Masterbatch for foam molding and foam molding
The masterbatch for foam molding, with a base resin and thermally expandable microcapsules of specified properties, addresses issues of expansion ratio, foaming speed, and appearance quality, delivering high-quality foamed products under strong shearing and low temperature conditions.
Patent Information
- Application Number
- JP2022025830
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-18
- Filing Date
- 2022-02-22
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2039-09-12
AI Technical Summary
Existing foam molding technologies face challenges in achieving high expansion ratios, suppressing foaming speed, maintaining good appearance quality, and ensuring uniform closed cell formation, particularly when strong shearing forces or low molding temperatures are involved, due to issues with chemical foaming agents and thermally expandable microcapsules.
A masterbatch for foam molding comprising a base resin with specific melt flow rate and melting point, combined with thermally expandable microcapsules of defined particle diameter and content, is used to control foaming speed and enhance appearance quality, while ensuring high expansion ratios and uniform cell formation.
The solution provides a foamed molded product with high expansion ratios, suppressed foaming speed, and excellent appearance quality, even under challenging conditions, while minimizing shearing and foaming variations during production.
Smart Images

Figure 0007564141000001 
Figure 0007564141000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a masterbatch for expansion molding which can be suitably used in molding where a strong shear force is applied or where a low molding temperature is required, and which can produce a foamed molded article having a high expansion ratio, a controlled expansion rate, and good appearance quality. The present invention also relates to a foamed molded article using the masterbatch for expansion molding. [Background technology]
[0002] Plastic foams are used in various applications because they can exhibit heat insulation, heat insulation, sound insulation, sound absorption, vibration resistance, weight reduction, etc. depending on the material of the foam and the state of the formed bubbles. One method for producing such plastic foams is to heat a master batch containing a chemical foaming agent to foam and mold it. However, master batches containing chemical foaming agents may not foam even when heated, and there is a risk of the foaming agent suddenly decomposing in an injection foam molding machine, making them difficult to handle. In addition, depending on the type of resin, it may be difficult to obtain a sufficient expansion ratio, making it difficult to obtain the desired hardness as a molded product.
[0003] On the other hand, Patent Document 1 describes that by using master batch pellets of an ethylene-α-olefin copolymer containing a chemical foaming agent, it is possible to obtain an injection foamed molded product having high hardness and expansion ratio and having uniform bubbles, regardless of the type of resin. However, when chemical foaming agents are decomposed by heating, they produce decomposition gas and foaming residue at the same time, and the residue remaining in the molded product can affect the adhesive properties of the molded product. In addition, when chemical foaming agents are used, not all cells are closed, and some parts are open, making it difficult to obtain a foamed molded product with high airtightness.
[0004] Patent Document 2 describes a foaming resin masterbatch that uses a polyolefin resin or a styrene resin as a base resin and uses thermally expandable microcapsules as a foaming agent instead of a chemical foaming agent. However, when the thermally expandable microcapsules described in Patent Document 2 were used, the expansion ratio of the resulting foam was low, and it was difficult to make the closed cells of the resulting foam have a uniform size.
[0005] In response to this, Patent Document 3 describes a method for producing a foamed composite board by foaming and molding a resin composition obtained by blending a masterbatch containing thermally expandable microcapsules with a masterbatch containing a chemical foaming agent. However, even when such a method is used, although some improvement in the expansion ratio is observed, the expansion ratio of the molded product is still low, and it is not possible to obtain the desired performance such as light weight and heat insulation. In addition, it is difficult to obtain a product with good appearance quality.
[0006] Furthermore, Patent Document 4 discloses a synthetic resin composition containing a thermally expandable microcapsule and a base resin, and a method for producing the same. In such a synthetic resin composition, by using a base resin having a melt flow rate within a predetermined range, it is said that the shells of the thermally expandable microcapsules are not destroyed, and the compatibility and affinity between the thermally expandable microcapsules and the base resin are excellent. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2000-178372 A [Patent Document 2] Japanese Patent Application Publication No. 11-343362 [Patent Document 3] JP 2005-212377 A [Patent Document 4] JP 2002-264173 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention aims to provide a masterbatch for expansion molding which can be suitably used in molding where a strong shear force is applied or where a low molding temperature is required, and which can give a foamed molded article having a high expansion ratio, a controlled expansion rate, and good appearance quality. Another aim of the present invention is to provide a foamed molded article using the masterbatch for expansion molding. [Means for solving the problem]
[0009] The present invention is a masterbatch for foam molding containing a base resin and thermally expandable microcapsules, wherein the base resin contains a resin having a melt flow rate of 0.1 to 60 g / 10 min and a melting point of 70 to 110°C, the thermally expandable microcapsules have an average particle diameter of 15 to 35 μm, and the content of the thermally expandable microcapsules is 52 to 70% by weight. The present invention will be described in detail below.
[0010] As a result of intensive research, the present inventors have found that when a resin having a predetermined melt flow rate and melting point is used as a base resin, and thermally expandable microcapsules are used as a foaming component, and the average particle size and content of the thermally expandable microcapsules are within a predetermined range, the composition can be suitably used in molding in which a strong shear force is applied or molding in which a low molding temperature is required. In addition, the present inventors have found that a foamed molded product having a high expansion ratio and good appearance quality can be obtained, and have completed the present invention.
[0011] The foam molding masterbatch of the present invention contains a base resin. In the present invention, the base resin contains a resin having a predetermined melt flow rate and melting point. This makes it possible to suppress the foaming speed. In addition, it is possible to produce a foamed molded article with good appearance quality.
[0012] The melt flow rate of the resin constituting the base resin is from a lower limit of 0.1 g / 10 min to an upper limit of 60 g / 10 min. By setting the melt flow rate to 0.1 g / 10 min or more, deformation of the master batch can be prevented, and by setting it to 60 g / 10 min or less, the appearance of the obtained molded article can be made good. The preferred lower limit of the melt flow rate is 1.0 g / 10 min, and the preferred upper limit is 55 g / 10 min. The melt flow rate is an index that indicates the fluidity of a resin, and is expressed as the amount of resin extruded from an opening (nozzle) at the bottom of a cylindrical container heated by a heater when a certain amount of synthetic resin is heated to a specified temperature (e.g., 190°C) and pressurized with a specified load (e.g., 2.16 kg) in the container per 10 minutes. The unit is g / 10 minutes, and it is measured by the method specified in JIS K 7210-1.
[0013] The melting point of the resin constituting the base resin is 70°C at the lower limit and 110°C at the upper limit. By setting the melting point at 70° C. or higher, blocking of the master batch can be prevented, and by setting the melting point at 110° C. or lower, foaming during the preparation of the master batch can be suppressed. The preferred lower limit of the melting point is 75°C, and the preferred upper limit is 105°C. The melting point means the peak temperature of the melting peak obtained by DSC measurement.
[0014] The base resin preferably contains at least one selected from the group consisting of acrylic resins, polyethylene resins, and olefin elastomers. This makes it possible to suppress the foaming rate. In addition, it is possible to produce a foamed molded product with good appearance quality.
[0015] Examples of the acrylic resin include homopolymers of acrylic monomers such as acrylic acid, methacrylic acid, and (meth)acrylic acid esters, and (meth)acrylic copolymers containing these. Examples of the (meth)acrylic acid ester include (meth)acrylates having an alkyl group having 1 to 10 carbon atoms, specifically, methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, etc. Examples of the (meth)acrylic acid ester include n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, etc. Here, the (meth)acrylic acid refers to acrylic acid or methacrylic acid.
[0016] In the (meth)acrylic copolymer, examples of other comonomers that are copolymerized together with the acrylic monomer include α-olefins, styrene, α-methylstyrene, vinyltoluene, acrylonitrile, methacrylonitrile, vinyl acetate, and the like. Among these, a copolymer of an acrylic monomer and an α-olefin is preferred, and an ethylene-methyl methacrylate copolymer (EMMA) is more preferred. These comonomers can be present in the acrylic resin in the form of a random copolymer, a graft copolymer or a block copolymer.
[0017] In the case of the (meth)acrylic copolymer, the preferred lower limit of the content of the acrylic monomer (% by weight of the acrylic monomer component relative to the total (meth)acrylic copolymer) is 10% by weight, and the preferred upper limit is 50% by weight. By using a (meth)acrylic copolymer having an acrylic monomer content within the above range, it is possible to improve moldability and dispersibility of the thermally expandable microcapsules.
[0018] The acrylic resin preferably has a weight average molecular weight of 10,000 or more. By setting the weight average molecular weight within the above range, a molded article having excellent appearance can be obtained. The weight average molecular weight (Mw) is measured as a polystyrene equivalent molecular weight by gel permeation chromatography (GPC).
[0019] The melting point of the acrylic resin is preferably 75 to 105° C. This allows a foamed molded article with excellent appearance to be obtained. The melting point means the peak temperature of the melting peak obtained by DSC measurement.
[0020] The melt flow rate of the acrylic resin is preferably 1 g / 10 min in the lower limit and 50 g / 10 min in the upper limit. By setting the Memelt flow rate to 1 g / 10 min or more, deformation of the master batch can be prevented, and by setting it to 50 g / 10 min or less, the appearance of the obtained molded article can be made good.
[0021] Examples of the polyethylene resin include low-density polyethylene resin, medium-density polyethylene resin, linear low-density polyethylene resin, high-density polyethylene resin, etc. Among these, low-density polyethylene resin is preferred.
[0022] The olefin-based elastomer may be a copolymer mainly composed of an olefin, and examples of the olefin mainly composed of an α-olefin copolymer include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, etc. Among these, a propylene-based elastomer is preferred. The olefin-based elastomer may contain a diene component in addition to an olefin. As the olefin-based elastomer containing such a diene component, EPDM resin (ethylene-propylene-diene rubber) is preferable.
[0023] The base resin may be 100% by weight of at least one selected from the group consisting of acrylic resins, polyethylene resins, and olefin elastomers, and it is also possible to appropriately mix one or more other resin components. In addition, when the above-mentioned other resin components are used, the ratio of at least one selected from the group consisting of the acrylic resin, the polyethylene resin, and the olefin-based elastomer is preferably 80% by weight or more, more preferably 90% by weight or more, and is usually less than 100% by weight.
[0024] The other resin components include rubber components. As the rubber components, natural rubber (NR), butadiene rubber (BR), styrene butadiene rubber (SBR), isoprene rubber (IR), acrylonitrile-butadiene rubber (NBR), butyl rubber (IIR), chloroprene rubber (CR), urethane rubber (U), silicone rubber (Si), etc. may be used. In addition, one or more types selected from the above rubber components may be mixed and used.
[0025] As the other resin component, a general thermoplastic resin may be used. Examples of the thermoplastic resin include general thermoplastic resins such as polyvinyl chloride, polypropylene, polypropylene oxide, and polystyrene, and engineering plastics such as polybutylene terephthalate, nylon, polycarbonate, and polyethylene terephthalate. Among these, at least one selected from the group consisting of polypropylene and polystyrene is preferred.
[0026] The preferred lower limit of the content of the base resin in the foam molding masterbatch of the present invention is 40% by weight, and the preferred upper limit is 50% by weight. If the content of the base resin is less than 40% by weight, foaming may occur during the preparation of the masterbatch, making it impossible to produce the masterbatch, whereas if the content of the base resin exceeds 50% by weight, the desired expansion ratio may not be obtained.
[0027] The foam molding masterbatch of the present invention contains thermally expandable microcapsules. The lower limit of the content of the thermally expandable microcapsules in the foam molding masterbatch of the present invention is 52% by weight, and the upper limit is 70% by weight. By making the content of the thermally expandable microcapsules 52% by weight or more, a desired expansion ratio can be obtained. By making the content of the thermally expandable microcapsules 70% by weight or less, foaming during the preparation of the masterbatch can be prevented, and as a result, the expansion ratio of the foam molded product can be improved. The preferred lower limit of the content of the thermally expandable microcapsules is 55% by weight, and the preferred upper limit is 60% by weight.
[0028] The shell constituting the thermally expandable microcapsules is preferably made of a polymer obtained by polymerizing a monomer mixture containing at least one polymerizable monomer (I) selected from acrylonitrile, methacrylonitrile and vinylidene chloride. By adding the polymerizable monomer (I), the gas barrier property of the shell can be improved.
[0029] Furthermore, when it is desired to further improve the heat resistance, the shell constituting the above-mentioned thermally expandable microcapsules is preferably made of a polymer obtained by polymerizing a monomer mixture containing 40 to 90% by weight of a polymerizable monomer (I) and 5 to 50% by weight of a radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and having 3 to 8 carbon atoms.
[0030] The preferred lower limit of the content of the polymerizable monomer (I) in the monomer mixture is 40% by weight, and the preferred upper limit is 90% by weight. If the content of the polymerizable monomer (I) in the monomer mixture is less than 40% by weight, the gas barrier property of the shell may be reduced, and the expansion ratio may be reduced. If the content of the polymerizable monomer (I) in the monomer mixture is more than 90% by weight, the heat resistance may not be improved. The more preferred lower limit of the content of the polymerizable monomer (I) in the monomer mixture is 50% by weight, and the more preferred upper limit is 80% by weight.
[0031] The radical polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and a carbon number of 3 to 8 may be, for example, one having one or more free carboxyl groups per molecule for ionic crosslinking. Specific examples include unsaturated monocarboxylic acids, unsaturated dicarboxylic acids and their anhydrides, monoesters of unsaturated dicarboxylic acids and their derivatives, etc. Examples of the unsaturated monocarboxylic acid include acrylic acid, methacrylic acid, ethacrylic acid, crotonic acid, and cinnamic acid. Examples of the unsaturated dicarboxylic acid include maleic acid, itaconic acid, fumaric acid, citraconic acid, and chloromaleic acid. Examples of the monoesters of the unsaturated dicarboxylic acids include monomethyl maleate, monoethyl maleate, monobutyl maleate, monomethyl fumarate, monoethyl fumarate, monomethyl itaconate, monoethyl itaconate, and monobutyl itaconate. These may be used alone or in combination of two or more. Among these, acrylic acid, methacrylic acid, maleic acid, maleic anhydride, and itaconic acid are particularly preferred.
[0032] The content of the segment derived from the radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and having 3 to 8 carbon atoms in the monomer mixture is preferably 5% by weight in lower limit and 50% by weight in upper limit. If the content of the segment derived from the radically polymerizable unsaturated carboxylic acid monomer (II) is less than 5% by weight, the maximum foaming temperature may be 190°C or lower, and if the content of the segment derived from the radically polymerizable unsaturated carboxylic acid monomer (II) is more than 50% by weight, the maximum foaming temperature is improved but the foaming ratio is reduced. The content of the segment derived from the radically polymerizable unsaturated carboxylic acid monomer (II) is more preferably 10% by weight in lower limit and 40% by weight in upper limit.
[0033] The monomer mixture is not particularly limited as long as the content of the segment derived from the polymerizable monomer (I) and the radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and having 3 to 8 carbon atoms is within the above-mentioned range, but it is preferable to use the following monomer mixtures (1) to (3).
[0034] The monomer mixture (1) contains 40 to 90% by weight of the polymerizable monomer (I) and 5 to 50% by weight of the radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and 3 to 8 carbon atoms, and does not contain a polymerizable monomer (III) having two or more double bonds in the molecule.
[0035] The monomer mixture (1) does not contain a polymerizable monomer (III) having two or more double bonds in the molecule. The polymerizable monomer (III) is generally used as a crosslinking agent. In the above-mentioned monomer mixture (1), a shell having sufficient strength can be obtained by using a monomer mixture containing a predetermined amount of the above-mentioned polymerizable monomer (I) and the radically polymerizable unsaturated carboxylic acid monomer (II). As a result, even if the above-mentioned monomer mixture does not contain a polymerizable monomer (III) having two or more double bonds in the molecule, a thermally expandable microcapsule having excellent shear resistance, heat resistance, and foaming properties can be obtained. The reason why the above-mentioned sufficient strength is obtained is not clear, but it is thought that crosslinking due to a dehydration condensation reaction between carboxyl groups is related to it. In addition, when the polymerizable monomer (III) is added, the particle shape of the thermally expandable microcapsule becomes distorted, resulting in a decrease in bulk density. If the bulk density is decreased, in the next step, particularly when a masterbatch is produced using extrusion molding, the thermally expandable microcapsule is more likely to be sheared, and the thermally expandable microcapsule tends to foam. As a result, a stable masterbatch cannot be produced due to a decrease in the true density of the masterbatch, and when foam molding is subsequently performed using injection molding or the like, the expansion ratio tends to vary.
[0036] In this way, the monomer mixture (1) makes it possible to obtain thermally expandable microcapsules having sufficient strength and heat resistance without using a polymerizable monomer (III) having two or more double bonds in the molecule. In this specification, "the monomer mixture does not contain a polymerizable monomer (III) having two or more double bonds in the molecule" means that the monomer mixture does not substantially contain the polymerizable monomer (III), and when the monomer mixture contains a very small amount of the polymerizable monomer (III), it is considered that the polymerizable monomer (III) is not contained.
[0037] The polymerizable monomer (III) may be a monomer having two or more radically polymerizable double bonds. Specific examples include divinylbenzene, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, etc. In addition, examples include 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, di(meth)acrylate of polyethylene glycol having a molecular weight of 200 to 600, glycerin di(meth)acrylate, trimethylolpropane di(meth)acrylate, etc. Further examples include trimethylolpropane tri(meth)acrylate, ethylene oxide modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, triallyl formal tri(meth)acrylate, and the like. Additionally, examples include pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dimethylol-tricyclodecane di(meth)acrylate, and the like.
[0038] The monomer mixture (2) contains 40 to 90% by weight of the polymerizable monomer (I), 5 to 50% by weight of the radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and having 3 to 8 carbon atoms, 0.2% by weight or less of the polymerizable monomer (III), and 0.1 to 10% by weight of a metal cation hydroxide (IV).
[0039] The monomer mixture (2) preferably contains a polymerizable monomer (III) having two or more double bonds in the molecule. The polymerizable monomer (III) functions as a crosslinking agent. By containing the polymerizable monomer (III), the strength of the shell can be increased, and the cell walls are less likely to break during thermal expansion.
[0040] The polymerizable monomer (III) is not particularly limited as long as it has a carboxyl group and is different from the radically polymerizable unsaturated carboxylic acid monomer (II) having 3 to 8 carbon atoms, and generally, a monomer having two or more radically polymerizable double bonds is preferably used. Specific examples include divinylbenzene, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, etc. Other examples include 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, di(meth)acrylate of polyethylene glycol having a molecular weight of 200 to 600, glycerin di(meth)acrylate, and trimethylolpropane di(meth)acrylate. Further examples include trimethylolpropane tri(meth)acrylate, ethylene oxide modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dimethylol-tricyclodecane di(meth)acrylate, and the like.
[0041] The preferred upper limit of the content of the polymerizable monomer (III) in the monomer mixture (2) is 0.2% by weight. If the polymerizable monomer (III) is added in an amount exceeding 0.2% by weight, the particle shape of the thermally expandable microcapsule becomes distorted, resulting in a decrease in bulk density. If the bulk density is decreased, in the next step, particularly when a masterbatch is produced using extrusion molding, the thermally expandable microcapsule is more likely to be sheared, and the thermally expandable microcapsule tends to foam. As a result, a stable masterbatch cannot be produced due to a decrease in the true density of the masterbatch, and when foam molding is subsequently performed using injection molding or the like, the expansion ratio tends to vary. In the present invention, the content of the polymerizable monomer (III) is set to 0.2% by weight or less, thereby preventing a decrease in bulk density. The preferred lower limit of the content of the polymerizable monomer (III) is 0% by weight, and the more preferred upper limit is 0.1% by weight.
[0042] The monomer mixture (2) preferably contains a metal cation hydroxide (IV). By containing the metal cation hydroxide (IV), an ionic bond occurs between the metal cation hydroxide (IV) and the carboxyl group of the radical polymerizable unsaturated carboxylic acid monomer (II), which increases the rigidity and makes it possible to improve the heat resistance. As a result, it becomes possible to obtain a thermally expandable microcapsule that does not burst or shrink for a long time in a high temperature range. In addition, since the elastic modulus of the shell is unlikely to decrease even in a high temperature range, the thermally expandable microcapsule does not burst or shrink even when a molding process such as kneading molding, calendar molding, extrusion molding, or injection molding is performed in which a strong shear force is applied. In addition, because the bond is an ionic bond rather than a covalent bond, the particle shape of the thermally expandable microcapsule becomes closer to a perfect sphere and is less likely to become distorted. This is thought to be because the bond strength of the crosslinking due to ionic bonds is weaker than that of the crosslinking due to covalent bonds, and therefore the volume of the thermally expandable microcapsule shrinks uniformly when the monomer is converted to a polymer during polymerization.
[0043] The metal cation of the metal cation hydroxide (IV) is not particularly limited as long as it is a metal cation that reacts with the radical polymerizable unsaturated carboxylic acid monomer (II) to form an ionic bond, and examples thereof include ions such as Na, K, Li, Zn, Mg, Ca, Ba, Sr, Mn, Al, Ti, Ru, Fe, Ni, Cu, Cs, Sn, Cr, and Pb. However, since the purpose is to form an ionic bond with the radical polymerizable unsaturated carboxylic acid monomer (II), it is necessary to be a hydroxide, and chlorides such as NaCl have a weak ionic bond and are not applicable here. Among these, ions of Ca, Zn, and Al, which are divalent to trivalent metal cations, are preferred, and Zn ions are particularly preferred. These metal cation hydroxides (IV) may be used alone or in combination of two or more.
[0044] The content of the metal cation hydroxide (IV) in the monomer mixture (2) is preferably 0.1% by weight at the lower limit and 10% by weight at the upper limit. If the content of the metal cation hydroxide (IV) is less than 0.1% by weight, the heat resistance may not be improved, and if the content of the metal cation hydroxide (IV) is more than 10% by weight, the expansion ratio may be significantly deteriorated. The more preferred lower limit of the content of the metal cation hydroxide (IV) is 0.5% by weight, and the more preferred upper limit is 5% by weight.
[0045] The monomer mixture (3) contains 40 to 90% by weight of the polymerizable monomer (I), 5 to 50% by weight of a radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and 3 to 8 carbon atoms, and 0.1 to 10% by weight of a metal cation hydroxide (IV), and does not contain a polymerizable monomer (III) having two or more double bonds in the molecule.
[0046] The monomer mixture (3) is characterized in that it does not contain a polymerizable monomer (III) having two or more double bonds in the molecule. Crosslinking by ionic bonds occurs between the radical polymerizable unsaturated carboxylic acid monomer (II) and the metal cation hydroxide (IV), so that the shell obtained has sufficient strength and heat resistance even when the monomer mixture does not contain a polymerizable monomer (III) having two or more double bonds in the molecule. When the polymerizable monomer (III) is added, the particle shape of the thermally expandable microcapsule becomes distorted, resulting in a decrease in bulk density. If the bulk density decreases, the thermally expandable microcapsule is more likely to be sheared in the next step, particularly when a masterbatch is produced using extrusion molding, so that the thermally expandable microcapsule tends to foam. As a result, a stable masterbatch cannot be produced due to a decrease in the true density of the masterbatch, and when foam molding is subsequently performed using injection molding or the like, the foaming ratio tends to vary.
[0047] In the monomer mixture (3), crosslinking by ionic bonds is predominant, and crosslinking by covalent bonds is reduced, so that it is possible to obtain thermally expandable microcapsules having sufficient strength and heat resistance without using the polymerizable monomer (III) having two or more double bonds in the molecule. In this specification, "the monomer mixture does not contain a polymerizable monomer (III) having two or more double bonds in the molecule" means that the polymerizable monomer (III) is substantially not contained, and when the polymerizable monomer (III) is contained in a very small amount, it is considered that the polymerizable monomer (III) is not contained.
[0048] In addition to the polymerizable monomer (I) and the radically polymerizable unsaturated carboxylic acid monomer (II), other monomers may be added to the monomer mixture. Examples of the other monomers include acrylic acid esters such as methyl acrylate, ethyl acrylate, butyl acrylate, and dicyclopentenyl acrylate, methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, butyl methacrylate, and isobornyl methacrylate, and vinyl monomers such as vinyl acetate and styrene. These other monomers can be appropriately selected and used according to the properties required for the thermally expandable microcapsules, and among these, methyl methacrylate, ethyl methacrylate, methyl acrylate, and the like are preferably used. The content of the other monomers in the total monomers constituting the shell is preferably less than 10% by weight. If the content of the other monomers is 10% by weight or more, the gas barrier properties of the cell wall are reduced and the thermal expansion is easily deteriorated, which is not preferable.
[0049] The monomer mixture contains a polymerization initiator for polymerizing the monomers. As the polymerization initiator, for example, dialkyl peroxide, diacyl peroxide, peroxy ester, peroxy dicarbonate, azo compound, etc. are suitably used. Examples of the dialkyl peroxide include methyl ethyl peroxide, di-t-butyl peroxide, isobutyl peroxide, and dicumyl peroxide. Examples of the diacyl peroxide include benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, and 3,5,5-trimethylhexanoyl peroxide. Examples of the peroxy ester include t-butyl peroxypivalate, t-hexyl peroxypivalate, t-butyl peroxyneodecanoate, t-hexyl peroxyneodecanoate, and 1-cyclohexyl-1-methylethyl peroxyneodecanoate. Examples of the peroxydicarbonate include bis(4-t-butylcyclohexyl) peroxydicarbonate, di-n-propyl-oxydicarbonate, diisopropyl peroxydicarbonate, di(2-ethylethylperoxy)dicarbonate, and dimethoxybutyl peroxydicarbonate. Examples of the azo compound include 2,2'-azobisisobutyronitrile, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 1,1'-azobis(1-cyclohexanecarbonitrile).
[0050] The preferred lower limit of the weight-average molecular weight of the polymer constituting the shell is 100,000, and the preferred upper limit is 2,000,000. If the weight-average molecular weight is less than 100,000, the strength of the shell may decrease, whereas if the weight-average molecular weight exceeds 2,000,000, the strength of the shell may become too high, resulting in a decrease in the expansion ratio.
[0051] The shell may further contain, as necessary, a stabilizer, an ultraviolet absorber, an antioxidant, an antistatic agent, a flame retardant, a silane coupling agent, a coloring agent, and the like.
[0052] The thermally expandable microcapsules have a volatile expansion agent encapsulated in the shell as a core agent. The volatile expanding agent is a substance that becomes gaseous at a temperature equal to or lower than the softening point of the polymer constituting the shell, and is preferably a low-boiling organic solvent. Examples of the volatile expanding agent include low molecular weight hydrocarbons, chlorofluorocarbons, tetraalkylsilanes, and the like. Examples of the low molecular weight hydrocarbons include ethane, ethylene, propane, propene, n-butane, isobutane, butene, isobutene, n-pentane, isopentane, neopentane, n-hexane, heptane, isooctane, and petroleum ether. Examples of the chlorofluorocarbons include CCl3F, CCl2F2, CClF3, and CClF2-CClF2. Examples of the tetraalkylsilane include tetramethylsilane, trimethylethylsilane, trimethylisopropylsilane, and trimethyl-n-propylsilane. Among these, isobutane, n-butane, n-pentane, isopentane, n-hexane, isooctane, petroleum ether, and mixtures thereof are preferred. These volatile blowing agents may be used alone or in combination of two or more. Furthermore, as the volatile expanding agent, a pyrolytic compound that is pyrolyzed by heating to become gaseous may be used.
[0053] In the thermally expandable microcapsules, among the above-mentioned volatile expanding agents, it is preferable to use low-boiling-point hydrocarbons having a carbon number of 5 or less. By using such hydrocarbons, it is possible to obtain thermally expandable microcapsules that have a high expansion ratio and start expanding quickly. Moreover, a pyrolytic compound that decomposes when heated to become gaseous may be used as the volatile expanding agent.
[0054] In the foam molding masterbatch of the present invention, the preferred lower limit of the content of the volatile expanding agent used as a core agent is 10% by weight, and the preferred upper limit is 25% by weight. The thickness of the shell varies depending on the content of the core agent, but if the content of the core agent is reduced and the shell becomes too thick, the foaming performance decreases, and if the content of the core agent is increased, the strength of the shell decreases. When the content of the core agent is set to 10 to 25% by weight, it is possible to prevent the thermally expandable microcapsule from collapsing and improve the foaming performance at the same time.
[0055] The above-mentioned thermally expandable microcapsules have a maximum foaming temperature (Tmax) with a lower limit of 180°C and an upper limit of 230°C. If the maximum foaming temperature is less than 180°C, the heat resistance is reduced, and the thermally expandable microcapsules burst and shrink in high temperature regions or during molding. In addition, foaming occurs due to shear during the production of the masterbatch, making it impossible to stably produce an unfoamed masterbatch. A more preferable lower limit of the maximum foaming temperature is 210°C. In this specification, the maximum foaming temperature means the temperature at which the diameter of a thermally expandable microcapsule becomes maximum (maximum displacement) when the diameter of the thermally expandable microcapsule is measured while being heated from room temperature.
[0056] The thermally expandable microcapsules preferably have a lower limit of 300 μm and an upper limit of 1500 μm for the maximum displacement (Dmax) measured by thermomechanical analysis. The above-mentioned maximum displacement amount refers to the value at which the diameter of a predetermined amount of thermally expandable microcapsules as a whole becomes maximum when the diameter of the predetermined amount of thermally expandable microcapsules is measured while being heated from room temperature. The upper limit of the foaming initiation temperature (Ts) is preferably 160°C, and more preferably 165°C. In this specification, the maximum foaming temperature means the temperature at which the thermally expandable microcapsule has reached a maximum displacement when its diameter is measured while being heated from room temperature.
[0057] The lower limit of the average particle size of the thermally expandable microcapsules is 15 μm, and the upper limit is 35 μm. When the average particle size is 15 μm or more, the foaming of the obtained molded body is sufficient, and when the average particle size is 35 μm or less, the appearance of the obtained molded body is good and the strength of the molded body can be sufficient. The preferred lower limit of the average particle size is 18 μm, and the preferred upper limit is 30 μm. The average particle size of the thermally expandable microcapsules means the volume average particle size measured using a particle size distribution measuring device or the like.
[0058] The preferred lower limit of the bulk density of the thermally expandable microcapsule is 0.40 g / cm 3 The bulk density is 0.40 g / cm 3If the bulk density is less than 0.42 g / cm, the thermally expandable microcapsules are likely to be subjected to shear, particularly when the masterbatch is produced by extrusion molding, and the thermally expandable microcapsules tend to foam. As a result, the true specific gravity of the masterbatch decreases, making it difficult to produce a stable masterbatch, and when foam molding is subsequently performed by injection molding or the like, the foaming ratio tends to vary. The preferable lower limit of the bulk density is 0.42 g / cm. 3 It is. The bulk specific gravity refers to a specific gravity based on the volume of an aggregate of thermally expandable microcapsules closely packed in a container etc. The bulk specific gravity can be measured in accordance with JIS K 6721.
[0059] The method for producing the thermally expandable microcapsules includes, for example, a step of preparing an aqueous medium, a step of dispersing an oily mixture containing 40 to 90% by weight of the polymerizable monomer (I), 5 to 50% by weight of a radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and having 3 to 8 carbon atoms, and a volatile expanding agent, in the aqueous medium, and then a step of polymerizing the monomers.
[0060] When producing the above-mentioned thermally expandable microcapsules, a step of preparing an aqueous medium is carried out first.Specifically, for example, water and a dispersion stabilizer, and if necessary, a co-stabilizer are added to a polymerization reaction vessel to prepare an aqueous dispersion medium containing a dispersion stabilizer.Also, if necessary, alkali metal nitrite, stannous chloride, stannic chloride, potassium dichromate, etc. may be added.
[0061] Examples of the dispersion stabilizer include silica, calcium phosphate, magnesium hydroxide, aluminum hydroxide, ferric hydroxide, barium sulfate, calcium sulfate, sodium sulfate, calcium oxalate, calcium carbonate, barium carbonate, and magnesium carbonate.
[0062] The amount of the dispersion stabilizer to be added is not particularly limited and is determined appropriately depending on the type of dispersion stabilizer, the particle size of the thermally expandable microcapsules, etc., but the preferred lower limit is 0.1 parts by weight and the preferred upper limit is 20 parts by weight per 100 parts by weight of the monomer.
[0063] Examples of the auxiliary stabilizer include a condensation product of diethanolamine and an aliphatic dicarboxylic acid, a condensation product of urea and formaldehyde, etc. Further examples include polyvinylpyrrolidone, polyethylene oxide, polyethyleneimine, tetramethylammonium hydroxide, gelatin, methylcellulose, polyvinyl alcohol, dioctyl sulfosuccinate, sorbitan ester, various emulsifiers, etc.
[0064] The combination of the dispersion stabilizer and the auxiliary stabilizer is not particularly limited, and examples thereof include a combination of colloidal silica and a condensation product, a combination of colloidal silica and a water-soluble nitrogen-containing compound, a combination of magnesium hydroxide or calcium phosphate and an emulsifier, etc. Among these, the combination of colloidal silica and a condensation product is preferred. Furthermore, as the above-mentioned condensation product, a condensation product of diethanolamine and an aliphatic dicarboxylic acid is preferable, and a condensation product of diethanolamine and adipic acid or a condensation product of diethanolamine and itaconic acid is particularly preferable.
[0065] Examples of the water-soluble nitrogen-containing compound include polyvinylpyrrolidone, polyethyleneimine, polyoxyethylene alkylamine, polydialkylaminoalkyl (meth)acrylate, polydialkylaminoalkyl (meth)acrylamide, polyacrylamide, polycationic acrylamide, polyamine sulfone, and polyallylamine. Examples of the polydialkylaminoalkyl(meth)acrylate include polydimethylaminoethyl methacrylate and polydimethylaminoethyl acrylate. Examples of the polydialkylaminoalkyl(meth)acrylamide include polydimethylaminopropylacrylamide, polydimethylaminopropylmethacrylamide, etc. Among these, polyvinylpyrrolidone is preferably used.
[0066] The amount of colloidal silica added is appropriately determined according to the particle size of the thermally expandable microcapsule, but the preferred lower limit is 1 part by weight and the preferred upper limit is 20 parts by weight relative to 100 parts by weight of vinyl monomer. The more preferred lower limit of the amount of colloidal silica added is 2 parts by weight and the more preferred upper limit is 10 parts by weight. The amount of the condensation product or water-soluble nitrogen-containing compound added is also appropriately determined according to the particle size of the thermally expandable microcapsule, but the preferred lower limit is 0.05 parts by weight and the preferred upper limit is 2 parts by weight relative to 100 parts by weight of monomer.
[0067] In addition to the above dispersion stabilizer and co-stabilizer, inorganic salts such as sodium chloride and sodium sulfate may be added. By adding an inorganic salt, it is possible to obtain thermally expandable microcapsules having a more uniform particle shape. The amount of the inorganic salt added is usually preferably 0 to 100 parts by weight per 100 parts by weight of the monomer.
[0068] The aqueous dispersion medium containing the dispersion stabilizer is prepared by mixing the dispersion stabilizer or co-stabilizer with deionized water, and the pH of the aqueous phase is appropriately determined depending on the type of dispersion stabilizer or co-stabilizer used. For example, when silica such as colloidal silica is used as the dispersion stabilizer, polymerization is carried out in an acidic medium, and to make the aqueous medium acidic, an acid such as hydrochloric acid is added as necessary to adjust the pH of the system to 3 to 4. On the other hand, when magnesium hydroxide or calcium phosphate is used, polymerization is carried out in an alkaline medium.
[0069] Next, in the method for producing a thermally expandable microcapsule, a step is carried out in which an oily mixture containing 40 to 90% by weight of the polymerizable monomer (I), 5 to 50% by weight of a radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and a carbon number of 3 to 8, and a volatile swelling agent is dispersed in an aqueous medium. In this step, the monomer and the volatile swelling agent may be added separately to the aqueous dispersion medium to prepare an oily mixture in the aqueous dispersion medium, but usually, the two are mixed in advance to prepare an oily mixture, which is then added to the aqueous dispersion medium. In this case, the oily mixture and the aqueous dispersion medium may be prepared in separate vessels, and the oily mixture may be dispersed in the aqueous dispersion medium by mixing them under stirring in the separate vessels, and then added to the polymerization reaction vessel. In addition, a polymerization initiator is used to polymerize the above monomers. The polymerization initiator may be added to the above oily mixed liquid in advance, or may be added after the aqueous dispersion medium and the oily mixed liquid are stirred and mixed in a polymerization reaction vessel.
[0070] Methods for emulsifying and dispersing the above-mentioned oily mixture in an aqueous dispersion medium to a predetermined particle size include a method of stirring the mixture using a homomixer (e.g., manufactured by Tokushu Kika Kogyo Co., Ltd.) or a method of passing the mixture through a static dispersion device such as a line mixer or an element-type static disperser. The aqueous dispersion medium and the polymerizable mixture may be supplied separately to the static dispersing device, or a dispersion liquid which has been previously mixed and stirred may be supplied.
[0071] The thermally expandable microcapsules can be produced by, for example, polymerizing the monomer by heating the dispersion liquid obtained through the above-mentioned process. The thermally expandable microcapsules produced by such a method have a high maximum foaming temperature, excellent heat resistance, and do not burst or shrink even in high temperature regions or during molding. In addition, since they have a high bulk density, they do not foam due to shear during masterbatch production, and unfoamed masterbatches can be stably produced.
[0072] The foam molding masterbatch of the present invention may contain a chemical foaming agent. By including the chemical foaming agent, for example, when a chemical foaming agent such as sodium bicarbonate is used, the foaming performance can be improved by CO2 generated during decomposition. In addition, by using the thermally expandable microcapsules in combination with a chemical foaming agent, it is possible to suppress the generation of open cells that tend to occur when a chemical foaming agent is used alone.
[0073] The chemical foaming agent is not particularly limited as long as it is in powder form at room temperature, and any conventionally used chemical foaming agent can be used.Specific examples of the chemical foaming agent include inorganic chemical foaming agents such as sodium hydrogen carbonate, and organic chemical foaming agents such as azodicarbonamide, N,N'-dinitrosopentamethylenetetramine, P,P'-oxybisbenzenesulfonylhydrazide, and paratoluenesulfonylhydrazide.
[0074] The foam molding masterbatch of the present invention may contain additives such as lubricants. By containing the lubricant, the shear applied to the thermally expandable microcapsules during the production of the masterbatch is suppressed, micro-bubbles are less likely to occur, and the dispersibility of the thermally expandable microcapsules can be improved, making it easier to produce the masterbatch. As a result, a masterbatch with a high concentration of thermally expandable microcapsules can be produced stably with good production efficiency.
[0075] The lubricant is not particularly limited as long as it is soluble at the temperature during the production of the masterbatch, and any lubricant that has been conventionally used as a lubricant can be used.Specific examples of the lubricant include polyethylene wax having a viscosity average molecular weight of 3,000 or less, fatty acid esters, fatty acids such as stearic acid, fatty acid derivatives, and those called composite lubricants whose main components are fatty acid amides. Examples of the fatty acid ester include glycerin fatty acid esters such as glycerin monostearate, diglycerin stearate, etc. Examples of the fatty acid derivative include fatty acids having a hydroxyl group added thereto. Among these, fatty acid derivatives are preferred, and in particular, by using fatty acids having hydroxyl groups added thereto, it is possible to prepare a master batch containing a high concentration of thermally expandable microcapsules in a high viscosity base resin. The fatty acid constituting the fatty acid ester, fatty acid, or fatty acid derivative preferably has 15-40 carbon atoms, more preferably 18-36 carbon atoms, and even more preferably 18-20 carbon atoms. The content of the lubricant in the expansion molding masterbatch of the present invention is preferably 1 to 15% by weight, and more preferably 5 to 12% by weight.
[0076] The masterbatch for expansion molding of the present invention may be in any of various forms, such as powder, granules, lumps, strands, pellets, and sheets.
[0077] The preferred lower limit of the true specific gravity of the foam molding masterbatch of the present invention is 0.80 g / cm 3 The true specific gravity is 0.80g / cm 3 If it is less than this, it means that the thermally expandable microcapsules in the master batch are inflated, and the expansion ratio of the molded article obtained after molding may decrease. A more preferable lower limit of the true specific gravity is 0.90 g / cm 3 , the preferred upper limit is 1.0 g / cm 3 It is. The true specific gravity above refers to the specific gravity of the material only, excluding pores, of the masterbatch at 20°C. It represents the ratio of the mass of a unit volume to the mass of an equal volume of water at 4° C. The true specific gravity can be measured by a method conforming to JIS K 7112 Method A (water displacement method).
[0078] The preferred lower limit of the bulk density of the foam molding masterbatch of the present invention is 0.35 g / cm 3 The bulk density is 0.35 g / cm 3If the bulk density is less than this, particularly in the case of injection molding, the master batch is weighed at a constant volume, and if the bulk density is low, the weight of the master batch will be small, which may result in a decrease in the expansion ratio of the resulting molded product. A more preferable lower limit of the bulk density is 0.38 g / cm 3 , the preferred upper limit is 0.50 g / cm 3 It is. The bulk specific gravity is based on the volume of the master batch aggregate packed most densely in a container or the like. The bulk density can be measured in accordance with JIS K 6721.
[0079] When the foam molding masterbatch of the present invention is in the form of granules or pellets, the preferred lower limit of the particle size is 450 mg / 30 pieces. If the particle size is less than 450 mg / 30 pieces, the particle size is small, so the surface area increases, and the base resin dissolves early due to temperature, shear, etc. in the molding machine, and the effect of increasing the melting point of the base resin in the masterbatch may decrease so that the thermally expandable microcapsules do not foam early in the cylinder. A more preferred lower limit of the particle size is 470 mg / 30 particles, and a more preferred upper limit is 600 mg / 30 particles. The above particle size is a guideline for the size of the masterbatch, and is expressed as the total weight of 30 masterbatches. The particle size can be measured by randomly sampling 30 masterbatches and measuring their weight.
[0080] The method for producing the foam molding masterbatch of the present invention is not particularly limited, and for example, raw materials such as a base resin containing an olefin-based elastomer and various additives such as a lubricant are pre-kneaded using a unidirectional twin-screw extruder or the like. Next, the mixture is heated to a predetermined temperature, a foaming agent consisting of thermally expandable microcapsules is added, and the kneaded mixture obtained by further kneading is cut into pellets of a desired size using a pelletizer to form a masterbatch. If micro-foaming occurs at this point, it is difficult to obtain a desired expansion ratio in the subsequent foam molding, and the variation will also increase. Alternatively, raw materials such as a base resin, thermally expandable microcapsules, and a lubricant may be kneaded in a batch mixer and then granulated in a granulator, or a pelletized master batch may be produced using an extruder and a pelletizer.
[0081] The kneading machine is not particularly limited as long as it can knead the thermally expandable microcapsules without destroying them, and examples thereof include a pressure kneader and a Banbury mixer.
[0082] A resin composition obtained by adding a matrix resin such as a thermoplastic resin to the foam molding masterbatch of the present invention is molded by a molding method such as injection molding, and foaming is caused by the thermally expandable microcapsules by heating during molding, thereby producing a foam molded article. Such a foam molded article also constitutes the present invention. The foamed molded article of the present invention obtained by such a method has a high expansion ratio and high appearance quality, has uniformly formed closed cells, and is excellent in light weight, heat insulation, impact resistance, rigidity, etc., and can be suitably used for applications such as building materials for housing, automotive parts, and shoe soles.
[0083] The matrix resin such as the thermoplastic resin is not particularly limited as long as it does not impede the object of the present invention, and for example, general thermoplastic resins such as polyvinyl chloride, polystyrene, polypropylene, polypropylene oxide, and polyethylene are used. In addition, engineering plastics such as polybutylene terephthalate, nylon, polycarbonate, and polyethylene terephthalate may be used. In addition, thermoplastic elastomers such as ethylene-based, vinyl chloride-based, olefin-based, urethane-based, and ester-based may be used, and these resins may be used in combination. In addition, it is preferable to use the same resin as the base resin as the matrix resin.
[0084] The amount of the expansion molding masterbatch of the present invention added relative to 100 parts by weight of the above thermoplastic resin is preferably 0.5 to 20 parts by weight, more preferably 1 to 10 parts by weight.
[0085] The molding method of the foamed molded article of the present invention is not particularly limited, and examples thereof include kneading molding, calendar molding, extrusion molding, injection molding, etc. In the case of injection molding, the process is not particularly limited, and examples thereof include the short-short method in which a resin material is partially placed in a mold and foamed, and the core-back method in which the mold is fully filled with the resin material and then opened to the desired foaming point.
[0086] Another embodiment of the present invention is a masterbatch for expansion molding, which when heated to 180°C has an expansion rate of 15% or less after 3 minutes and an expansion rate of 25% or less after 5 minutes. The expansion rate after 3 minutes is preferably 12% or less, and the expansion rate after 5 minutes is preferably 24% or less.
[0087] The above-mentioned expansion ratio after 3 minutes refers to the ratio of the "foam height after 3 minutes" to the "foam height after 30 minutes" when 0.2 g of the expansion molding masterbatch is heated at 180°C for 30 minutes. The expansion ratio after 5 minutes refers to the ratio of the "foam height after 5 minutes" to the "foam height after 30 minutes" when the expansion molding masterbatch is heated at 180°C for 30 minutes.
[0088] Applications of the molded articles obtained by the molding method for foamed molded articles of the present invention and other embodiments of the present invention include, for example, automobile interior materials such as door trims and instrument panels, automobile exterior materials such as bumpers, etc. Applications also include building materials such as wood powder plastics, shoe soles, artificial cork, etc. Effect of the Invention
[0089] According to the present invention, it is possible to provide a masterbatch for foam molding, which can be suitably used in molding in which a strong shear force is applied or in which a low molding temperature is required, and which can obtain a foam molded article having a high expansion ratio, a suppressed expansion rate, and good appearance quality. In addition, by achieving the suppression of the expansion rate, it is possible to prevent adhesion between the foam molding masterbatches and between the thermally expandable microcapsules in the molding machine. Furthermore, it is possible to provide a foam molded article using the masterbatch for foam molding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0090] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0091] (Preparation of thermally expandable microcapsules) Into a polymerization reaction vessel, 300 parts by weight of water, 89 parts by weight of sodium chloride as a regulator, 0.07 parts by weight of sodium nitrite as a water-soluble polymerization inhibitor, 8 parts by weight of colloidal silica (manufactured by Asahi Denka Co., Ltd.) as a dispersion stabilizer, and 0.3 parts by weight of polyvinylpyrrolidone (manufactured by BASF Co., Ltd.) as a dispersion stabilizer were charged, and an aqueous dispersion medium was prepared. Next, an oily mixture consisting of a metal salt, a monomer, a volatile expansion agent, and a polymerization initiator in the amounts shown in Table 1 was added to the aqueous dispersion medium and mixed to prepare a dispersion liquid. The total amount of the dispersion liquid was 15 kg. The obtained dispersion liquid was stirred and mixed with a homogenizer, charged into a nitrogen-substituted pressure polymerization vessel (20 L), pressurized (0.2 MPa), and reacted at 60°C for 20 hours to prepare a reaction product. The obtained reaction product was repeatedly dehydrated and washed with water using a centrifuge, and then dried to obtain thermally expandable microcapsules (No. 1 to 6). In Table 1, the polymerizable monomer (I) is referred to as monomer (I), the radical polymerizable unsaturated carboxylic acid monomer (II) is referred to as monomer (II), and the polymerizable monomer (III) is referred to as monomer (III).
[0092] (Examples 1 to 9, Comparative Examples 1 to 9) (Preparation of master batch pellets) 100 parts by weight of the base resin shown in Table 2 and the type and amount of lubricant shown in Table 2 were kneaded in a Banbury mixer, and when the temperature reached approximately 100°C, the obtained thermally expandable microcapsules were added in the amount shown in Table 2, and the mixture was kneaded for a further 30 seconds, extruded, and simultaneously pelletized to obtain masterbatch pellets. In Table 2, EMMA stands for ethylene-methyl methacrylate copolymer, LDPE stands for low-density polyethylene, and TPO stands for olefin-based elastomer. The following resins were used: [EMMA (1)] Ethylene-methacrylate copolymer: melt flow rate 20 g / 10 min, melting point 79°C, MMA content 25 wt% (Sumitomo Chemical Co., Ltd., Acryft WK402) [EMMA (2)] Ethylene-methacrylate copolymer: melt flow rate 7 g / 10 min, melting point 80°C, MMA content 25 wt% (Sumitomo Chemical Co., Ltd., Acryft WK307) [EMMA (3)] Ethylene-methacrylate copolymer: melt flow rate 450 g / 10 min, melting point 67°C, MMA content 28 wt% (Sumitomo Chemical Co., Ltd., Acryliff CM5021) [LDPE (1)] Low-density polyethylene resin: melt flow rate 45 g / 10 min, melting point 108°C (Tosoh Corporation, Petrothene 209) [LDPE (2)] Low-density polyethylene resin: melt flow rate 7.6 g / 10 min, melting point 120°C (Tosoh Corporation, Petrothene 1384R) [TPO] Propylene elastomer: Melt flow rate 3.6g / 10min, melting point 80℃, ethylene content 11% by weight (Exon Mobil Vistamax3000)
[0093] (Production of foamed molded products) 3 parts by weight of the obtained master batch pellets were mixed with 100 parts by weight of an olefin-based elastomer (Milastomer 7030BS manufactured by Mitsui Chemicals, Inc.), and the obtained mixed pellets were fed to the hopper of an extrusion molding machine, melt-kneaded, and extrusion-molded to obtain a plate-shaped foamed molded product. The extrusion conditions were a mold temperature of 190°C.
[0094] (evaluation) The following performances were evaluated for the thermally expandable microcapsules (Nos. 1 to 6) and the molded articles obtained in Examples 1 to 9 and Comparative Examples 1 to 9. The results are shown in Tables 1 and 2.
[0095] (1) Evaluation of thermally expandable microcapsules (1-1) Volume average particle size The volume average particle diameter was measured using a particle size distribution diameter measuring device (LA-910, manufactured by HORIBA Corporation).
[0096] (1-2) Foaming start temperature, maximum foaming temperature, maximum displacement The foaming initiation temperature (Ts), maximum displacement (Dmax) and maximum foaming temperature (Tmax) were measured using a thermomechanical analyzer (TMA) (TMA2940, manufactured by TA instruments). Specifically, 25 μg of the sample was placed in an aluminum container with a diameter of 7 mm and a depth of 1 mm, and heated from 80°C to 220°C at a temperature increase rate of 5°C / min while applying a force of 0.1 N from above. The displacement in the vertical direction of the measuring probe was measured, and the temperature at which the displacement started to increase was taken as the foaming initiation temperature, the maximum value of the displacement as the maximum displacement, and the temperature at the maximum displacement as the maximum foaming temperature.
[0097] [Table 1]
[0098] (2) Evaluation of masterbatch pellets (2-1) Measurement of foaming rate (foaming rate after 3 minutes, foaming rate after 5 minutes) Regarding the foam molding masterbatch, 0.2 g of the masterbatch was placed in a test tube (φ16 mm, length 100 mm) and heated at 180°C using an ESPEC oven, while measuring the foam height after 3 minutes, 5 minutes, and 30 minutes. Then, the ratio (%) of the "foam height after 3 minutes" to the "foam height after 30 minutes" was calculated to obtain the "foam ratio after 3 minutes." Similarly, the ratio (%) of the "foam height after 5 minutes" to the "foam height after 30 minutes" was calculated to obtain the "foam ratio after 5 minutes."
[0099] (2-2) Measurement of true specific gravity The true specific gravity of the masterbatch pellets was measured using a specific gravity meter MD-200S (manufactured by Mirage) in accordance with JIS K 7112 Method A (underwater displacement method).
[0100] (2-3) Measurement of bulk density The measurement was performed according to a method conforming to JIS K 6721.
[0101] (2-4) Particle size measurement Thirty pellets were randomly sampled from the obtained master batch pellets, and the total weight was measured.
[0102] (3) Evaluation of the molded product (3-1) Density and expansion ratio The density before foaming and the density of the resulting molded product (after foaming) were measured by a method in accordance with JIS K 7112 Method A (underwater displacement method). The expansion ratio was calculated from the density of the molded body before and after expansion.
[0103] (3-2) Surface properties The surface roughness (Rz) of the molded body surface was measured using a 3D shape measuring instrument (Keyence Corporation). The evaluation criteria were as follows: a measured Rz value of less than 50 μm was marked as ○, 50 μm≦Rz value≦100 μm was marked as △, and more than 100 μm was marked as ×.
[0104] [Table 2] [Industrial Applicability]
[0105] According to the present invention, there can be provided a masterbatch for expansion molding which can be suitably used in molding in which a strong shear force is applied or in which a low molding temperature is required, and which can give a foamed molded article having a high expansion ratio, a suppressed expansion rate, and good appearance quality. In addition, there can be provided a foamed molded article using the masterbatch for expansion molding.
Claims
1. A foam molding masterbatch containing a base resin and thermally expandable microcapsules, The base resin contains a resin having a melt flow rate of 7 to 60 g / 10 min and a melting point of 70 to 110° C., The base resin contains an acrylic resin, The thermally expandable microcapsules have a maximum foaming temperature of 180° C. or higher and an average particle size of 15 to 30 μm; The content of the thermally expandable microcapsules is 52 to 70% by weight.
1. A masterbatch for foam molding comprising:
2. Thermally expandable microcapsules are made of a polymer shell and contain a volatile expansion agent as a core agent. The shell is made of a polymer obtained by polymerizing a monomer mixture containing at least one polymerizable monomer (I) selected from acrylonitrile, methacrylonitrile, and vinylidene chloride.
2. The foam molding masterbatch according to claim 1.
3. The shell is made of a polymer obtained by polymerizing a monomer mixture containing 40 to 90% by weight of a polymerizable monomer (I) consisting of at least one selected from acrylonitrile, methacrylonitrile, and vinylidene chloride, and 5 to 50% by weight of a radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and having 3 to 8 carbon atoms.
3. The foam molding masterbatch according to claim 2.
4. 4. The foam molding masterbatch according to claim 2 or 3, characterized in that the monomer mixture contains 40 to 90% by weight of a polymerizable monomer (I) consisting of at least one selected from acrylonitrile, methacrylonitrile and vinylidene chloride, and 5 to 50% by weight of a radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and having 3 to 8 carbon atoms, and does not contain a polymerizable monomer (III) having two or more double bonds in the molecule.
5. 4. The master batch for foam molding according to claim 2 or 3, characterized in that the monomer mixture contains 40 to 90% by weight of a polymerizable monomer (I) consisting of at least one selected from acrylonitrile, methacrylonitrile, and vinylidene chloride, 5 to 50% by weight of a radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and 3 to 8 carbon atoms, and 0.2% by weight or less of a polymerizable monomer (III) having two or more double bonds in the molecule, and / or 0.1 to 10% by weight of a metal cation hydroxide (IV).
6. 4. The foam molding master batch according to claim 2 or 3, characterized in that the monomer mixture contains 40 to 90% by weight of a polymerizable monomer (I) consisting of at least one selected from acrylonitrile, methacrylonitrile, and vinylidene chloride, 5 to 50% by weight of a radically polymerizable unsaturated carboxylic acid monomer (II) having a carboxyl group and having 3 to 8 carbon atoms, and 0.1 to 10% by weight of a metal cation hydroxide (IV), and does not contain a polymerizable monomer (III) having two or more double bonds in the molecule.
7. 7. The masterbatch for expansion molding according to claim 1, 2, 3, 4, 5 or 6, which, when heated to 180° C., has an expansion rate of 15% or less after 3 minutes and 25% or less after 5 minutes.
8. True specific gravity is 0.9 g / cm 3 8. The masterbatch for foam molding according to claim 1, 2, 3, 4, 5, 6 or 7, wherein
9. 9. The foam molding masterbatch according to claim 1, 2, 3, 4, 5, 6, 7 or 8, characterized in that the base resin contains a resin having a melting point of 70 to 105°C.
10. A foam-molded article produced using the foam-molding masterbatch according to claim 1, 2, 3, 4, 5, 6, 7, 8 or 9.
Citation Information
Patent Citations
Production of thermoplastic elastomer
JP1996337698A
Thermoplastic elastomer foam
JP1999343362A
Foamable pellet, injection molded foam, and production of injection molded foam
JP2000178372A
Method for manufacturing synthetic resin molded article