content is set to 0.080%. There is no particular lower limit for the Al content, but in order to obtain a sufficient deoxidizing effect, it is desirable to set the Al content to 0.003% or more. The Al content is preferably 0.015% or more, and 0.050% or less.

[0028] N: 0.0020~0.0100% N is a useful element that bonds with V in steel and improves the strength of the base material as VN, and a N content of 0.0020% or more is required. However, if the N content exceeds 0.0100%, the carbonitrides formed become coarse and the toughness of the base material is significantly impaired, which is not preferable. Therefore, in the present invention, the N content is set to 0.0020 to 0.0100%. The N content is preferably set to 0.0025% or more, and 0.0070% or less.

[0029] Furthermore, in the present invention, it is not sufficient for each element to simply satisfy the above-mentioned range; it is important that the value of Ceq calculated from C, Mn, Si, V, etc. in the steel, that is, the value of Ceq calculated according to the relationship of the following formula (1), satisfies a predetermined range.

[0030] Therefore, the present inventors investigated the base metal toughness and weldability and obtained the following findings. By increasing Ceq, it is possible to increase the strength of the base material. However, if Ceq is too high, a large amount of upper bainite is generated in the microstructure of the base material, and the amount of martensite generated in the heat-affected zone of the base material during welding also increases. As a result, the toughness of the base material and the toughness of the welded zone are reduced, so the upper limit of Ceq calculated by the following formula (1) is set to 0.44%, and more preferably 0.43% or less. There is no particular restriction on the lower limit of Ceq calculated by the following formula (1), but from the viewpoint of ensuring the strength of the base material, it is preferable that Ceq be 0.34% or more. More preferably, it is 0.38% or more. Ceq=C+Mn / 6+Si / 24+Ni / 40+Cr / 5+Mo / 4+V / 14 (1) Here, the element notation in formula (1) indicates the content (mass%) of each element, and the content of elements that are not included is set to 0.

[0031] The composition of the H-section steel of the present invention is such that the balance other than the components described above is Fe and unavoidable impurities.

[0032] The above-mentioned components are the basic components, and the H-shaped steel of the present invention has the properties targeted by the present invention with these basic components. In the present invention, in order to further improve the strength, ductility, toughness, and welded joint properties of the base material, the following optional elements may be contained as necessary in addition to the above-mentioned basic components. Each of the following components, Cr, Cu, Ni, Mo, Nb, B, Ca, Mg, and REM, may be contained as necessary, so these components may be 0%.

[0033] One or more selected from Cr: 1.0% or less, Cu: 1.0% or less, Ni: 1.0% or less, Mo: 1.0% or less, Nb: 0.10% or less, B: 0.010% or less, Ca: 0.10% or less, Mg: 0.10% or less, and REM: 0.10% or less Cr:1.0% or less Cr is an element that can further increase the strength of steel through solid solution strengthening. However, if its content exceeds 1.0%, it is undesirable because it promotes upper bainite transformation and reduces toughness. Therefore, when Cr is contained as necessary, the Cr content is preferably 1.0% or less. The Cr content is more preferably 0.005% or more. Also, it is more preferably 0.5% or less.

[0034] Cu: 1.0% or less Cu is an element that can further increase the strength of steel by solid solution strengthening. However, if its content exceeds 1.0%, Cu cracking is likely to occur. Therefore, when Cu is contained as necessary, the Cu content is preferably 1.0% or less. The Cu content is more preferably 0.005% or more. Also, it is more preferably 0.5% or less.

[0035] Ni: 1.0% or less Ni is an element that can increase the strength of steel without deteriorating ductility. In addition, since Cu cracking can be suppressed by adding it in combination with Cu, it is desirable to also contain Ni when the composition contains Cu. However, if the Ni content exceeds 1.0%, the hardenability of the steel increases and the toughness tends to decrease. Therefore, when Ni is contained as necessary, it is preferable that the Ni content is 1.0% or less. The Ni content is more preferably 0.005% or more. Also, it is more preferably 0.5% or less.

[0036] Mo: 1.0% or less Mo is an element that can further increase the strength of steel through solid solution strengthening. However, if its content exceeds 1.0%, a large amount of upper bainite is formed in the steel, and toughness tends to decrease. Therefore, when Mo is contained as necessary, the Mo content is preferably 1.0% or less. The Mo content is more preferably 0.005% or more, and more preferably 0.5% or less.

[0037] Nb: 0.10% or less Nb is an element that can improve tensile strength and yield strength by precipitating as carbonitride. However, if its content exceeds 0.10%, it is not preferable because excessive precipitation strengthening makes it difficult to ensure a low yield ratio, promotes precipitation embrittlement, and significantly impairs the toughness of the base material. Therefore, when Nb is contained as necessary, it is preferable that the Nb content is 0.10% or less. The Nb content is more preferably 0.010% or more. Also, it is more preferably 0.030% or less.

[0038] B: 0.010% or less B is an element that has the effect of segregating to grain boundaries in steel and improving grain boundary strength. It also forms composite precipitates with TiN, which become nucleation sites for intragranular ferrite, and is an element that is effective in improving toughness by refining the microstructure. On the other hand, if its content exceeds 0.010%, the toughness decreases due to the grain boundary precipitation of coarse carbonitrides. Therefore, when B is contained as necessary, the B content is preferably 0.010% or less. The B content is more preferably 0.001% or more. Also, it is more preferably 0.003% or less.

[0039] Ca: 0.10% or less Ca has the effect of transforming oxides and sulfides in sulfide-based inclusions into those with high stability at high temperatures, and granulating the sulfide-based inclusions. This inclusion shape control effect by Ca can improve the toughness and ductility of the base material. However, if the Ca content exceeds 0.10%, the cleanliness tends to decrease and the toughness tends to decrease. Therefore, when Ca is contained as necessary, it is preferable that the Ca content be 0.10% or less. The Ca content is more preferably 0.0010% or more. Also, it is more preferably 0.0050% or less.

[0040] Mg: 0.10% or less Mg has the effect of transforming oxides and sulfides in sulfide-based inclusions into those with high stability at high temperatures and granulating them. This shape control effect of Mg on inclusions can improve the toughness and ductility of the base material. However, if the Mg content exceeds 0.10%, the cleanliness tends to decrease and the toughness tends to decrease. Therefore, when Mg is contained as necessary, it is preferable that the Mg content is 0.10% or less. The Mg content is more preferably 0.0010% or more. Also, it is more preferably 0.0050% or less.

[0041] REM: 0.10% or less REM (rare earth metals) have the effect of transforming oxides and sulfides in sulfide-based inclusions into those with high stability at high temperatures, and granulating the sulfide-based inclusions. The shape control effect of REM on the inclusions can improve the toughness and ductility of the base material. However, if the REM content exceeds 0.10%, the cleanliness tends to decrease and the toughness tends to decrease. Therefore, if REM is contained as necessary, it is preferable that the REM content be 0.10% or less. The REM content is more preferably 0.0010% or more. Also, it is more preferably 0.0050% or less.

[0042] Next, the reasons for limiting the microstructure of the H-section steel of the present invention will be explained.

[0043] The H-shaped steel of the present invention has a microstructure in which the average ferrite grain size at the 1 / 6 flange width position from the inner surface of the flange to the 1 / 2 flange thickness position is 6 to 30 μm and the maximum ferrite grain size is 70 μm or less.

[0044] Here, the "1 / 6 flange width position" refers to the position indicated by reference symbol 3 (3a) in an H-shaped steel 10 having a pair of flanges 2 arranged on both ends of a web 1, as shown in Fig. 1. In other words, it is a position spaced 1 / 6 of the flange width from one end of the flange 2 toward the center. Also, the "inner surface of the flange" refers to the flange surface 4 on the side that comes into contact with the web 1. Note that, since the cross-sectional shape of an H-shaped steel is line-symmetrical in the vertical and horizontal directions, the other three positions (reference symbols 3b, 3c, and 3d) that are symmetrical to reference symbol 3a shown in Fig. 1 can also be positions that are 1 / 6 of the flange width.

[0045] In order to achieve the tensile strength of 520 MPa or more, the yield strength of 355 MPa or more, the impact absorption energy at 0°C of 70 J or more, and the yield ratio of 80% or less, which are the objectives of the present invention, it is important to control the average ferrite grain size and the maximum value of the ferrite grain size in the region from the inner surface of the flange to the center of the thickness of the flange at the 1 / 6 position of the flange width (i.e., up to the 1 / 2t position, where t is the flange thickness) within a predetermined range. Note that, since the outermost surface of the flange inevitably contains scale and a decarburized layer, the above "inner surface of the flange" refers to a position 1 mm away from the inner surface.

[0046] That is, when the average ferrite grain size in the above region of the flange thickness exceeds 30 μm, the number of grain boundaries that act as barriers to crack propagation decreases relatively, and the toughness of the base material deteriorates. On the other hand, when the average ferrite grain size in the above region of the flange thickness is less than 6 μm, the yield strength increases significantly relative to the tensile strength, resulting in a yield ratio exceeding 80%, which makes it impossible to secure the desired yield ratio and also reduces the tensile strength. For these reasons, the average ferrite grain size in the above region of the flange thickness is set to 6 to 30 μm, preferably 8 μm or more, and more preferably 26 μm or less.

[0047] Furthermore, even if the above average ferrite grain size satisfies the range of 6 to 30 μm, if the maximum value of the ferrite grain size exceeds 70 μm, it becomes difficult to stably ensure the desired base material toughness. For this reason, the maximum value of the ferrite grain size in the above region of the flange thickness is set to 70 μm or less, preferably 60 μm or less.

[0048] Next, a method for manufacturing an H-beam steel according to the present invention will be described.

[0049] The present invention is a manufacturing method in which a steel material having the above-mentioned composition is heated to 1100 to 1350°C, and then hot-rolled to form an H-shaped steel. In the hot rolling, before finish rolling, the outer surface of the flange is cooled at least once to a temperature equal to or lower than T°C calculated by the formula (2) described below, and then finish rolling is performed during recuperation at a temperature equal to or lower than (T+130)°C, and then the outer surface of the flange is cooled at an average cooling rate of 0.10°C / sec or more. Here, "during recuperation" refers to the period from the point in time when cooling (intermediate cooling) of the outer surface of the flange is completed to the time when the outer surface temperature of the flange is increasing over time due to heat conduction from inside the flange. In the present invention, there is no particular limitation on the method for producing the steel material (slab or beam blank). For example, the steel may be produced by a smelting process that includes a converter or a vacuum degassing process, and the steel material may be produced by a continuous casting method or an ingot casting-bloom rolling method, for example.

[0050] Heating temperature: 1100~1350℃ In the manufacture of H-shaped steel, it is important to control the shape by hot rolling, and in order to process in a high temperature range where the deformation resistance is small, the steel material needs to be heated to 1100°C or higher. Furthermore, in order to fully dissolve VN, it is preferable to heat the steel material to 1200°C or higher. On the other hand, if the heating temperature is too high, TiN dissolves and the effect of suppressing the coarsening of austenite grains is reduced, resulting in coarsening of the structure and reduced toughness. For this reason, the heating temperature of the steel material is set to 1350°C or lower, and preferably 1300°C or lower.

[0051] Hot rolling In the hot rolling of the present invention, before finish rolling, the outer surface of the flange is cooled at least once to a temperature equal to or lower than T°C calculated by the following formula (2), and then finish rolling is performed during recuperation. Thereafter, the outer surface of the flange is cooled at a predetermined average cooling rate. T[℃]=-8700 / {log(V N)-3.63}-423 ···(2) Here, the elemental notation in formula (2) indicates the content (mass%) of each element. Note that "log" in equation (2) is the common logarithm.

[0052] Cooling temperature of the outer surface of the flange: T℃ or less In order to satisfy the above-mentioned average ferrite grain size and maximum ferrite grain size, the outer flange surface of the H-shaped steel of the present invention is cooled to a temperature below the temperature defined by formula (2) (below T°C) at least once before finish rolling (intermediate cooling process).

[0053] The cooling (intermediate cooling) in this process is preferably performed by one-fluid cooling (water cooling) using water as the coolant, or two-fluid cooling using both water and air as the coolants. In the case of water cooling, the flange outer surface can be cooled by, for example, spray cooling, pipe laminar cooling, or slit laminar cooling. In the case of two-fluid cooling, the flange outer surface can be cooled by, for example, mist cooling using a mist cooling nozzle that mixes water with high-pressure air. The temperature during this intermediate cooling can be measured by measuring the temperature of the flange outer surface with a radiation thermometer. Here, the "flange outer surface" refers to the flange surface 5 on the side not in contact with the web 2 in the H-shaped steel 10 shown in FIG. 1.

[0054] The above "up to a temperature of T°C or lower calculated by the following formula (2)" means that the temperature of the outer surface of the flange is reduced to T°C or lower at least once by the above-mentioned water cooling or mist cooling.

[0055] This intermediate cooling promotes the precipitation of VN on the austenite grain boundaries, and by allowing moderate Ostwald ripening in the subsequent recuperation process, ferrite formation from VN that exceeds the critical nucleus size during cooling after finish rolling is effectively generated. In addition, by applying the above intermediate cooling before finish rolling, a temperature gradient is applied in the flange thickness direction. This introduces strain into the flange plate thickness during finish rolling during recuperation, and as a result, strain-induced precipitation of VN also promotes ferrite formation after finish rolling.

[0056] In the present invention, if the intermediate cooling is not performed before the finish rolling, the temperature gradient in the flange thickness direction becomes small, and as a result, even if the finish rolling is performed, a sufficient amount of strain-induced precipitation of VN may not be obtained. This reduces the grain refinement effect of VN, and the microstructure having the average ferrite grain size and the maximum ferrite grain size of 70 μm or less may not be obtained. In contrast, by performing the finish rolling during the reheating, it is possible to stably obtain a microstructure having the desired average ferrite grain size and the maximum ferrite grain size of 70 μm or less.

[0057] For the above reasons, the cooling temperature of the flange outer surface in the intermediate cooling step performed before finish rolling is set to T°C or lower, and more preferably to (T-50)°C or lower. There is no particular lower limit for the cooling temperature of the flange outer surface. From the viewpoint of preventing the excessive formation of upper bainite and martensite, which leads to a decrease in the toughness of the base material, the cooling temperature is preferably set to 300°C or higher.

[0058] In addition, the number of cooling times in the intermediate cooling step is preferably two or more. There is no particular upper limit to this number. In addition to the saturation of the effect of promoting ferrite generation using VN by intermediate cooling, from the viewpoint of suppressing an excessive increase in manufacturing costs, the number of cooling times is preferably four or less. In addition, even when the intermediate cooling step is performed two or more times, the cooling temperature from the second time onwards is set to be equal to or lower than the temperature (T°C or lower) of the above formula (2). For example, when the number of cooling times is set to two, the first cooling (intermediate cooling) is performed to a temperature equal to or lower than the above cooling temperature T°C, and then, the flange width 1 / 6 position is set as a representative position, and the temperature of the flange outer surface at this position is restored to T°C or higher, and the relevant portion is cooled again to T°C or lower by the above water cooling or mist cooling.

[0059] Finish rolling temperature: (T+130)℃ or less In the finish rolling performed during reheating after intermediate cooling, the temperature is controlled to (T+130)°C or less to promote strain-induced precipitation of VN, and as a result, the desired average ferrite grain size can be stably obtained. The temperature is preferably (T+100)°C or less. There is no particular lower limit for the finishing temperature, but from the viewpoint of preventing a decrease in the toughness of the base material due to the introduction of excessive processing strain into the ferrite, it is preferably 600°C or more, more preferably 625°C or more, and even more preferably 650°C or more.

[0060] Average cooling rate of the outer surface of the flange: 0.10℃ / sec or more In the cooling after the finish rolling, if the average cooling rate of the outer surface of the flange is less than 0.10°C / sec, the soft ferrite phase fraction increases. As a result, it is difficult to ensure the mechanical properties of tensile strength of 520 MPa or more and yield strength of 355 MPa or more that are the objective of the present invention. Therefore, the average cooling rate is set to 0.10°C / sec or more. It is preferably set to 5°C / sec or more. There is no particular upper limit to the average cooling rate. From the viewpoint of preventing excessive formation of upper bainite or martensite that leads to a decrease in the toughness of the base material, the average cooling rate of the outer surface of the flange is preferably set to 45.0°C / sec or less, more preferably set to 40°C / sec or less, and even more preferably set to 30°C / sec or less.

[0061] The average cooling rate (°C / sec) after finish rolling was calculated by measuring the temperature of the outer flange surface with a radiation thermometer and converting the temperature change from the start of cooling to the end of cooling per unit time (seconds) as described in the Examples. Here, the start of cooling refers to the timing at which cooling of the outer flange surface with various coolants is started, and the end of cooling corresponds to the timing at which the cooling is ended. When air cooling is used for cooling after finish rolling, the cooling start point is set to immediately after the end of rolling, and the average cooling rate is calculated from the time until the outer flange surface temperature reaches 550°C.

[0062] By adjusting the component composition and performing hot rolling as described above, it is possible to obtain excellent mechanical properties in hot-rolled H-shaped steel, such as a tensile strength of 520 MPa or more, a yield strength of 355 MPa or more, an impact absorption energy vE0 at 0°C of 70 J or more, and a yield ratio of 80% or less. The size, web, and flange thickness of the H-shaped steel targeted by the present invention are not particularly limited, and the steel can also be applied to thin-web H-shaped steel in which the web thickness is relatively thinner than the flange thickness and in which it is difficult to achieve both high strength and shape. EXAMPLES

[0063] The configuration and effects of the present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and appropriate modifications can be made within the scope of the present invention, and all of these modifications are included in the technical scope of the present invention.

[0064] Steel materials adjusted to various chemical compositions shown in Table 1 were hot-rolled according to the conditions shown in Table 2 to produce H-shaped steels with various flange thicknesses. The flange thickness dimensions of the H-shaped steels are shown in Table 2.

[0065] The average cooling rate after finish rolling was calculated by measuring the temperature of the outer flange surface with a radiation thermometer and converting the temperature change from the start of cooling to the end of cooling per unit time (seconds) to calculate the average cooling rate (°C / sec). The temperature in the intermediate cooling process before finish rolling ("intermediate water cooling temperature" shown in Table 2) is the value obtained by measuring the outer flange surface temperature immediately after intermediate cooling with a radiation thermometer. In Table 1, "-" indicates that an element is not intentionally added, and includes not only cases where the element is not contained (0%) but also cases where it is unavoidably contained.

[0066] The obtained H-beams were subjected to evaluation of the average ferrite grain size, tensile tests, and toughness tests. Each evaluation is described in detail below.

[0067] <Ferrite grain size> From the obtained H-section steel, samples for microstructure observation were cut out from five locations: at 1 / 6 of the flange width (see Figure 1), 1 mm from the inner surface, 1 / 8t (t is flange thickness), 1 / 4t, 3 / 8t, and 1 / 2t. The observation surfaces were parallel to the rolling direction and flange thickness direction. These observation surfaces were polished and etched, and then microstructure observation was performed at a magnification of 200x using an optical microscope. Two fields of view (0.12 mm) were taken at each location. 2 / 1 field of view, 5 locations in 2 fields of view each, total 1.20mm 2 ) and the equivalent circle diameter was measured by image analysis to determine the average ferrite grain size and the maximum ferrite grain size.

[0068] <Tensile test> A JIS No. 1A tensile test piece, as specified in JIS Z2201, was taken from the obtained H-shaped steel at a position 1 / 6 of the flange width, with the tensile direction being the length direction of the H-shaped steel. A tensile test in accordance with JIS Z2241 was carried out to determine the tensile strength and yield strength.

[0069] <Toughness test> A 2 mm V-notch Charpy impact test specimen as specified in JIS Z2202 was taken from the obtained H-shaped steel at a position 1 / 6 of the flange width and 1 / 4t (t is the flange thickness) from the inner surface of the flange. A Charpy impact test was conducted in accordance with JIS Z2242 to measure the absorbed energy (vE0) at 0°C.

[0070] The results of the above surveys are shown in Table 2.

[0071] [Table 1]

[0072] [Table 2]

[0073] As shown in Table 2, the test results (Test Nos. 1 to 20 in Table 2) of H-shaped steels manufactured using suitable steels satisfying the chemical composition of the present invention and using manufacturing methods within the scope of the present invention (heating temperature, intermediate cooling before finish rolling, and average cooling rate of the flange outer surface after finish rolling) all satisfied the desired properties (tensile strength: 520 MPa or more, yield strength: 355 MPa or more, yield ratio: 80% or less, impact absorption energy vE0 at 0°C: 70 J or more).

[0074] On the other hand, in the comparative examples (Test Nos. 21 to 40 in Table 2) in which the chemical composition of the H-shaped steel did not satisfy the conditions of the present invention or the manufacturing method within the scope of the present invention was not applied, the values ​​of any of the tensile strength, yield strength, yield ratio, and toughness did not satisfy the required properties. [Explanation of symbols]

[0075] 1. Web 2 Flanges 3 Flange width 1 / 6 position 4 Inner surface of flange 5 Outer surface of flange 10 H-beam

Claims

1. In mass %, C: 0.13-0.20%, Si: 0.05-0.60%, Mn: 0.80 to 1.80%, P: 0.025% or less, S: 0.030% or less, V: 0.010-0.100%, Ti: 0.005-0.030%, Al: 0.080% or less, and N: 0.0020-0.0100% and Ceq according to the following formula (1) is contained in a range satisfying 0.44% or less, with the balance being Fe and unavoidable impurities. A steel material having a composition is heated to 1100 to 1350 ° C., and then hot-rolled to form an H-shaped steel, In the hot rolling, before finish rolling, the outer surface of the flange is cooled at least once to a temperature equal to or lower than T°C calculated by the following formula (2), and then finish rolling is performed during recuperation at a temperature equal to or lower than (T+130)°C, and then the outer surface of the flange is cooled at an average cooling rate of 0.7°C / sec or more and 45.0°C / sec or less. The microstructure has an average ferrite grain size of 6 to 30 μm from the inner surface of the flange to the 1 / 2 position of the flange thickness at the 1 / 6 position of the flange width, and a maximum ferrite grain size of 70 μm or less; Tensile strength at 1 / 6 flange width position is 520 MPa or more, and yield strength is 355 MPa or more, Impact absorption energy vE0 at 1 / 4 of the flange thickness from the inner surface of the flange at 1 / 6 of the flange width is 70 J or more at 0°C. and the yield ratio at the 1 / 6 flange width position is 80% or less. Ceq=C+Mn / 6+Si / 24+Ni / 40+Cr / 5+Mo / 4+V / 14...(1) Here, the element notation in formula (1) indicates the content (mass%) of each element, and the content of elements that are not included is set to 0. T[℃]=-8700 / {log(V・N)-3.63}-423...(2) Here, the element designations in formula (2) indicate the contents (mass%) of each element.

2. The composition further comprises, in mass%, Cr: 1.0% or less, Cu: 1.0% or less, Ni: 1.0% or less, Mo: 1.0% or less, Nb: 0.10% or less, B: 0.010% or less, Ca: 0.10% or less, Mg: 0.10% or less, and REM: 0.10% or less The method for manufacturing H-beam steel according to claim 1, characterized in that the steel contains one or more selected from the following:

Citation Information

Patent Citations

  • Continuous treater for refrigeration treatment, etc. of article

    JP1988054572A

  • Production of oxide grain dispersed cast bloom and rolled shape steel with superior toughness, using this cast bloom as stock

    JP1995216498A

  • Manufacture of extremely thick wide-flange steel excellent in toughness and weldabitlity

    JP1996197102A

  • Extra thick wide flange shape excellent in strength, toughness, weldability, and earthquake resistance and its production

    JP1997125140A

  • Production of extra thick wide flange shape

    JP1998068016A