Method for separating polybutene

JP7564099B2Active Publication Date: 2024-10-08LG CHEM LTD
View PDF -1 Cites 0 Cited by

Patent Information

Application Number
JP2021526299
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-01-18
Filing Date
2020-01-17
Publication Date
2024-10-08
Estimated Expiration
2040-01-17

Smart Images

  • Figure 0007564099000002
    Figure 0007564099000002
  • Figure 0007564099000001
    Figure 0007564099000001
Patent Text Reader

Abstract

The present invention relates to a method for separating polybutene, comprising the steps of: (1) introducing a polybutene solution containing polybutene, a halogenated hydrocarbon solvent, and a non-polar hydrocarbon solvent, the polybutene solution having a viscosity of 1 cp to 50 cp as measured at 25°C using a rotational viscometer, into a distillation column; (2) separating the halogenated hydrocarbon solvent and the non-polar hydrocarbon solvent from the upper part of the distillation column, and separating a polybutene solution containing polybutene and the non-polar hydrocarbon solvent and having a viscosity of 10 cp to 150 cp from the lower part of the distillation column; and (3) separating the non-polar hydrocarbon solvent and polybutene from the polybutene solution separated from the lower part of the distillation column via step (2).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0007026 filed on January 18, 2019, and all contents disclosed in the documents of said Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a method for separating polybutene, and more particularly, to a method for separating polybutene, which can separate polybutene oligomers or polymers and reaction solvents from a reaction solution containing polybutene oligomers or polymers in which polymerization has been completed, and in particular, can reduce the residual content of a specific solvent in the polymer to an extremely low level. [Background technology]

[0003] Polybutene is a compound used as a raw material for a variety of chemical products, such as lubricating oil additives and fuel detergents.

[0004] Polybutene is generally produced by polymerizing olefin components with a carbon number of 4 (C4) derived from the naphtha cracking process using a Friedel-Craft type catalyst. The raw material used is C4 raffinate-1, which is the residue left after extracting 1,3-butadiene from the C4 raw material. It contains paraffins such as isobutane and normal butane, and olefins such as 1-butene, 2-butene, and isobutene. Among the olefin components of the C4 raffinate-1, isobutene, which accounts for approximately 30 to 50% by weight, has the highest reactivity, so the produced polybutene is mainly composed of isobutene units.

[0005] Polyisobutene is classified into low, medium and high molecular weight ranges according to the molecular weight range. Low molecular weight polyisobutene has a number average molecular weight of about 10,000 or less, and there are two product groups: normal polybutene and high reactive polybutene (HR-PB). The high reactive polybutene has carbon-carbon double bonds mainly located at the terminals of polybutene, and is used as a fuel additive or engine oil additive after introducing functional groups using terminal vinylidene functional groups (>80%).

[0006] Polybutene is a liquid oligomer, and its viscosity increases with increasing molecular weight. Polybutene is obtained after polymerization in the form of a mixed solution with a reaction solvent, and methods for separating polybutene from the solution include a method using a distillation column, a method using a flash drum, and a method using a devolatilizer.

[0007] Among these, the distillation column can separate a mixture at high purity by utilizing the difference in boiling points, but has the problem that it is difficult to handle high-viscosity substances and the separation efficiency drops sharply as the viscosity increases. On the other hand, the flash drum or devolatilizer boils low-boiling point substances in the mixture state and removes them to the top, and collects the remaining substances at the bottom, so it can handle high-viscosity substances and has low equipment costs, but has the problem that it is difficult to separate at high purity.

[0008] Therefore, there is a need to develop a separation method that can separate oligomers or polymers and reaction solvents with high purity with excellent separation efficiency, and in particular, can reduce the residual content of a specific solvent in the oligomer or polymer to an extremely low level. Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide a method for separating polybutene, which can separate oligomers or polymers and reaction solvents with high purity with excellent separation efficiency. [Means for solving the problem]

[0010] In order to achieve the above object, the present invention provides a method for separating polybutene, comprising: (1) introducing into a distillation column a polybutene solution containing polybutene, a halogenated hydrocarbon solvent, and a non-polar hydrocarbon solvent, and having a viscosity of 1 cp to 50 cp as measured using a rotational viscometer at 25° C.; (2) separating the halogenated hydrocarbon solvent and the non-polar hydrocarbon solvent from an upper portion of the distillation column, and separating from a lower portion of the distillation column a polybutene solution containing polybutene and the non-polar hydrocarbon solvent, and having a viscosity of 10 cp to 150 cp; and (3) separating the non-polar hydrocarbon solvent and polybutene from the polybutene solution separated from the lower portion of the distillation column via step (2). Effect of the Invention

[0011] According to the method for separating polybutene of the present invention, polybutene oligomer or polymer can be separated with high efficiency from a polybutene solution after polymerization, the residual content of the solvent contained in the polybutene oligomer or polymer can be reduced to an extremely low level, and the energy consumption used in the separation process of the entire oligomer or polymer can be reduced, so that the method can be useful in the production process of polybutene oligomer or polymer. [Brief description of the drawings]

[0012] The following drawings in this specification are illustrative of preferred embodiments of the present invention and, together with the above-mentioned invention, serve to further understand the technical concept of the present invention, and therefore the present invention should not be interpreted as being limited only to the matters depicted in such drawings. [Figure 1] FIG. 1 is a schematic diagram showing an example of a separation system used in a method for separating polybutene according to an example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will now be described in further detail to aid in the understanding of the present invention.

[0014] The terms and words used in the description of the present invention and the claims should not be interpreted limited to their ordinary or dictionary meanings, but should be interpreted as meanings and concepts that fit the technical idea of ​​the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to best describe his / her invention.

[0015] The term "oligomer" as used herein means a low polymer formed by small polymerization of monomers and having a number average molecular weight in the range of less than 10,000.

[0016] As a concept relative to the oligomer, the term "polymer" refers to a polymer compound formed by polymerizing monomers and having a number average molecular weight of 10,000 or more.

[0017] In the present invention, the terms "comprising", "including", "having" and their derivatives are not intended to exclude the presence of any additional components, steps or procedures, whether or not they are specifically disclosed. To avoid any uncertainty, all compositions claimed through the use of the term "comprising" may contain any additional additives, adjuvants, or compounds, whether polymeric or otherwise, unless stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any consecutive description any other component, step or procedure, except that it is not essential to operability. The term "consisting of" excludes any component, step or procedure not specifically described or listed.

[0018] The method for separating polybutene according to the present invention includes the steps of: (1) introducing a polybutene solution containing polybutene, a halogenated hydrocarbon solvent, and a non-polar hydrocarbon solvent, and having a viscosity of 1 cp to 50 cp as measured using a rotational viscometer at 25° C., into a distillation column; (2) separating the halogenated hydrocarbon solvent and the non-polar hydrocarbon solvent from an upper portion of the distillation column, and separating a polybutene solution containing polybutene and the non-polar hydrocarbon solvent, and having a viscosity of 10 cp to 150 cp, from a lower portion of the distillation column; and (3) separating the non-polar hydrocarbon solvent and polybutene from the polybutene solution separated from the lower portion of the distillation column via step (2).

[0019] (1) Feeding a polybutene solution containing polybutene, a halogenated hydrocarbon solvent, and a non-polar hydrocarbon solvent and having a viscosity of 1 cp to 50 cp as measured at 25° C. using a rotational viscometer into a distillation column The polybutene solution introduced into the distillation column in step (1) is a polybutene solution containing polymerized polybutene, a halogenated hydrocarbon solvent, and a non-polar hydrocarbon solvent, and is not particularly limited as long as it is a solution of a polybutene oligomer or polymer product obtained by a method for producing polybutene using isobutene monomer known in the art. The solvent contained in the polybutene solution in step (1) includes a halogenated hydrocarbon solvent and a non-polar hydrocarbon solvent.

[0020] In the method for separating polybutene of the present invention, the polymerized polybutene may be obtained by polymerizing a polymerization solution containing a mixed solvent of a halogenated hydrocarbon solvent and a non-polar hydrocarbon solvent, and an isobutene monomer. When a mixed solvent containing a halogenated hydrocarbon solvent and a non-polar hydrocarbon solvent is used for the polymerization of polybutene, there is an effect that the toxicity of the halogenated hydrocarbon solvent is reduced compared to the case where a halogenated hydrocarbon solvent is used alone.

[0021] In addition, the polarity of the solvent affects the reactivity during polymerization of polybutene, but polybutene oligomers in the low molecular weight range can be obtained by mixing a non-polar hydrocarbon solvent with a halogenated hydrocarbon solvent to control the dielectric constant of the mixed solvent.

[0022] The halogenated hydrocarbon solvent may be one or more selected from the group consisting of chloromethane, dichloromethane, trichloromethane, 1-chlorobutane, and chlorobenzene, and the non-polar hydrocarbon solvent may be an aliphatic hydrocarbon solvent, an aromatic hydrocarbon solvent, or a mixture thereof. For example, it may be one or more selected from the group consisting of butane, pentane, neopentane, hexane, cyclohexane, methylcyclohexane, heptane, octane, benzene, toluene, xylene, and ethylbenzene. The aliphatic hydrocarbon solvent may be one or more selected from the group consisting of butane, pentane, neopentane, hexane, cyclohexane, methylcyclohexane, heptane, and octane, and the aromatic hydrocarbon solvent may be one or more selected from the group consisting of benzene, toluene, xylene, and ethylbenzene.

[0023] In the method for separating polybutene of the present invention, the polybutene solution fed into the distillation column may have a viscosity of 1 cp to 50 cp, specifically 2 cp to 40 cp, more specifically 3 cp to 30 cp, as measured at 25° C. using a rotational viscometer.

[0024] The polybutene solution may have a solids content of 10% to 25% by weight, specifically 10% to 20% by weight, and more specifically 15% to 20% by weight.

[0025] (2) separating the halogenated hydrocarbon solvent and the non-polar hydrocarbon solvent from the top of the distillation column, and separating a polybutene solution containing polybutene and the non-polar hydrocarbon solvent and having a viscosity of 10 cp to 150 cp from the bottom of the distillation column. In step (2), the halogenated hydrocarbon solvent is mainly removed using a distillation column. Specifically, the polybutene solution is introduced into a distillation column, and the temperature, pressure, and reflux ratio of the distillation column are adjusted to separate the halogenated hydrocarbon solvent and a portion of the non-polar hydrocarbon solvent from the top of the distillation column, and a polybutene solution containing polybutene and the non-polar hydrocarbon solvent and having a viscosity of 10 cp to 150 cp is separated from the bottom of the distillation column.

[0026] The halogenated hydrocarbon solvent is removed by separating the halogenated hydrocarbon solvent from the top of the distillation column. In step (2), the halogenated hydrocarbon solvent and a portion of the non-polar hydrocarbon solvent are separated from the top of the distillation column. When the reflux ratio of the distillation column is increased, the ratio of the halogenated hydrocarbon solvent in the solvent separated from the top of the distillation column can be increased. However, in order to increase the reflux ratio of the distillation column, a lot of energy must be used for distillation, so in order to separate mainly only the halogenated hydrocarbon solvent from the top of the distillation column, a lot of energy must be used for distillation to increase the reflux ratio of the distillation column. On the other hand, when the reflux ratio of the distillation column is decreased, the halogenated hydrocarbon solvent may remain in the polybutene solution separated from the bottom of the distillation column.

[0027] Therefore, in step (2), the reflux ratio of the distillation column must be adjusted so that the amount of halogenated hydrocarbon solvent remaining in the finally separated polybutene can be appropriately reduced while not wasting energy unnecessarily.

[0028] In the step (2), the reflux ratio of the distillation column may be 0.1 to 1, specifically 0.2 to 1, and more specifically 0.2 to 0.4. When the reflux ratio of the distillation column satisfies the above range, the content of halogenated hydrocarbon solvent contained in the polybutene solution separated from the bottom of the distillation column is appropriately reduced, so that the residual content of halogenated hydrocarbon contained in the final polybutene can be at an extremely low level.

[0029] When the reflux ratio of the distillation column satisfies the above range, the solvent separated from the top of the distillation column in step (2) comprises a halogenated hydrocarbon solvent and a non-polar hydrocarbon solvent, and the halogenated hydrocarbon solvent and the non-polar hydrocarbon solvent may have a weight ratio of 20:80 to 80:20, specifically a weight ratio of 30:70 to 80:20, more specifically a weight ratio of 40:60 to 70:30.

[0030] In step (2), the temperature at the top of the distillation column may be 50°C to 70°C, and the temperature at the bottom may be 85°C to 105°C, specifically, the temperature at the top of the distillation column may be 54°C to 66°C, and the temperature at the bottom may be 85°C to 102°C, more specifically, the temperature at the top of the distillation column may be 54.2°C to 66.0°C, and the temperature at the bottom may be 85.8°C to 101.8°C.

[0031] In step (2), the pressure of the distillation column may be from 1.5 bar to 3 bar, specifically from 1.5 bar to 2.5 bar, and more specifically from 1.5 bar to 2 bar.

[0032] Meanwhile, the temperature of the distillation column may be determined by the pressure of the distillation column. In one embodiment of the present invention, for example, when the pressure of the column is 1.5 bar, the temperature at the top of the distillation column may be 54.2°C to 56.6°C, and the temperature at the bottom may be 85.8°C to 90.6°C, and when the pressure of the column is 2.0 bar, the temperature at the top of the distillation column may be 63.5°C to 66.0°C, and the temperature at the bottom may be 96.5°C to 101.8°C. The temperature of the distillation column may be adjusted according to the viscosity and solid content of the polybutene solution, and for example, the temperature of the column may increase as the viscosity and solid content of the polybutene solution increase.

[0033] When the temperature, pressure and reflux ratio of the distillation column satisfy the above ranges, a polybutene solution containing polybutene and a non-polar hydrocarbon solvent and having a viscosity of 10 cp to 150 cp can be separated from the bottom of the distillation column. The viscosity of the polybutene solution can be specifically 15 cp to 120 cp, more specifically 20 cp to 100 cp. The solid content of the polybutene solution containing polybutene and a non-polar hydrocarbon solvent can be 40 wt% to 60 wt%, specifically 40 wt% to 55 wt%, more specifically 43 wt% to 50 wt%.

[0034] The polybutene solution separated from the bottom of the distillation column may have a viscosity and solids content within the above ranges. When the above ranges are satisfied, separation of polybutene, non-polar hydrocarbon solvent, and halogenated hydrocarbon solvent through the distillation column is properly performed, and when the viscosity of the polybutene solution separated from the bottom of the distillation column increases, the separation efficiency of the distillation column decreases, which may prevent the problem of operation becoming difficult.

[0035] In the method for separating polybutene of the present invention, the halogenated hydrocarbon solvent is separated through the top of the distillation column, and a sufficient amount of solvent is separated from the bottom together with polybutene, thereby allowing the polybutene solution to maintain a low viscosity, thereby preventing a decrease in separation efficiency of the distillation column and difficulty in operation when the viscosity of the polybutene solution separated from the bottom increases. That is, the method for separating polybutene of the present invention includes a process of controlling the pressure, temperature, and reflux ratio of the distillation column to effectively remove the halogenated hydrocarbon solvent from the top of the distillation column without inputting excessive energy, and controlling the amount of non-polar hydrocarbon solvent contained in polybutene so that a polybutene solution having a viscosity in the above range can be separated from the bottom of the distillation column.

[0036] (3) separating the non-polar hydrocarbon solvent and polybutene from the polybutene solution separated from the bottom of the distillation column in step (2); The polybutene solution separated from the bottom of the distillation column in step (2) is a solution from which the halogenated hydrocarbon solvent is primarily separated, and the remaining non-polar hydrocarbon solvent can be removed in step (3).

[0037] The step of separating the non-polar hydrocarbon solvent and polybutene from the polybutene solution separated from the lower part of the distillation column may be performed, for example, using a devolatilizer. When the non-polar hydrocarbon solvent and polybutene are separated using the devolatilizer, the non-polar hydrocarbon solvent may be separated from the upper part of the devolatilizer, and high-viscosity polybutene may be separated from the lower part.

[0038] In one embodiment of the present invention, the temperature of the devolatilizer may be 180°C to 320°C, and the pressure may be 0.4 bar to 1.2 bar, and specifically, the temperature of the devolatilizer may be 200°C to 300°C, and the pressure may be 0.5 bar to 1 bar. If the pressure of the devolatilizer decreases, the energy used for increasing the temperature decreases, but the entrainment phenomenon in which the polymer rises to the top occurs, and if the pressure of the devolatilizer increases, the entrainment phenomenon in which the polymer rises to the top decreases, but the energy used for increasing the temperature increases, so the pressure of the devolatilizer may be adjusted to satisfy the pressure range. In addition, the temperature of the devolatilizer may be adjusted according to the pressure, and if the pressure decreases, the temperature may decrease, and if the pressure increases, the temperature may increase, and may be appropriately adjusted within the temperature range.

[0039] The polybutene solution separated from the lower part of the distillation column may be heated before being fed into the devolatilizer, and thus the present invention may further include passing the polybutene solution separated from the lower part of the distillation column through a preheater before being fed into the devolatilizer. By passing through the preheater, the amount of heat required to vaporize the non-polar hydrocarbon solvent contained in the polybutene solution can be supplied.

[0040] The polybutene solution separated from the bottom of the distillation column in step (2) is obtained by separating the halogenated hydrocarbon solvent through the distillation column, but may still contain some halogenated hydrocarbon solvent. For example, the polybutene solution separated from the bottom of the distillation column may contain, for example, 100 ppm to 5,000 ppm of halogenated hydrocarbon solvent, specifically 300 ppm to 3,000 ppm of halogenated hydrocarbon solvent, and more specifically 500 ppm to 1,000 ppm of halogenated hydrocarbon solvent. The halogenated hydrocarbon solvent contained in the polybutene solution may be further removed from the polybutene together with the non-polar hydrocarbon solvent in the step of separating the non-polar hydrocarbon solvent and polybutene in step (3).

[0041] Thus, the polybutene separated in step (3) may contain less than 5 ppm of halogenated hydrocarbon solvent and less than 0.05 wt. % of non-polar hydrocarbon solvent, specifically 1 ppm to 5 ppm of halogenated hydrocarbon solvent and 0.01 wt. % to 0.05 wt. % of non-polar hydrocarbon solvent.

[0042] FIG. 1 is a schematic diagram showing an example of a separation system used in a method for separating polybutene according to an embodiment of the present invention.

[0043] As shown in FIG. 1, a separation system used in a method for separating polybutene according to an embodiment of the present invention includes a distillation column 100 and a devolatilizer 200. In one embodiment of the present invention, a polybutene solution containing polybutene, a halogenated hydrocarbon solvent, and a non-polar hydrocarbon solvent and having a solid content of 10% to 25% by weight is fed into the distillation column 100 through a first feed line 110, and a first solvent discharge line 120 is disposed at the top of the distillation column 100, from which the halogenated hydrocarbon solvent and the non-polar hydrocarbon solvent are separated and discharged. A first discharge line 130 is disposed at the bottom of the distillation column 100, from which a polybutene solution containing polybutene and a non-polar hydrocarbon solvent and having a solid content of 40% to 60% by weight is discharged. The polybutene solution discharged from the first discharge line 130 is fed to the devolatilizer 200 through a second supply line 210 connected to the devolatilizer 200, and may be heated by passing through a preheater 240 before being fed to the devolatilizer 200. A second solvent discharge line 220 is located at the top of the devolatilizer 200, from which the non-polar hydrocarbon solvent is separated and discharged, and a second discharge line 230 is located at the bottom of the devolatilizer 200, from which polybutene is separated and discharged.

[0044] [Example] Hereinafter, the present invention will be described in more detail with reference to examples and experimental examples. However, the present invention is not limited to these examples and experimental examples. The embodiments according to the present invention may be modified in several different forms, and the scope of the present invention should not be construed as being limited to the examples detailed below. The examples of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.

[0045] In the following examples and comparative examples, the separation method according to the present invention was simulated using a commercial process replicating program ASPEN PLUS. Constants required for the simulation were values ​​built into the program, values ​​listed in the literature, etc.

[0046] <Polymerization example: Production of polybutene> A continuous polymerization was carried out by feeding 1,000kg / hr of isobutylene as a monomer, and 1,600kg / hr of dichloromethane and 2,400kg / hr of n-hexane as solvents into the reactor. When the polymerization was completed, the catalyst was removed by passing through an adsorption tower, and a polymer solution was obtained after polymerization through this. The polymer solution had a polymer of 1,000kg / hr, 1,600kg / hr of dichloromethane (DCM), and 2,400kg / hr of n-hexane. The viscosity of the polymer solution was 30cp when measured using a rotational viscometer at 25℃.

[0047] [Example 1] In order to separate the solvent and the polymer, the polymer solution obtained in the polymerization example was fed into a distillation column. At this time, the column temperature, pressure and reflux ratio were adjusted to a column pressure of 1.5 bar, the temperature at the top / bottom of the column of 54.2°C / 85.8°C, and the reflux ratio of 0.2, and 1,600 kg / hr of dichloromethane (DCM) and 900 kg / hr of n-hexane were obtained from the top of the distillation column. In this case, 1,000 kg / hr of polybutene polymer and the remaining 1,500 kg / hr of n-hexane were obtained from the bottom of the distillation column. The polybutene polymer solution obtained at the bottom was fed into a devolatilizer via a preheater. The temperature and pressure conditions were 200°C and 0.5 bar. 999.5 kg / hr of n-hexane was obtained at the top of the devolatilizer, and polybutene polymer was obtained at the bottom. In this case, the content of DCM in the polymer was 5 ppm based on the total content of the polymer, and the content of n-hexane was 0.05 wt %.

[0048] [Example 2] The same process as in Example 1 was carried out, except that the reflux ratio was adjusted to 0.1. 1,600 kg / hr of dichloromethane (DCM) and 900 kg / hr of n-hexane were obtained from the top of the distillation column, 1,000 kg / hr of polybutene polymer and the remaining 1,500 kg / hr of n-hexane were obtained from the bottom of the distillation column, and 999.5 kg / hr of n-hexane was obtained from the top of the devolatilizer and polybutene polymer was obtained from the bottom. The content of DCM in the polymer was 10 ppm based on the total content of the polymer, and the content of n-hexane was 0.05 wt%.

[0049] [Example 3] The same process as in Example 1 was carried out, except that the reflux ratio was adjusted to 0.4. 1,600 kg / hr of dichloromethane (DCM) and 900 kg / hr of n-hexane were obtained from the top of the distillation column, 1,000 kg / hr of polybutene polymer and the remaining 1,500 kg / hr of n-hexane were obtained from the bottom of the distillation column, and 999.5 kg / hr of n-hexane was obtained from the top of the devolatilizer and polybutene polymer was obtained from the bottom. The content of DCM in the polymer was 5 ppm based on the total content of the polymer, and the content of n-hexane was 0.05 wt%.

[0050] [Example 4] The same process as in Example 1 was carried out, except that the reflux ratio was adjusted to 0.8. 1,600 kg / hr of dichloromethane (DCM) and 900 kg / hr of n-hexane were obtained from the top of the distillation column, 1,000 kg / hr of polybutene polymer and the remaining 1,500 kg / hr of n-hexane were obtained from the bottom of the distillation column, and 999.5 kg / hr of n-hexane was obtained from the top of the devolatilizer and polybutene polymer was obtained from the bottom. The content of DCM in the polymer was 1.5 ppm based on the total content of the polymer, and the content of n-hexane was 0.05 wt%.

[0051] [Example 5] The same process as in Example 1 was carried out, except that the reflux ratio was adjusted to 1.0. 1,600 kg / hr of dichloromethane (DCM) and 900 kg / hr of n-hexane were obtained from the top of the distillation column, 1,000 kg / hr of polybutene polymer and the remaining 1,500 kg / hr of n-hexane were obtained from the bottom of the distillation column, and 999.5 kg / hr of n-hexane was obtained from the top of the devolatilizer and polybutene polymer was obtained from the bottom. The content of DCM in the polymer was 5 ppm based on the total content of the polymer, and the content of n-hexane was 0.05 wt%.

[0052] [Example 6] In order to separate the solvent and the polymer, the polymer solution obtained in the polymerization example was fed into a distillation column. At this time, the column temperature, pressure and reflux ratio were adjusted to a column pressure of 1.5 bar, the temperature at the top / bottom of the column of 56.6°C / 90.6°C, and the reflux ratio of 0.2, and 1,600 kg / hr of DCM and 1,730 kg / hr of n-hexane were obtained from the top of the distillation column. In this case, 1,000 kg / hr of polymer and the remaining 670 kg / hr of n-hexane were obtained from the bottom of the distillation column. The polybutene polymer solution obtained at the bottom was fed into a devolatilizer via a preheater. The temperature and pressure conditions were 200°C and 0.5 bar. 999.5 kg / hr of n-hexane was obtained at the top of the devolatilizer, and polybutene polymer was obtained at the bottom. In this case, the content of DCM in the polymer was 5 ppm based on the total content of the polymer, and the content of n-hexane was 0.05 wt%.

[0053] [Example 7] In order to separate the solvent and the polymer, the polymer solution obtained in the polymerization example was fed into a distillation column. At this time, the column temperature, pressure and reflux ratio were adjusted to 1.5 bar column pressure, 51.6°C / 84.6°C temperature at the top / bottom of the column, and 3.0, so that 1,000 kg / hr of polymer and 2,250 kg / hr of n-hexane were obtained at the bottom of the distillation column, and the solid content was about 30 wt%. In this case, 1,600 kg / hr of DCM and 150 kg / hr of n-hexane were obtained at the top of the distillation column. In order to obtain mainly DCM at the top while not leaving DCM at the bottom of the distillation column, the reflux ratio had to be increased, and a lot of energy was input. Then, it was fed into a devolatilizer through a preheater, and the temperature and pressure conditions were the same as in Example 1. The DCM content and n-hexane content in the polybutene polymer at the bottom were the same as in Example 1.

[0054] [Example 8] The same process as in Example 1 was carried out, except that the reflux ratio was adjusted to 0.08. 1,600 kg / hr of dichloromethane (DCM) and 900 kg / hr of n-hexane were obtained from the top of the distillation column, 1,000 kg / hr of polybutene polymer and the remaining 1,500 kg / hr of n-hexane were obtained from the bottom of the distillation column, and 999.5 kg / hr of n-hexane was obtained from the top of the devolatilizer and polybutene polymer was obtained from the bottom. The content of DCM in the polymer was 20 ppm based on the total content of the polymer, and the content of n-hexane was 0.05 wt%.

[0055] [Comparative Example 1] The polymer solution obtained in the polymerization example was fed into a flash drum instead of a distillation column. The temperature and pressure of the flash drum were adjusted to 71.5° C. and 1.5 bar, respectively, and 1,000 kg / hr of polymer and 1,000 kg / hr of solvent were obtained from the bottom. At this time, about 200 kg / hr of DCM and about 800 kg / hr of n-hexane were present in the solvent. The polymer solution obtained at the bottom was fed into a devolatilizer via a preheater as in Example 1. The temperature and pressure conditions were the same as in Example 1. The polymer was obtained at the bottom of the devolatilizer, and in this case, the content of DCM in the polymer was at the level of 60 ppm based on the total content of the polymer, and the content of n-hexane was 0.05 wt%.

[0056] [Comparative Example 2] The polymer solution obtained in the polymerization example was introduced into a distillation column in the same manner as in Example 1. The column temperature, pressure and reflux ratio were adjusted to 1.5 bar (column pressure), 58.6°C / 150°C (upper / lower temperature), and 0.2 (reflux ratio) to obtain a polymer at the bottom of the distillation column, with the DCM content being 5 ppm and the n-hexane content being 15 wt% relative to the polymer content. The polymer obtained at the bottom had a solid content of 85 wt% and a very high viscosity of 1,500 cp.

[0057] <Experimental Example> <Viscosity measurement> In Examples 1 to 8 and Comparative Examples 1 and 2, the viscosity of each polybutene polymer solution obtained from the bottom of the distillation column or flash drum was measured.

[0058] The viscosity was measured using a Brookfield viscometer equipped with a spindle for measuring a shear rate of 100 / s, and the spindle was immersed in a container filled with each of the polybutene polymer solutions, and the viscosity was measured for about 1 minute at 25° C. The results of the viscosity measurement are shown in Table 1 below.

[0059] <Measurement of DCM content and n-hexane content in polymer> The contents of DCM and n-hexane in the polymers obtained in Examples 1 to 8 and Comparative Examples 1 and 2 were analyzed by gas chromatography (GC / FID, GC-03).

[0060] After stabilizing the instrument and injecting a standard sample (DCM or n-hexane) to prepare a calibration curve, the sample was injected and the content was calculated using the calibration curve.

[0061] [GC / FID conditions] Method type: Measurement method - quantitative analysis Column:DB-5(0.53mm ID x 30mL, 1.5μmd.f.capillary) Oven temperature:Initial Value & Time:50℃、5min Program Rate: 15℃ / min Final Value & Time: 300℃, 10min Detector temperature: 300℃ Gas Flow rate:Column(He):5mL / min Injector:on column Injection volume: 0.2μL <Steam energy consumption> The required heat amount (duty) was calculated using Aspen Plus under the process conditions of Examples 1 to 8 and Comparative Examples 1 and 2, and converted into the required steam energy. 2 kg / hr of steam energy is required per 1 Mcal / hr of heat amount.

[0062] <Equipment cleaning cycle> The equipment cleaning cycles during polybutene separation in Examples 1 to 8 and Comparative Examples 1 and 2 were measured and are shown in Table 1 below. The equipment cleaning cycles were determined by measuring the time when polymer deposition gradually progresses in the reboiler of the distillation column, the devolatilizer, or the preheater of the flash drum, and the heat exchanger cannot be controlled at the target temperature.

[0063] [Table 1]

[0064] Referring to Table 1, the methods of Examples 1 to 8 were able to simultaneously achieve low DCM and n-hexane contents in the polymer, but when a flash drum was used instead of a distillation column as in Comparative Example 1, the DCM content in the polymer was high, and when only a distillation column was used as in Comparative Example 2, the DCM content in the polymer could be reduced, but the n-hexane content was high, and since the viscosity of the polymer obtained from the bottom of the distillation column was high, the polymer deposition in the device became severe, and the device had to be cleaned more frequently. As a result, it was confirmed that the method for separating polybutene according to one embodiment of the present invention can effectively separate residual solvent from the polybutene produced, while also solving the problem of polymer deposition occurring when the viscosity of the polybutene polymer obtained from the bottom of the distillation column is high.

[0065] Meanwhile, when examining the results of Examples 1 to 8, in Example 6, the viscosity of the polybutene solution obtained from the bottom of the distillation column before being fed into the devolatilizer was 140 cp, and in this case, compared with Examples 1 to 5, 7, and 8, in which the viscosity was 20 to 30 cp, polymer deposition increased and the equipment cleaning cycle increased from twice a year to three times a year. Therefore, it was confirmed that in order to reduce the equipment cleaning cycle, it is necessary to additionally adjust the viscosity of the polybutene solution obtained from the bottom of the distillation column as necessary.

[0066] In addition, in the case of Example 7, low DCM and n-hexane contents were achieved in the final polymer, and the equipment cleaning cycle was also maintained at a low level. However, a large amount of steam energy was used by increasing the reflux ratio to separate DCM and n-hexane into pure water at the top and bottom of the distillation column, respectively. In the case of Example 8, although the amount of steam energy used was similar to that of Examples 3 and 4, the DCM content in the final polymer was relatively high at 20 ppm. Therefore, it was confirmed that it is necessary to further adjust the process conditions to obtain a more appropriate reflux ratio in order to effectively remove DCM while reducing the energy consumption used in the entire oligomer or polymer separation process.

[0067] As a result, as in the method of the present invention, for a polybutene solution containing polybutene, a halogenated hydrocarbon solvent, and a non-polar hydrocarbon solvent, a polybutene solution having a viscosity of 10 cp to 150 cp is first separated from the halogenated hydrocarbon solvent and the non-polar hydrocarbon solvent through a distillation column, and a non-polar hydrocarbon solvent and polybutene are separated from the polybutene solution having a viscosity of 10 cp to 150 cp. In addition, the method can minimize the halogenated hydrocarbon solvent contained in the polybutene solution by controlling the viscosity of the polybutene solution obtained from the bottom of the distillation column during the process and by controlling the reflux ratio of the distillation column during the process. It has been confirmed that the method can provide even more excellent effects, such as solving the problem of polymer deposition in the apparatus due to the high viscosity of the polymer obtained from the bottom of the distillation column and increasing the frequency of cleaning the apparatus. [Explanation of symbols]

[0068] 100: Distillation column 110: First feed line 120: First solvent discharge line 130: First discharge line 200: Devolatilizer 210: Second supply line 220: Second solvent discharge line 230: Second discharge line 240: Preheater

Claims

1. (1) introducing a polybutene solution containing polybutene, a halogenated hydrocarbon solvent, and a non-polar hydrocarbon solvent and having a viscosity of 1 cp to 50 cp as measured at 25° C. using a rotational viscometer into a distillation column; (2) separating the halogenated hydrocarbon solvent and the non-polar hydrocarbon solvent from the top of the distillation column, and separating a polybutene solution containing the polybutene and the non-polar hydrocarbon solvent and having a viscosity of 10 cp to 150 cp from the bottom of the distillation column; and (3) separating the non-polar hydrocarbon solvent and the polybutene from the polybutene solution separated from the bottom of the distillation column via step (2); In step (2), the reflux ratio of the distillation column is from 0.1 to 1; In the step (2), the temperature at the top of the distillation column is 50° C. to 70° C., and the temperature at the bottom is 85° C. to 105° C.; In step (2), the pressure of the distillation column is 1.5 bar to 3 bar; The step of separating the non-polar hydrocarbon solvent and the polybutene includes the steps of: feeding the polybutene solution separated from the lower part of the distillation column into a devolatilizer; separating the non-polar hydrocarbon solvent from the upper part of the devolatilizer; and separating the polybutene from the lower part of the devolatilizer. Method for separating polybutene.

2. 2. The method for separating polybutene according to claim 1, wherein the polybutene solution fed into the distillation column has a solid content of 10% by weight to 25% by weight.

3. 3. The method for separating polybutene according to claim 1 or 2, wherein the halogenated hydrocarbon solvent and the non-polar hydrocarbon solvent separated from the top of the distillation column in step (2) have a weight ratio of 20:80 to 80:

20.

4. The method for separating polybutene according to any one of claims 1 to 3, wherein the polybutene solution separated from the bottom of the distillation column in step (2) has a viscosity of 15 cp to 120 cp.

5. The method for separating polybutene according to any one of claims 1 to 4, wherein the polybutene solution separated from the bottom of the distillation column in step (2) contains 100 ppm to 5,000 ppm of halogenated hydrocarbon solvent.

6. The polybutene solution separated from the bottom in step (2) comprises polybutene having a solid content of 40% by weight to 60% by weight and a non-polar hydrocarbon solvent.

7. The method for separating polybutene according to any one of claims 1 to 6, further comprising passing the polybutene solution separated from the bottom of the distillation column through a preheater before being introduced into the devolatilizer.

8. The method for separating polybutene according to any one of claims 1 to 7, wherein the temperature of the devolatilizer is from 180°C to 320°C and the pressure is from 0.4 bar to 1.2 bar.

9. The method for separating polybutene according to any one of claims 1 to 8, wherein the polybutene separated in step (3) contains 5 ppm or less of halogenated hydrocarbon solvents and 0.05 wt. % or less of non-polar hydrocarbon solvents.

10. The method for separating polybutene according to any one of claims 1 to 9, wherein the halogenated hydrocarbon solvent is one or more selected from the group consisting of chloromethane, dichloromethane, trichloromethane, 1-chlorobutane, and chlorobenzene.

11. The method for separating polybutene according to any one of claims 1 to 10, wherein the non-polar hydrocarbon solvent is one or more selected from the group consisting of butane, pentane, neopentane, hexane, cyclohexane, methylcyclohexane, heptane, octane, benzene, toluene, xylene, and ethylbenzene.