Manufacturing of elastomeric parts by duplication based on reference standard models

The method of overmolding calendered elastomeric sheets around natural models addresses the challenge of reproducing fine textural details in elastomeric parts, enabling accurate and scalable production of textured elastomeric components.

JP7563876B2Active Publication Date: 2024-10-08BIWI SA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2019222885
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-05
Filing Date
2019-12-10
Publication Date
2024-10-08
Estimated Expiration
2039-12-10

AI Technical Summary

Technical Problem

Current molding methods fail to accurately reproduce the textural subtleties of natural materials like leather, feathers, and hides in elastomeric parts due to limitations in resolution and the inability to create mold surfaces with grain sizes smaller than 1 millimeter, leading to indistinguishable textured parts.

Method used

A method involving the use of calendered elastomeric sheets to form flexible molding cavities by overmolding around natural models, followed by vulcanization, allowing for the creation of highly textured elastomeric parts with precise surface texture replication.

Benefits of technology

Enables the production of elastomeric parts with highly accurate surface texturing, transferring the natural material's texture without manual finishing, and achieving industrial scalability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563876000001
    Figure 0007563876000001
  • Figure 0007563876000002
    Figure 0007563876000002
Patent Text Reader

Abstract

To overcome the shortcomings of conventional methods for obtaining textured elastomeric parts.SOLUTION: The present invention relates to the manufacture of textured molding cavities, especially for molding elastomeric parts with surface texturing. The method is based on obtaining texturing from a natural model, the surface condition of which is reproduced on the elastomeric part by overmolding the model between two sheets of calendered elastomeric material and vulcanizing it at a temperature of 80 to 200°C for 20 to 60 minutes. The present invention also relates to a molding cavity made of elastomeric material thereby obtained and a method of molding textured elastomer parts obtained by vulcanizing a sheet of calendered elastomeric raw material in the inventive cavity on a base element of the same partially vulcanized elastomeric material. Finally, the present invention relates to textured and elastomeric parts obtained using the molding method of the present invention.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of manufacturing elastomeric parts, and more particularly to a method for creating moulding cavities for elastomeric parts with surface texturing, in particular a natural material type texturing or a texturing obtained by own know-how.

[0002] The invention also relates to a method for molding a part made of an elastomeric material with surface texturing from such a cavity.

[0003] The invention can be advantageously applied in the fields of watchmaking, luxury goods, leather goods, packaging, display cases, in particular packaging with rubber or various elastomers or other industrial sectors. [Background technology]

[0004] It is known to manufacture components such as watch bands from natural or synthetic rubber or from various plastic materials. Generally, these bracelets are made by molding, the moulds of which may contain structures that allow graphic elements such as brands or logos to appear on the bracelet, or possibly surface textures, locally or more widely, intended to produce certain aesthetic and / or tactile effects. Only the relief allows shapes and indications to be perceived both visually and tactilely.

[0005] However, current molding methods do not appear to provide localized or large-area surface texturing of elastomeric parts that results in a faithful depiction of the texture of natural materials, such as leather, feathers, flaky skin, rough hide, etc., such that the rendering of the textured part is indistinguishable, at least to the naked eye and / or to the touch, from such natural materials.

[0006] This is in particular due to the fact that currently known molding cavities are unable to reproduce with sufficient accuracy the fineness of the texture of natural materials, due to the lack of resolution of the methods for realizing and / or reproducing the surfaces of these natural materials.

[0007] In fact, moulding cavities for elastomeric materials are conventionally obtained by removing material using a laser according to a digital model obtained by computer-aided design, or by forming (stamping, moulding) a hard metal or plastic cavity that is resistant to the vulcanisation temperature of the elastomeric material to be moulded. Unfortunately, these techniques do not allow the industrial production of mould surfaces with granularities of more than a millimetre, let alone tenths of a millimetre, except by manual final processing. However, many natural or synthetic biomaterials, such as for example feathers, skins or hair, have large variations in surface dimensions or the individual dimensions are simply too small to be moulded or reproduced accurately. Summary of the Invention [Problem to be solved by the invention]

[0008] The object of the present invention is to overcome the drawbacks of the methods for obtaining textured elastomeric parts, such as bracelets as described above, but not only bracelets. [Means for solving the problem]

[0009] To achieve these aims, the invention relates to a method having the features set out in the claims.

[0010] More particularly, according to a first object, the invention relates to a method for making a textured moulding cavity, in particular for moulding elastomeric parts with surface texturing, comprising the following steps: - providing a natural model in which the surface conditions are to be reproduced on the elastomeric part; - placing the natural model between two sheets of a first calendered elastomeric material to form a cavity acquisition assembly. - placing the cavity acquisition assembly between two sheets of a second calendered elastomeric material different from the first elastomeric material calendered into an elastomer so as to cover the cavity acquisition assembly. - placing the whole between two compression plates of a stoving shuttle and closing said shuttle by clamping said two plates against each other so as to compress between said plates the sheet of second calendered material on the cavity acquisition assembly. - heating the stoving shuttle at a temperature between 80°C and 200°C for 20 minutes to 60 minutes to at least partially vulcanize each sheet of calendered elastomeric raw material to overmold one side of said natural model. - opening the shuttle and removing the natural model from between the cavity acquisition blocks to obtain two textured molding cavities, the molding cavities containing at least partially vulcanized sheets of calendered and vulcanized elastomeric raw material.

[0011] This method therefore makes it possible to create molding cavities of flexible, highly textured elastomeric material, without the need for machining modifications or finishing, and by obtaining a very accurate negative of the surface texture of any base model, natural or otherwise, it is possible to transfer this texture to the subsequently molded elastomeric part, rather than with rigid molds as known from the prior art.

[0012] According to a second object, the invention also relates to the flexible moulding cavity obtained by the process described above.

[0013] Finally, according to a third object, the invention relates to a method for moulding a part of an elastomeric material, and to an elastomeric part obtained by this method, comprising the following steps: a) using a moulding cavity according to any one of claims 6 to 8. b) placing a sheet of calendered elastomeric feedstock into said molding cavity; c) placing on the sheet of calendered elastomeric raw material an element of partially vulcanized pre-shaped elastomeric material having substantially the shape of the part to be obtained; d) placing the molding cavity with the elastomeric raw material sheet and pre-molded elements stacked therein between two compression plates of a stove shuttle and pressing the two plates together to compress the elastomeric raw material sheet and pre-molded elements into the cavity. e) heating the shuttle after closing for at least 30 minutes at a temperature of 150°C to 220°C, preferably 160°C to 200°C, to vulcanize the elastomeric raw material sheet and pre-molded element together to form a textured elastomeric part. f) separating the textured elastomeric part formed by firing after firing, the face of the part being textured from the calendered feedstock in contact with the cavity prior to firing.

[0014] Other characteristics and advantages of the invention will appear more clearly from the following description, taken in conjunction with the accompanying drawings, in which: [Brief description of the drawings]

[0015] [Figure 1] 2A-2D are schematic diagrams illustrating the steps of a method for forming a moulding cavity according to the invention; [Diagram 2] FIG. 2 is a schematic diagram illustrating the steps of a method for molding a textured elastomeric part using a cavity obtained by the method of FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] In the following description, the method of creating a mold cavity and using the resulting cavity to mold a textured elastomeric part is described with particular reference to making watch bands, but this application is not intended to limit the scope of the invention, which applies equally to the creation of mold cavities and textured elastomeric molded articles of all types and applications.

[0017] First referring to Fig. 1, according to a first object of the invention, a method for making a textured moulding cavity is presented. In contrast to the known moulding cavities of the prior art and their manufacturing techniques, the invention proposes the manufacture of a cavity, i.e. a flexible mould, itself made of elastomeric material, which is overmolded like a negative onto a natural model in order to achieve texturing in the smallest details, transferring the texture thereby obtained to the elastomeric moulded part during a moulding method which will be described in detail below with reference to Fig. 2.

[0018] The creation of textured elastomeric cavities and their use to mold textured elastomeric parts is also a key feature of the method proposed by the present invention.

[0019] According to the general diagram depicted in FIG. 1, the present invention is primarily directed to a method for realizing textured molding cavities, in particular for molding elastomeric parts with surface texturing.

[0020] Before the actual cavity is provided, in a first step 1 it is desirable to prepare a model whose surface finish will be reproduced on the elastomeric part. Such a model may be of any nature and origin and may have a surface finish that is very diverse but preferably not smooth, i.e. with irregularities. These irregularities may be very small, in particular of the order of a few tenths of a millimeter in depth or length / width, or roughness of the order of a few millimeters or centimeters. The model to be reproduced may preferably be of natural material of animal, vegetable, lithographic or other nature. These may include, but are not limited to, skins, leather, fur, feathers, bark, rocks, etc.

[0021] Once the model has been selected, then in a second step 2, it is necessary to form a cavity acquisition assembly by placing the model between two sheets of a first calendered elastomeric feedstock material and vulcanizing said sheets of calendered elastomeric feedstock material.

[0022] The use of raw sheets, i.e. unvulcanized calendered elastomeric materials obtained by superposing elastomeric materials to form tailored strips and / or sheets, is of particular importance for the method of the invention. In fact, such sheets make it possible to adapt the thickness and material of the cavities made according to the chosen model, without the need for modifications, by completely "printing" the surface texture finish by overmolding, as will be explained below.

[0023] Within the scope of the present invention, preferably calendered sheets having a thickness of 0.5 to 10 mm, more preferably 1 to 3 mm, are used for the cavity acquisition assembly.

[0024] Each sheet of calendered and conditioned raw material is intended to prepare a flexible half-mold of the overmolded model, the thickness of which must be at least 10% greater than half the thickness of the model. The invention is therefore not particularly limited to overmolding models with a thickness greater than 10 mm, but the invention is in fact particularly suitable for obtaining textured cavities from models with a relatively small thickness of less than 1 centimeter, a thickness that is particularly suitable for making overmolding with delicate hard materials.

[0025] The first elastomeric material constituting these calendered sheets is also chosen from fluoroelastomer materials, in particular fluoroelastomer materials of the FKM type, or from nitrile (NBR). Fluoroelastomers are particularly suitable for overmolding and obtaining texture from relatively dense and resistant materials such as leather, rough hides or stone, while nitrile is more suitable for overmolding brittle materials and delicate surface roughness such as hair or feathers.

[0026] Once the model is sandwiched between two sheets of a first calendered elastomeric material, a so-called cavity acquisition assembly is obtained. It is then placed in a third step 3 between two sheets of a second calendered elastomeric material, different from the first, to cover it. The second calendered elastomeric material must have different properties from the first calendered elastomeric material and is preferably composed of raw or partially vulcanized ethylene propylene diene monomer (EPDM). Such a material has the advantage that it does not adhere to the first elastomeric material during the subsequent firing of the cavity.

[0027] The assembly thereby formed must be heated for hardening, and therefore for vulcanization, the sheet of calendered raw material around the model, from which it is desired to obtain a texture. To do so, in a fourth step 4, said assembly is placed between the two compression plates of the stoving shuttle, which are clamped closed against each other so as to compress the sheet and the cavity obtaining assembly between said sheet of the second calendered material and the shuttle plates.

[0028] Advantageously, each of the shuttle clamping plates has an internal silicone compression sole with different Shore A hardness, indeed preferably a first sole with a Shore A hardness of 20-30° and a second sole with a Shore A hardness of 40-50°.

[0029] Such a difference in hardness between the soles is particularly advantageous, since it results in a good compression of the cavity acquisition assembly, and thereby a good overmolding of the model in the sheet of calendered elastomeric raw material, by pressing the hardest sole on said cavity acquisition assembly taken from the EPDM sheet into the softest sole.

[0030] Once the shuttle plates are clamped, the shuttle is then placed in an oven in a fifth step 5 for heating with its contents at a temperature of 80-200°C for 20-60 minutes, where each sheet of calendered elastomeric raw material is at least partially vulcanized and overmolded onto one side of the model.

[0031] For most materials and models, a baking time of 30-45 minutes at 160-200°C is perfectly adapted to achieve full vulcanization of the first calendered material and to obtain a fully textured half-mold on the surface of the chosen model, but for fragile models, a lower temperature of 120-150°C and a heating time of up to 60 minutes is recommended.

[0032] Once baking is complete, the shuttle is simply removed from the furnace (or oven), which is opened in a sixth step 6 to release the sheet of second calendered elastomeric material, thereby releasing the half-molds of each textured cavity formed around the model obtained from the vulcanized first calendered elastomeric material.

[0033] The quality of said cavities obtained from the first moulding is then checked, in particular the integrity and texturing quality.7 In case of defects, the manufacturing method is repeated as described above from new sheets of the calendered first and second elastomeric materials, until of course a cavity of good quality is obtained.

[0034] Once a good quality cavity is obtained 8, an etching or finishing step 9 can then be performed, if necessary, to integrate or imprint a specific additional texture into the cavity, which is then stored for use in the molding method as described below. Molded cavities that do not meet the requirements are discarded 10 and recycled.

[0035] Once a flexible textured elastomeric cavity has been obtained as described above, the present invention also proposes a method for molding a part made of elastomeric material, such as, but not limited to, a textured watch band piece, by means of a model obtained by the flexible cavity. Such a molding method is shown diagrammatically in FIG.

[0036] The molding method of the invention starts with the provision (a) of a molding cavity as obtained above, as well as a first pre-molded elastomeric element having the substantial shape of the part to be obtained. This first pre-molded element can result from a previous molding, for example by compressing the elastomer in a mold having the desired outer shape, at a temperature at which the elastomer is not vulcanized.

[0037] The second step of the method is to place a sheet of raw material, i.e. uncured calendered elastomeric material, in the molding cavity (b) and then place the above-mentioned first elastomeric element thereon (c) in said cavity. The sheet of calendered elastomeric raw material is used to obtain the texture of the molding cavity and at the same time coats the first elastomeric element during molding, where it is melted by vulcanization as described below.

[0038] It should be noted that the calendered sheet of raw material and the first pre-molded elastomeric element can be of different colors if necessary to create certain aesthetic effects. Advantageously, however, both the calendered sheet of raw material and the pre-molded element are made of similar elastomeric materials, so that they can be vulcanized together and provide a perfect mechanical adhesion during molding. Preferably, the raw material sheets and the pre-molded element of ethylene propylene diene monomer (EPDM) may be chosen. The pre-molded element is partially vulcanized, in particular at least T30 and at most T80, before the start of the final molding.

[0039] Once this preparation has been carried out, the next step (d) consists in placing the sheet of elastomeric raw material and the moulding cavity with the superimposed pre-moulded element between the two compression plates of the stoving shuttle.

[0040] The stoving shuttle can be of similar characteristics to those used to form the molding cavity as described above. Each clamping plate forming the stoving shuttle can include a silicone compression sole, each preferably of a different Shore A hardness, the Shore A hardness being in the range as described above.

[0041] Next, the shuttle is inserted into the molding press to press the two plates together so as to compress the elastomeric raw material sheet and the pre-molded element into the molding cavity (e), which is heated at a temperature of 150-220°C, preferably 160-200°C, for at least 30 minutes to vulcanize the elastomeric raw material sheet and the pre-molded element together.

[0042] This heating can come from heating by convection in an oven or, preferably, from conductive heating of the press jaws in contact with the metal parts of the shuttle plate. In fact, this second heating method is optimal in terms of controlling the heating temperature in the center of the shuttle and therefore the vulcanization temperature of the sheet of raw material on the pre-molded element. The heating can be adapted according to electronically controlled set points in the clamping press. Thermocouples are integrated in the press jaws, which continuously measure the temperature in contact with the clamping shuttle and transmit the measurements to the electronic control device of the press in order to be able to adapt the heating temperature taking into account the desired heating profile according to the thermal resistance parameters of the shuttle material.

[0043] The forming press jaws exert a pressure of at least 5 tons, preferably 7 tons, on the compression plates of the stoving shuttle during the entire heating process during forming. In fact, such a pressure is necessary to guarantee a good adhesion between the materials when vulcanizing the green sheet on the pre-formed element, without them squeezing out of the forming cavity.

[0044] It should also be noted that the molding of several pre-molded elements can be carried out simultaneously without affecting the quality of the elements. To do so, it is sufficient to stack a number of cavities between as many compression plates as possible, in each of which a sheet of the calendered elastomeric raw material and a pre-molded element to be coated and textured are placed. Advantageously, up to six elastomeric parts can be molded simultaneously using six cavities and seven compression plates, thus forming a stepped shuttle inserted between the jaws of the molding press.

[0045] In such multi-moulding configurations, it is important to ensure that silicone spacers are strategically positioned between each compression plate and the moulding cavity on the one hand, and between each compression plate and the pre-moulded element on the other hand, in order to apply the most even pressure at each moulding stage.

[0046] Once baking is complete, the molding press is then opened and the shuttle is removed. The compression plates are then separated to access the molded elastomeric part, which goes from a mostly vulcanized sheet of pre-molded calendered raw material, with the texture imparted by the transfer of the molding cavities on the part, to a now fully vulcanized element.

[0047] It is sufficient that the parts thus formed are collected (f) for inspection, removal of flash, possible final processing, and packaging for later end use.

[0048] The above description has been given as a non-exhaustive example of the invention. Their preferred purpose may be to make a watch band made of elastomeric material. However, the skilled person may adapt it to make various watch components in particular, such as an insert intended to be housed in a watch ring, or the back of a case, or any other part that may be made of elastomer and that is interesting to apply textured decorative elements on the elastomer, without leaving the scope of the invention.

Claims

1. 1. A method for making a textured molding cavity, comprising: - providing a natural model (1) whose surface conditions are to be reproduced on an elastomeric part; (2) placing the natural model between two sheets of a first calendered elastomeric material to form a cavity acquisition assembly; (3) placing the cavity acquisition assembly between two sheets of a second calendered elastomeric material different from the first calendered elastomeric material to cover the cavity acquisition assembly; (4) placing the whole between two compression plates of a stoving shuttle and closing said shuttle by clamping said two plates together, thereby compressing said second sheet of calendered material on said cavity acquisition assembly between said plates; heating said stoving shuttle at a temperature between 80°C and 200°C for 20 minutes to 60 minutes to at least partially vulcanize each sheet of first calendered elastomeric material and overmold said natural model on one side thereof; opening the shuttle to remove the natural model from between the cavity acquisition assemblies, thereby obtaining two textured molding cavities having a sheet of at least partially vulcanized first calendered elastomeric material; A method comprising:

2. 2. The method of claim 1, wherein the first calendered elastomeric material is selected from fluoroelastomeric materials.

3. 2. The method according to claim 1, characterized in that the first calendered elastomeric material is of the FKM type or is nitrile (NBR).

4. 4. The method according to claim 1, wherein the second calendered elastomeric material is ethylene propylene diene monomer (EPDM).

5. 5. The method according to claim 1, wherein the shuttle fastening plates each have a silicone compression inner sole with a different Shore A hardness.

6. 6. The method according to claim 5, characterized in that the first sole has a Shore A hardness of 20-30° and the second sole has a Shore A hardness of 40-50°.

7. 1. A method for molding an elastomeric material part, comprising the steps of: a. creating a textured molding cavity according to the method of any one of claims 1 to 6; b. placing a sheet of calendered elastomeric feedstock into said mold cavity; c) placing an element of partially vulcanized pre-formed elastomeric material having the shape of the resulting part on said sheet of calendered elastomeric raw material; d) placing the molding cavity, within which the elastomeric raw material sheet and the pre-formed element are superimposed, between two compression plates of a stove shuttle and pressing the two plates together to compress the elastomeric raw material sheet and the pre-formed element into the cavity; e. heating the shuttle after closing to a temperature of 150° C. to 220° C. for at least 30 minutes to vulcanize the elastomeric feedstock sheet and the pre-formed element together, thereby forming a textured elastomeric part; f. separating the formed textured elastomeric part after firing, the part having a textured surface that was obtained from the calendered feedstock in contact with the cavity prior to firing; A method comprising:

8. 8. The method of claim 7, wherein the calendered raw material sheet and the pre-formed element are made from elastomeric materials of similar chemical nature, thereby allowing them to be crosslinked together.

9. 9. The method according to claim 7 or 8, characterized in that the calendered sheets of raw material and the pre-formed elements are made of ethylene propylene diene monomer (EPDM).

10. 10. The method according to any one of claims 7 to 9, characterized in that the compression plates are held against each other under a pressure of at least 5 tons during the heat treatment.

11. 11. The method according to any one of claims 7 to 10, characterized in that the pre-shaped element is vulcanized to at least T30 and at most T80 before the heating step.

12. 12. Method according to any one of claims 7 to 11, characterized in that silicone spacers are provided between a compression plate and the moulding cavity on the one hand and between the other compression plate and the pre-moulded element on the other hand.

Citation Information

Patent Citations

  • Elastomer clock part i.e. watch strap, fabricating method, involves molding assembly by compression to reticulate elastomer blank and calendered sheet together, and carrying out material removal operation to reveal elastomer blank

    CH701737B1

  • Method of making leatherrlike sheet of high quality feeling

    JP1979041304A

  • Method of making sophiscated leatherrlike sheet

    JP1979041305A

  • Highly moisture-permeable leathery sheetlike material

    JP1989192882A

  • Unevenness forming method for sheet material, sheet-like rubber mold produced by the method, and foamed rubber sheet

    JP2004351836A