Fluorosilicone rubber composition and cured molded product

A fluorosilicone rubber composition with specific components enhances roll processability and mechanical properties by using organopolysiloxane, reinforcing silica, and a curing agent, addressing adhesion and releasability issues while maintaining fluorine content and resistance.

JP7564055B2Active Publication Date: 2024-10-08SHIN ETSU CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021078886
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-07
Publication Date
2024-10-08
Estimated Expiration
2041-05-07

AI Technical Summary

Technical Problem

Fluorosilicone rubber compositions face issues with strong roll adhesion and poor roll releasability due to the influence of 3,3,3-trifluoropropyl groups, leading to increased costs and reduced oil and fuel resistance when using certain additives.

Method used

A fluorosilicone rubber composition comprising organopolysiloxane with 60 mol% fluoroalkyl groups, reinforcing silica, linear trifluoropropylmethylpolysiloxane, linear fluorooxyalkylene group-containing polymer, and a curing agent, which improves roll processability and maintains high fluorine content.

Benefits of technology

The composition achieves excellent roll processability and maintains mechanical properties while retaining high fluorine content, reducing costs associated with expensive additives and preserving oil and fuel resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564055000001
    Figure 0007564055000001
  • Figure 0007564055000002
    Figure 0007564055000002
  • Figure 0007564055000003
    Figure 0007564055000003
Patent Text Reader

Abstract

To provide a fluorosilicone rubber composition having excellent roll processability while having a high fluorine content.SOLUTION: A fluorosilicone rubber composition comprises: (A) 100 pts.mass of an organopolysiloxane having two or more alkenyl groups bonded to silica atoms per molecule, the number of siloxane units having a fluoroalkyl group being 60 mol% or greater relative to the total number of all siloxane units, and the average degree of polymerization as calculated from the weight-average molecular weight being 2,000 or greater; (B) 5-100 pts.mass of reinforcing silica having a specific surface area according to the BET method of 50 m2 / g or greater; (C) 0.1-20 pts.mass of a linear trifluoropropylmethylpolysiloxane having both ends blocked by trifluoropropylmethylhydroxysilyl groups; (D) 0.01-5 pts.mass of a linear fluoroxyalkylene-group-containing polymer; and (E) a curing agent in an amount effective for curing.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fluorosilicone rubber composition and a cured molded product. [Background technology]

[0002] Silicone rubber has excellent weather resistance, electrical properties, low compression set, heat resistance, cold resistance, etc., and is therefore widely used in various fields, including electrical equipment, automobiles, construction, medicine, and food. In particular, fluorosilicone rubber compositions, which are based on fluorosilicone raw rubber, whose main chain of the base polymer is essentially composed of a repeating structure of (3,3,3-trifluoropropyl)methylsiloxane units having 3,3,3-trifluoropropyl groups as side chain substituents, have excellent solvent resistance, and are widely used as diaphragms, O-rings, oil seal materials, etc., as transportation equipment parts and petroleum-related equipment parts. Currently, the demand for silicone rubber is increasing, and the development of silicone rubber with excellent properties is desired.

[0003] However, it is known that fluorosilicone rubber has strong roll adhesion due to the influence of 3,3,3-trifluoropropyl groups, and has poor roll releasability. Various compositions have been proposed to improve this roll releasability. For example, methods of adding a perfluoroalkyl group-containing siloxane (Patent Document 1) or adding a polyorganosiloxane containing 5 to 25 mass% of vinyl groups (Patent Document 2) are known. Furthermore, a method of improving roll adhesion by adding a polyorganosiloxane having a degree of polymerization of 100 or more and 3,3,3-trifluorosilane or a partial hydrolysis condensate thereof, in which the monovalent organic group bonded to the silicon atom is selected from an alkyl group, a phenyl group, and a vinyl group, and 2 to 25 mol% of the total organic groups are vinyl, has also been disclosed (Patent Document 3). Furthermore, an improvement has also been attempted by blending reinforcing silica surface-treated with silane or siloxane having a γ-trifluoropropyl group and adding a siloxane with both ends blocked with silanol (Patent Document 4).

[0004] However, it has been found that these methods have negative aspects, such as increased costs due to the expensive additives themselves, and the addition of polysiloxanes containing alkyl or vinyl groups can reduce the inherent oil resistance and fuel resistance of fluorosilicone rubber. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 3-227352 [Patent Document 2] Japanese Patent Application Publication No. 53-146757 [Patent Document 3] Special Publication No. 61-57868 [Patent Document 4] Japanese Patent Application Publication No. 05-311078 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in view of the above circumstances, and has as its object to provide a fluorosilicone rubber composition which has excellent roll processability even when it has a high fluorine content. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides A fluorosilicone rubber composition comprising: (A) 100 parts by mass of an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms in each molecule, the number of fluoroalkyl group-containing siloxane units being 60 mol % or more of the total number of all siloxane units, and having an average degree of polymerization of 2,000 or more as calculated from the weight average molecular weight, (B) Specific surface area by BET method: 50 m 2 / g or more: 5 to 100 parts by mass of reinforcing silica, (C) linear trifluoropropylmethylpolysiloxane, both ends of which are capped with trifluoropropylmethylhydroxysilyl groups: 0.1 to 20 parts by mass, (D) a linear fluorooxyalkylene group-containing polymer: 0.01 to 5 parts by mass, and (E) Hardener: Effective hardening amount The present invention provides a fluorosilicone rubber composition comprising:

[0008] Such a fluorosilicone rubber composition has excellent roll processability even if it has a high fluorine content.

[0009] It is also preferred that the organopolysiloxane of component (A) is linear and that both molecular chain terminals of the organopolysiloxane are groups selected from the group consisting of trimethylsiloxy, dimethylvinylsiloxy, dimethylhydroxysiloxy, methyldivinylsiloxy, and trivinylsiloxy groups.

[0010] Such component (A) is more preferable as the base polymer for the fluorosilicone rubber composition of the present invention.

[0011] Furthermore, the linear fluorooxyalkylene group-containing polymer of the component (D) is represented by the following formula (3), (4) or (5): HOCH2O(CF2O) m1 (CF2CF2O) n1 CH2OH (3) (In the formula, m1 and n1 are numbers that satisfy the range of the number average molecular weight of 1,000 to 5,000.) CF3O(CF2O) m2 (CF2CF2O) n2 CF3(4) (In the formula, m2 and n2 are numbers that satisfy the range of the number average molecular weight of 1,000 to 10,000.) HOCH2CF2O(CF2CF2O) n3 (CF2O) m3 CF2CH2OH (5) (In the formula, m3 and n3 are numbers that satisfy the range of the number average molecular weight of 1,000 to 5,000.) It is preferable that the formula is represented by the following formula:

[0012] Such component (D) is more useful as the roll processability improver of the present invention.

[0013] In addition, the curing agent of the component (E) is preferably a combination of an organohydrogenpolysiloxane and a hydrosilylation catalyst.

[0014] The curing agent of the component (E) is preferably an organic peroxide.

[0015] When component (E) is a combination of an organohydrogenpolysiloxane and a hydrosilylation catalyst, or an organic peroxide, the fluorosilicone rubber composition of the present invention can be cured satisfactorily.

[0016] The present invention also provides a cured molded article comprising the above-mentioned cured fluorosilicone rubber composition.

[0017] The fluorosilicone rubber composition of the present invention can be molded while being heat cured to provide a cured molded product made of a rubber-like elastomer. Effect of the Invention

[0018] According to the present invention, it is possible to obtain a fluorosilicone rubber composition which exhibits good roll processability when uncured, even when the composition has a high fluorine content. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] As mentioned above, there has been a need to provide a fluorosilicone rubber composition that has excellent roll processability even when it has a high fluorine content.

[0020] As a result of intensive research conducted by the present inventors in order to achieve the above-mentioned object, they discovered that by blending a silicone rubber composition containing an organopolysiloxane containing at least 60 mol % of silicon atoms bonded to 3,3,3-trifluoropropyl groups and having an average degree of polymerization of 2,000 or more, reinforcing silica, a linear trifluoropropylmethylpolysiloxane capped at both ends with trifluoropropylmethylhydroxysilyl groups, a linear fluorooxyalkylene group-containing polymer, and a curing agent, it is possible to obtain a fluorosilicone rubber composition which has excellent roll processability even in a high fluorine content, which led to the completion of the present invention.

[0021] That is, the present invention provides: A fluorosilicone rubber composition comprising: (A) 100 parts by mass of an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms in each molecule, the number of fluoroalkyl group-containing siloxane units being 60 mol % or more of the total number of all siloxane units, and having an average degree of polymerization of 2,000 or more as calculated from the weight average molecular weight, (B) Specific surface area by BET method: 50 m 2 / g or more: 5 to 100 parts by mass of reinforcing silica, (C) linear trifluoropropylmethylpolysiloxane, both ends of which are capped with trifluoropropylmethylhydroxysilyl groups: 0.1 to 20 parts by mass, (D) a linear fluorooxyalkylene group-containing polymer: 0.01 to 5 parts by mass, and (E) Hardener: Effective hardening amount The fluorosilicone rubber composition contains

[0022] The present invention will be described in detail below, but the present invention is not limited thereto.

[0023] [Fluorosilicone rubber composition] The present invention relates to a fluorosilicone rubber composition containing the above-mentioned components (A) to (E). Each component will be described in detail below.

[0024] [(A) Organopolysiloxane] Component (A) is an organopolysiloxane that is the main component (base polymer) of the composition. Component (A) is an organopolysiloxane that has two or more alkenyl groups bonded to silicon atoms in each molecule, in which the number of siloxane units having fluoroalkyl groups accounts for 60 mol% or more of the total number of all siloxane units, and in which the average degree of polymerization calculated from the weight average molecular weight is 2,000 or more.

[0025] The organopolysiloxane of component (A) has an average degree of polymerization of 2,000 or more, and preferably has an average degree of polymerization in the range of 2,000 to 100,000, more preferably 2,000 to 50,000, and particularly preferably 2,000 to 20,000. If the average degree of polymerization is less than 2000, the fluorosilicone rubber composition of the present invention will not satisfy the properties required for millable rubber, and roll kneading properties and the like will be significantly deteriorated, which is not preferred. In the present invention, the average degree of polymerization is a value calculated from the weight average molecular weight in terms of polystyrene in GPC (gel permeation chromatography) analysis measured under the following conditions.

[0026] [Measurement conditions] Component (A) Developing solvent: Tetrahydrofuran (THF) ·Flow rate: 1mL / min Detector: Refractive index detector (RI) Column: 4 TSKGEL SUPERMULTIPORE HZ-H (Tosoh Corporation) Column temperature: 25℃ Sample injection volume: 10 μL (0.1% by mass in THF solution) ·Molecular weight markers Polystyrene

[0027] In the present invention, component (A) is preferably a non-liquid organopolysiloxane gum that has a high degree of polymerization (high viscosity) and has no self-flowability at room temperature (25° C.).

[0028] In the (A) component, the number of siloxane units having a fluoroalkyl group is 60 mol% or more, preferably 65 mol% or more, based on the total number of all siloxane units. There is no particular upper limit, and it is sufficient if it is 100 mol% or less, preferably less than 100 mol%, more preferably 99.8 mol% or less, and may be 98 mol% or less.

[0029] The fluoroalkyl group-containing siloxane unit may have one or two fluoroalkyl groups bonded to the silicon atom.

[0030] The component (A) is preferably represented by the following average composition formula (1). R 1 n SiO (4-n) / 2 (1) (In the formula, R 1 are each independently a monovalent hydrocarbon group having 1 to 20 carbon atoms or a fluoroalkyl group having 1 to 20 carbon atoms, and n is a positive number of 1.95 to 2.04.

[0031] In the above average composition formula (1), R 1 are each independently a monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 12, more preferably 1 to 8 carbon atoms, or a fluoroalkyl group having 1 to 20 carbon atoms, preferably 1 to 10, more preferably 1 to 6 carbon atoms. Examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, and butyl groups, cycloalkyl groups such as cyclohexyl groups, alkenyl groups such as vinyl, allyl, butenyl, and hexenyl groups, aryl groups such as phenyl and tolyl groups, and aralkyl groups such as β-phenylpropyl groups. Among these, methyl, vinyl, and phenyl groups are preferred, and methyl and vinyl groups are more preferred. Examples of the fluoroalkyl group include 3,3,3-trifluoropropyl, 3,3,4,4,4-pentafluorobutyl, 3,3,4,4,5,5,5-heptafluoropentyl, and 3,3,4,4,5,5,6,6,6-nonafluorohexyl groups. Of these, the 3,3,3-trifluoropropyl group is preferable.

[0032] In the above average composition formula (1), n ​​is a positive number from 1.95 to 2.04, and preferably a positive number from 1.98 to 2.02. When n is in the range of 1.95 to 2.04, the resulting cured product exhibits sufficient rubber elasticity.

[0033] The organopolysiloxane of component (A) must have at least two alkenyl groups in one molecule, and preferably has 2 to 50 alkenyl groups. In the above average composition formula (1), the alkenyl group is R 1 Of the total number of moles, the alkenyl group preferably accounts for 0.001 to 10 mol %, and more preferably 0.01 to 5 mol %. The alkenyl group is preferably a vinyl group or an allyl group, and particularly preferably a vinyl group.

[0034] The structure of the organopolysiloxane of component (A) is not particularly limited, but it is preferable that the main chain contains a diorganosiloxane unit (R 1 2SiO 2 / 2 ) repeating units, and both ends of the molecular chain are triorganosiloxy groups (R 1 3SiO 1 / 2 It is preferable that the diorganopolysiloxane is a linear diorganopolysiloxane terminated with R 1 is as described above.

[0035] It is preferable that both molecular chain terminals of the organopolysiloxane of component (A) are blocked with a group selected from the group consisting of trimethylsiloxy, dimethylvinylsiloxy, dimethylhydroxysiloxy, methyldivinylsiloxy, and trivinylsiloxy. These terminal groups at both molecular chain terminals may be the same or different.

[0036] These organopolysiloxanes may be used alone or in combination of two or more types having different degrees of polymerization or molecular structures.

[0037] In the fluorosilicone rubber composition of the present invention, the content of component (A) is preferably 44 to 96 mass %, more preferably 50 to 90 mass %, and even more preferably 60 to 80 mass %.

[0038] [(B) Reinforcing Silica] The reinforcing silica of component (B) acts as a filler that imparts excellent mechanical properties to the resulting fluorosilicone rubber composition. The reinforcing silica may be either precipitated silica (wet silica) or fumed silica (dry silica), and is preferably one that has numerous silanol groups on its surface.

[0039] In the present invention, the reinforcing silica (B) has a specific surface area of ​​50 m2 by the BET method. 2 / g or more. Preferably, it is 100 to 400m 2 / g. This specific surface area is 50m 2 If it is less than 1 / g, the reinforcing effect of the silicone rubber imparted by component (B) will be insufficient.

[0040] The reinforcing silica of component (B) may be used in an untreated state, or may be surface-treated, as necessary, with an organosilicon compound such as organopolysiloxane, organopolysilazane, chlorosilane, alkoxysilane, etc. The reinforcing silica may be used alone or in combination of two or more types.

[0041] The amount of reinforcing silica, component (B), blended is 5 to 100 parts by mass, preferably 10 to 80 parts by mass, and more preferably 20 to 70 parts by mass, per 100 parts by mass of the organopolysiloxane, component (A). If the amount of component (B) blended is above the above upper limit or below the above lower limit, not only will the processability of the resulting fluorosilicone rubber composition decrease, but the mechanical properties such as tensile strength and tear strength of the silicone rubber cured product obtained by curing the fluorosilicone rubber composition will be insufficient.

[0042] [(C) Linear trifluoropropylmethylpolysiloxane, both ends of which are capped with trifluoropropylmethylhydroxysilyl groups] Component (C), a linear trifluoropropylmethylpolysiloxane terminated with trifluoropropylmethylhydroxysilyl groups, acts as a dispersibility improver (surface treatment agent) for the reinforcing silica in the fluorosilicone rubber composition of the present invention.

[0043] The component (C) is preferably represented by the following average composition formula (2). [ka] (In the formula, x is a positive number from 1 to 35.)

[0044] In the above average composition formula (2), x is a positive number of 1 to 35, and preferably a positive number of 3 to 15. When x is 35 or less, the number of parts added for dispersing the reinforcing silica is appropriate, and as a result, a decrease in viscosity can be prevented and excellent roll processability, which is the object of the present invention, can be obtained.

[0045] The amount of linear trifluoropropylmethylpolysiloxane, component (C), added is 0.1 to 20 parts by mass, and more preferably 1 to 10 parts by mass, per 100 parts by mass of organopolysiloxane, component (A). If the amount of component (C) added is less than 0.1 part by mass, so-called plastic reversion occurs, whereas if it is more than 20 parts by mass, the viscosity of the resulting fluorosilicone rubber composition becomes too low, and the effect of improving roll processability of the present invention is not obtained.

[0046] [(D) Linear Fluorooxyalkylene Group-Containing Polymer] Component (D) is a linear fluorooxyalkylene group-containing polymer which, in the fluorosilicone rubber composition of the present invention, acts as an additive to improve the roll processability of the resulting fluorosilicone rubber composition.

[0047] The linear fluorooxyalkylene group-containing polymer of component (D) may be a commercially available product, such as that sold under the trade name FOMBLIN by Solvay Solexis, Inc. Specific examples include FOMBLIN D2 (number average molecular weight 1,500), FOMBLIN M07 (number average molecular weight 5,400), FOMBLIN M15 (number average molecular weight 9,700), and FOMBLIN Z03 (number average molecular weight 4,000).

[0048] Examples of such polymers include those having structures represented by the following formulas (3), (4) and (5). HOCH2O(CF2O) m1 (CF2CF2O) n1 CH2OH (3) (In the formula, m1 and n1 are numbers that satisfy the range of the number average molecular weight of 1,000 to 5,000.) CF3O(CF2O) m2 (CF2CF2O) n2 CF3(4) (In the formula, m2 and n2 are numbers that satisfy the range of the number average molecular weight of 1,000 to 10,000.) HOCH2CF2O(CF2CF2O) n3 (CF2O) m3 CF2CH2OH (5) (In the formula, m3 and n3 are numbers that satisfy the range of the number average molecular weight of 1,000 to 5,000.)

[0049] In the present invention, the number average molecular weight of the above component (D) refers to the number average molecular weight measured under the following conditions in GPC (gel permeation chromatography) analysis using perfluoro(polyoxypropylene ethyl ether) as the standard substance.

[0050] [Measurement conditions] Developing solvent: Methyl (perfluorobutyl) ether (product name: NOVEC HFE7100, manufactured by 3M) ·Flow rate: 0.6mL / min Detector: Refractive index detector (RI) Column: 2 TSKGEL SUPERHM-M (Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 10 μL (0.1% by mass concentration NOVEC HFE7100 solution) ·Molecular weight marker Perfluoro(polyoxypropylene ethyl ether)

[0051] The blending amount of component (D) is 0.01 to 5 parts by mass, and preferably 0.1 to 3 parts by mass, per 100 parts by mass of the organopolysiloxane of component (A). If the blending amount of component (D) is too small, the roll processability of the fluorosilicone rubber composition will not improve, whereas if the blending amount is too large, the plasticity of the silicone rubber compound (fluorosilicone rubber composition) will decrease, which is economically undesirable.

[0052] [(E) Hardener] The curing agent (E) is not particularly limited as long as it can cure the fluorosilicone rubber composition of the present invention. The component (E) may be used alone or in combination of two or more. Examples of the component (E) include an organic peroxide curing agent (E-1) and an addition reaction type curing agent (E-2). The amount of the component (E) is preferably 0.1 to 50 parts by mass, more preferably 0.1 to 40 parts by mass, and even more preferably 0.2 to 10 parts by mass, based on 100 parts by mass of the organopolysiloxane (A).

[0053] (E-1) Organic peroxide curing agent Examples of the (E-1) organic peroxide curing agent include benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, p-methylbenzoyl peroxide, o-methylbenzoyl peroxide, 2,4-dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, di-t-butyl peroxide, t-butyl perbenzoate, and 1,6-hexanediol-bis-t-butylperoxycarbonate.

[0054] The amount of organic peroxide curing agent is preferably 0.1 to 10 parts by mass, and more preferably 0.2 to 5 parts by mass, per 100 parts by mass of component (A). If the amount is 0.1 part by mass or more, curing is sufficient, and if it is 10 parts by mass or less, the cured silicone rubber will not yellow due to decomposition residues of the organic peroxide.

[0055] (E-2) Addition reaction curing agent As the addition reaction curing agent (E-2), it is preferable to use an organohydrogenpolysiloxane in combination with a hydrosilylation catalyst.

[0056] The organohydrogenpolysiloxane may have a linear, cyclic, branched, or three-dimensional network structure, so long as it contains preferably 2 or more, more preferably 3 or more, even more preferably 3 to 200, and even more preferably about 4 to 100 hydrogen atoms bonded to silicon atoms in one molecule (i.e., hydrosilyl groups). The hydrosilyl groups may be at the molecular chain terminals, in the middle of the molecular chain, or both.

[0057] The organohydrogenpolysiloxane may be any organohydrogenpolysiloxane known as a crosslinking agent for addition reaction curing type silicone rubber compositions. For example, an organohydrogenpolysiloxane represented by the following average composition formula (6) can be used. R 2 p H q SiO (4-p-q) / 2 (6) (R 2 are each independently a monovalent hydrocarbon group having 1 to 12 carbon atoms. p is 0 <p<3、qは0<q≦3であり、0<p+q≦3である。)

[0058] In the above average composition formula (6), R 2They are each independently a monovalent hydrocarbon group having 1 to 12 carbon atoms, preferably 1 to 8 carbon atoms, and preferably having no aliphatic unsaturated bond. Specifically, alkyl groups such as methyl group, ethyl group, propyl group, cycloalkyl groups such as cyclohexyl group, aryl groups such as phenyl group, tolyl group, aralkyl groups such as benzyl group, 2-phenylethyl group, 2-phenylpropyl group, etc. may be mentioned. Among them, an alkyl group is preferable, and a 3,3,3-trifluoropropyl group, 3,3,4,4,4-pentafluorobutyl group, 3,3,4,4,5,5,5-heptafluoropentyl group, in which some or all of the hydrogen atoms of the alkyl group are substituted with a halogen atom, preferably a fluorine atom, and a fluoroalkyl group such as 3,3,4,4,5,5,6,6,6-nonafluorohexyl group may also be used.

[0059] In the above average composition formula (6), p satisfies 0 < p < 3, preferably 0.5 ≤ p ≤ 2.2, more preferably 1.0 ≤ p ≤ 2.0, q satisfies 0 < q ≤ 3, preferably 0.002 ≤ q ≤ 1.1, more preferably 0.005 ≤ q ≤ 1, and p + q is a positive number satisfying 0 < p + q ≤ 3, preferably 1 ≤ p + q ≤ 3, more preferably 1.002 ≤ p + q ≤ 2.7.

[0060] The above organohydrogenpolysiloxane preferably has a viscosity of 0.5 to 10,000 mPa·s at 25°C, particularly preferably 1 to 300 mPa·s. In the present invention, the viscosity is a value measured at 25°C using a rotational viscometer by the method described in JIS K 7117-1:1999.

[0061] Examples of organohydrogenpolysiloxanes include 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, tris(hydrogendimethylsiloxy)methylsilane, tris(hydrogendimethylsiloxy)phenylsilane, methylhydrogencyclopolysiloxane, methylhydrogensiloxane-dimethylsiloxane cyclic copolymer, methylhydrogenpolysiloxane capped with trimethylsiloxy groups at both ends, dimethylsiloxane-methylhydrogensiloxane copolymer capped with trimethylsiloxy groups at both ends, dimethylpolysiloxane capped with dimethylhydrogensiloxy groups at both ends, dimethylsiloxane capped with dimethylhydrogensiloxy groups at both ends, and dimethylsiloxane capped with dimethylhydrogensiloxy groups at both ends. copolymer of methylhydrogensiloxane and methylhydrogensiloxane, copolymer of methylhydrogensiloxane and diphenylsiloxane both ends blocked with trimethylsiloxy groups, copolymer of methylhydrogensiloxane, diphenylsiloxane and dimethylsiloxane both ends blocked with trimethylsiloxy groups, copolymer of methylhydrogensiloxane, methylphenylsiloxane and dimethylsiloxane both ends blocked with trimethylsiloxy groups, copolymer of methylhydrogensiloxane, dimethylsiloxane and diphenylsiloxane both ends blocked with dimethylhydrogensiloxy groups, copolymer of methylhydrogensiloxane, dimethylsiloxane and methylphenylsiloxane both ends blocked with dimethylhydrogensiloxy groups, (CH3)2HSiO 1 / 2 Units and (CH3)3SiO 1 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and SiO 4 / 2 Units and (C6H5)3SiO 1 / 2 and copolymers consisting of these units, and compounds in which part or all of the methyl groups in the above exemplary compounds have been substituted with other alkyl groups, phenyl groups, or the like.

[0062] The amount of the organohydrogenpolysiloxane is preferably 0.1 to 40 parts by mass per 100 parts by mass of component (A). The ratio of the number of hydrogen atoms (hydrosilyl groups) bonded to silicon atoms to one alkenyl group of component (A) is preferably in the range of 0.5 to 10, more preferably 0.7 to 5. If the ratio is equal to or greater than the lower limit, crosslinking is sufficient, and sufficient mechanical strength is obtained. If the ratio is equal to or less than the upper limit, physical properties after curing are not deteriorated, and in particular, deterioration of heat resistance of the silicone rubber and increase in compression set can be prevented.

[0063] The hydrosilylation catalyst is a catalyst that causes a hydrosilylation addition reaction between the alkenyl group of the (A) component and the silicon-bonded hydrogen atom (hydrosilyl group) of the organohydrogenpolysiloxane. Examples of the hydrosilylation catalyst include platinum group metal catalysts. There are simple platinum group metals and their compounds, and any catalyst for addition reaction curing type silicone rubber compositions that is known in the art may be used. For example, platinum catalysts such as particulate platinum metal adsorbed on a carrier such as silica, alumina, or silica gel, platinic chloride, chloroplatinic acid, and alcohol solutions of chloroplatinic acid hexahydrate, palladium catalysts, and rhodium catalysts may be used, with platinum or platinum compounds (platinum catalysts) being preferred.

[0064] The amount of catalyst added may be any amount that can promote the addition reaction. Usually, the catalyst is used in the range of 1 ppm by mass to 1% by mass, and preferably 10 to 500 ppm by mass, relative to the organopolysiloxane of component (A) in terms of the amount of platinum group metal. If the amount of catalyst is equal to or greater than the lower limit, the addition reaction is sufficiently promoted and curing is sufficient. If the amount is equal to or less than the upper limit, the reaction promotion effect according to the amount added is obtained, which is economical.

[0065] [Other optional ingredients] In addition to the components mentioned above, the fluorosilicone rubber composition of the present invention may contain, if necessary, quartz powder, crystalline silica, non-reinforcing silica such as diatomaceous earth, calcium carbonate, carbon black such as acetylene black, furnace black, channel black, colorants, heat resistance improvers such as red iron oxide and cerium oxide, flame retardancy improvers such as platinum, titanium oxide and triazole compounds, acid acceptors, thermal conductivity improvers such as alumina and boron nitride, mold release agents, and the like.

[0066] The fluorosilicone rubber composition of the present invention can be obtained by uniformly mixing the above-mentioned components using a mixing device such as a two-roll mill, a Banbury mixer, or a Dow mixer (kneader). It is preferable to first mix components (A), (B), (C), and (D) to prepare a base compound, and then add component (E).

[0067] The base compound is preferably prepared by heat treatment at 20 to 250° C., particularly 50 to 200° C., for 0.1 to 10 hours, particularly 0.1 to 5 hours.

[0068] [Cured molded product] The fluorosilicone rubber composition of the present invention can be molded while being heat cured to give a cured molded product made of a rubber-like elastic body (cured silicone rubber).

[0069] The method for curing the fluorosilicone rubber composition is not particularly limited, but may be any method that applies sufficient heat to decompose the curing agent and vulcanize the fluorosilicone rubber composition. The temperature conditions for curing vary depending on the curing method, but are usually 80 to 400°C, particularly 100 to 200°C, for 3 seconds to 160 minutes, particularly 3 seconds to 20 minutes. There is also no particular limit to the molding method, and molding methods such as continuous vulcanization by extrusion molding, press molding (pressure molding), and injection molding can be used. Furthermore, secondary vulcanization may be performed at 150 to 250°C for about 1 to 10 hours, if necessary. EXAMPLES

[0070] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0071] The organopolysiloxanes (organopolysiloxane gums) of component (A) used in the examples and comparative examples are as follows: In the following, the mole percentage of siloxane units refers to the ratio of each siloxane unit to the total number of siloxane units.

[0072] (A) Organopolysiloxane raw rubber: Organopolysiloxane raw rubber consisting of 99.825 mol % of 3,3,3-trifluoropropylmethylsiloxane units, 0.125 mol % of methylvinylsiloxane units, and 0.05 mol % of dimethylvinylsiloxy units, having an average degree of polymerization of 4,000.

[0073] [Example 1] (A) 100 parts by mass of organopolysiloxane raw rubber, (B) a material having a BET specific surface area of ​​200 m 2 40 parts by mass of fumed silica (Aerosil 200, manufactured by Nippon Aerosil Co., Ltd.) having a molecular weight of 1.0 to 1.2 g / g, (C1) 6.0 parts by mass of a linear 3,3,3-trifluoropropylmethylpolysiloxane having trifluoropropylmethylhydroxysilyl groups at both ends, an average degree of polymerization of 4, and a viscosity of 15 mPa s at 25°C, and (D1) 0.3 parts by mass of a linear fluorooxyalkylene group-containing polymer (product name "FOMBLIN D2", manufactured by Solvay Solexis, number average molecular weight: 1,500) were kneaded in a kneader and heated at 150°C for 2 hours while being mixed in the kneader to prepare a base compound (1).

[0074] To the base compound (1), 0.6 parts by mass of 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane as a curing agent (E) was added per 100 parts by mass of organopolysiloxane raw rubber (A) using a two-roll mill, and the mixture was mixed uniformly to obtain a raw rubber-like silicone rubber composition.

[0075] The silicone rubber composition was subjected to the roll processability test described below.

[0076] [Example 2] A silicone rubber composition was obtained in the same manner as in Example 1, except that the amount of (D1) linear fluorooxyalkylene group-containing polymer (product name "FOMBLIN D2") added was 0.5 parts by mass. The obtained composition was subjected to the roll processability test described below.

[0077] [Example 3] A silicone rubber composition was obtained in the same manner as in Example 1, except that (D1) linear fluorooxyalkylene group-containing polymer (trade name "FOMBLIN D2") was replaced with 0.3 parts by mass of (D2) linear fluorooxyalkylene group-containing polymer (trade name "FOMBLIN M07", manufactured by Solvay Solexis, number average molecular weight: 5,400). The obtained composition was subjected to the roll processability test described below.

[0078] [Comparative Example 1] A silicone rubber composition was prepared in the same manner as in Example 1, except that the linear fluorooxyalkylene group-containing polymer was not added, and the resulting composition was subjected to the roll processability test described below.

[0079] [Comparative Example 2] A silicone rubber composition was prepared in the same manner as in Example 1, except that the linear trifluoropropylmethylpolysiloxane of component (C1) was replaced with 6.0 parts by mass of diphenylsilanediol as component (C2). The resulting composition was subjected to the roll processability test described below.

[0080] The roll processability test method is shown below.

[0081] Roll workability test method 200 g of the silicone rubber composition was kneaded 20 times on a 6-inch twin roll with a hard chrome-plated surface, and the adhesiveness to the roll surface was checked. The composition was rated as ◯ if it could be easily peeled off by hand, △ if it stuck to the surface with some sticking, and × if it stuck strongly.

[0082] Table 1 below shows the compositions of the examples and comparative examples and the results of the roll processability test. [Table 1]

[0083] From the results shown in Table 1, it can be seen that Examples 1 to 3, which contain all of the components (A) to (E) used in the present invention, showed good roll processability. On the other hand, Comparative Example 1, which does not contain the component (D), showed strong adhesion and poor roll processability. Furthermore, Comparative Example 2, which uses diphenylsilanediol (C2), which is similar to the component (C) but is not used in the present invention, instead of the component (C) used in the present invention, showed some improvement in roll processability due to the inclusion of the component (D), but was inferior in roll processability to Examples 1 to 3, which contain all of the components (A) to (E) used in the present invention.

[0084] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. A fluorosilicone rubber composition comprising: (A) 100 parts by mass of a linear organopolysiloxane gum having in each molecule two or more alkenyl groups bonded to silicon atoms, the number of fluoroalkyl group-containing siloxane units being 60 mol % or more of the total number of all siloxane units, and having an average degree of polymerization of 2,000 or more as calculated from the weight average molecular weight, (B) BET specific surface area: 50 m 2 / g or more: 5 to 100 parts by mass of reinforcing silica, (C) a linear trifluoropropylmethylpolysiloxane, both ends of which are capped with trifluoropropylmethylhydroxysilyl groups, represented by the following average composition formula (2): 0.1 to 20 parts by mass, [Formula 1] (In the formula, x is a positive number from 3 to 15.) (D) a linear fluorooxyalkylene group-containing polymer represented by the following formula (5): 0.01 to 5 parts by mass, and HOCH 2 CF 2 O (CF 2 CF 2 O) n3 (CF 2 O) m 3 CF 2 CH 2 OH (5) (In the formula, m3 and n3 are numbers that satisfy the range of the number average molecular weight of 1,000 to 5,000.) (E) Curing agent: effective curing amount A fluorosilicone rubber composition comprising:

2. 2. The fluorosilicone rubber composition according to claim 1, characterized in that both molecular chain terminals of the linear organopolysiloxane rubber of component (A) are groups selected from the group consisting of trimethylsiloxy groups, dimethylvinylsiloxy groups, dimethylhydroxysiloxy groups, methyldivinylsiloxy groups, and trivinylsiloxy groups.

3. 3. The fluorosilicone rubber composition according to claim 1, wherein the curing agent of component (E) is a combination of an organohydrogenpolysiloxane and a hydrosilylation catalyst.

4. 3. The fluorosilicone rubber composition according to claim 1, wherein the curing agent of component (E) is an organic peroxide.

5. 5. A cured molded product comprising a cured product of the fluorosilicone rubber composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Fluorosilicone composition and its production method

    JP1978146757A

  • Diagnosis aiding system for automobile fault

    JP1986057868A

  • Rubber composition and vulcanized product

    JP1991227352A

  • Fluorosilicone rubber composition and method for producing the same

    JP1993311078A

  • Silicone rubber composition for making keypad, and keypad

    JP2020037629A