Manufacturing method and manufacturing equipment for press-molded products

A two-step mold process with a punch, pad, and die applies tension to reduce tensile residual stress in press-formed products, improving fatigue strength and efficiency by minimizing residual stress in bends.

JP7564448B2Active Publication Date: 2024-10-09NIPPON STEEL CORPORATION
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021039898
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-12
Publication Date
2024-10-09
Estimated Expiration
2041-03-12

AI Technical Summary

Technical Problem

Press-formed products exhibit significant tensile residual stress on the inside of bends, which reduces fatigue strength, especially in automobile parts, and existing methods to reduce this stress, such as heat treatment and shot peening, are inefficient and can cause surface roughness or require separate processes.

Method used

A method involving a two-step process using a mold with a punch, pad, and die to apply tension to the bent portion during press working, reducing compressive stress on the outside and tensile stress on the inside by crushing the convex portion with the die, thereby minimizing residual stress in the press-formed product.

Benefits of technology

The method effectively reduces tensile residual stress on the inside of bends in press-formed products, improving fatigue strength and maintaining production efficiency without separate treatments, thus enhancing the quality of automobile parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564448000002
    Figure 0007564448000002
  • Figure 0007564448000003
    Figure 0007564448000003
  • Figure 0007564448000004
    Figure 0007564448000004
Patent Text Reader

Abstract

To reduce tensile residual stress generated in the inside of bending in a bent part of a press molded article in a pressing step.SOLUTION: A method for manufacturing a press molded article (50) includes a first step and a second step. The first step presses a metal plate (30), and thereby obtains an intermediate article (40). The second step presses the intermediate article (40) using a mold (21) including a punch (26), a pad (28) and dies (27L and 27R), and obtains a press molded article (50). The second step includes the steps of: mounting the intermediate article (40) on the punch (26) so that a top plate (41) is arranged on a punch top surface (261) and projections (42L and 42R) are arranged at positions corresponding to punch shoulders (262L and 262R); pressing the top late (41) with the pad (28); bringing the dies (27L and 27R) into contact with flanges (44L and 44R); and crushing the projections (42L and 42R) with the dies (27L and 27R).SELECTED DRAWING: Figure 5A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a manufacturing method and manufacturing equipment for a press-molded product. [Background technology]

[0002] Conventionally, press-formed products have been used as components for constructing automobile bodies and the like. Press-formed products are manufactured by pressing metal sheets. More specifically, press-formed products are manufactured by drawing or bending a metal sheet as a material using a mold including a die and a punch.

[0003] In press working of metal plates, springback occurs when the press-formed product formed by the die is released from the die. That is, when the metal plate is bent by the die during press working, tensile stress occurs on the outside of the bend and compressive stress occurs on the inside of the bend in the bent part, but when the forming is completed and the press-formed product is removed from the die, elastic recovery of the material occurs. As a result, stress occurs in the bent part of the press-formed product in a direction opposite to the direction of the stress during press working. This reverse stress due to springback is added to the stress at the end of forming, so that compressive stress remains on the outside of the bend and tensile stress remains on the inside of the bend in the bent part of the press-formed product.

[0004] In press-formed products used as automobile parts, it is preferable that the tensile residual stress on the inner side of the bend is small. For example, in automobile undercarriage parts such as suspension members, relatively large stresses are repeatedly generated in the bent parts when the automobile starts, runs, or brakes, so that the greater the tensile stress remaining on the inner side of the bend, the lower the fatigue strength of the bent parts.

[0005] In order to resist fatigue failure caused by repeated loads, appropriate materials and plate thicknesses are used when manufacturing press-formed products for automobile parts. Also, to meet the need for lighter vehicles, metal plates, which are the raw materials, are becoming stronger and thinner. However, thinner materials result in higher repeated loads on press-formed products manufactured from the materials. Therefore, in order to achieve both weight reduction (thinner materials) and fatigue strength, it is necessary to reduce the tensile stress remaining on the inside of the bend in the bent part of the press-formed product.

[0006] Known methods for removing tensile residual stress from a press-formed product include heat treatment, shot peening, and impact treatment using an ultrasonic vibrator. However, these treatments must be performed in a separate process from the press working process, which reduces the manufacturing efficiency of the press-formed product and increases the number of steps and costs required for manufacturing the press-formed product. In addition, shot peening is difficult to treat only the bent portion of the press-formed product, and also has the problem of causing surface roughness of the press-formed product. Therefore, it is preferable that the tensile residual stress in the bent portion of the press-formed product is reduced in the press working process.

[0007] For example, Patent Document 1 discloses a technique for performing a so-called ironing process on a metal sheet material in order to reduce tensile residual stress. In Patent Document 1, the clearance between the die and the punch is set to be equal to or larger than the thickness of the metal sheet and equal to or smaller than 1.02 times the thickness. According to Patent Document 1, by setting the clearance in this manner, the residual stress in the portion of the metal sheet that is in contact with the shoulder of the die before bending begins is smaller than the residual stress in the portion that will finally come into contact with the shoulder, thereby improving the fatigue properties of the press-formed product.

[0008] Patent Document 2 discloses a press device that includes a die, a punch, and a pad facing the top surface of the punch. In this press device, the die descends, and the die and the punch shoulder press the metal sheet to form a bent portion in the metal sheet, and then the pad descends toward the top surface of the punch. A recess is formed in the top surface of the punch, and this recess forms a space below the metal sheet, so that when the descending pad presses the metal sheet, the material of the metal sheet flows into the recess side of the top surface of the punch. According to Patent Document 2, such an inflow of material applies a tensile force to the inside of the bend of the bent portion, reducing the compressive stress and reducing the amount of springback after demolding. Therefore, the tensile residual stress on the inside of the bend can be reduced.

[0009] Patent Documents 3 to 5 disclose techniques for modifying the shape of a press-formed product itself in order to reduce the amount of springback after demolding. In Patent Documents 3 to 5, in a press-formed product having a generally hat-shaped cross section, unevenness or steps are provided on the vertical wall portion. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2002-316215 A [Patent Document 2] International Publication No. 2017 / 131042 [Patent Document 3] JP 2004-314123 A [Patent Document 4] JP 2006-272378 A [Patent Document 5] JP 2017-196646 A Summary of the Invention [Problem to be solved by the invention]

[0011] As described above, when a press-formed product is manufactured by pressing a metal plate, compressive stress remains on the outside of the bend and tensile stress remains on the inside of the bend in the bent portion of the press-formed product. In order to obtain a press-formed product having better fatigue properties, it is particularly necessary to reduce the tensile residual stress on the inside of the bend. In addition, from the viewpoint of preventing an increase in the manufacturing steps and manufacturing costs of the press-formed product, it is preferable that the tensile residual stress on the inside of the bend is reduced in the press working process.

[0012] An object of the present disclosure is to reduce tensile residual stress that occurs on the inner side of a bent portion of a press-molded product during a press working process. [Means for solving the problem]

[0013] The manufacturing method of the press-molded product according to the present disclosure includes a first step and a second step. In the first step, an intermediate product is obtained by pressing a metal plate. The intermediate product includes a top plate, a convex portion, a vertical wall, and a flange. The convex portion is connected to the top plate and protrudes upward from the top plate. The vertical wall extends downward from the convex portion. The flange extends from a lower end of the vertical wall to an opposite side of the top plate. In the second step, the intermediate product is press-molded using a die to obtain a press-molded product. The die includes a punch, a pad, and a die. The pad is disposed above the punch so as to face the punch. The die is disposed above the punch and to the side of the pad. The punch includes a punch top surface, a punch shoulder, and a punch side surface. The punch shoulder is continuous with the punch top surface. The punch side surface extends downward from the punch shoulder. The die includes an upper die shoulder, a die side surface, and a die lower surface. The upper die shoulder corresponds to the punch shoulder. The die side extends downward from the upper die shoulder corresponding to the punch side. The die lower surface is connected to the lower end of the die side via the lower die shoulder. The second step includes the steps of placing the intermediate formed product on the punch so that the top plate is disposed on the punch top surface and the convex portion is disposed in a position corresponding to the punch shoulder, lowering a pad to press the top plate on the punch top surface with the pad, lowering the die and contacting the die with the flange while the top plate is pressed with the pad, and further lowering the die after the die contacts the flange to crush the convex portion with the die. Effect of the Invention

[0014] According to the present disclosure, the tensile residual stress occurring on the inner side of the bend in the bent portion of a press-formed product can be reduced in the press working process. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a diagram that illustrates a manufacturing facility according to an embodiment and a process for manufacturing a press-formed product using the manufacturing facility. [Diagram 2] FIG. 2 is a cross-sectional view showing a schematic configuration of a press device for producing an intermediate molded product, which is included in the production facility according to the embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing a schematic configuration of a press device for producing a press-formed product, which is included in the production facility according to the embodiment. [Figure 4A] FIG. 4A is a schematic diagram for explaining a first step of the method for manufacturing a press-formed product according to the embodiment. [Figure 4B] FIG. 4B is a schematic diagram for explaining a first step of the method for manufacturing a press-formed product according to the embodiment. [Figure 4C] FIG. 4C is a schematic view for explaining a first step of the method for manufacturing a press-formed product according to the embodiment. [Figure 4D] FIG. 4D is a schematic diagram for explaining a first step of the method for manufacturing a press-formed product according to the embodiment. [Figure 4E] FIG. 4E is a schematic diagram for explaining a first step of the method for manufacturing a press-formed product according to the embodiment. [Figure 5A] FIG. 5A is a schematic view for explaining a second step of the method for producing a press-formed product according to the embodiment. [Figure 5B] FIG. 5B is a schematic view for explaining a second step of the method for manufacturing a press-formed product according to the embodiment. [Figure 5C] FIG. 5C is a schematic view for explaining a second step of the method for manufacturing a press-formed product according to the embodiment. [Figure 5D] FIG. 5D is a schematic view for explaining a second step of the method for manufacturing a press-formed product according to the embodiment. [Figure 5E] FIG. 5E is a schematic view for explaining a second step of the method for manufacturing a press-formed product according to the embodiment. [Figure 5F] FIG. 5F is a schematic view for explaining a second step of the method for manufacturing a press-formed product according to the embodiment. [Figure 5G] FIG. 5G is a schematic view for explaining a second step of the method for manufacturing a press-formed product according to the embodiment. [Figure 5H] FIG. 5H is a schematic view for explaining a second step of the method for manufacturing a press-formed product according to the embodiment. [Figure 6]FIG. 6 is a graph showing the relationship between the height / width of the convex portion of the intermediate product obtained in the first step in the manufacturing method of the press-molded product according to the embodiment and the tensile residual stress on the inner side of the bend in the bent portion of the press-molded product. [Figure 7] FIG. 7 is a graph showing the relationship between the radius of curvature of the apex of a convex portion of an intermediate product and the tensile residual stress on the inner side of a bent portion of a press-formed product. [Figure 8] FIG. 8 is a graph showing the relationship between the height of the intermediate product and the tensile residual stress on the inner side of the bend in the bent portion of the press-formed product. [Figure 9] FIG. 9 is a graph showing the relationship between the flange angle of the intermediate product and the tensile residual stress on the inner side of the bend in the bent portion of the press-formed product. [Figure 10] FIG. 10 is a graph showing the relationship between the length of the flange of the intermediate product and the tensile residual stress on the inner side of the bend in the bent portion of the press-formed product. [Figure 11] FIG. 11 is a graph showing the relationship between the radius of curvature of the lower die shoulder of the die used in the second step in the manufacturing method of the press-molded product according to the embodiment and the tensile residual stress on the inner side of the bend in the bent portion of the press-molded product. [Figure 12] FIG. 12 is a graph showing the relationship between the position of the convex portion of the intermediate product with respect to the pad profile of the die and the tensile residual stress on the inner side of the bend in the bent portion of the press-formed product in the second step. [Figure 13] FIG. 13 is a graph showing the relationship between the work hardening exponent of a metal plate that is the material of a press-formed product and the tensile residual stress on the inner side of a bent portion of the press-formed product. [Figure 14] FIG. 14 is a schematic diagram showing a method for producing a press-molded product according to a modified example of the above embodiment. [Figure 15] FIG. 15 is a graph showing the effects of the manufacturing method of the press-formed product according to the above-described modified example. [Figure 16] FIG. 16 is a perspective view showing a schematic configuration of a press-formed product according to an embodiment. [Figure 17]FIG. 17 is a graph showing the stress distribution in the plate thickness direction at the end of forming and the residual stress distribution in the plate thickness direction after springback, with respect to the stress generated in the bending circumferential direction in the bent portion of a conventional press-formed product. [Figure 18] FIG. 18 is a graph showing the stress distribution in the plate thickness direction at the end of forming and the residual stress distribution in the plate thickness direction after springback, based on the findings of the present inventors, with respect to the stress generated in the bending circumferential direction in the bent portion of a press-formed product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] In order to confirm the distribution of stress occurring in the bent portion of the press-formed product, the inventors carried out a CAE analysis of the press working using commercially available software (LS-DYNA ver971 rev7.12, manufactured by ANSYS, Inc.). The analysis conditions were as follows: Tensile strength of material: 980MPa Material thickness: 3.0mm Bend R (inner radius of curvature): 4.0 mm Shape of press-molded product (after processing): Two vertical walls and a top plate connecting the vertical walls (no flanges)

[0017] Regarding the stress generated in the circumferential direction in the bent part of a press-formed product, the stress distribution in the plate thickness direction at the end of forming and the residual stress distribution in the plate thickness direction after springback are shown in Figure 17. Figure 17 shows the stress (stress in the circumferential direction of the bend) generated on a line from the R apex (center of R) on the inside of the bend to the R apex on the outside of the bend in the bent part of the press-formed product. As can be seen from Figure 17, at the end of forming, in the bent part of the press-formed product, tensile stress occurs on the outside of the bend and compressive stress occurs on the inside of the bend. On the other hand, after springback, compressive residual stress occurs on the outside of the bend and tensile residual stress occurs on the inside of the bend in the bent part of the press-formed product.

[0018] The inventors noticed that compressive residual stress occurs in the bent portion of a press-formed product after springback not only in the region on the outside of the bend but also in the vicinity of the neutral axis (center of plate thickness) in the region on the inside of the bend, and came up with the idea of ​​applying tension to the bent portion during press working. The inventors thought that by performing press working while applying tension to the portion of the material that will become the bent portion, it is possible to reduce the compressive stress in the region on the inside of the bend at the end of forming, and therefore the tensile residual stress after springback would also be reduced.

[0019] A CAE analysis was performed under the same conditions as above, except that the material was bent while tension was applied, and the stress distribution shown in Fig. 18 was obtained. As can be seen from Fig. 18, when a bent portion of a press-formed product was formed while tension was applied, the compressive stress on the inner side of the bend at the end of forming was reduced, and the tensile residual stress on the inner side of the bend after springback was reduced and further became compressive stress. Therefore, the present inventors have investigated a method for applying tension to the portion that will become the bent portion of the press-formed product during press working, and have completed a manufacturing method for a press-formed product according to an embodiment.

[0020] The manufacturing method of the press-formed product according to the embodiment includes a first step and a second step. In the first step, an intermediate product is obtained by pressing a metal plate. The intermediate product includes a top plate, a convex portion, a vertical wall, and a flange. The convex portion is connected to the top plate and protrudes upward from the top plate. The vertical wall extends downward from the convex portion. The flange extends from a lower end of the vertical wall to an opposite side of the top plate. In the second step, the intermediate product is press-formed using a die to obtain a press-formed product. The die includes a punch, a pad, and a die. The pad is disposed above the punch so as to face the punch. The die is disposed above the punch and to the side of the pad. The punch includes a punch top surface, a punch shoulder, and a punch side surface. The punch shoulder is continuous with the punch top surface. The punch side surface extends downward from the punch shoulder. The die includes an upper die shoulder, a die side surface, and a die lower surface. The upper die shoulder corresponds to the punch shoulder. The die side surface extends downward from the upper die shoulder corresponding to the punch side surface. The die lower surface is connected to the lower end of the die side surface via the lower die shoulder. The second step includes the steps of placing the intermediate formed product on the punch so that the top plate is disposed on the punch top surface and the convex portion is disposed in a position corresponding to the punch shoulder, lowering a pad to press the top plate on the punch top surface with the pad, lowering the die and contacting the die with the flange while the top plate is being pressed with the pad, and further lowering the die after the die contacts the flange to crush the convex portion with the die (first configuration).

[0021] In the manufacturing method of the press-formed product according to the first configuration, after the metal plate is pressed into an intermediate product in the first step, the intermediate product is pressed using a die including a punch, a pad, and a die in the second step to obtain a press-formed product. In the second step, the intermediate product is first placed on the punch, and the top plate of the intermediate product is pressed from above by the pad. In this state, the die is brought into contact with the flange of the intermediate product, and the die is lowered as it is. The flange of the intermediate product is not bent back immediately after the die comes into contact, but is bent back gradually as the die descends. Therefore, the flange is caught on the lower die shoulder while the forming proceeds, and tension acts on the convex portion and vertical wall provided between the top plate and the flange of the intermediate product. That is, tension is applied to the portion of the intermediate product that will become the bent portion in the final press-formed product. Therefore, the compressive stress on the inside of the bend at the end of forming can be reduced in the bent portion of the press-formed product. As a result, the tensile stress remaining on the inside of the bend after springback can be reduced.

[0022] Furthermore, in the second step, as the die descends, the protrusions of the intermediate product located at the position corresponding to the punch shoulder are crushed by the die and undergo bending back deformation. In the process in which the protrusions are bent back by the die and pressed into the punch shoulder, compressive stress occurs in the area on the die side (outside of the bend) and tensile stress occurs in the area on the punch side (inside of the bend). These stresses can reduce the tensile stress that occurs on the outside of the bend and the compressive stress that occurs on the inside of the bend when the intermediate product fits (wraps) around the punch shoulder and forms a bent part, that is, when the second step is completed. As a result, the tensile residual stress that occurs on the inside of the bend in the bent part of the press-formed product after springback can be reduced.

[0023] It is difficult to flatten a convex portion arranged at a position corresponding to a punch shoulder by simply applying tension from the periphery. However, in the manufacturing method of the press-formed product according to the first configuration, the convex portion is crushed by the die in the second step. This allows the convex portion to be firmly flattened. More specifically, the descending die hits the convex portion and crushes the convex portion from the top, so that a large stress is generated from the base of the convex portion toward the top. In other words, a large tensile stress is generated in the region on the inner side of the bend. Therefore, the compressive stress generated on the inner side of the bend at the end of the second step can be effectively reduced. As a result, the tensile residual stress generated on the inner side of the bend in the bent portion of the press-formed product after springback can be reduced.

[0024] In this way, as forming proceeds while the flange is caught on the lower die shoulder, tension is applied to the convex portion and vertical wall between the top plate and the flange in the intermediate formed product, and the convex portion is crushed from the top, so that the compressive stress generated on the inside of the bend at the end of the second step can be significantly reduced. As a result, the tensile residual stress generated on the inside of the bend in the bent portion of the press-formed product after springback can be significantly reduced.

[0025] As described above, according to the manufacturing method of the press-formed product of the first configuration, the tensile residual stress generated on the inner side of the bend in the bent portion of the press-formed product can be reduced in the press working process.

[0026] In the above manufacturing method, when the intermediate molded product is placed on the punch, it is preferable that the upper end of the convex portion is located more inward than the lower end of the die side surface in the width direction of the die, and the lower end of the vertical wall is located more outward than the upper end of the punch side surface in the width direction of the die (second configuration).

[0027] According to the second configuration, when the intermediate formed product is placed on the punch, that is, at the start of the second step, the upper end of the convex portion is located inside the lower end of the die side surface in the die width direction. This makes it possible to prevent the convex portion from being crushed by the lower die shoulder or the die lower surface at the beginning of the second step. In other words, it is possible to crush the convex portion by the die at the middle or later stage of the second step, and generate tensile stress in the region on the inner side of the bend. Therefore, the compressive stress generated on the inner side of the bend at the end of the second step can be more effectively reduced. Therefore, the tensile residual stress generated on the inner side of the bend in the bent portion of the press-formed product can be more reliably reduced.

[0028] In the intermediate molded product placed on the punch, when the lower end of the vertical wall is located inside the upper end of the punch side surface in the width direction of the die, the top plate of the intermediate molded product floats above the top surface of the punch. If press molding is performed in this state, the intermediate molded product cannot be stably held down by the pad, and the intermediate molded product may shift in the width direction (left and right direction) of the die during molding, and the dimensional accuracy of the final press molded product cannot be obtained. In contrast, in the second configuration, the intermediate molded product is configured such that, when placed on the punch, the lower end of the vertical wall is located outside the upper end of the punch side surface in the width direction of the die. Therefore, the top plate of the intermediate molded product does not float above the top surface of the punch, and the intermediate molded product can be stably placed on the punch. In addition, when the top plate of the intermediate molded product is held down by the pad, the pad can be prevented from floating. Therefore, the dimensional accuracy of the press molded product obtained in the second process can be stabilized.

[0029] In the intermediate molded product, when the vertical distance from the connection between the convex portion and the top plate to the upper end of the convex portion is H1 [mm] and the widthwise distance of the intermediate molded product from the connection between the convex portion and the top plate to the upper end of the convex portion is W1 [mm], it is preferable that H1 / W1 is 0.5 or more and 2.0 or less (third configuration).

[0030] According to the third configuration, in the intermediate molded product, the ratio H1 / W1 between the vertical distance (height of the protrusion) H1 from the connection between the protrusion and the top plate to the top end of the protrusion and the widthwise distance (width of the protrusion) W1 from the connection between the protrusion and the top plate to the top end of the protrusion is 0.5 or more. This makes the protrusion rise relatively steeply from the top plate, so that the amount of deformation of the protrusion caused by the die during bending back can be ensured. Therefore, when the protrusion is bent back in the second step, tensile stress can be more effectively generated in the region on the inner side of the bend. Therefore, the compressive stress generated on the inner side of the bend at the end of the second step can be more reliably reduced, and the effect of reducing the tensile stress remaining on the inner side of the bend can be improved in the bent part of the press molded product.

[0031] In the third configuration, the ratio H1 / W1 of the height H1 to the width W1 of the protruding portion of the intermediate molded product is 2.0 or less. This prevents the protruding portion from becoming excessively steep in shape relative to the top plate, making it possible to prevent the protruding portion from buckling when the protruding portion is crushed by the die in the second process.

[0032] In the above-mentioned manufacturing method, the convex portion may include an apex portion that is arc-shaped in a cross-sectional view of the intermediate molded product. The apex portion preferably has a radius of curvature of 4 mm or more and 16 mm or less (fourth configuration).

[0033] In the fourth configuration, the convex portion includes an arc-shaped apex in the cross-sectional view of the intermediate molded product. By making the radius of curvature of this apex 4 mm or more, it is possible to suppress the convex portion from buckling when the convex portion is crushed by the die. In addition, by making the radius of curvature of the apex 16 mm or less, the convex portion does not have an excessively gentle shape, so that in the second step, tensile stress can be more effectively generated on the inner side of the bend due to bending back deformation of the convex portion. Therefore, it is possible to further reduce the compressive stress generated on the inner side of the bend at the end of the second step, and it is possible to more reliably reduce the tensile stress remaining on the inner side of the bend in the bent portion of the press-molded product.

[0034] In the die used in the second step of the above-mentioned manufacturing method, the punch shoulder is, for example, arc-shaped in cross section of the punch. When the intermediate molded product is placed on the punch, a distance D2 [mm] in the width direction of the die from the end of the punch shoulder on the punch top side to the upper end of the convex portion is preferably positive when the upper end of the convex portion is located outside the end of the punch shoulder on the punch top side in the width direction and is negative when the upper end of the convex portion is located inside in the width direction, satisfying the following formula (fifth configuration): -1.0×Rp×(π-θ)≦D2≦2.5×Rp×(π-θ) Here, Rp is the radius of curvature of the punch shoulder (mm), and θ is the angle (rad) between the top surface of the punch and the side surface of the punch.

[0035] According to the fifth configuration, the distance D2 in the width direction of the die from the end of the punch shoulder on the punch top side to the upper end of the convex portion is set to satisfy the above formula in relation to the radius of curvature Rp of the punch shoulder and the angle θ between the punch top and the punch side surface. By setting the distance D2 in this way, the convex portion is likely to overlap the punch shoulder in the width direction of the die, so that tensile stress can be generated more widely on the inside of the bend during press forming due to the bending back deformation of the convex portion in the punch shoulder region. Therefore, the compressive stress generated on the inside of the bend when the intermediate formed product fits the punch shoulder to form a bent portion can be more effectively reduced. As a result, the tensile stress remaining on the inside of the bend after springback in the bent portion of the press-formed product can be more reliably reduced.

[0036] In the intermediate molded product, the distance in the up-down direction from the end of the vertical wall side of the flange to the top plate is preferably 6 mm or more (sixth configuration).

[0037] If the height of the intermediate formed product, that is, the vertical distance from the end of the vertical wall of the flange to the top plate, is insufficient, when the die in contact with the flange descends in the second step, the vertical wall may bend overall, and the tension applied to the convex portion and the vertical wall may decrease. In contrast, in the sixth configuration, the height of the intermediate formed product is ensured to be 6 mm or more. This makes it possible to suppress the vertical wall of the intermediate formed product from bending in the second step, and to more effectively apply tension to the convex portion and the vertical wall. Therefore, in the bent portion of the press-formed product, the compressive stress on the inside of the bend at the end of forming can be further reduced, and the effect of reducing the tensile stress remaining on the inside of the bend after springback can be improved.

[0038] In the above manufacturing method, when the intermediate molded product is placed on the punch, the angle that the flange makes with respect to the horizontal plane is preferably greater than -40° and less than 40°, with the angle being positive when the flange is rotated upward around the end of the vertical wall and negative when the flange is rotated downward (seventh configuration).

[0039] According to the seventh configuration, the angle that the flange of the intermediate product makes with respect to the horizontal plane is ensured to be -40° or more. This makes it easier for the flange to be caught by the lower die shoulder when the die comes into contact with the flange of the intermediate product and descends in the second step. This makes it possible to more reliably apply tension to the convex portion and vertical wall provided between the top plate and the flange in the intermediate product. This makes it possible to more effectively reduce the compressive stress on the inner side of the bend at the end of forming in the bent portion of the press-formed product, and improves the effect of reducing the tensile stress remaining on the inner side of the bend after springback.

[0040] In the seventh configuration, the angle that the flange of the intermediate molded product makes with the horizontal plane is 40° or less, which makes it possible to prevent the flange from buckling or the die from being damaged by the tip of the flange when the die comes into contact with the flange.

[0041] In the above manufacturing method, the lower die shoulder preferably has an arc shape having a radius of curvature of 1 mm or more and 12 mm or less in a cross-sectional view of the die (eighth configuration).

[0042] In the manufacturing method according to the embodiment, in the second step, the top plate of the intermediate product is pressed by a pad, and then the die is brought into contact with the flange of the intermediate product. When the die descends in this state, the flange is caught by the lower die shoulder, and tension is applied to the intermediate product between the pad and the lower die shoulder. In order to make it easier to catch the flange on the lower die shoulder, it is preferable to make the radius of curvature of the lower die shoulder small to a certain extent. In addition, a smaller radius of curvature of the lower die shoulder allows the flange to continue to be caught on the lower die shoulder until near the bottom dead center of the die. If the radius of curvature of the lower die shoulder is excessively large, the contact area between the intermediate product and the lower die shoulder will also be excessively large. In this case, when the die descends, the vertical wall and flange of the intermediate product are deflected as a whole, the catch of the flange on the lower die shoulder becomes weak, and the tension applied to the intermediate product between the pad and the lower die shoulder decreases. In consideration of this point, in the eighth configuration, the radius of curvature of the lower die shoulder is set to 12 mm or less. This makes it possible to limit the contact area between the intermediate product and the lower die shoulder in the second step, and makes it easier for the flange to catch on the lower die shoulder, so that tension can be applied more effectively to the intermediate product between the pad and the lower die shoulder. As a result, in the bent portion of the press-formed product, the compressive stress on the inside of the bend at the end of forming can be further reduced, and the effect of reducing the tensile stress remaining on the inside of the bend after springback can be improved.

[0043] If the radius of curvature of the lower die shoulder is less than 1 mm, the lower die shoulder may leave a bite mark on the press-formed product or cause the press-formed product to have a large bending tendency. Therefore, as in the eighth configuration, the radius of curvature of the lower die shoulder is preferably 1 mm or more.

[0044] In the above manufacturing method, the work hardening coefficient of the metal plate is preferably 0.04 or less (ninth configuration).

[0045] According to the ninth configuration, the work hardening index of the metal plate is sufficiently small, 0.04 or less. Therefore, work hardening of the material is unlikely to occur in the first process of obtaining an intermediate formed product from this metal plate and in the second process of obtaining a press-formed product from the intermediate formed product. In this case, the stress generated in the material is small in each process, and as a result, the stress due to springback is also small. Therefore, in each process, the residual stress, which is the sum of the stress at the end of forming and the reversal stress due to springback, can be reduced.

[0046] The manufacturing facility according to the embodiment is a manufacturing facility for manufacturing a press-formed product. The manufacturing facility includes a first mold and a second mold. The first mold molds a metal plate into an intermediate product. The intermediate product includes a top plate, a convex portion, a vertical wall, and a flange. The convex portion is connected to the top plate and protrudes upward from the top plate. The vertical wall extends downward from the convex portion. The flange extends from the lower end of the vertical wall to the opposite side of the top plate. The second mold molds the intermediate product into a press-formed product. The second mold includes a punch, a pad, and a die. The punch includes a punch top surface, a punch shoulder continuous with the punch top surface, and a punch side surface extending downward from the punch shoulder. The punch is configured so that the top plate is disposed on the punch top surface and the convex portion is disposed at a position corresponding to the punch shoulder when the intermediate product is molded into a press-formed product. The pad is disposed above the punch and configured to be movable up and down. The pad is configured to face a top plate disposed on the top surface of the punch when the intermediate product is formed into a press-formed product. The die is disposed above the punch and to the side of the pad, and configured to be movable up and down. The die includes an upper die shoulder corresponding to the punch shoulder, a die side surface extending downward from the upper die shoulder corresponding to the punch side surface, and a die lower surface connected to a lower end of the die side surface via the lower die shoulder. The die is configured so that the die lower surface faces the flange when the intermediate product is formed into a press-formed product.

[0047] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. In each drawing, the same or corresponding components are denoted by the same reference numerals, and the same description will not be repeated.

[0048] [Manufacturing equipment] 1 is a diagram showing a manufacturing facility 100 according to the present embodiment and a process for manufacturing a press-molded product by the manufacturing facility 100. The press-molded product is, for example, an automobile suspension part or a frame part such as a ladder frame. Examples of the automobile suspension part include arm parts such as an upper arm, a lower arm, or a trail link, as well as suspension members and torsion beams.

[0049] As shown in Fig. 1, a manufacturing facility 100 includes press devices 10 and 20. The press device 10 forms an intermediate product 40 from a metal plate 30 as a material. The press device 20 forms a press-formed product 50 as a final product from the intermediate product 40. Hereinafter, the configurations of each of the press devices 10 and 20 will be described with reference to Figs. 2 and 3.

[0050] [Press equipment for intermediate molded products] FIG. 2 is a cross-sectional view showing a schematic configuration of the press device 10 for obtaining the intermediate molded product 40 shown in FIG. 1. As shown in FIG. 2, the press device 10 includes a die 11, a bed 12, a slide 13, and die holders 14 and 15. The die 11 includes a punch 16 and a die 17. The punch 16 and the die 17 extend in a direction intersecting the plane of FIG. 2. Hereinafter, for the convenience of explanation, with respect to the press device 10 and its components, the direction in which the die 11, i.e., the punch 16 and the die 17 extend is referred to as the longitudinal direction, and the direction in which the punch 16 and the die 17 approach and move away from each other (the vertical direction in the plane of FIG. 2) is referred to as the vertical direction (vertical direction). A direction perpendicular to the plane consisting of the longitudinal direction and the vertical direction, i.e., a direction crossing the punch 16 and the die 17, is referred to as the left-right direction or width direction. Also, with respect to the press device 10 and its components, a cross section cut by a plane perpendicular to the longitudinal direction is referred to as a transverse section.

[0051] The punch 16 is supported by a bed 12, which is a part of the main body of the press device 10, via a die holder 14. That is, the die holder 14 is fixed to the upper surface of the bed 12, and the punch 16 is disposed on this die holder 14. A plate-shaped spacer may be inserted between the bed 12 and the die holder 14 to adjust the position of the punch 16 in the vertical direction.

[0052] The punch 16 includes a punch top surface 161, left and right convex surfaces 162L, 162R, left and right punch side surfaces 163L, 163R, and left and right punch flange surfaces 164L, 164R.

[0053] In this embodiment, punch top surface 161 has groove portion 161a extending in the longitudinal direction. Groove portion 161a may extend over the entire longitudinal direction of punch top surface 161, or may be provided on a portion of punch top surface 161 in the longitudinal direction. In this embodiment, punch top surface 161 has an asymmetric shape with respect to a vertical plane parallel to the longitudinal direction, that is, an asymmetric shape. However, punch top surface 161 may also have a symmetric shape.

[0054] Convex surfaces 162L, 162R are provided on both sides of punch top surface 161. Convex surfaces 162L, 162R are provided contiguous to punch top surface 161. Convex surfaces 162L, 162R are typically provided contiguous to punch top surface 161 over the entire punch top surface 161.

[0055] The convex surface 162L is connected to the left edge of the punch top surface 161. The convex surface 162L protrudes upward from the punch top surface 161. More specifically, the convex surface 162L protrudes upward compared to a portion of the punch top surface 161 that is on the outer side (left side) in the width direction from the groove portion 161a. The convex surface 162L has a convex shape that rises once from the punch top surface 161 toward the outer side in the width direction and then descends. The top of the convex surface 162L is, for example, substantially arc-shaped in a cross-sectional view of the punch 16. Hereinafter, the term "substantially arc-shaped" includes not only a curve that constitutes a part of a perfect circle, but also a smooth curve such as an elliptical curve or a spline curve. In addition, the radius of curvature in the case of a smooth curve other than a curve that constitutes a part of a perfect circle is defined as the radius of a circle that passes through three points, namely, both ends of the curve and the midpoint of the curve, when cut in a cross section.

[0056] The convex surface 162R is provided continuously with the right edge of the punch top surface 161. The convex surface 162R protrudes upward from the punch top surface 161. More specifically, the convex surface 162R protrudes upward compared to a portion of the punch top surface 161 that is on the outer side (right side) in the width direction from the groove portion 161a. The convex surface 162R has a convex shape that rises once from the punch top surface 161 toward the outer side in the width direction and then descends. For example, the top of the convex surface 162R is substantially arc-shaped in a cross-sectional view of the punch 16. The convex surface 162R may have a symmetrical shape to the convex surface 162L with respect to a vertical plane parallel to the longitudinal direction, or may have an asymmetrical shape.

[0057] The punch side surfaces 163L and 163R extend downward from the convex surfaces 162L and 162R, respectively, in a cross-sectional view of the punch 16. The punch side surface 163L is provided continuously with the left convex surface 162L. The punch side surface 163R is provided continuously with the right convex surface 162R. In the example of this embodiment, each of the punch side surfaces 163L and 163R is inclined with respect to a vertical plane parallel to the longitudinal direction so that its lower end is located outward in the width direction from its upper end. The punch side surfaces 163L and 163R may have a symmetrical shape with respect to the vertical plane parallel to the longitudinal direction, or may have an asymmetrical shape. In addition, the punch side surfaces 163L and 163R may be smooth curves provided continuously with the convex surfaces 162L and 162R. The punch side surfaces 163L, 163R or the convex surfaces 162L, 162R may be curved (inflected) inward or outward in the width direction midway from the upper ends of the convex surfaces 162L, 162R toward the punch flange surfaces 164L, 164R.

[0058] The punch flange surfaces 164L, 164R extend outward in the width direction from the punch side surfaces 163L, 163R, respectively, in a cross-sectional view of the punch 16. The punch flange surfaces 164L, 164R may extend substantially horizontally from the punch side surfaces 163L, 163R, or at least one of them may extend at an incline with respect to the horizontal plane. For example, the angle that each of the punch flange surfaces 164L, 164R makes with respect to the horizontal plane can be set in the range of -40° or more and 40° or less, with the case where the punch flange surfaces 164L, 164R rotate upward around the inner end in the width direction being positive, and the case where the punch flange surfaces 164L, 164R rotate downward being negative. The angle between the punch flange surfaces 164L, 164R and the horizontal plane is preferably -10° or more and 10° or less. Here, the horizontal plane refers to a plane perpendicular to the direction (up-down direction) in which the punch 16 and the die 17 approach and separate from each other. The angle that the punch flange surfaces 164L, 164R make with respect to the horizontal plane means the angle (acute angle side) that the punch flange surfaces 164L, 164R make with the width direction in a cross section cut by a plane consisting of the up-down direction and the width direction.

[0059] The punch flange surface 164L is provided continuously with the lower end of the left punch side surface 163L. The punch flange surface 164R is provided continuously with the lower end of the right punch side surface 163R. The boundary portion between the punch flange surface 164L and the punch side surface 163L is preferably subjected to R chamfering. Similarly, the boundary portion between the punch flange surface 164R and the punch side surface 163R is preferably subjected to R chamfering. In other words, the boundary portion between the punch flange surface 164L and the punch side surface 163L and the boundary portion between the punch flange surface 164R and the punch side surface 163R are preferably substantially arc-shaped in the cross-sectional view of the punch 16.

[0060] The die 17 is disposed above the punch 16. The die 17 is attached to the slide 13 via the die holder 15. That is, the die holder 15 is fixed to the lower surface of the slide 13, and the die 17 is fixed to the lower surface of the die holder 15. A plate-shaped spacer may be inserted between the slide 13 and the die holder 15 to adjust the position of the die 17 in the vertical direction. The slide 13 is configured to be able to rise and fall relative to the punch 16, for example, by a mechanical or hydraulic mechanism (not shown) provided in the press device 10. As the slide 13 rises and falls, the die 17 also rises and falls relative to the punch 16.

[0061] The die 17 has a molding surface corresponding to the molding surface of the punch 16. The molding surface of the die 17 has a shape offset from the molding surface of the punch 16 by approximately the same amount as the thickness of the metal sheet 30 processed by the metal mold 11. The molding surface of the die 17 has a shape offset from the molding surface of the punch 16 by, for example, 0.9 to 1.2 times the thickness of the metal sheet 30. The die 17 includes a die bottom surface 171, left and right concave surfaces 172L, 172R, left and right die side surfaces 173L, 173R, and left and right die flange surfaces 174L, 174R.

[0062] The die bottom surface 171 faces the punch top surface 161. The die bottom surface 171 is formed in a shape corresponding to the shape of the punch top surface 161. In this embodiment, the die bottom surface 171 has a protruding ridge portion 171a that corresponds to the groove portion 161a of the punch top surface 161.

[0063] Concave surfaces 172L, 172R are provided on both sides of the die bottom surface 171 in correspondence with the convex surfaces 162L, 162R of the punch 16, respectively. The concave surfaces 172L, 172R are provided continuously with the die bottom surface 171. Like the convex surfaces 162L, 162R of the punch 16, the concave surfaces 172L, 172R are typically provided continuously with the die bottom surface 171 over the entire longitudinal direction of the die bottom surface 171.

[0064] The concave surface 172L is connected to the left edge of the die bottom surface 171. The concave surface 172L is recessed upward relative to the die bottom surface 171. More specifically, the concave surface 172L is recessed upward compared to a portion of the die bottom surface 171 that is on the outer side (left side) in the width direction than the protruding streak portion 171a. The concave surface 172L has a concave shape that rises once from the die bottom surface 171 toward the outer side in the width direction and then falls. The concave shape of the concave surface 172L corresponds to the convex shape of the convex surface 162L of the punch 16. For example, the bottom of the concave surface 172L is substantially arc-shaped in a cross-sectional view of the die 17.

[0065] The concave surface 172R is provided continuously with the right edge of the die bottom surface 171. The concave surface 172R is recessed upward with respect to the die bottom surface 171. More specifically, the concave surface 172R is recessed upward compared to a portion of the die bottom surface 171 that is on the outer side (right side) in the width direction from the protruding streak portion 171a. The concave surface 172R has a concave shape that rises once from the die bottom surface 171 toward the outer side in the width direction and then falls. The concave shape of the concave surface 172R corresponds to the convex shape of the convex surface 162R of the punch 16. For example, the bottom of the concave surface 172R is substantially arc-shaped in a cross-sectional view of the punch 16.

[0066] The die side surfaces 173L and 173R extend downward from the concave surfaces 172L and 172R, respectively, in a cross-sectional view of the die 17. The die side surfaces 173L and 173R correspond to the punch side surfaces 163L and 163R, respectively. The die side surface 173L is provided continuously with the left concave surface 172L. The die side surface 173R is provided continuously with the right concave surface 172R. In the example of this embodiment, each of the die side surfaces 173L and 173R corresponds to the punch side surfaces 163L and 163R, and is inclined with respect to a vertical plane parallel to the longitudinal direction.

[0067] The die flange surfaces 174L, 174R extend outward in the width direction from the lower ends of the die side surfaces 173L, 173R, respectively, in a cross-sectional view of the die 17. The die flange surfaces 174L, 174R correspond to the punch flange surfaces 164L, 164R, respectively. The angles that the die flange surfaces 174L, 174R make with respect to the horizontal plane are substantially equal to the angles that the punch flange surfaces 164L, 164R make with respect to the horizontal plane.

[0068] The die flange surface 174L is provided continuously with the left die side surface 173L. The die flange surface 174R is provided continuously with the right die side surface 173R. The corners between the die flange surface 174L and the die side surface 173L are preferably R-chamfered. Similarly, the corners between the die flange surface 174R and the die side surface 173R are preferably R-chamfered. That is, the corners between the die flange surface 174L and the die side surface 173L and the corners between the die flange surface 174R and the die side surface 173R are preferably substantially arc-shaped in the cross-sectional view of the die 17.

[0069] [Press equipment for final molded products] FIG. 3 is a cross-sectional view showing a schematic configuration of a press device 20 for obtaining a press-molded product 50 (FIG. 1) as a final product.

[0070] As shown in FIG. 3, the press device 20 includes a die 21, a bed 22, a slide 23, and die holders 24 and 25. The die 21 includes a punch 26, left and right dies 27L and 27R, and a pad 28. The punch 26 and the dies 27L and 27R extend in a direction intersecting the plane of FIG. 3. With respect to the press device 20 and its components, the direction in which the die 21, particularly the punch 26 and the dies 27L and 27R, extend is referred to as the longitudinal direction, and the direction in which the punch 26 and the dies 27L and 27R approach and move away from each other (the vertical direction in the plane of FIG. 3) is referred to as the vertical direction (vertical direction). A direction perpendicular to a plane consisting of the longitudinal direction and the vertical direction, i.e., a direction crossing the punch 26 and the dies 27L and 27R, is referred to as the horizontal direction or width direction. With respect to the press device 20 and its components, a cross section cut by a plane perpendicular to the longitudinal direction is referred to as a transverse section.

[0071] The punch 26 is supported by a bed 22, which is a part of the main body of the press device 20, via a die holder 24. That is, the die holder 24 is fixed to the upper surface of the bed 22, and the punch 26 is disposed on this die holder 24. A plate-shaped spacer may be inserted between the bed 22 and the die holder 24 to adjust the position of the punch 26 in the vertical direction.

[0072] The punch 26 includes a punch top surface 261, left and right punch shoulders 262L, 262R, and left and right punch side surfaces 263L, 263R.

[0073] In this embodiment, a groove 261a extending in the longitudinal direction is formed in the punch top surface 261. The groove 261a is formed, for example, in a shape and size corresponding to the groove 161a (FIG. 2) of the punch top surface 161 in the press apparatus 10 shown in FIG. 2. In the example shown in FIG. 3, the punch top surface 261, like the punch top surface 161 (FIG. 2), has an asymmetric shape with respect to a vertical plane parallel to the longitudinal direction, that is, an asymmetric shape. However, the punch top surface 261 may also have a symmetric shape.

[0074] The punch shoulders 262L, 262R are provided contiguous to the punch top surface 261. More specifically, the punch shoulder 262L is continuous with a left edge of the punch top surface 261, and the punch shoulder 262R is continuous with a right edge of the punch top surface 261. Each of the punch shoulders 262L, 262R is substantially arc-shaped in a cross-sectional view of the punch 26. The punch shoulders 262L, 262R are ridges (corners) between the punch top surface 261 and the punch side surfaces 263L, 263R, respectively.

[0075] The punch side surface 263L extends downward from the left punch shoulder 262L in the cross-sectional view of the punch 26. The punch side surface 263R extends downward from the right punch shoulder 262R in the cross-sectional view of the punch 26. Each of the punch side surfaces 263L, 263R is inclined with respect to a vertical plane parallel to the longitudinal direction so that the lower end is located outward in the width direction from the upper end. The angles (acute angle side) that the punch side surfaces 263L, 263R make with the vertical plane may be the same or different. The angles between the punch side surfaces 263L, 263R and the vertical plane are preferably 20° or less. The angle (acute angle side) that the punch side surfaces 263L, 263R make with the vertical plane parallel to the longitudinal direction means the angle (acute angle side) that the punch side surfaces 263L, 263R make with the vertical direction in a cross section cut by a plane consisting of the up-down direction and the width direction.

[0076] The dies 27L and 27R are disposed above the punch 26 and to the side of the pad 28. The dies 27L and 27R are attached to the slide 23 via the die holder 25. That is, the die holder 25 is fixed to the lower surface of the slide 23, and the dies 27L and 27R are fixed to the lower surface of the die holder 25. A plate-shaped spacer may be inserted between the slide 23 and the die holder 25 to adjust the positions of the dies 27L and 27R in the vertical direction. The slide 23 is configured to be able to rise and fall relative to the punch 26, for example, by a mechanical or hydraulic mechanism (not shown) provided in the press device 20. As the slide 23 rises and falls, the dies 27L and 27R also rise and fall relative to the punch 26.

[0077] The left die 27L includes an upper die shoulder 271L, a die side surface 272L, a lower die shoulder 273L, a die lower surface 274L, and a die upper surface 275L. The right die 27R includes an upper die shoulder 271R, a die side surface 272R, a lower die shoulder 273R, a die lower surface 274R, and a die upper surface 275R. The left and right dies 27L and 27R may have a symmetrical shape with respect to a vertical plane parallel to the longitudinal direction, or may have an asymmetrical shape.

[0078] The upper die shoulders 271L, 271R are provided corresponding to the left and right punch shoulders 262L, 262R, respectively. The upper die shoulders 271L, 271R are substantially arc-shaped in cross-section of the dies 27L, 27R corresponding to the punch shoulders 262L, 262R, respectively. The upper die shoulders 271L, 271R are ridges (corners) between the die side surfaces 272L, 272R and the die top surfaces 275L, 275R.

[0079] Die top surfaces 275L, 275R are disposed on the inside of the upper die shoulders 271L, 271R in the width direction. The die top surface 275L is provided continuous with the right end of the upper die shoulder 271L and faces the punch top surface 261. The die top surface 275R is provided continuous with the left end of the upper die shoulder 271R and faces the punch top surface 261. Die side surfaces 272L, 272R are disposed on the outside of the upper die shoulders 271L, 271R in the width direction. The die side surface 272L is provided continuous with the left end of the upper die shoulder 271L. The die side surface 272R is provided continuous with the right end of the upper die shoulder 271R.

[0080] The die side surface 272L extends downward from the upper die shoulder 271L in a cross-sectional view of the die 27L. The die side surface 272R extends downward from the upper die shoulder 271R in a cross-sectional view of the die 27R. The die side surfaces 272L and 272R are provided corresponding to the left and right punch side surfaces 263L and 263R, respectively. The die side surfaces 272L and 272R are inclined with respect to a vertical plane parallel to the longitudinal direction so that the lower ends are positioned outward in the width direction from the upper ends in correspondence with the punch side surfaces 263L and 263R, respectively. The angle (acute angle side) that the die side surfaces 272L and 272R make with respect to the vertical plane is substantially equal to the angle (acute angle side) that the punch side surfaces 263L and 263R make with respect to the vertical plane parallel to the longitudinal direction.

[0081] In the left die 27L, the lower die shoulder 273L is provided contiguous with the lower end of the die side surface 272L. In the right die 27R, the lower die shoulder 273R is provided contiguous with the lower end of the die side surface 272R. The lower die shoulders 273L, 273R are substantially arc-shaped in the cross-sectional view of the dies 27L, 27R, respectively. The lower die shoulders 273L, 273R are ridges (corners) between the die side surfaces 272L, 272R and the die lower surfaces 274L, 274R. The radius of curvature Rd of the lower die shoulders 273L, 273R L ,Rd R are preferably 1 mm or more and 12 mm or less, respectively.

[0082] In the left die 27L, the die lower surface 274L is connected to the lower end of the die side surface 272L via the lower die shoulder 273L. In the right die 27R, the die lower surface 274R is connected to the lower end of the die side surface 272R via the lower die shoulder 273R. The die lower surfaces 274L, 274R extend outward in the width direction from the lower die shoulders 273L, 273R in the cross-sectional view of the dies 27L, 27R, respectively. In this embodiment, the die lower surfaces 274L, 274R extend horizontally from the lower die shoulders 273L, 273R. However, at least one of the die lower surfaces 274L, 274R may be inclined with respect to the horizontal plane. The horizontal plane refers to a plane perpendicular to the direction in which the dies 27L, 27R rise and fall (up and down direction).

[0083] The pad 28 is disposed above the punch 26 so as to face the punch top surface 261. The pad 28 is disposed between the left and right dies 27L, 27R. The pad 28 is attached to the slide 23 via the die holder 25, so that the pad 28 can be raised and lowered relative to the punch 26.

[0084] The pad 28 has a pad body 281 and a support member 282. The lower surface of the pad body 281 faces the punch top surface 261. The lower surface of the pad body 281 is formed in a shape corresponding to the punch top surface 261. In this embodiment, a convex rib portion 281a extending in the longitudinal direction is provided on the lower surface of the pad body 281 in correspondence with the groove portion 261a of the punch top surface 261. The support member 282 elastically supports the pad body 281 with respect to the die holder 25. The support member 282 is an expandable member constituted of, for example, a spring or a fluid pressure cylinder.

[0085] [Method of manufacturing press-molded products] Hereinafter, a method for manufacturing a press-formed product using the manufacturing equipment 100 will be described. The manufacturing method for a press-formed product according to this embodiment includes a first step of obtaining an intermediate product 40 by pressing a metal plate 30, and a second step of obtaining a press-formed product 50 by pressing the intermediate product 40. In the first step, a press device 10 is used, and in the second step, a press device 20 is used.

[0086] (1st step) 4A to 4E are schematic diagrams for explaining the first step. First, referring to FIG. 4A, when the first step is performed, a metal plate 30 is prepared as a material. The metal plate 30 is typically a steel plate. The plate thickness t of the metal plate 30 is, for example, 2.0 mm or more and 8.0 mm or less. The metal plate 30 has a tensile strength of, for example, 270 MPa or more and 1180 MPa or less. When the press-molded product 50 to be manufactured is an arm part among the suspension parts of an automobile, the tensile strength of the metal plate 30 is usually 590 MPa or more. When the press-molded product 50 to be manufactured is a frame part such as a ladder frame of an automobile, the tensile strength of the metal plate 30 is usually 590 MPa or more.

[0087] The work hardening index of the metal plate 30 is preferably 0.04 or less. The ratio (yield ratio) YR=YS / TS of the yield stress YS to the tensile strength TS of the metal plate 30 is preferably 0.95 or more. The work hardening index is an index showing the ease of work hardening of the metal plate 30, and the larger the value, the easier the material is to work harden. The work hardening index (n value) is defined in JIS G 0202:2013, and is measured by the method specified in, for example, JIS Z 2253:2011. The yield ratio YR is a value that is inversely correlated with the n value, and therefore decreases as the n value increases.

[0088] Next, the prepared metal sheet 30 is pressed by the die 11 included in the press device 10. When the press process is started, the metal sheet 30 is placed on the punch 16 with the die 17 positioned at the top dead center as shown in FIG. 4B. The metal sheet 30 is supported by at least one of the convex surfaces 162L, 162R, for example. Next, the slide 13 is lowered to lower the die 17 toward the metal sheet 30 on the punch 16.

[0089] As shown in Fig. 4C, when the die 17 comes into contact with the metal sheet 30, the metal sheet 30 starts to deform along the forming surfaces of the punch 16 and the die 17. As shown in Fig. 4D, when the die 17 reaches the bottom dead center, the metal sheet 30 is pressed between the punch 16 and the die 17, and an intermediate formed product 40 is completed.

[0090] Fig. 4E is a cross-sectional view (transverse cross-sectional view) of the intermediate molded product 40 obtained in the first step when cut along a plane perpendicular to the longitudinal direction. The longitudinal direction and width direction of the intermediate molded product 40 coincide with the longitudinal direction and width direction of the mold 11 (Fig. 2). As shown in Fig. 4E, the intermediate molded product 40 includes a top plate 41, left and right protrusions 42L, 42R, left and right vertical walls 43L, 43R, and left and right flanges 44L, 44R.

[0091] The top plate 41 is a portion of the intermediate product 40 that is formed by the punch top surface 161 and the die bottom surface 171 (FIG. 2). The top plate 41 is formed with grooves 41a corresponding to the grooves 161a of the punch top surface 161 and the protruding strips 171a of the die bottom surface 171.

[0092] The left and right convex portions 42L, 42R are connected to the top plate 41. The convex portion 42L is a portion of the intermediate molded product 40 formed by the convex surface 162L of the punch 16 and the concave surface 172L of the die 17 (FIG. 2). The convex portion 42R is a portion of the intermediate molded product 40 formed by the convex surface 162R of the punch 16 and the concave surface 172R of the die 17 (FIG. 2). Each of the convex portions 42L, 42R protrudes upward from the top plate 41. More specifically, the convex portion 42L protrudes upward from a portion of the top plate 41 that is on the outer side (left side) of the groove portion 41a in the width direction. The convex portion 42R protrudes upward from a portion of the top plate 41 that is on the outer side (right side) of the groove portion 41a in the width direction.

[0093] The protrusions 42L, 42R include apexes 421L, 421R, respectively. Each of the apexes 421L, 421R is substantially arc-shaped in a cross-sectional view of the intermediate molded product 40. Each of the apexes 421L, 421R preferably has a radius of curvature of 4 mm or more and 16 mm or less. The radius of curvature here is the radius of curvature on the inner side of the bend of the apexes 421L, 421R.

[0094] The portion of the left protrusion 42L on the top plate 41 side, i.e., the base 422L of the protrusion 42L, is, for example, substantially arc-shaped in a cross-sectional view of the intermediate molded product 40. The end (R end) of the base 422L on the top plate 41 side is the connection part between the protrusion 42L and the top plate 41. In this embodiment, the distance in the width direction of the intermediate molded product 40 from this connection part to the upper end of the protrusion 42L is defined as the width W1 of the protrusion 42L. L The height H1 of the protrusion 42L is defined as the vertical distance from the connection between the protrusion 42L and the top plate 41 to the upper end of the protrusion 42L. L [mm], where height H1 L is the vertical distance between the center of thickness of the connection portion and the center of thickness of the upper end of the protrusion 42L.

[0095] Height H1 of protruding part 42L L is preferably 5 mm or more and 25 mm or less. L Height H1 L Ratio of:H1 L / W1 L is preferably 0.5 or more and 2.0 or less.

[0096] Similarly, the portion of the right protrusion 42R on the top plate 41 side, i.e., the base 422R of the protrusion 42R, is, for example, substantially arc-shaped in a cross-sectional view of the intermediate molded product 40. The end (R end) of the base 42R on the top plate 41 side is the connection between the protrusion 42R and the top plate 41. In this embodiment, the distance in the width direction of the intermediate molded product 40 from this connection to the upper end of the protrusion 42R is defined as the width W1 of the protrusion 42R. R The height H1 of the protrusion 42R is defined as the vertical distance from the connection between the protrusion 42R and the top plate 41 to the upper end of the protrusion 42R. R [mm], where height H1 R is the vertical distance between the center of thickness of the connection portion and the center of thickness of the upper end of the protrusion 42R.

[0097] Height H1 of protrusion 42R R is preferably 5 mm or more and 25 mm or less. R Height H1R Ratio of:H1 R / W1 R is preferably 0.5 or more and 2.0 or less.

[0098] The left and right vertical walls 43L, 43R extend downward from the convex portions 42L, 42R, respectively, in a cross-sectional view of the intermediate molded product 40. The vertical wall 43L is disposed to the left of the convex portion 42L and connects the convex portion 42L and the flange 44L. The vertical wall 43R is disposed to the right of the convex portion 42R and connects the convex portion 42R and the flange 44R. The connection portion between the vertical wall 43L and the convex portion 42L and the connection portion between the vertical wall 43R and the convex portion 42R may have a smooth shape that is continuously provided from the convex portions 42L, 42R to the vertical walls 43L, 43R. The vertical walls 43L, 43R or the convex portions 42L, 42R may be curved (inflected) inward or outward in the width direction on the way from the upper ends of the convex portions 42L, 42R to the left and right flanges 44L, 44R.

[0099] The left and right flanges 44L, 44R extend from the lower ends of the vertical walls 43L, 43R, respectively, to the opposite side of the top plate 41, in a cross-sectional view of the intermediate molded product 40. The left flange 44L extends from the vertical wall 43L to the outside in the width direction (left side), in a cross-sectional view of the intermediate molded product 40. The right flange 44R extends from the vertical wall 43R to the outside in the width direction (right side), in a cross-sectional view of the intermediate molded product 40. The flanges 44L, 44R are connected to the vertical walls 43L, 43R via arc-shaped corners 45L, 45R, respectively, in a cross-sectional view of the intermediate molded product 40.

[0100] The height H2 of the intermediate molded product 40 is preferably 6 mm or more. The height H2 of the intermediate molded product 40 refers to the vertical distance from the ends of the flanges 44L, 44R on the vertical walls 43L, 43R side, i.e., the R ends of the corners 45L, 45R on the flanges 44L, 44R side, to the top plate 41. Note that the height H2 is the vertical distance between the center of the plate thickness of the ends of the flanges 44L, 44R on the vertical walls 43L, 43R side and the center of the plate thickness of the top plate 41 at the connection portion with the protrusions 42L, 42R. If the vertical distance from the center of thickness of the end of flange 44L on the vertical wall 43L side to the center of thickness of the top plate 41 at the connection with convex portion 42L is different from the vertical distance from the center of thickness of the end of flange 44R on the vertical wall 43R side to the center of thickness of the top plate 41 at the connection with convex portion 42R, the smaller of the two distances is defined as the height H2 of the intermediate molded product 40.

[0101] (2nd process) After the first step is completed, the second step is carried out. Figures 5A to 5H are schematic diagrams for explaining the second step. In the second step, the intermediate molded product 40 obtained in the first step is subjected to press working by a die 21 included in a press device 20. The second step includes steps (a) to (d) described below.

[0102] Process (a) Referring to FIG. 5A, first, in step (a), the intermediate molded product 40 is placed on the punch 26 of the die 21. More specifically, the intermediate molded product 40 is placed on the punch 26 so that the top plate 41 is placed on the punch top surface 261. The intermediate molded product 40 is also placed on the punch 26 so that the protrusions 42L, 42R are placed at positions corresponding to the punch shoulders 262L, 262R, respectively. The top plate 41 is placed, for example, so that the position of the groove 41a coincides with the position of the groove 261a of the punch top surface 261. The protrusions 42L, 42R continuous with the top plate 41 are preferably positioned outside the pad profile P in the width direction of the die 21. The pad profile P is a boundary portion between the pad main body 281 and the dies 27L, 27R.

[0103] The protrusions 42L, 42R are disposed at positions corresponding to the punch shoulders 262L, 262R, respectively, meaning that the protrusions 42L, 42R are disposed so that at least a portion of the protrusions 42L, 42R is pressed by the punch shoulders 262L, 262R and the upper die shoulders 271L, 271R. For example, the protrusions 42L, 42R are disposed so that at least a portion of the protrusions 42L, 42R overlaps with the punch shoulders 262L, 262R in the width direction of the die 21.

[0104] 5B, when the intermediate molded product 40 is placed on the punch 26, the upper end of the protrusion 42L is preferably located inside the lower end of the die side surface 272L (the end of the R of the lower die shoulder 273L on the die side surface 272L) in the width direction of the mold 21. That is, the distance in the width direction between the upper end of the protrusion 42L and the lower end of the die side surface 272L is set to D1. L [mm], D1 L It is preferable that the distance D1 is >0. L Regarding , it is positive when the upper end of the protrusion 42L is located widthwise inside the lower end of the die side surface 272L, and it is negative when the upper end of the protrusion 42L is located widthwise outside the lower end of the die side surface 272L.

[0105] Similarly, when the intermediate molded product 40 is placed on the punch 26, the upper end of the protrusion 42R is preferably located inside the lower end of the die side surface 272R (the R end of the lower die shoulder 273R on the die side surface 272R side) in the width direction of the mold 21. In other words, the distance in the width direction between the upper end of the protrusion 42R and the lower end of the die side surface 272R is set to D1. R [mm], D1 R It is preferable that the distance D1 is >0. R Regarding , it is positive when the upper end of the protrusion 42R is located widthwise inside the lower end of the die side surface 272R, and it is negative when the upper end of the protrusion 42R is located widthwise outside the lower end of the die side surface 272R.

[0106] More preferably, when the intermediate molded product 40 is placed on the punch 26, each distance D2 in the width direction of the die 21 from the end (R end) of the punch shoulders 262L, 262R on the punch top surface 261 side to the upper ends of the protrusions 42L, 42R is L ,D2R [mm] is set to satisfy the following formula (1). In formula (1), the distance D2 L ,D2 R These are collectively expressed as D2. In addition, in formula (1), the radius of curvature Rp of the punch shoulders 262L and 262R L ,Rp R "mm", and the angle θ between the punch top surface 261 and the punch side surface 263L in cross section L ,θ R [rad] are collectively expressed as Rp and θ. That is, in the following formula (1), the distance D2 is the distance D2 L If so, Rp and θ are Rp L ,θ L and the distance D2 is the distance D2 R If so, Rp and θ are Rp R ,θ R Regarding the distance D2, it is positive when the upper ends of the convex portions 42L, 42R are located on the outer side in the width direction than the ends of the corresponding punch shoulders 262L, 262R on the punch top surface 261 side, and it is negative when the upper ends are located on the inner side in the width direction. -1.0×Rp×(π-θ)≦D2≦2.5×Rp×(π-θ)···(1)

[0107] When the intermediate molded product 40 is placed on the punch 26, the lower end of the vertical wall 43L is preferably positioned outside the upper end of the punch side surface 263L (the R end of the punch shoulder 262L on the punch side surface 263L) in the width direction of the die 21. In other words, the distance in the width direction between the lower end of the vertical wall 43L and the upper end of the punch side surface 263L is set to D3. L [mm], D3 L >0. Distance D3 L Regarding the distance D3, it is positive when the lower end of the vertical wall 43L is located outside the upper end of the punch side surface 263L in the width direction, and it is negative when the lower end of the vertical wall 43L is located inside the upper end of the punch side surface 263L in the width direction. L In this regard, the lower end of the vertical wall 43L refers to the outer side of the bend of the corner portion 45L, that is, of the two R ends on the inner side (the punch 26 side) of the intermediate molded product 40, the R end on the vertical wall 43L side.

[0108] Similarly, when the intermediate molded product 40 is placed on the punch 26, the lower end of the vertical wall 43R is preferably positioned outside the upper end of the punch side surface 263R (the R end of the punch shoulder 262R on the punch side surface 263R side) in the width direction of the die 21. In other words, the distance in the width direction between the lower end of the vertical wall 43R and the upper end of the punch side surface 263R is set to D3. R [mm], D3 R >0. Distance D3 R Regarding the distance D3, it is positive when the lower end of the vertical wall 43R is located outside the upper end of the punch side surface 263R in the width direction, and it is negative when the lower end of the vertical wall 43R is located inside the upper end of the punch side surface 263R in the width direction. R In this regard, the lower end of the vertical wall 43R refers to the outer side of the bend of the corner portion 45R, that is, of the two R ends on the inner side (punch 26 side) of the intermediate molded product 40, the R end on the vertical wall 43R side.

[0109] Referring to FIG. 5C, when the intermediate product 40 is placed on the punch 26, the angles φ that the flanges 44L and 44R make with respect to the horizontal plane are L ,φ R and φ are preferably equal to or larger than −40° and equal to or smaller than 40°. L ,φ R is greater than or equal to -10° and less than or equal to 10°. More preferably, the angle φ L , angle φ R is substantially 0°. The angle φ L ,φ R The angle φ is the acute angle between the flanges 44L and 44R and the width direction in a cross section cut along a plane consisting of the vertical and width directions. L ,φ R Regarding the angle φ of the flanges 44L and 44R, the angle φ is positive when the flanges 44L and 44R rotate upward around the end of the vertical walls 43L and 43R (the R end (inside of the bend) of the corners 45L and 45R on the flanges 44L and 44R), and negative when the flanges 44L and 44R rotate downward. L , angle φ R may be equal or different from each other.

[0110] Length of flange 44L, 44R L L ,L R It is preferable that each of the lengths L is 10 mm or more. L ,L R are the lengths along the flanges 44L, 44R from the ends of the flanges 44L, 44R on the vertical walls 43L, 43R side (the R ends (inside the bend) of the corners 45L, 45R on the flanges 44L, 44R side) to the tips (free ends) of the flanges 44L, 44R.

[0111] Process (b) Referring again to FIG. 5A, in step (a), when the intermediate molded product 40 is placed on the punch 26, the die lower surfaces 274L, 274R face the flanges 44L, 44R, and the pad 28 faces the top plate 41 on the punch top surface 261. Referring to FIG. 5D, in step (b), the pad 28 is lowered to press the top plate 41 of the intermediate molded product 40 on the punch top surface 261 with the pad 28. Specifically, the slide 23 is lowered to lower the dies 27L, 27R and the pad 28 attached to the slide 23 toward the intermediate molded product 40. The pad 28 contacts the intermediate molded product 40 on the punch 26 prior to the dies 27L, 27R. The pad 28 presses the top plate 41 of the intermediate molded product 40 from above with the pad main body 281.

[0112] Process (c) 5E, after the top plate 41 of the intermediate molded product 40 is pressed by the pad body 281, the slide 23 further descends. At this time, the support member 282 supporting the pad body 281 contracts, causing the dies 27L, 27R to descend relatively to the pad body 281 in the state of pressing the top plate 41. In step (c), the dies 27L, 27R are thus lowered, and the dies 27L, 27R are brought into contact with the flanges 44L, 44R with the top plate 41 pressed by the pad 28.

[0113] Process (d) After the dies 27L and 27R come into contact with the flanges 44L and 44R of the intermediate molded product 40, the dies 27L and 27R further descend while the flanges 44L and 44R and their vicinity are hooked on the lower die shoulders 273L and 273R. That is, after the dies 27L and 27R come into contact with the flanges 44L and 44R of the intermediate molded product 40, the dies 27L and 27R further descend while still in contact with the flanges 44L and 44R. With reference to FIG. 5F, as the dies 27L and 27R descend, the upper die shoulders 271L and 271R or their vicinity come into contact with the protruding parts 42L and 42R and start to crush the protruding parts 42L and 42R. The protruding parts 42L and 42R are gradually crushed, for example, by the upper die shoulders 271L and 271R as well as the die upper surfaces 275L and 275R. When crushed, the protrusions 42L, 42R do not buckle locally, but the entire protrusions 42L, 42R conform to the punch 26. Thus, in step (d), after the dies 27L, 27R come into contact with the flanges 44L, 44R of the intermediate molded product 40, the dies 27L, 27R are further lowered to crush the protrusions 42L, 42R by the dies 27L, 27R. Meanwhile, the flanges 44L, 44R are gradually drawn toward the punch 26 as the dies 27L, 27R descend.

[0114] 5G, the dies 27L, 27R finally reach the bottom dead center, and the intermediate molded product 40 is pressed between the upper die shoulders 271L, 271R and the punch shoulders 262L, 262R, and between the die side surfaces 272L, 272R and the punch side surfaces 263L, 263R. The intermediate molded product 40 is also pressed between the pad body 281 and the punch top surface 261. In this way, the press-molded product 50 is manufactured.

[0115] When the dies 27L, 27R reach the bottom dead point, the flanges 44L, 44R of the intermediate product 40 are completely drawn toward the punch 26 and positioned between the die side surfaces 272L, 272R and the punch side surfaces 263L, 263R. However, it is preferable that the flanges 44L, 44R are in contact with the dies 27L, 27R until just before the dies 27L, 27R reach the bottom dead point. On the other hand, the protruding portions 42L, 42R of the intermediate product 40 are completely crushed by the dies 27L, 27R when the dies 27L, 27R reach the bottom dead point. At least a part of the protruding portions 42L, 42R is pressed between the upper die shoulders 271L, 271R and the punch shoulders 262L, 262R.

[0116] FIG. 5H is a perspective view partially showing the manufactured press-formed product 50. The press-formed product 50 has a top plate 51, left and right vertical walls 52L, 52R, and left and right bent portions 53L, 53R. A groove portion 51a extending in the longitudinal direction is formed in the top plate 51. The upper end of the left vertical wall 52L is connected to the left edge of the top plate 51 via the left bent portion 53L. The upper end of the right vertical wall 52R is connected to the right edge of the top plate 51 via the right bent portion 53R. The lower ends of the vertical walls 52L, 52R are each free ends. Each of the bent portions 53L, 53R is substantially arc-shaped in a cross-sectional view of the press-formed product 50.

[0117] [effect] In the manufacturing method according to the present embodiment, the metal plate 30 is press-formed into an intermediate product 40 in the first step, and then the intermediate product 40 is press-formed in the second step to obtain a press-formed product 50. In the second step, the dies 27L, 27R are brought into contact with the flanges 44L, 44R of the intermediate product 40 while the top plate 41 of the intermediate product 40 is pressed from above by the pad 28. The dies 27L, 27R are lowered while the flanges 44L, 44R are hooked on the lower die shoulders 273L, 273R. This allows tension to be applied to the intermediate product 40, which is a portion that is on the outer side in the width direction from the region pressed by the pad 28 and reaches the region that is in contact with the lower die shoulders 273L, 273R, that is, the portion that will become the bent portion 53L, 53R of the press-formed product 50. Therefore, the compressive stress on the inner side of the bend at the end of forming can be reduced in the bent portion 53L, 53R of the press-formed product 50. As a result, the tensile stress caused by springback is reduced, and the tensile stress remaining on the inner side of the bend in the bent portions 53L, 53R of the press-formed product 50 can be reduced.

[0118] In the manufacturing method according to the present embodiment, the protrusions 42L, 42R of the intermediate product 40 are crushed by the dies 27L, 27R in the second step and undergo bending back deformation. In the process in which the protrusions 42L, 42R are bent back by the dies 27L, 27R and pressed into the punch shoulders 262L, 262R, compressive stress occurs in the region of the protrusions 42L, 42R on the die 27L, 27R side (outside of the bend) and tensile stress occurs in the region of the punch 26 side (inside of the bend). These stresses can reduce the tensile stress occurring on the outside of the bend and the compressive stress occurring on the inside of the bend when the intermediate product 40 fits into the punch shoulders 262L, 262R to form the bent portions 53L, 53R. Therefore, the tensile stress remaining on the inside of the bend can be reduced in the bent portions 53L, 53R of the press-formed product 50 after springback.

[0119] It is difficult to flatten the convex portions 42L, 42R by only applying tension from the periphery to the convex portions 42L, 42R arranged at positions corresponding to the punch shoulders 262L, 262R. However, in the manufacturing method according to the present embodiment, the convex portions 42L, 42R are crushed from above by the dies 27L, 27R in the second step, so that the convex portions 42L, 42R can be flattened firmly. More specifically, the descending dies 27L, 27R hit the convex portions 42L, 42R and crush the convex portions 42L, 42R from the tops 421L, 421R. This generates a large stress from the bases 422L, 422R of the convex portions 42L, 42R toward the tops 421L, 421R. That is, a large tensile stress is generated in the region of the convex portions 42L, 42R on the punch 26 side (inside the bend). Therefore, the compressive stress generated on the inside of the bend at the end of the second process can be effectively reduced, and the tensile residual stress generated on the inside of the bend in the bent portions 53L, 53R of the press-formed product 50 after springback can be reduced.

[0120] In this manner, the dies 27L, 27R descend with the flanges 44L, 44R hooked on the lower die shoulders 273L, 273R, and hit the convex portions 42L, 42R while applying tension to the portions that will become the bent portions 53L, 53R of the press-formed product 50, and crush the convex portions 42L, 42R from the apexes 421L, 421R. This makes it possible to significantly reduce the compressive stress generated on the inner side of the bend at the end of the second step, and to significantly reduce the tensile residual stress generated on the inner side of the bend in the bent portions 53L, 53R of the press-formed product 50 after springback.

[0121] As described above, according to the manufacturing method of the press-formed product 50 according to this embodiment, the tensile residual stress generated on the inner side of the bent portions 53L, 53R of the press-formed product 50 can be reduced in the press working process.

[0122] The press working step is preferably performed using a simple press mechanism and a simple forming motion. The press working step using a simple press mechanism and a simple forming motion refers to a press working step that can be realized, for example, by using a single-action press device and substantially only by the movement of the upper die downward toward the lower die. In the manufacturing method according to this embodiment, a single-action press device 20 is used in the second step. The press device 20 substantially forms the press-formed product 50 from the intermediate product 40 only by the movement of simultaneously lowering the dies 27L, 27R and the pad 28 toward the punch 26. That is, in this embodiment, the press working step using a simple press mechanism and a simple forming motion can reduce the tensile residual stress generated on the inner side of the bent portions 53L, 53R of the press-formed product 50.

[0123] In the manufacturing method according to the present embodiment, when the intermediate product 40 is placed on the punch 26, that is, at the start of the second step, it is preferable that the upper ends of the convex parts 42L, 42R are located inside the lower ends of the die side surfaces 272L, 272R in the width direction of the die 21. This makes it possible to prevent the convex parts 42L, 42R from being crushed by the lower die shoulders 273L, 273R or the die lower surfaces 274L, 274R at the beginning of the second step. In other words, after tension is applied to the convex parts 42L, 42R by contact between the dies 27L, 27R and the flanges 44L, 44R, the convex parts 42L, 42R can be crushed by the dies 27L, 27R, and tensile stress can be generated more effectively in the region on the inner side of the bend. Therefore, in the bent parts 53L, 53R of the press-formed product 50, the compressive stress generated on the inner side of the bend at the end of the second step can be more reliably reduced, and the effect of reducing the tensile stress remaining on the inner side of the bend after springback can be improved.

[0124] In the manufacturing method according to this embodiment, when the intermediate molded product 40 is placed on the punch 26, the lower ends of the vertical walls 43L, 43R are positioned outside the upper ends of the punch side surfaces 263L, 263R in the width direction of the die 21. That is, the intermediate molded product 40 is fitted into the punch 26 without the top plate 41 floating up from the punch 26 at the start of the second step. Therefore, in the second step, when the top plate 41 of the intermediate molded product 40 is pressed by the pad 28, the pad 28 can be prevented from floating up, and molding can be performed stably. Therefore, the dimensional accuracy of the press-molded product 50 obtained in the second step can be stabilized.

[0125] At the protruding portion 42L of the intermediate molded product 40, the width W1 L Height H1 L Ratio of:H1 L / W1 L is preferably 0.5 or more and 2.0 or less. Similarly, in the protrusion 42R of the intermediate molded product 40, the width W1 R Height H1 R Ratio of:H1 R / W1 R is preferably 0.5 or more and 2.0 or less. Fig. 6 is a graph showing the relationship between the height H1 / width W1 and the tensile residual stress on the inner side of the bent portions 53L, 53R of the press-formed product 50. In Fig. 6, the width W1 of the protrusions 42L, 42R L ,W1 R and height H1 L ,H1 R are collectively referred to as width W1 and height H1. Fig. 6 and Figs. 7 to 13, which will be described later, show the results of a CAE analysis performed using commercially available software (LS-DYNA ver971 rev7.12, manufactured by ANSYS, Inc.) on press working for forming a press-formed product 50 having a bending R (inner curvature radius of bending) of bending parts 53L and 53R of 4.0 mm and a vertical wall height of 25 mm from a metal plate 30 having a tensile strength of 980 MPa and a plate thickness of 3.0 mm.

[0126] As shown in FIG. 6, when H1 / W1 is 0.5 or more, the tensile residual stress on the inner side of the bend is reduced by 100 MPa or more compared to the case where a conventional press working is performed without using the intermediate molded product 40. Therefore, H1 / W1 is preferably 0.5 or more. The tensile residual stress on the inner side of the bend is reduced as H1 / W1 increases. However, as H1 / W1 increases, the convex parts 42L, 42R rise more steeply from the top plate 41, so that there is a possibility that the convex parts 42L, 42R will buckle when the convex parts 42L, 42R are crushed by the dies 27L, 27R in the second step. In order to make the convex parts 42L, 42R less likely to buckle, it is preferable that H1 / W1 is 2.0 or less.

[0127] In this embodiment, the convex portions 42L, 42R of the intermediate product 40 each include a top portion 421L, 421R that is substantially arc-shaped in cross section. The radius of curvature of each of the top portions 421L, 421R is preferably 4 mm or more and 16 mm or less. The radius of curvature here refers to the value on the inside (the punch 16 side) of the convex portions 42L, 42R. FIG. 7 is a graph showing the relationship between the radius of curvature of the top portions 421L, 421R and the tensile residual stress on the inside of the bent portions 53L, 53R of the press-formed product 50.

[0128] As can be seen from FIG. 7, if the radius of curvature of the apexes 421L, 421R is 16 mm or less, the tensile residual stress on the inner side of the bend is reduced by 100 MPa or more compared to when a conventional press working is performed without using the intermediate molded product 40. Therefore, the radius of curvature of the apexes 421L, 421R is preferably 16 mm or less. The tensile residual stress on the inner side of the bend is reduced as the radius of curvature of the apexes 421L, 421R becomes smaller. However, the radius of curvature of the apexes 421L, 421R is preferably 4 mm or more. This is to make it difficult for the buckling of the apexes 42L, 42R to occur when the dies 27L, 27R crush the apexes 42L, 42R in the second step.

[0129] In this embodiment, when the intermediate molded product 40 is placed on the punch 26, that is, at the start of the second process, it is preferable that each distance D2 [mm] in the width direction of the mold 21 from the end of the punch shoulders 262L, 262R on the punch top surface 261 side to the upper ends of the convex portions 42L, 42R is set so as to satisfy the following formula (1). -1.0×Rp×(π-θ)≦D2≦2.5×Rp×(π-θ)···(1)

[0130] By setting the distance D2 in this manner, the protrusions 42L, 42R are likely to overlap in the range of the punch shoulders 262L, 262R in the width direction of the die 21. Therefore, the stress caused by the bending back deformation of the protrusions 42L, 42R can be generated widely in the region of the punch shoulders 262L, 262R. Therefore, the compressive stress generated on the inner side of the bend when the intermediate molded product 40 fits into the punch shoulders 262L, 262R to form the bent portions 53L, 53R can be more effectively reduced. As a result, the tensile residual stress generated on the inner side of the bend in the bent portions 53L, 53R of the press-molded product 50 can be more reliably reduced.

[0131] In this embodiment, the height H2 of the intermediate product 40 is preferably 6 mm or more. Fig. 8 is a graph showing the relationship between the height H2 of the intermediate product 40 and the tensile residual stress on the inner side of the bent portions 53L, 53R of the press-formed product 50.

[0132] As shown in Fig. 8, the tensile residual stress on the inner side of the bend is reduced as the height H2 of the intermediate molded product 40 increases, compared to when a conventional press working is performed without using the intermediate molded product 40. In particular, if the height H2 of the intermediate molded product 40 is 6 mm or more, the tensile residual stress on the inner side of the bend is reduced by 200 MPa or more, and a significant residual stress reduction effect is exhibited. This is because the height H2 of the intermediate molded product 40 is sufficiently secured, and when the dies 27L, 27R in contact with the flanges 44L, 44R descend in the second step, the vertical walls 43L, 43R are prevented from bending, and the flanges 44L, 44R are formed while being firmly caught by the lower die shoulders 273L, 273R, so that tension can be applied to the intermediate molded product 40 more effectively.

[0133] In this embodiment, the height H2 of the intermediate molded product 40 is defined as the vertical distance from the ends of the flanges 44L, 44R on the vertical walls 43L, 43R side to the top plate 41. When the vertical distance from the center of thickness of the end of the flange 44L on the vertical wall 43L side to the center of thickness of the top plate 41 at the connection with the protrusion 42L is different from the vertical distance from the center of thickness of the end of the flange 44R on the vertical wall 43R side to the center of thickness of the top plate 41 at the connection with the protrusion 42R, the smaller of the two distances is the height H2. However, it is preferable that the two distances are substantially equal.

[0134] For example, in the intermediate product 40, if the vertical distance on the flange 44L side is long, that is, in the die 11 in the first step, if the left punch side surface 163L is higher than the right punch side surface 163R, the die flange surface 174L contacts the metal sheet 30 before the die flange surface 174R when the metal sheet 30 is pressed. Therefore, the metal sheet 30 may move into the space between the punch flange surface 164L and the die flange surface 174L, which may prevent stable press working. On the other hand, if the height of the left punch side surface 163L is substantially equal to the height of the right punch side surface 163R, the metal sheet 30 is less likely to move, and stable press working can be achieved in the first step.

[0135] In this embodiment, when the intermediate product 40 is placed on the punch 26, that is, at the start of the second step, the angles φ L ,φ R is preferably -40° or more and 40° or less. Fig. 9 is a graph showing the relationship between the angle φ and the tensile residual stress on the inner side of the bent portions 53L, 53R of the press-formed product 50. In Fig. 9, the angle φ of the flanges 44L, 44R L ,φ R are collectively expressed as angle φ.

[0136] As shown in FIG. 9, when the angle φ of the flanges 44L, 44R is −40° or more, the tensile residual stress on the inner side of the bend is reduced by 100 MPa or more compared to when a conventional press working is performed without using the intermediate molded product 40. Therefore, the angle φ is preferably −40° or more. The tensile residual stress on the inner side of the bend is reduced as the angle φ increases. However, if the angle φ is too large, in the second step, the tip of the flange 44L, 44R, which is the free end, may contact the die 27L, 27R instead of the surface of the flange 44L, 44R, and the flange 44L, 44R may buckle. In addition, when the flange 44L, 44R contacts the die 27L, 27R at its tip, the contact surface pressure of the flange 44L, 44R against the die 27L, 27R may increase, and the die 27L, 27R may be damaged. Therefore, the angle φ of the flanges 44L, 44R is preferably 40° or less. More preferably, the angle φ of the flanges 44L, 44R is equal to or larger than −10° and equal to or smaller than 10°.

[0137] In this embodiment, the length L of the flanges 44L and 44R of the intermediate molded product 40 is L ,L R 10 is a graph showing the relationship between the length L and the tensile residual stress on the inner side of the bent portions 53L and 53R of the press-formed product 50. In FIG. 10, the length L of the flanges 44L and 44R is L ,L R are collectively expressed as length L.

[0138] As shown in FIG. 10, if the length L of the flanges 44L, 44R is 10 mm or more, the tensile residual stress on the inner side of the bend is reduced by 100 MPa or more compared to the case of performing a conventional press working without using the intermediate molded product 40. This is because the length L of the flanges 44L, 44R is sufficiently secured, so that the flanges 44L, 44R are easily caught by the lower die shoulders 273L, 273R until the later stage of forming in the second step, and tension is more effectively applied to the protrusions 42L, 42R and the vertical walls 43L, 43R. The tensile residual stress on the inner side of the bend is reduced as the length L of the flanges 44L, 44R is larger. Therefore, it is preferable that the length L of the flanges 44L, 44R is 10 mm or more.

[0139] Regarding the mold 21 used in the second step of the manufacturing method according to this embodiment, the lower die shoulders 273L and 273R have a curvature radius Rd of 1 mm or more and 12 mm or less in a cross-sectional view of the dies 27L and 27R. L ,Rd R 11 is a graph showing the relationship between the radius of curvature Rd and the tensile residual stress on the inner side of the bent portions 53L and 53R of the press-formed product 50. In FIG. 11, the radius of curvature Rd of the lower die shoulders 273L and 273R is L ,Rd R are collectively referred to as the radius of curvature Rd.

[0140] As shown in FIG. 11, when the radius of curvature Rd of the lower die shoulders 273L, 273R is 12 mm or less, the tensile residual stress on the inner side of the bend is significantly reduced compared to when a conventional press working is performed without using the intermediate molded product 40. Therefore, the radius of curvature Rd is preferably 12 mm or less. The tensile residual stress on the inner side of the bend is reduced as the radius of curvature Rd is smaller. However, when the radius of curvature Rd is less than 1 mm, the lower die shoulders 273L, 273R may leave a bite mark on the press-formed product 50 or may cause a large bending tendency in the press-formed product 50. Therefore, the radius of curvature Rd of the lower die shoulders 273L, 273R is preferably 1 mm or more.

[0141] In this embodiment, when the intermediate product 40 is placed on the punch 26, that is, at the start of the second step, each of the convex portions 42L, 42R is preferably located outside the pad profile P in the width direction of the die 21. Fig. 12 is a graph showing the relationship between the positions of the convex portions 42L, 42R with respect to the pad profile P and the tensile residual stress on the inner side of the bend in the bent portions 53L, 53R of the press-molded product 50.

[0142] As shown in FIG. 12, when a part of the convex parts 42L, 42R is located on the inner side of the pad profile P in the width direction and interferes with the pad body 281, the effect of reducing the tensile residual stress on the inner side of the bend is smaller than when the convex parts 42L, 42R are located on the outer side of the pad profile P in the width direction and do not interfere with the pad body 281. Furthermore, when a part of the convex parts 42L, 42R is located on the inner side of the pad profile P in the width direction and interferes with the pad body 281, the outer periphery of the pad body 281 may be stuck into the convex parts 42L, 42R, causing scratches on the press-molded product 50. Therefore, it is preferable that the entire convex parts 42L, 42R are located on the outer side of the pad profile P in the width direction so that the convex parts 42L, 42R do not interfere with the pad body 281 at the start of the second step. However, as can be seen from Figure 12, when the intermediate molded product 40 is used to obtain the press-molded product 50, even if the convex portions 42L, 42R interfere with a part of the pad main body 281, the tensile residual stress on the inside of the bend can be significantly reduced compared to conventional press processing that does not use the intermediate molded product 40.

[0143] The residual stress of the press-formed product 50 is the sum of the stress at the end of the forming of the press-formed product 50 and the reversal stress due to springback when the press-formed product 50 is released from the mold. If the stress generated in the material during forming is small, the stress due to springback is also small, and the residual stress of the press-formed product 50 is reduced. Therefore, in the manufacturing method according to this embodiment, a metal plate 30 having a work hardening index of 0.04 or less is preferably used as the material of the press-formed product 50. If the work hardening index of the material is 0.04 or less, work hardening is unlikely to occur in the first and second steps, and the stress generated in the press-formed product 50 at the end of forming is also small. Therefore, the residual stress of the press-formed product 50 can be reduced.

[0144] Fig. 13 is a graph showing the relationship between the work hardening exponent (n value) of the metal plate 30 and the tensile residual stress on the inner side of the bend in the bent parts 53L, 53R of the press-formed product 50. As shown in Fig. 13, when the press-formed product 50 is obtained using the intermediate formed product 40, the tensile residual stress on the inner side of the bend can be reduced compared to conventional press working that does not use the intermediate formed product 40. However, when the n value of the metal plate 30 is 0.04, the tensile residual stress on the inner side of the bend can be reduced more significantly than when the n value of the metal plate 30 is 0.08. Therefore, the n value of the metal plate 30 is preferably 0.04 or less.

[0145] For example, when a press-formed product is manufactured from a metal plate material by drawing, the end of the material in the width direction is clamped between a die having a horizontal lower surface and a holder having a horizontal upper surface from the beginning of forming. In this case, tension is applied to the material from the beginning of forming. However, in drawing, the end of the material is clamped between the die and the holder even at the end of forming. Therefore, the press-formed product manufactured has a shape having a top plate, vertical walls connected to the left and right side edges of the top plate, and flanges protruding outward in the width direction from the lower ends of each vertical wall, that is, an approximately hat shape in cross section. In order to manufacture a press-formed product without a flange using drawing, it is necessary to once form the material into an approximately hat shape using a punch, a die, and a holder, and then trim the material after forming with the left and right vertical walls. However, since trimming of the material is generally performed parallel to the plate thickness direction, for example, when trimming left and right vertical walls that are inclined with respect to a vertical plane, a trimming blade of a pull-out type equipped with a complex cam mechanism or the like is required. In this case, problems occur such as an increase in the number of steps required to design the trim blade, an increase in the manufacturing cost of the trim blade, etc. Also, there is a problem that the yield of material decreases due to trimming the vertical wall.

[0146] On the other hand, in this embodiment, although the flanges 44L, 44R of the intermediate product 40 contact the dies 27L, 27R during the second step, when the dies 27L, 27R reach the bottom dead center, they are completely drawn toward the punch 26 and pressed between the die side surfaces 272L, 272R and the punch side surfaces 263L, 263R. Therefore, it is possible to directly mold the press-formed product 50 without a flange without performing trimming. Therefore, there is no need for the design man-hours and manufacturing costs of trimming blades as in the case of using drawing, and a decrease in material yield can be prevented.

[0147] In general press working, the positional deviation of the material may be a problem. For example, when the heights of the left and right punch sides are different, the die with the larger height of the punch side of the left and right dies contacts the material first, which is likely to cause the material to be misaligned. When the material is positioned using a pilot pin or the like, if the material is misaligned, the peripheral portion of the hole for the pilot pin in the material is deformed. On the other hand, in this embodiment, in the second step, the pad 28 (the lower surface of the pad body 281) presses the top plate 41 of the intermediate molded product 40, and then the dies 27L and 27R are brought into contact with the intermediate molded product 40. Therefore, it is possible to prevent the intermediate molded product 40 from being misaligned during press working. Therefore, the press-molded product 50 can be manufactured with high precision.

[0148] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments, and various modifications are possible without departing from the spirit of the present disclosure.

[0149] In the above embodiment, the metal plate 30 is formed into the intermediate product 40 in the first step, and then in the second step, the intermediate product 40 is used as is and formed into the press-formed product 50. However, one or more intermediate steps can be provided between the first step and the second step. That is, the intermediate product 40 can be processed after the first step, and the processed intermediate product 40 can be provided to the second step.

[0150] For example, between the first and second steps, one or more through holes can be formed in the top plate 41 of the intermediate molded product 40. The through holes may be simply round holes, or may be holes (burring holes) formed by burring with protruding hole edges.

[0151] 14, for example, the intermediate product 40 obtained in the first step can be processed to change the shapes of the vertical walls 43L, 43R and the flanges 44L, 44R while maintaining the shapes of the top plate 41 and the protrusions 42L, 42R. The intermediate product 40 processed in the intermediate step between the first and second steps is molded into a press-molded product 50 in the second step, similar to the above embodiment.

[0152] Fig. 15 is a graph showing the relationship between the presence or absence of an intermediate step and the tensile residual stress on the inner side of the bend in the bent parts 53L, 53R of the press-formed product 50. Fig. 15 shows the results obtained when a CAE analysis was performed using the above-mentioned commercially available software on a press process for forming a press-formed product 50 having a bend R (curvature radius on the inner side of the bend) of the bent parts 53L, 53R of 4.0 mm and a vertical wall height of 25 mm from a metal plate 30 having a tensile strength of 980 MPa and a plate thickness of 3.0 mm. In the intermediate step, the vertical walls 43L, 43R and flanges 44L, 44R were processed as shown in Fig. 14 while maintaining the shapes of the top plate 41 and the convex parts 42L, 42R, and were formed into a shape between the intermediate product 40 obtained in the first step and the press-formed product 50 obtained in the second step.

[0153] As can be seen from Figure 15, regardless of whether there is an intermediate step between the first and second steps, by subjecting the intermediate molded product 40 including the convex portions 42L, 42R and the flanges 44L, 44R to the second step, the tensile residual stress on the inside of the bend can be reduced compared to conventional press processing.

[0154] In the above embodiment, an example has been described in which the intermediate product 40 is press-formed by the die 11 composed of the punch 16 and the die 17. That is, in the above embodiment, the intermediate product 40 is formed from the metal plate 30 by so-called stamping in the first step. However, the method of obtaining the intermediate product 40 is not limited to this. For example, the intermediate product 40 can be obtained by pad bending forming in which the top plate 41 is pressed with a pad while being formed, or by drawing forming in which the flanges 44L, 44R are pressed with a holder. The configuration of the die 11 for forming the intermediate product 40 can be appropriately selected.

[0155] In the above embodiment, an example has been described in which the press device 10 including the die 11 is used in the first step, and the press device 20 including the die 21 and separate from the press device 10 is used in the second step. However, the die 11 for the first step and the die 21 for the second step may be installed in one press device. For example, the first step and the second step can be performed by a transfer type press device provided with both the dies 11 and 21.

[0156] In the above embodiment, the intermediate product 40 includes the left and right convex portions 42L, 42R. However, the intermediate product 40 may include only one of the left and right convex portions 42L, 42R. That is, one of the left and right bent portions 53L, 53R of the press-formed product 50 can be formed while applying tension due to bending back deformation of the convex portion, and the other can be formed without applying tension due to bending back deformation of the convex portion. For example, when it is necessary to reduce the tensile residual stress on the inner side of the bend and obtain excellent fatigue characteristics in one of the left and right bent portions 53L, 53R of the press-formed product 50, while excellent fatigue characteristics are not necessary in the other, tension due to bending back deformation of the convex portion may be applied only to the side requiring excellent fatigue characteristics.

[0157] Similarly, the intermediate product 40 may include only one of the left and right flanges 44L, 44R. That is, in the second step, one of the left and right bent portions 53L, 53R of the press-formed product 50 can be formed while applying tension by hooking the flange on the lower die shoulder, and the other can be formed without applying such tension. For example, when it is necessary to reduce the tensile residual stress on the inner side of the bend and obtain excellent fatigue properties in one of the left and right bent portions 53L, 53R of the press-formed product 50, while excellent fatigue properties are not necessary in the other, tension by the flange can be applied only to the side requiring excellent fatigue properties.

[0158] In the above embodiment, the convex portions 42L, 42R of the intermediate molded product 40 have the apexes 421L, 421R that are entirely arc-shaped, respectively. However, the apexes 421L, 421R do not necessarily have to be entirely arc-shaped. For example, the apexes 421L, 421R may have flat portions extending outward in the width direction in a cross-sectional view of the intermediate molded product 40 so that the convex portions 42L, 42R have a wide shape.

[0159] In the above embodiment, the punches 16, 26 used in each step have grooves 161a, 261a formed on the punch top surfaces 161, 261. However, the punch top surfaces 161, 261 may have steps instead of the grooves 161a, 261a. The steps may extend over the entire punch top surfaces 161, 261 in the longitudinal direction, or may be provided on a portion of the punch top surfaces 161, 261. When the punch top surfaces 161, 261 have steps, corresponding steps are also provided on the bottom surface 171 of the die 17 used in the first step and on the lower surface of the pad 28 used in the second step. When the punch top surface 161 has steps, the top plate 41 of the intermediate molded product 40 has steps corresponding to the steps on the punch top surface 161. When a step is provided on the punch top surface 261, a step corresponding to the step on the punch top surface 261 is formed on the top plate 51 of the press-formed product 50.

[0160] However, the punch top surfaces 161, 261, the top plate 41 of the intermediate product 40, and the top plate 51 of the press-molded product 50 do not have to have a groove or a step. In other words, the punch top surfaces 161, 261, the top plate 41 of the intermediate product 40, and the top plate 51 of the press-molded product 50 may have a flat shape as a whole.

[0161] The overall shape of the press-molded product 50 can be appropriately selected according to the purpose of use, etc. For example, the press-molded product 50 may be linear when viewed from the top plate 51 side (in a plan view), may be curved to the left or right, or may be curved up or down (curved when viewed from the width direction). The press-molded product 50 may have a shape that combines two or more types of straight parts and curved parts when viewed from the width direction. Furthermore, the press-molded product 50 may have a shape in which a part having a roughly U-shaped cross section branches into multiple parts, such as a three-pronged shape or a four-pronged shape. The shapes of the first-step mold 11 and the second-step mold 21 can be selected according to the final shape of the press-molded product 50.

[0162] The press-molded product 50 does not need to have a uniform cross-sectional shape over its entirety. As long as the press-molded product has at least a part of a generally U-shaped cross section, the press device and manufacturing method according to each of the above embodiments can be applied. EXAMPLES

[0163] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to the following examples.

[0164] In order to confirm the effect of the present disclosure, a CAE analysis was performed on the press processing for forming a metal plate (steel plate) having a tensile strength TS of 980 MPa and a plate thickness t of 3.0 mm into a press-formed product 60 shown in FIG. 16 by the manufacturing method according to the above embodiment. The press-formed product 60 has a top plate 61, left and right vertical walls 62, and left and right bending portions 63. A groove portion 61a is formed in the top plate 61. The lower end of each vertical wall 62 is a free end. In other words, no flange is provided at the lower end of each vertical wall 62. The width of the top plate 61 is 80.0 mm, and the height of the vertical wall 62 is 25.0 mm. In addition, the bending R (curvature radius of the bending inner side) of the bending portion 63 is 4.0 mm. The press-formed product 60 is curved in a plan view. The bending R of the bending inner side of the press-formed product 60 is 250.0 mm. The curvature R of the outer curve is 36.0 mm, obtained by adding the curvature R of the inner curve to the width of the top plate 61. Note that these dimensions are the dimensions on the inside of the press-formed product 60 (the surface on the inner side of the bend of the bent portion 63).

[0165] In the CAE analysis, commercially available software (LS-DYNA ver971 rev7.12, manufactured by ANSYS) was used to perform forming analysis and springback analysis to evaluate the maximum value of the residual stress (maximum principal stress) on the inner surface of the bent section 63 as the residual stress on the inner side of the bend. If the residual stress value is positive, it is tensile, and if it is negative, it is compressive. In the CAE analysis, of the elements divided in the plate thickness direction, the value of the element on the inner surface of the bend was used as the value of the inner surface of the bend. The results of the analysis are shown in Table 1.

[0166] [Table 1]

[0167] No. 1 in Table 1 is a result (comparative example) when a press-formed product 60 was formed by general pad bending. That is, in No. 1, the press-formed product 60 was formed from a metal plate as a material using a die consisting of a punch, a die, and a pad, without forming an intermediate product 40 as described in the above embodiment. In No. 1, after the press forming was completed and springback occurred, a residual stress of 580 MPa occurred on the surface inside the bend of the bent part 63 of the press-formed product 60.

[0168] Nos. 2 to 27 in Table 1 are results when a press-formed product 60 was formed by the method according to the present disclosure. That is, in Nos. 2 to 27, first, an intermediate product similar to the intermediate product 40 described in the above embodiment was formed (first step), and this intermediate product was pad-bent to form the press-formed product 60 (second step). In the second step, at the start of forming, the upper ends of the convex parts of the intermediate product were positioned widthwise inward from the lower ends of the die side surfaces, and the lower ends of the vertical walls of the intermediate product were positioned widthwise outward from the upper ends of the punch side surfaces.

[0169] As shown in Table 1, most of Nos. 2 to 27 had reduced residual stress on the inner surface of the bent portion 63 of the press-formed product 60 compared to the comparative example No. 1. In particular, Nos. 2 to 15 had reduced residual stress by 100 MPa or more compared to the comparative example No. 1. Thus, according to the method of the present disclosure, the tensile stress remaining on the inner surface of the bent portion 63 of the press-formed product 60 can be reduced.

[0170] [Work hardening index (n value)] In No. 15, in which the work hardening exponent (n value) of the raw metal plate was as low as 0.04, the residual stress on the inner surface of the bent portion 63 of the press-formed product 60 was significantly smaller than that in No. 2, in which the raw material n value was 0.09. Therefore, it can be said that the use of a metal plate having an n value of 0.04 or less improves the effect of reducing tensile residual stress.

[0171] [Dimensions of protruding parts] (Height H1 / Width W1) In No. 16, the ratio of height H1 to width W1: H1 / W1 is 0.4 in the convex portion of the intermediate molded product molded in the first step. In this No. 16, the residual stress on the inner surface of the bent portion 63 of the press-molded product 60 was 531 MPa, and the effect of reducing the tensile residual stress was relatively small compared to the comparative example No. 1. On the other hand, in No. 4, in which H1 / W1 was 0.5, the residual stress was 463 MPa, and a high effect of reducing the tensile residual stress was obtained. Therefore, in order to further improve the effect of reducing the tensile residual stress, it is preferable that H1 / W1 is 0.5 or more. Moreover, from the results of No. 16 and No. 4, it is preferable that the height H1 of the convex portion is 5 mm or more.

[0172] In No. 17, where H1 / W1 was 2.1, buckling of the convex portion of the intermediate molded product occurred when the convex portion was crushed by the die in the second step. On the other hand, in No. 3, where H1 / W1 was 2.0, buckling of the convex portion did not occur. Therefore, in order to suppress buckling of the convex portion, it is preferable that H1 / W1 is 2.0 or less. Also, based on the results of No. 17 and No. 3, it is preferable that the height H1 of the convex portion is 25 mm or less.

[0173] (Apex curvature radius) In No. 18, the bending radius (inner radius of curvature of the bending) of the top of the convex part of the intermediate molded product formed in the first step is 2 mm. In this No. 18, buckling of the convex part occurred when the convex part was crushed by the die in the second step. On the other hand, in No. 5, in which the bending radius of the top of the convex part is 4 mm, buckling of the convex part did not occur, and the residual stress was also significantly reduced compared to No. 1, which is a comparative example. Therefore, in order to obtain a high reduction effect of the tensile residual stress without causing buckling of the convex part, it is preferable that the bending radius of the top of the convex part is 4 mm or more.

[0174] In No. 19, in which the bending radius of the top of the convex portion was 20 mm, the residual stress on the inner surface of the bent portion 63 of the press-formed product 60 was 509 MPa, and the effect of reducing the tensile residual stress was relatively small compared to the comparative example No. 1. On the other hand, in No. 6, in which the bending radius of the top of the convex portion was 16 mm, the residual stress was 396 MPa, which was reduced by nearly 200 MPa compared to No. 1. From these results, in order to further improve the effect of reducing the tensile residual stress, it is preferable that the bending radius of the top of the convex portion is 16 mm or less.

[0175] (flange length) In No. 20, the flange length L of the intermediate product formed in the first step is 8 mm. In this No. 20, the residual stress on the inner surface of the bent portion 63 of the press-formed product 60 was 537 MPa, and the effect of reducing the tensile residual stress was relatively small compared to the comparative example No. 1. On the other hand, in No. 7, in which the flange length L was 10 mm, the residual stress was 415 MPa, which was reduced by 100 MPa or more compared to No. 1. Therefore, in order to further improve the effect of reducing the tensile residual stress, it is preferable that the flange length L is 10 mm or more.

[0176] [Molding height of intermediate molded product] In No. 21, the height H2 of the intermediate molded product molded in the first step is 4 mm. In this No. 21, the residual stress on the inner surface of the bent portion 63 of the press-molded product 60 was 529 MPa, and the effect of reducing the tensile residual stress was relatively small compared to the comparative example No. 1. On the other hand, in No. 8, in which the height H2 of the intermediate molded product was 6 mm, the residual stress was 391 MPa, which was significantly reduced compared to No. 1. Therefore, in order to further improve the effect of reducing the tensile residual stress, it is preferable that the height H2 of the intermediate molded product is 6 mm or more.

[0177] [Relationship between intermediate molded product and second process mold] (Relative position of the protrusion to the die) At the start of the second step, when the intermediate molded product is placed in the mold, the distance D2 [mm] in the width direction of the mold from the R end of the punch top side of the punch shoulder to the top end of the convex part can be set in relation to the radius of curvature Rp [mm] of the punch shoulder and the angle θ [rad] of the punch side relative to the punch top. In No. 22, in which D2 / (Rp×(π-θ)) was set to -1.2, the residual stress on the inner surface of the bent part 63 of the press-molded product 60 was 503 MPa, and the effect of reducing the tensile residual stress was relatively small compared to No. 1, which is a comparative example. In No. 23, in which D2 / (Rp×(π-θ)) was set to 2.7, the residual stress was 543 MPa, and the effect of reducing the tensile residual stress was relatively low. On the other hand, in No. 9, in which D2 / (Rp×(π-θ)) was set to -1.0, and in No. 10, in which D2 / (Rp×(π-θ)) was set to 2.5, the residual stress was 341 MPa and 451 MPa, respectively, which was a reduction of 100 MPa or more compared to No. 1. From this result, in order to further improve the effect of reducing the tensile residual stress, it is preferable to set the distance D2 to be -1.0×Rp×(π-θ) or more and 2.5×Rp×(π-θ) or less.

[0178] (Flange angle) In No. 24, the angle φ of the flange of the intermediate product with respect to the horizontal plane is -45° at the start of the second step. That is, the flange of the intermediate product is rotated 45° downward around the end of the vertical wall side. In this No. 24, the residual stress on the inner surface of the bent portion 63 of the press-formed product 60 is 524 MPa, and the effect of reducing the tensile residual stress is relatively small compared to the comparative example No. 1. On the other hand, in No. 11, in which the flange angle φ is -40°, the residual stress is 463 MPa, which is reduced by 100 MPa or more compared to No. 1. Therefore, in order to further improve the effect of reducing the tensile residual stress, it is preferable that the flange angle φ of the intermediate product at the start of the second step is -40° or more.

[0179] In No. 25, the angle φ of the flange of the intermediate molded product with respect to the horizontal plane is 45° at the start of the second step. That is, the flange of the intermediate molded product rotates 45° upward around the end on the vertical wall side. In this No. 25, the tip (free end) of the flange of the intermediate molded product comes into contact with the die and buckles in the second step. In addition, in the case of No. 25, the tip of the flange is likely to rub against the die, which may cause damage to the die. On the other hand, in No. 12, in which the flange angle φ is 40°, the flange did not buckle, and the residual stress was significantly reduced compared to No. 1, which is a comparative example. Therefore, in order to obtain a high reduction effect of tensile residual stress without causing flange buckling, it is preferable that the flange angle φ is 40° or less.

[0180] (radius of curvature of lower die shoulder) In No. 26, the radius of curvature of the lower die shoulder (die shoulder Rd) in the die used in the second step was set to 0.5 mm. The lower die shoulder is the part on which the flange of the intermediate product is caught when the die is lowered in the second step. In No. 26, the lower die shoulder caused a large bending tendency in the press-formed product 60 in the second step. On the other hand, in No. 13, in which the die shoulder Rd was set to 1 mm, the press-formed product 60 did not substantially have a bending tendency, and the residual stress on the inner surface of the bent portion 63 of the press-formed product 60 was also significantly reduced compared to No. 1, which is a comparative example. Therefore, in order to obtain a high reduction effect of the tensile residual stress without causing a bending tendency, it is preferable that the die shoulder Rd is 1 mm or more.

[0181] In No. 27, in which the die shoulder Rd was 15 mm, the residual stress was 513 MPa, and the effect of reducing the tensile residual stress was relatively small compared to the comparative example No. 1. On the other hand, in No. 14, in which the die shoulder Rd was 12 mm, the residual stress was 438 MPa, which was reduced by more than 100 MPa compared to No. 1. Therefore, in order to improve the effect of reducing the tensile residual stress, it is preferable that the die shoulder Rd in the second process is 12 mm or less. [Explanation of symbols]

[0182] 100: Manufacturing equipment 11: Mold (first mold) 21: Mold (second mold) 26: Punch 261: Punch top surface 262L, 262R: Punch shoulder 263L, 263R: Punch side 27L, 27R: Die 271L, 271R: Upper die shoulder 272L, 272R: Die side 273L, 273R: Lower die shoulder 274L, 274R: Die bottom surface 28: Pad 30: Metal plate 40: Intermediate molded product 41: Tabletop 42L, 42R: Convex 421L,421R:Top 43L, 43R: Vertical wall 44L, 44R: Flange 50: Press-molded products

Claims

1. A method for manufacturing a press-molded product, comprising the steps of: A first step of obtaining an intermediate molded product by pressing a metal plate, the intermediate molded product including a top plate, a protrusion connected to the top plate and protruding upward from the top plate, a vertical wall extending downward from the protrusion, and a flange extending from a lower end of the vertical wall to an opposite side of the top plate; a second step of pressing the intermediate product using a die including a punch, a pad disposed above the punch so as to face the punch, and a die disposed above the punch and to the side of the pad to obtain the press-molded product; Equipped with The punch includes a punch top surface, a punch shoulder continuous with the punch top surface, and a punch side surface extending downward from the punch shoulder, The die includes an upper die shoulder corresponding to the punch shoulder, a die side surface extending downward from the upper die shoulder corresponding to the punch side surface, and a die lower surface connected to a lower end of the die side surface via a lower die shoulder, The second step comprises: placing the intermediate product on the punch such that the top plate is disposed on the top surface of the punch and the protrusion is disposed at a position corresponding to the punch shoulder; a step of lowering the pad and pressing the top plate on the top surface of the punch with the pad; a step of lowering the die and bringing the die into contact with the flange while the top plate is pressed by the pad; a step of further lowering the die after the die has come into contact with the flange, and crushing the protrusion with the die; A manufacturing method comprising:

2. The method according to claim 1, a manufacturing method in which, when the intermediate molded product is placed on the punch, an upper end of the convex portion is positioned more inward than a lower end of the die side surface in the width direction of the mold, and a lower end of the vertical wall is positioned more outward than an upper end of the punch side surface in the width direction of the mold.

3. The method according to claim 1 or 2, A manufacturing method in which, when the vertical distance from the connection between the convex portion and the top plate to the upper end of the convex portion is H1 [mm], and the widthwise distance of the intermediate molded product from the connection to the upper end is W1 [mm], H1 / W1 is 0.5 or more and 2.0 or less.

4. The method according to any one of claims 1 to 3, The convex portion has an arc shape in a cross-sectional view of the intermediate molded product and includes an apex having a radius of curvature of 4 mm or more and 16 mm or less.

5. The method according to any one of claims 1 to 4, The punch shoulder has an arc shape in a cross-sectional view of the punch, a manufacturing method in which, when the intermediate molded product is placed on the punch, a distance D2 [mm] in the width direction of the die from the end of the punch shoulder on the punch top surface side to the upper end of the convex portion satisfies the following formula, where the distance D2 [mm] is positive when the upper end is located outer than the end of the punch shoulder in the width direction and is negative when the upper end is located inner in the width direction. -1.0×Rp×(π-θ)≦D2≦2.5×Rp×(π-θ) Here, Rp is the radius of curvature of the punch shoulder (mm), and θ is the angle (rad) between the punch top surface and the punch side surface.

6. The method according to any one of claims 1 to 5, A manufacturing method in which, in the intermediate molded product, the vertical distance from the end of the flange on the vertical wall side to the top plate is 6 mm or more.

7. The method according to any one of claims 1 to 6, when the intermediate molded product is placed on the punch, the angle that the flange forms with respect to the horizontal plane is positive when the flange is rotated upward around the end of the vertical wall, and negative when the flange is rotated downward, and is greater than -40° and less than 40°.

8. The method according to any one of claims 1 to 7, The method of claim 1, wherein the lower die shoulder is arcuate in shape having a radius of curvature of 1 mm or more and 12 mm or less when viewed in cross section of the die.

9. The method according to any one of claims 1 to 8, The manufacturing method, wherein the metal plate has a work hardening coefficient of 0.04 or less.

10. A manufacturing facility for manufacturing a press-molded product, a first mold for molding a metal plate into an intermediate molded product including a top plate, a protrusion connected to the top plate and protruding upward from the top plate, a vertical wall extending downward from the protrusion, and a flange extending from a lower end of the vertical wall to an opposite side of the top plate; A second mold for molding the intermediate molded product into the press-molded product; Equipped with The second mold is a punch including a punch top surface, a punch shoulder continuous with the punch top surface, and a punch side surface extending downward from the punch shoulder, wherein when the intermediate formed product is formed into the press-formed product, the top plate is disposed on the punch top surface and the protrusion is disposed at a position corresponding to the punch shoulder; a pad that is arranged above the punch and can be raised and lowered, the pad facing the top plate that is arranged on a top surface of the punch when the intermediate molded product is molded into the press-molded product; a die that can be raised and lowered and is disposed above the punch and to the side of the pad, the die including an upper die shoulder corresponding to the punch shoulder, a die side surface that extends downward from the upper die shoulder corresponding to the punch side surface, and a die lower surface that is connected to a lower end of the die side surface via a lower die shoulder, the die lower surface facing the flange when the intermediate molded product is molded into the press-molded product; Manufacturing facilities, including

Citation Information

Patent Citations

  • Method of manufacturing bent article with excellent fatigue property, and bent article

    JP2002316215A

  • Hat type formed component excellent in shape fixability and mold for press forming

    JP2004314123A

  • Press formed article of metallic sheet, and press working method and press die for metallic sheet

    JP2006272378A

  • Method of press-forming press-formed component excellent in shape freezing property

    JP2009262168A

  • Method and apparatus for forming tailored blank plate

    JP2011025263A