Thermoplastic elastomer composition
A thermoplastic elastomer composition with a hydrogenated block copolymer, resin, softener, and polyolefin elastomer addresses anisotropy issues, enhancing performance in films and sheets through improved elastic recovery and tear strength.
Patent Information
- Application Number
- JP2022526083
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-06
- Filing Date
- 2020-11-02
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-11-02
AI Technical Summary
Existing thermoplastic elastomer compositions suffer from anisotropy issues, which cause variations in properties based on the direction of stress, leading to uneven performance in films and sheets.
A thermoplastic elastomer composition comprising a hydrogenated block copolymer, a thermoplastic resin, a rubber softener, and a polyolefin elastomer, with specific proportions and structures to enhance elastic recovery, tear strength, and stress relaxation while reducing anisotropy.
The composition achieves improved elastic recovery, tear strength, and stress relaxation with reduced anisotropy, making it suitable for various film and sheet applications.
Smart Images

Figure 0007564205000006 
Figure 0007564205000007 
Figure 0007564205000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic elastomer composition based on specific types and proportions of hydrogenated block copolymer (A), thermoplastic resin (B), rubber softener (C), and polyolefin elastomer (D) as detailed below. The thermoplastic elastomer composition of the present invention has a good combination of elastic recovery, tear strength, stress relaxation, and reduced (improved) anisotropy that makes it suitable for use in a wide variety of film and sheet applications. [Background technology]
[0002] Among hydrogenated block copolymers, hydrogenated styrene-based thermoplastic elastomers are thermoplastic elastomers that are excellent in weather resistance, heat resistance, impact resistance, flexibility, and elastic recovery. Compositions containing hydrogenated block copolymers provide excellent mechanical strength, flexibility, weather resistance, ozone resistance, thermal stability, and transparency, and are therefore used in a wide range of fields, such as automotive products, home appliances, medical products, construction products, toys, everyday items, and miscellaneous goods.
[0003] In particular, applications such as films and sheets require elastic recovery, tear strength at 25°C, and stress relaxation properties, and in order to satisfy these physical properties, a method has been proposed in which a mixture of a hydrogenated styrene-based thermoplastic elastomer, a plasticizer, and various thermoplastic resins is used.
[0004] For example, Patent Document 1 generally discloses a thermoplastic elastomer composition comprising a hydrogenated styrene-based block copolymer, a thermoplastic resin, and a rubber softener. More specifically, Patent Document 2 discloses a thermoplastic elastomer composition comprising 55-60% by weight of a hydrogenated SEEPS block copolymer having a specific number average molecular weight and mass ratio of isoprene / 1,3-butadiene, 7-12% by weight of polystyrene (thermoplastic resin), 15-30% by weight of oil (rubber softener), and 5-20% by weight of a hydrogenated aliphatic hydrocarbon resin (tackifier).
[0005] The elastomer compositions described in Patent Documents 1 and 2 can fully satisfy the elastic recovery, tear strength, and stress relaxation required for applications such as films and sheets. However, the compositions may have a problem of anisotropy.
[0006] In general, anisotropy is the orientation of molecules within a material during processing. This orientation causes differences in the properties of the finished product depending on the direction in which the article is stressed. This can result in easier activation of tears in the direction of orientation, or weaker properties opposite the orientation. The effects of these orientations can be overcome in the design process, but these additional processes can add unnecessary costs. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] U.S. Patent No. 9,321,874 [Patent Document 2] U.S. Patent No. 9,056,975 Summary of the Invention [Problem to be solved by the invention]
[0008] It is an object of the present invention to provide a thermoplastic elastomer composition having a good combination of elastic recovery, tear strength at 25° C., stress relaxation, and reduced (improved) anisotropy. [Means for solving the problem]
[0009] The present invention addresses the above-mentioned problems by providing a thermoplastic elastomer composition having a good combination of elastic recovery, tear strength at 25°C, stress relaxation, and low anisotropy, comprising specific types and ratios of hydrogenated block copolymer (A), thermoplastic resin (B), rubber softener (C), and polyolefin elastomer (D) as detailed below.
[0010] More specifically, the present invention relates to a thermoplastic elastomer composition comprising a hydrogenated block copolymer component (A), a thermoplastic resin component (B), and a rubber softener component (C), (1) The hydrogenated block copolymer component (A) is (i) having two or more polymer blocks (a) containing structural units derived from an aromatic vinyl compound and one or more polymer blocks (b) containing structural units derived from isoprene and / or structural units derived from 1,3-butadiene; (ii) has a glass transition temperature (measured as shown in the examples) of less than about -45°C; and (iii) a hydrogenated block copolymer having a crystallization peak temperature (Tc) of about -3 to about 15°C (measured as shown in the examples); (2) The thermoplastic elastomer composition further comprises a polyolefin elastomer component (D), (3) The thermoplastic elastomer composition contains, relative to 100 parts by mass of (A)+(B)+(C)+(D), about 18 to about 60 parts by mass of a hydrogenated block copolymer component (A), about 3 to about 24 parts by mass of a thermoplastic resin component (B), about 3 to about 25 parts by mass of a rubber softener component (C), and about 5 to about 76 parts by mass of a polyolefin elastomer component (D). A thermoplastic elastomer composition is provided.
[0011] In one embodiment, the thermoplastic elastomer composition has an islands-in-a-sea structure of a sea phase and an island phase, wherein the sea phase is one of (i) the polyolefin elastomer (D) or (ii) a component other than the polyolefin elastomer (D), the island phase is the other of (i) or (ii), and the island phase comprises a plurality of islands having, on average, a major axis (measured as shown in the examples) of about 100 nm or more.
[0012] In another embodiment, the island phase comprises islands having, on average, a major axis of about 5 μm or less and an aspect ratio (major axis / minor axis) of about 3 or less (measured as shown in the Examples).
[0013] In another embodiment, polymer block (b) of the hydrogenated block copolymer contains structural units derived from isoprene and structural units derived from 1,3-butadiene.
[0014] In another embodiment, the mass ratio of structural units derived from isoprene to structural units derived from 1,3-butadiene is from about 49.9 / 50.1 to about 40.1 / 59.9.
[0015] In another embodiment, polymer block (b) of the hydrogenated block copolymer contains only structural units derived from 1,3-butadiene.
[0016] In another embodiment, the content of the polymer block (a) in the hydrogenated block copolymer is about 20% by mass to about 34% by mass, based on the total mass of the hydrogenated block copolymer.
[0017] In another embodiment, the thermoplastic resin component (B) comprises a polystyrene-based resin.
[0018] In another embodiment, the thermoplastic elastomer composition further comprises about 3 to about 15 parts by mass of a hydrogenated block copolymer component (E) based on 100 parts by mass of (A)+(B)+(C)+(D)+(E), wherein the hydrogenated block copolymer component (E) comprises a hydrogenated block copolymer obtained by hydrogenating a polymer block (x) containing more than about 70% by mass of a structural unit derived from an aromatic vinyl compound and a polymer block (y) containing about 30% by mass or more of a structural unit derived from at least one selected from the group consisting of a conjugated diene compound and isobutylene, and the hydrogenated block copolymer has a glass transition temperature (Tg) of about -45°C to about 30°C, and the polymer block (x) in the hydrogenated block copolymer is present in an amount of about 4% by mass to about 30% by mass based on the total mass of the hydrogenated block copolymer.
[0019] In another embodiment, the polyolefin elastomer (D) includes a polypropylene-based elastomer containing structural units derived from ethylene, and the content of the structural units derived from ethylene is about 13.0% by mass to about 15.9% by mass based on the total mass of the polypropylene-based elastomer.
[0020] The present invention further provides films or sheets of the thermoplastic elastomeric compositions as well as articles (eg, diapers) made therefrom.
[0021] These and other embodiments, features, and advantages of the present invention will be more readily understood by those of ordinary skill in the art from reading the following detailed description. [Brief description of the drawings]
[0022] [Figure 1] 1 is a cross-sectional image (magnification 2000 times) of the thermoplastic elastomer composition (film) of Example 6 taken using a transmission electron microscope (TEM). [Diagram 2] 1 is a cross-sectional image (magnification: 5000 times) of the thermoplastic elastomer composition (film) of Example 6 taken using a transmission electron microscope (TEM). [Diagram 3] 1 is a cross-sectional image (magnification: 2000 times) of the thermoplastic elastomer composition (film) of Example 8 taken using a transmission electron microscope (TEM). [Figure 4] 1 is a cross-sectional image (magnification: 5000 times) of the thermoplastic elastomer composition (film) of Example 8 taken using a transmission electron microscope (TEM). [Diagram 5] 1 is a cross-sectional image (magnification: 2000 times) of the thermoplastic elastomer composition (film) of Example 5 taken using a transmission electron microscope (TEM). [Figure 6] 1 is a cross-sectional image (magnification: 5000 times) of the thermoplastic elastomer composition (film) of Example 5 taken using a transmission electron microscope (TEM). [Figure 7]1 is a cross-sectional image (magnification: 2000 times) obtained by photographing a cross-sectional image of the thermoplastic elastomer composition (film) of Example 3 using a transmission electron microscope (TEM). [Figure 8] 1 is a cross-sectional image (magnification: 5000 times) obtained by photographing a cross-sectional image of the thermoplastic elastomer composition (film) of Example 3 using a transmission electron microscope (TEM). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Next, the present invention will be described in more detail.
[0024] In the context of this specification, all publications, patent applications, patents, and other references cited herein are expressly incorporated by reference in their entirety for all purposes as if fully set forth herein, unless otherwise indicated.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs. In case of conflict, the present specification, including definitions, will control.
[0026] Unless expressly specified otherwise, trademarks are shown in capital letters.
[0027] Unless otherwise specified, all percentages, parts, ratios, etc. are by weight.
[0028] Unless otherwise specified, pressures expressed in psi are gauge pressures and pressures expressed in kPa are absolute pressures. However, pressure differences are expressed as absolute pressures (e.g., Pressure 1 is 25 psi higher than Pressure 2).
[0029] When an amount, concentration, or other value or parameter is indicated as a range or a list of upper and lower limits, this should be understood as specifically disclosing all ranges formed from any pair of upper and lower limits of any range, regardless of whether the range is disclosed individually.When a range of numerical values is recited herein, unless otherwise specified, the range is intended to include its endpoints, and all integers and fractions within the range.It is not intended that the scope of the present disclosure be limited to the specific values recited when defining the range.
[0030] When the term "about" is used in describing a value or an endpoint of a range, the disclosure should be understood to include the specific value or endpoint referred to. In other words, "about 25 to about 50" explicitly discloses the "25" and "50" endpoints, as well as the range "25 to 50."
[0031] As used herein, the terms "comprises," "comprising," "includes," "including," "has," "having," or any other variations thereof, are intended to cover a non-exclusive inclusion. For example, a process, method, article, or apparatus that includes a list of elements is not necessarily limited to only those elements but can include other elements not expressly listed or inherent to such process, method, article, or apparatus.
[0032] Further, unless expressly specified to the contrary, "or" and "and / or" refer to inclusive rather than exclusive. For example, condition A or condition B, or condition A and / or condition B, is satisfied by any one of the following: A being true (or present) and B being false (or absent), A being false (or absent) and B being true (or present), and both A and B being true (or present).
[0033] The use of "a" or "an" to describe various elements and components herein is merely for convenience and to give a general sense of the disclosure. The description should be read to include one or at least one, and the singular also includes the plural unless otherwise clear.
[0034] The term "major portion," as used herein, means greater than 50% of the referenced material, unless otherwise specified herein. Unless specified, percentages are on a molar basis when referring to molecules (e.g., hydrogen, methane, carbon dioxide, carbon monoxide, and hydrogen sulfide), and are otherwise on a mass basis.
[0035] As used herein, unless otherwise specified, the term "substantial portion" or "substantially" means all or nearly all or the majority as would be understood by one of ordinary skill in the relevant art in the context in which it is used. This is intended to allow for reasonable variations from 100% that are typically made in industrial or commercial scale situations.
[0036] The terms "depleted" or "reduced" are synonymous with less than that originally present. For example, removing a substantial portion of a material from a stream will produce a depleted stream that is substantially depleted of that material. Conversely, the terms "enriched" or "increased" are synonymous with more than was originally present.
[0037] The term "number average molecular weight" or "Mn" means number average molecular weight, and the term "weight average molecular weight" or "Mw" means weight average molecular weight, which are determined by gel permeation chromatography (GPC) based on a calibration curve of standard polystyrene. The measuring device and measuring conditions are as shown in the examples.
[0038] The crystallization peak temperature (Tc) is herein determined using a differential scanning calorimeter (DSC) and is defined as the peak top temperature of the exothermic peak observed when a sample is heated from 30° C. to 150° C. at a heating rate of 10° C. / min and then cooled to −100° C. at a cooling rate of 10° C. / min. The measurement is as shown in the examples.
[0039] The term "thermoplastic" has its ordinary meaning, i.e., a material that can become plastic when heated and harden when cooled over multiple cycles, as understood by those of ordinary skill in the relevant art.
[0040] The term "elastomer" also has its ordinary meaning, ie, a material having elastic properties as understood by those skilled in the relevant art.
[0041] The term "substantially homogeneous mixture" means that the components of the mixture are substantially uniformly distributed throughout the mixture by weight. The mixture may have discrete domains (of the same or different size) of one component within a continuous domain of another component, where the discrete domains are substantially uniformly distributed (by weight) within the continuous domain. The level of homogeneity is intended to be that achievable by typical industrial mixing equipment operated under commercially applicable conditions, as will be recognized by those skilled in the relevant art.
[0042] For convenience, many elements of the invention may be discussed separately, alternative lists may be provided, and numerical values may be ranges, but for purposes of this disclosure, this should not be considered a limitation on the scope or support of the disclosure with respect to any claim of any combination of such separate components, lists, or ranges. Unless otherwise specified, each and every combination possible in this disclosure should be considered to be expressly disclosed for all purposes.
[0043] Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present disclosure, suitable methods and materials are described herein. Thus, the materials, methods, and examples herein are illustrative only and, except as specifically stated, are not intended to be limiting.
[0044] Hydrogenated block copolymer component (A) The hydrogenated block copolymer component (A) includes (i) a hydrogenated block copolymer formed by hydrogenating a block copolymer having two or more polymer blocks (a) containing structural units derived from an aromatic vinyl compound and one or more polymer blocks (b) containing structural units derived from isoprene and / or 1,3-butadiene. The resulting hydrogenated block copolymer has a glass transition temperature (Tg) of less than about -45°C and a crystallization peak temperature (Tc) of about -3°C to about 15°C.
[0045] One type of hydrogenated block copolymer can be used alone, or two or more types of hydrogenated block copolymers can be used in combination.
[0046] The polymer block (a) in the hydrogenated block copolymer preferably contains structural units derived from an aromatic vinyl compound in an amount of about 50% by mass or more, about 80% by mass or more, about 90% by mass or more, about 95% by mass or more, or substantially 100% by mass, based on the total mass of the polymer block (a). "Derived from an aromatic vinyl compound" means that the structural unit is a structural unit formed as a result of addition polymerization of an aromatic vinyl compound. Hereinafter, "derived from" will be used in a similar manner.
[0047] Suitable aromatic vinyl compounds include, for example, styrene, α-methylstyrene, p-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, vinyltoluene, 1-vinylnaphthalene, 2-vinylnaphthalene, etc. Among these, styrene and α-methylstyrene are preferred, and styrene is more preferred. The polymer block (a) may be composed of only one of these aromatic vinyl compounds, or may be composed of two or more of these aromatic vinyl compounds.
[0048] As long as the object and effect of the present invention are not hindered, the polymer block (a) may contain structural units derived from copolymerizable monomers other than aromatic vinyl compounds, for example, structural units derived from conjugated dienes such as isoprene, butadiene, 2,3-dimethyl-butadiene, 1,3-pentadiene, 1,3-hexadiene, farnesene, myrcene, etc. The content of structural units derived from other polymerizable monomers in the polymer block (a) is preferably about 10% by mass or less, about 5% by mass or less, about 3% by mass or less, or substantially 0% by mass, based on the total mass of the polymer block (a).
[0049] The polymer block (b) in the hydrogenated block copolymer contains at least one structural unit derived from isoprene and / or at least one structural unit derived from 1,3-butadiene (hereinafter sometimes simply referred to as butadiene). The polymer block (b) may contain a structural unit derived from isoprene and a structural unit derived from butadiene, or may contain only a structural unit derived from butadiene.
[0050] The polymer block (b) in the hydrogenated block copolymer contains at least one of a structural unit derived from isoprene and a structural unit derived from butadiene in an amount of about 50% by mass or more, about 80% by mass or more, about 90% by mass or more, about 95% by mass or more, or substantially 100% by mass, based on the total mass of the polymer block (b). The polymerization form of the polymer block (b) is not particularly limited, and may be random or block.
[0051] Furthermore, from the viewpoint of tensile strength and stress relaxation property, the mass ratio of the structural units derived from isoprene to the structural units derived from butadiene in the polymer block (b) (isoprene / butadiene) is preferably about 49.9 / 50.1, about 49 / 51, or about 48 / 52 to about 40.1 / 59.9, about 41 / 59, or about 42 / 58. The mass ratio is calculated from H-NMR spectrum using the block copolymer before hydrogenation as described in the Examples.
[0052] Furthermore, when the polymer block (b) contains only structural units derived from butadiene, the tear strength at 32°C can be made even more excellent.
[0053] Furthermore, there is no particular limitation on the bond form between isoprene and butadiene in the polymer block (b), that is, the so-called microstructure. For example, isoprene can take the form of 1,2-bond (vinyl bond), 3,4-bond (vinyl bond) or 1,4-bond, and butadiene can take the form of 1,2-bond (vinyl bond) or 1,4-bond. Only one of these bond forms may be present, or two or more of them may be present. Furthermore, any of these bond forms may be present in any ratio, but from the viewpoint of tensile strength, the amount of 1,4-bonds consisting of structural units of isoprene and butadiene is preferably about 50 mol% or more, or about 60 mol% or more, or about 80 mol% or more, or about 90 mol% or more, based on the total moles of units from isoprene and butadiene, from the viewpoint of tensile strength. As an upper limit, such an amount is preferably about 95 mol% or less. Furthermore, from the viewpoint of tensile strength and flexibility, the amount of 1,4-bonds constituted by butadiene structural units is preferably 20 mol% or more, more preferably 30 mol% or more, and even more preferably 35 mol% or more, and is preferably 60 mol% or less, more preferably 50 mol% or less, and even more preferably 45 mol% or less, based on the total moles of butadiene.
[0054] In this specification, the amount of 1,4-bonds is calculated from H-NMR spectrum using a block copolymer before hydrogenation according to the method described in the Examples.
[0055] Furthermore, the polymer block (b) may contain structural units derived from other polymerizable monomers (other than structural units derived from isoprene and butadiene), for example, structural units derived from conjugated dienes such as 2,3-dimethyl-butadiene, 1,3-pentadiene, 1,3-hexadiene, farnesene, and myrcene, and structural units derived from aromatic vinyl compounds such as styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-propylene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, and vinyl-vinyl 2-vinyl compounds, as long as the purpose and effect of the present invention are not hindered. The content of structural units derived from other polymerizable monomers in the polymer block (b) is preferably about 10% by mass or less, about 5% by mass or less, about 3% by mass or less, and / or 0% by mass, based on the total mass of the polymer block (b).
[0056] In the hydrogenated block copolymer, the polymer block (b) is preferably hydrogenated in such a manner that at least about 50 mol%, or at least about 80 mol%, or at least about 90 mol%, or at least about 95 mol%, or at least about 96 mol%, or up to 100 mol%, of the carbon-carbon double bonds in the structural units derived from isoprene and butadiene are hydrogenated from the viewpoints of heat resistance, weather resistance, and tensile strength. This value is sometimes referred to as the hydrogenation ratio.
[0057] In the above hydrogenation ratio, the content of carbon-carbon double bonds in the structural units derived from isoprene and butadiene in the polymer block (b) is measured by H-NMR spectroscopy before and after hydrogenation, and the hydrogenation ratio is obtained from the measured value. More specifically, the value is measured according to the method described in the Examples.
[0058] Polymer block (b) becomes crystalline by hydrogenating the carbon-carbon double bonds. The crystallization peak temperature of the hydrogenated block copolymer can be controlled within the range described below by comprehensively adjusting the butadiene content in polymer block (b), the randomness of the isoprene and butadiene chains, the microstructure, the hydrogenation rate, and the like.
[0059] Generally, crystallinity is observed when about 12 methylene groups are linked in a straight chain. In other words, when 1,4-linked butadienes with three linked butadienes are produced, crystallinity is observed if there is a completely hydrogenated chain. In contrast, when 1,4-linked polyisoprene is completely hydrogenated, it becomes an ethylene-propylene alternating copolymer structure and does not have crystallinity. Therefore, in order to increase the crystallization peak temperature, it is effective to increase the butadiene content, increase the butadiene chains, increase the amount of 1,4-bonds, and increase the hydrogenation rate. Conversely, in order to decrease the crystallization peak temperature, it is effective to increase the isoprene content, increase the randomness of the isoprene-butadiene chains, decrease the amount of 1,4-bonds, and decrease the hydrogenation rate.
[0060] Furthermore, the crystallization peak temperature of the hydrogenated block copolymer is also affected by the temperature during the polymerization reaction of the polymer block (b) and the supply rate of isoprene and butadiene. Therefore, in order to obtain a desired crystallization peak temperature, it is necessary to adjust these appropriately. In other words, by controlling the temperature during the polymerization reaction, the mass ratio of isoprene to butadiene, and the supply rate of isoprene and butadiene, the crystallization peak temperature of the hydrogenated block copolymer can be controlled to a specific value described later.
[0061] The content of the polymer block (a) in the hydrogenated block copolymer is preferably about 20% by mass or about 25% by mass to about 34% by mass or about 33% by mass based on the total mass of the hydrogenated block copolymer. When the content of the polymer block (a) in the hydrogenated block copolymer is about 20% by mass or more, the tensile strength is excellent, and when it is about 34% by mass or less, the stress relaxation property is excellent. This range is also preferable from the viewpoint of molding processability.
[0062] The content of polymer block (a) in the hydrogenated block copolymer is a value obtained from the H-NMR spectrum after hydrogenation, and more specifically, a value measured according to the method described in the Examples.
[0063] The bonding mode between the polymer block (a) and the polymer block (b) in the hydrogenated block copolymer may be linear, branched, radial, or any combination thereof.
[0064] For example, when polymer block (a) is represented by "A" and polymer block (b) is represented by "B", examples thereof include a triblock copolymer represented by "ABA", a tetrablock copolymer represented by "ABAB", a pentablock copolymer represented by "ABABA" and "BABAB", and an (AB)nX type copolymer (X represents a coupling agent residue, and n represents an integer of 3 or more). Among these, from the viewpoint of ease of production, a triblock copolymer represented by "ABA" and a tetrablock copolymer represented by "ABAB" are preferred as the hydrogenated block copolymer (A), and a triblock copolymer represented by "ABA" is more preferably used.
[0065] Here, in this specification, when the same type of polymer blocks are linearly bonded via a bifunctional coupling agent or the like, the entirety of the bonded polymer blocks is treated as one polymer block. Accordingly, including the above examples, polymer blocks that should be strictly represented as YXY (X represents a coupling residue) are generally represented as Y, except when it is necessary to distinguish them from a single polymer block Y. In this specification, since this type of polymer block containing a coupling agent residue is treated as above, for example, a block copolymer containing a coupling agent residue and that should be strictly represented as ABXBA (X represents a coupling agent residue) is represented as ABA and is treated as an example of a triblock copolymer.
[0066] The hydrogenated block copolymer has a glass transition temperature (Tg) of less than about -45°C. If the hydrogenated block copolymer has a glass transition temperature of about -45°C or higher, the tensile strength and tear strength may be poor. From this viewpoint, the hydrogenated block copolymer preferably has a glass transition temperature of -65°C or about -60°C to less than about -50°C or about -51°C.
[0067] The glass transition temperature can be measured in accordance with JIS K7121:2012, specifically, by the method described in the examples.
[0068] The hydrogenated block copolymer has a crystallization peak temperature (Tc) of about -3°C to about 15°C, as defined below.
[0069] If the crystallization peak temperature of the hydrogenated block copolymer is less than about -3°C, the tensile strength may be poor, and if it exceeds about 15°C, the stress relaxation property may be poor. From this viewpoint, the crystallization peak temperature is preferably from about 0°C or about 2°C or about 5°C to about 14°C or about 13°C or about 11°C.
[0070] The weight average molecular weight (Mw) of the hydrogenated block copolymer is preferably about 50,000 or about 60,000 or about 65,000 or about 70,000 to about 500,000 or about 400,000 or about 300,000 or about 115,000. When the weight average molecular weight of the hydrogenated block copolymer is about 50,000 or more, the tensile strength is excellent, and when it is about 500,000 or less, the moldability is excellent.
[0071] From the viewpoint of stress relaxation properties, the molecular weight distribution (Mw / Mn) of the hydrogenated block copolymer is preferably 1.5 or less, or about 1.01 to about 1.5, or about 1.3, or about 1.2, or about 1.1, or about 1.05.
[0072] The hydrogenated block copolymer may have one or more functional groups, such as a carboxyl group, a hydroxyl group, an acid anhydride group, an amino group, and / or an epoxy group, in the molecular chain and / or at the molecular terminal, as long as the effects of the present invention are not significantly impaired.
[0073] Method for producing hydrogenated block copolymer The hydrogenated block copolymer can be produced, for example, by an anionic polymerization method. Specifically, it can be produced by carrying out a polymerization reaction by, for example, (1) a method of sequentially polymerizing an aromatic vinyl compound with isoprene and butadiene using an alkyllithium compound as an initiator; (2) a method of sequentially polymerizing an aromatic vinyl compound with isoprene and butadiene using an alkyllithium compound as an initiator, and then coupling by adding a coupling agent; or (3) a method of sequentially polymerizing isoprene and butadiene and then an aromatic vinyl compound using a dilithium compound as an initiator; and then carrying out a hydrogenation reaction.
[0074] The isoprene and butadiene may be co-fed separately to the reactor and mixed in the reactor, or the isoprene and butadiene may be premixed and fed to the reactor, or both the former and latter methods may be used.
[0075] Alkyllithium compounds include, for example, methyllithium, ethyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, and pentyllithium.
[0076] Examples of coupling agents include divinylbenzene; polyfunctional epoxy compounds such as epoxidized 1,2-polybutadiene, epoxidized soybean oil, and 1,3-bis(N,N-glycidylaminomethyl)cyclohexane; halogen compounds such as dimethyldichlorosilane, dimethyldibromosilane, trichlorosilane, methyltrichlorosilane, tetrachlorosilane, and tetrachlorotin; ester compounds such as methyl benzoate, ethyl benzoate, phenyl benzoate, diethyl oxalate, diethyl malonate, diethyl adipate, dioctyl adipate, dimethyl phthalate, diethyl phthalate, dimethyl isophthalate, and dimethyl terephthalate; carbonate compounds such as dimethyl carbonate, diethyl carbonate, and diphenyl carbonate; and alkoxysilane compounds such as dimethyldimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, tetramethoxysilane, tetraethoxysilane, bis(trimethoxysilyl)hexane, and bis(triethoxysilyl)ethane.
[0077] Examples of dilithium compounds include naphthalene dilithium, dithiohexylbenzene, and the like.
[0078] The polymerization reaction is preferably carried out in the presence of a solvent. The solvent is not particularly limited as long as it is inactive to the initiator and does not adversely affect the reaction, and examples thereof include saturated aliphatic hydrocarbons such as hexane, cyclohexane, heptane, octane, and decane; and aromatic hydrocarbons such as toluene, benzene, and xylene. The polymerization reaction is usually carried out at about 0°C or about 30°C or about 40°C or about 50°C to about 100°C or about 90°C or about 80°C for about 0.5 hours to about 50 hours from the viewpoint of microstructure control.
[0079] In addition, a Lewis base may be used as a cocatalyst in the polymerization reaction. Examples of the Lewis base include ethers such as dimethyl ether, diethyl ether, and tetrahydrofuran; glycol ethers such as ethylene glycol dimethyl ether and diethylene glycol dimethyl ether; and amines such as triethylamine, N,N,N',N'-tetramethylethylenediamine, and N-methylmorpholine. These Lewis bases may be used alone or in combination of two or more.
[0080] The hydrogenation reaction may be carried out immediately after the polymerization reaction, or may be carried out after isolating the block copolymer after the polymerization reaction.
[0081] When the block copolymer is isolated once after the polymerization reaction, the block copolymer can be isolated by pouring the obtained polymerization reaction liquid into a poor solvent for the block copolymer, such as methanol, to coagulate the block copolymer, or by pouring the polymerization reaction liquid together with steam into hot water to remove the solvent by azeotropy (steam stripping), and then drying the block copolymer.
[0082] The hydrogenation reaction of the block copolymer is carried out in the presence of hydrogenation catalysts such as Raney nickel; heterogeneous catalysts in which metals such as platinum (Pt), palladium (Pd), ruthenium (Ru), rhodium (Rh), or nickel (Ni) are supported on a carrier such as carbon, alumina, or diatomaceous earth; Ziegler catalysts consisting of a combination of transition metal compounds (nickel octylate, nickel naphthenate, nickel acetylacetonate, cobalt octylate, cobalt naphthenate, cobalt acetylacetonate, etc.) and organoaluminum compounds and organolithium compounds such as triethylaluminum and triisobutylaluminum; and metallocene catalysts consisting of bis(cyclopentadienyl) compounds of transition metals such as titanium, zirconium, and hafnium and organometallic compounds such as lithium, sodium, potassium, aluminum, zinc, and magnesium. The reaction can be carried out at a reaction temperature of about 20°C to about 200°C and a hydrogen pressure of about 0.1 MPa to about 20 MPa for a time period of about 0.1 hours to 100 hours.
[0083] When the polymerization reaction and the hydrogenation reaction are carried out successively, the hydrogenated block copolymer can be isolated by pouring the hydrogenation reaction liquid into a poor solvent for the hydrogenated block copolymer, such as methanol, to coagulate it, or by pouring the hydrogenation reaction liquid together with steam into hot water to remove the solvent by azeotropy (steam stripping), and then drying.
[0084] The content of the hydrogenated block copolymer component (A) in the thermoplastic elastomer composition is about 18 parts by mass or about 20 parts by mass or about 25 parts by mass to about 60 parts by mass or about 55 parts by mass or about 50 parts by mass per 100 parts by mass of the hydrogenated block copolymer component (A), the thermoplastic resin component (B), the rubber softener component (C), and the polyolefin elastomer component (D). If the content of the hydrogenated block copolymer component (A) is less than about 18 parts by mass, the tear strength, tensile strength, and stress relaxation properties may be poor, and if it exceeds about 60 parts by mass, the anisotropy may deteriorate and the molding processability may decrease.
[0085] Thermoplastic resin component (B) Examples of thermoplastic resins suitable for use in the thermoplastic resin component (B) of the present invention include polystyrene resins, polyethylene resins, polypropylene resins, acrylic resins, polyphenylene ether resins, polycarbonate resins, polyvinyl acetate resins, polyester resins, polyamide resins, polyvinyl chloride resins, petroleum resins, and hydrogenated petroleum resins.
[0086] The petroleum resin means a product obtained by polymerizing a fraction containing unsaturated hydrocarbon monomers produced as a by-product by thermal cracking of petroleum naphtha or the like.
[0087] In addition, the component corresponding to the polyolefin elastomer (D) described later is not included in the thermoplastic resin (B).
[0088] The thermoplastic resins may be used alone or in combination of two or more. Among them, polystyrene-based resins are preferably used as the thermoplastic resin (B).
[0089] Polystyrene resins include polystyrene [general-purpose polystyrene (GPPS) and high-impact polystyrene (HIPS)], polyorthomethylstyrene, polyparamethylstyrene, polydimethylstyrene, polymethylstyrene, polychlorostyrene, polyisopropylstyrene, polytertiary butylstyrene, poly-α-methylstyrene, polyethylvinyltoluene, styrene-maleimide copolymer, styrene-N-phenylmaleimide copolymer, styrene-N-phenylmaleimide-acrylonitrile copolymer, styrene-N-phenylmaleimide-methacrylonitrile copolymer, and styrene-N-phenylmaleimide-methacrylonitrile copolymer. Examples of such rubber-reinforced acrylic ester rubber include methyl acrylate copolymer, styrene-N-phenylmaleimide-butyl acrylate copolymer, rubber-reinforced impact resistant polystyrene, acrylonitrile-styrene copolymer (AS resin), acrylonitrile-butadiene-styrene copolymer (ABS resin), acrylonitrile-ethylene-propylene rubber-reinforced styrene copolymer (AES resin), acrylonitrile-polyacrylic acid ester rubber-reinforced styrene copolymer (AAS resin), methyl methacrylate-styrene copolymer (MS resin), and methyl methacrylate-butadiene-styrene copolymer (MBS resin).
[0090] In one embodiment, the weight average molecular weight (Mw) of the polystyrene resin is preferably within the range of about 1,000 or about 2,000 or about 3,000 to about 400,000 or about 350,000 or about 300,000. When the weight average molecular weight of the polystyrene resin is about 1,000 or more, the stress relaxation property of the obtained thermoplastic elastomer composition is improved and problems such as odor are reduced, and when it is about 400,000 or less, the processability of the thermoplastic elastomer composition is improved.
[0091] The polystyrene resin may be one type of polystyrene resin or a combination of two or more types of polystyrene resins, for example, a combination of a high molecular weight polystyrene resin and a low molecular weight polystyrene resin.
[0092] The weight average molecular weight of such a high molecular weight polystyrene resin is preferably within the range of about 100,000 or about 120,000 or about 150,000 to about 400,000 or about 350,000 or about 300,000. When the weight average molecular weight of the high molecular weight polystyrene resin is about 100,000 or more, the stress relaxation property of the obtained thermoplastic elastomer composition is improved and problems such as odor are reduced, and when it is about 400,000 or less, the processability of the thermoplastic elastomer composition is improved.
[0093] The weight average molecular weight of such low molecular weight polystyrene resin is preferably within the range of about 1,000 or about 2,000 or about 3,000 to less than about 100,000 or about 50,000 or about 20,000. When the weight average molecular weight of the low molecular weight polystyrene resin is about 1,000 or more, the stress relaxation property of the obtained thermoplastic elastomer composition is improved and problems such as odor are reduced, and when it is less than 100,000, the dispersibility of the thermoplastic elastomer composition is improved. Furthermore, the tear strength at 25°C is good.
[0094] The Z-average molecular weight (Mz) of such a low molecular weight polystyrene resin is preferably within the range of about 1,000 or about 2,000 or about 5,000 to about 30,000 or about 11,000 or about 9,000. When the Z-average molecular weight of the low molecular weight polystyrene resin is within the above range, the tear resistance (Slow) at 25°C and the tear strength in the Elmendorf test become good.
[0095] In this specification, the Z-average molecular weight is a value calculated in terms of standard polystyrene by gel permeation chromatography (GPC).
[0096] The glass transition temperature (Tg) of such a low molecular weight polystyrene resin is preferably about 40°C, about 50°C, or about 60°C to about 110°C, about 95°C, or about 80°C, from the viewpoints of tear resistance (Slow) at 25°C and tear strength in the Elmendorf test.
[0097] The glass transition temperature can be measured in accordance with JIS K7121:2012.
[0098] Such high molecular weight polystyrene resins are commonly known and commercially available, for example, Styrolution PS3190 (INEOS Styrolution America LLC).
[0099] Such low molecular weight polystyrene resins are commonly known and commercially available, for example, Kristalex™ 5140 (EASTMAN Chemical Company), Kristalex™ 3100 (EASTMAN Chemical Company), Piccotex™ 120 (EASTMAN Chemical Company), and Piccotex™ 100 (EASTMAN Chemical Company).
[0100] Examples of suitable polyethylene-based resins include ethylene homopolymers, such as high density polyethylene and low density polyethylene, and various ethylene copolymers in which ethylene is the major monomer component, such as ethylene-propylene copolymers, ethylene-1-butene copolymers, ethylene-1-hexene copolymers, ethylene-1-heptene copolymers, ethylene-1-octene copolymers, ethylene-4-methyl-1-pentene copolymers, ethylene-1-nonene copolymers, ethylene-1-decene copolymers, ethylene-α-olefin copolymers, e.g., ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, ethylene-methacrylic acid copolymers, ethylene-methacrylic acid copolymers, and ethylene homopolymers and copolymers modified with maleic anhydride.
[0101] Examples of suitable polypropylene-based resins include homopolypropylene, random polypropylene, and block polypropylene.
[0102] Examples of suitable polyester resins include polyethylene terephthalate, polybutylene terephthalate, polylactic acid, and polycaprolactone.
[0103] Examples of suitable polyamide resins include polyamide 6, polyamide 6·6, polyamide 6·10, polyamide 11, polyamide 12, polyamide 6·12, polyhexamethylenediamine terephthalamide, polyhexamethylenediamine isophthalamide, and xylene group-containing polyamides.
[0104] The content of the thermoplastic resin component (B) is about 3 parts by mass or about 5 parts by mass or about 10 parts by mass to about 24 parts by mass or about 20 parts by mass or about 18 parts by mass per 100 parts by mass of the hydrogenated block copolymer component (A), the thermoplastic resin component (B), the rubber softener component (C), and the polyolefin elastomer component (D). If the content of the thermoplastic resin component (B) is less than about 3 parts by mass, the tear strength may decrease, and if it exceeds about 24 parts by mass, the stress relaxation property may decrease.
[0105] Rubber softener component (C) Examples of rubber softeners suitable for use as the rubber softener component (C) include mineral oils such as paraffinic process oil and naphthenic process oil, vegetable oils such as peanut oil and rosin, phosphoric acid esters, low molecular weight polyethylene glycols, liquid paraffin, and synthetic oils such as low molecular weight ethylene, ethylene-α-olefin copolymer oligomers, liquid polybutene, liquid polyisoprene or hydrogenated products thereof, and liquid polybutadiene or hydrogenated products thereof. These may be used alone or in combination of two or more.
[0106] Among them, paraffin-based oils such as paraffin-based process oils and liquid paraffin are preferably used. The paraffin-based oil preferably has a kinetic viscosity of about 20 mm at 40°C. 2 / s or about 50 mm 2 / s~approx. 1,500mm 2 / s or approximately 1,000 mm 2 / s or about 500 mm 2 / s.
[0107] The content of the rubber softener component (C) is about 3 parts by mass or about 5 parts by mass or about 8 parts by mass or about 10 parts by mass to about 25 parts by mass or about 20 parts by mass or about 18 parts by mass or about 15 parts by mass per 100 parts by mass of the hydrogenated block copolymer component (A), the thermoplastic resin component (B), the rubber softener component (C), and the polyolefin elastomer component (D). If the content of the rubber softener (C) is less than about 3 parts by mass, molding processability may decrease, and if it exceeds about 25 parts by mass, tensile strength may decrease.
[0108] Polyolefin elastomer component (D) Polyolefin elastomers Examples of polyolefin elastomers suitable for use in component (D) include polymers derived primarily from one or more alpha-olefin monomers, such as polyethylene elastomers, polypropylene elastomers, and the like.
[0109] Here, the polyethylene elastomer refers to an elastomer containing a majority (by mass) of ethylene, and the polypropylene elastomer refers to an elastomer containing a majority (by mass) of propylene. Among them, it is preferable to use a polypropylene-based elastomer from the viewpoints of processability and heat resistance.
[0110] Examples of structural units derived from other than ethylene contained in the polyethylene elastomer include structural units derived from propylene, and structural units derived from α-olefins such as 1-butene, 1-hexene, 1-heptene, 1-octene, 4-methyl-1-pentene, 1-nonene, and 1-decene. Among them, from the viewpoints of processability and tear strength, ethylene / propylene random copolymers and ethylene / butene random copolymers are preferred.
[0111] Examples of structural units derived from other than propylene contained in the polypropylene elastomer include structural units derived from ethylene and structural units derived from α-olefins such as 1-butene, 1-hexene, 1-heptene, 1-octene, 4-methyl-1-pentene, 1-nonene, and 1-decene.
[0112] Examples of polypropylene-based elastomers include homopolypropylene, propylene / ethylene random copolymers, propylene / ethylene block copolymers, propylene / butene random copolymers, propylene / ethylene / butene random copolymers, propylene / pentene random copolymers, propylene / hexene random copolymers, propylene / octene random copolymers, propylene / ethylene / pentene random copolymers, propylene / ethylene / hexene random copolymers, etc. Among these, from the viewpoints of processability and heat resistance, propylene / ethylene random copolymers and propylene / butene random copolymers are preferred, and from the viewpoint of tear strength, propylene / ethylene random copolymers are more preferred.
[0113] The content of structural units derived from propylene in the polypropylene elastomer is preferably more than about 50 mass%, about 70 mass%, about 75 mass%, or about 80 mass%, and up to about 99 mass%, about 98 mass%, about 95 mass%, or about 90 mass%, based on the total mass of the polypropylene-based elastomer, from the viewpoints of tear strength and heat resistance.
[0114] When the polypropylene elastomer contains a structural unit derived from ethylene, the content thereof is preferably about 1 mass %, or about 2 mass %, or about 5 mass %, or about 10 mass % to about 50 mass %, or about 30 mass %, or about 25 mass %, or about 20 mass %, based on the total mass of the polypropylene elastomer, from the viewpoints of tear strength and stress relaxation property.
[0115] In particular, when the polyolefin elastomer contains a polypropylene elastomer containing structural units derived from ethylene, and the content of the structural units derived from ethylene is preferably about 13.0 mass% or about 14.5 mass% to about 15.9 mass% or about 14.8 mass% relative to the total mass of the polypropylene elastomer, in addition to improving the tear strength at 32°C and the tear strength at 38°C, a good balance of flexibility is achieved.
[0116] The polypropylene-based elastomer preferably has a melt flow rate (MFR) of about 1 g / 10 min, about 1.5 g / 10 min, or about 2 g / 10 min to about 300 g / 10 min, about 100 g / 10 min, or about 50 g / 10 min, measured at a temperature of 230° C. and a load of 2.16 kg according to ASTM D1238. When the MFR of the polypropylene elastomer is within the above range, the polypropylene elastomer can be molded into a film, sheet, etc. at high speed.
[0117] The density of the polypropylene-based elastomer is preferably about 0.850 g / cm 3 or about 0.855 g / cm 3 or about 0.860 g / cm 3 ~Approx. 0.910g / cm 3 or about 0.890 g / cm 3 or about 0.880 g / cm 3 The density of the polypropylene elastomer is in the range of about 0.850 g / cm 3 If it is more than 0.910g / cm, the tear strength is excellent. 3 When the thickness is not more than this, the stress relaxation property is excellent.
[0118] The density of the polypropylene-based elastomer can be measured in accordance with ASTM D1505.
[0119] The Vicat softening point of the polypropylene elastomer is preferably about 40° C. or about 45° C. or about 50° C. to about 100° C. or about 80° C. or about 70° C. When the Vicat softening point of the polypropylene elastomer is about 40° C. or higher, it has excellent heat resistance, and when it is about 100° C. or lower, it has excellent stress relaxation properties.
[0120] The Vicat softening point of the polypropylene-based elastomer can be measured in accordance with ASTM D1525.
[0121] The weight average molecular weight (Mw) of the polypropylene elastomer is preferably about 40,000 or about 100,000 or about 200,000 to about 500,000 or about 400,000 or about 350,000. When the weight average molecular weight of the polypropylene elastomer is about 40,000 or more, it has excellent mechanical properties, and when it is about 500,000 or less, it has excellent moldability.
[0122] Polyolefin elastomers are commonly known and commercially available, for example, Vistamaxx™ 6102, 6202, 3020FL, 3980FL, and 3588FL (ExxonMobil).
[0123] The content of the polyolefin elastomer component (D) is about 5 parts by mass or about 8 parts by mass or about 10 parts by mass or about 20 parts by mass to about 76 parts by mass or about 70 parts by mass or about 60 parts by mass or about 55 parts by mass per 100 parts by mass of the hydrogenated block copolymer component (A), the thermoplastic resin component (B), the rubber softener component (C), and the polyolefin elastomer component (D). If the content of the polyolefin elastomer component (D) is less than about 5 parts by mass, the anisotropy may deteriorate (increase), and if it exceeds about 76 parts by mass, the elastic recovery, tear strength, and stress relaxation properties may decrease.
[0124] Furthermore, when the content of the polyolefin elastomer (D) is preferably within the range of about 55% by mass to about 70% by mass or about 65% by mass, based on the total amount of the thermoplastic elastomer composition, the tear strength at 32°C and the tear strength at 38°C can be improved.
[0125] Hydrogenated block copolymer (E) It is preferable that the thermoplastic elastomer composition of the present invention further contains a hydrogenated block copolymer component (E) from the viewpoint of reducing anisotropy.
[0126] A hydrogenated block copolymer suitable for the hydrogenated block copolymer (E) is formed by hydrogenating a block copolymer having a polymer block (x) containing more than about 70 mass% (based on the total mass of the polymer block (x)) of structural units derived from an aromatic vinyl compound, and a polymer block (y) containing about 30 mass% or more (based on the total mass of the polymer block (y)) of structural units derived from at least one selected from the group consisting of a conjugated diene compound and isobutylene.
[0127] One type of hydrogenated block copolymer can be used alone, or two or more types of hydrogenated block copolymers can be used in combination.
[0128] The polymer block (x) in the hydrogenated block copolymer contains more than about 70% by mass of structural units derived from aromatic vinyl compounds. If the content of structural units derived from aromatic vinyl compounds is less than about 70% by mass, the tensile strength and stress relaxation properties may decrease. From this viewpoint, the content of structural units derived from aromatic vinyl compounds is preferably about 80% by mass or more, about 85% by mass or more, about 90% by mass or more, about 95% by mass or more, or substantially 100% by mass.
[0129] Examples of the aromatic vinyl compound include the same aromatic vinyl compounds as those used for the hydrogenated block copolymer of the hydrogenated block copolymer component (A). Among them, from the viewpoint of tensile strength, styrene, α-methylstyrene, p-methylstyrene, and mixtures thereof are preferred, and styrene is more preferred.
[0130] The polymer block (x) may contain structural units derived from polymerizable monomers other than aromatic vinyl compounds at a ratio of about 30% by mass or less, about 20% by mass or less, about 10% by mass or less, about 5% by mass or less, or substantially 0% by mass (non-existent), as long as the purpose and effect of the present invention are not hindered. Examples of structural units derived from other polymerizable monomers include the same structural units derived from other polymerizable monomers as those used for the hydrogenated block copolymer of the hydrogenated block copolymer component (A).
[0131] When the polymer block (x) contains a structural unit derived from another polymerizable monomer, the bonding form is not particularly limited and may be either random or tapered.
[0132] The hydrogenated block copolymer may have at least one polymer block (x). When the hydrogenated block copolymer has two or more polymer blocks (x), the polymer blocks (x) may be the same or different. In this specification, the term "polymer blocks are different" means that at least one of the monomer units constituting the polymer blocks, the weight average molecular weight, the stereoregularity, and, when a plurality of monomer units are present, the ratio of the monomer units and the form of copolymerization (random, gradient, block) are different.
[0133] The content of the polymer block (x) in the hydrogenated block copolymer (E) (when a plurality of polymer blocks (x) are contained, the total content thereof) is about 4% by mass, about 8% by mass, about 10% by mass, or about 11% by mass to about 30% by mass, about 25% by mass, about 20% by mass, or about 15% by mass. If the content of the polymer block (x) is less than about 4% by mass, the processability may decrease, and if it exceeds about 30% by mass, the stress relaxation property and anisotropy may deteriorate.
[0134] The content of the polymer block (x) in the hydrogenated block copolymer (E) is a value obtained by H-NMR spectrum after hydrogenation, more specifically, a value measured according to the method described in the Examples.
[0135] The polymer block (y) in the hydrogenated block copolymer (E) contains about 30% by mass or more of structural units derived from at least one selected from the group consisting of conjugated diene compounds and isobutylene. If the content of structural units derived from at least one selected from the group consisting of conjugated diene compounds and isobutylene is less than about 30% by mass, the tensile strength may decrease. From this viewpoint, the content of structural units derived from at least one selected from the group consisting of conjugated diene compounds and isobutylene is preferably about 50% by mass or more, about 65% by mass or more, or about 80% by mass or more.
[0136] The polymer block (y) in the hydrogenated block copolymer (E) may contain about 30% by mass or more of structural units derived from a conjugated diene compound, may contain 30% by mass or more of structural units derived from isobutylene, or may contain 30% by mass or more of structural units derived from a mixture of a conjugated diene compound and isobutylene. The polymer block (y) may have only structural units derived from one type of conjugated diene compound, or may have structural units derived from two or more types of conjugated diene compounds.
[0137] When the polymer block (y) has two or more kinds of structural units, the bonding form thereof may be random, tapered, completely alternating, partially block-like, block, or a combination of two or more of them.
[0138] Examples of conjugated diene compounds include isoprene, butadiene, hexadiene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, farnesene, myrcene, and mixtures thereof. Among them, isoprene, butadiene, and a mixture of isoprene and butadiene are preferred, and any of these may be used, and among these, isoprene is more preferred. In the case of a mixture of butadiene and isoprene, there is no particular restriction on the mixing ratio [isoprene / butadiene] (mass ratio), but it is preferably about 5 / 95 or about 10 / 90 or about 40 / 60 or about 45 / 55 to about 95 / 5 or about 90 / 10 or about 70 / 30 or about 65 / 35 or about 55 / 45. The mixing ratio [isoprene / butadiene], expressed as a molar ratio, is preferably about 5 / 95, about 10 / 90, about 40 / 60, or about 45 / 55 to about 95 / 5, about 90 / 10, about 70 / 30, or about 55 / 45.
[0139] When the structural unit constituting the polymer block (y) in the hydrogenated block copolymer is any one of a structural unit derived from isoprene, a structural unit derived from butadiene, and a structural unit derived from a mixture of isoprene and butadiene, the hydrogenated block copolymer may contain 1,2-bonds and / or 3,4-bonds in the case of butadiene, and may contain 1,2-bonds, 3,4-bonds and / or 1,4-bonds in the case of isoprene.
[0140] In the hydrogenated block copolymer, the total content of 3,4-bond units and 1,2-bond units in the polymer block (y) (hereinafter sometimes referred to as vinyl bond amount) is preferably about 20 mol% or more, about 40 mol% or more, or about 50 mol% or more. Although not particularly limited, the vinyl bond amount in the polymer block (y) is preferably about 90 mol% or less, or about 85 mol% or less. Here, the vinyl bond is a value calculated by measuring H-NMR according to the method described in the Examples.
[0141] When the polymer block (y) is composed only of butadiene, the term "content of 3,4-bond units and 1,2-bond units" is replaced with "content of 1,2-bond units".
[0142] The polymer block (y) in the hydrogenated block copolymer may contain structural units derived from conjugated diene compounds and polymerizable monomers other than isobutylene, as long as the purpose and effect of the present invention are not hindered. In this case, the content of structural units derived from conjugated diene compounds and polymerizable monomers other than isobutylene in the polymer block (y) is preferably less than about 70% by mass, or less than about 50% by mass, or less than about 35% by mass, or less than about 20% by mass, or less than about 15% by mass, and is 5% by mass or more.
[0143] The other polymerizable monomers are preferably at least one compound selected from the group consisting of aromatic vinyl compounds such as styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, pt-butylstyrene, 2,4-dimethylstyrene, vinylnaphthalene and vinylanthracene, as well as methyl methacrylate, methyl vinyl ether, N-vinylcarbazole, β-pinene, p-menthane-8,9-diol, dipentene, methylenenorbornene, 2-methylenetetrahydrofuran, 1,3-cyclopentadiene, 1,3-cyclohexadiene, 1,3-cycloheptadiene, etc. Among them, styrene, α-methylstyrene and p-methylstyrene are preferred, and styrene is more preferred.
[0144] When the polymer block (y) contains structural units derived from a conjugated diene compound and a polymerizable monomer other than isobutylene, the specific combinations are preferably isoprene and styrene, butadiene and styrene, a mixture of isoprene and butadiene and styrene, and more preferably isoprene and styrene, and a mixture of isoprene and butadiene and styrene.
[0145] When the polymer block (y) contains structural units derived from a conjugated diene compound and a polymerizable monomer other than isobutylene, the bonding form is not particularly limited and may be either random or tapered.
[0146] The hydrogenated block copolymer may have at least one polymer block (y). When the hydrogenated block copolymer has two or more polymer blocks (y), the polymer blocks (y) may be the same or different.
[0147] The bonding mode between the polymer block (x) and the polymer block (y) in the hydrogenated block copolymer may be linear, branched, radial, or any combination thereof. Of these, the bonding mode between the polymer block (x) and the polymer block (y) is preferably linear, and examples thereof include a diblock copolymer represented by "PQ", a triblock copolymer represented by "PQP", a tetrablock copolymer represented by "PQPQ", a pentablock copolymer represented by "PQPQP" and "QPQPQ", and a (PQ)nX type copolymer (X represents a coupling agent residue, and n represents an integer of 3 or more) when the polymer block (x) is represented by "P" and the polymer block (y) is represented by "Q". Of these, a linear triblock copolymer or a diblock copolymer is preferred, and a PQP type triblock copolymer is preferably used from the viewpoint of processability.
[0148] In the hydrogenated block copolymer (E), the polymer block (y) is preferably hydrogenated in at least about 80 mol%, or at least about 85 mol%, or at least about 88 mol% of the carbon-carbon double bonds in the structural units derived from the conjugated diene compound and isobutylene from the viewpoint of tensile strength. There is no particular upper limit to the hydrogenation rate, but the upper limit may be about 99 mol%, or about 98 mol%.
[0149] On the other hand, when crosslinking or foaming is taken into consideration, the hydrogenation rate may be about 50 mol % or less, or about 10 mol % or less, or about 5 mol % or less, or about 3 mol % or less.
[0150] The hydrogenation rate is a value calculated from the measured values by measuring the content of carbon-carbon double bonds in the structural units derived from the conjugated diene compound and isobutylene in the polymer block (y) using H-NMR spectrum before and after hydrogenation. More specifically, this is a value measured according to the method described in the examples.
[0151] The glass transition temperature (Tg) of the hydrogenated block copolymer is about -45°C to about 30°C. If the glass transition temperature of the hydrogenated block copolymer (E) is less than about -45°C, the anisotropy may deteriorate, and if it exceeds about 30°C, the stress relaxation property may decrease. From this viewpoint, the glass transition temperature of the hydrogenated block copolymer (E) is preferably about -40°C to about 10°C or about 0°C.
[0152] The glass transition temperature can be measured in accordance with JIS K7121:2012, specifically, by the method described in the examples.
[0153] The weight average molecular weight (Mw) of the hydrogenated block copolymer is preferably about 20,000 or about 50,000 or about 70,000 or about 90,000 or about 130,000 to about 800,000 or about 700,000 or about 600,000 or about 500,000 or about 450,000. When the weight average molecular weight of the hydrogenated block copolymer is about 20,000 or more, it has excellent tensile strength, and when it is about 800,000 or less, it has excellent moldability.
[0154] The molecular weight distribution (Mw / Mn) of the hydrogenated block copolymer is preferably about 1.5 or less, or about 1.4 or less, or about 1.3 or less, or about 1.2 or less to about 1.0.
[0155] The hydrogenated block copolymer (E) may have one or more functional groups, such as a carboxyl group, a hydroxyl group, an acid anhydride group, an amino group, and an epoxy group, in the molecular chain and / or at the molecular terminal, as long as the effects of the present invention are not significantly impaired.
[0156] Method for producing hydrogenated block copolymer (E) The hydrogenated block copolymer (E) can be produced by a solution polymerization method, an emulsion polymerization method, a solid-phase polymerization method, or the like. Among these, the solution polymerization method is preferred, and known methods such as an ionic polymerization method such as anionic polymerization or cationic polymerization, or a radical polymerization method can be applied. Among these, the anionic polymerization method is preferred. The production method by the anionic polymerization method is as described above in the section on the production method of the hydrogenated block copolymer of the hydrogenated block copolymer component (A).
[0157] The content of the hydrogenated block copolymer component (E) is preferably about 3 parts by mass or about 4 parts by mass or about 5 parts by mass to about 15 parts by mass or about 13 parts by mass or about 12 parts by mass based on the total mass of the hydrogenated block copolymer component (A), the thermoplastic resin component (B), the rubber softener component (C), the polyolefin elastomer component (D), and the hydrogenated block copolymer component (E). When the content of the hydrogenated block copolymer (E) is about 3 parts by mass or more, the anisotropy is reduced, and when it is about 15 parts by mass or less, the tensile strength is excellent.
[0158] Other optional ingredients In addition to the above components, other components may be blended into the thermoplastic elastomer composition of the present invention depending on the purpose, within the scope that does not significantly impair the effects of the present invention.
[0159] Examples of other components include various additives such as fillers, antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, neutralizing agents, lubricants, antifogging agents, antiblocking agents, tackifiers, colorants, flame retardants, antistatic agents, crosslinking agents, conductivity imparting agents, antibacterial agents, and antifungal agents, thermoplastic resins other than the above-mentioned components, and elastomers other than the above-mentioned essential components, etc. Any of these may be used alone or in combination of two or more.
[0160] The total content of the hydrogenated block copolymer (A), the thermoplastic resin (B), the rubber softener (C), and the polyolefin elastomer (D) in the thermoplastic elastomer composition of the present invention is preferably about 80 mass % or more, about 85 mass % or more, or about 90 mass % or more, based on the total mass of the thermoplastic elastomer composition.
[0161] The thermoplastic elastomer composition of the present invention can be produced by mixing the hydrogenated block copolymer (A), the thermoplastic resin (B), the rubber softener (C), the polyolefin elastomer (D), the hydrogenated block copolymer (E) which is blended as required, and other optional components. As a mixing method, a conventionally used method can be adopted, for example, after uniformly mixing using a mixing device such as a high-speed mixer, a ribbon blender, or a V-type blender, the mixture may be melt-kneaded using a kneading device such as a mixing roll, a kneader, a Banbury mixer, a Brabender mixer, or a single-screw or twin-screw extruder. Kneading is generally performed at a temperature of about 120°C to about 280°C.
[0162] sea island structure From the viewpoint of reducing anisotropy, the thermoplastic elastomer composition of the present invention preferably has a sea-island structure of resin components consisting of the polyolefin elastomer component (D) and a component other than the polyolefin elastomer component (D). Here, the sea-island structure means a phase-separated structure in which an island phase exists in a sea phase. The polyolefin elastomer component (D) may be the island phase and the component other than the polyolefin elastomer component (D) may be the sea phase, or the polyolefin elastomer component (D) may be the sea phase and the component other than the polyolefin elastomer component (D) may be the island phase. From the viewpoint of reducing anisotropy, it is preferable that the polyolefin elastomer component (D) is the sea phase and the component other than the polyolefin elastomer component (D) is the island phase, and from the viewpoint of improving tear strength and stress relaxation property, it is preferable that the polyolefin elastomer component (D) is the island phase and the component other than the polyolefin elastomer component (D) is the sea phase. Furthermore, from the viewpoint of tear strength, it is preferred that the polyolefin elastomer component (D) and components other than the polyolefin elastomer component (D) are finely dispersed in the thermoplastic elastomer composition.
[0163] From the viewpoint of reducing anisotropy, the thermoplastic elastomer composition of the present invention preferably does not have a co-continuous structure. Here, the co-continuous structure means a network structure in which two or more components are mixed with each other while forming a continuous phase.
[0164] The morphology (phase structure) of the polyolefin elastomer component (D) and components other than the polyolefin elastomer component (D) can be appropriately adjusted by the content of the polyolefin elastomer component (D) in the thermoplastic elastomer composition and the molding method (temperature, speed).
[0165] Here, it was found that when the content of polyolefin elastomer component (D) in the thermoplastic elastomer composition is about 30% by mass to about 45% by mass, the thermoplastic elastomer composition tends to have a co-continuous structure and the tear strength tends to decrease. Furthermore, it was found that when the content of polyolefin elastomer component (D) is within the above range, when a polystyrene resin is used as the thermoplastic resin or when the thermoplastic elastomer composition further contains a hydrogenated block copolymer component (E), the thermoplastic elastomer composition tends to have a co-continuous structure and the tear strength tends to increase.
[0166] The sea-island structure can be confirmed by the following method.
[0167] A transmission electron microscope (TEM) JEM-2100F (manufactured by JEOL Ltd.) is used to take a cross-sectional image of the thermoplastic elastomer composition (film), and the cross-sectional morphology of the thermoplastic elastomer composition (film) is observed from the obtained cross-sectional image. The thermoplastic elastomer composition molded into a sheet is cut into an appropriate size, embedded in a thermosetting epoxy resin, and then sliced to a thickness of 80 nm in a frozen state using a cryo-ultramicrotome EM UC7 / FC7 (manufactured by Leica Microsystems Inc.) to prepare ultrathin sections, which are used as observation samples. The sample is subjected to a gas-phase staining process using ruthenium tetroxide at room temperature (23°C) to perform an electronic staining process and to microscopic observation. Observations are performed at 23°C under ultra-high vacuum, at a magnification of 2000 times, with an observation field of view of 10.6 μm x 10.6 μm, and at a magnification of 5000 times, with an observation field of view of 4.25 μm x 4.25 μm.
[0168] Whether the structure is a sea-island structure or a co-continuous structure is determined by checking the film cross-section image taken with a TEM at a magnification of 2000x and a field of view of 10.6μm×10.6μm, and a structure in which 90% of the separated structures in the image reach both ends of the image is defined as a co-continuous structure. Whether the island structure is a fine dispersion is determined by checking the film cross-section image taken with a TEM at a magnification of 5000x and a field of view of 4.25μm×4.25μm, instead of the co-continuous structure according to the above criteria, and measuring the major axis length of the islands from a representative image of a 2μm square area using DigitalMicrograph software (Gatan), and an island length with an average of 1.5μm or less is defined as a fine dispersion.
[0169] The island phases constituting the sea-island structure preferably have a major axis of about 100 nm or more, or about 150 nm or more, or about 200 nm or more, and preferably about 5 μm or less, or about 3 μm or less, or about 1.5 μm or less. When the major axis of the island phase is about 100 nm or more and about 5 μm or less, the tear strength is improved.
[0170] The long axis of the above island phase can be confirmed in an image of the film cross section taken by TEM at a magnification of 5000 times and an observation field of view of 4.25 μm × 4.25 μm. From an image of a representative area of 2 μm square, the long axis length of the islands can be measured using DigitalMicrograph software (Gatan).
[0171] From the viewpoint of reducing anisotropy, the island phase constituting the sea-island structure preferably has an aspect ratio (major axis / minor axis) of about 3 or less, about 2.5 or less, or about 2 or less. The lower limit of the aspect ratio is preferably about 1.
[0172] When the polyolefin elastomer component (D) is an island phase, from the viewpoint of reducing anisotropy, the area ratio of the island phase in the sea-island structure is preferably about 10% or about 20% or about 30% to about 80% or about 70% or about 60%.
[0173] When the polyolefin elastomer component (D) is a sea phase, from the viewpoint of good tear strength and stress relaxation property, the area ratio of the sea phase in the sea-island structure is preferably about 10% or about 20% or about 30% to about 80% or about 70% or about 60%.
[0174] The ratio of the sea phase and the ratio of the island phase in the sea-island structure can be measured by confirming an image of a cross section of a film taken using a TEM at a magnification of 2000 times and an observation field size of 10.6 μm × 10.6 μm, and measuring the area ratio of the sea phase to the island phase.
[0175] The thermoplastic elastomer composition of the present invention preferably has a tear strength in an Elmendorf (MD) test of about 300 N or more, or about 500 N or more.
[0176] The stress relaxation (long term) of the thermoplastic elastomer composition of the present invention is preferably about 60% or more, or about 65% or more.
[0177] The tear strength and stress relaxation property (long term) in the Elmendorf (MD) test can be measured by the method described in the Examples.
[0178] The stress relaxation in a tensile test of the thermoplastic elastomer composition of the present invention is preferably about 27% or less, or about 25% or less.
[0179] The anisotropic stress relaxation property of the thermoplastic elastomer composition of the present invention is preferably about 2.0 times or less, or about 1.8 times or less.
[0180] The stress relaxation property in a tensile test and the anisotropic stress relaxation property can be measured by the method described in the Examples.
[0181] Use of the thermoplastic elastomer composition The thermoplastic elastomer composition of the present invention has good elastic recovery, tear strength at 25°C, and stress relaxation properties, and can reduce anisotropy. Therefore, in film and sheet applications, the composition can be suitably used as stretch films and sheets for sanitary material components and personal care material components, daily necessities such as diapers, industrial products, home appliances, food containers, packaging materials, medical products such as bandages, miscellaneous goods, sporting goods, and the like.
[0182] Depending on the application, tear strength at 32° C. and / or tear strength at 38° C. are required. Applications requiring tear strength at 32° C. include rubber components for swimsuits, swimming equipment such as goggles, industrial bungee cords, fishing lures, grip equipment for tennis and other sports, elastic films for disposable rubber gloves used in cold regions and inside freezers, and rubber bands for exercise.
[0183] Examples of means for improving the tear strength at 32°C include using a hydrogenated block copolymer in which the polymer block (b) in the hydrogenated block copolymer (A) contains only structural units derived from 1,3-butadiene; when a hydrogenated petroleum resin is used as the thermoplastic resin (B), appropriately adjusting the blending amount of the hydrogenated petroleum resin and oil [rubber softener (C)]; appropriately adjusting the content of polyolefin elastomer (D); and appropriately adjusting the content of structural units derived from ethylene contained in the polyolefin elastomer (D).
[0184] Applications requiring tear strength at 38°C include rubber components in clothing (rubber components in underwear, lingerie, shapewear, sportswear, and grip components), daily necessities such as sanitary products, condoms, adult toys, sports bandages, medical dressings, wound care, medical tourniquets, and medical aids such as for relieving lower back pain.
[0185] Examples of means for improving the tear strength at 38°C include appropriately adjusting the content of the polyolefin elastomer (D) and appropriately adjusting the content of structural units derived from ethylene contained in the polyolefin elastomer (D). EXAMPLES
[0186] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0187] In the following Examples and Comparative Examples, the physical properties of the hydrogenated block copolymer components (A) and (E) and the thermoplastic elastomer composition were evaluated by the following methods.
[0188] Measurement method of crystallization peak temperature and glass transition temperature Using a differential scanning calorimeter (DSC), the crystallization peak temperature was determined from the exothermic peak observed during the temperature drop process in the 2nd step described below, and the glass transition temperature was determined from the endothermic peak observed during the temperature rise process in the 3rd step described below.
[0189] Equipment: DSC6200 (Seiko Instruments Inc.) Heating rate: 10℃ / min Cooling rate: 10℃ / min Nitrogen flow rate: 40mL / min Temperature profile: 1st: 30℃ → 150℃ (held for 5 minutes) 2nd: 150℃ → -100℃ (held for 5 minutes) 3rd: -100℃ → 150℃
[0190] Methods for measuring hydrogenation rate, styrene content, amount of 1,4-bonds in polymer block (b), mass ratio of structural units derived from isoprene to structural units derived from butadiene, and amount of vinyl bonds in polymer block (y) Both are H-NMR 1The mass ratio of the 1,4-bonds in the polymer block (b) was measured using a block copolymer before hydrogenation, and the ratio of the peak area of the 1,4-bonds to the sum of the peak areas of the 1,2-bonds and 3,4-bonds and the peak area of the 1,4-bonds was calculated. The mass ratio of the structural units derived from isoprene and the structural units derived from butadiene was measured using a block copolymer before hydrogenation.
[0191] Equipment: JNM-Lambda 500 (manufactured by JEOL Ltd.) Solvent: deuterated chloroform Measurement temperature: 50℃
[0192] How to calculate weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) were determined by gel permeation chromatography (GPC) in terms of standard polystyrene.
[0193] Equipment: GPC-8020 (Tosoh Corporation) Solvent: Tetrahydrofuran Measurement temperature: 40℃ Flow rate: 1mL / min Injection volume: 150μL, concentration: 5mg / 10cc (hydrogenated block copolymer / THF)
[0194] Morphology For the thermoplastic elastomer compositions (films) obtained in Examples 3, 5, 6, and 8, a transmission electron microscope (TEM) JEM-2100F (manufactured by JEOL Ltd.) was used to take cross-sectional images of the thermoplastic elastomer compositions (films), and the morphology of the cross-section of the film was observed from the cross-sectional images obtained. The thermoplastic elastomer compositions molded into sheets were cut into appropriate sizes and embedded in thermosetting epoxy resin, and then sliced to a thickness of 80 nm in a frozen state using a cryo-ultramicrotome EM UC7 / FC7 (manufactured by Leica Microsystems, Inc.) to prepare ultrathin sections, which were used as observation samples. The samples were subjected to gas-phase staining treatment using ruthenium tetroxide at room temperature (23°C) and subjected to electronic staining treatment and microscopic observation. The observations were performed at 23° C. under ultra-high vacuum at a magnification of 2000 times and a visual field of 10.6 μm×10.6 μm, and at a magnification of 5000 times and a visual field of 4.25 μm×4.25 μm.
[0195] 1 to 8 are morphology images obtained by observing cross-sectional images of a thermoplastic elastomer composition (film) cut along the machine direction (MD) during film production using a transmission electron microscope.
[0196] In Figures 1 to 8, the light colored areas correspond to the polyolefin elastomer component (D), and the dark colored areas correspond to resin components other than the polyolefin elastomer component (D). The dark colored areas are stained by structures having double bonds, specifically, hydrogenated block copolymer component (A), hydrogenated block copolymer component (E), Styrolution PS3190, and Kristalex (trademark) 5140. The morphology was measured and evaluated by analyzing the lengths of the long and short axis directions of the island phases within each photographed size using DigitalMicrograph software (Gatan) according to the evaluation criteria described below.
[0197] Tear resistance (slow) (1) Tear resistance at 25°C The thermoplastic elastomer composition (TD direction) molded into a sheet was cut into 50.8 mm x 25.4 mm using a die according to ASTM D882 to prepare test specimens (6 pieces). The thickness of each test specimen was measured and recorded in mils. Then, a mark was made in the center of each test specimen, and a 2 mm cut was made on the edge of the test specimen. The test specimen was inserted into a pneumatic film grip (1 / 2 inch pad with 1 inch line grip) of an Instron 5567 (Instron Corporation) equipped with Bluehill 3 software and a 100 N load cell, the measurement temperature was set to 25°C, and then the test specimen was stretched to 175% elongation at 250 mm / min with a crosshead, and held for 1 hour unless the test specimen was torn or broken. The number of test specimens that did not tear in two after holding for 1 hour was taken as the result of tear resistance at 25°C. A test specimen that did not tear in two or more was considered to pass.
[0198] (2) Tear resistance at 32°C Two test pieces were prepared in the same manner as in the test for tear resistance at 25°C. The test piece was inserted into a pneumatic film grip (1 / 2 inch pad with 1 inch line grip) of an Instron 5567 (Instron) equipped with Bluehill 3 software and a 100N load cell, the measurement temperature was set to 32°C, and the test piece was then stretched to 150% elongation at 250 mm / min with a crosshead, and held for 10 hours unless the test piece was torn or broken. After holding for 10 hours, the time required for the test piece to be pulled and torn in two was measured, and the average value was taken as the result of tear resistance at 32°C.
[0199] (3) Tear resistance at 38°C The tear resistance at 38°C was measured in the same manner as in (2) above, except that in the test for tear resistance at 32°C, the measurement temperature was changed to 38°C.
[0200] Elmendorf (MD) Examination The following tests were carried out in accordance with ASTM D1922.
[0201] The thermoplastic elastomer composition (MD direction) molded into a sheet was used to prepare slit test pieces (10 pieces) in accordance with ASTM D1922 using a die. The thickness (μm) of each test piece was measured, and the mass (g) of each test piece was obtained. The test piece was fixed to the test location of an Elmendorf Tearing Tester (Thwing-Albert), the test button was pressed to insert a pendulum, and the test piece was torn using a 1600g weight, and the results were recorded in gf. As a result of the test, the number of test pieces that could not be torn was recorded, and the average tear strength of the torn test pieces was calculated and recorded.
[0202] Stress relaxation (long term) The thermoplastic elastomer composition molded into a sheet (TD direction) was cut into test specimens using a die to a size of 50.8 mm x 25.4 mm according to ASTM D882. The thickness of the test specimens was measured and recorded in mils. The test specimens were used to perform tests using an Instron 5567 (Instron) equipped with Bluehill 3 software and a 100 N load cell according to the following procedure, and the stress relaxation property was calculated using the following formula.
[0203] (1) A test piece was set in an Instron 5567 and stretched to 500% elongation at 250 mm / min, and then returned to 0% elongation.
[0204] (2) The bottom film grip was released to allow the specimen to relax for 30 seconds, and then the bottom film grip was closed again.
[0205] (3) The test piece was stretched at 250 mm / min to 50% elongation and held for 10 hours.
[0206] Stress relaxation (%) = tensile strength (MPa) after 50% elongation and 10 hours / tensile strength (MPa) immediately after 50% elongation × 100
[0207] Tensile Test (TD) The thermoplastic elastomer composition (TD direction) molded into a sheet was cut into 50.8 mm x 25.4 mm using a die according to ASTM D882 to prepare test specimens (6 pieces). The thickness (inches) at the center of each test specimen was measured. The test specimen was inserted into the pneumatic grip of an Instron 5567 (Instron) equipped with Bluehill 3 software and a 100 N load cell, and the test specimen was stretched at 250 mm / min until it reached 200% elongation at the crosshead, held at 200% elongation for 30 seconds, and then returned to 0% elongation in 60 seconds, and the stress relaxation property was calculated according to the following formula. The 100 N load cell was used with a pneumatic film grip, which had a 12.7 mm x 25.4 mm grip on one side and a 25.4 mm line grip on the other side.
[0208] Stress relaxation (%) = [tensile strength (MPa) immediately after 200% elongation - tensile strength (MPa) after 200% elongation and holding for 30 seconds] / tensile strength (MPa) immediately after 200% elongation × 100
[0209] anisotropy The thermoplastic elastomer composition molded into a sheet (MD) was cut into 50.8 mm x 25.4 mm using a die according to ASTM D882 to prepare test specimens (6 pieces). The thickness (inches) at the center of each test specimen was measured. The test specimens were tested according to the procedure described in the tensile test (TD) above using an Instron 5567 (Instron) equipped with Bluehill 3 software and a 100 N load cell, and the stress relaxation in the MD direction was calculated. The ratio (F2 / F1) between the stress relaxation in the TD direction (F1) calculated in the tensile test (TD) above and the stress relaxation in the MD direction (F2) was calculated, and this was taken as the anisotropic stress relaxation.
[0210] Production Example 1: Production of hydrogenated block copolymer (A1) A pressure vessel that had been purged with nitrogen and dried was charged with 3,000 mL of cyclohexane as a solvent and 9.2 mL of 10.5 wt % sec-butyllithium (cyclohexane solution) as an initiator, and the temperature was raised to 60°C. Then, 100 mL of styrene was added and the solution was polymerized for 60 minutes.
[0211] Then, at the same temperature, 4.3 mL of isoprene and 5.7 mL of butadiene were added simultaneously, and the reaction was repeated for 3.8 min by adding equal amounts of isoprene and butadiene in one go, one after the other. Finally, 265 mL of isoprene and 360 mL of butadiene were added, after which the reaction was continued for another 90 min.
[0212] Further, 100 mL of styrene was added at the same temperature and polymerization was carried out for 60 minutes, after which the polymerization was terminated with 0.52 mL of methanol to obtain a reaction liquid containing a polystyrene-poly(isoprene / butadiene)-polystyrene triblock copolymer.
[0213] To this reaction liquid, 29.3 g of palladium carbon (palladium loading: 5 wt%) was added as a hydrogenation catalyst, and hydrogenation reaction was carried out at 150°C and a hydrogen pressure of 2 MPa for 10 hours. After cooling and depressurization, the palladium carbon was removed by filtration, and the filtrate was concentrated and vacuum dried to obtain a hydrogenated product of polystyrene-poly(isoprene / butadiene)-polystyrene triblock copolymer (hereinafter referred to as hydrogenated block copolymer (A1)). The physical properties of the obtained hydrogenated block copolymer (A1) were evaluated according to the above-mentioned method. The results are shown in Table 1.
[0214] Production Example 2: Production of hydrogenated block copolymer (A2) In a nitrogen-purged, dried pressure vessel, 50 kg of cyclohexane as a solvent and 147 g (equivalent to 15.4 g of sec-butyl lithium) of 10.5% by mass cyclohexane solution as an anionic polymerization initiator were charged, and 128 g of tetrahydrofuran was charged as a Lewis base. After heating to 50°C, 2.42 kg of styrene (1) was added and polymerized for 1 hour, followed by adding 10.76 kg of butadiene at 40°C and polymerizing for 2 hours, and then heating to 50°C, 2.42 kg of styrene (2) was added and polymerized for 1 hour to obtain a reaction liquid containing a polystyrene-polybutadiene-polystyrene triblock copolymer.
[0215] Palladium carbon (palladium loading: 5% by mass) was added as a hydrogenation catalyst to this reaction liquid in an amount of 5% by mass relative to the block copolymer, and the reaction was carried out at 150° C. and a hydrogen pressure of 2 MPa for 10 hours.
[0216] After cooling and depressurization, the palladium carbon was removed by filtration, the filtrate was concentrated and further dried in vacuum to obtain a hydrogenated polystyrene-polybutadiene-polystyrene triblock copolymer (hereinafter referred to as hydrogenated block copolymer (A2)). The physical properties of the obtained hydrogenated block copolymer (A2) were evaluated according to the above-mentioned method. The results are shown in Table 1.
[0217] Production Example 3: Production of hydrogenated block copolymer (E) In a nitrogen-purged, dried pressure vessel, 50 kg of cyclohexane as a solvent and 76 g of sec-butyllithium (10.5 wt % cyclohexane solution) (equivalent to 8.0 g of sec-butyllithium) as an anionic polymerization initiator were charged, and 310 g of tetrahydrofuran was charged as a Lewis base. After heating to 50°C, 0.5 kg of styrene (1) was added and polymerized for 1 hour, followed by adding a mixture of 8.2 kg of isoprene and 6.5 kg of butadiene [isoprene / butadiene (mass ratio) = 55 / 45] at 40°C and polymerizing for 2 hours, and then adding 1.5 kg of styrene (2) and polymerizing for 1 hour to obtain a reaction liquid containing a polystyrene-poly(isoprene / butadiene)-polystyrene triblock copolymer.
[0218] Palladium carbon (palladium loading: 5% by mass) was added as a hydrogenation catalyst to this reaction liquid in an amount of 5% by mass relative to the block copolymer, and the reaction was carried out at 150° C. and a hydrogen pressure of 2 MPa for 10 hours.
[0219] After cooling and depressurization, the palladium carbon was removed by filtration, the filtrate was concentrated and further vacuum dried to obtain a hydrogenated polystyrene-poly(isoprene / butadiene)-polystyrene triblock copolymer (hereinafter referred to as hydrogenated block copolymer (E)). The physical properties of the obtained hydrogenated block copolymer (E) were evaluated according to the above-mentioned method. The results are shown in Table 1.
[0220] [Table 1]
[0221] Examples 1 to 32 and Comparative Examples 1 to 5 A 27 mm Leistritz twin screw extruder equipped with an extended mixing section set at a temperature of T1° C. was used to premix the ingredients of the types and amounts listed in Tables 2A, 2B, 2C, and 2D, and then a film of the thermoplastic elastomer composition was obtained using a Thermo Fisher 20 mm single screw machine set at a temperature of T2° C. The results of measuring the physical properties of the resulting thermoplastic elastomer composition are shown in Tables 2A, 2B, 2C, and 2D.
[0222] Details of each of the components listed in Tables 2A, 2B, 2C, and 2D used in preparing the thermoplastic elastomer compositions are as follows:
[0223] Hydrogenated block copolymer component (A): Hydrogenated block copolymer (A1) (Production Example 1) Hydrogenated block copolymer (A2) (Production Example 2)
[0224] Thermoplastic resin component (B): Hydrocarbon resin (hydrogenated petroleum resin): Regalite® R1125 (EASTMAN Chemical Company) Polypropylene - P4C5B-030 (Flint Hills Resources) High molecular weight polystyrene resin - Styrolution PS3190 (INEOS Styrolution America LLC) (Mw - 250,000) Low molecular weight polystyrene resin - Kristalex™ 5140 (EASTMAN Chemical Company) (Mw - 4,900, Mz - 9,800, Tg - 90°C) Low molecular weight polystyrene resin - Piccotex™ 120 (EASTMAN Chemical Company) (Mw - 4,100, Mz - 7,200, Tg - 70°C) Low molecular weight polystyrene resin - Piccotex™ 100 (EASTMAN Chemical Company) (Mw - 2,400, Mz - 4,100, Tg - 50°C) Low molecular weight polystyrene resin - Kristalex™ 3100 (EASTMAN Chemical Company) (Mw - 1,500, Mz - 2,500, Tg - 51°C)
[0225] Rubber softener component (C): Oil: Krystol (trademark) 550 (Petro-Canada Lubricants LLC) (Kinematic viscosity at 40°C: 105 mm 2 / s) Oil: Renoil 1700W (Renkert Oil) (Kinematic viscosity at 40°C: 307.7 mm 2 / s)
[0226] Polyolefin elastomer component (D): Polyolefin elastomer - Vistamaxx(TM) 6102 (ExxonMobil) (Structural units derived from ethylene: 16% by mass) Polyolefin elastomer - Vistamaxx(TM) 3020FL (ExxonMobil) (Structural units derived from ethylene: 11% by mass)
[0227] Hydrogenated block copolymer component (E) Hydrogenated Block Copolymer (E) (Production Example 3)
[0228] [Table 2]
[0229] [Table 3]
[0230] [Table 4]
[0231] [Table 5]
[0232] In Examples 1 to 32, which use thermoplastic elastomer compositions containing hydrogenated block copolymer (A), thermoplastic resin (B), rubber softener (C), and polyolefin elastomer (D) each satisfying a specific condition, the anisotropic stress relaxation is as low as 2.0 times or less, and it is understood that the anisotropy is reduced. Each of the thermoplastic elastomer compositions of Examples 1 to 32 fully meets the tear strength, stress relaxation property, and tensile strength required for applications such as films and sheets. Furthermore, the thermoplastic elastomer compositions of Examples 8, 13, 15, 18, 23, and 24 have improved tear strength at 32°C, and the thermoplastic elastomer compositions of Examples 5, 22, and 25 to 32 have improved tear strength at 32°C and tear strength at 38°C.
[0233] From the cross-sectional images of the thermoplastic elastomer composition (film) of Example 6 shown in Figures 1 and 2 and the cross-sectional images of the thermoplastic elastomer composition (film) of Example 8 shown in Figures 3 and 4, it can be seen that the thermoplastic elastomer compositions (films) of Examples 6 and 8 both contain fine dispersions of polyolefin elastomer (D) and components other than the polyolefin elastomer (D), and have excellent tear strength.
[0234] From the cross-sectional images of the thermoplastic elastomer composition (film) of Example 5 shown in Figures 5 and 6, it can be seen that the thermoplastic elastomer composition (film) of Example 5 has excellent tear strength because the polyolefin elastomer (D) is the sea phase and the components other than the polyolefin elastomer (D) are the island phase. Furthermore, in the cross-sectional image of the film in Figure 5, the observation field was confirmed with a shooting size of 10.6 μm × 10.6 μm, and it was found that the proportion of the sea phase was 59.2%. Furthermore, in the cross-sectional image of the film in Figure 5, the observation field was confirmed with a shooting size of 4.25 μm × 4.25 μm, and from the image of a representative 2 μm square range, the long axis length and short axis length of the islands were measured using DigitalMicrograph (Gatan Co., Ltd.), and the long axis of the island phase was 1.8 μm, the short axis of the island phase was 0.23 μm, and the aspect ratio (long axis / short axis) was 8.
[0235] From the cross-sectional images of the thermoplastic elastomer composition (film) of Example 3 shown in Figures 7 and 8, it can be seen that in the thermoplastic elastomer composition (film) of Example 3, the polyolefin elastomer (D) and components other than the polyolefin elastomer (D) form a co-continuous structure. [Explanation of symbols]
[0236] 1. Polyolefin elastomer component (D) 2. Components other than polyolefin elastomer component (D)
Claims
1. A thermoplastic elastomer composition comprising a hydrogenated block copolymer component (A), a thermoplastic resin component (B), and a rubber softener component (C), (1) The hydrogenated block copolymer component (A) is (i) Two or more polymer blocks (a) containing structural units derived from an aromatic vinyl compound, and one or more polymer blocks (b) containing structural units derived from isoprene and / or 1,3-butadiene, wherein the aromatic vinyl compound is styrene; The polymer block (b) contains structural units derived from isoprene and structural units derived from 1,3-butadiene, or contains only structural units derived from 1,3-butadiene, (ii) having a glass transition temperature (measured as shown in the examples) of from -65°C to less than -45°C; and (iii) having a crystallization peak temperature (Tc) of -3°C to 15°C (measured as shown in the examples); Hydrogenated block copolymers are included, (2) The thermoplastic resin component (B) is at least one selected from a polystyrene-based resin, a polyethylene-based resin, a polypropylene-based resin, a petroleum resin, and a hydrogenated petroleum resin; (3) The thermoplastic elastomer composition further comprises a polyolefin elastomer component (D), the polyolefin elastomer component (D) comprises a polypropylene-based elastomer containing a structural unit derived from ethylene, and the content of the structural unit derived from ethylene is 13.0% by mass to 15.9% by mass based on the total mass of the polypropylene-based elastomer, and (4) The thermoplastic elastomer composition contains, per 100 parts by mass of (A)+(B)+(C)+(D), 18 to 60 parts by mass of a hydrogenated block copolymer component (A), 3 to 24 parts by mass of a thermoplastic resin component (B), 3 to 25 parts by mass of a rubber softener component (C), and 5 to 76 parts by mass of a polyolefin elastomer component (D). Thermoplastic elastomer composition.
2. The thermoplastic elastomer composition according to claim 1, which has a sea-island structure of a sea phase and an island phase, wherein the sea phase is one of (i) the polyolefin elastomer (D) or (ii) a component other than the polyolefin elastomer (D), the island phase is the other of (i) or (ii), and the island phase includes a plurality of islands having an average major axis of 100 nm or more and 5 μm or less (measured as shown in the examples).
3. The thermoplastic elastomer composition according to claim 2, wherein the island phase comprises islands having, on average, a major axis of 100 nm to 5 μm and an aspect ratio (major axis / minor axis) of 1 to 3 (measured as shown in the examples).
4. The thermoplastic elastomer composition according to any one of claims 1 to 3, wherein the polymer block (b) of the hydrogenated block copolymer contains a structural unit derived from isoprene and a structural unit derived from 1,3-butadiene.
5. The thermoplastic elastomer composition according to claim 4, wherein a mass ratio of the structural units derived from isoprene to the structural units derived from 1,3-butadiene is 49.9 / 50.1 to 40.1 / 59.
9.
6. The thermoplastic elastomer composition according to any one of claims 1 to 3, wherein the polymer block (b) of the hydrogenated block copolymer (A) contains only structural units derived from 1,3-butadiene.
7. The thermoplastic elastomer composition according to any one of claims 1 to 6, wherein a content of the polymer block (a) in the hydrogenated block copolymer is 20 mass% to 34 mass% based on a total mass of the hydrogenated block copolymer.
8. The thermoplastic elastomer composition according to any one of claims 1 to 7, wherein the thermoplastic resin component (B) comprises a polystyrene-based resin.
9. 9. The thermoplastic elastomer composition according to claim 1, further comprising 3 to 15 parts by mass of a hydrogenated block copolymer component (E) based on a total mass of the thermoplastic elastomer composition, wherein the hydrogenated block copolymer component (E) comprises a hydrogenated block copolymer obtained by hydrogenating a polymer block (x) containing more than 70% by mass of a structural unit derived from an aromatic vinyl compound and a polymer block (y) containing 30% by mass or more of a structural unit derived from at least one selected from the group consisting of a conjugated diene compound and isobutylene, the hydrogenated block copolymer having a glass transition temperature (Tg) of -45°C to 30°C, and the polymer block (x) in the hydrogenated block copolymer is present in an amount of 4% by mass to 30% by mass based on the total mass of the hydrogenated block copolymer.
10. A film or sheet of the thermoplastic elastomer composition according to any one of claims 1 to 9.
Citation Information
Patent Citations
Rubber composition
JP1998168235A
Thermoplastic elastomer composition
JP2001220513A
Thermoplastic elastomer composition and production method thereof
JP2003003038A
Resin composition for powder molding
JP2004231817A
Thermoplastic elastomer composition
JP2011184503A