Reflective photomask blanks and reflective photomasks

JP7563992B2Active Publication Date: 2024-10-08TOPPAN PHOTOMASK CO LTD
View PDF -1 Cites 0 Cited by

Patent Information

Application Number
JP2021003105
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-12
Publication Date
2024-10-08
Estimated Expiration
2041-01-12

Smart Images

  • Figure 0007563992000002
    Figure 0007563992000002
  • Figure 0007563992000003
    Figure 0007563992000003
  • Figure 0007563992000004
    Figure 0007563992000004
Patent Text Reader

Abstract

To provide a reflection type photomask blank that can suppress or lighten a projection effect of a reflection type photomask for patterning transcription using light of a wavelength in an extreme-ultraviolet region as a light source, and has sufficient heat resistance in performing exposure.SOLUTION: A photomask blank is constituted to have a substrate 1, a reflective layer 2 including a multilayer film formed on the substrate 1, and an absorption layer 4 formed on the reflective layer 2. Then, the absorption layer 4 is allowed to contain indium (In) and nitrogen (N) at 50 atom% or more in total. Further, the atomic ratio (N / In) of nitrogen (N) for indium (In) in the absorption layer 4 is 0.5 or more and 1.5 or less. Furthermore, the thickness of the absorption layer 4 is 17nm or more and 45nm or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reflective photomask for use in lithography using light in the ultraviolet region as a light source, and a reflective photomask blank for producing the same. [Background technology]

[0002] In the manufacturing process of semiconductor devices, the demand for miniaturization of photolithography technology is increasing along with the miniaturization of semiconductor devices. The minimum resolution dimension of the transfer pattern in photolithography depends heavily on the wavelength of the exposure light source, and the shorter the wavelength, the smaller the minimum resolution dimension can be. For this reason, the exposure light source is being replaced from the conventional ArF excimer laser light with a wavelength of 193 nm to light in the EUV (Extreme Ultra Violet) region with a wavelength of 13.5 nm.

[0003] Light in the EUV region is absorbed at a high rate by most substances, so a reflective photomask is used as a photomask for EUV exposure (EUV mask) (see, for example, Patent Document 1). Patent Document 1 discloses an EUV photomask obtained by forming a reflective layer made of a multilayer reflective film in which molybdenum (Mo) layers and silicon (Si) layers are alternately laminated on a glass substrate, forming a light absorbing layer mainly composed of tantalum (Ta) thereon, and forming a mask pattern on this light absorbing layer.

[0004] Furthermore, as mentioned above, EUV lithography cannot use refractive optics that utilize the transmission of light, so the optical components of the exposure machine are reflective (mirrors) rather than lenses. This creates a problem in that the incident light and reflected light on the reflective photomask (EUV mask) cannot be designed to be coaxial, so EUV lithography normally employs a method in which the optical axis is tilted 6 degrees from the vertical direction of the EUV photomask, and the reflected light reflected at an angle of minus 6 degrees is guided to the semiconductor substrate.

[0005] As such, in EUV lithography, the optical axis is tilted via a mirror, which can cause the so-called "projection effect" to occur, in which the EUV light incident on the EUV mask casts a shadow of the mask pattern (patterned absorbing layer) of the EUV mask.

[0006] Current EUV mask blanks use a tantalum (Ta)-based film with a thickness of 60 to 90 nm as the light absorption layer. When performing pattern transfer exposure with an EUV mask fabricated using this mask blank, there is a possibility that contrast will decrease at the shadow edge of the mask pattern depending on the relationship between the incident direction of the EUV light and the orientation of the mask pattern. This can lead to problems such as increased line edge roughness of the transferred pattern on the semiconductor substrate and inability to form the line width to the targeted dimension, resulting in a deterioration of transfer performance.

[0007] Therefore, the light absorbing layer is being considered to be changed from tantalum (Ta) to a material with high absorbency (extinction coefficient) for EUV light. However, depending on the material used for the light absorbing layer of the reflective mask blank, it may not be able to withstand the heat generated during EUV exposure, and the formed transfer pattern (mask pattern) may not be able to be stably maintained, resulting in a deterioration in transferability. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2011-176162 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention aims to provide a reflective photomask blank and a reflective photomask that can suppress or reduce the projection effect of a reflective photomask for patterning transfer using light with a wavelength in the extreme ultraviolet region as a light source, and that has sufficient heat resistance during exposure. [Means for solving the problem]

[0010] In order to solve the above problems, a reflective photomask blank according to one embodiment of the present invention is a reflective photomask blank for producing a reflective photomask for pattern transfer using extreme ultraviolet light as a light source, comprising a substrate, a reflective layer including a multilayer film formed on the substrate, and an absorbing layer formed on the reflective layer, wherein the absorbing layer contains indium (In) and nitrogen (N) in total at 50 atomic % or more, the atomic ratio (N / In) of nitrogen (N) to indium (In) in the absorbing layer is 0.5 or more and 1.5 or less, and the layer thickness of the absorbing layer is 17 nm or more and 45 nm or less.

[0011] The absorbing layer may further contain one or more elements selected from the group consisting of tantalum (Ta), platinum (Pt), tellurium (Te), zirconium (Zr), hafnium (Hf), titanium (Ti), tungsten (W), silicon (Si), chromium (Cr), gallium (Ga), molybdenum (Mo), tin (Sn), palladium (Pd), nickel (Ni), boron (B), fluorine (F), oxygen (O), carbon (C), and hydrogen (H).

[0012] The optical element further comprises a capping layer between the reflective layer and the absorbing layer.

[0013] Furthermore, a reflective photomask according to one embodiment of the present invention is a reflective photomask for pattern transfer using extreme ultraviolet light as a light source, comprising a substrate, a reflective layer including a multilayer film formed on the substrate, and an absorbing pattern layer formed on the reflective layer, wherein the absorbing pattern layer contains a total of 50 atomic % or more of indium (In) and nitrogen (N), the atomic ratio (N / In) of nitrogen (N) to indium (In) in the absorbing pattern layer is 0.5 or more and 1.5 or less, and the layer thickness of the absorbing pattern layer is 17 nm or more and 45 nm or less.

[0014] The absorbing pattern layer may further contain one or more elements selected from the group consisting of tantalum (Ta), platinum (Pt), tellurium (Te), zirconium (Zr), hafnium (Hf), titanium (Ti), tungsten (W), silicon (Si), chromium (Cr), gallium (Ga), molybdenum (Mo), tin (Sn), palladium (Pd), nickel (Ni), boron (B), fluorine (F), oxygen (O), carbon (C) and hydrogen (H). Effect of the Invention

[0015] According to one aspect of the present invention, a reflective photomask that has improved transfer performance to a semiconductor substrate in patterning using light with a wavelength in the extreme ultraviolet region as a light source and has heat resistance during exposure can be expected. In other words, the reflective photomask blank and reflective photomask according to one aspect of the present invention suppress or reduce the projection effect of a reflective photomask for patterning transfer using light with a wavelength in the extreme ultraviolet region as a light source, and have sufficient resistance to EUV light irradiation. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a structure of a reflective photomask blank according to an embodiment. [Diagram 2] 1 is a schematic cross-sectional view showing a structure of a reflective photomask according to an embodiment. [Diagram 3] 1 is a graph showing the optical constants of various elements at the wavelength of EUV light. [Figure 4] FIG. 2 is a schematic cross-sectional view showing the structure of a reflective photomask blank according to an embodiment. [Diagram 5] 5A to 5C are schematic cross-sectional views showing a manufacturing process of a reflective photomask according to an embodiment of the present invention. [Figure 6] 5A to 5C are schematic cross-sectional views showing a manufacturing process of a reflective photomask according to an embodiment of the present invention. [Figure 7] 5A to 5C are schematic cross-sectional views showing a manufacturing process of a reflective photomask according to an embodiment of the present invention. [Figure 8] 5A to 5C are schematic cross-sectional views showing a manufacturing process of a reflective photomask according to an embodiment of the present invention. [Figure 9] FIG. 2 is a schematic plan view showing the shape of a mask pattern of an absorber layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to the embodiments shown below. In the embodiments shown below, technically preferable limitations are imposed for carrying out the present invention, but these limitations are not essential requirements for the present invention.

[0018] Fig. 1 is a schematic cross-sectional view showing the structure of a reflective photomask blank 10 according to an embodiment of the present invention. Also, Fig. 2 is a schematic cross-sectional view showing the structure of a reflective photomask 20 according to an embodiment of the present invention. Here, the reflective photomask 20 according to the embodiment of the present invention shown in Fig. 2 is formed by patterning the absorption layer 4 of the reflective photomask blank 10 according to the embodiment of the present invention shown in Fig. 1.

[0019] (Overall structure) As shown in FIG. 1, a reflective photomask blank 10 according to an embodiment of the present invention comprises a substrate 1, a reflective layer 2 formed on the substrate 1, a capping layer 3 formed on the reflective layer 2, and an absorbing layer 4 formed on the capping layer 3.

[0020] (substrate) For example, a flat Si substrate, a synthetic quartz substrate, etc. can be used for the substrate 1 according to the embodiment of the present invention. In addition, low thermal expansion glass containing titanium can be used for the substrate 1, but the present invention is not limited to these as long as the material has a small thermal expansion coefficient.

[0021] (reflective layer) The reflective layer 2 according to the embodiment of the present invention may be a multilayer reflective film made of a combination of materials having significantly different refractive indices for EUV light, as long as it reflects the EUV light (extreme ultraviolet light) that is the exposure light. The reflective layer 2 including the multilayer reflective film may be formed by repeatedly stacking layers of a combination of Mo (molybdenum) and Si (silicon), or Mo (molybdenum) and Be (beryllium), for example, for about 40 periods.

[0022] (capping layer) The capping layer 3 according to the embodiment of the present invention is made of a material that is resistant to dry etching performed when forming a transfer pattern (mask pattern) on the absorption layer 4, and functions as an etching stopper that prevents damage to the reflective layer 2 when etching the absorption layer 4. The capping layer 3 is made of, for example, Ru (ruthenium). Here, depending on the material of the reflective layer 2 and the etching conditions, the capping layer 3 may not be formed. Although not shown, a back conductive film can be formed on the surface of the substrate 1 on which the reflective layer 2 is not formed. The back conductive film is a film for fixing the reflective photomask 20 by utilizing the principle of an electrostatic chuck when the reflective photomask 20 is placed in an exposure machine.

[0023] (Absorption layer) As shown in FIG. 2, by removing a part of the absorbing layer 4 of the reflective photomask blank 10, i.e., by patterning the absorbing layer 4, an absorbing pattern (absorbing pattern layer) 41 of the reflective photomask 20 is formed. In EUV lithography, EUV light is incident at an angle and reflected by the reflective layer 2, but due to a projection effect in which the absorbing pattern 41 obstructs the light path, the transfer performance onto the wafer (semiconductor substrate) may deteriorate. This deterioration in transfer performance can be reduced by reducing the thickness of the absorbing layer 4 that absorbs EUV light. In order to reduce the thickness of the absorbing layer 4, it is preferable to use a material that is more absorbent for EUV light than conventional materials, that is, a material with a high extinction coefficient k at a wavelength of 13.5 nm.

[0024] Figure 3 is a graph showing the optical constants of each metal material for EUV light with a wavelength of 13.5 nm. The horizontal axis of Figure 3 represents the refractive index n, and the vertical axis represents the extinction coefficient k. The extinction coefficient k of tantalum (Ta), which is the main material of the conventional absorption layer 4, is 0.041. If a compound material has a larger extinction coefficient k than this, it is possible to make the thickness of the absorption layer 4 thinner than before. If the extinction coefficient k is 0.06 or more, it is possible to make the thickness of the absorption layer 4 sufficiently thin, and the projection effect can be reduced.

[0025] As shown in FIG. 3, materials that satisfy the above optical constants (nk values) include, for example, silver (Ag), platinum (Pt), indium (In), cobalt (Co), tin (Sn), nickel (Ni), and tellurium (Te). However, these metal materials have a problem that the volatility of the element halides is low and dry etching properties are poor. For this reason, even if a reflective photomask blank having an absorption layer formed of these metal materials is produced, the absorption layer pattern cannot be patterned, and as a result, the reflective photomask blank cannot be processed into a reflective photomask. Alternatively, the melting points of these metal materials are low, so that they cannot withstand the heat during the production of a reflective photomask or during EUV exposure, resulting in a reflective photomask that is poor in practical use.

[0026] In order to avoid the above-mentioned drawbacks, the absorption layer of the reflective photomask blank and reflective photomask of the present invention contains InN, which is a nitride of indium. In alone has a melting point of around 157°C, which is lower than the heat temperature during the production of a reflective photomask or during EUV exposure, and there is a problem with thermal stability. On the other hand, the melting point of an oxide InO film is sufficiently high at 800°C or higher, but by converting it into a nitride, it can be made to 1100°C or higher. This gives the InN film sufficient resistance to the heat during the production of a reflective photomask or during EUV exposure.

[0027] In addition, since the InN film is chemically stable and can be dry etched using chlorine-based gas, the reflective photomask blank can be processed into a reflective photomask. This is because the volatility of InCl3, a compound of In and chlorine (Cl), is higher than that of the highly absorbing materials other than In shown in Figure 3.

[0028] The material containing indium (In) and nitrogen (N) for forming the absorption layer 4 preferably has an atomic ratio (N / In) of nitrogen (N) to indium (In) of 0.5 or more and 1.5 or less. When the atomic ratio of indium (In) to nitrogen (N) in the material constituting the absorption layer 4 is 0.5 or more, sufficient heat resistance can be imparted. In addition, since it was confirmed that a film cannot be formed with an atomic ratio of nitrogen (N) to indium (In) exceeding 1.5, this was set as the upper limit. In addition, since the atomic ratio (N / In) is stoichiometrically stable when it is 1.0, it is more preferable that it is in the range of 0.7 to 1.2, and even more preferable that it is in the range of 0.8 to 1.0.

[0029] Furthermore, the material constituting the absorbing layer 4 preferably contains 50 atomic % or more of indium (In) and nitrogen (N) in total. This is because, although there is a possibility that both the EUV light absorbency and heat resistance may decrease if the absorbing layer 4 contains components other than indium (In) and nitrogen (N), if the components other than indium (In) and nitrogen (N) are less than 50 atomic %, the decrease in EUV light absorbency and heat resistance is very slight, and there is almost no decrease in performance as the absorbing layer 4 of the EUV mask.

[0030] Materials other than indium (In) and nitrogen (N) may be mixed, for example, with Ta, Pt, Te, Zr, Hf, Ti, W, Si, Cr, Ga, Mo, Sn, Pd, Ni, B, F, O, C, or H. In other words, the absorption layer 4 may further contain, in addition to indium (In) and nitrogen (N), one or more elements selected from the group consisting of Ta, Pt, Te, Zr, Hf, Ti, W, Si, Cr, Ga, Mo, Sn, Pd, Ni, B, F, O, C, and H.

[0031] For example, by mixing Ta, Pt, Te, Sn, Pd, and Ni into the absorbing layer 4, it is possible to provide the film (absorbing layer 4) with electrical conductivity while ensuring high absorption against EUV light. Therefore, it is possible to improve the inspectability in the mask pattern inspection using DUV (Deep Ultra Violet) light with a wavelength of 190 to 260 nm. Alternatively, when Ga, Hf, Zr, Mo, Cr, and F are mixed into the absorbing layer 4, it is possible to make the film more amorphous. Therefore, it is possible to improve the roughness and in-plane dimensional uniformity of the absorbing layer pattern (mask pattern) after dry etching, or the in-plane uniformity of the transferred image. Also, when Ti, W, and Si are mixed into the absorbing layer 4, it is possible to improve the resistance to cleaning.

[0032] Furthermore, the content of one or more elements selected from the group consisting of Ta, Pt, Te, Zr, Hf, Ti, W, Si, Cr, Ga, Mo, Sn, Pd, Ni, B, F, O, C, and H in the absorption layer 4 and the absorption pattern layer 41 is more preferably in the range of 5 atomic % or more and 35 atomic % or less, and even more preferably in the range of 10 atomic % or more and 30 atomic % or less, relative to the total number of atoms constituting the absorption layer 4 or the total number of atoms constituting the absorption pattern layer 41.

[0033] 1 and 2 show a single-layer absorbent layer 4, the absorbent layer 4 according to the embodiment of the present invention is not limited thereto. The absorbent layer 4 according to the embodiment of the present invention may be, for example, one or more absorbent layers, i.e., a multi-layer absorbent layer.

[0034] As described above, a compound material mainly composed of Ta has been applied to the absorption layer 4 of the conventional EUV reflective photomask. In this case, in order to obtain an optical density OD (Equation 1), which is an index showing the contrast of the light intensity between the absorption layer 4 and the reflection layer 2, of 1 or more, the thickness of the absorption layer 4 needs to be 40 nm or more, and in order to obtain an OD of 2 or more, the thickness of the absorption layer 4 needs to be 70 nm or more. The extinction coefficient k of Ta is 0.041, but by applying a compound material containing indium (In) and nitrogen (N) with an extinction coefficient k of 0.06 or more to the absorption layer 4, according to Beer's law, it is possible to thin the thickness of the absorption layer 4 to 17 nm if the OD is at least 1 or more, and to reduce the thickness of the absorption layer 4 to 45 nm or less if the OD is 2 or more. However, if the thickness of the absorption layer 4 exceeds 45 nm, the projection effect becomes the same as that of a conventional absorption layer 4 with a thickness of 60 nm formed of a compound material mainly composed of Ta. OD = -log(Ra / Rm) (Equation 1)

[0035] Therefore, the thickness of the absorption layer 4 according to the embodiment of the present invention is preferably 17 nm or more and 45 nm or less. In other words, when the thickness of the absorption layer 4 is within the range of 17 nm or more and 45 nm or less, the projection effect can be sufficiently reduced and the transfer performance is improved compared to the conventional absorption layer 4 formed of a compound material mainly composed of Ta. Note that the optical density (OD) value is the contrast between the absorption layer 4 and the reflective layer 2, and when the OD value is less than 1, sufficient contrast cannot be obtained and the transfer performance tends to decrease. The above-mentioned "main component" refers to a component that is contained in an amount of 50 atomic % or more relative to the number of atoms in the entire absorbing layer.

[0036] Examples of the reflective photomask blank and the reflective photomask according to the present invention will be described below.

[0037] [Example 1] First, a method for producing the reflective photomask blank 10 will be described with reference to FIG. In Example 1, first, as shown in FIG. 4, a synthetic quartz substrate 11 having low thermal expansion characteristics was prepared. Then, a reflective layer 12 was formed on the prepared substrate 11 by stacking 40 laminated films each including a pair of silicon (Si) and molybdenum (Mo). The thickness of the reflective layer 12 was set to 280 nm. Then, a capping layer 13 was formed as an intermediate film on the formed reflective layer 12. Ruthenium (Ru) was used as the material of the capping layer 13. The thickness of the capping layer 13 was set to 3.5 nm.

[0038] Next, an absorption layer 14 containing indium (In) and nitrogen (N) in a total of 100 atomic % was formed on the capping layer 13. Here, as a result of measurement by XPS (X-ray photoelectron spectroscopy), the atomic ratio (N / In) of indium (In) and nitrogen (N) in the absorption layer 14 was 1.0 (=1:1). Furthermore, as a result of measurement by XRD (X-ray diffraction device), the crystallinity of the absorption layer 14 was slightly crystalline, but was amorphous. Furthermore, the layer thickness of the absorption layer 14 was set to 33 nm. Next, a back conductive film 15 was formed of chromium nitride (CrN) on the surface of the substrate 11 opposite to the surface on which the reflective layer 12 was formed. The layer thickness of the back conductive film 15 was set to 100 nm.

[0039] Through the above procedure, the reflective photomask blank 100 of Example 1 was produced. The deposition (formation of each layer) of each film (reflective layer 12, capping layer 13, absorbing layer 14) on the substrate 11 was performed using a multi-target sputtering device. The thickness of each film was controlled by the sputtering time. The absorbing layer 14 was deposited by reactive sputtering, controlling the amount of oxygen introduced into the chamber during sputtering, so that the N / In ratio was 1.0.

[0040] Next, a method for producing the reflective photomask 200 will be described with reference to FIGS. As shown in FIG. 5, first, a positive chemically amplified resist (SEBP9012: manufactured by Shin-Etsu Chemical Co., Ltd.) was applied by spin coating onto the absorption layer 14 of the reflective photomask blank 100. The layer thickness of the positive chemically amplified resist was set to 120 nm. The applied positive chemically amplified resist was then baked at 110° C. for 10 minutes to form a resist film 16. A predetermined pattern was then drawn on the resist film 16 using an electron beam lithography machine (JBX3030: manufactured by JEOL Ltd.). Then, a pre-baking process was performed at 110° C. for 10 minutes, and then a development process was performed using a spray developer (SFG3000: manufactured by Sigma Meltec Co., Ltd.). As a result, a resist pattern 16a was formed as shown in FIG. 6.

[0041] Next, using the resist pattern 16a as an etching mask, the absorbing layer 14 was patterned with a mask pattern by dry etching mainly using a chlorine-based gas. As a result, an absorbing pattern (absorbing pattern layer) 141 was formed in the absorbing layer 14 as shown in Fig. 7. Next, the resist pattern 16a was peeled off to produce a reflective photomask 200 of Example 1 as shown in Fig. 8.

[0042] In this embodiment, the absorption pattern 141 formed in the absorption layer 14 includes a 64 nm line-and-space (LS) pattern, a 200 nm line-width LS pattern for measuring the film thickness of the absorption layer using an AFM, and a 4 mm square absorption layer removed portion for measuring the EUV reflectance on a reflective photomask 200 for transfer evaluation. In this embodiment, the 64 nm line-width LS pattern was designed in each of the x and y directions as shown in FIG. 9 so that the influence of the projection effect due to EUV irradiation can be easily seen. The thickness of the absorbing layer 14 was measured by a transmission electron microscope. The thickness was also measured in the following Examples 2 to 5 and Comparative Examples 1 to 7 in the same manner.

[0043] [Example 2] In Example 2, a layer was formed as the absorbing layer 14 in which the atomic ratio (N / In) of indium (In) to nitrogen (N) was 1.0, the total content of indium (In) and nitrogen (N) was 70 atomic % of the entire absorbing layer 14, and the remaining 30 atomic % was Ga. The layer thickness of the absorbing layer 14 was 33 nm. A reflective photomask blank 100 and a reflective photomask 200 of Example 2 were produced in the same manner as in Example 1 except for the above.

[0044] [Example 3] In Example 3, a layer was formed as the absorption layer 14 in which the atomic ratio (N / In) of indium (In) to nitrogen (N) was 1.0, the total content of indium (In) and nitrogen (N) was 70 atomic % of the entire absorption layer 14, and the remaining 30 atomic % was Ta. The layer thickness of the absorption layer 14 was set to 33 nm. A reflective photomask blank 100 and a reflective photomask 200 of Example 3 were produced in the same manner as in Example 1.

[0045] [Example 4] In Example 4, a layer was formed as the absorbing layer 14 in which the atomic ratio (N / In) of indium (In) to nitrogen (N) was 0.5 and the total content of indium (In) and nitrogen (N) was 100 atomic % of the entire absorbing layer 14. In addition, the layer thickness of the absorbing layer 14 was set to 33 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Example 4 were produced in the same manner as in Example 1.

[0046] [Example 5] In Example 5, a layer was formed as the absorbing layer 14 in which the atomic ratio (N / In) of indium (In) to nitrogen (N) was 1.5 and the total content of indium (In) and nitrogen (N) was 100 atomic % of the entire absorbing layer 14. In addition, the layer thickness of the absorbing layer 14 was 33 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Example 5 were produced in the same manner as in Example 1.

[0047] [Comparative Example 1] In Comparative Example 1, a layer was formed as the absorbing layer 14 in which the atomic ratio (N / In) of indium (In) to nitrogen (N) was 0 and the indium (In) content was 100 atomic % of the entire absorbing layer 14. The thickness of the absorbing layer 14 was set to 33 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Comparative Example 1 were produced in the same manner as in Example 1.

[0048] [Comparative Example 2] In Comparative Example 2, a layer was formed as the absorbing layer 14 in which the atomic ratio (N / In) of indium (In) to nitrogen (N) was 1.0 and the total content of indium (In) and nitrogen (N) was 100 atomic % of the entire absorbing layer 14. In addition, the layer thickness of the absorbing layer 14 was set to 50 nm. Otherwise, a reflective photomask blank 100 and a reflective photomask 200 of Comparative Example 2 were produced in the same manner as in Example 1.

[0049] [Comparative Example 3] In Comparative Example 3, a layer was formed as the absorbing layer 14 in which the atomic ratio (N / In) of indium (In) to nitrogen (N) was 1.0, the total content of indium (In) and nitrogen (N) was 30 atomic % of the entire absorbing layer 14, and the remaining 70 atomic % was Te. The thickness of the absorbing layer 14 was 26 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Comparative Example 3 were produced in the same manner as in Example 1.

[0050] [Comparative Example 4] In Comparative Example 4, a layer was formed as the absorbing layer 14 in which the atomic ratio (N / In) of indium (In) to nitrogen (N) was 1.0, the total content of indium (In) and nitrogen (N) was 45 atomic % of the entire absorbing layer 14, and the remaining 55 atomic % was Te. The thickness of the absorbing layer 14 was 26 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Comparative Example 4 were produced in the same manner as in Example 1.

[0051] [Comparative Example 5] In Comparative Example 4, a layer was formed as the absorbing layer 14 in which the atomic ratio (N / In) of indium (In) to nitrogen (N) was 0.4 and the total content of indium (In) and nitrogen (N) was 100 atomic % of the entire absorbing layer 14. In addition, the layer thickness of the absorbing layer 14 was 33 nm. Otherwise, a reflective photomask blank 100 and a reflective photomask 200 of Comparative Example 5 were produced in the same manner as in Example 1.

[0052] [Comparative Example 6] In Comparative Example 6, a layer was formed as the absorbing layer 14 in which the atomic ratio (N / In) of indium (In) to nitrogen (N) was 1.0 and the total content of indium (In) and nitrogen (N) was 100 atomic % of the entire absorbing layer 14. In addition, the layer thickness of the absorbing layer 14 was set to 15 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Comparative Example 6 were produced in the same manner as in Example 1.

[0053] [Comparative Example 7] In Comparative Example 7, a layer was formed as the absorbing layer 14 in which the atomic ratio (N / In) of indium (In) to nitrogen (N) was 1.0 and the total content of indium (In) and nitrogen (N) was 100 atomic % of the entire absorbing layer 14. In addition, the layer thickness of the absorbing layer 14 was 47 nm. Otherwise, the reflective photomask blank 100 and the reflective photomask 200 of Comparative Example 7 were produced in the same manner as in Example 1.

[0054] [existing] In addition to the above-mentioned Examples 1 to 5 and Comparative Examples 1 to 7, a reflective photomask blank having a conventional tantalum (Ta)-based absorption layer and a reflective photomask (hereinafter also referred to as "existing Ta-based mask") were also produced. The reflective photomask blank, like Examples 1 to 5 and Comparative Examples 1 to 7, has a reflective layer (repeated 40 times) formed by repeatedly stacking a molybdenum (Mo) layer and a silicon (Si) layer on a synthetic quartz substrate having low thermal expansion characteristics, a capping layer 13 made of ruthenium (Ru) with a layer thickness of 3.5 nm, and an absorption layer 14. However, the absorption layer 14 was formed by depositing a layer of TaO with a layer thickness of 2 nm on a layer of TaN with a layer thickness of 58 nm. Also, like Examples 1 to 5 and Comparative Examples 1 to 7, the reflective photomask (existing Ta-based mask) was patterned by patterning a mask pattern on the absorption layer 14 of this reflective photomask.

[0055] The evaluation items evaluated in this example will be described below. (Wafer exposure evaluation) Using an EUV exposure tool (NXE3300B, manufactured by ASML), the mask patterns of the reflective photomasks 200 of Examples 1 to 5 and Comparative Examples 1 to 7 were transferred and exposed onto a semiconductor substrate coated with an EUV positive chemically amplified resist. The exposure dose was adjusted so that the x-direction LS pattern shown in FIG. 9 was transferred as designed. Then, the transferred resist patterns were observed and line widths were measured using an electron beam dimension measuring device, and a comparison was made by simulation of how the HV bias value changed in the reflective photomasks 200 of Examples 1 to 5 and Comparative Examples 1 to 7.

[0056] The HV bias value is the line width difference of the transfer pattern depending on the orientation of the mask pattern, that is, the difference between the line width in the horizontal (H) direction and the line width in the vertical (V) direction. The line width in the H direction indicates the line width of the linear pattern perpendicular to the plane formed by the incident light and the reflected light (hereinafter, sometimes referred to as the "incident plane"), and the line width in the V direction indicates the line width of the linear pattern parallel to the incident plane. In other words, the line width in the H direction is the length in the direction parallel to the incident plane, and the line width in the V direction is the length in the direction perpendicular to the incident plane.

[0057] (Heat resistance) Before and after exposure using an EUV exposure device (NXE3300B: manufactured by ASML), the layer thickness and reflectance Ra of the absorption pattern layer 141 of the reflective photomask 200 were measured, and it was confirmed whether there was any change in the film thickness reduction and reflectance Ra of the absorption pattern layer 141 before and after EUV exposure. When no change in the film thickness reduction and reflectance Ra of the absorption pattern layer 141 was confirmed, a "◯" was entered in the "heat resistance" column, and when film thickness reduction and a change in the reflectance Ra were confirmed, an "X" was entered in the "heat resistance" column since long-term use is difficult.

[0058] Table 1 shows the HV bias and heat resistance of Examples 1 to 5, Comparative Examples 1 to 7, and the existing Ta-based mask. [Table 1] Table 1 shows a comparison of the HV biases of each embodiment and each comparative example. According to Table 1, as a result of transfer exposure to a semiconductor substrate by EUV light using an existing Ta-based mask, the pattern dimension in the y direction was 20 nm and the HV bias value was 8.65 nm. In contrast, the HV bias of the reflective photomask 200 of Example 1 was 5.13 nm, the HV bias of the reflective photomask 200 of Example 2 was 4.17 nm, the HV bias of the reflective photomask 200 of Example 3 was 4.61 nm, the HV bias of the reflective photomask 200 of Example 4 was 5.13 nm, and the HV bias of the reflective photomask 200 of Example 5 was 5.13 nm. In addition, the HV bias of the reflective photomask 200 of Comparative Example 3 was 5.01 nm, the HV bias of the reflective photomask 200 of Comparative Example 4 was 5.25 nm, and the HV bias of the reflective photomask 200 of Comparative Example 5 was 5.13 nm. Therefore, it was confirmed that the projection effect can be suppressed or reduced compared to the existing Ta-based mask. Note that the transfer pattern of the reflective photomask 200 of Comparative Example 6 had large roughness due to insufficient contrast, and the transfer patterns of the reflective photomasks 200 of Comparative Examples 1, 2, and 7 were not resolved, so that the HV bias could not be evaluated.

[0059] Table 1 shows a comparison of heat resistance between each example and each comparative example. In Table 1, when the existing Ta-based mask was used, almost no change in film loss and reflectance Ra was confirmed. Similarly, when the reflective photomasks 200 of Examples 1 to 5 and Comparative Examples 2, 6, and 7 were used, almost no change in film loss and reflectance Ra was confirmed. Therefore, in Table 1, "○" and "◎" are written in the "heat resistance" column for "Existing", "Example 1", "Example 2", "Example 3", "Example 4", "Example 5", "Comparative Example 2", "Comparative Example 6", and "Comparative Example 7". Therefore, it was confirmed that the reflective photomask 200 has a heat resistance higher than that of the existing Ta-based mask. In particular, the reflective photomask 200 of Example 5 was marked with "◎" because no change in film loss and reflectance Ra was confirmed. In contrast, when the reflective photomasks 200 of Comparative Example 1 and Comparative Examples 3 to 5 were used, almost no change in film loss and reflectance Ra was confirmed. Therefore, "×" is written in the "heat resistance" column for "Comparative Example 1", "Comparative Example 3", "Comparative Example 4", and "Comparative Example 5".

[0060] Table 1 shows the overall evaluation of HV bias and heat resistance. In Table 1, if the HV bias value is lower than the HV bias value (8.65) of the existing Ta-based mask and the heat resistance column is "○" or "◎", "○" is written in the "Judgment" column. Also, if the HV bias value is higher than the HV bias value (8.65) of the existing mask or if the heat resistance column is "×", "×" is written in the "Judgment" column. Therefore, in Table 1, "○" is written in the "Judgment" column for "Example 1", "Example 2", "Example 3", "Example 4", and "Example 5". In contrast, "×" is written in the "Judgment" column for "Comparative Example 1", "Comparative Example 2", "Comparative Example 3", "Comparative Example 4", "Comparative Example 5", "Comparative Example 6", and "Comparative Example 7". Since the HV bias value of "Existing" is 8.65, "△" is written in the "Judgment" column.

[0061] As a result, if the reflective photomask 200 has an absorption pattern layer 141 containing indium (In) and nitrogen (N) in total of 50 atomic % or more, an atomic ratio (N / In) of nitrogen (N) to indium (In) in the absorption pattern layer 141 of 0.5 to 1.5, and a layer thickness of the absorption pattern layer 141 of 17 nm to 45 nm, the optical density OD value and heat resistance are both good, the projection effect can be reduced, the life is long, and the transfer performance is high. That is, it was confirmed that a reflective photomask 200 with better transfer performance can be obtained. In other words, it can be said that it was confirmed that by using the reflective photomask blank 100 according to the above embodiment, the projection effect of a reflective photomask for patterning transfer using light of a wavelength in the extreme ultraviolet region as a light source can be suppressed or reduced, and a reflective photomask 200 having sufficient heat resistance during exposure can be manufactured. [Industrial Applicability]

[0062] The reflective photomask blank and reflective photomask according to the present invention can be suitably used for forming fine patterns by EUV exposure in the manufacturing process of semiconductor integrated circuits and the like. [Explanation of symbols]

[0063] Reference Signs List 1...substrate, 2...reflective layer, 3...capping layer, 4...absorption layer, 41...absorption pattern (absorption pattern layer), 10...reflective photomask blank, 20...reflective photomask, 11...substrate, 12...reflective layer, 13...capping layer, 14...absorption layer, 141...absorption pattern (absorption pattern layer), 15...back conductive film, 16...resist film, 16a...resist pattern, 100...reflective photomask blank, 200...reflective photomask

Claims

1. A reflective photomask blank for producing a reflective photomask for pattern transfer using extreme ultraviolet light as a light source, comprising: A substrate; a reflective layer including a multilayer film formed on the substrate; an absorbing layer formed on the reflective layer, The absorption layer contains indium (In) and nitrogen (N) in a total amount of 50 atomic % or more, an atomic ratio (N / In) of nitrogen (N) to indium (In) in the absorption layer is 0.5 or more and 1.5 or less; The thickness of the absorption layer is 17 nm or more and 45 nm or less. Reflective photomask blank.

2. The absorbing layer further comprises one or more elements selected from the group consisting of tantalum (Ta), platinum (Pt), tellurium (Te), zirconium (Zr), hafnium (Hf), titanium (Ti), tungsten (W), silicon (Si), chromium (Cr), gallium (Ga), molybdenum (Mo), tin (Sn), palladium (Pd), nickel (Ni), boron (B), fluorine (F), oxygen (O), carbon (C), and hydrogen (H). The reflective photomask blank according to claim 1 .

3. A capping layer is included between the reflective layer and the absorbing layer. The reflective photomask blank according to claim 1 or 2.

4. A reflective photomask for pattern transfer using extreme ultraviolet light as a light source, A substrate; a reflective layer including a multilayer film formed on the substrate; an absorbing pattern layer formed on the reflective layer; The absorption pattern layer contains indium (In) and nitrogen (N) in a total amount of 50 atomic % or more, The atomic ratio (N / In) of nitrogen (N) to indium (In) in the absorption pattern layer is 0.5 or more and 1.5 or less; The thickness of the absorption pattern layer is 17 nm or more and 45 nm or less. Reflective photomask.

5. The absorbing pattern layer further comprises one or more elements selected from the group consisting of tantalum (Ta), platinum (Pt), tellurium (Te), zirconium (Zr), hafnium (Hf), titanium (Ti), tungsten (W), silicon (Si), chromium (Cr), gallium (Ga), molybdenum (Mo), tin (Sn), palladium (Pd), nickel (Ni), boron (B), fluorine (F), oxygen (O), carbon (C), and hydrogen (H).

5. The reflective photomask according to claim 4.