Steel

A steel material with controlled chromium distribution addresses seizure and enhances durability and fracture resistance in cold forged products by maintaining lubricating film adhesion, resulting in improved manufacturing outcomes.

JP7564439B2Active Publication Date: 2024-10-09NIPPON STEEL CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020208803
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-16
Publication Date
2024-10-09
Estimated Expiration
2040-12-16

AI Technical Summary

Technical Problem

Cold forged products, particularly bolts, experience increased surface roughness due to seizure during the manufacturing process, which is exacerbated by the lack of a lubricating film, and they also face challenges in achieving high durability ratios and delayed fracture resistance, especially in hydrogen-generating environments.

Method used

A steel material with a specific chemical composition and controlled distribution of solid solution chromium concentration, ranging from 0.20 to 0.60 times the average concentration, is used to enhance seizure resistance and improve the durability ratio and delayed fracture resistance by maintaining an appropriate lubricating film adhesion during cold forging.

Benefits of technology

The steel material exhibits excellent seizure resistance, high durability ratio, and enhanced delayed fracture resistance, ensuring smooth surfaces and improved product integrity in cold forged products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564439000003
    Figure 0007564439000003
  • Figure 0007564439000001
    Figure 0007564439000001
  • Figure 0007564439000002
    Figure 0007564439000002
Patent Text Reader

Abstract

To provide a steel material that is excellent in seizure resistance during being cold-forged after a lubrication film is formed on the steel material and has high endurance ratio and excellent delayed fracture resistance.SOLUTION: A steel material is provided which has a chemical composition comprised of by mass%: 0.10 to 0.40% of C; 0.40% or less of Si; 0.76 to 1.30% of Mn; 0.030% or less of P; 0.040% or less of S; 0.05 to 1.20% of Cr; 0.005 to 0.100% of Al; 0.001 to 0.015% of N; 0.005 to 0.100% of Ti; 0.0003 to 0.0100% of B; 0.003 to 0.100% of Nb; and the balance consisting of Fe and impurities, and in the surface area of 31.25 mm range in the longitudinal direction of the steel material, when the first to 21st measurement points are specified in the longitudinal direction, and the solid solution Cr concentration at a position of 5 μm depth from the surface at each measurement point is measured, there are at least 5 types or more of solid solution Cr concentration satisfying the formula (1). 0.20≤([solid solution Crmax]-[solid solution Crmin]) / [Crbase]≤0.60 (1).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel material, and more particularly to a steel material that is used as a raw material for cold forged products. [Background technology]

[0002] Bolts used for fastening automobiles and buildings are formed by cold forging, which has a high yield rate and can reduce manufacturing costs. Recently, in order to further reduce manufacturing costs, finishing cutting of intermediate products after cold forging may be omitted in the manufacturing process of cold forged products. Cold forged products in which finishing cutting is omitted are required to have a smooth finished surface as is, as cold forged. In particular, the problem with cold forged products is that the surface roughness increases in areas with a high degree of cold working. The occurrence of excessively rough areas on the surface of such cold forged products is also called the occurrence of rough skin on the surface.

[0003] Specifically, a bolt, which is a cold forged product, is manufactured, for example, by the following manufacturing process, omitting finish cutting. A wire rod manufactured by hot rolling is prepared. The wire rod is pickled and descaled. A lubricating coating process is performed on the wire rod from which the scale has been removed, forming a lubricating coating on the surface of the wire rod. The wire rod with the lubricating coating formed thereon is subjected to wire drawing (cold drawing) to manufacture a steel wire. The steel wire is cold forged to manufacture an intermediate product in the shape of a bolt. The intermediate product is quenched and tempered to manufacture a bolt, which is a cold forged product.

[0004] In the above manufacturing process, wire rod on which a lubricating coating is formed is subjected to wire drawing to manufacture a steel wire. The lubricating coating remains on the surface of this steel wire. Cold forging is performed on the steel wire on which the lubricating coating is formed to manufacture an intermediate product in the shape of a bolt. However, if the lubricating coating on the surface of the steel wire is lacking or peeled off in the cold forging process, the steel wire and the die for cold forging come into direct contact without the lubricating coating during cold forging. In this case, friction between the steel wire and the die increases excessively, causing seizure. The occurrence of seizure causes roughness of the surface of the cold forged product. In particular, in the case of manufacturing bolts, the bearing surface of the bolt flange portion is highly cold worked during cold forging, making seizure more likely to occur. Therefore, in steel materials that undergo cold forging after a lubricating coating is formed, there is a demand for improved seizure resistance during cold forging.

[0005] Furthermore, recently, in order to improve the safety of automobiles and buildings, bolts with a high durability ratio (= fatigue strength / tensile strength) that can be used even under high fluctuating axial forces are also required. In order to increase the durability ratio of bolts, a method of increasing the content of alloy elements in the steel material used as the material can be considered. However, when a bolt with a high durability ratio is used in an environment where hydrogen is generated (hereinafter referred to as a hydrogen generation environment), delayed fracture due to hydrogen embrittlement may occur. Therefore, steel materials that are used as materials for cold forged products such as bolts are required to have a high durability ratio and excellent delayed fracture resistance when manufactured as cold forged products.

[0006] International Publication No. 2017 / 002770 (Patent Document 1) and Japanese Patent Application Laid-Open No. 2015-105428 (Patent Document 2) disclose cold forged products having high strength and excellent delayed fracture resistance.

[0007] The bolt disclosed in Patent Document 1 contains, in mass%, C: 0.32-0.39%, Si: 0.15% or less, Mn: 0.40-0.65%, P: 0.020% or less, S: 0.020% or less, Cr: 0.85-1.25%, Al: 0.005-0.060%, Ti: 0.010-0.050%, B: 0.0010-0.0030%, N: 0.0015-0.0080%, Mo: 0. The alloy contains C: 0-0.05%, V: 0-0.05%, Cu: 0-0.50%, Ni: 0-0.30%, and Nb: 0-0.05%, with the balance being Fe and impurities, and has a chemical composition that satisfies 4.9≦10C+Si+2Mn+Cr+4Mo+5V≦6.1 and Mn / Cr≦0.55, has a tensile strength of 1000-1300 MPa, and satisfies [solute Cr] / Cr≧0.70.

[0008] The bolt disclosed in Patent Document 1 suppresses the formation of Cr carbonitrides and increases the amount of solute Cr by lowering the Mn / Cr ratio and not carrying out heat treatment for softening before wire drawing and cold forging, or, even if heat treatment is carried out, by limiting the holding time of the steel material at 700°C or higher to less than 40 minutes. Patent Document 1 states that this makes it possible to increase the strength against hydrogen embrittlement of the tempered martensite, which is the microstructure of the bolt.

[0009] The steel material disclosed in Patent Document 2 contains, by weight, C: 0.20-0.35%, Si: 0.01% or more, Mn: 0.3-1.5%, P: 0.020% or less (excluding 0%), S: 0.020% or less (excluding 0%), Cr: 0.10-1.5%, Al: 0.01-0.10%, B: 0.0005-0.005%, and N: 0.001% or more, and further contains at least one of Ti: 0.02-0.10% and Nb: 0.02-0.10%, with the balance being iron and unavoidable impurities. Furthermore, when the B content of the steel surface is calculated assuming that the B content of the D0 / 4 part (D0 represents the diameter of the steel) of the steel is 100%, the percentage is 75% or less on average, the difference between the maximum and minimum values ​​of this percentage is 25% or less, and the prior austenite grain size number in the region from the steel surface to a depth of 100 μm is No. 8 or more. By deboronizing the surface of this steel, boron compounds that are the starting point of delayed fracture are reduced and the prior austenite grain size is refined. As a result, Patent Document 2 states that excellent delayed fracture resistance is obtained in cold forged products. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] International Publication No. 2017 / 002770 [Patent Document 2] JP 2015-105428 A Summary of the Invention [Problem to be solved by the invention]

[0011] However, Patent Documents 1 and 2 do not consider the seizure resistance of steel during cold forging after forming a lubricating coating on the steel surface in the manufacturing process of cold forged products using steel, which is the raw material for the cold forged products.

[0012] An object of the present disclosure is to provide a steel material that has excellent seizure resistance during cold forging after a lubricating coating is formed on the steel material surface in a manufacturing process, and that has a high durability ratio and excellent resistance to delayed fracture when made into a cold forged product. [Means for solving the problem]

[0013] The steel material of the present disclosure is Chemical composition, in mass%, C: 0.10-0.40%, Si: 0.40% or less, Mn: 0.76-1.30%, P: 0.030% or less, S: 0.040% or less, Cr: 0.05~1.20%, Al: 0.005 to 0.100%, N: 0.001 to 0.015%, Ti: 0.005 to 0.100%, B: 0.0003~0.0100%, Nb: 0.003 to 0.100%, and The balance is Fe and impurities. In a surface region of the steel material extending 31.25 mm in the longitudinal direction, a first measurement point is located at 0.23 mm from the end of the surface region, and second to twentieth measurement points are located at 1.56 mm intervals from the first measurement point in the longitudinal direction. A 21st measurement point is located at 31.02 mm from the end of the surface region in the longitudinal direction. When the solute Cr concentrations at a depth of 5 μm from the surface are measured at the first to 21st measurement points, there are at least five types of solute Cr concentrations measured, and the maximum solute Cr concentration among the solute Cr concentrations is defined as [Solute Cr max ] (mass%), and the minimum solute Cr concentration is [Solute Cr min ] (mass%), and the Cr concentration in the chemical composition of the steel is defined as [Cr base ] (mass%), formula (1) is satisfied. 0.20≦([Solid Cr max ]-[Solid Cr min ]) / [Cr base ]≦0.60 (1) Effect of the Invention

[0014] The steel material of the present disclosure has excellent seizure resistance during cold forging after forming a lubricating coating on the steel material surface in the manufacturing process. Furthermore, when a cold forged product is manufactured using the steel material of the present disclosure, the cold forged product has a high durability ratio and excellent delayed fracture resistance. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a plan view in the longitudinal direction of a steel material of this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present inventors have investigated steel materials that have excellent seizure resistance during cold forging after forming a lubricating coating on the surface of the steel material in the manufacturing process of cold forged products, and that have a high durability ratio and excellent resistance to delayed fracture when made into cold forged products.

[0017] The present inventors first investigated means for obtaining a high durability ratio and excellent delayed fracture resistance when a steel material is cold forged and heat treated to obtain a cold forged product, and as a result, the present inventors obtained the following findings.

[0018] Durability ratio is fatigue strength σ w is a value obtained by dividing by the tensile strength TS. The present inventors have investigated and examined the effect of chemical components on the durability ratio. The durability ratio of cold forged products decreases when (1) the amount of solute C in the steel is insufficient during quenching, (2) the hardenability of the steel is low and a sufficient amount of martensite structure cannot be obtained after quenching, and (3) the precipitation of alloy carbides during tempering is low. Therefore, it is effective to increase the solute C in the steel during quenching and to contain Mn and B, which increase the hardenability of the steel, and to contain Cr, which precipitates carbides during tempering. In particular, when the hardenability is insufficient, a significant decrease in the durability ratio occurs. Therefore, it is effective to add a sufficient amount of Mn, which has a high effect of improving hardenability.

[0019] The microstructure of the cold forged product is a tempered martensite structure. Delayed fracture in this structure occurs by the following mechanism. Hydrogen generated on the surface of the steel in a hydrogen generation environment penetrates into the steel. The penetrated hydrogen accumulates at the prior austenite grain boundaries in the stress concentration area in the steel. Intergranular cracking occurs due to the accumulated hydrogen, and this intergranular cracking corresponds to delayed fracture. The present inventor investigated and examined the effect of chemical components on delayed fracture. As a result, it was found that (4) suppressing the coarsening of prior austenite grain size and (5) reducing impurity elements segregating at grain boundaries are effective. Therefore, in this embodiment, nitrides of Al and carbides of Ti and Nb are generated to suppress the coarsening of prior austenite grains by the pinning effect. Furthermore, the content of impurity elements P and S is reduced.

[0020] Based on the above considerations from the viewpoint of chemical composition, the present inventors considered that a steel material having a chemical composition, in mass%, of C: 0.10-0.40%, Si: 0.40% or less, Mn: 0.76-1.30%, P: 0.030% or less, S: 0.040% or less, Cr: 0.05-1.20%, Al: 0.005-0.100%, N: 0.001-0.015%, Ti: 0.005-0.100%, B: 0.0003-0.0100%, Nb: 0.003-0.100%, Cu: 0-0.40%, Ni: 0-0.40%, Mo: 0-0.20%, and the balance being Fe and impurities, would increase the durability ratio of a cold forged product after cold forging and heat treatment (quenching and tempering), and would have excellent delayed fracture resistance.

[0021] However, in the case of steel having the above-mentioned chemical composition, in the manufacturing process of cold forged products, the steel may have low seizure resistance during cold forging after forming a lubricating film on the steel surface. Therefore, the present inventors have investigated the seizure resistance of steel during cold forging after forming a lubricating film. As a result, the following findings have been obtained.

[0022] The seizure phenomenon occurs when the steel surface and the die for cold forging come into direct contact with each other due to the lack or peeling of the lubricating film, resulting in wear. On the other hand, seizure does not occur as long as the lubricating film is stably held between the steel surface and the die. If the variation in the solute Cr concentration at a depth of 5 μm from the steel surface in the longitudinal direction of the steel is large, the steel surface can have a surface property with high affinity with the lubricating film. As a result, the adhesion of the lubricating film on the steel surface can be increased, and seizure resistance during cold forging can be suppressed. On the other hand, if the variation in the solute Cr concentration in the longitudinal direction of the steel is too large, the adhesion of the lubricating film on the steel surface becomes excessively high. In this case, the lubricating film cannot follow the deformation of the steel during cold forging, and the lubricating film is partially broken. As a result, a portion where the lubricating film is lacking occurs during cold forging, and seizure may occur.

[0023] Based on the above findings, the inventors considered that if the variation in the solute Cr concentration in the longitudinal direction of the steel surface could be adjusted to an appropriate range, the adhesion of the lubricating coating on the steel surface would be in an appropriate range, and the seizure resistance would be significantly improved during cold forging. Based on the above considerations, the distribution of the solute Cr concentration in the longitudinal direction of the steel surface having the above-mentioned chemical composition was examined. As a result, in a surface region of 31.25 mm in the longitudinal direction of the steel, a position 0.23 mm from the end of the surface region was set as the first measurement point, and the second to twentieth measurement points were specified at a pitch of 1.56 mm in the longitudinal direction from the first measurement point, and a position 31.02 mm in the longitudinal direction from the end of the surface region was specified as the 21st measurement point. When the solute Cr concentration was measured at a depth of 5 μm from the surface at the first to 21st measurement points, it was found that if the following conditions 1 and 2 are satisfied, the seizure resistance of the steel during cold forging after the formation of the lubricating coating is significantly improved. [Condition 1] There are at least five different solute Cr concentrations measured in the surface region, i.e., there are five or more different solute Cr concentrations. [Condition 2] The maximum solute Cr concentration among the measured solute Cr concentrations (21 solute Cr concentrations) is defined as [Solute Cr max ] (mass%). The minimum solute Cr concentration is defined as [Solute Cr min] (mass%). Furthermore, the Cr concentration in the chemical composition of the steel is defined as [Cr base In this case, the steel material of the present embodiment satisfies formula (1). 0.20≦([Solid Cr max ]-[Solid Cr min ]) / [Cr base ]≦0.60 (1)

[0024] The steel material of this embodiment has been completed based on the above technical concept, and has the following configuration.

[0025] [1] A steel material, Chemical composition, in mass%, C: 0.10-0.40%, Si: 0.40% or less, Mn: 0.76-1.30%, P: 0.030% or less, S: 0.040% or less, Cr: 0.05~1.20%, Al: 0.005 to 0.100%, N: 0.001 to 0.015%, Ti: 0.005 to 0.100%, B: 0.0003~0.0100%, Nb: 0.003 to 0.100%, and The balance is Fe and impurities. In a surface region of the steel material extending 31.25 mm in the longitudinal direction, a first measurement point is located at 0.23 mm from the end of the surface region, and second to twentieth measurement points are located at 1.56 mm intervals from the first measurement point in the longitudinal direction. A 21st measurement point is located at 31.02 mm from the end of the surface region in the longitudinal direction. When the solute Cr concentrations at a depth of 5 μm from the surface are measured at the first to 21st measurement points, there are at least five types of solute Cr concentrations measured, and the maximum solute Cr concentration among the solute Cr concentrations is defined as [Solute Cr max ] (mass%), and the minimum solute Cr concentration is [Solute Cr min ] (mass%), and the Cr concentration in the chemical composition of the steel is defined as [Crbase ] (mass%) satisfies formula (1), Steel material. 0.20≦([Solid Cr max ]-[Solid Cr min ]) / [Cr base ]≦0.60 (1)

[0026] [2] The steel material according to [1], The chemical composition further includes, in place of a portion of Fe, Cu: 0.40% or less, Ni: 0.40% or less, and Mo: 0.20% or less Contains one or more selected from the group consisting of Steel material.

[0027] Hereinafter, the steel material of this embodiment will be described in detail. In this specification, "%" relating to an element means mass % unless otherwise specified.

[0028] [Regarding the form of the steel material of this embodiment] The steel material of this embodiment may be a steel bar or a wire rod. The steel material of this embodiment may further be a steel wire. The steel material of this embodiment is suitable as a material for cold forged products. That is, the steel material of this embodiment is suitable for use in cold forged products.

[0029] The chemical composition of the steel material of this embodiment contains the following elements.

[0030] C: 0.10-0.40% Carbon (C) increases the durability ratio of the cold forged product manufactured using the steel material of this embodiment. If the C content is less than 0.10%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the C content exceeds 0.40%, the toughness of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the cold forging crack resistance of the steel material decreases. Therefore, the C content is 0.10 to 0.40%. The preferable lower limit of the C content is 0.11%, more preferably 0.12%, and more preferably 0.15%. The preferable upper limit of the C content is 0.39%, more preferably 0.38%, and more preferably 0.35%.

[0031] Si:0.40% or less Silicon (Si) is an impurity. If the Si content exceeds 0.40%, the toughness of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the cold forging crack resistance of the steel material decreases. Therefore, the Si content is 0.40% or less. The preferred upper limit of the Si content is 0.35%, more preferably 0.30%, more preferably 0.25%, and even more preferably 0.20%. The Si content is preferably as low as possible. However, excessive reduction of the Si content reduces productivity and increases manufacturing costs. Therefore, in consideration of normal industrial production, the preferred lower limit of the Si content is more than 0%, more preferably 0.01%, more preferably 0.02%, and even more preferably 0.03%.

[0032] Mn: 0.76 to 1.30% Manganese (Mn) deoxidizes steel. Mn also improves the hardenability of steel and increases its strength. Therefore, the durability ratio of a cold forged product manufactured using the steel of this embodiment is increased. If the Mn content is less than 0.76%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Mn content exceeds 1.30%, the toughness of the steel decreases and the cold forging crack resistance of the steel decreases even if the contents of other elements are within the range of this embodiment. Therefore, the Mn content is 0.76 to 1.30%. The preferred lower limit of the Mn content is 0.77%, more preferably 0.78%, and more preferably 0.80%. The preferred upper limit of the Mn content is 1.29%, more preferably 1.28%, and more preferably 1.25%.

[0033] P:0.030% or less Phosphorus (P) is an impurity. If the P content exceeds 0.030%, even if the contents of other elements are within the range of this embodiment, P will excessively segregate to the prior austenite grain boundaries, lowering the grain boundary strength. As a result, the delayed fracture resistance of the cold forged product manufactured using the steel material of this embodiment will decrease. Therefore, the P content is 0.030% or less. The preferred upper limit of the P content is 0.028%, more preferably 0.025%, and even more preferably 0.020%. The P content is preferably as low as possible. However, excessive reduction of the P content reduces productivity and increases manufacturing costs. Therefore, in consideration of normal industrial production, the preferred lower limit of the P content is more than 0%, more preferably 0.001%, more preferably 0.002%, and even more preferably 0.003%.

[0034] S: 0.040% or less Sulfur (S) is an impurity. If the S content exceeds 0.040%, even if the contents of other elements are within the range of this embodiment, S will excessively segregate to the prior austenite grain boundaries, lowering the grain boundary strength. As a result, the delayed fracture resistance of the cold forged product manufactured using the steel material of this embodiment will decrease. Therefore, the S content is 0.040% or less. The preferred upper limit of the S content is 0.035%, more preferably 0.030%, and even more preferably 0.020%. The S content is preferably as low as possible. However, excessive reduction of the S content reduces productivity and increases manufacturing costs. Therefore, in consideration of normal industrial production, the preferred lower limit of the S content is more than 0%, more preferably 0.001%, more preferably 0.002%, and even more preferably 0.003%.

[0035] Cr: 0.05~1.20% Chromium (Cr) enhances the adhesion between the steel surface and the lubricant (lubricating coating). As a result, in the manufacturing process of a cold forged product using the steel of this embodiment, the seizure resistance during cold forging is enhanced. Cr further enhances the hardenability of the steel, and enhances the durability ratio of the cold forged product manufactured using the steel of this embodiment. If the Cr content is less than 0.05%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Cr content exceeds 1.20%, the toughness of the steel decreases, and the cold forging crack resistance of the steel decreases, even if the contents of other elements are within the range of this embodiment. Therefore, the Cr content is 0.05 to 1.20%. The preferred lower limit of the Cr content is 0.10%, more preferably 0.20%, and more preferably 0.25%. The preferred upper limit of the Cr content is 1.15%, more preferably 1.10%, and more preferably 1.00%.

[0036] Al: 0.005 to 0.100% Aluminum (Al) deoxidizes steel. Furthermore, Al bonds with N to form Al nitrides. The Al nitrides exert a pinning effect to suppress the coarsening of austenite grains. As a result, the delayed fracture resistance of the cold forged product manufactured using the steel material of this embodiment is improved. If the Al content is less than 0.005%, the above effect cannot be sufficiently obtained. On the other hand, if the Al content exceeds 0.100%, coarse Al nitrides are generated even if the contents of other elements are within the range of this embodiment. The coarse Al nitrides become the starting point of fracture, so that the cold forging crack resistance of the steel material is reduced. Therefore, the Al content is 0.005 to 0.100%. The preferable lower limit of the Al content is 0.006%, more preferably 0.007%, and more preferably 0.008%. The preferable upper limit of the Al content is 0.090%, more preferably 0.080%, and more preferably 0.070%. In the chemical composition of the steel material of this embodiment, the Al content means the total Al content.

[0037] N: 0.001 to 0.015% Nitrogen (N) combines with Al, Ti, and B to form nitrides. These nitrides exert a pinning effect to suppress the coarsening of austenite grains. As a result, the delayed fracture resistance of the cold forged product manufactured using the steel material of this embodiment is improved. If the N content is less than 0.001%, the above effect cannot be sufficiently obtained. On the other hand, if the N content exceeds 0.015%, coarse nitrides are generated even if the contents of other elements are within the range of this embodiment. The coarse nitrides become the starting point of fracture, so that the cold forging crack resistance of the steel material is reduced. Therefore, the N content is 0.001 to 0.015%. The preferable lower limit of the N content is 0.002%, more preferably 0.003%, and more preferably 0.004%. The preferable upper limit of the N content is 0.014%, more preferably 0.013%, and more preferably 0.012%.

[0038] Ti: 0.005 to 0.100% Titanium (Ti) combines with N to form nitrides and inhibits solute B from becoming nitrides. This enhances the hardenability of the steel. Ti also forms carbides, nitrides, and carbonitrides, exerting a pinning effect and inhibiting coarsening of austenite grains. As a result, the delayed fracture resistance of the cold forged product manufactured using the steel of this embodiment is improved. If the Ti content is less than 0.005%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Ti content exceeds 0.100%, coarse nitrides are generated even if the contents of other elements are within the range of this embodiment. The coarse nitrides become the starting points of fracture, and the cold forging crack resistance of the steel is reduced. Therefore, the Ti content is 0.005 to 0.100%. The preferable lower limit of the Ti content is 0.006%, more preferably 0.007%, and even more preferably 0.008%. The upper limit of the Ti content is preferably 0.090%, more preferably 0.080%, and further preferably 0.070%.

[0039] B: 0.0003~0.0100% Boron (B) segregates at the austenite grain boundaries during quenching, improving the hardenability of the steel material. As a result, the durability ratio of the cold forged product manufactured using the steel material of this embodiment is improved. If the B content is less than 0.0003%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the B content exceeds 0.0100%, coarse nitrides are generated even if the contents of other elements are within the range of this embodiment. Since the coarse nitrides become the starting point of fracture, the cold forging crack resistance of the steel material decreases. Therefore, the B content is 0.0003 to 0.0100%. The preferred lower limit of the B content is 0.0004%, more preferably 0.0005%, and more preferably 0.0006%. The preferred upper limit of the B content is 0.0090%, more preferably 0.0080%, and more preferably 0.0070%.

[0040] Nb: 0.003 to 0.100% Niobium (Nb) combines with C to form carbides, exerts a pinning effect, and suppresses the coarsening of austenite grains. As a result, the delayed fracture resistance of the cold forged product manufactured using the steel material of this embodiment is improved. If the Nb content is less than 0.003%, the above effect cannot be sufficiently obtained. On the other hand, if the Nb content exceeds 0.100%, coarse carbides are generated even if the contents of other elements are within the range of this embodiment. The coarse carbides become the starting point of fracture, so that the cold forging crack resistance of the steel material is reduced. Therefore, the Nb content is 0.003 to 0.100%. The preferable lower limit of the Nb content is 0.004%, more preferably 0.005%, and more preferably 0.006%. The preferable upper limit of the Nb content is 0.090%, more preferably 0.080%, and more preferably 0.070%.

[0041] The balance of the chemical composition of the steel material of the present embodiment is composed of Fe and impurities. Here, the term "impurities" refers to substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of the steel material, and are permissible within a range that does not adversely affect the steel material of the present embodiment.

[0042] [About optional elements] The chemical composition of the steel material of the present embodiment may further contain one or more elements selected from the group consisting of Cu, Ni, and Mo, instead of a part of Fe. All of these elements are optional elements and may not be contained. When contained, all of these elements improve the hardenability of the steel material and increase the durability ratio of the cold forged product manufactured using the steel material of the embodiment.

[0043] Cu:0.40% or less Copper (Cu) is an optional element and may not be contained. That is, the Cu content may be 0%. When it is contained, that is, when the Cu content is more than 0%, Cu enhances the hardenability of the steel material and enhances the strength of the steel material. Therefore, the durability ratio of the cold forged product manufactured using the steel material of this embodiment is increased. If even a small amount of Cu is contained, the above effect can be obtained to a certain extent. However, if the Cu content exceeds 0.40%, even if the contents of other elements are within the range of this embodiment, high-hardness martensite may be generated in the steel material after hot rolling. In this case, the steel material may break during wire drawing. Therefore, the Cu content is 0.40% or less. That is, the Cu content is 0 to 0.40%, and when Cu is contained, it is more than 0 to 0.40%. That is, when it is contained, the Cu content is 0.40% or less. The preferable lower limit of the Cu content is 0.01%, more preferably 0.02%, and more preferably 0.03%. The upper limit of the Cu content is preferably 0.35%, more preferably 0.30%, further preferably 0.25%, and further preferably 0.20%.

[0044] Ni: 0.40% or less Nickel (Ni) is an optional element and may not be contained. That is, the Ni content may be 0%. When it is contained, that is, when the Ni content is more than 0%, Ni increases the hardenability of the steel material and increases the strength of the steel material. Therefore, the durability ratio of the cold forged product manufactured using the steel material of this embodiment is increased. If even a small amount of Ni is contained, the above effect can be obtained to a certain extent. However, if the Ni content exceeds 0.40%, even if the contents of other elements are within the range of this embodiment, high-hardness martensite may be generated in the steel material after hot rolling. In this case, the steel material may break during wire drawing. Therefore, the Ni content is 0.40% or less. That is, the Ni content is 0 to 0.40%, and when Ni is contained, it is more than 0 to 0.40%. That is, when it is contained, the Ni content is 0.40% or less. The preferable lower limit of the Ni content is 0.01%, more preferably 0.02%, and more preferably 0.03%. The upper limit of the Ni content is preferably 0.35%, more preferably 0.30%, further preferably 0.25%, and further preferably 0.20%.

[0045] Mo: 0.20% or less Molybdenum (Mo) is an optional element and may not be contained. That is, the Mo content may be 0%. When it is contained, that is, when the Mo content is more than 0%, Mo increases the hardenability of the steel material and increases the strength of the steel material. Mo further generates carbides and increases the strength of the steel material by precipitation strengthening. Therefore, the durability ratio of the cold forged product manufactured using the steel material of this embodiment is increased. If even a small amount of Mo is contained, the above effect can be obtained to a certain extent. However, if the Mo content exceeds 0.20%, high hardness martensite may be generated in the steel material after hot rolling even if the contents of other elements are within the range of this embodiment. In this case, the steel material may break during wire drawing. Therefore, the Mo content is 0.20% or less. That is, the Mo content is 0 to 0.20%, and when Mo is contained, it is more than 0 to 0.20%. That is, when Mo is contained, the Mo content is 0.20% or less. The lower limit of the Mo content is preferably 0.01%, more preferably 0.02%, and even more preferably 0.03%. The upper limit of the Mo content is preferably 0.18%, more preferably 0.16%, and even more preferably 0.14%.

[0046] [Method of measuring the chemical composition of steel] The chemical composition of the steel material of this embodiment can be measured by a known compositional analysis method. Specifically, a drill is used to generate chips from the R / 2 position of the steel material (the center position of the radius R in a cross section perpendicular to the longitudinal direction of the steel material), and the chips are collected. The collected chips are dissolved in acid to obtain a solution. ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry) is performed on the solution to perform elemental analysis of the chemical composition. The C content and S content are determined by a known high-frequency combustion method (combustion-infrared absorption method). The N content is determined by a known inert gas fusion-thermal conductivity method. The Cr concentration (mass%) obtained by the above measurement method is expressed as [Cr base ] is defined as

[0047] [Distribution of dissolved Cr concentration on steel surface] In this embodiment, the range of 31.25 mm in the longitudinal direction of the steel material is defined as the "surface region". Any region within the range of 31.25 mm in the longitudinal direction of the steel material may be selected as the "surface region". In the surface region, the Cr concentration distribution has a certain degree of variation. The Cr concentration distribution in the surface region is defined as follows.

[0048] FIG. 1 is a plan view of the steel material of this embodiment in the longitudinal direction. With reference to FIG. 1, an arbitrary range of 31.25 mm in the longitudinal direction of the surface of the steel material is defined as a surface region AR. A position 0.23 mm from an end P0 of the surface region AR in the longitudinal direction of the steel material is defined as a first measurement point P1. Then, a second measurement point P2 to a twentieth measurement point P20 are specified at a pitch of 1.56 mm in the longitudinal direction (the longitudinal direction on the opposite side to the end P0) from the first measurement point P1. Furthermore, a position 31.02 mm from the end P0 in the longitudinal direction (the longitudinal direction on the same side as P1 to P20) is defined as a 21st measurement point P21. A position 31.25 mm from the end P0 in the longitudinal direction (the longitudinal direction on the same side as P1 to P21) is defined as an end P22. The end P22 corresponds to the end of the surface region opposite to the end P0.

[0049] The dissolved Cr concentrations are measured at positions 5 μm deep from the surface at the first measurement point P1 to the twenty-first measurement point P21. At this time, the dissolved Cr concentrations measured satisfy the following conditions 1 and 2. [Condition 1] In the steel material of this embodiment, there are at least five different solute Cr concentrations measured in the surface region AR, i.e., there are five or more solute Cr concentrations with different values. [Condition 2] The maximum solute Cr concentration among the measured solute Cr concentrations (21 solute Cr concentrations) is defined as [Solute Cr max ] (mass%). The minimum solute Cr concentration is defined as [Solute Cr min ] (mass%). Furthermore, the Cr concentration in the chemical composition of the steel is defined as [Cr base In this case, the steel material of the present embodiment satisfies formula (1). 0.20≦([Solid Cr max ]-[Solid Cr min ]) / [Cr base]≦0.60 (1) Conditions 1 and 2 will be explained below.

[0050] [Regarding condition 1] When the number of solute Cr concentrations with different values ​​is less than 5 out of 21 solute Cr concentrations measured in the surface region, that is, when the number of solute Cr concentrations with different values ​​is 4 or less, the variation in Cr concentration on the surface of the steel material is small. In this case, the adhesion of the lubricant (lubricating film) decreases in the lubricating film treatment step before the wire drawing process. Therefore, in the steel material after the lubricating film treatment step and the wire drawing process, the lubricating film is likely to peel off, and seizure is likely to occur during the cold forging process. In other words, the seizure resistance of the steel material decreases.

[0051] If there are five or more solute Cr concentrations with different values ​​among the 21 solute Cr concentrations measured in the surface region, the adhesion of the lubricant (lubricating coating) can be improved in the lubricating coating treatment step before the wiredrawing step, provided that the content of each element in the chemical composition of the steel is within the range of this embodiment and condition 2 is satisfied. As a result, peeling of the lubricating coating can be suppressed in the steel after the lubricating coating treatment step and the wiredrawing step, and the seizure resistance of the steel during the cold forging step is improved.

[0052] The preferred lower limit of the number of types of solute Cr concentrations is 6, more preferably 7, and even more preferably 8. It is preferred that the number of types of solute Cr concentrations in the surface region AR is as large as possible. In other words, it is preferred that the number of solute Cr concentrations with different values ​​in the surface region AR is as large as possible, and it is preferred that the variation in the solute Cr concentrations in the surface region AR is as large as possible. However, if the number of types of solute Cr concentrations in the surface region AR is excessively large, the productivity will decrease significantly and the manufacturing costs will increase. Therefore, in consideration of normal industrial production, the preferred upper limit of the number of types of solute Cr concentrations (i.e., the number of solute Cr concentrations with different values) is 20, more preferably 19, and even more preferably 17.

[0053] [Regarding condition 2] F1=([solid solution Cr max]-[Solid Cr min ]) / [Cr base ] is defined as. F1 is an index showing the variation of the dissolved Cr concentration at the steel surface relative to the Cr concentration at the core of the steel. If F1 is less than 0.20, the variation of the dissolved Cr concentration at the steel surface is too small relative to the Cr concentration at the core of the steel. In this case, the adhesion of the lubricant (lubricating film) decreases in the lubricating film treatment process before the wire drawing process. Therefore, in the steel after the lubricating film treatment process and the wire drawing process, the lubricating film is easily peeled off, and seizure is easily generated during the cold forging process. In other words, the seizure resistance of the steel decreases.

[0054] On the other hand, if F1 exceeds 0.60, the variation in the dissolved Cr concentration at the steel surface is too large compared to the Cr concentration at the core of the steel. In this case, the adhesion of the lubricant (lubricating film) becomes excessively high in the lubricating film treatment process before the wire drawing process. As a result, during cold forging, the lubricating film cannot follow the deformation of the steel and part of the lubricating film breaks. In this case, an area where the lubricating film is deficient occurs on the steel surface during cold forging, and seizure occurs. In other words, the seizure resistance during the cold forging process is reduced in the steel on which the lubricating film is formed.

[0055] If F1 is 0.20 to 0.60, the adhesion of the lubricant (lubricating coating) can be improved in the lubricating coating treatment step before the wiredrawing step, provided that the content of each element in the chemical composition of the steel falls within the range of this embodiment and condition 1 is satisfied. As a result, peeling of the lubricating coating can be suppressed in the steel after the lubricating coating treatment step and the wiredrawing step, and the seizure resistance of the steel during the cold forging step is improved.

[0056] The lower limit of F1 is preferably 0.22, more preferably 0.24, and even more preferably 0.30. The upper limit of F1 is preferably 0.58, more preferably 0.54, and even more preferably 0.50.

[0057] [Method for measuring the dissolved Cr concentration at each measurement point P1 to P21 in the surface region AR] The solute Cr concentration at each of the measurement points P1 to P21 in the surface region AR can be measured by the following method. X-ray photoelectron spectroscopy is used for the measurement. A sample including the surface region AR of the steel material is taken. The surface region AR of the taken sample is sputtered to a depth of 5 μm with an argon ion gun with an accelerating voltage of 4 kV. Each of the measurement points P1 to P21 in the surface region AR after sputtering (i.e., each of the measurement points P1 to P21 at a depth of 5 μm from the surface) is irradiated with X-rays with a beam diameter of 50 μm. The solute Cr concentration is quantified based on the kinetic energy and intensity of the photoelectrons obtained from each of the measurement points P1 to P21.

[0058] Among the 21 solute Cr concentrations measured, the number of different solute Cr concentrations (i.e., the types of solute Cr concentrations) was determined. In addition, the maximum solute Cr concentration among the measured solute Cr concentrations was defined as [Solute Cr max ] (mass%). The minimum solute Cr concentration is defined as [Solute Cr min ] (mass %) is defined as

[0059] [About the microstructure of steel] The microstructure of the steel material of this embodiment is not particularly limited. For example, the total area ratio of ferrite and pearlite in the microstructure of the steel material is 50.0% or more, with the remainder being bainite. For example, the total area ratio of ferrite and pearlite in the microstructure of the steel material of this embodiment may be 60.0% or more, 70.0% or more, or 80.0% or more. In the microstructure of the steel material, regions other than bainite, ferrite, and pearlite are, for example, retained austenite, precipitates (including cementite), and inclusions. The area ratios of the retained austenite, precipitates, and inclusions are negligibly small.

[0060] [Method for measuring the area ratio of ferrite and pearlite] The total area ratio (%) of ferrite and pearlite and the area ratio (%) of bainite in the microstructure of the steel material of this embodiment are measured by the following method. A sample is taken from the R / 2 position of the steel material in a cross section (hereinafter referred to as a cross section) perpendicular to the longitudinal direction (axial direction) of the steel material. Of the surfaces of the taken sample, the surface corresponding to the cross section is used as the observation surface. After mirror polishing the observation surface, the observation surface is etched using 2% nitric acid alcohol (Nital etching solution). The etched observation surface is observed using an optical microscope at 500x magnification to generate photographic images of 20 arbitrary fields of view. The size of each field of view is 100 μm×100 μm.

[0061] In each field of view, the contrast of each phase, such as ferrite, pearlite, and bainite, is different. Therefore, each phase is identified based on the contrast. Among the identified phases, the total area (μm 2 ), and the total area of ​​pearlite (μm 2 The ratio of the total area of ​​ferrite and the total area of ​​pearlite in all visual fields to the total area of ​​all visual fields is defined as the total area ratio of ferrite and pearlite (%). Using the total area ratio of ferrite and pearlite, the area ratio of bainite (%) is calculated using the following method. Bainite area ratio (%) = 100.0 - total area ratio of ferrite and pearlite (%) The total area ratio (%) of ferrite and pearlite is a value obtained by rounding off to one decimal place.

[0062] The steel material of this embodiment has a chemical composition in which the content of each element falls within the range of this embodiment, and the surface region satisfies conditions 1 and 2. Therefore, the steel material of this embodiment has excellent seizure resistance by maintaining the adhesion of the lubricating coating within an appropriate range in the manufacturing process of the cold forged product. Furthermore, when the steel material of this embodiment is cold forged and then quenched and tempered to manufacture a cold forged product, the cold forged product has a high durability yield ratio and excellent delayed fracture resistance.

[0063] [Steel manufacturing method] An example of a method for manufacturing the steel material of this embodiment will be described. Note that, as long as the steel material of this embodiment has the above configuration, the manufacturing method is not limited to the manufacturing method described below. However, the manufacturing method described below is a suitable example for manufacturing the steel material of this embodiment.

[0064] An example of the method for producing a steel material according to the present embodiment includes a material preparation step, a hot working step, a pickling step, and a wire drawing step. Each step will be described below.

[0065] [Material preparation process] In the material preparation step, a material is prepared in which the content of each element in the chemical composition falls within the range of this embodiment. The material is produced, for example, by the following method. Molten steel is produced in which the content of each element in the chemical composition falls within the range of this embodiment. The molten steel is used to produce a material (a slab or an ingot) by a casting method. For example, the molten steel is used to produce a slab (bloom) by a well-known continuous casting method. Or, the molten steel is used to produce an ingot by a well-known ingot-making method.

[0066] [Hot processing process] In the hot working step, the material (bloom or ingot) prepared in the material preparation step is subjected to hot working to produce an intermediate steel material. The shape of the intermediate steel material is not particularly limited. The intermediate steel material is, for example, a steel bar or a wire rod.

[0067] The hot working process includes a rough rolling process and a finish rolling process. In the rough rolling process, the material is hot rolled to produce a billet. For example, a blooming mill is used in the rough rolling process. The material is bloomed by the blooming mill to produce a billet. If a continuous rolling mill is installed downstream of the blooming mill, the billet after blooming may be further hot rolled by the continuous rolling mill to produce a billet of a smaller size. In the continuous rolling mill, a horizontal stand having a pair of horizontal rolls and a vertical stand having a pair of vertical rolls are alternately arranged in a row. Through the above steps, the material is produced into a billet in the rough rolling process. The heating temperature in the heating furnace in the rough rolling process is not particularly limited, but is, for example, 1100 to 1300°C.

[0068] In the finish rolling process, a billet is first heated using a heating furnace. The heated billet is then hot-rolled using a continuous rolling mill to produce an intermediate steel material (steel bar or wire rod). The heating temperature in the heating furnace in the finish rolling process is not particularly limited, but is, for example, 1000 to 1300°C.

[0069] The steel material after the finish rolling step is cooled (naturally cooled) to produce the intermediate steel material of this embodiment.

[0070] [Pickling process] In the pickling process, an intermediate steel material produced by the hot working process is subjected to pickling treatment. In the pickling process, the intermediate steel material (wire rod or steel bar) is immersed in acid to descale it. The conditions for the pickling may be well known conditions. The temperature of the pickling bath is 10 to 50°C, and the acid concentration of the pickling bath is 2 to 30%. The immersion time in the pickling bath (total immersion time) is 10 to 199 minutes. The pickling bath contains, for example, hydrochloric acid, but sulfuric acid may also be used.

[0071] The pickling process adjusts the Cr concentration distribution in the surface region of the steel material to satisfy conditions 1 and 2. Cr is less soluble in acid than Fe. Therefore, when the Fe in the intermediate steel material (base material) dissolves due to acid immersion, the dissolved Cr is concentrated partially on the steel material surface, and the dissolved Cr concentration in the surface region AR varies. The pickling process adjusts the variation in the dissolved Cr concentration so that the steel material after the wire drawing process satisfies conditions 1 and 2.

[0072] An example of a method for adjusting the variation in the dissolved Cr concentration on the steel surface during pickling treatment is as follows: Masking tape is attached to an intermediate steel material before pickling treatment as follows. (1) Prepare masking tape that is 1.0 to 4.9 mm wide. (2) Apply one piece of masking tape around the intermediate steel material, the same length as its circumference in the direction perpendicular to its longitudinal direction (the circumference of its cross section). (3) Next to the masking tape you have just applied, apply one piece of masking tape of the same length and width without any gaps or overlaps. (4) The above operation (3) is repeated to apply the masking tape continuously in the longitudinal direction of the intermediate steel material without any gaps or overlaps. Then, when the cumulative length of the masking tape in the longitudinal direction of the intermediate steel material reaches 20 mm, the masking tape in the portion exceeding 20 mm is removed. (5) (2) to (4) are repeated in 20 mm increments to apply masking tape to the entire length of the intermediate steel material. (6) In the longitudinal direction of the intermediate steel material, one piece of masking tape is peeled off in an area of ​​20 mm (hereinafter referred to as unit surface) and pickling treatment is performed. The masking tape to be peeled off is in the same position on each unit surface. (7) and (6) are repeated to carry out the acid washing process repeatedly until all the masking tape has been removed. The immersion time in each of the pickling treatments in (6) and (7) is not particularly limited, but is, for example, 1 to 5 minutes.

[0073] [Wire drawing process] In the wire drawing process, the intermediate steel material after the pickling process is subjected to cold wire drawing (cold drawing) to produce the steel material of this embodiment. The wire drawing process includes a lubricating coating process and a cold drawing process.

[0074] [Lubricant film formation process] In the lubricating coating forming process, a known lubricant is applied to the surface of the intermediate steel material after the pickling process to form a lubricating coating. The type of lubricant (lubricating coating) and the lubrication conditions are not particularly limited. Examples of the lubricant include zinc phosphate, lime soap, metal soap, and lubricants containing inorganic salts without added phosphorus and lubricants. In the lubricating coating forming process, the intermediate steel material is immersed in a lubricating bath containing a lubricant to form a lubricating coating on the surface of the intermediate steel material. The immersion time in the lubricating bath is not particularly limited, but is, for example, 1 minute to 30 minutes.

[0075] [Cold drawing process] In the cold drawing process, the intermediate steel material on which the lubricating film is formed is subjected to a known cold drawing process. The shape of the die and the area reduction rate in the cold drawing process are not particularly limited. The opening angle on the entry side of the die is, for example, 10 to 25°. The area reduction rate in the cold drawing process is, for example, 1 to 50%.

[0076] The above manufacturing process allows the steel material of this embodiment having the above configuration to be manufactured. Note that the above manufacturing method is one example. Therefore, as long as the steel material having the above configuration can be manufactured, the manufacturing method is not limited to the above method. However, the above manufacturing method is a suitable manufacturing method for the steel material of this embodiment.

[0077] The manufacturing method of the steel material of this embodiment may not include a wire drawing process. That is, the steel material of this embodiment may be manufactured by carrying out a material preparation process, a hot working process, and a pickling process. Therefore, the steel material of this embodiment may be a steel bar or wire, or may be a steel wire. When the steel material is manufactured without carrying out the wire drawing process, when manufacturing a cold forged product described later, the steel material is subjected to a wire drawing process, and then the manufacturing method of the cold forged product described later is carried out to manufacture the cold forged product.

[0078] [Manufacturing method of cold forged products] As an example of a method for manufacturing a cold forged product using the steel material of this embodiment, an example of a method for manufacturing a bolt will be described. The method for manufacturing a cold forged product includes a cold forging process and a heat treatment process. In addition, when the steel material of this embodiment is manufactured without performing a wire drawing process after the pickling process, the above-mentioned wire drawing process is performed on the steel material before the cold forging process. The cold forging process and the heat treatment process will be described below.

[0079] [Cold forging process] In the cold forging process of the bolt, a press forging machine is used to perform cold working (cold forging) on ​​the steel material to manufacture an intermediate product. In the cold forging process, the lubricating coating formed on the steel material in the wire drawing process is used as it is. The cold forging process includes, for example, a head forming process by upsetting, a shaft forming process by forward extrusion, and a thread forming process by rolling. All of these processes are well known. Among these processes, in the head forming process, seizure is likely to occur due to lack of the lubricating coating, especially on the seat surface of the flange part. However, in the steel material of this embodiment, the Cr concentration distribution on the surface is appropriate, so the adhesion of the lubricating coating is in an appropriate state. Therefore, seizure is unlikely to occur in the head forming process, and excellent seizure resistance is obtained. In the cold forging process when the cold forged product is a bolt, the expansion ratio of the flange part (the value obtained by dividing the diameter of the steel material after forging by the diameter of the intermediate product before forging) is, for example, 1.1 to 2.5. The forging speed in the cold forging step is, for example, 10 to 500 mm / sec.

[0080] [Heat treatment process] In the heat treatment process, the intermediate product after the cold forging process is subjected to well-known quenching and tempering treatments. In the quenching process, for example, the quenching temperature is 800 to 950°C, and the holding time at the quenching temperature is 10 to 60 minutes. After the holding time has elapsed, the intermediate product is quenched (oil cooled) in oil at 50 to 100°C. Specifically, the intermediate product is immersed in an oil bath at the above temperature until the temperature of the intermediate product is 200°C or less. In the tempering process, the tempering temperature is 400 to 600°C, and the holding time at the tempering temperature is 30 to 120 minutes. After the holding time has elapsed, the intermediate product is immersed in a water bath at 10 to 30°C to make the temperature of the intermediate product 50°C or less.

[0081] The cold forged product (bolt) is manufactured by the above manufacturing process. The cold forged product thus manufactured has a high durability ratio and excellent resistance to delayed fracture.

[0082] In the above description, a bolt has been described as an example of a cold forged product. However, the cold forged product using the steel material of the present embodiment is not limited to a bolt. The steel material of the present embodiment can be widely applied to cold forged products other than bolts. EXAMPLES

[0083] The effect of one aspect of the present invention will be explained more specifically with reference to examples. The conditions in the following examples are one example of conditions adopted to confirm the feasibility and effect of the steel material of this embodiment. Therefore, the present invention is not limited to this one example of conditions. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.

[0084] Molten steel having the chemical composition shown in Table 1 was produced.

[0085] [Table 1]

[0086] The "-" portion in Table 1 means that the content of the corresponding element was below the detection limit. In other words, it means that the content of the corresponding element was 0%. Specifically, in Test No. 1 in Table 1, it means that the Cu content was 0% when rounded off to the third decimal place, the Ni content was 0% when rounded off to the third decimal place, and the Mo content was 0% when rounded off to the third decimal place.

[0087] [Material preparation process and hot processing process] The molten steel was used to produce a bloom by continuous casting. After heating the bloom, it was subjected to a rough rolling process called blooming and then rolling by a continuous rolling mill to produce a billet with a cross section perpendicular to the longitudinal direction of 160 mm x 160 mm. The heating temperature in blooming was 1200°C.

[0088] The manufactured billet was used to carry out a finish rolling process to manufacture intermediate steel materials (wire materials) having a diameter of 15 mm. The heating temperature in the heating furnace for each test number in the finish rolling process was 1200° C. The intermediate steel materials after the finish rolling were allowed to cool.

[0089] [Pickling process] The intermediate steel material of each test number was cut into a length of 1000 mm to prepare an intermediate steel material test piece. The intermediate steel material test piece of each test number was subjected to the following pickling treatment. (1) Masking tape of the width (mm) shown in the "Masking width (mm)" column in Table 2 was prepared. (2) Masking tape was attached around the circumference of the intermediate steel test piece with the corresponding test number. (3) Next to the masking tape that had been applied, a piece of masking tape of the same length and width was applied around the area, without any gaps or overlaps. (4) The above operation (3) was repeated to apply the masking tape continuously in the longitudinal direction of the intermediate steel test piece without gaps or overlaps. Then, when the cumulative length of the masking tape in the longitudinal direction of the intermediate steel test piece reached 20 mm, the masking tape in the portion exceeding 20 mm was removed. (5) (2) to (4) were repeated 50 times in 20 mm increments, and masking tape was applied to the entire length of the intermediate steel test piece, 1,000 mm. (6) One piece of masking tape was peeled off from each 20 mm area (hereinafter referred to as unit surface) in the longitudinal direction of the intermediate steel test piece, and pickling treatment was performed. The masking tape to be peeled off was at the same position on each unit surface. In the pickling treatment, the entire length of the intermediate steel test piece was immersed in a 10% hydrochloric acid aqueous solution (pickling bath) maintained at 25°C. The immersion time was 1 minute or more. (7) and (6) were repeated to repeat pickling until all the masking tape was removed from the intermediate steel test pieces. The final immersion time in the pickling bath was set to 5 minutes, and the total immersion time in the pickling baths for all pickling treatments was defined as the total pickling time (minutes) (shown in the "Total pickling time (minutes)" column in Table 2).

[0090] [Table 2]

[0091] [Wire drawing process] The intermediate steel test pieces after the pickling process were immersed in a lime soap solution for 15 minutes to form a lime soap coating (lubricating coating) on ​​the surface of the intermediate steel test pieces. After the lubricating coating was formed, cold drawing was performed. The opening angle on the entry side of the die used for cold drawing was 15°. Cold drawing was performed on the intermediate steel test pieces with a diameter of 15 mm to produce steel material (steel wire) with a diameter of 12 mm. The reduction in area in cold drawing was 36%. The unit surface area (20 mm) of the masking tape became 31.25 mm after cold drawing.

[0092] Steel test pieces of each test number were manufactured by the above manufacturing process. The microstructure of each steel test piece was observed by the above method to measure the area ratio of ferrite and pearlite, and the area ratio of bainite. As a result, in each test number, the total area ratio of ferrite and pearlite was 80.0% or more, and the remainder was bainite.

[0093] [Manufacturing of cold forged products] The steel test pieces having the respective test numbers were subjected to the following cold forging process and heat treatment process to manufacture cold forged products.

[0094] [Cold forging process] The steel test pieces were cut to 100 mm. The bolt heads were upset using a press forging machine with a forging speed of 300 mm / sec to produce intermediate bolt-shaped products with a flange diameter of 18 mm (expansion ratio 1.5).

[0095] [Heat treatment process] The intermediate product was quenched and tempered. The quenching temperature was 860°C, and the holding time was 30 minutes. After the holding time had elapsed, the intermediate product was oil-cooled in oil at 50-100°C. The tempering temperature was 470°C, and the holding time was 60 minutes. After the holding time had elapsed, the intermediate product was immersed in a water bath at 10-30°C to reduce the temperature of the intermediate product to 50°C or less.

[0096] By the above manufacturing process, cold forged products (bolts) with each test number were manufactured.

[0097] The following evaluation tests were further carried out on the steel test pieces and cold forged products (bolts) of each test number.

[0098] [Evaluation test] [Steel chemical composition analysis test] The chemical composition of the steel test pieces of each test number was determined by the following method. Chips were generated from the R / 2 position of the steel (the center position of the radius R in the cross section perpendicular to the longitudinal direction of the steel) and the chips were collected. The collected chips were dissolved in acid to obtain a solution. ICP-AES was performed on the solution to perform elemental analysis of the chemical composition. The C content and S content were determined by the well-known high-frequency combustion method (combustion-infrared absorption method). The N content was determined by the well-known inert gas fusion-thermal conductivity method. As a result of the measurements, the chemical composition of the steel test pieces of each test number was as shown in Table 1. The Cr concentration (mass%) obtained by the above measurement method was calculated as [Cr base ] was defined as follows.

[0099] [Solute Cr concentration measurement test at each measurement point P1 to P21] In the steel test piece of each test number, as shown in FIG. 1, an arbitrary range of 31.25 mm in the longitudinal direction of the surface of the steel was defined as the surface region AR. A position 0.23 mm in the longitudinal direction from the end P0 of the surface region AR was defined as the first measurement point P1. The second measurement point P2 to the twentieth measurement point P20 were identified at a pitch of 1.56 mm in the longitudinal direction (the longitudinal direction opposite to the end P0) from the first measurement point P1. Furthermore, a position 31.02 mm in the longitudinal direction (the longitudinal direction on the same side as P1 to P20) from the end P0 was defined as the 21st measurement point P21. A position 31.25 mm in the longitudinal direction (the longitudinal direction on the same side as P1 to P21) from the end P0 was defined as the end P22. The end P22 corresponded to the end of the surface region opposite to the end P0.

[0100] The solute Cr concentration at each measurement point P1 to P21 in the surface region AR was measured by the following method. X-ray photoelectron spectroscopy was used for the measurement. A sample including the surface region AR of the steel material was taken. The surface region AR of the taken sample was sputtered to a depth of 5 μm with an argon ion gun with an acceleration voltage of 4 kV. Each measurement point P1 to P21 (i.e., each measurement point P1 to P21 at a depth of 5 μm from the surface) in the surface region AR after sputtering was irradiated with an X-ray having a line diameter of 50 μm. The solute Cr concentration was quantified based on the kinetic energy and intensity of the photoelectrons obtained from each measurement point P1 to P21. By the above method, the solute Cr concentration (mass%) at the measurement points P1 to P21 in the surface region AR of the steel test piece of each test number was measured. The value obtained by rounding off the 2nd decimal place of the Cr concentration at the measurement points P1 to P21 was taken as the Cr concentration (mass%) at the measurement points.

[0101] The number of different solute Cr concentrations (i.e., types of solute Cr concentrations) DN was calculated from the 21 solute Cr concentrations measured. The number DN is shown in Table 2. Furthermore, the maximum solute Cr concentration among the measured solute Cr concentrations was defined as [Solute Cr max ] (mass%). The minimum solute Cr concentration was defined as [Solute Cr min The obtained [Solute Cr] was defined as (mass%). max ] and [Solute Cr min ] are shown in Table 2.

[0102] [Seizure resistance evaluation test] 100 intermediate products were produced by cold forging the steel material of each test number. The surface roughness (arithmetic mean roughness Ra) of the flange seat surface of any 20 intermediate products among the intermediate products (100 products) after cold forging was measured at three locations at a 20° pitch in the radial direction using a roughness meter. The arithmetic mean value of the arithmetic mean roughness Ra of 3 locations x 20 products was defined as the arithmetic mean roughness Ra (μm) for that test number. The arithmetic mean roughness Ra was measured in accordance with JIS B 0601 (1994), the standard value of the cutoff value was 0.8 mm, and the evaluation length was 3.0 mm. Based on the obtained arithmetic mean roughness Ra, the seizure resistance was evaluated as follows. Grade A: Arithmetic mean roughness Ra is 1.00 μm or less Grade B: Arithmetic mean roughness Ra is more than 1.00 to 1.25 μm Rating C: Arithmetic mean roughness Ra is more than 1.25 to 1.50 μm Rating D: Arithmetic mean roughness Ra is more than 1.50 to 1.75 μm Rating X: Arithmetic mean roughness Ra exceeds 1.75 μm The steel materials were judged to have excellent seizure resistance in the cases of ratings A to D. The steel materials were judged to have poor seizure resistance in the case of rating X. The evaluation results are shown in Table 2.

[0103] [Durability evaluation test for cold forged products] Test pieces No. 14A specified in JIS Z 2241 (2011) were taken from the area (internal area) excluding the area from the surface to a depth of 1 mm (surface area) of the cold forged product of each test number.

[0104] First, the tensile strength TS (MPa) of the cold forged product of each test number was determined using the two test pieces taken. Specifically, a tensile test in accordance with JIS B 1051 (2014) was carried out at room temperature (25°C) in air, and the tensile strength of each of the two test pieces was determined. The arithmetic average value of the tensile strength of each of the two test pieces was defined as the tensile strength TS (MPa) of the cold forged product of that test number.

[0105] Next, using the collected test pieces, the fatigue strength σ of the cold forged products of each test number was w Specifically, in accordance with JIS Z 2273 (1978), a sine wave, phase 0 (MPa) alternating amplitude fatigue test was carried out in air at room temperature (25°C). The fatigue test was started with a load of 0.6 times the tensile strength TS (MPa) obtained by the above method as the initial amplitude stress. The amplitude stress was reduced by 20 MPa from 0.6 times the tensile strength TS (MPa) for each test, and the test was repeated 10 times. 7 The maximum stress that does not break within σ is the fatigue strength. w (MPa) and the frequency was 15 Hz.

[0106] Obtained fatigue strength σ w Using the results of and tensile strength TS, the durability ratio of the cold forged product of that test number was calculated according to the following formula. Durability ratio = fatigue strength σ w / Tensile strength TS

[0107] The obtained durability ratio was evaluated as follows. S rating: Durability ratio is 0.52 or higher Rating A: Durability ratio is 0.50 to 0.51 Rating B: Durability ratio is 0.48 to 0.49 Rating C: Durability ratio is 0.46 to 0.47 Rating D: Durability ratio is 0.44 to 0.45 Rating X: Durability ratio is 0.43 or less In the cases of evaluations S to D, the durability ratio of the cold forged product was evaluated as high. In the case of evaluation X, the durability ratio of the cold forged product was judged to be low. The evaluation results are shown in Table 2.

[0108] [Resistance to delayed fracture] Twenty cold-forged products (bolts) of each test number were selected. The selected cold-forged products (bolts) were fastened to a fastening block so that the axial force was 80% of the yield strength YS. The yield strength YS was determined by performing a tensile test in accordance with JIS B 1051 (2014) at room temperature (25°C) in the air. The 20 cold-forged products (bolts) after fastening were placed in a neutral salt water spray environment in accordance with JIS Z 2371 (2015) to measure the fracture frequency after 30 days of exposure. Based on the fracture frequency (= number of bolts with confirmed fractures / 20 bolts), the delayed fracture resistance was evaluated as follows: Rating A: Breakage frequency is 0 / 20 to 1 / 20 Rating B: Breakage frequency is 2 / 20 to 4 / 20 Rating C: Breakage frequency is 5 / 20 to 7 / 20 Rating X: Breakage frequency is 8 / 20 or more In the cases of evaluations A to C, the cold forged product was judged to have excellent delayed fracture resistance. In the case of evaluation X, the cold forged product was judged to have low delayed fracture resistance.

[0109] [Evaluation Results] Referring to Table 2, the contents of each element in the chemical composition of the steel materials of test numbers 1 to 12, 14, 15, 17 to 20, 22 to 25, 27 to 33, and 36 to 43 were appropriate. Furthermore, the manufacturing conditions were also appropriate. Therefore, the number of types of solute Cr concentrations (the number of solute Cr concentrations with different values) on the steel material surface was 5 or more. Furthermore, F1 satisfied formula (1). As a result, the steel materials of these test numbers had excellent seizure resistance during cold forging after the formation of the lubricating coating. Furthermore, the cold forged products manufactured using these steel material test pieces had a high durability ratio and excellent delayed fracture resistance.

[0110] On the other hand, in the test number 13, the Cr content in the chemical composition of the steel was low. Therefore, the seizure resistance of the steel during cold forging after the formation of the lubricating coating was low. Furthermore, the durability ratio of the cold forged product was low.

[0111] In test number 34, the chemical composition of the steel was appropriate, but the width of the masking tape used in the pickling process was inappropriate. Therefore, the number of types of solid solution Cr concentration in the surface region AR was less than 5. As a result, the seizure resistance of the steel during cold forging after the formation of the lubricating coating was low.

[0112] In test number 35, the chemical composition of the steel was appropriate, but the total pickling time in the pickling process was too long. Therefore, F1 exceeded the upper limit of formula (1). As a result, the steel had poor seizure resistance during cold forging after the formation of the lubricating coating.

[0113] In test number 44, the chemical composition of the steel was appropriate, but the total pickling time in the pickling process was too short. Therefore, F1 was less than the lower limit of formula (1). As a result, the steel had poor seizure resistance during cold forging after the formation of the lubricating coating.

[0114] In test number 16, the Al content was too low. In test number 21, the Ti content was too low. In test number 26, the Nb content was too low. As a result, these test numbers had low delayed fracture resistance.

[0115] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure.

Claims

1. A steel material, The chemical composition, in mass%, is C: 0.10-0.40%, Si: 0.40% or less, Mn: 0.76-1.30%, P: 0.030% or less, S: 0.040% or less, Cr: 0.05-1.20%, Al: 0.005-0.100%, N: 0.001-0.015%, Ti: 0.005-0.100%, B: 0.0003 to 0.0100%, Nb: 0.003 to 0.100%, and The balance is Fe and impurities. In a surface region of the steel material in a range of 31.25 mm in the longitudinal direction, a first measurement point is located at 0.23 mm from the end of the surface region, and second to twentieth measurement points are located at 1.56 mm intervals in the longitudinal direction from the first measurement point. A 21st measurement point is located at 31.02 mm from the end of the surface region in the longitudinal direction. When the solute Cr concentrations at a depth of 5 μm from the surface are measured at the first to 21st measurement points, there are at least five types of solute Cr concentrations measured, and the maximum solute Cr concentration among the solute Cr concentrations is defined as [Solute Cr max ] (mass%), and the minimum solute Cr concentration is defined as [Solute Cr min ] (mass%), and the Cr concentration in the chemical composition of the steel material is defined as [Cr base ] (mass%) satisfies formula (1), Steel material. 0.20≦([Solid solution Cr max ]-[Solid solution Cr min ]) / [Cr base ]≦0.60 (1)

2. The steel material according to claim 1, The chemical composition further includes, in place of a portion of Fe, Cu: 0.40% or less, Ni: 0.40% or less, and Mo: 0.20% or less, Contains one or more selected from the group consisting of Steel material.

Citation Information

Patent Citations

  • High strength pc steel bar excellent in delayed fracture characteristic and its production

    JP1997078191A

  • High strength PC steel bar excellent in delayed fracture characteristic and its production

    JP1997279303A

  • Spring steel wire rod having superior pickling characteristics

    JP2007138260A

  • Rolled wire rod and production method therefor

    JP2008007853A

  • Steel wire for bolt excellent in delayed fracture resistance, high-strength bolt, and production method for them