Polyvinyl chloride-based carbon fiber reinforced composite material
By using vinyl chloride resin particles with a specific degree of polymerization and chlorinated vinyl chloride resin particles, the composite material addresses impregnation challenges, resulting in improved mechanical and thermal properties.
Patent Information
- Application Number
- JP2020135945
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-03
- Filing Date
- 2020-08-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-08-11
AI Technical Summary
Vinyl chloride resin compositions exhibit high melt viscosity and low thermal stability, making it difficult to impregnate into carbon fiber base materials, which hinders the formation of composite materials with improved mechanical properties, heat resistance, and flame retardance.
A carbon fiber reinforced composite material is developed using a matrix resin composed of vinyl chloride resin particles with a degree of polymerization of 600 or less, and chlorinated vinyl chloride resin particles with a degree of polymerization between 400 and 1000, which are impregnated into the carbon fiber base material to enhance interfacial adhesion and impregnation properties.
The composite material achieves excellent flame retardancy, durability, oil resistance, and mechanical properties such as bending strength and creep properties, while maintaining high heat resistance.
Smart Images

Figure 0007563917000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon fiber reinforced composite material in which a carbon fiber substrate is impregnated with a vinyl chloride resin composition. [Background technology]
[0002] Carbon fiber reinforced composite materials (hereinafter sometimes abbreviated as CFRP), which are made of carbon fibers and matrix resin, have high specific strength, specific elastic modulus, excellent mechanical properties, and high functional properties such as weather resistance and chemical resistance. Therefore, CFRP has attracted attention in aircraft structural members, wind turbine blades, automobile exterior panels, and general industrial applications, and the demand for it is increasing year by year.
[0003] Currently, most of the matrix resins used in CFRPs on the market are thermosetting resins such as epoxy. This is because thermosetting resins have low viscosity and high impregnation into carbon fibers. On the other hand, CFRPs that use thermosetting resins as the matrix resin have issues such as low processability and recyclability. Therefore, in recent years, due to the demand for improved impact resistance, high productivity, and interest in recycling, the use of thermoplastic resins such as polyolefins and polyamide polymer alloys as matrix resins has attracted attention.
[0004] In order to utilize the excellent properties of carbon fiber, such as light weight and mechanical strength, it is important that the carbon fiber is uniformly dispersed in the matrix resin, and from the viewpoint of improving impregnation, it is necessary that the viscosity of the resin during impregnation is low. However, thermoplastic resins generally undergo thermal decomposition under high temperature conditions, and many of them have high viscosity even in the molten state, which can easily cause problems such as insufficient resin impregnation.
[0005] On the other hand, to utilize the excellent mechanical properties of carbon fibers, it is also important that the interfacial adhesion between the carbon fibers and the matrix resin is excellent. For example, propylene-based resins have poor interfacial adhesion to carbon fibers, and it is difficult to obtain the expected mechanical properties by simply melt-kneading propylene-based resins and carbon fibers. To improve this problem, modified propylene-based resins have been developed in which maleic anhydride or the like is graft-bonded to propylene-based resins, and the addition of these resins has been attempted to improve the interfacial adhesion between propylene-based resins and carbon fibers.
[0006] Although CFRPs using thermoplastic resins such as polyolefins and polyamide-based polymer alloys as matrix resins have been put to practical use, there are still cases where the poor chemical resistance and flame retardancy performance that depend on the matrix resin remains an issue.
[0007] Meanwhile, vinyl chloride resin, which is a general-purpose thermoplastic resin, is known to be excellent in flame retardancy, durability, oil resistance, and chemical resistance, and is also extremely small in creep deformation and excellent in mechanical strength compared to ethylene-based resins and propylene-based resins. However, vinyl chloride resin has a high melt viscosity among thermoplastic resins, and in terms of the molding processing temperature, i.e., the manufacturing of CFRP, the processing temperature when impregnating carbon fiber with vinyl chloride resin is close to the thermal decomposition temperature of vinyl chloride resin, so it is expected that impregnation of carbon fiber will be difficult, and there have been no examples of its practical use yet. In fact, in Patent Document 1, vinyl chloride resin is only blended in an amount as a secondary component, and is only handled as a mixture with a thermosetting resin that dissolves vinyl chloride resin.
[0008] One solution to lower the melt viscosity of polyvinyl chloride resin is to use a polyvinyl chloride resin with a low degree of polymerization. However, it is known that polyvinyl chloride resin with a degree of polymerization below about 500 has poor mechanical properties, and generally, polyvinyl chloride resins with a degree of polymerization of 600 or more are used for injection molding, and polyvinyl chloride resins with a degree of polymerization of 800 or more are used for extrusion molding. Therefore, there is concern that CFRP using polyvinyl chloride resin with a low degree of polymerization may have problems with mechanical properties.
[0009] Furthermore, chlorinated polyvinyl chloride resin (CPVC) is known, which is made by post-chlorinating polyvinyl chloride resin with the aim of improving the heat resistance, flame retardancy, and low smoke properties of polyvinyl chloride resin. However, since chlorinated polyvinyl chloride resin has a higher melt viscosity than polyvinyl chloride resin, it is believed that impregnating carbon fiber with CPVC would be more difficult.
[0010] On the other hand, as a method for producing fiber reinforced plastics (FRP) using polyvinyl chloride resin, other means for impregnation using a resin in a high-temperature molten state as described above are known, such as a solution impregnation method in which the resin is dissolved in a solvent and impregnated, a powder impregnation method in which resin particles are impregnated in air without being melted (Patent Document 2), and a colloid impregnation method in which the resin is impregnated using a colloidal dispersion system (Patent Document 3).
[0011] Polyvinyl chloride resin is generally polymerized by aqueous suspension polymerization or emulsion polymerization, and obtained as fine particles of about 0.1 to 100 μm. Therefore, powder impregnation method or colloid impregnation method can be used. However, although there are applications for glass fiber, flax fiber, and basalt fiber, there are no reports on carbon fiber. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2017-95537 A [Patent Document 2] Japanese Patent Application Publication No. 10-58448 [Patent Document 3] JP 2017-193710 A Summary of the Invention [Problem to be solved by the invention]
[0013] As described above, vinyl chloride resin compositions have high melt viscosity and low thermal stability. Therefore, it is assumed that vinyl chloride resin compositions are difficult to impregnate into carbon fiber substrates and difficult to form composites. Among them, vinyl chloride resins with high polymerization degrees and chlorinated vinyl chloride resins are assumed to be difficult to impregnate into carbon fiber substrates, but since they are expected to improve mechanical properties, heat resistance, flame retardancy, and low smoke, CFRPs containing these resins as matrix resins are in demand.
[0014] Therefore, an object of the present invention is to provide a carbon fiber reinforced composite material containing a vinyl chloride resin as a matrix resin, which has excellent impregnation properties and interfacial adhesion with carbon fibers, and has good bending strength and heat resistance. [Means for solving the problem]
[0015] The present inventors have conducted intensive research to solve the above-mentioned problems, and have found that the above-mentioned problems can be solved by impregnating a carbon fiber substrate that has been contacted with vinyl chloride resin particles having a predetermined degree of polymerization and chlorinated vinyl chloride resin particles with a vinyl chloride resin having a predetermined degree of polymerization, and have arrived at the present invention. That is, the gist of the present invention is as follows.
[0016] [1] The following component (A), the following component (B) and / or component (C), A carbon fiber reinforced composite material comprising a carbon fiber substrate impregnated with a matrix resin comprising the above-mentioned compound. Component (A): A resin composition containing a vinyl chloride resin having a degree of polymerization of 600 or less. Component (B): PVC resin particles with a degree of polymerization of 600 or more Component (C): Chlorinated PVC resin particles with a degree of polymerization of 400 or more and less than 1,000 [2] The carbon fiber reinforced composite material according to [1], which is obtained by impregnating a carbon fiber base material that has been contacted with more than 0 parts by mass of the component (B) and / or the component (C) per 100 parts by mass of a matrix resin with the component (A). [3] The carbon fiber reinforced composite material according to [1] or [2], wherein the average particle size of each of the particles of the component (B) and the component (C) is 2 μm or less. [4] A method for producing the carbon fiber reinforced composite material according to any one of [1] to [3], A step of contacting a carbon fiber substrate with a colloidal dispersion containing more than 0 parts by mass of the component (B) and / or the component (C) relative to 100 parts by mass of a matrix resin; A step of impregnating the carbon fiber substrate contacted with the colloidal dispersion with the component (A); A method for producing a carbon fiber reinforced composite material, comprising: [5] A method for producing the carbon fiber reinforced composite material according to any one of [1] to [3], A step of contacting a carbon fiber substrate with more than 0 parts by mass of the component (B) and / or the component (C) relative to 100 parts by mass of a matrix resin; A step of impregnating the carbon fiber substrate in contact with the component (B) and / or the component (C) with the component (A); A method for producing a carbon fiber reinforced composite material, comprising: [6] A molded article made of the carbon fiber reinforced composite material according to any one of [1] to [3]. Effect of the Invention
[0017] According to the present invention, in a polyvinyl chloride-based carbon fiber reinforced composite material using a vinyl chloride-based resin as a matrix resin, by impregnating a carbon fiber substrate in which either vinyl chloride-based resin particles or chlorinated vinyl chloride-based resin particles having a predetermined degree of polymerization have been brought into contact with the carbon fiber substrate, or both of these particles are impregnated with a vinyl chloride-based resin having a predetermined degree of polymerization, it is possible to provide a polyvinyl chloride-based carbon fiber reinforced composite material which has good interfacial adhesion to and impregnation with the carbon fiber, and which is excellent in flame retardancy, durability, oil resistance, and chemical resistance as well as excellent mechanical properties such as bending strength and creep characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] <Carbon fiber reinforced composite materials> The carbon fiber reinforced composite material according to the present invention is obtained by impregnating a carbon fiber substrate with a matrix resin, and contains, as the matrix resin, component (A): a resin composition containing a vinyl chloride resin having a degree of polymerization of 600 or less, component (B): vinyl chloride resin particles having a degree of polymerization of 600 or more, and / or component (C): chlorinated polyvinyl chloride resin particles having a degree of polymerization of 400 or more and less than 1000. Each element constituting the carbon fiber reinforced composite material will be described in detail below.
[0019] <Component (A): Vinyl chloride resin composition> In the present invention, the vinyl chloride resin composition of component (A) functions as a matrix resin of a carbon fiber reinforced composite material. The vinyl chloride resin composition of component (A) contains a vinyl chloride resin as a main component. The vinyl chloride resin used in the present invention is not particularly limited, but it is necessary that the degree of polymerization is 600 or less. A vinyl chloride resin having a degree of polymerization exceeding 600 has a high melt viscosity and is difficult to impregnate into a carbon fiber substrate. From the viewpoint of achieving both the impregnation into a carbon fiber substrate and the mechanical properties of the resulting molded product, the preferable range of the degree of polymerization is 300 to 500. In this specification, the term "degree of polymerization" means the average degree of polymerization.
[0020] The vinyl chloride resin usable as component (A) of the present invention is not particularly limited, and in addition to a homopolymer of a vinyl chloride monomer, for example, (1) a copolymer of a vinyl chloride monomer and a polymerizable monomer other than a vinyl chloride monomer, (2) a graft copolymer in which a vinyl chloride monomer or a vinyl chloride resin is grafted onto a polymer other than a vinyl chloride resin, and (3) a polymer alloy in which a vinyl chloride monomer or a vinyl chloride resin is mixed with a polymer other than a vinyl chloride resin, etc. are also included. Furthermore, chlorinated vinyl chloride resins obtained by chlorinating these vinyl chloride resins are also included. These vinyl chloride resins may be used alone or in combination of two or more kinds.
[0021] (1) The polymerizable monomer in the copolymer of vinyl chloride monomer and a polymerizable monomer other than vinyl chloride monomer is not particularly limited, and examples thereof include α-olefins having 2 to 16 carbon atoms (e.g., ethylene, propylene, and butylene); vinyl esters of aliphatic carboxylic acids having 2 to 16 carbon atoms (e.g., vinyl acetate and vinyl propionate); alkyl vinyl ethers having 2 to 16 carbon atoms (e.g., butyl vinyl ether and cetyl vinyl ether); alkyl (meth)acrylates having 1 to 16 carbon atoms (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, and butyl acrylate); aryl (meth)acrylates (e.g., phenyl methacrylate); aromatic vinyls (e.g., styrene and α-substituted styrenes (e.g., α-methylstyrene)); vinyl halides (e.g., vinylidene chloride and vinylidene fluoride); and N-substituted maleimides (N-phenylmaleimide and N-cyclohexylmaleimide).
[0022] (2) Polymers that can be used to give graft copolymers with vinyl chloride monomers or vinyl chloride resins include any polymers that can be graft-polymerized with vinyl chloride monomers, regardless of whether they are homopolymers or copolymers. Examples of such polymers include copolymers of α-olefins and vinyl esters (e.g., ethylene-vinyl acetate copolymers); copolymers of α-olefins, vinyl esters, and carbon monoxide (e.g., ethylene-vinyl acetate-carbon monoxide copolymers); copolymers of α-olefins and alkyl (meth)acrylates (e.g., ethylene-methyl methacrylate copolymers and ethylene-ethyl acrylate copolymers); copolymers of α-olefins, alkyl (meth)acrylates, and carbon monoxide (e.g., ethylene-butyl acrylate-carbon monoxide copolymers); copolymers of two or more different α-olefins (e.g., ethylene-propylene copolymers); copolymers of unsaturated nitriles and dienes (e.g., acrylonitrile-butadiene copolymers); polyurethanes; and chlorinated polyolefins (e.g., chlorinated polyethylene and chlorinated polypropylene).
[0023] (3) Other polymers used as polymer alloys (including interpenetrating polymer network structures) with vinyl chloride resins are not particularly limited. For example, thermosetting resins include epoxy resins, phenolic resins, vinyl ester resins, benzoxazine resins, polyimide resins, oxetane resins, maleimide resins, unsaturated polyester resins, urea resins, and melamine resins. In addition, thermoplastic resins include, for example, chlorinated resins such as chlorinated vinyl chloride and chlorinated polyethylene, polyolefin resins such as polyethylene resins and polypropylene resins, aliphatic polyamide resins such as polyamide 66, polyamide 6, and polyamide 12, semi-aromatic polyamide resins having aromatic components as acid components, aromatic polyester resins such as polyethylene terephthalate resin (PET) and polybutylene terephthalate resin (PBT), polycarbonate resins, polystyrene resins (polystyrene resins, AS resins, ABS resins, etc.), and aliphatic polyester resins such as polylactic acid.
[0024] In the case of a polymer alloy, the blending ratio of the vinyl chloride resin to the entire matrix resin may be 1 to 95 mass%, preferably 5 to 80 mass%, and more preferably 10 to 70 mass%. By having the blending ratio of the vinyl chloride resin within the above range, effects according to the performance of the matrix resin, such as improved heat resistance, strength, impact resistance, and flame retardancy, can be obtained.
[0025] If improved heat resistance and flame retardancy compared to ordinary polyvinyl chloride resins are desired, it is advisable to select a material containing chlorinated polyvinyl chloride resin as the main component.
[0026] The vinyl chloride resin composition of component (A) contains the vinyl chloride resin as the main component, but may contain additives that are generally blended with vinyl chloride resins. Examples of various additives that may be added to component (A) include heat stabilizers, lubricants, processing aids, impact modifiers, heat resistance improvers, antioxidants, UV absorbers, antistatic agents, light stabilizers, fillers, pigments, flame retardants, and plasticizers. Only one type of additive may be used, or two or more types may be used in combination.
[0027] The heat stabilizer is not particularly limited, and examples thereof include a heat stabilizer and a heat stabilization assistant, etc. The heat stabilizer is not particularly limited, and examples thereof include an organic tin-based stabilizer, a lead-based stabilizer, a calcium-zinc-based stabilizer, a barium-zinc-based stabilizer, and a barium-cadmium-based stabilizer, etc., and an organic stabilizer is preferably used.
[0028] Examples of the organic tin stabilizer include dibutyltin mercapto, dioctyltin mercapto, dimethyltin mercapto, dibutyltin mercapto, dibutyltin maleate, dibutyltin maleate polymer, dioctyltin maleate, dioctyltin maleate polymer, dibutyltin laurate, and dibutyltin laurate polymer, etc. The above stabilizers may be used alone or in combination of two or more.
[0029] The heat stabilization assistant is not particularly limited, and examples thereof include epoxidized soybean oil, phosphoric acid ester, polyol, hydrotalcite, zeolite, etc. The heat stabilization assistant may be used alone or in combination of two or more kinds.
[0030] The lubricant includes an internal lubricant and an external lubricant. The internal lubricant is used to reduce the flow viscosity of the molten resin during molding and to prevent frictional heat generation. The internal lubricant is not particularly limited, and examples thereof include butyl stearate, lauryl alcohol, stearyl alcohol, epoxy soybean oil, glycerin monostearate, stearic acid, and bisamide. The above lubricants may be used alone or in combination of two or more.
[0031] The external lubricant is used for the purpose of increasing the sliding effect between the molten resin and the metal surface during molding. The external lubricant is not particularly limited, and examples thereof include paraffin wax, polyolefin wax, ester wax, and montanic acid wax. The above lubricants may be used alone or in combination of two or more.
[0032] The processing aid is not particularly limited, and conventionally known processing aids can be used, such as homopolymers or copolymers of alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, and butyl methacrylate, copolymers of alkyl methacrylates and alkyl acrylates such as methyl acrylate, ethyl acrylate, and butyl acrylate, copolymers of alkyl methacrylates and aromatic vinyl compounds such as styrene, α-methylstyrene, and vinyltoluene, copolymers of alkyl methacrylates and vinyl cyan compounds such as acrylonitrile and methacrylonitrile, and the like, and these can be used alone or in combination of two or more. Among these, alkyl acrylate-alkyl methacrylate copolymers having a mass average molecular weight of 100,000 to 2,000,000 can be preferably used. Specifically, n-butyl acrylate-methyl methacrylate copolymers and 2-ethylhexyl acrylate-methyl methacrylate-butyl methacrylate copolymers can be mentioned. The above processing aids may be used alone or in combination of two or more.
[0033] The impact modifier is not particularly limited, and conventionally known impact modifiers can be used without any particular limitation, and examples thereof include polybutadiene, polyisoprene, polychloroprene, chlorinated polyethylene, fluororubber, styrene-butadiene copolymer rubber, methyl methacrylate-butadiene-styrene copolymer, methyl methacrylate-butadiene-styrene graft copolymer, acrylonitrile-styrene-butadiene copolymer rubber, acrylonitrile-styrene-butadiene graft copolymer, styrene-butadiene-styrene block copolymer rubber, styrene-isoprene-styrene copolymer rubber, styrene-ethylene-butylene-styrene copolymer rubber, ethylene-propylene copolymer rubber, ethylene-propylene-diene copolymer rubber (EPDM), silicone-containing acrylic rubber, silicone / acrylic composite rubber graft copolymer, silicone rubber, etc. The impact modifier may be used alone or in combination of two or more.
[0034] The heat resistance improver is not particularly limited, and examples thereof include α-methylstyrene-based and N-phenylmaleimide-based resins, etc. The heat resistance improver may be used alone or in combination of two or more kinds.
[0035] The antioxidant is not particularly limited, and examples thereof include phenol-based antioxidants such as 4,4'-butylidenebis-(6-t-butyl-3-methylphenol), phosphite-based antioxidants such as tris(mixed mono- and di-nonylphenyl)phosphite, and thioether-based antioxidants such as distearyl thiodipropionate. Among them, phenol-based antioxidants such as 4,4'-butylidenebis-(6-t-butyl-3-methylphenol) having low high-temperature decomposition inhibition function are particularly preferred. The antioxidants may be used alone or in combination of two or more.
[0036] The ultraviolet absorbing agent is not particularly limited, and examples thereof include salicylic acid ester ultraviolet absorbing agents, benzophenone ultraviolet absorbing agents, benzotriazole ultraviolet absorbing agents, and cyanoacrylate ultraviolet absorbing agents, etc. The ultraviolet absorbing agents may be used alone or in combination of two or more kinds.
[0037] The antistatic agent is not particularly limited, and a conventionally known antistatic agent can be used, and an anionic surfactant, a cationic surfactant, a nonionic surfactant, an amphoteric surfactant, etc. can be used. Examples of the anionic surfactant include fatty acid salts, higher alcohol sulfate salts, liquid fatty oil sulfate salts, fatty amines, sulfate salts of amides, sulfonic acid salts of dibasic fatty acid esters, fatty acid amide sulfonates, alkylaryl sulfonates, formalin condensed naphthalene sulfonates, and mixtures thereof. Examples of the cationic surfactant include fatty amine salts, quaternary ammonium salts, alkylpyridinium salts, and mixtures thereof. Examples of the nonionic surfactant include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenol esters, polyoxyethylene alkyl esters, sorbitan alkyl esters, polyoxyethylene sorbitan alkyl esters, and mixtures thereof. A mixture of a nonionic surfactant and an anionic surfactant or a cationic surfactant may also be used. Examples of amphoteric surfactants include imidazoline type, higher alkylamino type (betaine type), sulfate ester, phosphate ester type, sulfonic acid type, etc. The antistatic agent may be used alone or in combination of two or more types.
[0038] The light stabilizer is not particularly limited, and examples thereof include hindered amine light stabilizers, etc. The light stabilizers may be used alone or in combination of two or more kinds.
[0039] The filler is not particularly limited, and examples thereof include inorganic fillers such as carbonates such as talc, heavy calcium carbonate, precipitated calcium carbonate, and colloidal calcium carbonate, aluminum hydroxide, magnesium hydroxide, titanium oxide, clay, mica, wollastonite, zeolite, silica, zinc oxide, magnesium oxide, carbon black, graphite, glass beads, glass fibers, carbon fibers, and metal fibers, as well as organic fibers such as polyamides, etc. The above fillers may be used alone or in combination of two or more.
[0040] The pigment is not particularly limited, and examples thereof include organic pigments and inorganic pigments. Examples of the organic pigments include azo-based organic pigments, phthalocyanine-based organic pigments, threne-based organic pigments, and dye lake-based organic pigments. Examples of the inorganic pigments include oxide-based inorganic pigments, molybdenum chromate-based inorganic pigments, sulfide-selenide-based inorganic pigments, and ferrocyanide-based inorganic pigments. The pigments may be used alone or in combination of two or more.
[0041] Examples of the flame retardant include metal hydroxides, bromine compounds, triazine ring-containing compounds, zinc compounds, phosphorus compounds, halogen-based flame retardants, silicone-based flame retardants, intumescent flame retardants, antimony oxide, and the like. These may be used alone or in combination of two or more.
[0042] The plasticizer may be added for the purpose of improving the processability during molding. The plasticizer is not particularly limited, and a conventionally known plasticizer can be used, for example, a phthalate ester plasticizer or a non-phthalate plasticizer. Examples of the phthalate ester plasticizer include dioctyl phthalate (DOP). Examples of the non-phthalate plasticizer include trimellitic acid compounds, phosphoric acid compounds, adipic acid compounds, citric acid compounds, ether compounds, polyester compounds, soybean oil compounds, cyclohexane dicarboxylate compounds, and terephthalic acid compounds. The plasticizer may be used alone or in combination of two or more.
[0043] <Component (B): PVC resin particles with a degree of polymerization of 600 or more> The carbon fiber reinforced composite material of the present invention contains, as a matrix resin impregnated into the carbon fiber substrate, either vinyl chloride resin particles having a degree of polymerization of 600 or more as component (B) or chlorinated polyvinyl chloride resin particles having a degree of polymerization of 400 or more and less than 1000 as component (C), or both. As described later, by impregnating a carbon fiber substrate in which specific vinyl chloride resin particles are in contact with carbon fibers with component (A), the mechanical properties and heat resistance of the carbon fiber reinforced composite material can be improved. That is, by having particles made of vinyl chloride resin having a degree of polymerization of 600 or more in contact with the carbon fiber surface of the carbon fiber substrate, when the resin composition of component (A) is impregnated into the carbon fiber substrate, a part of component (B) exists in the vicinity of the fiber surface of the carbon fiber substrate while maintaining the particulate form, so that the particles function as spacers between the carbon fibers, and the impregnation of the resin composition of component (A) is improved. In addition, most of the particle surface of component (B) melts and adheres to the carbon fiber surface of the carbon fiber substrate and component (A), improving the interfacial adhesion. As a result, a polyvinyl chloride-based carbon fiber reinforced composite material that is excellent in flame retardancy, durability, oil resistance, and chemical resistance, as well as mechanical properties such as bending strength and creep characteristics, can be realized. When the molecular weights of the vinyl chloride resin of component (A) and the vinyl chloride resin of component (B) are different, the presence of component (B) in the vicinity of the carbon fiber can be confirmed by measuring the surface hardness of a micro area using AFM-IR, utilizing the difference in hardness between the two. On the other hand, when the molecular weights of the vinyl chloride resin of component (A) and the vinyl chloride resin of component (B) are approximately the same, the vinyl chloride resin particles of component (B) that have been in contact with the carbon fiber substrate beforehand will be integrated with the vinyl chloride resin in component (A) when the resin composition of component (A) is impregnated into the carbon fiber substrate, and therefore the two cannot be distinguished from each other.
[0044] The vinyl chloride resin constituting the vinyl chloride resin particles of component (B) may be the same as that of component (A) described above, but it is necessary to use one with a degree of polymerization of 600 or more. The vinyl chloride resin constituting the vinyl chloride resin particles of component (B) does not include chlorinated polyvinyl chloride resins described below. The vinyl chloride resin constituting the vinyl chloride resin particles has a preferred degree of polymerization of 1500.
[0045] The vinyl chloride resin particles of component (B) preferably have an upper limit of the average particle size of 2 μm or less, more preferably 1 μm or less. The lower limit of the average particle size is preferably 0.01 μm or more, more preferably 0.1 μm or more. By using vinyl chloride resin particles having a predetermined average particle size, they are easily inserted between the carbon fibers when contacted with the carbon fiber substrate, and are easily contacted with the carbon fibers. The average particle size can be measured by a particle size distribution meter or a scanning electron microscope. The vinyl chloride resin particles having the above average particle size can be a commercially available product having a small average particle size produced by emulsion polymerization or fine suspension polymerization. Alternatively, a commercially available vinyl chloride resin may be finely pulverized using an appropriate pulverizing device to be adjusted to have the above average particle size.
[0046] <Component (C): Chlorinated PVC resin particles having a degree of polymerization of 400 or more and less than 1,000> The carbon fiber reinforced composite material of the present invention contains, as a matrix resin impregnated into the carbon fiber substrate, component (C), which is a chlorinated vinyl chloride resin particle having a degree of polymerization of 400 or more and less than 1000, instead of or in addition to the above-mentioned component (B). By impregnating a carbon fiber substrate in which chlorinated vinyl chloride resin particles having a predetermined degree of polymerization are contacted with carbon fibers with component (A), the mechanical properties and heat resistance of the carbon fiber reinforced composite material can be further improved. In addition, as with the above-mentioned vinyl chloride resin particles of component (B), by having chlorinated vinyl chloride resin particles (component (C)) having a predetermined degree of polymerization contact the carbon fiber surface of the carbon fiber substrate, when the resin composition of component (A) is impregnated into the carbon fiber substrate, a part of component (C) is present in the vicinity of the fiber surface of the carbon fiber substrate while maintaining the particulate form, so that the particles function as spacers between the carbon fibers, improving the impregnation of the resin composition of component (A). In addition, most of the particle surface of component (C) melts and adheres to the carbon fiber surface of the carbon fiber material and component (A), improving the interfacial adhesion. By utilizing the difference in the polymerization degree of the vinyl chloride resin of component (A) and component (B), the presence of component (C) in the vicinity of the carbon fiber can be confirmed by measuring the surface hardness of a micro area using AFM-IR. Even if the polymerization degrees of component (A) and component (B) are similar to that of component (C), the respective components present in the vicinity of the carbon fiber can be identified by comparing the chlorination degree by imaging Raman measurement using Raman spectroscopy.
[0047] The chlorinated vinyl chloride resin used as the particles of component (C) is a chlorinated vinyl chloride resin described in component (A). The chlorination degree of the chlorinated vinyl chloride resin is preferably 60 to 72 mass% from the viewpoint of heat resistance. The chlorine content of the chlorinated vinyl chloride resin can be measured in accordance with JIS K 7229.
[0048] The lower limit of the polymerization degree of the chlorinated vinyl chloride resin is preferably 600 or more, and the upper limit is preferably 800 or less.
[0049] The chlorinated vinyl chloride resin particles of component (C) preferably have an upper limit of the average particle size of 2 μm or less, more preferably 1 μm or less. The lower limit of the average particle size is preferably 0.01 μm or more, more preferably 0.1 μm or more. As with the vinyl chloride resin particles of component (B), by using vinyl chloride resin particles having a predetermined average particle size, when the particles are brought into contact with a carbon fiber substrate, the particles are easily inserted between the carbon fibers and easily come into contact with the carbon fibers. As with component (B), the average particle size can be measured by a particle size distribution meter or a scanning electron microscope. As the chlorinated vinyl chloride resin particles having the above average particle size, a commercially available product having a small average particle size produced by emulsion polymerization or fine suspension polymerization can be used. Alternatively, a commercially available chlorinated vinyl chloride resin may be finely pulverized using an appropriate pulverizing device to be adjusted to have the above average particle size.
[0050] [Carbon fiber base material] The carbon fiber substrate constituting the carbon fiber reinforced composite material according to the present invention will now be described. Carbon fiber is a fiber made of materials containing carbon. The concept includes both combined use with other fibers and use alone. The carbon fiber substrate is a carbon fiber fabric having carbon fiber bundles made of a plurality of carbon fibers as warp and weft bundles. The carbon fiber is a concept including short carbon fiber, long carbon fiber, and continuous carbon fiber. Short carbon fibers are carbon fibers having a fiber length of 1 mm or less. Long carbon fiber refers to carbon fiber having a fiber length of 5 cm or less. Continuous carbon fibers are carbon fibers other than short fibers and long fibers.
[0051] The material of the carbon fiber is not particularly limited, and may be carbon fiber such as PAN (polyacrylonitrile) carbon fiber and pitch carbon fiber, or may be a combination of multiple types of other fibers; metal fibers such as steel fiber; inorganic fibers such as glass fiber, ceramic fiber, and boron fiber; organic fibers such as aramid, polyester, polyethylene, nylon, vinylon, polyacetal, polyparaphenylene benzoxazole, and high-strength polypropylene; and natural fibers such as kenaf and hemp. From the viewpoint of specific strength, it is preferable that the fiber is composed only of carbon fiber.
[0052] As the carbon fibers, short carbon fibers, long carbon fibers, and continuous carbon fibers can be appropriately used, but continuous carbon fibers are preferred from the viewpoint of the mechanical properties of the resulting CFRP.
[0053] The form of the carbon fiber is not particularly limited as long as it is a continuous fiber, and examples thereof include a form in which the tow direction is aligned in one direction and held by a weft auxiliary thread, a form in which the fibers are woven in the warp and weft directions (cross), and a form in which a plurality of fiber sheets in which the fiber direction is aligned in one direction are overlapped and stitched together with an auxiliary thread so that the fiber directions are different, to form a multiaxial warp knit. Carbon fiber can be produced by each production method based on the above forms to obtain a carbon fiber substrate (B).
[0054] Each carbon fiber is generally a single fiber, and a plurality of carbon fibers are gathered to form a carbon fiber bundle. The number of carbon fibers constituting each carbon fiber bundle is preferably 1,000 to 50,000, more preferably 2,000 to 40,000, and further preferably 5,000 to 25,000.
[0055] The fiber diameter of the filament is preferably 3 μm or more, and preferably 12 μm or less. If the fiber diameter is 3 μm or more, sufficient strength is obtained, and for example, when the filament moves laterally on the surface of a roll or spool in various processing processes, it is possible to suppress breakage or fuzz accumulation. The upper limit is usually about 12 μm because it is easy to manufacture carbon fibers.
[0056] Although not particularly limited, the plurality of carbon fiber bundles are preferably in the form of a sheet. The basis weight of the carbon fiber bundle in the form of a sheet is, for example, 100 g / m 2 More than 600g / m 2 Less than 150 g / m 2 More than 500g / m 2 The weight per unit area is preferably equal to or more than the lower limit in terms of efficiency when the obtained CFRP sheet is laminated or otherwise subjected to secondary processing, and is preferably equal to or less than the upper limit in terms of ease of obtaining impregnation.
[0057] As the carbon fiber substrate, it is preferable to use carbon fiber bundles that have been previously opened (hereinafter, sometimes referred to as opened carbon fiber bundles) for the purpose of facilitating impregnation with the matrix resin. The opening step is not particularly limited, and examples thereof include a method of including spacer particles, a method of squeezing the fibers with a round bar, a method of using airflow, and a method of vibrating the fibers with ultrasonic waves. The method of including spacer particles is preferable, and by widening the inter-fiber distance in this way, even if high tension is applied to the carbon fibers in the manufacturing stage, the inter-fiber distance is already widened, so that the resin is easily impregnated. In addition, even if tension is applied to the fibers, the inter-fiber distance is unlikely to become narrow.
[0058] The spacer particles penetrate between the carbon fibers in each fiber bundle, thereby opening the carbon fiber bundle. The spacer particles that penetrate between the carbon fibers may bridge the carbon fibers. Here, "bridge" means that the spacer particles that penetrate between the carbon fibers have a structure in which they are arranged so as to bridge at least two carbon fibers. The spacer particles may be bonded to the carbon fibers via the carbon allotropes present on the particle surfaces. The carbon fibers bridge the carbon fibers and the spacer particles are bonded to the carbon fibers, making it easier to maintain the open state of the fiber bundle more firmly.
[0059] The spacer particles are not particularly limited, and may include, for example, a carbon allotrope. In the spacer particles, examples of the carbon allotrope include amorphous carbon, graphite, diamond, etc. Examples of the amorphous carbon include amorphous carbon. Among these, amorphous carbon is preferred, and amorphous carbon is more preferred.
[0060] The average particle size of the spacer particles is preferably 1 to 20 μm. By using spacer particles with a size in this range, the spacer particles can be easily inserted between the carbon fibers and the carbon fiber bundle can be more widely spread. The average particle size of the spacer particles is more preferably 2 to 20 μm, and particularly preferably 4 to 15 μm.
[0061] The total amount of spacer particles attached to the carbon fiber bundles after the fiber-spreading treatment is preferably 0.5 to 20 mass %, more preferably 1 to 10 mass %, based on the spread carbon fiber bundle. By setting the amount of attachment to the lower limit or more, the carbon fiber bundles can be appropriately spread. Also, by setting the amount of attachment to the upper limit or less, the spread carbon fiber bundles are prevented from containing more spacer particles than necessary, which would cause a decrease in mechanical properties.
[0062] The carbon fiber substrate is as described above, and for example, an appropriate carbon fiber material, shape, and basis weight can be selected. Alternatively, a woven fabric having a desired structure may be produced using commercially available carbon fiber bundles.
[0063] [Method of manufacturing carbon fiber reinforced composite materials] Next, a method for producing a carbon fiber reinforced composite material according to the present invention will be described. The method for producing a carbon fiber reinforced composite material according to one embodiment of the present invention includes contacting a carbon fiber substrate with a colloidal dispersion containing more than 0 parts by mass of the component (B) and the component (C) per 100 parts by mass of a matrix resin, and then impregnating the carbon fiber substrate to which the colloidal dispersion has been attached with the component (A).
[0064] In addition, a method for producing a carbon fiber reinforced composite material according to another embodiment of the present invention includes contacting a carbon fiber substrate with more than 0 parts by mass of the component (B) and / or the component (C) relative to 100 parts by mass of a matrix resin, and then impregnating the carbon fiber substrate contacted with the component (B) and / or the component (C) with the component (A). Each step in the method for producing a carbon fiber reinforced composite material according to the present invention will be described in detail below.
[0065] First, a carbon fiber substrate is prepared. The carbon fiber substrate is as described above, and for example, an appropriate carbon fiber material, shape, and basis weight can be selected. Alternatively, a woven fabric having a desired structure may be prepared using commercially available carbon fiber bundles.
[0066] The carbon fiber substrate used may be the carbon fiber bundle as described above, but it is preferable to use a spread carbon fiber bundle in which the carbon fibers have been spread in advance. Various methods can be considered for spreading the carbon fiber bundle, and as one example, the carbon fiber bundle may be provided with spacer particles arranged between the carbon fibers. By arranging the spacer particles between the carbon fibers, the carbon fiber bundle is spread, and the thermoplastic resin can be sufficiently impregnated into the carbon fiber fabric. In addition, air spreading may be used in which an air flow is applied to a space created by bending the fiber bundle to a certain size to spread the fibers.
[0067] Next, a predetermined colloidal dispersion is brought into contact with the carbon fiber substrate. That is, by bringing the above-mentioned colloidal dispersion of resin particles of component (B) and resin particles of component (C) into contact with the carbon fiber substrate, the resin particles penetrate between the carbon fibers, and as a result, as described later, it becomes easier to impregnate the vinyl chloride resin of component (A) into the carbon fiber substrate, and the interface adhesion is improved, and the mechanical properties are also improved. In addition, by including chlorinated vinyl chloride resin particles, the heat resistance is also improved. In this specification, "contact" refers to a state in which the carbon fiber substrate is in contact with the carbon fiber surface.
[0068] In one embodiment of the present invention, instead of using a colloidal dispersion of the resin particles of component (B) and the resin particles of component (C), the resin particles of component (B) and / or component (C) themselves may be directly contacted with the carbon fiber substrate.
[0069] The method of contacting the resin particles of the above-mentioned components (B) and / or (C) with the carbon fiber surface of the carbon fiber substrate is not particularly limited, and a known method such as spraying and contacting powdered resin particles can be adopted, but since it is easy and convenient to make the resin particles penetrate into the gaps between the carbon fibers, a method of contacting a colloidal dispersion of resin particles with the carbon fiber substrate can be preferably adopted. The colloidal dispersion can be prepared by mixing the above-mentioned components (B) and (C) with a suitable solvent containing a surfactant.
[0070] The surfactant capable of preparing the colloidal dispersion is not particularly limited, and conventionally known surfactants such as anionic surfactants, nonionic surfactants, and nonionic surfactants can be used. Examples of the anionic surfactant include alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate; alkyl sulfate ester salts such as sodium lauryl sulfate and sodium tetradecyl sulfate; sulfosuccinates such as sodium dioctyl sulfosuccinate and sodium dihexyl sulfosuccinate; fatty acid salts such as sodium laurate and potassium semi-hardened beef tallow fatty acid; ethoxy sulfate salts such as sodium polyoxyethylene lauryl ether sulfate and sodium polyoxyethylene nonyl phenyl ether sulfate; alkanesulfonates; and sodium alkyl ether phosphate esters. Examples of the nonionic surfactant include polyoxyethylene nonyl phenyl ether and polyoxyethylene sorbitan lauryl ester. Examples of nonionic surfactants include sorbitan trioleate, sorbitan monooleate, sorbitan monolaurate, polyoxyethylene alkyl ether, polyoxyethylene / polyoxypropylene alkyl ether, polyoxyethylene sorbitan fatty acid ester (trade name "Tween" series (registered trademark)), polyoxyethylene pt-octylphenyl ether (trade name "Triton" series (registered trademark)), polyoxyethylene pt-nonylphenyl ether (trade name "TritonN" series (registered trademark)), alkyl polyglucoside fatty acid diethanolamide, alkyl monoglyceryl ether, etc. These surfactants may be used alone or in combination of two or more kinds.
[0071] The prepared colloidal dispersion may be directly applied to or immersed in a carbon fiber substrate. However, it is preferable to apply a voltage to the carbon fiber substrate as a positive or negative electrode while the carbon fiber substrate is immersed in the colloidal dispersion, and to bring the colloidal particles (i.e., the resin particles of components (B) and (C)) into contact with the surface of the carbon fiber by electrophoresis.
[0072] The ratio of the resin particles of the components (B) and / or (C) in the colloidal dispersion must be more than 0 parts by mass relative to 100 parts by mass of the matrix resin. From the viewpoint of improving impregnation and mechanical properties, the lower limit of the ratio of the resin particles of the components (B) and / or (C) is preferably 0.1 parts by mass or more relative to 100 parts by mass of the matrix resin, and more preferably 1 part by mass or more. The upper limit of the ratio of the resin particles of the components (B) and / or (C) is preferably 50 parts by mass or less relative to 100 parts by mass of the matrix resin, and more preferably 20 parts by mass or less. The ratio of the resin particles of the components (B) and (C) means the ratio of the total content of the components (B) and (C) relative to 100 parts by mass of the matrix resin. In addition, even when the resin particles of the components (B) and / or (C) themselves are directly contacted with the carbon fiber substrate instead of the colloidal dispersion, the ratio of the resin particles of the components (B) and / or (C) relative to the matrix resin is the same as above.
[0073] Next, the vinyl chloride resin composition of component (A) is impregnated into the carbon fiber substrate that has been contacted with the colloidal dispersion containing the resin particles of component (B) and / or (C). As a method for impregnating with component (A), a conventionally known method can be adopted without any particular limitation. For example, the vinyl chloride resin composition can be impregnated into the carbon fiber substrate by overlapping a film made of the vinyl chloride resin composition on the carbon fiber substrate and performing heat press molding, or by performing melt extrusion molding of the vinyl chloride resin composition on the carbon fiber substrate. In addition, the vinyl chloride resin composition of component (A) can be impregnated into the carbon fiber substrate in which the resin particles of component (B) and / or (C) are directly contacted with the carbon fiber substrate in the same manner as above.
[0074] The carbon fiber reinforced composite material may be prepared by stacking a plurality of carbon fiber base materials impregnated with the vinyl chloride resin composition. In this case, by stacking the carbon fiber base materials such that the weave directions of the carbon fiber fabrics are shifted at a certain angle, a carbon fiber reinforced composite material having even greater mechanical strength can be obtained.
[0075] For the hot pressing, extrusion molding or press molding can be used, and a carbon fiber reinforced composite material having a desired shape can be obtained by using a molding die. The temperature during hot pressing can be set to a temperature at which the vinyl chloride resin composition used softens or melts or higher.
[0076] The carbon fiber reinforced composite material of the present invention obtained as described above has good bending strength. In the present invention, the bending strength of the carbon fiber reinforced composite material in a three-point bending test is preferably 400 MPa or more. If the bending strength is 400 MPa or more, it can be suitably used in applications requiring high strength, such as aircraft structural members, wind turbine blades, and automobile exterior panels. The three-point bending test is in accordance with JIS K 7074, and the radius of the jig indenter for the bending test is 5 mm, and the width of the indenter is 2 mm. The measurement is performed using a jig indenter for the bending test of a predetermined size.
[0077] The lower limit of the fiber volume fraction of the carbon fiber reinforced composite material is preferably 30% or more, more preferably 35% or more. The upper limit of the fiber volume fraction is preferably 65% or less, more preferably 60% or less. By making the carbon fiber reinforced composite material have a fiber volume fraction in the above range, it is possible to obtain a carbon fiber reinforced composite material having excellent mechanical strength. The fiber volume fraction of the carbon fiber reinforced composite material can be adjusted by the basis weight of the carbon fiber base material used and the degree of impregnation with the vinyl chloride resin composition of component (A). In this specification, the fiber volume fraction (Vf) means a value calculated by the following formula. Vf(%)=100×carbon fiber thickness(mm)÷carbon fiber reinforced composite material thickness(mm) EXAMPLES
[0078] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0079] <Preparation of a film made of the vinyl chloride resin composition as component (A)> 100 parts by mass of vinyl chloride resin (Tokuyama Sekisui Kogyo, SL-P40, degree of polymerization about 400) was mixed with 2 parts by mass of heat stabilizer (Nitto Kasei, AT5300, methyltin mercapto) and 0.5 parts by mass of lubricant (Honeywell, AC316A, oxidized polyethylene wax) in a super mixer, heated, and then cooled in a cooling mixer to obtain a vinyl chloride resin composition. The obtained vinyl chloride resin composition was formed into a film using a calendar molding machine to produce a resin film.
[0080] <Preparation of spread carbon fiber bundle> A monomer solution in which the monomer is dissolved was prepared by uniformly mixing 10 parts by mass of 1,5-dihydroxynaphthalene, 4 parts by mass of 40% by mass methylamine aqueous solution, and 8 parts by mass of formalin (formaldehyde content: 37% by mass) with 800 parts by mass of ethanol water (ethanol content: 50% by mass) as a solvent. Next, 10 parts by mass of particles made of divinylbenzene crosslinked polymer (manufactured by Sekisui Chemical Co., Ltd., product name "Micropearl SP", average particle size 10 μm) was added to the monomer solution to prepare an opening impregnation liquid.
[0081] Next, a carbon fiber fabric consisting of PAN-based carbon fiber bundles (number of carbon fibers: 3000, average diameter of carbon fibers: 7 μm, basis weight: 200 g / m 2 A carbon fiber woven fabric (0.19 mm thick, plain weave) was prepared. The carbon fiber woven fabric was immersed in the above-mentioned spread impregnation liquid, then removed, and then heated at 200°C for 2 minutes. This heating caused a polymerization reaction of the naphthoxazine resin and carbonization, producing amorphous carbon derived from the naphthoxazine resin, and a woven fabric of spread carbon fiber bundles was obtained. The total adhesion amount of organic particles and carbon allotropes in the spread carbon fiber bundles was 1 mass%.
[0082] <Preparation of component (B)> [Particle B1] A colloidal dispersion was prepared by mixing polyvinyl chloride resin particles (Kaneka, PSH-24, polymerization degree approximately 3000) and ethanol in a mass ratio of 1:1.5. Ion-exchanged water was added to the resulting colloidal dispersion so that the particle concentration was 0.0001 mass%, and the mixture was stirred. The Z-average particle diameter was measured using a particle size distribution analyzer (Malvern Panalytical, Zetasizer Nano ZS90). The Z-average particle diameter was 1480 nm.
[0083] [Particle B2] A colloidal dispersion was prepared in the same manner as above, except that PSL-31 (average degree of polymerization 940) manufactured by Kaneka was used as the vinyl chloride resin particles, and the Z-average particle diameter was measured. The Z-average particle diameter was 1710 nm.
[0084] [Particle B3] A colloidal dispersion was prepared in the same manner as above, except that Kaneka PCH-72 (average degree of polymerization: 2000) was used as the vinyl chloride resin particles, and the Z-average particle diameter was measured. The Z-average particle diameter was 1840 nm.
[0085] <Preparation of component (C)> [Particle C1] A colloidal dispersion was prepared in the same manner as above, except that chlorinated polyvinyl chloride resin (HA-53K, Tokuyama Sekisui Corporation, average polymerization degree 1000, chlorination degree 67% by mass) was used instead of the polyvinyl chloride resin particles, which was prepared by grinding chlorinated polyvinyl chloride resin in an agate mortar for 15 minutes. The Z-average particle diameter was measured. The Z-average particle diameter was 1610 nm.
[0086] [Particle C2] A colloidal dispersion was prepared in the same manner as above, except that HA-28K (average polymerization degree 700, chlorination degree 67 mass%) made by grinding chlorinated polyvinyl chloride resin in an agate mortar for 15 minutes was used as the chlorinated polyvinyl chloride resin particles, and the Z-average particle diameter was measured. The Z-average particle diameter was 1520 nm.
[0087] [Particle C3] A colloidal dispersion was prepared in the same manner as above, except that HA-05K (average polymerization degree 500, chlorination degree 67 mass%) made by grinding chlorinated polyvinyl chloride resin in an agate mortar for 5 minutes was used as the chlorinated polyvinyl chloride resin particles, and the Z-average particle diameter was measured. The Z-average particle diameter was 1470 nm.
[0088] [Example 1] A colloidal dispersion of particles B1 was applied to a spread carbon fiber bundle, and the particles B1 were brought into contact with the carbon fiber surfaces of the spread carbon fiber bundle. Next, 9 layers of the spread carbon fiber bundles contacted with the particles B1 and 10 layers of the resin film were laminated alternately, and the laminate was pressurized stepwise from 0 to 6 MPa at 200°C for a total of 15 minutes to obtain a carbon fiber reinforced composite material. The obtained carbon fiber reinforced composite material was designated as sample "Experiment 1" for property evaluation. For the “Experimental-1” sample, it was confirmed that particle B1 was in contact with the carbon fiber by measuring the surface hardness of a microscopic area using AFM-IR (Anasys Instruments, Inc., nanoIR2).
[0089] [Example 2] A carbon fiber reinforced composite material was obtained in the same manner as in Example 1, except that a colloidal dispersion of particles B2 was used instead of the colloidal dispersion of particles B1 in Example 1. The obtained carbon fiber reinforced composite material was designated as sample "Experimental-2" for evaluating physical properties. For the “Experimental-2” sample, it was confirmed that particle B2 was in contact with the carbon fiber by measuring the surface hardness of a micro-area using AFM-IR (Anasys Instruments nanoIR2).
[0090] [Example 3] A carbon fiber reinforced composite material was obtained in the same manner as in Example 1, except that a colloidal dispersion of particles C1 was used instead of the colloidal dispersion of particles B1 in Example 1. The obtained carbon fiber reinforced composite material was designated as sample "Experiment 3" for evaluating physical properties. For the "Sample-3" sample, it was confirmed that particle C1 was in contact with the carbon fiber by comparing the degree of chlorination using an imaging Raman microscope (Thermo Fisher, DXR2xi).
[0091] [Example 4] A carbon fiber reinforced composite material was obtained in the same manner as in Example 1, except that a colloidal dispersion of particles C2 was used instead of the colloidal dispersion of particles B1 in Example 1. The obtained carbon fiber reinforced composite material was designated as sample "Experimental-4" for evaluating physical properties. For the "Sample-4" sample, it was confirmed that particle C2 was in contact with the carbon fiber by comparing the degree of chlorination using an imaging Raman microscope (Thermo Fisher, DXR2xi).
[0092] [Example 5] A carbon fiber reinforced composite material was obtained in the same manner as in Example 1, except that a mixture of a colloidal dispersion of particles B1 and a colloidal dispersion of particles C1 was used instead of the colloidal dispersion of particles B1 in Example 1. The obtained carbon fiber reinforced composite material was designated as sample "Experimental-5" for evaluating physical properties. For the "Sample-5" sample, the contact of particle B1 with carbon fiber was confirmed by measuring the surface hardness of a micro area using AFM-IR (Anasys Instruments, nanoIR2). In addition, the contact of particle C1 with carbon fiber was confirmed by comparing the degree of chlorination using an imaging Raman microscope (Thermo Fisher, DXR2xi).
[0093] [Example 6] A carbon fiber reinforced composite material was obtained in the same manner as in Example 1, except that a colloidal dispersion of particles B3 was used instead of the colloidal dispersion of particles B1 in Example 1. The obtained carbon fiber reinforced composite material was designated as sample "Experimental-6" for property evaluation. For the "Experimental-6" sample, it was confirmed by measuring the surface hardness of a micro-area using AFM-IR (Anasys Instruments, Inc. nanoIR2) that particles B3 were in contact with the carbon fiber.
[0094] A carbon fiber reinforced composite material was obtained in the same manner as in Example 1, except that a colloidal dispersion of particles C3 was used instead of the colloidal dispersion of particles B1 in Example 1. The obtained carbon fiber reinforced composite material was designated as sample "Experimental-7" for property evaluation. For the "Experimental-7" sample, it was confirmed by comparing the degree of chlorination using an imaging Raman microscope (Thermo Fisher, DXR2xi) that particles C3 were in contact with the carbon fiber.
[0095] [Comparative Example 1] Except for not coating the colloidal dispersion of particles B1 on the spread fiber bundle, a carbon fiber reinforced composite material was obtained in the same manner as in Example 1. The obtained carbon fiber reinforced composite material was designated as a sample "Comparative-1" for evaluating physical properties.
[0096] [Comparative Example 2] A carbon fiber reinforced composite material was obtained in the same manner as in Example 1, except that the degree of polymerization of the resin film of component (A) was changed to 640 and the colloidal dispersion of particles B1 was not applied to the spread fiber bundle. The obtained carbon fiber reinforced composite material was designated as a sample "Comparative-2" for evaluating physical properties.
[0097] A carbon fiber reinforced composite material was obtained in the same manner as in Example 1, except that the degree of polymerization of the resin film of component (A) was changed to 800 and the colloidal dispersion of particles B1 was not applied to the spread fiber bundle. The obtained carbon fiber reinforced composite material was designated as sample "Comparative-3" for evaluating physical properties.
[0098] <Measurement of deflection temperature under load> From the samples "Experimental-1" to "Experimental-7" and "Comparison-1" to "Comparison-3", test pieces with a length (l) of 80±2 mm, a width (b) of 10±0.2 mm, and a thickness of 2±0.2 mm were used as measurement samples, with a support distance (L) of 64 mm, a flatwise surface, and a temperature range of 30 to 150°C. The deflection temperature under load of the test pieces was measured using a test machine (Yasuda Seiki Seisakusho, 148 HDPC Heat Distortion Tester) in accordance with JIS K 7191. The measurement results are shown in Table 1. In addition, heat resistance was evaluated according to the following evaluation criteria based on the deflection temperature under load. The evaluation results are shown in Table 1. ○: Deflection temperature under load is 90℃ or higher ×: Deflection temperature under load is less than 90℃
[0099] <Bending strength measurement> From samples "Experimental-1" to "Experimental-7" and "Ratio-1" to "Ratio-3", test pieces with a length (l) of 100±1 mm, width (b) of 15±0.2 mm, and thickness of 2±0.4 mm were prepared as measurement samples, and the distance between supports (L) was set to 80 mm. The test pieces were then subjected to bending strength measurement (MPa) using a testing machine (Shimadzu Corporation, AUTOGRAPH AGS-H) in accordance with JIS K 7074 using a three-point bending method. At this time, the radius of the jig indenter for the bending test was 5 mm, and the radius of the support was 2 mm. The measurement results are shown in Table 1. In addition, the mechanical properties were evaluated based on the bending strength in accordance with the following evaluation criteria. The evaluation results are shown in Table 1. ○: Bending strength is 400MPa or more ×: Bending strength is less than 400 MPa
[0100] <Calculation of fiber volume fraction (Vf)> For samples “Experimental-1” to “Experimental-7” and “Ratio-1” to “Ratio-3”, the fiber volume fraction (Vf) was calculated by the following formula. The calculated Vf (%) is shown in Table 1.
[0101] [Table 1]
[0102] As is clear from the evaluation results in Table 1, the CFRPs (Examples 1 to 7) using carbon fiber substrates in contact with polyvinyl chloride resin particles (component B) and / or chlorinated vinyl chloride resin particles (component C) have superior heat resistance and mechanical properties compared to the CFRPs (Comparative Examples 1 to 3) produced by conventional methods.
Claims
1. A carbon fiber reinforced composite material comprising a carbon fiber substrate impregnated with a matrix resin, The carbon fiber substrate is a spread carbon fiber bundle having spacer particles disposed between the carbon fibers, The matrix resin is The following component (A), the following component (B) and / or component (C), A carbon fiber reinforced composite material comprising: Component (A): A resin composition containing a vinyl chloride resin having a degree of polymerization of 600 or less. Component (B): Particles of vinyl chloride resin having a degree of polymerization of 600 or more Component (C): Chlorinated vinyl chloride resin particles having a degree of polymerization of 400 or more and less than 1,000
2. 2. The carbon fiber reinforced composite material according to claim 1, wherein the component (A) is impregnated into a carbon fiber base material that has been contacted with more than 0 parts by mass of the component (B) and / or the component (C) relative to 100 parts by mass of a matrix resin.
3. A carbon fiber reinforced composite material as described in claim 1 or 2, wherein the spacer particles contain a carbon allotrope.
4. A carbon fiber reinforced composite material described in any one of claims 1 to 3, wherein the average particle diameter of the spacer particles is 4 to 15 μm.
5. The carbon fiber reinforced composite material according to any one of claims 1 to 4, wherein the average particle size of each of the particles of the component (B) and the component (C) is 2 µm or less.
6. A method for producing the carbon fiber reinforced composite material according to any one of claims 1 to 5, comprising the steps of: A step of preparing a carbon fiber substrate comprising a spread carbon fiber bundle having spacer particles disposed between the carbon fibers; A step of contacting the carbon fiber substrate with a colloidal dispersion containing more than 0 parts by mass of the component (B) and / or the component (C) relative to 100 parts by mass of a matrix resin; A step of impregnating the carbon fiber substrate contacted with the colloidal dispersion with the component (A); A method for producing a carbon fiber reinforced composite material, comprising:
7. A method for producing the carbon fiber reinforced composite material according to any one of claims 1 to 5, comprising the steps of: A step of preparing a carbon fiber substrate comprising a spread carbon fiber bundle having spacer particles disposed between the carbon fibers; A step of contacting a carbon fiber substrate with more than 0 parts by mass of the component (B) and / or the component (C) relative to 100 parts by mass of a matrix resin; A step of impregnating the carbon fiber substrate in contact with the component (B) and / or the component (C) with the component (A); A method for producing a carbon fiber reinforced composite material, comprising:
8. A molded article comprising the carbon fiber reinforced composite material according to any one of claims 1 to 5.
Citation Information
Patent Citations
JP1975033258A
Method for producing a fiber-reinforced resin tape loop -
JP1989001524A
Sheet for stamping molding
JP1991021449A
Production of fiber-reinforced polyvinyle chloride series resin composite material
JP1991158211A
Fiber reinforced sheet and its manufacture
JP1993016138A