Titanium sponge manufacturing method

By controlling the bath surface height and temperature during the titanium sponge production process, the formation of thick titanium sponge on the side wall is suppressed, ensuring efficient cooling, smooth bath flow, and facilitating easy removal of the sponge lump, thus enhancing productivity.

JP7564613B2Active Publication Date: 2024-10-09TOHO TITANIUM CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2019119023
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-06-26
Publication Date
2024-10-09
Estimated Expiration
2039-06-26

AI Technical Summary

Technical Problem

The formation of a thick, inwardly swelling titanium sponge on the inner surface of the side wall of a metal reduction reaction vessel during the production of titanium sponge leads to reduced cooling efficiency, impeded bath flow, and difficulties in removing the titanium sponge lump, affecting productivity and workability.

Method used

Control the height and temperature of the molten bath surface during the reduction process by maintaining a specific temperature range (700°C to 950°C) and ensuring a minimum ratio of the total moving distance of the bath surface to the effective space height of 0.12 or more, while intermittently supplying titanium tetrachloride and magnesium chloride, to suppress the formation of thick titanium sponge on the side wall.

Benefits of technology

This method effectively suppresses the formation of thick titanium sponge, enhances cooling efficiency, maintains smooth bath flow, and improves the workability of removing the titanium sponge lump, thereby increasing productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564613000002
    Figure 0007564613000002
  • Figure 0007564613000003
    Figure 0007564613000003
  • Figure 0007564613000004
    Figure 0007564613000004
Patent Text Reader

Abstract

To provide a method for producing sponge titanium which can suppress formation of thick wall surface production sponge titanium onto an inner surface of a side wall of a metallic reduction reaction vessel.SOLUTION: A method for producing sponge titanium includes a reduction step of supplying titanium tetrachloride to a molten bath containing metal magnesium in a metallic reduction reaction vessel to produce a sponge titanium lump, in the reduction step, every time 10 mass% of the titanium tetrachloride based on the total supply amount is supplied until the supply amount of the titanium tetrachloride reaches at least 50 mass% of the total supply amount of the titanium tetrachloride, the total movement distance of the bath surface of the molten bath is set at 0.12 or more in terms a ratio to an effective space height in the metallic reduction reaction vessel, and a temperature of the side wall of the metallic reduction reaction vessel at the position of the bath surface in the height direction is within a range of 700-950°C.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a method for producing sponge titanium by supplying titanium tetrachloride to a molten bath containing metallic magnesium in a metal reduction reaction vessel to produce sponge titanium mass. [Background technology]

[0002] For example, to produce titanium sponge by the Kroll process, which is widely used industrially, a reduction step is carried out in which molten magnesium metal is stored in a metallic reduction reaction vessel to form a molten bath, and titanium tetrachloride is dropped onto the bath surface. In the reduction step, the magnesium metal acts as a reducing agent to reduce the titanium tetrachloride to metallic titanium, which grows as a titanium sponge mass inside the metallic reduction reaction vessel.

[0003] The following reaction is believed to occur within the metallic reduction reaction vessel: Titanium tetrachloride, dropped from above, reacts with metallic magnesium near the bath surface, producing metallic titanium and magnesium chloride. The magnesium chloride produced near the bath surface sinks deeper below the surface due to the difference in specific gravity between it and metallic magnesium, while metallic magnesium rises to the surface. As a result of this bath flow, metallic magnesium remains on the bath surface, and the reduction reaction of titanium tetrachloride with metallic magnesium continues to occur near the bath surface.

[0004] After the reduction step, a separation step is generally carried out. In this step, the magnesium chloride in the metallic reduction reaction vessel, and any remaining metallic magnesium, are drained, and then, for example, the metallic reduction reaction vessel is heated to a high temperature while the internal pressure is reduced. In the separation step, the metallic magnesium remaining in the metallic reduction reaction vessel and the by-product magnesium chloride are separated from the titanium sponge mass in the metallic reduction reaction vessel. The titanium sponge mass is then removed from the metallic reduction reaction vessel and crushed to produce granular titanium sponge.

[0005] Patent Documents 1 and 2 describe techniques that focus on the discharge of magnesium chloride from a metal reduction reaction vessel and the supply of metallic magnesium into the metal reduction reaction vessel in the reduction step. Specifically, Patent Document 1 aims to "provide a titanium sponge production method which enables increased productivity by preventing a decrease in yield resulting from the tapping operation of MgCl2 and the charging operation of molten Mg," and discloses "a titanium sponge production method which is characterized by producing titanium sponge by adding TiCl4 dropwise to molten Mg contained in a reaction vessel, performing an intermittent tapping operation to remove the by-product MgCl2 from the vessel, and reducing the amount of MgCl2 tapped in the latter half of the reaction compared to the first half of the reaction."

[0006] Furthermore, Patent Document 2 states that "an object of the present invention is to provide a high-quality, economical method for producing titanium sponge which increases the utilization rate of molten magnesium charged during reduction operation, thereby improving productivity (titanium yield), and which also prevents deterioration in quality due to charging." It also proposes "a method for producing titanium sponge in a reduction reaction vessel by the Kroll process, in which the supply of TiCl4 is temporarily stopped during the reduction reaction, and during this period molten magnesium is added to the vessel from above."

[0007] On the other hand, Patent Document 3 describes "a method for producing titanium sponge by reducing titanium tetrachloride with magnesium, which comprises filling a reaction vessel with molten magnesium, maintaining the average temperature of the wall surface of the reaction vessel in contact with the vicinity of the reaction surface of the molten magnesium bath in which the reduction reaction proceeds at or below the melting point of magnesium chloride, and supplying the titanium tetrachloride to the vicinity of the reaction surface of the molten magnesium bath." According to this, "high-purity titanium sponge can be produced efficiently, and as a result, high-purity titanium can be produced with a high yield." [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Laid-Open No. 2004-43872 [Patent Document 2] Japanese Patent Application Laid-Open No. 2012-184476 [Patent Document 3] Japanese Patent Application Laid-Open No. 2008-190024 Summary of the Invention [Problem to be solved by the invention]

[0009] In the reduction step, as the reduction reaction progresses, as shown in FIG. 4, titanium sponge chunks TS grow on the bottom 53 side of the metallic reduction reaction vessel 51, and also a substantially annular wall-formed titanium sponge WS is formed on the upper side of the inner surface of the side wall 52 near the position of the bath surface Sb, rising from the inner surface.

[0010] If this wall-generated titanium sponge WS is formed in a large inward bulge as shown in Figure 5, the following problems may occur: The vicinity of the bath surface Sb in the metallic reduction reaction vessel 51 becomes hot due to the heat generated by the reduction reaction, and therefore, in order to reduce damage to the lid and to control the temperature inside the vessel within a desired range, the metallic reduction reaction vessel 51 is sometimes cooled by air cooling or the like from the outside. However, the wall-formed titanium sponge WS formed as a thick layer from the inner surface of the side wall 52 toward the inside near the bath surface Sb reduces the effect of this cooling near the bath surface Sb.

[0011] Furthermore, if a large wall-formed titanium sponge WS is formed near the bath surface Sb, the area of ​​the bath surface Sb will decrease, preventing the smooth flow of the above-mentioned metallic magnesium and magnesium chloride into the bath and inhibiting the reduction reaction. Furthermore, the wall-formed titanium sponge WS that bulges inward from the inner surface of the side wall 52 hinders the removal of the titanium sponge lumps TS from the metal reduction reaction vessel 51, thereby making it difficult to remove the titanium sponge lumps TS.

[0012] At present, no effective method or solution has been found for the formation of such large wall-surface-grown titanium sponge WS and the problems caused by it. Patent Documents 1 to 3 also do not consider the wall-surface-grown titanium sponge WS at all.

[0013] An object of the present invention is to provide a method for producing titanium sponge which can suppress the formation of a thick titanium sponge on the inner surface of the side wall of a metallic reduction reactor. [Means for solving the problem]

[0014] As a result of extensive research, the inventors have found that the tendency for wall-surface titanium sponge to form can be changed by fluctuating the height of the molten bath surface over a certain range while maintaining the bath surface of the molten bath at a specific temperature within a predetermined period from the beginning to the middle of the reduction step.

[0015] Based on this knowledge, the method includes a reduction step in which titanium tetrachloride is supplied to a molten bath containing metallic magnesium in a metallic reduction reaction vessel to produce a titanium sponge mass, and the total movement distance of the bath surface of the molten bath is set to a ratio of 0.12 or more to the height of the available space in the metallic reduction reaction vessel every time 10 mass% of the total amount of titanium tetrachloride is supplied until the amount of titanium tetrachloride supplied in the reduction step reaches at least 50 mass% of the total amount of titanium tetrachloride supplied, and the temperature of the side wall of the metallic reduction reaction vessel at the position of the bath surface in the height direction is set to a range of 700°C to 950°C.

[0016] In the reduction step, it is preferable that the magnesium chloride produced in the metallic reduction reaction vessel is intermittently discharged from the metallic reduction reaction vessel.

[0017] In the reduction step, metallic magnesium can be intermittently supplied into the metallic reduction reaction vessel. [Effects of the Invention]

[0018] According to the method for producing titanium sponge of the present invention, it is possible to suppress the formation of thick wall-grown titanium sponge on the upper inner surface of the side wall of a metallic reduction reaction vessel. [Brief explanation of the drawings]

[0019] [Figure 1] FIG. 1 is a vertical cross-sectional view showing an example of a metallic reduction reaction vessel that can be used in the reduction step of a titanium sponge production method according to one embodiment of the present invention, together with a reduction furnace. [Figure 2] FIG. 2 is an enlarged longitudinal cross-sectional view schematically showing wall-surface-generated titanium sponge produced in the reduction step of a titanium sponge manufacturing method according to one embodiment of the present invention. [Figure 3] 3(a) and (b) are examples of graphs each showing a part of the change in the ratio of bath surface height (Hs / He) to the amount of titanium tetrachloride supplied. [Figure 4] FIG. 1 is a vertical cross-sectional view of a metallic reduction reaction vessel, showing titanium sponge masses and titanium sponge formed on the wall surface formed in the metallic reduction reaction vessel in a conventional reduction process. [Figure 5] FIG. 2 is an enlarged vertical cross-sectional view schematically showing wall-surface-generated titanium sponge produced in a conventional reduction process. DETAILED DESCRIPTION OF THE INVENTION

[0020] Hereinafter, an embodiment of the present invention will be described in detail. A method for producing titanium sponge according to one embodiment of the present invention includes a reduction step in which titanium tetrachloride is supplied to a molten bath containing metallic magnesium in a metallic reduction reaction vessel to produce titanium sponge mass. In particular, during the reduction step, the total distance traveled by the bath surface of the molten bath is set to a ratio of 0.12 or more to the height of the available space in the metallic reduction reaction vessel every time 10% by mass of titanium tetrachloride is supplied, until the supply amount of titanium tetrachloride reaches at least 50% by mass of the total supply amount of titanium tetrachloride, and the temperature of the side wall of the metallic reduction reaction vessel at the height position of the bath surface is set to a range of 700°C to 950°C.

[0021] After the reduction step, in many cases, the liquid magnesium chloride and metallic magnesium are removed from the metallic reduction reaction vessel, and then a separation step is carried out in which the pressure inside the metallic reduction reaction vessel is reduced to separate the metallic magnesium and magnesium chloride from the titanium sponge mass. After the separation step, the titanium sponge mass is removed from the metallic reduction reaction vessel and crushed to form granular titanium sponge.

[0022] (Reduction process) The reduction process uses a metallic reduction reactor 1, as shown in FIG. 1. This metallic reduction reactor 1 includes a cylindrical or other tubular side wall 2, a bottom 3 that seals one axial end of the side wall 2 (the lower end in FIG. 1), and a lid 4 attached to an opening at the other axial end of the side wall 2 (the upper end in FIG. 1). The side wall 2 is provided with a by-product discharge pipe 5 connected to a portion of the side wall 2 near the bottom 3, and the lid 4 is provided with a raw material supply pipe 6. Generally, as in the illustrated example, a grate 7 is disposed on the bottom 3 side of the metallic reduction reactor 1, which operates to push up the titanium sponge mass TS when removing it from the metallic reduction reactor 1. The metallic reduction reactor 1 is disposed in a reduction furnace 8, where the reduction process is performed. Although not shown, the reduction furnace 8 is provided with multiple independently controllable air-cooling ports along its height, through which air can be blown onto the side wall 2 to cool the metallic reduction reactor 1. In this embodiment, it is preferable to cool the metallic reduction reaction vessel 1 at least at a height where the bath surface Sb exists.

[0023] To perform the reduction step using the metallic reduction reaction vessel 1, for example, metallic magnesium as a reducing agent is stored in a molten state inside the metallic reduction reaction vessel 1, and the interior of the metallic reduction reaction vessel 1 becomes a molten bath Bm. Then, the metallic reduction reaction vessel 1 is heated in a reduction furnace 8 while also being locally cooled, and titanium tetrachloride (TiCl4) as a raw material is supplied dropwise onto the bath surface Sb of the molten bath Bm from above through a raw material supply pipe 6 attached to the lid 4. The titanium tetrachloride thus supplied comes into contact with the metallic magnesium, and is reduced by the metallic magnesium based on the reaction: TiCl4 + 2Mg → Ti + 2MgCl2.

[0024] Here, magnesium chloride (MgCl2) as a by-product settles downward from the bath surface Sb due to its larger specific gravity compared to metallic magnesium. Meanwhile, metallic magnesium in the bath rises toward the bath surface Sb due to its relatively small specific gravity. This difference in specific gravity between magnesium chloride and metallic magnesium causes the bath to flow, with metallic magnesium positioned at the bath surface Sb. A reaction continues between this metallic magnesium and the dripped titanium tetrachloride, primarily resulting in the growth of titanium sponge mass TS in the bath. The magnesium chloride that settles downward may be discharged to the outside of the metallic reduction reaction vessel 1 through the by-product discharge pipe 5 on the bottom 3 side of the metallic reduction reaction vessel 1.

[0025] The titanium tetrachloride used in the reduction step can be, for example, purified liquid titanium tetrachloride obtained after purification in a rectification column. This purified titanium tetrachloride is obtained, for example, by purifying crude titanium tetrachloride, which is produced by reacting a raw material ore such as titanium ore with a carbon source such as coke and chlorine gas, in a rectification column. However, the titanium tetrachloride is not limited to the above-mentioned purified titanium tetrachloride, as long as it is usable in the reduction step. Furthermore, the magnesium chloride produced in the reduction step can be decomposed into metallic magnesium and chlorine gas by subjecting it to molten salt electrolysis in an electrolytic cell. The metallic magnesium thus obtained can be reused in the reduction step.

[0026] As this reduction process progresses, as the titanium sponge mass TS grows on the bottom 3 side of the metallic reduction reaction vessel 1, wall-surface-grown titanium sponge WS may form, swelling inward from the inner surface of the side wall 2 above the inner surface at a height near the bath surface Sb. If the wall-formed titanium sponge WS near the bath surface Sb is formed thickly, the presence of the wall-formed titanium sponge WS may result in insufficient cooling of the bath surface Sb by air cooling or the like around the side wall 2, and there is a concern that the temperature rise of the bath surface Sb due to the heat generated by the reduction reaction may not be effectively suppressed.

[0027] Furthermore, the larger the area of ​​the bath surface Sb of the molten bath Bm, the smoother the bath flow caused by the movement of metallic magnesium and magnesium chloride within the bath. Smooth bath flow is especially important from the middle to the end of the reduction process, as not only is the temperature of the bath surface Sb likely to rise, but the amount of metallic magnesium in the molten bath Bm also decreases. Bath flow also has the advantage of suppressing the temperature rise of the bath surface Sb. However, if a thick layer of wall-formed titanium sponge WS is present near the bath surface Sb, it will reduce the surface area of ​​the bath surface Sb and hinder bath flow.

[0028] After the reduction step and separation step are completed, the lid 4 is removed from the metallic reduction reaction vessel 1 and the grate 7 is raised to remove the titanium sponge lump TS from the metallic reduction reaction vessel 1. At this time, if the titanium sponge WS has formed a large bulge on the inner surface of the side wall 2, the titanium sponge lump TS and the titanium sponge WS will interfere with each other, making it difficult to remove the titanium sponge lump TS.

[0029] To address this problem, in this embodiment, the height and temperature of the bath surface Sb of the molten bath Bm are adjusted during a predetermined period from at least the beginning to the middle of the reduction process so that a thin layer of wall-formed titanium sponge WS is formed over a relatively wide area. Specifically, every time 10% by mass of titanium tetrachloride is supplied, the ratio of the total movement distance of the bath surface Sb of the molten bath Bm to the height He of the working space in the metallic reduction reaction vessel is set to 0.12 or more, until the total supply amount of titanium tetrachloride supplied throughout the reduction process reaches at least 50% by mass. Furthermore, during the predetermined period, the temperature of the side wall 2 of the metallic reduction reaction vessel 1 at the position of the bath surface Sb in the height direction is set to a range of 700°C to 950°C. Here, the ratio of the total movement distance of the bath surface Sb to the height He of the working space is also referred to as the ratio of the total movement distance of the bath surface Sb.

[0030] According to this, during the predetermined period from the start of the reduction process, the bath surface Sb is maintained within a specific temperature range and changes significantly in the height direction. As a result, the wall-surface titanium sponge WS is formed by thin deposition on the upper inner surface of the side wall 2 near the bath surface Sb, as schematically shown in Figure 2, and the wall-surface titanium sponge WS is prevented from swelling inward of the metallic reduction reaction vessel 1.

[0031] As a result, since the thickness of the wall-grown titanium sponge WS is relatively thin, the area near the bath surface Sb can be effectively cooled by air cooling from around the vessel. Furthermore, a reduction in the area of ​​the bath surface Sb due to the swelling of the wall-grown titanium sponge WS is suppressed, allowing the bath to flow smoothly. Furthermore, the presence of the thin wall-grown titanium sponge WS improves the workability of removing the titanium sponge mass TS from the metal reduction vessel 1 after the separation step.

[0032] Here, the total movement distance of the bath surface Sb of the molten bath is based on the initial height of the molten salt bath Sb in the metallic reduction reaction vessel 1 before the start of the supply of titanium tetrachloride, and can be calculated using the amount of titanium tetrachloride supplied (amount dripped), the inner diameter of the side wall 2 of the metallic reduction reaction vessel 1, and, if magnesium chloride is discharged and / or metallic magnesium is supplied in the reduction step, the amount of magnesium chloride discharged and / or metallic magnesium supplied. For example, if neither magnesium chloride is discharged nor metallic magnesium is supplied, the bath surface Sb of the molten bath will continuously rise during the reduction step as titanium tetrachloride is supplied. Therefore, in this case, the movement distance of the bath surface Sb in the direction in which the bath surface Sb of the molten bath rises is calculated based on the amount of titanium tetrachloride supplied and the inner diameter of the side wall 2 of the metallic reduction reaction vessel 1, and this is taken as the total movement distance of the bath surface Sb. Alternatively, when magnesium chloride is discharged and / or metallic magnesium is supplied, the total movement distance of the bath surface Sb of the molten bath is calculated taking into consideration not only the movement distance in the bath surface upward direction accompanying the supply of titanium tetrachloride as described above, but also the movement distance in the bath surface downward direction due to the discharge of magnesium chloride and / or the movement distance in the bath surface upward direction due to the supply of metallic magnesium.

[0033] In the reduction step, the fluctuation in the height of the bath surface Sb when titanium tetrachloride is supplied can be expressed by the change in the ratio (Hs / He) of the height Hs of the bath surface Sb of the molten bath to the height He of the available space in the metallic reduction reaction vessel 1.

[0034] Here, the height Hs of the bath surface Sb means the length along the height direction (vertical direction, up and down direction in Figure 1) from the position of the bottom surface of the titanium sponge lump TS formed in the reduction step to the position of the bath surface Sb. In the example shown, the titanium sponge lump TS is formed on the surface 7a of the grate 7, and the bottom surface of the titanium sponge lump TS is located on the surface 7a of the grate 7, so the height Hs of the bath surface Sb of the molten bath is the length in the height direction from the position of the surface 7a of the grate 7 to the position of the bath surface Sb. The height Hs of the bath surface Sb can be determined from the initial height of the molten salt bath Sb in the metallic reduction reaction vessel 1 before the supply of titanium tetrachloride, using the amount of titanium tetrachloride supplied, the inner diameter of the side wall 2 of the metallic reduction reaction vessel 1, and, if magnesium chloride is discharged and / or metallic magnesium is supplied in the reduction step, the amount of magnesium chloride discharged and / or the amount of metallic magnesium supplied.

[0035] Here, the effective space height He within the metallic reduction reaction vessel 1 refers to the maximum height in the vertical direction that the bath surface Sb can rise above the surface 7a of the grate 7 with which the bottom surface of the titanium sponge lumps TS contacts. In the illustrated example, the raw material supply pipe 6 protrudes from the lid 4 toward the space within the metallic reduction reaction vessel 1, and so the effective space height He is the heightwise length from the position of the surface 7a of the grate 7 (the position of the bottom surface of the titanium sponge lumps TS) to the position of the lower end of the raw material supply pipe 6.

[0036] Calculating the bath surface height ratio (Hs / He) during the supply of titanium tetrachloride into the metallic reduction reaction vessel 1 can yield graphs showing the change in the bath surface height ratio (Hs / He) relative to the amount of titanium tetrachloride supplied, as shown in Figures 3(a) and 3(b). The graphs in Figures 3(a) and 3(b) each show the change in the bath surface height ratio (Hs / He) from the point at which 10 mass% of the total amount of titanium tetrachloride was supplied to the point at which 30 mass% was supplied. Here, as shown by the solid broken lines in Figures 3(a) and 3(b), the bath surface height ratio (Hs / He) fluctuates significantly over a short span due to the intermittent discharge of magnesium chloride from the metallic reduction reaction vessel 1 and the intermittent supply of metallic magnesium to the metallic reduction reaction vessel 1 every relatively short period of time. The total movement distance of the bath surface Sb corresponds to the sum of the magnitudes of the components along the vertical axis of the broken lines in Figure 3. Using this total movement distance and the height of the effective space, the ratio of the total movement distance of the bath surface of the molten bath to the height of the effective space in the metallic reduction reaction vessel is calculated every time 10 mass% of titanium tetrachloride is supplied relative to the total supply amount of titanium tetrachloride, and this ratio is set to be 0.12 or more.

[0037] If the ratio of the total movement distance of the bath surface Sb for every 10% by mass of titanium tetrachloride supplied falls below 0.12 during the period until the titanium tetrachloride supply amount reaches 50% by mass of the total supply amount, the fluctuation of the bath surface Sb is insufficient, and the wall-formed titanium sponge WS forms a large bulge inside the metal reduction reaction vessel 1 within a relatively narrow range in the height direction, resulting in the above-mentioned problem. From the viewpoint of appropriately and significantly moving the bath surface Sb, it is preferable that the ratio of the total movement distance of the bath surface Sb for every 10% by mass of titanium tetrachloride supplied be 0.16 or more. There is no particular preferred upper limit for the ratio of the total movement distance of the bath surface Sb, but it may be, for example, 0.30 or less.

[0038] Furthermore, if the temperature of the side wall 2 at the bath surface Sb falls below 700°C until the supply of titanium tetrachloride reaches 50% by mass of the total supply, in addition to the expected reaction of TiCl4 + 2Mg → Ti + 2MgCl2, a reaction to produce lower titanium chlorides such as TiCl2 occurs, and the rate of this reaction tends to increase. Furthermore, the bath surface temperature approaches the melting point of magnesium too closely. On the other hand, if the temperature of the side wall 2 exceeds 950°C, evaporation of metallic magnesium progresses, and the rate of the reduction reaction of titanium tetrachloride in the gas phase tends to increase. By setting the temperature of the side wall 2 at the bath surface Sb to 800°C to 950°C, the reaction to produce lower titanium chlorides such as TiCl2 can be further reduced. The temperature of the side wall 2 can be measured using a thermometer such as a thermocouple installed outside the vessel at the side wall 2.

[0039] After the supply amount of titanium tetrachloride reaches 50% by mass of the total supply amount of titanium tetrachloride, it is no longer necessary to control the ratio of the total movement distance of the bath surface Sb and the temperature of the side wall 2 as described above. However, even within a certain period after the supply amount of titanium tetrachloride reaches 50% by mass of the total supply amount of titanium tetrachloride, the ratio of the total movement distance of the bath surface Sb and / or the temperature of the side wall 2 may be controlled in the same manner.

[0040] During the period from the start of titanium tetrachloride supply to the end of supplying 50% by mass of titanium tetrachloride, the height Hs of the bath surface Sb that reaches its highest point during that period, i.e., the maximum value Hsmax, and the height Hs of the bath surface Sb that reaches its lowest point during that period, i.e., the minimum value Hsmin, preferably satisfy the relationship (Hsmax - Hsmin) / He ≥ 0.15, more preferably the relationship (Hsmax - Hsmin) / He ≥ 0.20. In this case, the bath surface Sb more reliably changes significantly in the height direction, resulting in a thin wall-formed titanium sponge WS. Note that, as described below, when metallic magnesium is supplied into the metal reduction reaction vessel 1 during the reduction step, the height of the bath surface Sb at the start of titanium tetrachloride supply can be set low, and therefore (Hsmax - Hsmin) / He may exceed 0.30.

[0041] As described above, in order to control the ratio of the total movement distance of the bath surface Sb, for example, one or more operations of supplying metallic magnesium into the metallic reduction reaction vessel 1 and discharging magnesium chloride from the metallic reduction reaction vessel 1 can be performed until the supply amount of titanium tetrachloride reaches at least 50 mass % of the total supply amount.

[0042] In the reduction step, metallic magnesium can be supplied continuously or intermittently into the metallic reduction reaction vessel 1. This makes it possible to prevent the metallic magnesium in the metallic reduction reaction vessel 1 from being depleted, thereby increasing productivity. In this case, the supply of metallic magnesium raises the bath surface Sb of the molten bath, so the initial height of the bath surface Sb before the start of the supply of titanium tetrachloride can be set relatively low. As a result, it becomes easier to increase the total travel distance of the bath surface Sb of the molten bath. Note that, since it may not be possible to supply titanium tetrachloride and metallic magnesium simultaneously, metallic magnesium may be supplied intermittently between the supplies of titanium tetrachloride.

[0043] Furthermore, when magnesium chloride is discharged from the metallic reduction reaction vessel 1 during the reduction step, the discharge of magnesium chloride may be either continuous or intermittent. Discharging magnesium chloride intermittently has the advantage of making it easier to adjust the fluctuation in the height of the bath surface Sb of the molten bath and the distance traveled. For example, if the time interval between discharges of magnesium chloride is extended to increase the amount discharged per discharge, the bath surface Sb will fluctuate significantly in the height direction. The intermittent discharge of magnesium chloride can be, for example, once every 7% to 10% by mass of titanium tetrachloride supplied relative to the total supply amount. The amount discharged per discharge can be 5% to 12% by mass of the total amount of MgCl discharged during the entire reduction step.

[0044] (separation process) After the reduction step is completed, in addition to the titanium sponge mass TS and wall-formed titanium sponge WS produced in the reduction step, there are also remaining impurities such as metallic magnesium that was not used in the reduction reaction, and magnesium chloride produced as a by-product of the reduction reaction, inside the metallic reduction reaction vessel 1. The separation step is carried out by removing these impurities in a liquid state and then reducing the pressure inside the metallic reduction reaction vessel 1 to separate the impurities from the titanium sponge mass TS, etc.

[0045] In the separation step, after the liquid is removed, the inside of the metallic reduction reaction vessel 1 is depressurized to create a vacuum atmosphere or the like while the metallic reduction reaction vessel 1 is heated to about 1000°C. As a result, impurities such as metallic magnesium and magnesium chloride present in the metallic reduction reaction vessel 1 are sucked and removed from the inside of the metallic reduction reaction vessel 1.

[0046] After the separation step, the titanium sponge chunks TS on the top are removed from the metallic reduction reaction vessel 1 using a grate 7 or the like provided on the bottom 3 side of the metallic reduction reaction vessel 1. The titanium sponge chunks TS are then crushed into granules to obtain titanium sponge. [Example]

[0047] The titanium sponge manufacturing method of the present invention was experimentally carried out, and its effects were confirmed. The following description will be given, however, for illustrative purposes only and is not intended to be limiting.

[0048] A reduction step was carried out using a metallic reduction reaction vessel and reduction furnace as shown in FIG. 1 to produce a titanium sponge mass. The metallic reduction reaction vessel used had an inner diameter of 1900 mm, an effective space height of 4300 mm, and a cylindrical side wall. In Examples 1 to 4 and Comparative Examples 1 to 3, titanium tetrachloride was supplied during the reduction step, and magnesium chloride was intermittently discharged throughout the entire reduction step. Magnesium chloride was discharged once every time titanium tetrachloride was supplied in an amount of 7% to 10% by mass of the total supply amount, with the amount discharged per discharge being within the range of 5% to 12% by mass of the total MgCl2 discharged during the entire reduction step. The conditions for Examples 1 to 4 and Comparative Examples 1 to 3 are shown in Table 1. In Example 5, magnesium chloride was not discharged during the reduction step, and the ratio of the total movement distance of the bath surface was set to 0.12 every time 10% by mass of titanium tetrachloride was supplied as the total supply amount until the dropwise addition of titanium tetrachloride reached 50% by mass of the total supply amount, and the side wall temperature at the bath surface position was set to 720°C.

[0049] The ratio of the total travel distance of the bath surface was determined every time 10% by mass of titanium tetrachloride was dropped using the amount of titanium tetrachloride dropped, the inner diameter of the metallic reduction reaction vessel, and the amount of magnesium chloride discharged, and the results for Examples 1 to 4 and Comparative Examples 1 to 3 are shown in Table 1. In Examples 1 to 4 and Comparative Examples 1 to 3, (Hsmax - Hsmin) / He was set to 0.15 or more during the period from the start of dropping titanium tetrachloride until 50% by mass of titanium tetrachloride was dropped. In Example 5, (Hsmax - Hsmin) / He was set to 0.25 or more until 50% by mass of titanium tetrachloride was dropped. However, if the side wall temperature at the bath surface position is set to less than 700°C, there was a concern that the temperature would approach the melting point of metallic magnesium and the reduction reaction would not be carried out properly, so tests were not conducted at such low temperatures.

[0050] For each of Examples 1 to 5 and Comparative Examples 1 to 3, after the reduction step, the maximum radial thickness of the wall-formed titanium sponge formed on the upper inner surface of the side wall of the metallic reduction reaction vessel was measured. The maximum radial thickness of the wall-formed titanium sponge was measured at four points circumferentially spaced at 90° intervals around the side wall of the metallic reduction reaction vessel at the location with the largest deposition thickness, and the values ​​measured at these four points were averaged. A wall-formed titanium sponge with a radial thickness of 200 mm or less was evaluated as passing, and any other thickness was evaluated as failing. The results are also shown in Table 1. The thickness evaluation of the wall-formed titanium sponge of Example 5 passed.

[0051] [Table 1]

[0052] As shown in Table 1, in Examples 1 to 4, the ratio of the total travel distance was set to 0.12 or more for every 10% by mass of titanium tetrachloride added up to 50% by mass of the total amount of titanium tetrachloride added, and the side wall temperature at the bath surface was set within the range of 700°C to 950°C, so that the titanium sponge formed on the wall surface met the pass criteria. Similar results were confirmed in Example 5. On the other hand, in Comparative Example 1, the ratio of the total movement distance was less than 0.12, so the evaluation result of the wall-formed titanium sponge was unacceptable. In Comparative Example 2, the ratio of the total movement distance from 40% by mass to 50% by mass of titanium tetrachloride dripping to the total supply amount was less than 0.12, so it was unacceptable. In Comparative Example 3, the side wall temperature at the bath surface position exceeded 950°C during the period when titanium tetrachloride dripping to 50% by mass of the total supply amount was unacceptable.

[0053] From the above, it has been found that the present invention can suppress the formation of a thick titanium sponge on the inner surface of the side wall of a metallic reduction reaction vessel. [Explanation of symbols]

[0054] 1, 51 Metal reduction reaction vessel 2, 52 side wall 3, 53 bottom 4 Lid 5 By-product discharge pipe 6 Raw material supply pipe 7. Roaster 7a Surface of the grate 8. Reduction furnace TS Titanium sponge mass WS Wall-generated titanium sponge Bm molten bath Sb bath surface Hs Height of the molten bath surface He Effective space height in the metal reduction reactor

Claims

1. 1. A method for producing titanium sponge, comprising a reduction step of supplying titanium tetrachloride to a molten bath containing metallic magnesium in a metallic reduction reaction vessel to produce titanium sponge mass, In the reduction step, the supply amount of titanium tetrachloride is at least until it reaches 50 mass% of the total supply amount of titanium tetrachloride. a ratio of a total movement distance of the bath surface of the molten bath to an effective space height in a metallic reduction reaction vessel is 0.12 or more every time 10% by mass of the total supply amount of titanium tetrachloride is supplied, and The temperature of the side wall of the metal reduction reaction vessel at the position of the bath surface in the height direction is within a range of 700° C. to 950° C.; A method for producing titanium sponge, in which an effective space height He in a metallic reduction reaction vessel, a maximum value Hsmax of the height of the bath surface, and a minimum value Hsmin of the height of the bath surface satisfy the relationship (Hsmax-Hsmin) / He≧0.15 during a period from when the supply of titanium tetrachloride is started to when 50% by mass of titanium tetrachloride is supplied.

2. 2. The method for producing titanium sponge according to claim 1, wherein the magnesium chloride produced in the metallic reduction reaction vessel in the reduction step is intermittently discharged from the metallic reduction reaction vessel.

3. 3. The method for producing titanium sponge according to claim 2, wherein the magnesium chloride is discharged once while titanium tetrachloride is supplied in an amount of 7% by mass to 10% by mass relative to the total amount of titanium tetrachloride supplied.

4. 4. The method for producing titanium sponge according to claim 2 or 3, wherein the amount of magnesium chloride discharged per one reduction step is 5% by mass to 12% by mass of the total amount of magnesium chloride discharged in the entire reduction step.

5. The method for producing titanium sponge according to any one of claims 1 to 4, wherein metallic magnesium is intermittently supplied into a metallic reduction reaction vessel in the reduction step.

6. In the reduction step, a wall-surface-generated titanium sponge is formed on the inner surface of the cylindrical side wall of the metallic reduction reaction vessel, protruding radially inward from the inner surface, A method for producing titanium sponge according to any one of claims 1 to 5, wherein the maximum radial thickness of the wall-formed titanium sponge is 200 mm or less.

Citation Information

Patent Citations

  • Method and device for producing coated film

    JP1984042060A

  • Method of producing sponge titanium

    JP2004043872A

  • Method for producing titanium sponge

    JP2008190024A

  • Method for producing sponge titanium

    JP2012184476A