Foams and vehicle interior materials
A polyolefin resin foam with enhanced elongation properties, achieved through controlled crosslinking and radiation, addresses the moldability limitations of existing sheets, allowing for complex and sharp shape conformance.
Patent Information
- Application Number
- JP2020165167
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Polyolefin resin foam sheets used in vehicle interior materials lack sufficient elongation properties to conform to complex and sharp shapes, limiting their moldability in secondary processing.
A foam with an elongation at break of 500% or more in the MD direction and 300% or more in the TD direction, a gel fraction difference of 3.0% by mass or less between surface and inner layers, and a foaming ratio of 15.5 cm³/g, achieved through electronic crosslinking and controlled ionizing radiation, is developed.
The foam exhibits excellent elongation properties, enabling it to conform to complex and sharp shapes without distortion, while maintaining moldability and reducing surface unevenness.
Smart Images

Figure 0007563930000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a foam and a vehicle interior material. [Background technology]
[0002] Polyolefin-based resin foam sheets are widely used as heat insulating materials, cushioning materials, etc. For example, in the automotive field, they are used as vehicle interior materials such as ceiling materials, doors, instrument panels, etc. These vehicle interior materials are usually formed into a predetermined shape by secondary processing such as vacuum molding or compression molding using a polyolefin-based resin foam sheet as a substrate. Therefore, the polyolefin-based resin foam sheet used for vehicle interior materials needs to have moldability during secondary processing.
[0003] For example, Patent Documents 1 to 3 disclose polyolefin resin foam sheets for improving moldability. Specifically, Patent Document 1 shows that in a foam having a density of 0.036 g / cc or more and less than 0.133 g / cc, the 160°C break point elongation (%) is 150% or more, the value obtained by multiplying the break point elongation (%) by the 100% modulus (MPa) measured at 160°C is 7 or more, and the crosslinking degree is 30 to 50%. Patent Document 2 shows that the average swelling ratio of the surface layer part from the surface of the foam sheet to a depth of 0.5 mm is 10 to 28 times. Patent Document 3 shows that the crosslinking degree of the surface layer part is 5% or more higher than the crosslinking degree of the middle layer part. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2016 / 039400 [Patent Document 2] JP 2001-294699 A [Patent Document 3] International Publication No. 2016 / 052555 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, the design of vehicle interior materials has become more complex, and vehicle interior materials are required to have complex and sharp shapes. However, the polyolefin resin foam sheets described in Patent Documents 1 to 3 have insufficient elongation properties, so the foam sheets cannot conform to complex and sharp shapes. For this reason, a foam with even better elongation properties is desired.
[0006] Therefore, an object of the present invention is to provide a foam having excellent elongation properties. [Means for solving the problem]
[0007] As a result of intensive investigations, the present inventors have found that a foam having a 160°C breaking elongation of a predetermined value or more can solve the above problems, and have completed the present invention as described below. That is, the present invention provides the following [1] to [7]. [1] A foam having a 160°C breaking elongation measured in accordance with JIS K6767 of 500% or more in the MD direction and 300% or more in the TD direction. [2] The foam according to the above item [1], wherein when the regions from the surface to a depth of 0.5 mm are defined as a first surface layer and a second surface layer, respectively, and the region between the first surface layer and the second surface layer is defined as an inner layer, the absolute value of the gel fraction difference (GO-GI) between the lower of the gel fractions (GO1) and (GO2) of the first surface layer and the gel fraction (GO) of the second surface layer and the gel fraction (GI) of the inner layer is 3.0 mass% or less. [3] The foam according to the above [2], having an average gel fraction of 27.0 mass% or more. [4] The foam according to any one of the above [1] to [3], which is a polyolefin resin foam. [5] The foam according to any one of the above [1] to [4], which is obtained by foaming an electronically crosslinked foamable composition. [6] Foaming ratio is 15.5 cm 3 The foam according to any one of the above [1] to [5], wherein the foam viscosity is 1 / g or more. [7] A vehicle interior material obtained by molding the foam according to any one of the above [1] to [6]. Effect of the Invention
[0008] According to the present invention, there are provided a foam having excellent elongation properties and a vehicle interior material obtained by molding the foam. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The foam of the present invention will now be described in detail. <Foam> The foam of the present invention has a 160°C breaking elongation measured according to JIS K6767 of 500% or more in the MD direction and 300% or more in the TD direction. This makes the foam of the present invention excellent in elongation properties. In this specification, "MD" means machine direction and refers to a direction that coincides with the extrusion direction of the foam. Also, "TD" means transverse direction and refers to a direction perpendicular to MD and parallel to the foam.
[0010] (Elongation at break at 160℃) The foam of the present invention has a 160°C breaking elongation of 500% or more in the MD direction and 300% or more in the TD direction, as measured according to JIS K6767. If the foam has a 160°C breaking elongation of less than 500% in the MD direction or less than 300% in the TD direction, when the foam is molded into a complex and sharp shape, the foam may not be able to follow the complex and sharp shape. In this case, the molded foam does not have a complex and sharp shape. From this viewpoint, the foam of the present invention has a 160°C breaking elongation of preferably 600% or more in the MD direction and 305% or more in the TD direction, more preferably 700% or more in the MD direction and 310% or more in the TD direction. The foam of the present invention also has a 160°C breaking elongation of preferably 750% or less in the MD direction and 400% or less in the TD direction. When the elongation at break at 160°C is 750% or less in the MD direction and 400% or less in the TD direction, the occurrence of unevenness (pockmarks) on the surface of the foam can be suppressed. From this viewpoint, the elongation at break at 160°C of the foam of the present invention is more preferably 690% or less in the MD direction and 310% or less in the TD direction.
[0011] (Difference in gel fraction between surface layer and inner layer) On the two main surfaces of the foam of the present invention, the regions extending from the surface to 0.5 mm therefrom are designated as a first surface layer and a second surface layer, respectively, and the region between the first surface layer and the second surface layer is designated as an inner layer. In this case, the absolute value of the gel fraction difference (GO-GI) between the lower gel fraction (GO) of the gel fractions (GO1) of the first surface layer and (GO2) of the second surface layer and the gel fraction (GI) of the inner layer is preferably 3.0% by mass or less. When the absolute value of the gel fraction difference (GO-GI) is 3.0% by mass or less, a foam having a 160°C breaking elongation of 500% or more in the MD direction and 300% or more in the TD direction can be easily obtained. As a result, when the foam is molded into a complex and sharp shape, the foam can follow the complex and sharp shape. From this viewpoint, the absolute value of the gel fraction difference (GO-GI) is more preferably 2.0% by mass or less, even more preferably 1.5% by mass or less, and even more preferably 1.0% by mass or less. Since the gel fraction of the foam is preferably uniform within the foam, the lower limit of the range of the absolute value of the gel fraction difference (GO-GI) is 0% by mass or more. It is more preferable that the absolute value of the gel fraction difference between the higher of the gel fractions of the first surface layer and the second surface layer and the gel fraction of the inner layer is also within the above range.
[0012] The gel fractions of the first and second surface layers and the inner layer of the foam can be measured, for example, as follows. First, a slicer is used to cut the foam into the first surface layer, the second surface layer, and the inner layer. If the foam is too soft and difficult to cut, it may be immersed in liquid nitrogen before cutting. The gel fraction of each of the cut first surface layer, second surface layer, and inner layer is measured as follows. A test piece of about 100 mg is taken from the foam layer, and the weight A (mg) of the test piece is precisely weighed. Next, this test piece is immersed in 30 cm of xylene at 120 °C. 3 After immersing the sample in the solution for 24 hours, the insoluble matter on the screen is filtered through a 200-mesh wire screen, vacuum-dried, and the weight B (mg) of the insoluble matter is precisely weighed. The gel fraction (mass%) is calculated from the obtained value using the following formula: Gel fraction (mass%) = 100 × (B / A)
[0013] The absolute value of the gel fraction difference (GO-GI) can be reduced, for example, as follows. The absolute value of the gel fraction difference of the foam can be reduced by irradiating both sides of a foam formed into a sheet with ionizing radiation at a low accelerating voltage to electronically crosslink the foam. Details of electronic crosslinking of the foam will be described later in the section on the method for producing a foam.
[0014] When the absolute value of the gel fraction difference (GO-GI) is 3.0% by mass or less, the foam can conform to a complex and sharp shape. This is believed to be due to the following reason. When the absolute value of the gel fraction difference (GO-GI) is 3.0% by mass or less, the distortion in the cross-sectional direction of the foam is small, which is believed to enable the foam to conform to complex and sharp shapes without breaking because stress is applied evenly to the foam when it is molded.
[0015] (Average gel fraction of foam) The average gel fraction of the foam (G ave The average gel fraction (G ave When the average gel fraction (G ave ) is more preferably 30% by mass or more. From the viewpoint of increasing the breaking elongation, the average gel fraction is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 38% by mass or less. As described above, the average gel fraction (G ave ) is the value obtained by adding the gel fraction of the first surface layer, the gel fraction of the second surface layer, and the gel fraction of the inner layer and dividing the resultant value by 3.
[0016] (Difference in Gel Fraction Between First Surface Layer and Second Surface Layer) The absolute value of the gel fraction difference (GO1-GO2) between the gel fraction (GO1) of the first surface layer and the gel fraction (GO2) of the second surface layer is preferably 1.0% by mass or less. This further reduces distortion in the cross-sectional direction of the foam. This allows stress to be applied more evenly to the foam when molding the foam, making it easier for the foam to conform to a complex and sharp shape. From this perspective, the absolute value of the gel fraction difference (GO1-GO2) between the gel fraction (GO1) of the first surface layer and the gel fraction (GO2) of the second surface layer is more preferably 0.7% by mass or less, even more preferably 0.6% by mass or less, and even more preferably 0.3% by mass or less. The lower limit of the range of the absolute value of the gel fraction difference (GO1-GO2) between the gel fraction (GO1) of the first surface layer and the gel fraction (GO2) of the second surface layer is not particularly limited, but is, for example, 0% by mass or more.
[0017] (Thickness of foam) From the viewpoint of using the foam as a vehicle interior material, the thickness of the foam of the present invention is preferably more than 1 mm and not more than 8 mm, more preferably 2 to 6 mm, even more preferably 3 to 5 mm, and still more preferably 3.5 to 4.5 mm.
[0018] (Expansion ratio of foam) The foam of the present invention preferably has an expansion ratio of 15.5 cm 3 The foam of the present invention has an expansion ratio of 15.5 cm 3 When the foam has a thickness of 15.5 cm or more, the foam can be made even lighter, and this allows the weight of the vehicle interior material using the foam of the present invention to be reduced. 3 Even at a high expansion ratio of 15.5 cm / g or more, the foam can conform to complex and sharp shapes and maintains excellent moldability. Note that as the expansion ratio of a foam increases, it becomes more difficult for the foam to conform to complex and sharp shapes. Therefore, when the expansion ratio of a foam is 15.5 cm / g or more, the foam can be molded to a shape that is complex and sharp. 3 When the expansion ratio of the foam of the present invention is 17 cm / g or more, the effect of the foam of the present invention that the foam can conform to a complex and sharp shape becomes more remarkable. From this viewpoint, the expansion ratio of the foam of the present invention is more preferably 17 cm / g or more. 3 / g or more, more preferably 19 cm 3 From the viewpoint of the strength of the foam, the foaming ratio of the foam of the present invention is 25 cm 3 The expansion ratio of the foam is determined by measuring the density of the foam in accordance with JIS K7222 and calculating the reciprocal thereof.
[0019] (Polyolefin resin foam) The foam of the present invention is preferably a polyolefin-based resin foam. This makes it possible to easily produce a foam that is excellent in moldability even when the expansion ratio is increased. The polyolefin-based resin foam is, for example, a foam that contains 75% by mass or more of a polyolefin-based resin relative to the total amount of resin components.
[0020] (Polyolefin resin) Examples of polyolefin resins include polypropylene resins, polyethylene resins, olefin thermoplastic elastomers, and ethylene-α-olefin copolymer rubbers. Among these polyolefin resins, it is preferable to contain at least a polypropylene resin in order to ensure a certain mechanical strength of the foam and to ensure good moldability even at high temperatures. It is more preferable that the polyolefin resin contains a polyethylene resin in addition to the polypropylene resin in order to ensure flexibility.
[0021] <Polypropylene resin> The polypropylene-based resin is not particularly limited, and examples thereof include propylene homopolymers and copolymers of propylene and other olefins. The copolymers of propylene and other olefins may be any of block copolymers, random copolymers, and random block copolymers, but are preferably random copolymers (random polypropylene). Examples of other olefins that can be copolymerized with propylene include α-olefins such as ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, and 1-decene, and among these, ethylene is preferred. Therefore, ethylene-propylene random copolymers are more preferred.
[0022] The content of the polypropylene resin is preferably 40 to 80% by mass based on the total amount of resin constituting the foam. By making the content of the polypropylene resin 40% by mass or more, it becomes easier to ensure mechanical strength and moldability at high temperatures. Also, by making the content 80% by mass or less, it becomes easier to ensure flexibility by blending a certain amount of other resin such as a polyethylene resin. From the above viewpoint, the content of the polypropylene resin is more preferably 50 to 70% by mass.
[0023] Among polypropylene-based resins, propylene homopolymers (polypropylene homopolymers) or random polypropylenes are preferred from the viewpoint of moldability, etc. Although one type of polypropylene-based resin may be used alone or two or more types may be used in combination, it is preferable to use two or more types in combination, and it is preferable to use a combination of random polypropylene and polypropylene homopolymer from the viewpoint of moldability, mechanical strength, flexibility, etc. When random polypropylene and polypropylene homopolymer are used in combination, from the viewpoint of achieving a good balance of moldability, mechanical strength, flexibility, etc., the mass ratio of random polypropylene to polypropylene homopolymer (random / homo) is preferably 0.2 to 5, more preferably 0.5 to 4, and even more preferably 1 to 3.
[0024] The polypropylene resin preferably has a melt flow rate (hereinafter, also referred to as "MFR") at 230°C of 0.1 to 20 g / 10 min. When the MFR of the polypropylene resin is within the above range, the flowability of the resin is improved while preventing the fluidity of the resin from becoming too high, improving the processability when the foamable composition described below is processed into a foam. From these viewpoints, the MFR of the polypropylene resin is more preferably 0.3 to 15 g / 10 min, and further preferably 0.4 to 12 g / 10 min.
[0025] <Polyethylene resin> The polyolefin resin in the foam of the present invention preferably contains a polyethylene resin in addition to a polypropylene resin. This can further improve the flexibility of the foam. In addition, it can facilitate electronic crosslinking of the foamable composition by ionizing radiation. The polyethylene resin is not particularly limited, and examples thereof include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, etc., among which linear low-density polyethylene is preferred. Examples of linear low-density polyethylene include ethylene / 1-butene copolymer, ethylene / 1-hexene copolymer, ethylene / 4-methyl-1-pentene copolymer, ethylene / 1-octene copolymer, etc., among which ethylene / 1-hexene copolymer is preferred. Linear low-density polyethylene has a density of 0.880 to 0.940 g / cm 3 and preferably has a density of 0.900 to 0.930 g / cm 3 The density is measured in accordance with JIS K7112. From the viewpoints of processability and flexibility, the melt flow rate (MFR) of the polyethylene resin at 190° C. is preferably from 0.5 to 20 g / 10 min, more preferably from 1.0 to 15 g / 10 min, and even more preferably from 1.5 to 12 g / 10 min.
[0026] The content of the polyethylene resin is preferably 20 to 60% by mass based on the total amount of the resin components constituting the foam. By making the content of the polyethylene resin 20% by mass or more, flexibility can be easily ensured. Also, by making the content 60% by mass or less, a considerable amount of other resins such as polypropylene resin can be blended, making it easier to ensure the mechanical strength of the foam. From these viewpoints, the content of the polyethylene resin is more preferably 30 to 50% by mass.
[0027] Other polyolefin resins may be used as the resin component. Examples of other polyolefin resins include ethylene-α-olefin copolymer rubber, olefin thermoplastic elastomer (TPO), ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-(meth)alkyl acrylate copolymer, and modified copolymers copolymerized with maleic anhydride. In addition, the foam may contain a resin other than the polyolefin resin, such as a styrene-based thermoplastic elastomer, as long as the effect of the present invention is not impaired. The content of the resin other than the polyolefin resin is, for example, 25% by mass or less, and preferably 10% by mass or less, based on the total amount of the resin components.
[0028] <Foamable Composition> The foam of the present invention is obtained by foaming a foamable composition containing a resin component such as the polyolefin resin, and is preferably obtained by crosslinking and foaming. The foamable composition usually contains a foaming agent as an additive, and preferably contains a crosslinking assistant, an antioxidant, etc.
[0029] (foaming agent) As the foaming agent, a thermally decomposable foaming agent is used, and for example, an organic or inorganic chemical foaming agent having a decomposition temperature of about 160 to 270° C. can be used. Examples of organic blowing agents include azo compounds such as azodicarbonamide, metal azodicarboxylates (e.g., barium azodicarboxylate), and azobisisobutyronitrile; nitroso compounds such as N,N'-dinitrosopentamethylenetetramine; hydrazine derivatives such as hydrazodicarbonamide, 4,4'-oxybis(benzenesulfonylhydrazide), and toluenesulfonylhydrazide; and semicarbazide compounds such as toluenesulfonylsemicarbazide. Examples of inorganic foaming agents include ammonium carbonate, sodium carbonate, ammonium hydrogen carbonate, sodium hydrogen carbonate, ammonium nitrite, sodium borohydride, and anhydrous monosodium citrate. Among these, from the viewpoint of obtaining fine bubbles and from the viewpoints of economy and safety, azo compounds and nitroso compounds are preferred, azodicarbonamide, azobisisobutyronitrile and N,N'-dinitrosopentamethylenetetramine are more preferred, and azodicarbonamide is particularly preferred.
[0030] The amount of the thermal decomposition type foaming agent added is preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, and even more preferably 5 to 10 parts by mass, per 100 parts by mass of the resin component so that the foam can be properly foamed without bursting the cells.
[0031] (Crosslinking aid) As the crosslinking aid, a polyfunctional monomer can be used. For example, trifunctional (meth)acrylate compounds such as trimethylolpropane trimethacrylate and trimethylolpropane triacrylate, compounds having three functional groups in one molecule such as trimellitic acid triallyl ester, 1,2,4-benzenetricarboxylic acid triallyl ester, and triallyl isocyanurate, bifunctional (meth)acrylate compounds such as 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol dimethacrylate, and neopentyl glycol dimethacrylate, compounds having two functional groups in one molecule such as divinylbenzene, diallyl phthalate, diallyl terephthalate, and diallyl isophthalate, ethylvinylbenzene, lauryl methacrylate, and stearyl methacrylate can be mentioned. The crosslinking aids can be used alone or in combination of two or more. Among the above, (meth)acrylate compounds are preferred. By adding a crosslinking aid to the foamable composition, it becomes possible to crosslink the foamable composition with a small amount of ionizing radiation, and therefore it is possible to prevent scission and deterioration of each resin molecule caused by irradiation with ionizing radiation. The content of the crosslinking aid is preferably 0.2 to 20 parts by mass relative to 100 parts by mass of the resin component. If the content is 0.2 parts by mass or more, it becomes easy to adjust the crosslinking degree to a desired value when foaming the foamable composition. Also, if the content is 20 parts by weight or less, it becomes easy to control the crosslinking degree imparted to the foamable composition. The content of the crosslinking aid is more preferably 0.5 to 10 parts by mass, and further preferably 1 to 8 parts by mass relative to 100 parts by mass of the resin component.
[0032] (Antioxidants) Examples of the antioxidant include phenol-based antioxidants, sulfur-based antioxidants, phosphorus-based antioxidants, amine-based antioxidants, etc. Among these, phenol-based antioxidants and sulfur-based antioxidants are preferred, and it is more preferred to use a phenol-based antioxidant and a sulfur-based antioxidant in combination. Examples of phenol-based antioxidants include 2,6-di-tert-butyl-p-cresol, n-octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenylacrylate, and tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane. Examples of the sulfur-based antioxidants include dilauryl thiodipropionate, dimyristyl thiodipropionate, distearyl thiodipropionate, and pentaerythrityl tetrakis(3-lauryl thiopropionate). Of these phenolic antioxidants, 2,6-di-tert-butyl-p-cresol is preferred, and of these sulfur-based antioxidants, dilauryl thiodipropionate is preferred. These antioxidants may be used alone or in combination of two or more kinds. The content of the antioxidant is preferably from 0.1 to 10 parts by mass, and more preferably from 0.2 to 5 parts by mass, based on 100 parts by mass of the resin component.
[0033] In addition, the foam composition may contain additives other than those described above, such as foaming assistants such as zinc oxide, zinc stearate, urea, and triazole-based compounds, flame retardants, metal damage inhibitors, antistatic agents, stabilizers, fillers, and pigments, as necessary.
[0034] <Method of manufacturing foam> The foam of the present invention can be produced, for example, by electronically crosslinking a foamable composition containing a resin component such as a polyolefin resin and an additive such as a thermally decomposable foaming agent, and then foaming the composition.
[0035] Specifically, it is industrially advantageous to produce the foam of the present invention by a method including the following steps (1) to (3). Step (1): A step of supplying each component of a foamable composition including a polyolefin resin and a thermal decomposition type foaming agent to a kneading device, kneading the components, and then obtaining a sheet-like foamable composition. Step (2): A step of irradiating the foamable composition obtained in step (1) with ionizing radiation to electronically crosslink the foamable composition. Step (3): A step of heating the foamable composition crosslinked in step (2) to a temperature equal to or higher than the decomposition temperature of the foaming agent to foam the composition, thereby obtaining a foam. Generally, the steps (2) and (3) are carried out while the sheet-like foamable composition is being transported by roll-to-roll.
[0036] In the step (1), the foamable composition is kneaded using a kneading machine such as a Banbury mixer or a pressure kneader, and then continuously extruded using an extruder, a calendar, conveyor belt casting, or the like, to produce a sheet-like foamable composition.
[0037] The ionizing radiation used in step (2) may include α-rays, β-rays, γ-rays, and electron beams, with electron beams being preferred. Since there is a limit to the penetration depth of ionizing radiation, and irradiation only from the first surface side results in a large difference in gel fraction between the first surface layer and the inner layer and the second surface layer, it is preferable to irradiate the sheet-shaped foamable composition with ionizing radiation from both the first surface side and the second surface side. The acceleration voltage of the ionizing radiation depends on the thickness of the foamable composition to be irradiated, but for example, when the thickness is more than 1 mm and 8 mm or less, it is preferably 300 to 600 kV. By setting the acceleration voltage of the ionizing radiation to 300 kV or more, the ionizing radiation can be transmitted through the sheet-shaped foamable composition. By setting the acceleration voltage of the ionizing radiation to 600 kV or less, it is possible to suppress the decrease in the gel fraction of the surface layer due to radiation-induced oxidative deterioration and scission of the main chain of the resin molecule, and to reduce the gel fraction difference between the surface layer and the inner layer of the sheet-shaped foamable composition. From this viewpoint, the acceleration voltage of the ionizing radiation is more preferably 500 to 590 kV when the thickness is more than 1 mm and 8 mm or less. The amount of ionizing radiation to be applied may be any amount sufficient to obtain a desired degree of crosslinking, and is preferably 0.1 to 8 Mrad, more preferably 0.5 to 3 Mrad, and even more preferably 1.0 to 2.4 Mrad.
[0038] In the past, it was considered that the acceleration voltage of the ionizing radiation should be a voltage that allows the ionizing radiation to sufficiently penetrate the sheet-shaped foamable composition, and the gel fraction of the sheet-shaped foamable composition was controlled solely by the amount of ionizing radiation applied. In addition, it was previously believed that when the thickness is greater than 1 mm and less than 8 mm, an acceleration voltage of ionizing radiation of 600 kV or less does not allow the ionizing radiation to sufficiently penetrate the sheet-shaped foamable composition, which tends to cause poor appearance and makes it difficult to foam properly. For this reason, in the past, when the thickness is greater than 1 mm and less than 8 mm, in order to allow the ionizing radiation to sufficiently penetrate the sheet-shaped foamable composition, the ionizing radiation was irradiated at an acceleration voltage of 800 kV or more. However, the present inventors have found, as a result of intensive research, that even when the thickness is greater than 1 mm and less than 8 mm, the above-mentioned gel fraction difference can be reduced without causing poor appearance by irradiating the sheet-shaped foamable composition with ionizing radiation at an acceleration voltage of 300 to 600 kV, particularly preferably 500 to 590 V.
[0039] In the step (3), the temperature at which the foamable composition is heated to foam varies depending on the decomposition temperature of the thermally decomposable foaming agent used as the foaming agent, but is usually 140 to 300°C, preferably 150 to 260°C.
[0040] In step (3), the foam is preferably stretched in either MD or CD or both after or while foaming. Alternatively, step (3) may be performed after step (1) without passing through step (2). That is, the sheet-shaped foamable composition may be foamed without crosslinking.
[0041] [Laminate] The foam of the present invention may be used alone, or may be used as a laminate by laminating, for example, a sheet-like material on at least one surface. In the laminate, the sheet-like material is usually adhered to the foam. Examples of the sheet-like material include a resin sheet, a thermoplastic elastomer sheet, and a fabric. When the laminate is used as an interior material for a vehicle, various fabrics such as a polyvinyl chloride sheet, a resin sheet made of a mixed resin of polyvinyl chloride and ABS resin, a thermoplastic elastomer sheet, a woven fabric, a knitted fabric, a nonwoven fabric, leather, artificial leather, and synthetic leather are preferably used. When the laminate is molded into a molded product, these sheet-like materials are preferably arranged on the surface of the molded product. In the laminate, the sheet-like material may be provided on only one surface of the foam or on both surfaces. For example, when the laminate is used as an interior material for a vehicle, the resin sheet, thermoplastic elastomer sheet, or fabric may be laminated on one surface of the foam, and a resin sheet made of polyethylene, polypropylene, or the like may be disposed on the other surface.
[0042] [Vehicle interior materials] The vehicle interior material of the present invention is obtained by molding the foam of the present invention. In order to obtain the vehicle interior material of the present invention, the foam of the present invention may be molded as it is, or the foam of the present invention may be molded into the above-mentioned laminate and then molded. Methods for molding the foam of the present invention include stamping molding, vacuum molding, compression molding, injection molding, and the like. The vehicle interior material of the present invention is more preferably used as an automobile interior material, for example, a ceiling material, a door, an instrument panel, and the like. EXAMPLES
[0043] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0044] The methods for measuring the various physical properties and the methods for evaluating the foams are as follows. (1) Thickness The thickness of the foam was measured using a dial gauge.
[0045] (2) Density and expansion ratio The density of the foam was measured in accordance with JIS K7222. The reciprocal of the density of the foam was taken as the expansion ratio.
[0046] (3) Gel fraction The gel fractions of the first surface layer, the second surface layer and the inner layer of the foam were measured by the method described in the above specification.
[0047] (4) Elongation at break at 160℃ The 160°C breaking elongation of the foam was measured in accordance with JIS K6767.
[0048] (5) Lightweight Mass (g) and area (m 2 ) and divide the foam mass by the area to obtain the foam basis weight (g / m 2 ) was calculated. The foams were evaluated for light weight according to the following criteria. ○: The basis weight of the foam is 250 g / m 2 below ×: The basis weight of the foam is 250 g / m 2 super
[0049] (6) Pockmarks on the exterior The surface condition of the foam was examined visually and by touch, and the appearance of the foam was evaluated according to the following criteria. ◯: The surface of the foam looks smooth and is smooth when touched with the hand. △: The surface of the foam is uneven, but feels smooth when touched with the hand. ×: Irregularities are visible on the surface of the foam, and can be felt by touch.
[0050] The components used in the examples and comparative examples are as follows. (Polypropylene resin) Random PP: Ethylene-propylene random copolymer, manufactured by Japan Polypropylene Corporation, product name "Novatec EG7F", MFR = 1.3g / 10min PP homopolymer: Polypropylene homopolymer, manufactured by Japan Polypropylene Corporation, product name "Novatec PP MA3", MFR=10g / 10min (Polyethylene resin) LLDPE: Linear low-density polyethylene resin, manufactured by Dow Chemical Company, product name "2036P", MFR=2.5g / 10min (Additives) Crosslinking agent: Trimethylolpropane trimethacrylate Antioxidant 1: 2,6-di-tert-butyl-p-cresol Antioxidant 2: Dilauryl thiodipropionate Foaming agent: Azodicarbonamide
[0051] The foams of Examples 1 to 4 and Comparative Examples 1 to 5 were produced as follows. The resin components and additives shown in Table 1 were charged into a single screw extruder in the amounts shown in Table 1, melt-kneaded and extruded at a resin temperature of 190° C. to obtain a sheet-like foam composition. The foamable composition was crosslinked by irradiating both sides of the obtained sheet-like foam composition with the accelerating voltage and irradiation amount shown in Table 1. The crosslinked foamable composition was then foamed in a gas phase oven at 250°C while being stretched in MD and TD to obtain a foam. The evaluation results of the foams of each Example and Comparative Example are shown in Table 1.
[0052] [Table 1]
[0053] It was found that the foams of Examples 1 to 4 above had excellent elongation properties because they had high elongation at break at 160° C. On the other hand, it was found that the foams of Comparative Examples 1 to 5 had poor elongation properties because they had low elongation at break at 160° C.
Claims
1. The 160°C breaking elongation measured in accordance with JIS K6767 is 500% or more in the MD direction and 300% or more in the TD direction; a region from the surface to a depth of 0.5 mm is defined as a first surface layer and a second surface layer, respectively, and a region between the first surface layer and the second surface layer is defined as an inner layer, an absolute value of a gel fraction difference (GO-GI) between a lower one of a gel fraction (GO1) of the first surface layer and a gel fraction (GO2) of the second surface layer and a gel fraction (GI) of the inner layer is 3.0 mass% or less, The average gel fraction is 27.0% by mass or more, The expansion ratio is 15.5 cm 3 / g or more, Contains polyethylene resin in addition to polypropylene resin, The polyolefin resin foam is formed by using a random polypropylene and a polypropylene homopolymer in combination.
2. 2. A vehicle interior material obtained by molding the foam according to claim 1.
Citation Information
Patent Citations
Production of cross-linked olefin resin foam
JP1992213341A
Polyolefin resin composition for crosslinked foam, crosslinked polyolefin resin foam and its production
JP2000086796A
Crosslinked polyolefin-based resin foam sheet and method for producing the same
JP2001294699A
Crosslinked polyolefin-based resin foam and method for producing the same
JP2004075976A
Composite foam sheet and molded body
JP2019177664A