Manufacturing method of composite material

A stepwise heating process for prepreg curing at low pressures addresses the limitations of autoclave molding, producing high-quality fiber-reinforced composites with minimal voids and equivalent mechanical properties.

JP7563893B2Active Publication Date: 2024-10-08TEIJIN LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020080872
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-30
Publication Date
2024-10-08
Estimated Expiration
2040-04-30

AI Technical Summary

Technical Problem

The existing autoclave molding method for producing fiber-reinforced composite materials is limited by the need for large and expensive equipment, requiring high capital investment and pressurization, which restricts its widespread application.

Method used

A method involving stepwise heating of prepreg at predetermined temperatures to impregnate fibers with a bismaleimide resin composition, including a first heating step to promote resin impregnation and a second heating step to remove volatile components under vacuum, all conducted at low pressures.

Benefits of technology

This approach enables the production of high-quality fiber-reinforced composite materials without the need for autoclave molding devices, ensuring minimal void formation and maintaining mechanical properties comparable to autoclave-cured materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563893000001
    Figure 0007563893000001
  • Figure 0007563893000002
    Figure 0007563893000002
  • Figure 0007563893000003
    Figure 0007563893000003
Patent Text Reader

Abstract

To provide a method for molding a prepreg which can manufacture a fiber-reinforced composite material having less voids without using an autoclave molding device.SOLUTION: A prepreg composed of a fiber-reinforced base material and a resin composition containing a bismaleimide resin is molded through a first heating step of holding the resin composition at a temperature (T1) that is equal to or higher than a temperature at which viscosity of the resin composition indicates 100 [Pa s] and equal to or lower than a temperature at which the viscosity of the resin composition indicates lowest viscosity for 30 minutes, and holding the resin composition at a temperature equal to or higher than a curing temperature of the bismaleimide resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a composite material, in particular, a method for producing a composite material comprising a step of heating and curing, in multiple stages, a prepreg made of a fiber-reinforced substrate and a resin composition containing a bismaleimide resin. [Background technology]

[0002] Fiber-reinforced composite materials are excellent in specific strength and specific elasticity and are therefore widely used in aerospace products, etc. A widely used method for producing fiber-reinforced composite materials is a composite material production method that includes a step of curing a prepreg in which a fiber-reinforced base material and an uncured thermosetting resin are integrated in advance.

[0003] One method for producing a composite material is the autoclave molding method. Patent Document 1 discloses that a fiber-reinforced composite material was produced by the autoclave molding method using a prepreg containing a bismaleimide resin composition. The autoclave molding method is a molding method in which prepregs are laminated in a molding die, enclosed in a bagging film, and heated and pressurized in an autoclave while removing air and volatiles under vacuum to thermoset the prepreg. The pressure in the autoclave is generally 0.6 to 1.0 (MPa).

[0004] Autoclave molding can produce highly reliable fiber-reinforced composite materials. However, autoclave molding equipment with high pressurizing capacity is large and expensive, requiring a large capital investment, so the application of autoclave molding is limited.

[0005] Therefore, there is a demand for a method for producing a highly reliable fiber-reinforced composite material by curing a prepreg without using an autoclave molding machine or by using an autoclave molding machine with low pressurizing capacity. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-157097 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a method for producing a highly reliable fiber-reinforced composite material by curing a prepreg without using an autoclave molding apparatus or by using an autoclave molding apparatus with low pressurizing capacity. [Means for solving the problem]

[0008] The present inventors have found that the above problems can be solved by gradually heating the prepreg at a predetermined temperature during molding, and have thus completed the present invention.

[0009] The present invention, which solves the above problems, is described below.

[0010] [1] A method for producing a composite material, comprising a step of curing a prepreg made of a fiber-reinforced substrate and a resin composition containing a bismaleimide resin, a first heating step of holding the prepreg at a first temperature (T1) for 30 minutes or more to impregnate the fibers with the resin composition; a curing step of maintaining the resin composition at a third temperature (T3) higher than the first temperature (T1) to cure the resin composition; A method for producing a composite material comprising the steps of: A method for producing a composite material, wherein a first temperature (T1) satisfies the following formula (1): Tb≦T1≦Ta (1) Ta: the temperature at which the resin composition exhibits the minimum viscosity Tb: Temperature at which the viscosity of the resin composition is 100 [Pa s]

[0011] The invention described in [1] above is a method for molding a prepreg made of a fiber-reinforced substrate and a bismaleimide resin composition, and is characterized in that it includes a first heating step of heating the bismaleimide resin composition in a low-viscosity state for a predetermined time before heating to a curing temperature T3 of the bismaleimide resin composition. This first heating step allows the bismaleimide resin composition to be sufficiently impregnated into the fiber-reinforced substrate. Therefore, in the obtained fiber-reinforced composite material, the generation of voids due to non-impregnation of the bismaleimide resin composition is suppressed.

[0012] [2] A method for producing a composite material according to [1], further comprising a second heating step of holding the prepreg at a second temperature (T2) for 30 minutes or more between the first heating step and the curing step, wherein the second temperature (T2) satisfies the following formula (2): T2 = Tc ± 20 [°C] (2) Tc: Peak temperature of the maximum peak observed in the range of 90 to 180°C in the total ion current chromatogram (TIC) of the prepreg measured at a heating rate of 10°C / min using a thermogravimetry-mass spectrometer (TG-MS).

[0013] The invention described in [2] above further includes a second heating step of vacuum removing volatiles generated from the bismaleimide resin composition. This second heating step allows the volatile components generated mainly from the bismaleimide resin composition to be sufficiently vacuum removed. Therefore, in the obtained fiber-reinforced composite material, the generation of voids caused by the volatile components of the bismaleimide resin composition is suppressed.

[0014] [3] The method for molding a prepreg according to [2], wherein the first temperature (T1)<the second temperature (T2)<the third temperature (T3).

[0015] In the invention described in [3] above, the first temperature (T1)<the second temperature (T2)<the third temperature (T3), and the prepreg is molded through three temperature zones each having a different function.

[0016] [4] The method for molding a prepreg according to [1], wherein the molding pressure is 0.5 MPa or less.

[0017] The invention described in [4] above is a method for molding a prepreg under no pressure or low pressure.

[0018] [5] The method for molding a prepreg according to [1], wherein the fiber-reinforced substrate is carbon fiber.

[0019] [6] The resin composition comprises the following components (a) and (b): (a) component: a bismaleimide compound, (b) component: alkenylphenol compound and / or alkenylphenol ether compound, The method for molding a prepreg according to [1], which contains as an essential component.

[0020] The inventions described in [5] and [6] above are methods for molding prepregs in which the fiber-reinforced base material or the resin composition is limited to a specified substance. Effect of the Invention

[0021] The method for producing a composite material according to the present invention, which includes a step of curing a prepreg, can produce a high-quality fiber-reinforced composite material even without pressure or under low pressure by heating for a predetermined time at a predetermined temperature range lower than the curing initiation temperature. Therefore, a high-quality fiber-reinforced composite material can be produced without using an autoclave molding device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The method for producing the composite material of the present invention will be described in detail below. In the method for producing a composite material of the present invention, a predetermined prepreg is molded under predetermined conditions. The prepreg to which the manufacturing method of the present invention is applied is a prepreg which comprises a fiber-reinforced base material and a bismaleimide resin composition containing an uncured bismaleimide resin, and which is previously integrated by impregnating the fiber-reinforced base material with a part or all of the bismaleimide resin composition.

[0023] (1) First heating step The prepreg molding method of the present invention has a first heating step of holding the prepreg at a temperature (T1) for 30 minutes or more. The temperature (T1) is lower than the curing temperature T3 of the bismaleimide resin compound. The first heating step is a step of impregnating a fiber-reinforced substrate with the bismaleimide resin composition constituting the prepreg in a highly fluid state, and replacing voids in the fiber-reinforced substrate with the bismaleimide resin composition under vacuum heating, thereby removing the voids from the prepreg.

[0024] The temperature (T1) at which the prepreg is held in the first heating step is a temperature that promotes impregnation and satisfies the following formula (1). Tb≦T1≦Ta (1) Ta: the temperature at which the resin composition exhibits the minimum viscosity Tb: Temperature at which the viscosity of the resin composition is 100 [Pa s]

[0025] The temperature (T1) is preferably equal to or higher than Td, and more preferably equal to or higher than Te. Td: The temperature at which the viscosity of the resin composition is 50 [Pa s] (Td≦Ta) Te: The temperature at which the viscosity of the resin composition is 15 [Pa s] (Te≦Ta)

[0026] Here, "maintaining at temperature (T1) for 30 minutes or more" does not mean gradually heating from Tb to Ta at a constant heating rate, but means maintaining a constant temperature (T1) within the range from Tb to Ta for 30 minutes or more. "Maintaining a constant temperature (T1) for 30 minutes or more" means maintaining the prepreg within a range of ±10°C of temperature (T1).

[0027] By heating for a predetermined time at a temperature near where the viscosity of the bismaleimide resin composition is low, the bismaleimide resin composition can be sufficiently impregnated into the fiber-reinforced substrate without applying high pressure. If the heating temperature is higher than Ta, voids are likely to occur in the obtained fiber-reinforced composite material due to insufficient impregnation of the resin composition.

[0028] The specific temperature T1 varies depending on the composition of the bismaleimide resin composition, but is generally 60 to 130° C., and preferably 80 to 110° C.

[0029] In the present invention, the temperatures Ta, Tb, Td and Te defined by the viscosity of the bismaleimide resin composition refer to temperatures obtained from a temperature-viscosity curve measured using a rheometer.

[0030] In the first heating step, the prepreg is held at temperature (T1) for 30 minutes or more, preferably 45 minutes or more, and more preferably 60 minutes or more. The upper limit of the holding time is not particularly limited, but in consideration of productivity, it is preferably 12 hours or less, and more preferably 6 hours or less.

[0031] (2) Second heating step The prepreg molding method of the present invention preferably includes a second heating step, which is performed after the first heating step and before the curing of the bismaleimide resin composition, in which the prepreg is held at a temperature (T2) for 30 minutes or more. The second heating step is a step in which moisture remaining in the prepreg and volatile components generated due to the chemical reaction of the bismaleimide resin composition are removed under vacuum heating.

[0032] The temperature (T2) at which the prepreg is held in the second heating step is a temperature at which volatile components are removed, and satisfies the following formula (2). T2 = Tc ± 20 [°C] (2) Tc: Peak temperature showing the maximum peak among the peaks observed in the range of 90 to 180°C in the total ion current chromatogram (TIC) of the prepreg measured at a heating rate of 10°C / min using a thermogravimetry-mass spectrometry (TG-MS). A total ion current chromatogram (TIC) is a chart in which the vertical axis represents the sum of all ions generated by the ion source and the horizontal axis represents time.

[0033] That is, the temperature (T2) at which the prepreg is held in the second heating step is in the range of (Tc-20) to (Tc+20) [°C]. The temperature (T2) is preferably in the range of (Tc-10) to (Tc+20) [°C], and more preferably in the range of Tc to (Tc+20) [°C]. By heating at this temperature for 30 minutes or more, the volatile components mainly derived from the bismaleimide resin composition can be sufficiently removed from the prepreg without applying high pressure. If the heating temperature is (Tc-20) [°C] or higher, the volatile components are particularly sufficiently removed. If the heating temperature is (Tc+20) [°C] or lower, thickening due to a partial curing reaction of the bismaleimide resin composition is unlikely to occur before the volatile components are removed, so the volatile components are particularly sufficiently removed. As a result, it is possible to particularly suppress the generation of voids in the obtained fiber reinforced composite material due to the volatile components generated from the prepreg.

[0034] Here, "maintaining at temperature (T2) for 30 minutes or more" does not mean gradually heating from (Tc-20) to (Tc+20) at a constant heating rate, but means maintaining a constant temperature (T2) within the range of (Tc-20) to (Tc+20) for 30 minutes or more. "Maintaining a constant temperature (T2) for 30 minutes or more" means maintaining the prepreg within a range of ±10°C of temperature (T2).

[0035] The specific temperature T2 varies depending on the volatile components contained in the bismaleimide resin composition, but is generally 110 to 160° C., and preferably 130 to 150° C.

[0036] In the second heating step, the prepreg is held at the temperature (T2) for 30 minutes or more, preferably 45 minutes or more, and more preferably 60 minutes or more. The upper limit of the holding time is not particularly limited, but in consideration of productivity, it is preferably 12 hours or less, and more preferably 6 hours or less.

[0037] (3) Curing process The prepreg molding method of the present invention includes, after the above-mentioned first heating step and / or second heating step, a curing step of curing the bismaleimide resin composition by heating to a predetermined temperature or higher.

[0038] The heating temperature T3 in the curing step varies depending on the composition of the bismaleimide resin composition, but is generally 160 to 205°C, preferably 170 to 195°C, and more preferably 175 to 190°C.

[0039] In the prepreg molding method of the present invention, the prepreg is heated stepwise, with temperature (T1)<temperature (T2)<temperature (T3), and it is preferable that the temperatures T1 and T2, and T2 and T3 have a difference of 10°C or more. It is also preferable that the temperature difference between T1 and T3 is 20°C or more, and it is more preferable that the temperature difference between T1 and T3 is 50°C or more. By heating at temperatures with a sufficient difference between them, it is possible to greatly suppress the formation of voids due to insufficient impregnation and voids due to volatile components.

[0040] (4) Prepreg The prepreg to which the composite material production method of the present invention is applied comprises a fiber-reinforced substrate and a bismaleimide resin composition containing an uncured bismaleimide resin.

[0041] (4-1) Bismaleimide resin composition The bismaleimide resin composition contains a known bismaleimide compound and, if necessary, various additives such as a thermoplastic resin, a filler, and a pigment. The bismaleimide compound (hereinafter, also referred to as BMI) to be blended in the bismaleimide resin composition may be any known bismaleimide compound, for example, a bismaleimide compound represented by the following chemical formula (1).

[0042] [ka]

[0043] [In the chemical formula (1), R1 to R4 each independently represent a group selected from the group consisting of -H, -CH3, -C2H5, -C3H7, -F, -Cl, -Br and -I. X will be described later.]

[0044] In the present invention, the bismaleimide compound preferably contains an aromatic bismaleimide, and may contain an aliphatic bismaleimide. In the present invention, the amount of the aromatic bismaleimide relative to the total amount of the bismaleimide compounds contained in the prepreg is preferably 70 mass% or more.

[0045] (4-1-1) Aromatic bismaleimide compounds When the bismaleimide compound contains an aromatic ring structure (hereinafter also referred to as an "aromatic bismaleimide compound"), X in chemical formula (1) preferably has a structure represented by any of the following chemical formulas (2) to (8).

[0046] [ka]

[0047] [ka]

[0048] [ka]

[0049] [ka]

[0050] [In the chemical formula (5), R5 represents -CH2-, -C(CH3)2-, -O-, or -SO2-.]

[0051] [ka]

[0052] [In the chemical formula (6), R5 represents -CH2-, -C(CH3)2-, -O-, or -SO2-. In addition, R6 to R9 each independently represent a group selected from the group consisting of -H, -CH3, -C2H5, -C3H7, -F, -Cl, -Br, and -I.]

[0053] [ka]

[0054] [In the chemical formula (7), R5 represents -CH2-, -C(CH3)2-, -O-, or -SO2-.]

[0055] [ka]

[0056] [In chemical formula (8), R 10 ~R 11 each independently represents -CH2-, -C(CH3)2-, -O-, or -SO2-. In chemical formula (8), n is 0 to 0.5.

[0057] Examples of such aromatic bismaleimide compounds include N,N'-4,4'-diphenylmethane bismaleimide, N,N'-4,4'-diphenylether bismaleimide, N,N'-m-phenylene bismaleimide, N,N'-p-phenylene bismaleimide, N,N'-m-toluylene bismaleimide, N,N'-4,4'-biphenylene bismaleimide, N,N'-4,4'-(3,3'-dimethylbiphenylene) bismaleimide, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, N,N'-4,4'-diphenylsulfone bismaleimide, and N,N'-4,4'-benzophenone bismaleimide.

[0058] From the viewpoint of the heat resistance of the fiber-reinforced composite material after heat curing, N,N'-4,4'-diphenylmethane bismaleimide, N,N'-4,4'-diphenylether bismaleimide, N,N'-m-toluylene bismaleimide, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, 4-methyl-1,3-phenylene bismaleimide, N,N'-4,4'-diphenylsulfone bismaleimide, and N,N'-4,4'-benzophenone bismaleimide are preferred, and N,N'-4,4'-diphenylmethane bismaleimide, N,N'-4,4'-diphenylether bismaleimide, N,N'-m-toluylene bismaleimide, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, and 4-methyl-1,3-phenylene bismaleimide are particularly preferred. These aromatic bismaleimide compounds may be used alone or in combination of two or more kinds.

[0059] The content of the aromatic bismaleimide compound in the bismaleimide-based resin composition is preferably 20 to 80 mass%, more preferably 30 to 65 mass%, and particularly preferably 35 to 60 mass% based on the total mass of the resin composition. When the content of the aromatic bismaleimide is within this range, the viscosity of the resin composition can be easily adjusted to an appropriate range, and voids during molding can be easily suppressed. In addition, it is easy to obtain a fiber-reinforced composite material that has both heat resistance and impact resistance. When the content of the aromatic bismaleimide compound is less than 20 mass%, the heat resistance of the fiber-reinforced composite material finally obtained using the resin composition tends to be low. When the content of the aromatic bismaleimide compound is more than 80 mass%, the impact resistance of the fiber-reinforced composite material finally obtained using the resin composition tends to be low.

[0060] (4-1-2) Aliphatic bismaleimide compounds When the bismaleimide compound does not contain an aromatic ring structure (hereinafter also referred to as an "aliphatic bismaleimide compound"), X in chemical formula (1) preferably has a structure represented by any of the following chemical formulas (9) to (11).

[0061] [ka]

[0062] [In the chemical formula (9), n is an integer of 10 or less, and preferably 1, 2, 3, 4, or 6.]

[0063] [ka]

[0064] [ka]

[0065] Examples of such aliphatic bismaleimide compounds include 1,6'-bismaleimide-(2,2,4-trimethyl)hexane, hexamethylenediamine bismaleimide, N,N'-1,2-ethylene bismaleimide, N,N'-1,3-propylene bismaleimide, and N,N'-1,4-tetramethylene bismaleimide. 1,6'-bismaleimide-(2,2,4-trimethyl)hexane and hexamethylenediamine bismaleimide are particularly preferred. The aliphatic bismaleimide compounds may be used alone or in combination of two or more.

[0066] The content of the aliphatic bismaleimide compound in the resin composition is preferably 3 to 30 mass%, more preferably 5 to 20 mass%, and particularly preferably 7 to 15 mass%, based on the total mass of the resin composition. If the amount of the aliphatic bismaleimide compound is less than 3 mass%, the toughness of the fiber reinforced composite material finally obtained using this resin composition is poor and the impact resistance is likely to decrease. If the content of the aliphatic bismaleimide compound exceeds 30 mass%, the heat resistance of the fiber reinforced composite material finally obtained tends to decrease.

[0067] (4-1-4) Alkenylphenol compounds and / or alkenylphenol ether compounds The bismaleimide resin composition may contain an alkenylphenol compound and / or an alkenylphenol ether compound. The alkenylphenol ether compound is obtained by reacting a phenolic compound with an alkenyl halide. The alkenylphenol ether compound blended in the resin composition is obtained by subjecting an alkenylphenol ether compound to Claisen rearrangement (JP Patent Publication 52-994). In the present invention, the alkenylphenol compound and / or the alkenylphenol ether compound may contain a rearrangement structure thereof.

[0068] The alkenylphenol compound and / or alkenylphenol ether compound is preferably allylphenol, methallylphenol or their ethers, and more preferably the alkenylphenol compound or alkenylphenol ether compound is a compound represented by the following chemical formulas (12) to (16).

[0069] [ka]

[0070] [In chemical formula (12), R 12 , R 13 , R 14 are each independently a hydrogen atom or an alkenyl group having 2 to 10 carbon atoms, and preferably an allyl group or a propenyl group. 12 , R 13 , R 14 At least one of them is an alkenyl group having 2 to 10 carbon atoms.]

[0071] [ka]

[0072] [In chemical formula (13), R 15 is a direct bond, -CH2-, -C(CH3)2-, -O-, -S-, -SO- or -SO2-. 16 , R 17 , R 18 , R 19 are each independently a hydrogen atom or an alkenyl group having 2 to 10 carbon atoms, and preferably an allyl group or a propenyl group. 16 , R 17 , R 18 , R 19 At least one of them is an alkenyl group having 2 to 10 carbon atoms.] Among the compounds represented by the chemical formula (13), the compound represented by the following chemical formula (14) is particularly preferred.

[0073] [ka]

[0074] [In chemical formula (14), R 15 represents a direct bond, -CH2-, -C(CH3)2-, -O-, -S-, -SO- or -SO2-.

[0075] [ka]

[0076] [In chemical formula (15), R 20 , R 21 is a direct bond, -CH2-, -C(CH3)2-, -O-, -S-, -SO- or -SO2-. 22 , R 23 , R 24 , R 25 , R 26 , R 27 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms, and preferably an allyl group or a propenyl group. 22 , R 23 , R 24 , R 25 , R 26 , R 27 At least one of them is an alkenyl group having 2 to 10 carbon atoms. P is an integer of 0 to 10.]

[0077] [ka]

[0078] [In chemical formula (16), R 15 represents a direct bond, -CH2-, -C(CH3)2-, -O-, -S-, -SO- or -SO2-. 28 , R 29 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms, and preferably an allyl group or a propenyl group. 28 , R 29 At least one of them is an alkenyl group having 2 to 10 carbon atoms.]

[0079] Examples of such alkenylphenol compounds or alkenylphenol ether compounds include O,O'-diallyl bisphenol A, 4,4'-dihydroxy-3,3'-diallyl diphenyl, bis(4-hydroxy-3-allyl phenyl)methane, 2,2'-bis(4-hydroxy-3,5-diallyl phenyl)propane, 2,2'-diallyl bisphenol F, 4,4'-dihydroxy-3,3'-diallyl diphenyl ether, 4,4'-bis-O-propenyl phenoxy-benzophenone, etc. Among these, O,O'-diallyl bisphenol A, 2,2'-bis(4-hydroxy-3,5-diallyl phenyl)propane, 2,2'-diallyl bisphenol F, etc. are preferred because the glass transition point of the resin after heat curing is high. O,O'-diallyl bisphenol A is particularly preferred because it reduces the viscosity of the present resin composition. In the present resin composition, the alkenylphenol compound and / or alkenylphenol ether may be used alone or in combination of two or more kinds.

[0080] The alkenylphenol compound and / or alkenylphenol ether compound functions as a curing agent for the bismaleimide compound. The blending amount in the present resin composition is preferably 10-70 [mass%], more preferably 20-50 [mass%], and particularly preferably 25-40 [mass%]. The present resin composition contains an alkenylphenol compound and / or an alkenylphenol ether compound appropriately within the above-mentioned predetermined range, so that the viscosity of the present resin composition can be adjusted and good molding processability can be obtained. In addition, the present resin composition can be sufficiently impregnated into the reinforcing fiber substrate, and can be sufficiently bonded to the reinforcing fiber substrate.

[0081] In the present resin composition, a part or all of the aromatic bismaleimide compound and / or the aliphatic bismaleimide compound may be dissolved in the alkenylphenol compound and / or the alkenylphenol ether compound. The present resin composition preferably contains a liquid phase component and a solid phase component, and the ratio of the solid phase component in the resin composition is preferably 5 to 50 [mass %], more preferably 15 to 45 [mass %], and particularly preferably 25 to 40 [mass %]. When the ratio of the solid phase component is in this range, the viscosity of the resin composition can be easily adjusted to an appropriate range, and voids during molding can be easily suppressed. In the present invention, the solid phase component refers to a component that exists in a solid form in the resin composition at a temperature of 80 [°C]. Among the solid phase components, the bismaleimide compound dissolves in the resin composition at a molding temperature of the prepreg formed using the present resin composition or lower. In addition, the liquid phase component refers to a component that exists in a liquid form in the resin composition at a temperature of 80 [°C].

[0082] When the ratio of the solid phase component in the resin composition exceeds 50 [mass %], the viscosity of the resin composition may become significantly high. As a result, the handling property may become significantly worse in the manufacturing process of the resin composition or the manufacturing process of the prepreg. When the ratio of the solid phase component in the resin composition is less than 5 [mass %], the bismaleimide compound is dissolved in the alkenylphenol compound and / or the alkenylphenol ether compound. Then, the curing reaction may proceed simultaneously by heating during this dissolution, and the molecular weight of the resin composition may increase, resulting in an increase in viscosity. As a result, the handling property may become significantly worse in the manufacturing process of the resin composition or the manufacturing process of the prepreg.

[0083] (4-1-5) Thermoplastic resin The resin composition preferably contains a thermoplastic resin. As the thermoplastic resin, a known thermoplastic resin can be used. Either a thermoplastic resin soluble in an alkenylphenol compound and / or an alkenylphenol ether compound (hereinafter also referred to as a "soluble thermoplastic resin") or a thermoplastic resin insoluble in an alkenylphenol compound and / or an alkenylphenol ether compound (hereinafter also referred to as an "insoluble thermoplastic resin") can be used.

[0084] In the present invention, "soluble in alkenylphenol compounds and / or alkenylphenol ether compounds" means that the resin is partially or completely soluble in the alkenylphenol compounds and / or alkenylphenol ether compounds under the temperature conditions for molding the fiber-reinforced composite material. The soluble thermoplastic resin dissolves in the resin composition by heating the resin composition during the molding process of the fiber-reinforced composite material, thereby increasing the viscosity of the resin composition. This makes it possible to prevent the resin composition from flowing during the molding process.

[0085] Examples of the soluble thermoplastic resin include polyethersulfone, polysulfone, polyetherimide, and polyimide.

[0086] When the soluble thermoplastic resin is blended, its content is preferably 0.1 to 15 [mass%], more preferably 1 to 10 [mass%]. When the content of the soluble thermoplastic resin is in this range, it becomes easy to adjust the viscosity of the resin composition to an appropriate range. When the content of the soluble thermoplastic resin is less than 0.1 [mass%], the viscosity of the resin composition does not increase sufficiently, which may cause the resin composition to flow. When the content of the soluble thermoplastic resin is more than 15 [mass%], the viscosity of the resin composition increases, which may significantly deteriorate the handling property.

[0087] The insoluble thermoplastic resin is blended in the resin composition as necessary. In the present invention, the term "thermoplastic resin insoluble in alkenylphenol compounds and / or alkenylphenol ether compounds" refers to a thermoplastic resin that is not dissolved in alkenylphenol compounds and / or alkenylphenol ether compounds at least under the temperature conditions for molding a fiber-reinforced composite material. An example of the insoluble thermoplastic resin is a polyimide resin.

[0088] When the insoluble thermoplastic resin is blended, the content is preferably 0.1 to 40 [mass%], more preferably 1 to 20 [mass%]. When the blending amount of the insoluble thermoplastic resin is within this range, the viscosity of the resin composition can be easily adjusted to an appropriate range, and it is easy to suppress voids during molding, and it is easy to obtain a fiber-reinforced composite material with excellent impact resistance. When the content of the insoluble thermoplastic resin is less than 0.1 [mass%], the viscosity of the resin composition does not increase sufficiently, which may cause the resin composition to flow. When the content of the insoluble thermoplastic resin is more than 20 [mass%], the viscosity of the resin composition may increase and the handling may be significantly deteriorated. The particle size of the insoluble thermoplastic resin is not particularly limited, but is preferably 0.1 to 100 [μm], more preferably 1 to 50 [μm].

[0089] (4-1-6) Other ingredients The resin composition may contain other components as long as they do not impair heat resistance, moldability, and toughness. Examples of other components include polymerization inhibitors, conductive particles, conductive fillers, inorganic fillers, rubber-like components, toughness imparting agents, stabilizers, mold release agents, colorants, thickeners, etc. The viscosity of the resin composition can be adjusted by adding a thickener.

[0090] (4-2) Fiber-reinforced substrate In the present prepreg, examples of the reinforcing fibers constituting the reinforcing fiber substrate include carbon fibers, glass fibers, aramid fibers, silicon carbide fibers, polyester fibers, ceramic fibers, alumina fibers, boron fibers, metal fibers, mineral fibers, rock fibers, and slag fibers. Among these reinforcing fibers, carbon fibers, glass fibers, and aramid fibers are preferred, and carbon fibers that have good specific strength and specific elastic modulus and can provide a lightweight and high-strength fiber-reinforced composite material are more preferred, and among carbon fibers, polyacrylonitrile (PAN)-based carbon fibers that have excellent tensile strength are particularly preferred.

[0091] When PAN-based carbon fibers are used as reinforcing fibers, the tensile modulus is preferably 170 to 600 [GPa], and particularly preferably 220 to 450 [GPa]. The tensile strength is 3920 [MPa] (400 kgf / mm 2 ) or more. By using such carbon fibers, the mechanical properties of the fiber-reinforced composite material can be improved.

[0092] The shape of the reinforcing fiber substrate is not limited, but a sheet-like material is preferable from the viewpoint of processability. Examples of the reinforcing fiber sheet include a sheet-like material in which a large number of reinforcing fibers are aligned in one direction, a bidirectional fabric such as a plain weave or twill weave, a multiaxial fabric, a nonwoven fabric, a mat, a knit, a braid, and a paper made from reinforcing fibers. The thickness of the reinforcing fiber sheet is preferably 0.01 to 3 [mm], and more preferably 0.1 to 1.5 [mm]. The basis weight of the reinforcing fiber sheet is 70 to 400 [g / m 2 ] is preferable, and 100 to 300 [g / m 2 ] is more preferred.

[0093] The content of the resin composition in the prepreg is preferably 20 to 60% by mass, more preferably 30 to 50% by mass, based on the total mass of the reinforcing fiber substrate and the resin composition. If the content of the resin composition is less than 20% by mass, voids may occur inside the fiber-reinforced composite material produced using the prepreg. If the content of the resin composition exceeds 60% by mass, the content of the reinforcing fibers is insufficient, and the strength of the resulting fiber-reinforced composite material is likely to decrease.

[0094] (5) Fiber-reinforced composite materials The fiber-reinforced composite material produced by the molding method of the present invention preferably has a void fraction of 1% or less, and more preferably 0.1% or less. The void ratio in the present invention means a value measured by image analysis of a cross-sectional photograph of a fiber-reinforced composite material.

[0095] Voids in fiber-reinforced composite materials occur intensively in the interlaminar portions. Therefore, the state of occurrence of voids in fiber-reinforced composite materials can be confirmed by measuring the interlaminar shear strength. The fiber-reinforced composite materials produced by the molding method of the present invention have interlaminar shear strength that is comparable to that obtained when a prepreg of the same composition is molded by the autoclave method. The reduction rate (ILSS reduction rate) is preferably 28% or less, more preferably 15% or less, more preferably 7% or less, and particularly preferably 5% or less, relative to the fiber-reinforced composite material obtained by molding the same prepreg by the autoclave method. EXAMPLES

[0096] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the examples described below.

[0097] The following materials were used for the prepreg:

[0098] [Aromatic bismaleimide compounds] BMI1100-H: BMI-1100H (product name) (N,N'-4,4'-diphenylmethane bismaleimide, manufactured by Daiwa Chemical Industry Co., Ltd.) TDAB: Compimide TDAB (trade name) (2,4-bismaleimidotoluene, manufactured by Evonik Industries AG) [Aliphatic bismaleimide compounds] BMI-TMH: BMI-TMH (product name) (1,6'-bismaleimide-(2,2,4-trimethyl)hexane, manufactured by Daiwa Chemical Industry Co., Ltd.) [Co-reactants] DABPA: DABPA (trade name) (2,2'-diallyl bisphenol A, manufactured by Daiwa Chemical Industry Co., Ltd.)

[0099] [Soluble thermoplastic resin] Ultem 1000-1000 (product name) ground material (polyetherimide, manufactured by SABIC Innovative Plastics, average particle size 15 [μm])

[0100] [Insoluble thermoplastic resin] AURUM PD450M (product name) (Polyimide, manufactured by Mitsui Chemicals, Inc.) P84 (product name) (Polyimide, manufactured by HP Polymers)

[0101] [Carbon fiber] "Tenax" (product name) IMS 65 E 23 24K 830tex (carbon fiber strand, manufactured by Teijin Limited, tensile modulus: 290 [GPa]) "Tenax" (product name) HTS 40 E 13 6K 400tex (carbon fiber strand, manufactured by Teijin Limited, tensile modulus: 240 [GPa]) "Tenax" (product name) UMS 55 F 23 12K 360tex (carbon fiber strand, manufactured by Teijin Limited, tensile modulus: 550 [GPa])

[0102] The physical properties of the fiber-reinforced composite materials were measured by the following methods.

[0103] [Void ratio] The BMI prepreg was laminated at [45° / -45° / 0° / 90°] for 5s and cured under the molding conditions shown in Table 1 to obtain a composite. The center of the composite was cut and a cross-sectional image was taken using a digital microscope VHX-5000 (Keyence Corporation). The void ratio was measured using the automatic area measurement function of the VHX-5000.

[0104] [Interlaminar shear strength] Measurement was performed in accordance with the ASTM-D2344 test method. The rate of decrease compared to Reference Example 1 was taken as the interlaminar shear strength decrease rate (ILSS decrease rate). [Compressive strength after damage (CAI)] Measurements were performed in accordance with the ASTM-D7136 and ASTM-D7137 test methods.

[0105] [Temperature-viscosity curve] Viscosity measurements of bismaleimide resin compositions were performed using a rheometer ARES-RDA manufactured by TA Instruments Co., Ltd. Using parallel plates with a diameter of 40 mm, the thickness of the resin between the parallel plates was set to 0.5 mm, and the viscosity was measured up to 200°C at a heating rate of 2°C / min under conditions of an angular velocity of 10 rad / sec. Ta, Tb, Td, and Te were read from the obtained temperature-viscosity curve. Ta: The temperature at which the resin composition has the lowest viscosity Tb: The temperature at which the viscosity of the resin composition becomes 100 [Pa s] Td: The temperature at which the viscosity of the resin composition is 50 [Pa s] (however, this temperature is lower than the temperature Ta at which the viscosity is at its minimum) Te: The temperature at which the viscosity of the resin composition becomes 15 [Pa s] (however, this temperature is lower than the temperature Ta at which the viscosity becomes minimum)

[0106] [TG-MS TIC] Thermogravimetry and mass spectrometry of the prepreg was performed using a NETZSCH TG-DSC / DTA STA 449 F1 Jupiter connected to a NETZSCH QMS mass spectrometer. Thermogravimetry and mass spectrometry were performed from room temperature to 180°C at a heating rate of 2°C / min in a He atmosphere, and Tc was read from the obtained total ion current chromatogram (TIC). Tc: Peak temperature showing the maximum peak among the peaks observed in the range of 90 to 180°C in the total ion current chromatogram (TIC) of the prepreg measured at a heating rate of 10°C / min using a thermogravimetry-mass spectrometry (TG-MS). Total ion current chromatogram (TIC): A chart that shows the sum of all ions produced in the ion source on the vertical axis and time on the horizontal axis.

[0107] Prepreg manufacturing [Production Example 1] A bismaleimide resin composition was prepared according to the composition shown in Production Example 1 in Table 1. The bismaleimide resin composition had Ta of 123°C, Tb of 63°C, Td of 70°C, and Te of 82°C. This bismaleimide resin composition was applied to a single-sided resin film with a basis weight of 50 [g / m2] using a film coater. 2 ] was applied onto a release film to obtain a resin sheet. Next, carbon fiber (IMS 65) strands were fed between the two resin sheets and aligned uniformly in one direction (carbon fiber volume content 57 [volume %], basis weight 190 [g / m 2 ]), the carbon fiber strands were formed into a sheet, which was then pressed and heated at 100[℃] using a roller to obtain a prepreg. The peak temperature (Tc) of the maximum peak among the peaks observed in the range of 90 to 180[℃] in the total ion current chromatogram (TIC) of the thermogravimetry-mass spectrometry (TG-MS) measurement of this prepreg was 135[℃].

[0108] [Production Example 2] A bismaleimide resin composition was prepared according to the composition shown in Production Example 2 in Table 1. This bismaleimide resin composition had a Ta of 125°C, a Tb of 64°C, a Td of 69°C, and a Te of 82°C. This bismaleimide resin composition was coated on one side of a resin film with a basis weight of 50 g / m2 using a film coater. 2 ] was applied onto a release film to obtain a resin sheet. Next, carbon fiber (IMS 65) strands were fed between the two resin sheets and aligned uniformly in one direction (carbon fiber volume content 57 [volume %], basis weight 190 [g / m 2 ]), the carbon fiber strands were formed into a sheet, which was then pressed and heated at 100[℃] using a roller to obtain a prepreg. The peak temperature (Tc) of the maximum peak among the peaks observed in the range of 90 to 180[℃] in the total ion current chromatogram (TIC) of the thermogravimetry-mass spectrometry (TG-MS) measurement of this prepreg was 135[℃].

[0109] [Production Example 3] A bismaleimide resin composition was prepared according to the composition shown in Production Example 3 in Table 1. This bismaleimide resin composition had a Ta of 150°C, a Tb of 60°C, a Td of 66°C, and a Te of 79°C. This bismaleimide resin composition was applied to a single-sided resin film with a basis weight of 50 g / m using a film coater. 2 ] was applied onto a release film to obtain a resin sheet. Next, carbon fiber (IMS 65) strands were fed between the two resin sheets and aligned uniformly in one direction (carbon fiber volume content 57 [volume %], basis weight 190 [g / m 2 ]), the carbon fiber strands were formed into a sheet, which was then pressed and heated at 100[℃] using a roller to obtain a prepreg. The peak temperature (Tc) of the maximum peak among the peaks observed in the range of 90 to 180[℃] in the total ion current chromatogram (TIC) of the thermogravimetry-mass spectrometry (TG-MS) measurement of this prepreg was 135[℃].

[0110] [Production Example 4] A bismaleimide resin composition was prepared according to the composition shown in Production Example 4 in Table 1. This bismaleimide resin composition had a Ta of 123°C, a Tb of 63°C, a Td of 70°C, and a Te of 82°C. This bismaleimide resin composition was coated on one side of a resin film with a basis weight of 50 g / m2 using a film coater. 2 ] was applied onto a release film to obtain a resin sheet. Next, carbon fiber (HTS 40) strands were fed between the two resin sheets and aligned uniformly in one direction (carbon fiber volume content 57 [volume %], basis weight 190 [g / m 2 ]), the carbon fiber strands were formed into a sheet, which was then pressed and heated at 100[℃] using a roller to obtain a prepreg. The peak temperature (Tc) of the maximum peak among the peaks observed in the range of 90 to 180[℃] in the total ion current chromatogram (TIC) of the thermogravimetry-mass spectrometry (TG-MS) measurement of this prepreg was 135[℃].

[0111] [Production Example 5] A bismaleimide resin composition was prepared according to the composition shown in Production Example 5 in Table 1. This bismaleimide resin composition had a Ta of 123°C, a Tb of 63°C, a Td of 70°C, and a Te of 82°C. This bismaleimide resin composition was applied to a single-sided resin film with a basis weight of 50 g / m using a film coater. 2 ] was applied onto a release film to obtain a resin sheet. Next, carbon fiber UMS55 strands were fed between two resin sheets and aligned uniformly in one direction (carbon fiber volume content 57 [volume %], basis weight 190 [g / m 2 ]), the carbon fiber strands were formed into a sheet, which was then pressed and heated at 100[℃] using a roller to obtain a prepreg. The peak temperature (Tc) of the maximum peak among the peaks observed in the range of 90 to 180[℃] in the total ion current chromatogram (TIC) of the thermogravimetry-mass spectrometry (TG-MS) measurement of this prepreg was 135[℃].

[0112] [Production Example 6] A bismaleimide resin composition was prepared according to the composition shown in Production Example 6 in Table 1. This bismaleimide resin composition had a Ta of 123°C, a Tb of 63°C, a Td of 70°C, and a Te of 82°C. This bismaleimide resin composition was applied to a single-sided resin film with a basis weight of 50 g / m using a film coater. 2 ] was applied onto a release film to obtain a resin sheet. Next, carbon fiber (IMS 65) strands were fed between the two resin sheets and aligned uniformly in one direction (carbon fiber volume content 65 [volume %], basis weight 270 [g / m 2 ]), the carbon fiber strands were formed into a sheet, which was then pressed and heated at 100[℃] using a roller to obtain a prepreg. The peak temperature (Tc) of the maximum peak among the peaks observed in the range of 90 to 180[℃] in the total ion current chromatogram (TIC) of the thermogravimetry-mass spectrometry (TG-MS) measurement of this prepreg was 135[℃].

[0113] [Reference example 1] The prepreg obtained in Production Example 1 was laminated in the manner of [45° / -45° / 0° / 90°] 5s, and cured in an autoclave at a pressure of 0.6 [MPa] and a temperature (T3) of 180 [℃] to obtain a fiber-reinforced composite material. No stepwise heating at temperatures (T1) and (T2) was performed. The void ratio of this fiber-reinforced composite material was 0.04 [%].

[0114] [Example 1, Comparative Examples 1 to 3] The prepreg obtained in Production Example 1 was laminated in the manner of [45° / -45° / 0° / 90°] 5s, and held in an autoclave under a pressure of 0.3 [MPa] for the temperature (T1) and time shown in Table 2, and then cured at a temperature (T3) of 180 [°C] to obtain a fiber-reinforced composite material. Heating at a temperature (T2) was not performed. The void fraction of this fiber-reinforced composite material and the ILSS reduction rate compared to Reference Example 1 were as shown in Table 2. Example 1, in which T1 in the first heating step satisfied the formula (1): Tb (63 [°C]) ≦ T1 (90 [°C]) ≦ Ta (123 [°C]), had almost the same performance as the fiber-reinforced composite material molded by the conventional autoclave molding method using high pressure (Reference Example 1).

[0115] [Examples 2 to 6] The prepreg obtained in Production Example 1 was laminated in the manner of [45° / -45° / 0° / 90°] for 5s, and held in an autoclave at a temperature (T1) of 90 [°C] for 60 minutes under the pressure conditions shown in Table 3, and then held at a temperature (T2) and time shown in Table 3, and cured at a temperature (T3) of 180 [°C] to obtain a fiber-reinforced composite material. The void fraction of this fiber-reinforced composite material and the ILSS reduction rate relative to Reference Example 1 were as shown in Table 3. Examples 4 to 6, which had a first heating step and a second heating step, showed better results.

[0116] [Examples 7 and 8] A fiber-reinforced composite material was obtained in the same manner as in Example 6, except that a prepreg containing a different insoluble thermoplastic resin was used. The void ratio, ILSS reduction rate and impact resistance (CAI) of this fiber-reinforced composite material compared to Reference Example 1 were as shown in Table 4. Even when the insoluble thermoplastic resin was changed, good results were maintained.

[0117] [Examples 9 and 10] A fiber-reinforced composite material was obtained in the same manner as in Example 6, except that a prepreg with a different carbon fiber brand was used. The void ratio of this fiber-reinforced composite material was as shown in Table 5. Even when the yarn brand was changed, good results were maintained.

[0118] [Comparative Example 4, Examples 11 and 12] As in Production Example 6, prepregs with a high fiber volume content were laminated in the manner of [45° / -45° / 0° / 90°] for 5s, and held in an autoclave under a pressure of 0.3 [MPa] at the temperatures (T1) and (T2) shown in Table 6 for the time shown in Table 6, and cured at a temperature (T3) of 180 [°C] to obtain a fiber-reinforced composite material. The void fraction of this fiber-reinforced composite material and the ILSS reduction rate relative to Reference Example 1 were as shown in Table 6. As the carbon fiber volume content increases, the relative amount of resin decreases, and there is a tendency for voids during molding to increase. However, it was confirmed that by adding the first heating step and the second heating step, good results were obtained even in Examples 11 and 12 with a high carbon fiber volume content.

[0119] [Table 1]

[0120] [Table 2]

[0121] [Table 3]

[0122] [Table 4]

[0123] [Table 5]

[0124] [Table 6]

Claims

1. A method for producing a composite material, comprising: a step of curing a prepreg comprising a fiber-reinforced substrate and a resin composition containing a bismaleimide resin, the prepreg containing an aromatic bismaleimide compound as the bismaleimide resin in an amount of 20 to 80% by mass relative to the total mass of the resin composition, First temperature (T 1 a first heating step in which the prepreg is held at the heating plate for 30 minutes or more to impregnate the fibers with the resin composition; First temperature (T 1 ) higher than a third temperature (T 3 ) and hardening the resin composition; A method for producing a composite material comprising the steps of: First temperature (T 1 ) satisfies the following formula (1): Tb≦T 1 ≦Ta (1) Ta: the temperature at which the resin composition exhibits the minimum viscosity Tb: the temperature at which the viscosity of the resin composition is 100 [Pa s]

2. Between the first heating step and the curing step, a second temperature (T 2 ) for 30 minutes or more, 2 2. The method for producing a composite material according to claim 1 , wherein the above formula (2) is satisfied: T 2 = Tc ± 20 [°C] ... (2) Tc: Peak temperature showing the maximum peak among the peaks observed in the range of 90 to 180 [°C] in the total ion current chromatogram (TIC) of the prepreg measured at a heating rate of 10 [°C / min] with a thermogravimetry-mass spectrometer (TG-MS).

3. First temperature (T 1 )<second temperature (T 2 )<Third temperature (T 3 3. The method for producing a composite material according to claim 2, wherein

4. The method for producing a composite material according to claim 1, wherein the pressure during molding is 0.5 MPa or less.

5. The method for producing a composite material according to claim 1, wherein the fiber-reinforced substrate is carbon fiber.

6. The resin composition comprises the following components (a) and (b): (a) component: a bismaleimide compound, (b) component: an alkenylphenol compound and / or an alkenylphenol ether compound, The method for producing a composite material according to claim 1, comprising the following as an essential component:

Citation Information

Patent Citations

  • Manufacture of prepreg for laminate and its device

    JP1993318476A

  • Thermosetting resin composition, prepreg and substrate using the same

    JP2005015552A

  • Resin composition for prepreg sheet, prepreg sheet and fiber-reinforced composite material

    JP2007297547A

  • Thermosetting bismaleimide-based resin composition, prepreg using the resin composition, and method for producing the same

    JP2014114369A

  • Allyl phenol novolak resin composition, cured product obtained by curing the same, production method of cured product, and fiber-reinforced resin molding

    JP2015117375A