Carburized steel for steel parts that exhibits excellent rolling fatigue properties in a foreign matter environment

A carburized steel with tailored chemical compositions and properties addresses the issue of reduced service life in environments with foreign substances by maintaining high hardness and austenite content, enhancing rolling fatigue properties and extending service life.

JP7563911B2Active Publication Date: 2024-10-08SANYO SPECIAL STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020130150
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-31
Publication Date
2024-10-08
Estimated Expiration
2040-07-31

AI Technical Summary

Technical Problem

Existing steels like JIS SUJ2 and SCM420 suffer from reduced service life due to surface indentations and stress concentration caused by foreign substances in lubricating oil, leading to peeling and wear, which conventional methods of surface hardening and optimizing retained austenite do not adequately address.

Method used

A carburized steel with specific chemical compositions and properties, including surface hardness of 700 Hv or more and 10-20% residual austenite, balanced by Cr, Si, and Mo content within the range of 5.8 < 6.4Si + 2.4Cr + Mo < 8.2, enhancing temper softening resistance.

Benefits of technology

The steel exhibits improved rolling fatigue properties and extended service life by preventing metal slip and crack formation in environments with foreign substances, ensuring high hardness and appropriate austenite content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563911000004
    Figure 0007563911000004
  • Figure 0007563911000005
    Figure 0007563911000005
  • Figure 0007563911000001
    Figure 0007563911000001
Patent Text Reader

Abstract

To provide a carburized steel for a steel component that suppresses softening of a texture at the generation of metal slip and exhibits excellent rolling fatigue characteristics under a foreign matter environment, by providing tempering softening resistance, in addition to appropriation of surface hardness and a residual austenite amount.SOLUTION: A carburized steel for steel components comprises chemical components, by mass%, C: 0.13 to 0.35%, Si: 0.30 to 0.85%, Mn: 0.15 to 0.35%, P:≤0.030%, S:≤0.030%, Cr: 1.60 to 2.00%, Al: 0.010 to 0.050%, N: 50 to 200 ppm, and B:≤50 ppm as main components, any one or both of Mo: 0.10 to 0.40%, Nb: 0.02 to 0.10% as selected elements, and the remainder consisting of Fe and inevitable impurities, satisfies the equation of 5.8<6.4Si+2.4Cr+Mo≤8.2, in addition, and has a surface hardness after the carburization of above 700 Hv and the surface residual austenite content of 10% to 20%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This invention 、 This relates to a carburized steel for steel parts that exhibits excellent rolling fatigue properties even in foreign object environments such as contaminated oil. [Background technology]

[0002] Traditionally, JIS steels such as SUJ2 and SCM420 have been used for rolling parts in machine structures. It is well known that reducing non-metallic inclusions in the steel, which can be the starting point for spalling, is an effective way to extend the life of these steels in clean environments. On the other hand, when these steel types are used in an environment where foreign matter such as wear powder generated by gear rubbing gets mixed into the lubricant, surface-originating spalling occurs, causing a significant shortening of the lifespan.First, a foreign matter gets caught between the rolling parts, causing an indentation on the surface of the part, and when the parts roll, stress is concentrated on the raised part of the indentation, eventually spalling originating from the surface occurs.

[0003] In environments where such foreign matter is likely to be mixed in, for example in automatic transmissions (ATs) used in automobiles, the generation of wear debris is difficult to avoid, so measures on the steel side are important in order to improve rolling fatigue properties.

[0004] It has been thought that suppressing the formation of indentations and reducing the stress concentration at the raised indentations would be effective in improving the service life. Effective measures for this include making the surface of the rolling parts harder than the foreign matter and optimizing the amount of retained austenite, and so proposals have been made focusing on these two factors.

[0005] For example, a carbonitrided bearing steel has been proposed for use in contaminated oil containing foreign matter, the composition of which is, by weight, C: 0.1 to 0.4%, Si: ≦1.0%, Mn: over 1.5 to 3%, P: ≦0.03%, S: ≦0.03%, Cr: 0.3 to 2.5%, Al: 0.005 to 0.050%, Ti: ≦0.003%, O: ≦0.0015%, N: ≦0.025%, with the balance being unavoidable impurities and Fe, and the surface hardness after carbonitriding or the subsequent secondary quenching and tempering treatment is 58HRC or more, and the amount of surface retained austenite is 20 to 50%. This carbonitrided bearing steel has an excellent rolling fatigue life in an environment containing foreign matter (see Patent Document 1).

[0006] Also, an invention has been proposed for a rolling part used in contaminated oil containing foreign matter, the rolling part being made of a steel containing 0.15-0.45% by weight C, 1.2-1.6% by weight Cr, 0.35-0.55% by weight Si, and 0.35-0.65% by weight Mn, with the balance being Fe and unavoidable impurities, and being subjected to heat treatment including carburizing so that the surface of the rolling surface has 0.9-2.0% by weight C and a surface hardness of 63 or more in Rockwell C hardness, fine spheroidal carbides are precipitated in the carburized layer, the average grain size of the spheroidal carbides is 5 μm or less and the amount thereof is 40% or less in area ratio, 70% or more of the spheroidal carbides have a grain size of 5 μm or less, and the amount of retained austenite in the carburized layer is 20-40% (see Patent Document 2). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2005-42188 A [Patent Document 2] Patent No. 3700044 Summary of the Invention [Problem to be solved by the invention]

[0008] In the inventions of the above-mentioned prior patents, the required surface hardness is obtained by specifying a higher carbon concentration on the surface or by performing carbonitriding, and in addition, the amount of retained austenite is required to be 20 to 40% or 20 to 50%. However, to obtain a more stable service life, it is not enough to simply harden the surface of the rolling parts or optimize the amount of retained austenite, because if metal slip occurs at the embossed area and the resulting frictional heat softens the structure, it will no longer be able to withstand the stress and cracks will form.

[0009] Therefore, the problem to be solved by the present invention is to provide a carburized steel for steel parts that has a hard surface for rolling parts, has an optimal amount of retained austenite, and suppresses softening when metal slip occurs by specifying the amounts of elements that have a favorable effect on temper softening resistance, thereby enabling the steel parts to exhibit excellent rolling fatigue properties even in an environment containing foreign matter. [Means for solving the problem]

[0010] The means of the present invention for solving the above problems is to specify the surface hardness and amount of retained austenite after carburizing of carburizing steel for steel parts, and further to limit the balance of the amounts of Cr, Si and Mo in order to increase the tempering softening resistance. Therefore, it is specified that the value X=6.4Si+2.4Cr+Mo in formula (1) satisfies a predetermined range (5.8 to 8.2). Moreover, the steel obtained has a surface hardness of 700Hv or more and a surface retained austenite content of 10% to 20% after carburization. In this way, the present invention has discovered that in addition to obtaining surface hardness and an appropriate amount of retained austenite, a steel with high softening resistance can be obtained by adjusting the balance of the amounts of Cr, Si and Mo.

[0011] That is, a first means for solving the problems of the present invention is a steel sheet having chemical components, in mass %, of C: 0.13 to 0.35%, Si: 0.30 to 0.85%, Mn: 0.15 to 0.35%, P: ≦0.030%, S: ≦0.030%, Cr: 1.60 to 2.00%, Al: 0.010 to 0.050%, N: 50 to 200 ppm, B: ≦50 ppm, with the balance being Fe and unavoidable impurities, 5.8<6.4Si+2.4Cr+Mo<8.2 satisfies formula (1), The carburizing steel for steel parts is characterized in that the surface hardness after carburizing is 700Hv or more and the amount of surface retained austenite is 10% to 20%. However, the mass % content of each chemical component is substituted for each element symbol in formula (1).

[0012] The second means has a chemical composition, in mass%, of C: 0.13-0.35%, Si: 0.30-0.85%, Mn: 0.15-0.35%, P: ≦0.030%, S: ≦0.030%, Cr: 1.60-2.00%, Al: 0.010-0.050%, N: 50-200 ppm, B: ≦50 ppm as main components, and further contains either or both of Mo: 0.10-0.40% and Nb: 0.02-0.10% as optional elements, with the balance being Fe and unavoidable impurities, 5.8<6.4Si+2.4Cr+Mo<8.2 satisfies formula (1), The carburizing steel for steel parts is characterized in that the surface hardness after carburizing is 700Hv or more and the amount of surface retained austenite is 10% to 20%. However, the mass % content of each chemical component is substituted for each element symbol in formula (1). Effect of the Invention

[0013] According to the means of the present invention, the carburized steel becomes a carburized steel for steel parts in which softening is suppressed even if metal slip occurs in an environment where foreign matter is mixed in, and by using this steel, it is possible to preferably obtain rolling parts with a long life.

[0014] That is, the carburized steel of the present invention has high surface hardness after carburization, an appropriate amount of retained austenite, and at the same time high resistance to softening due to tempering, thereby achieving a long service life for rolling parts in a foreign matter environment. [Brief description of the drawings]

[0015] [Figure 1] The shape and dimensions (mm) of the thrust type test specimen are shown. [Diagram 2] As one embodiment of the heat treatment pattern of the present invention, the heating rate, holding temperature, holding time, and cooling method during carburizing, quenching, and tempering are shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Before describing the embodiments of the present invention, the reasons for specifying each chemical composition of the carburized steel in the present invention will be described. The percentages shown below are by mass.

[0017] C: 0.13 to 0.35% C is an element necessary to ensure the strength of the carburized layer and core after carburizing, which is suitable for machine structural parts. If C is less than 0.13%, the effect is not sufficiently obtained, and conversely, if C exceeds 0.35%, the toughness of the core is reduced. Therefore, C is set to 0.13 to 0.35%. Preferably, C is set to 0.15 to 0.30%.

[0018] Silicon: 0.30 to 0.80% Silicon is an element necessary for deoxidization during the smelting of steel, and is an element that improves hardenability and temper softening resistance, and has the effect of suppressing strength degradation in high-temperature environments caused by heat generation due to metal sliding, etc. However, if the Si content is less than 0.25%, the deoxidizing effect is insufficient, and if the Si content exceeds 0.8%, workability is reduced. Therefore, the Si content is set to 0.25 to 0.8%. Preferably, the Si content is set to 0.35 to 0.65%.

[0019] Mn: 0.15 to 0.35% Mn is an element necessary for deoxidation during steel smelting, and also improves hardenability and increases the amount of retained austenite after carburization. If Mn is less than 0.15%, the deoxidation effect is insufficient. If Mn is more than 0.35%, the amount of retained austenite becomes excessive, resulting in a decrease in strength. Therefore, Mn is set to 0.15 to 0.35%. More preferably, Mn is set to 0.20 to 0.30%.

[0020] P:≦0.030% P is an unavoidable impurity. If the P content exceeds 0.030%, the toughness decreases due to grain boundary segregation. Therefore, the P content is set to 0.030% or less.

[0021] S:≦0.030% S is an unavoidable impurity. If the S content exceeds 0.030%, the toughness and fatigue strength decrease due to the formation of MnS. Therefore, the S content is set to 0.030% or less.

[0022] Cr: 1.60~2.00% Cr has the effect of improving strength by improving hardenability, suppressing strength loss at high temperatures by improving tempering softening resistance, and improving wear resistance. It also has the effect of preventing the loss of retained austenite by stabilizing the retained austenite. However, if the Cr content exceeds 2.00%, the material hardness increases, leading to a decrease in workability, and the formation of coarse carbides leads to a decrease in fatigue strength. In addition, if the Cr content is too high, an oxide film mainly composed of Cr is formed on the surface of the steel during carburization, inhibiting carburization. Therefore, Cr is set to 1.60 to 2.00%. Preferably, Cr is set to 1.70 to 1.90%.

[0023] Al: 0.010~0.050% Al is an element necessary for deoxidation. However, if the amount of Al is less than 0.010%, the effect is not sufficient. On the other hand, if the amount of Al added is increased beyond 0.050%, the amount of alumina-based inclusions formed in the steel increases, decreasing the fatigue strength. Therefore, the Al content is set to 0.010 to 0.050%, and more preferably, to 0.010 to 0.030%.

[0024] N: 50-200 ppm N has the effect of stabilizing austenite. If N is 50 ppm or less, this effect cannot be obtained sufficiently. On the other hand, if N is contained in excess of 200 ppm, the amount of nitrides increases, and fatigue strength decreases. Therefore, the N content is set to 50 to 200 ppm. More preferably, N is set to 50 to 150 ppm.

[0025] B:≦50 ppm B is an element that improves hardenability and also improves toughness by inhibiting the grain boundary precipitation of P. However, this effect saturates when the content exceeds 50 ppm. Therefore, B is set to 50 ppm or less.

[0026] Mo and Nb are optional additional elements, and either one or both may be contained in the present invention.

[0027] Mo: 0.10-0.40% Mo is one of the selectively added elements. It is an effective element for improving hardenability and toughness, and is also effective for improving temper softening resistance. However, excessive Mo leads to a decrease in workability and an increase in material costs. Therefore, the content is set to 0.010 to 0.040%.

[0028] Nb: 0.02 to 0.10% Nb is one of the selected elements. It forms carbonitrides with C and N, and the pinning effect refines the crystal grains, improving fatigue strength. However, if the Nb content is too high, the toughness of the steel decreases. Therefore, the content is set to 0.02 to 0.10%.

[0029] Next, the reason for limiting the surface hardness after carburization will be described. (Surface hardness after carburizing must be 700Hv or more) If the surface hardness is less than 700Hv, when rolling parts, such as bearings, are used in lubricating oil containing foreign matter, indentations that can become peeling points are likely to form on the surface of the part, and the wear resistance is reduced, shortening the life of the part. Therefore, the surface hardness is set to 700Hv or more.

[0030] The reason for limiting the amount of retained austenite on the surface after carburizing will be described below. (The amount of surface retained austenite after carburizing is 10% to 20%) If the amount of retained austenite on the surface after carburizing is less than 10%, toughness will decrease and the crack growth rate will increase, making it impossible to alleviate stress when foreign matter gets caught in the sliding parts of the parts. If the amount of retained austenite on the surface after carburizing exceeds 20%, the necessary surface hardness cannot be secured and the life of the rolling parts will be shortened. Therefore, the amount of retained austenite on the surface after carburizing is set to 10% to 20%.

[0031] 5.8<6.4Si+2.4Cr+Mo<8.2...Equation (1) By balancing the amounts of Cr, Si, and Mo within the specified range, steel with high softening resistance can be obtained. Therefore, the following is specified as formula (1): 5.8<6.4Si+2.4Cr+Mo<8.2. Note that the mass% content of each chemical component is substituted for each element symbol in formula (1). In other words, when the value of 6.4Si+2.4Cr+Mo based on the steel composition satisfies the range of more than 5.8 and less than 8.2 specified in the means of the present invention, the temper softening resistance is improved, and even if metal is generated in the indentation bulge, the occurrence of cracks can be suppressed.

[0032] Hereinafter, embodiments of the present invention will be described with reference to tables as appropriate. First, 100 kg steel ingots having the chemical compositions of components A to P shown in Table 1 were melted in a vacuum melting furnace. These steels were then hot-forged at 1250°C to form steel bars having a diameter of 64 mm, and normalized at 900°C for 4 hours to obtain the test materials.

[0033] [Table 1] The underlined parts are outside the scope of the present invention.

[0034] <Evaluation of characteristics> The properties of each test material were evaluated in terms of (1) surface hardness after carburization (measured using an Hv hardness tester), (2) the amount of surface retained austenite after carburization (test pieces were cut out after carburization and measured using an X-ray diffraction device), (3) temper softening resistance (measured using an HRC hardness tester), and (4) peeling resistance (measured using a thrust-type friction and wear tester).

[0035] (1) Surface hardness after carburizing Using each of the above test materials, thrust type test pieces were prepared as shown in Figure 1. Then, general gas carburizing was performed under the conditions shown in Figure 2, and finally, the surface was polished to prepare test pieces of the specified dimensions. When the carburized surface of the steel of the present invention was analyzed by EPMA, it was confirmed that the C concentration on the surface was 0.6% or more, indicating that the steel was sufficiently carburized. Using an Hv hardness tester, any location on the test surface of the test piece was measured five times under a load of 300 kgf, and the average value was taken as the Vickers hardness.

[0036] (2) Amount of retained austenite on the surface after carburizing After carburizing, the test surface of the thrust test piece was subjected to X-ray diffraction measurement, and the volume fraction of the retained austenite was calculated using the integrated intensity of the diffracted X-ray intensity distribution of the martensite and austenite phases.

[0037] (3) Resistance to tempering Softening resistance was evaluated by cutting 15mm blocks from the carburized test pieces. These blocks were placed in a Kanthal furnace maintained at 300℃ and held there for 10 hours. After cooling in air, the hardness was measured five times at random locations on the test piece's surface using an Hv hardness tester under a load of 300kgf. The change in hardness between the average value and the original hardness before heat treatment was used to evaluate softening resistance.

[0038] (4) Peel resistance The peeling resistance was evaluated by testing the number of cycles until peeling using a thrust-type friction and wear tester under the conditions shown in Table 2. The peeling resistance in Table 3 shows the life ratio to JIS steel SCM420, listed as comparative steel I.

[0039] As described above, the above evaluations (1) to (4) were carried out using steels having compositions A to P. The evaluation results of the steels A to H of the present invention and the comparative steels I to P are shown in Table 3.

[0040] [Table 2]

[0041] [Table 3] The underlined parts indicate that the range defined by the present invention is not met.

[0042] Steels A to H of the present invention are steels of the present invention whose chemical composition, surface hardness, amount of retained austenite, and composition satisfy the ranges of formula (1) specified by the present invention. All of these steels of the present invention have the required surface hardness and amount of retained austenite, and have sufficient resistance to temper softening, so that they have good rolling fatigue life.

[0043] Comparative steel I has the same chemical composition as JIS steel SCM420. It contains less Si and Cr than the chemical composition specified in the present invention, and the value of formula (1) does not satisfy the specified range. Because of the small amount of Si, the deoxidizing effect is insufficient, and coarse oxides are observed. In addition, because of the small amount of Cr, the tempering softening resistance is low.

[0044] Comparative steel J is a comparative steel that does not satisfy the requirements of the present invention because the C content is less than the lower limit. The core hardness was insufficient, so good peeling resistance could not be exhibited.

[0045] Comparative steel K has a Si content greater than the upper limit and does not satisfy the requirements of the present invention. Since the value of formula (1) does not fall within the range of the requirements, the temper softening resistance is low and the peeling resistance is low.

[0046] Comparative steel L has a Mn content greater than the upper limit and does not satisfy the requirements of the present invention. Because of the high Mn content, the amount of retained austenite after carburization is large and the surface hardness is low.

[0047] Comparative steel M has a Cr content higher than the upper limit and does not satisfy the requirements of the present invention. It was confirmed that a large amount of coarse carbides were formed due to the high Cr content. In addition, the surface hardness was low because the carburization was inhibited during carburization.

[0048] Comparative steel N is a comparative steel that does not satisfy the requirements of the present invention because it contains more Mo than the upper limit. Since the value of formula (1) does not satisfy the required range, the temper softening resistance is low and the peeling resistance is low.

[0049] Comparative steel O has a Nb content greater than the upper limit and does not satisfy the requirements of the present invention. It was confirmed that the Nb content was too high, resulting in the formation of too many carbonitrides.

[0050] Comparative steel P is a comparative steel that does not satisfy the requirements of the present invention because the Si and Cr contents are less than the lower limit. The Si and Cr contents are low, and the value of formula (1) does not satisfy the range of the requirements of the present invention. Because of the low Si content, the deoxidizing effect is insufficient, and coarse oxides are observed. In addition, because of the low Cr content, the tempering softening resistance is low.

[0051] From the above, it can be seen that improved spalling resistance is not necessarily achieved simply by the steel having high surface hardness and an appropriate amount of retained austenite. In addition, when the steel has the chemical composition specified in the present invention and the value of formula (1) falls within the specified range, the steel can exhibit an excellent rolling fatigue life in a foreign matter environment.

Claims

1. The chemical components are, in mass%, C: 0.13-0.35%, Si: 0.30-0.85%, Mn: 0.15-0.35%, P: ≦0.030%, S: ≦0.030%, Cr: 1.60-2.00%, Al: 0.010-0.050%, N: 50-200 ppm, B: ≦50 ppm, with the balance being Fe and unavoidable impurities; 5.8<6.4Si+2.4Cr+Mo<8.2 ... Formula (1) is satisfied, A carburized steel for steel parts that exhibits excellent rolling fatigue properties even in a foreign matter environment, characterized in that the surface hardness after carburization is 700 Hv or more and the amount of surface retained austenite is 10% to 20%. In the formula (1), the mass % content of each element is substituted for the symbol of each element.

2. In addition to the chemical composition according to claim 1, Contains one or both of the following selective elements: Mo: 0.10-0.40%; Nb: 0.02-0.10%; The balance is Fe and unavoidable impurities, 5.8<6.4Si+2.4Cr+Mo<8.2 ... Formula (1) is satisfied, A carburized steel for steel parts that exhibits excellent rolling fatigue properties even in a foreign matter environment, characterized in that the surface hardness after carburization is 700 Hv or more and the amount of surface retained austenite is 10% to 20%. In the formula (1), the mass % content of each element is substituted for the symbol of each element.

Citation Information

Patent Citations

  • Gear couple excellent in surface fatigue strength

    JP2001200348A

  • Rolling device

    JP2004076823A

  • Carbonitrided bearing steel with excellent rolling fatigue life under debris-contaminated environment

    JP2005042188A

  • Component and method for producing the same

    JP2018141217A

  • Steel for machine structural use excellent in cold workability and crystal grain coarsening characteristic

    JP2020023728A