Liquid crystal polymer resin composition, its manufacturing method, and semiconductor transport carrier
The liquid crystal polymer resin composition, incorporating carbon fibers and carbon precursors, addresses the challenge of achieving appropriate surface resistance and tape releasability in semiconductor carriers, ensuring effective electrostatic dissipation and electromagnetic shielding.
Patent Information
- Application Number
- JP2020091374
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-26
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-05-26
AI Technical Summary
Conventional liquid crystal polymer resin compositions used for semiconductor carriers face challenges in achieving an appropriate surface resistance value in the static electricity diffusion region while maintaining excellent tape releasability, leading to issues with skin layer peeling when adhesive tapes are removed.
A liquid crystal polymer resin composition comprising carbon fibers with a specific weight average fiber length and carbon precursors with a volume resistivity range, blended in specific ratios, along with optional conductive carbon black, to achieve the desired surface resistance and tape releasability.
The composition allows for molding articles with suitable surface resistance values in the static electricity diffusion region and excellent tape removability, suitable for semiconductor carriers, providing effective electrostatic dissipation and electromagnetic shielding.
Smart Images

Figure 0007564642000002 
Figure 0007564642000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal polymer resin composition, a method for producing the same, and a carrier for transporting semiconductors. [Background technology]
[0002] Semiconductive resin compositions in which conductive fillers are dispersed in thermoplastic resins such as polybutylene terephthalate, polycarbonate, and polyether ether ketone are excellent in functions such as antistatic properties, dust adsorption prevention properties, electromagnetic wave shielding properties, etc. Taking advantage of these functions, semiconductive resin compositions are used in semiconductor transport carriers for transporting or storing semiconductor wafers, semiconductor elements, etc. (e.g., Patent Document 1).
[0003] On the other hand, molded articles obtained from liquid crystal polymers have high strength, high heat resistance and high dimensional accuracy, and therefore are used as materials for forming various electronic parts. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-121402 A Summary of the Invention [Problem to be solved by the invention]
[0005] Therefore, semiconductive resin compositions in which conductive fillers are dispersed in liquid crystal polymers are expected to be used as semiconductor transport carriers with high strength and high heat resistance. 5 ~1.0×10 11 It is required that the semiconductor carriers have a surface resistance value of Ω, which is a suitable static electricity dissipation region (International Electrotechnical Commission (IEC) 61340). Furthermore, semiconductor transport carriers are often used repeatedly by sticking strong adhesive sticky tape for display purposes on the semiconductor transport carriers and then peeling it off.
[0006] However, among the molded articles obtained from conventional liquid crystal polymer resin compositions, those that exhibit a surface resistance value in a moderate static electricity dissipation region have a surface skin layer that peels off when a strong adhesive sticky note tape is peeled off. That is, many of the molded articles obtained from conventional liquid crystal polymer resin compositions have problems with tape peelability. Conversely, those that have excellent tape peelability do not exhibit a surface resistance value in a moderate static electricity dissipation region.
[0007] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a liquid crystal polymer resin composition that exhibits a surface resistance value in a moderate static electricity diffusion region and is capable of molding a molded article having excellent tape peelability, a method for producing the same, and a carrier for transporting semiconductors. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention employs the following configuration.
[0009] [1] A liquid crystal polymer resin composition comprising the following components (A), (B'), and (C): (A) Liquid crystal polymer (B') Carbon fiber having a weight average fiber length of less than 150 μm (C) Volume resistivity is 10 2 ~10 10 Carbon precursor with a density of Ω cm A liquid crystal polymer resin composition, wherein the content of the component (B') is 10 to 30 parts by mass relative to 100 parts by mass of the component (A), the content of the component (C) is 5 to 35 parts by mass relative to 100 parts by mass of the component (A), and the total content of the components (B') and (C) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A). [2] Further comprising component (D) conductive carbon black, The liquid crystal polymer resin composition according to [1], wherein the total content of the components (B'), (C) and (D) is 25 to 60 parts by mass per 100 parts by mass of the component (A). [3] A semiconductor transport carrier having a main body made of the liquid crystal polymer resin composition according to [1] or [2] above.
[0010] [4] A method for producing a liquid crystal polymer resin composition by melt-kneading the following components (A), (B), and (C): (A) Liquid crystal polymer (B) Carbon fiber having a weight average fiber length of less than 3000 μm (C) Volume resistivity is 10 2 ~10 10 Carbon precursor with a density of Ω cm A method for producing a liquid crystal polymer resin composition, wherein the blending ratio of the component (B) is 10 to 30 parts by mass relative to 100 parts by mass of the component (A), the blending ratio of the component (C) is 5 to 35 parts by mass relative to 100 parts by mass of the component (A), and the combined blending ratio of the components (B) and (C) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A). Effect of the Invention
[0011] According to the present invention, it is possible to provide a liquid crystal polymer resin composition that exhibits a surface resistance value in a moderate static electricity dissipation region and is capable of molding a molded article having excellent tape peelability, a method for producing the same, and a carrier for transporting semiconductors. [Brief description of the drawings]
[0012] [Figure 1] 1 is a perspective view showing a schematic diagram of an example of a semiconductor transport carrier according to the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] <Liquid crystal polymer resin composition> The liquid crystal polymer resin composition of the present embodiment contains the following components (A), (B'), and (C). (A) Liquid crystal polymer (B') Carbon fiber having a weight average fiber length of less than 150 μm (C) Volume resistivity is 10 2 ~1010 Carbon precursor with a density of Ω cm
[0014] (A) Liquid crystal polymer In this embodiment, the liquid crystal polymer resin composition contains a liquid crystal polymer as component (A). A liquid crystal polymer (LCP) is a thermoplastic resin that exhibits liquid crystal-like properties in which linear chains of molecules are regularly arranged in a molten state. A liquid crystal polymer resin composition containing a liquid crystal polymer (LCP) also preferably exhibits liquid crystallinity in a molten state, and is preferably one that melts at a temperature of 450°C or less. By containing a liquid crystal polymer, the liquid crystal polymer resin composition has high strength, high heat resistance, and high dimensional accuracy.
[0015] The liquid crystal polymer (LCP) used in this embodiment may be a liquid crystal polyester, a liquid crystal polyester amide, a liquid crystal polyester ether, a liquid crystal polyester carbonate, or a liquid crystal polyester imide. The liquid crystal polymer (LCP) used in this embodiment is preferably a liquid crystal polyester, and more preferably a wholly aromatic liquid crystal polyester made using only aromatic compounds as raw material monomers.
[0016] Typical examples of the liquid crystal polyester used in this embodiment include those obtained by polymerizing (polycondensing) aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid, and at least one compound selected from the group consisting of aromatic diol, aromatic hydroxyamine, and aromatic diamine, those obtained by polymerizing a plurality of aromatic hydroxycarboxylic acids, those obtained by polymerizing aromatic dicarboxylic acid and at least one compound selected from the group consisting of aromatic diol, aromatic hydroxyamine, and aromatic diamine, and those obtained by polymerizing polyester such as polyethylene terephthalate and aromatic hydroxycarboxylic acid. Here, the aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid, aromatic diol, aromatic hydroxyamine, and aromatic diamine may each be independently replaced in part or in whole by their polymerizable derivatives.
[0017] Examples of polymerizable derivatives of compounds having a carboxyl group, such as aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids, include those obtained by converting a carboxyl group to an alkoxycarbonyl group or an aryloxycarbonyl group (esters), those obtained by converting a carboxyl group to a haloformyl group (acid halides), and those obtained by converting a carboxyl group to an acyloxycarbonyl group (acid anhydrides). Examples of polymerizable derivatives of compounds having a hydroxyl group, such as aromatic hydroxycarboxylic acids, aromatic diols, and aromatic hydroxyamines, include those obtained by acylation of a hydroxyl group to an acyloxyl group (acylated products). Examples of polymerizable derivatives of compounds having an amino group, such as aromatic hydroxyamines and aromatic diamines, include those obtained by acylation of an amino group to an acylamino group (acylated products).
[0018] The liquid crystal polyester used in this embodiment preferably has a repeating unit represented by the following formula (1) (hereinafter, sometimes referred to as "repeating unit (1)"), and more preferably has a repeating unit (1), a repeating unit represented by the following formula (2) (hereinafter, sometimes referred to as "repeating unit (2)"), and a repeating unit represented by the following formula (3) (hereinafter, sometimes referred to as "repeating unit (3)").
[0019] (1)-O-Ar 1 -CO- (2)-CO-Ar 2 -CO- (3)-X-Ar 3 -Y- (In formulas (1) to (3), Ar 1 represents a phenylene group, a naphthylene group, or a biphenylylene group; Ar 2 and Ar 3 each independently represents a phenylene group, a naphthylene group, a biphenylene group, or a group represented by the following formula (4). X and Y each independently represent an oxygen atom or an imino group. Ar 1 , Ar 2 and Ar 3Each hydrogen atom in the group represented by the formula (I) may be independently substituted with a halogen atom, an alkyl group, or an aryl group. (4)-Ar 4 -Z-Ar 5 - (In formula (4), Ar 4 and Ar 5 each independently represents a phenylene group or a naphthylene group; Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group, or an alkylidene group.
[0020] The liquid crystal polyester used in the present embodiment contains a repeating unit represented by the repeating unit (1), the repeating unit (2), or the repeating unit (3), the content of the repeating unit (1) is 30 mol % or more and 100 mol % or less based on the total amount of the repeating unit (1), the repeating unit (2), or the repeating unit (3); the content of the repeating unit (2) is 0 mol % or more and 35 mol % or less based on the total amount of the repeating unit (1), the repeating unit (2), or the repeating unit (3); The content of the repeating unit (3) is preferably from 0 mol % to 35 mol % based on the total amount of the repeating unit (1), the repeating unit (2) or the repeating unit (3).
[0021] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a s-butyl group, a t-butyl group, an n-hexyl group, a 2-ethylhexyl group, an n-octyl group, and an n-decyl group, and the number of carbon atoms is preferably 1 to 10. Examples of the aryl group include a phenyl group, an o-tolyl group, an m-tolyl group, a p-tolyl group, a 1-naphthyl group, and a 2-naphthyl group, and the number of carbon atoms is preferably 6 to 20. When the hydrogen atom is substituted with these groups, the number is Ar 1 , Ar 2 or Ar 3 For each of the groups represented by the following formula, the number is preferably 2 or less, and more preferably 1 or less.
[0022] Examples of the alkylidene group include a methylene group, an ethylidene group, an isopropylidene group, an n-butylidene group, and a 2-ethylhexylidene group, and the number of carbon atoms is preferably 1 to 10.
[0023] The repeating unit (1) is a repeating unit derived from a specific aromatic hydroxycarboxylic acid. Preferred repeating units (1) include Ar 1 is a p-phenylene group (a repeating unit derived from p-hydroxybenzoic acid), and Ar 1 is a 2,6-naphthylene group (a repeating unit derived from 6-hydroxy-2-naphthoic acid). In this specification, the term "derived from" means that the chemical structure of the functional group that contributes to the polymerization is changed due to the polymerization of the raw material monomer, and no other structural changes are caused.
[0024] The repeating unit (2) is a repeating unit derived from a specific aromatic dicarboxylic acid. Preferred repeating units (2) include Ar 2 is a p-phenylene group (a repeating unit derived from terephthalic acid), Ar 2 is an m-phenylene group (a repeating unit derived from isophthalic acid), Ar 2 is a 2,6-naphthylene group (a repeating unit derived from 2,6-naphthalenedicarboxylic acid), and Ar 2 is a diphenylether-4,4'-diyl group (a repeating unit derived from diphenylether-4,4'-dicarboxylic acid).
[0025] The repeating unit (3) is a repeating unit derived from a specific aromatic diol, aromatic hydroxylamine or aromatic diamine. Preferred repeating units (3) include Ar 3 is a p-phenylene group (repeating units derived from hydroquinone, p-aminophenol or p-phenylenediamine), and Ar 3is a 4,4'-biphenylylene group (a repeating unit derived from 4,4'-dihydroxybiphenyl, 4-amino-4'-hydroxybiphenyl or 4,4'-diaminobiphenyl).
[0026] The content of the repeating unit (1) is preferably 30 mol % or more and 100 mol % or less, more preferably 30 mol % or more and 80 mol % or less, even more preferably 40 mol % or more and 70 mol % or less, and particularly preferably 45 mol % or more and 65 mol % or less, based on the total amount of all repeating units (the value obtained by dividing the mass of each repeating unit constituting the liquid crystal polymer by the formula weight of each repeating unit to determine the substance amount equivalent (mol) of each repeating unit, and then adding them up).
[0027] The content of the repeating unit (2) is preferably from 0 mol% to 35 mol% inclusive, more preferably from 10 mol% to 35 mol% inclusive, even more preferably from 15 mol% to 30 mol% inclusive, and particularly preferably from 17.5 mol% to 27.5 mol% inclusive, based on the total amount of all repeating units.
[0028] The content of the repeating unit (3) is preferably from 0 mol% to 35 mol% inclusive, more preferably from 10 mol% to 35 mol% inclusive, even more preferably from 15 mol% to 30 mol% inclusive, and particularly preferably from 17.5 mol% to 27.5 mol% inclusive, based on the total amount of all repeating units.
[0029] The sum of the content of the repeating unit (1) of the liquid crystal polyester, the content of the repeating unit (2) of the liquid crystal polyester and the content of the repeating unit (3) of the liquid crystal polyester does not exceed 100 mol %.
[0030] The higher the content of the repeating unit (1), the more likely it is that the melt fluidity, heat resistance, strength, and rigidity will improve. However, if the content is too high, the melt temperature and melt viscosity will tend to increase, and the temperature required for molding will tend to become higher.
[0031] The ratio of the content of the repeating unit (2) to the content of the repeating unit (3), expressed as [content of the repeating unit (2)] / [content of the repeating unit (3)] (mol / mol), is preferably 0.9 / 1 to 1 / 0.9, more preferably 0.95 / 1 to 1 / 0.95, and even more preferably 0.98 / 1 to 1 / 0.98.
[0032] The liquid crystal polymer used in the present embodiment may have two or more of the repeating units (1) to (3) independently. The liquid crystal polymer may have a repeating unit other than the repeating units (1) to (3), and the content of such a repeating unit is preferably 0 mol % to 10 mol %, more preferably 0 mol % to 5 mol %, based on the total amount of all the repeating units.
[0033] The liquid crystal polymer used in the present embodiment preferably has a repeating unit (3) in which X and Y are each an oxygen atom. That is, it is preferable to have a repeating unit derived from a specific aromatic diol, since this tends to reduce the melt viscosity, and it is more preferable to have only repeating units (3) in which X and Y are each an oxygen atom.
[0034] The liquid crystal polymer used in this embodiment is preferably produced by melt-polymerizing raw material monomers corresponding to the repeating units constituting the polymer, and solid-phase polymerizing the resulting polymer (hereinafter, sometimes referred to as "prepolymer"). This makes it possible to produce a high molecular weight liquid crystal polymer with high heat resistance, strength, and rigidity with good operability. The melt polymerization may be carried out in the presence of a catalyst, and examples of the catalyst include metal compounds such as magnesium acetate, stannous acetate, tetrabutyl titanate, lead acetate, sodium acetate, potassium acetate, and antimony trioxide, and nitrogen-containing heterocyclic compounds such as 4-(dimethylamino)pyridine and 1-methylimidazole, and nitrogen-containing heterocyclic compounds are preferably used.
[0035] The flow starting temperature of the liquid crystal polymer used in this embodiment is preferably 280° C. or higher, more preferably 280° C. or higher and 400° C. or lower, and even more preferably 280° C. or higher and 380° C. or lower. The higher the flow start temperature of the liquid crystal polymer used in this embodiment, the more the heat resistance, strength and rigidity of the molded article obtained from the liquid crystal polymer resin composition tend to improve. On the other hand, if the flow start temperature of the liquid crystal polymer exceeds 400°C, the melting temperature and melt viscosity of the liquid crystal polymer tend to increase. Therefore, the temperature required for molding the liquid crystal polymer tends to increase.
[0036] In this specification, the flow initiation temperature of a liquid crystal polymer is also called the flow temperature or flow temperature, and is a temperature that is an indicator of the molecular weight of the liquid crystal polymer (see "Liquid Crystal Polymer - Synthesis, Forming, and Application" edited by Naoyuki Koide, CMC Corporation, June 5, 1987, p. 95). The flow initiation temperature was measured by applying a pressure of 9.8 MPa (100 kg / cm) to the liquid crystal polymer using a capillary rheometer. 2 ) while heating at a rate of 4°C / min under a load of 1000 V and extruding from a nozzle with an inner diameter of 1 mm and a length of 10 mm, this is the temperature at which the material shows a viscosity of 4800 Pa s (48,000 poise).
[0037] In the liquid crystal polymer resin composition, the content of the component (A) is preferably 60 to 80 mass%, more preferably 61 to 79 mass%, even more preferably 62 to 78 mass%, and particularly preferably 65 to 77 mass%, relative to 100 mass% of the liquid crystal polymer resin composition.
[0038] (B') Carbon fiber having a weight average fiber length of less than 150 μm In this embodiment, the liquid crystal polymer resin composition contains component (B') "carbon fiber having a weight average fiber length of less than 150 μm", and the content of component (B') is 10 to 30 parts by mass per 100 parts by mass of component (A).
[0039] As the carbon fiber in the liquid crystal polymer resin composition, various carbon fibers such as polyacrylonitrile (PAN)-based, pitch-based (coal pitch-based, petroleum pitch-based), cellulose-based, lignin-based, etc., can be used. Among these, at least one carbon fiber selected from the group consisting of PAN-based carbon fiber and pitch-based carbon fiber is particularly preferred.
[0040] There is no particular limitation on the weight average fiber length of the carbon fibers in the liquid crystal polymer resin composition, so long as it is less than 150 μm.
[0041] The weight average fiber length of the carbon fibers in the liquid crystal polymer resin composition can be obtained by the following procedure. First, the liquid crystal polymer resin composition is heated in an air atmosphere to remove the resin, and an ashing residue containing the carbon fibers is obtained. The ashing residue is dispersed in an aqueous solution containing a surfactant, and diluted with pure water to obtain a diluted sample solution. Using a particle shape image analyzer, the diluted sample solution obtained is passed through a flow cell, and the carbon fibers moving in the liquid are imaged one by one. The obtained image is binarized, and the circumscribed rectangle major axis of 30,000 carbon fibers in the processed image is measured, and the weight average fiber length of the carbon fibers in the liquid crystal polymer resin composition is obtained by the following formula (5). Lw=Σ Li 2 / Σ Li (5) Lw: Weight average fiber length Li: Circumscribed rectangle major axis of the i-th carbon fiber
[0042] The weight average fiber length of the carbon fibers in the liquid crystal polymer resin composition is less than 150 μm, and the content of the component (B') is 10 to 30 parts by mass per 100 parts by mass of the component (A). This allows the surface resistance of the molded product obtained by molding the liquid crystal polymer resin composition to be 1.0×10 or less while maintaining excellent tape peelability of the molded product obtained by molding the liquid crystal polymer resin composition. 5 ~1.0×10 11 The surface resistance of a molded article obtained by molding a liquid crystal polymer resin composition can be easily controlled to a value in the appropriate static electricity diffusion region of 1.0×10 Ω while maintaining excellent tape peelability. 5In order to easily control the resistance to a moderate value of Ω or more, the weight average fiber length of the carbon fibers in the liquid crystal polymer resin composition is preferably 146 μm or less, more preferably 142 μm or less, and even more preferably 138 μm or less. 11 Since it is easy to control the resistance to an appropriate value of Ω or less, the weight average fiber length of the carbon fibers in the liquid crystal polymer resin composition is preferably 60 μm or more, more preferably 70 μm or more, and even more preferably 80 μm or more.
[0043] The weight average fiber length of the carbon fibers in the liquid crystal polymer resin composition is preferably 60 μm or more and less than 146 μm, more preferably 70 μm or more and 142 μm or less, further preferably 80 μm or more and 138 μm or less, and particularly preferably 90 μm or more and 135 μm or less.
[0044] The average diameter of the carbon fibers in the liquid crystal polymer resin composition is preferably 3 to 15 μm. If the average diameter of the carbon fibers is less than 3 μm, the effect as a reinforcing material tends to be small, whereas if the average diameter of the carbon fibers is more than 15 μm, the moldability tends to decrease, and the surface appearance of the molded product tends to deteriorate.
[0045] In the liquid crystal polymer resin composition of this embodiment, the content of the component (B') is 10 to 30 parts by mass, preferably 11 to 29 parts by mass, more preferably 12 to 28 parts by mass, and even more preferably 22 to 27.5 parts by mass, relative to 100 parts by mass of the component (A).
[0046] (C) Volume resistivity is 10 2 ~10 10 Carbon precursor with a density of Ω cm The liquid crystal polymer resin composition of the present embodiment is a component (C) "having a volume resistivity of 10 2 ~10 10 The content of the component (C) is 5 to 35 parts by mass with respect to 100 parts by mass of the component (A).
[0047] Volume resistivity is 102 ~10 10 A carbon precursor having a resistivity of Ω·cm can be obtained by, for example, calcining an organic substance in an inert atmosphere at a temperature of 400° C. to 900° C. according to the method described in JP 2002-121402 A (Patent Document 1). The carbon precursor can be produced, for example, by a method of (i) heating pitch or tar such as petroleum tar, petroleum pitch, coal tar, or coal pitch, aromatizing and polycondensing the mixture, and, if necessary, oxidizing and infusible in an oxygen atmosphere, and further heating and calcining in an inert atmosphere, (ii) infusible a thermoplastic resin such as polyacrylonitrile or polyvinyl chloride in an oxygen atmosphere, and further heating and calcining in an inert atmosphere, or (iii) curing a thermosetting resin such as a phenol resin or a furan resin, and then heating and calcining in an inert atmosphere.
[0048] The carbon precursor is a material that has been treated in such a way that the carbon content is 97% by mass or less and is not completely carbonized. The carbon content of the carbon precursor is preferably 80 to 97% by mass, and more preferably within the range of 85 to 97% by mass. This allows the volume resistivity of the material in a state that is not completely carbonized to be 10 2 ~10 10 A carbon precursor with a volume resistivity of 10 Ω·cm can be obtained. 3 ~10 9 Ω cm is preferred, 10 4 ~10 8 Ω·cm is more preferable.
[0049] The volume resistivity of the carbon precursor can be measured as follows. The carbon precursor is pressure molded to obtain a plate-shaped molded body. This plate-shaped molded body is heat-treated at 580°C for 1 hour in a nitrogen gas flow to obtain a measurement sample. The volume resistivity of this measurement sample is measured in accordance with JIS K 7194.
[0050] The volume resistivity of the carbon precursor in the liquid crystal polymer resin composition is 10 2 ~10 10and the content ratio of the component (C) is 5 to 35 parts by mass relative to 100 parts by mass of the component (A), the surface resistance value can be increased to 1.0×10 while maintaining excellent tape peelability of the molded article obtained by molding the liquid crystal polymer resin composition. 5 ~1.0×10 11 This makes it easier to control Ω to a moderate value.
[0051] The surface resistance value of the molded article obtained by molding the liquid crystal polymer resin composition can be measured, for example, by using a resistance measuring system manufactured by PROSTAT, Inc., USA.
[0052] In the liquid crystal polymer resin composition of this embodiment, the carbon precursor is usually used in the form of particles or fibers. The average particle size of the carbon precursor particles is preferably 1 mm or less. If the average particle size of the carbon precursor particles is too large, it becomes difficult to obtain a molded product with a good appearance when the liquid crystal polymer resin composition is molded. The average particle size of the carbon precursor particles is usually 0.1 μm to 1 mm, preferably 1 to 800 μm, and more preferably 5 to 500 μm. In many cases, good results can be obtained by using carbon precursor particles with an average particle size of about 5 to 50 μm.
[0053] In the liquid crystal polymer resin composition of this embodiment, the content of the component (C) is 5 to 35 parts by mass, preferably 5 to 32 parts by mass, more preferably 6 to 32 parts by mass, even more preferably 6.5 to 14 parts by mass, and particularly preferably 6.5 to 11 parts by mass, relative to 100 parts by mass of the component (A).
[0054] In the liquid crystal polymer resin composition of this embodiment, the total content of the component (B') and the component (C) is 25 to 60 parts by mass, preferably 28 to 58 parts by mass, more preferably 28 to 50 parts by mass, and even more preferably 28 to 40 parts by mass, relative to 100 parts by mass of the component (A).
[0055] In the liquid crystal polymer resin composition of the present embodiment, the weight average fiber length of the carbon fiber in the liquid crystal polymer resin composition is less than 150 μm, and the volume resistivity of the carbon precursor in the liquid crystal polymer resin composition is 102 ~10 10 The resistivity of the component (B') is 10 to 30 parts by mass relative to 100 parts by mass of the component (A), the content of the component (C) is 5 to 35 parts by mass relative to 100 parts by mass of the component (A), and the total content of the components (B') and (C) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A), so that a molded article can be molded which exhibits a surface resistance value in an appropriate static electricity dissipation region and has excellent tape releasability.
[0056] (Other ingredients) The liquid crystal polymer resin composition of the present embodiment may contain, as necessary, one or more components such as (D) conductive carbon black, a thermoplastic resin, a filler, an additive, etc., in addition to the components (A), (B'), and (C).
[0057] (D) Conductive carbon black The liquid crystal polymer resin composition of the present embodiment may contain (D) conductive carbon black. The conductive carbon black used here may be one obtained by any manufacturing method, and specific examples thereof include channel black, furnace black, acetylene black, etc. From the viewpoint of dispersibility in the liquid crystal polymer resin composition, the average particle size is preferably 30 μm or less.
[0058] The content of the component (D) is preferably 0 to 20 parts by mass, more preferably 0.5 to 18 parts by mass, and further preferably 1 to 15 parts by mass, relative to 100 parts by mass of the component (A).
[0059] The total content ratio of the component (B'), the component (C) and the component (D) is preferably 25 to 60 parts by mass, more preferably 28 to 60 parts by mass, and further preferably 30 to 50 parts by mass, relative to 100 parts by mass of the component (A).
[0060] In the liquid crystal polymer resin composition of the present embodiment, the weight average fiber length of the carbon fiber in the liquid crystal polymer resin composition is less than 150 μm, and the volume resistivity of the carbon precursor in the liquid crystal polymer resin composition is 10 2 ~10 10 When the resistivity is Ω·cm, the content of the component (B') is 10 to 30 parts by mass relative to 100 parts by mass of the component (A), the content of the component (C) is 5 to 35 parts by mass relative to 100 parts by mass of the component (A), the total content of the components (B') and (C) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A), and the total content of the components (B'), (C) and (D) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A), a molded article can be molded which exhibits a surface resistance value in an appropriate static electricity dissipation region and has better tape releasability.
[0061] ·Thermoplastic resin Examples of thermoplastic resins other than liquid crystal polymers contained in the liquid crystal polymer resin composition include thermoplastic resins other than liquid crystal polymers, such as polypropylene, polyamide, polyesters other than liquid crystal polyesters, polysulfone, polyphenylene sulfide, polyether ketone, polycarbonate, polyphenylene ether, and polyetherimide.
[0062] The content of the thermoplastic resin other than the liquid crystal polymer may be 0 to 20 parts by mass, 0 to 10 parts by mass, 0 to 5 parts by mass, or 0 part by mass, relative to 100 parts by mass of the component (A).
[0063] ·Filling material The filler may include plate-like fillers, spherical fillers, and other particulate fillers, and may be either inorganic or organic.
[0064] Examples of the plate-like inorganic filler include talc, mica, graphite, wollastonite, barium sulfate, and calcium carbonate. The mica may be muscovite, phlogopite, fluorphlogopite, or tetrasilicic mica.
[0065] Examples of particulate inorganic fillers include silica, alumina, titanium oxide, boron nitride, silicon carbide, and calcium carbonate.
[0066] Additives Examples of the additives include antioxidants, heat stabilizers, ultraviolet absorbers, antistatic agents, surfactants, flame retardants, and colorants.
[0067] The liquid crystal polymer resin composition of the present embodiment has the following aspects.
[0068] A liquid crystal polymer resin composition comprising the following components (A), (B'), and (C): (A) Liquid crystal polymer (B') Carbon fiber having a weight average fiber length of less than 150 μm (C) Volume resistivity is 10 2 ~10 10 Carbon precursor with a density of Ω cm A liquid crystal polymer resin composition, wherein the content of the component (B') is 10 to 30 parts by mass relative to 100 parts by mass of the component (A), the content of the component (C) is 5 to 35 parts by mass relative to 100 parts by mass of the component (A), and the total content of the components (B') and (C) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A).
[0069] "2" The liquid crystal polymer resin composition according to "1", wherein the content of the component (B') is preferably 11 to 29 parts by mass, more preferably 12 to 28 parts by mass, and even more preferably 22 to 27 parts by mass, relative to 100 parts by mass of the component (A).
[0070] "3" The liquid crystal polymer resin composition according to "1" or "2", wherein the content of the component (C) is preferably 5 to 32 parts by mass, more preferably 6 to 32 parts by mass, even more preferably 6.5 to 14 parts by mass, and particularly preferably 6.5 to 11 parts by mass, relative to 100 parts by mass of the component (A).
[0071] "4" The liquid crystal polymer resin composition according to any one of "1" to "3", wherein the total content ratio of the component (B') and the component (C) is preferably 26 to 60 parts by mass, more preferably 28 to 50 parts by mass, and even more preferably 28 to 36 parts by mass, relative to 100 parts by mass of the component (A).
[0072] "5" Further, component (D) conductive carbon black is contained, The liquid crystal polymer resin composition according to any one of "1" to "4", wherein the total content ratio of the component (B'), the component (C) and the component (D) is 25 to 60 parts by mass, preferably 25 to 60 parts by mass, more preferably 28 to 60 parts by mass, and further preferably 30 to 50 parts by mass, relative to 100 parts by mass of the component (A).
[0073] "6" The liquid crystal polymer resin composition according to "5", wherein the content of the component (D) is 0 to 20 parts by mass, preferably 0.5 to 18 parts by mass, and more preferably 1 to 16 parts by mass, relative to 100 parts by mass of the component (A).
[0074] The liquid crystal polymer resin composition of the present embodiment can be produced, for example, by mixing the components (A), (B'), and (C) with other components as necessary. The liquid crystal polymer resin composition of the present embodiment can also be produced by melt-kneading as described below.
[0075] <Method of producing liquid crystal polymer resin composition> The method for producing a liquid crystal polymer resin composition of the present embodiment is a method for producing a liquid crystal polymer resin composition by melt-kneading the following components (A), (B), and (C): (A) Liquid crystal polymer (B) Carbon fiber having a weight average fiber length of less than 3000 μm (C) Volume resistivity is 10 2 ~10 10 Carbon precursor with a density of Ω cm The blending ratio of the component (B) is 10 to 30 parts by mass per 100 parts by mass of the component (A), the blending ratio of the component (C) is 5 to 35 parts by mass per 100 parts by mass of the component (A), and the combined blending ratio of the components (B) and (C) is 25 to 60 parts by mass per 100 parts by mass of the component (A).
[0076] In the method for producing a liquid crystal polymer resin composition of the present embodiment, the component (D) conductive carbon black can be further blended, and the other components described above can be blended as necessary.
[0077] In the method for producing a liquid crystal polymer resin composition of the present embodiment, the blending ratio of each component is the same as the content ratio of each component described above in the resulting liquid crystal polymer resin composition.
[0078] That is, in the manufacturing method of the liquid crystal polymer resin composition of this embodiment, the blending ratio of the component (B) is 10 to 30 parts by mass relative to 100 parts by mass of the component (A), the blending ratio of the component (C) is 5 to 35 parts by mass relative to 100 parts by mass of the component (A), and the combined blending ratio of the components (B) and (C) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A), so that a molded article exhibiting a surface resistance value in a moderate static electricity diffusion region and having excellent tape peelability can be molded from the obtained liquid crystal polymer resin composition.
[0079] In the method for producing a liquid crystal polymer resin composition of this embodiment, the blending ratio of the component (B) is 10 to 30 parts by mass relative to 100 parts by mass of the component (A), the blending ratio of the component (C) is 5 to 35 parts by mass relative to 100 parts by mass of the component (A), the combined blending ratio of the components (B) and (C) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A), and the combined blending ratio of the components (B), (C) and (D) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A), thereby making it possible to mold a molded product that exhibits a surface resistance value in a moderate static electricity diffusion region and has better tape peelability.
[0080] For example, the components (A), (B), and (C) are mixed with other components as necessary, and melt-kneaded while degassing in a twin-screw extruder. The resulting mixture is extruded in the form of strands through a circular nozzle (discharge port), and then pelletized with a strand cutter to form a pellet-shaped liquid crystal polymer resin composition.
[0081] It can be understood that the composition and properties of the liquid crystal polymer in the pellet-shaped liquid crystal polymer resin composition do not change from the composition and properties of the liquid crystal polymer in the raw material. It can be understood that the volume resistivity of the carbon precursor in the pellet-shaped liquid crystal polymer resin composition does not change from the volume resistivity of the raw material carbon precursor. The weight average fiber length of the carbon fibers in the pellet-shaped liquid crystal polymer resin composition varies depending on the manufacturing conditions of the pellet-shaped liquid crystal polymer resin composition, but tends to be approximately 0% to 95% shorter than the weight average fiber length of the carbon fibers used as the raw material for component (B).
[0082] Since the weight average fiber length of the carbon fiber in the liquid crystal polymer resin composition can be suitably adjusted, the weight average fiber length of the carbon fiber of component (B) is less than 3000 μm, preferably 1000 μm or less, and more preferably 200 μm or less. The weight average fiber length of the carbon fiber of component (B) is preferably 60 μm or more, more preferably 100 μm or more, and even more preferably 140 μm or more. The weight average fiber length of the carbon fiber of component (B) is preferably 60 μm or more and less than 3000 μm, more preferably 100 μm or more and 1000 μm or less, and even more preferably 140 μm or more and 200 μm or less.
[0083] The weight average fiber length of the carbon fibers of component (B) can be determined by the following procedure. The carbon fibers of component (B) are dispersed in an aqueous solution containing a surfactant, and diluted with pure water to obtain a diluted sample solution. Using a particle shape image analyzer, the diluted sample solution obtained is passed through a flow cell, and the carbon fibers moving through the solution are imaged one by one. The obtained image is binarized, and the circumscribed rectangle major axis of 30,000 carbon fibers in the processed image is measured, and the weight average fiber length of the carbon fibers of component (B) is determined by the following formula (5). Lw=Σ Li 2 / Σ Li (5) Lw: Weight average fiber length Li: Circumscribed rectangle major axis of the i-th carbon fiber
[0084] However, when the weight average fiber length of the carbon fibers of component (B) exceeds 1000 μm, it can be determined by the following procedure. The carbon fibers of component (B) are dispersed in an aqueous solution containing a surfactant to obtain a sample solution. A portion of the sample solution is taken and observed under a microscope to measure the lengths of more than 500 carbon fibers, and the weight average fiber length of the carbon fibers of component (B) is determined by the above formula (5).
[0085] When producing a pellet-shaped liquid crystal polymer resin composition using a twin-screw extruder, even if carbon fibers having the same weight average fiber length are used as raw materials, the weight average fiber length of the carbon fibers in the pellet-shaped liquid crystal polymer resin composition can be controlled by changing the screw configuration of the twin-screw extruder. If the length of the kneading zone (kneading section) of the twin-screw extruder is short, the weight average fiber length of the carbon fibers in the pellet-shaped liquid crystal polymer resin composition tends to be long. A short weight average fiber length of the carbon fibers in the pellet-shaped liquid crystal polymer resin composition can be achieved by increasing the length of the kneading zone (kneading section).
[0086] The method for producing a liquid crystal polymer resin composition of the present embodiment has the following aspects.
[0087] A method for producing a liquid crystal polymer resin composition by melt-kneading the following components (A), (B), and (C): (A) Liquid crystal polymer (B) Carbon fiber having a weight average fiber length of less than 3000 μm (C) Volume resistivity is 10 2 ~10 10 Carbon precursor with a density of Ω cm A method for producing a liquid crystal polymer resin composition, wherein the blending ratio of the component (B) is 10 to 30 parts by mass relative to 100 parts by mass of the component (A), the blending ratio of the component (C) is 5 to 35 parts by mass relative to 100 parts by mass of the component (A), and the combined blending ratio of the components (B) and (C) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A).
[0088] "102" The method for producing a liquid crystal polymer resin composition according to "101", wherein the blending ratio of the component (B) is preferably 11 to 29 parts by mass, more preferably 12 to 28 parts by mass, and even more preferably 22 to 27.5 parts by mass, relative to 100 parts by mass of the component (A).
[0089] "103" The method for producing a liquid crystal polymer resin composition according to "101" or "102", wherein the blending ratio of the component (C) is preferably 5 to 32 parts by mass, more preferably 6 to 32 parts by mass, even more preferably 6.5 to 14 parts by mass, and particularly preferably 6.5 to 11 parts by mass, relative to 100 parts by mass of the component (A).
[0090] "104" A method for producing a liquid crystal polymer resin composition according to any one of "101" to "103", wherein the total blending ratio of the component (B) and the component (C) is preferably 28 to 60 parts by mass, more preferably 28 to 55 parts by mass, and even more preferably 28.5 to 50 parts by mass, relative to 100 parts by mass of the component (A).
[0091] "105" Further, component (D) conductive carbon black is contained, The method for producing a liquid crystal polymer resin composition according to any one of "101" to "104", wherein the total blending ratio of the component (B), the component (C) and the component (D) is 25 to 60 parts by mass, preferably 25 to 60 parts by mass, more preferably 28 to 60 parts by mass, and further preferably 30 to 50 parts by mass, relative to 100 parts by mass of the component (A).
[0092] "106" The method for producing a liquid crystal polymer resin composition according to "105", wherein the blending ratio of the component (D) is 0 to 20 parts by mass, preferably 0.5 to 18 parts by mass, and more preferably 1 to 16 parts by mass, per 100 parts by mass of the component (A).
[0093] (Molded body) The liquid crystal polymer resin composition of the present embodiment is molded into a 1.0×10 5 ~1.0×10 11 A molded article having a surface resistance value in the appropriate static electricity diffusion region of Ω can be obtained. As a method for molding a molded article from the liquid crystal polymer resin composition, a melt molding method is preferable, and examples thereof include an injection molding method, an extrusion molding method such as a T-die method or an inflation method, a compression molding method, a blow molding method, a vacuum molding method, and a press molding method. Among them, an injection molding method is preferable.
[0094] For example, when the liquid crystal polymer resin composition is used as a molding material and molded by injection molding, the liquid crystal polymer resin composition is melted using a known injection molding machine, and the molten liquid crystal polymer resin composition is injected into a mold to mold it. Examples of known injection molding machines include hydraulic horizontal molding machines UH1000 and PS40E5ASE models manufactured by Nissei Plastic Industrial Co., Ltd.
[0095] The cylinder temperature of the injection molding machine is appropriately determined depending on the type of liquid crystal polymer, and is preferably set to a temperature 10 to 80°C higher than the flow initiation temperature of the liquid crystal polymer used, for example 320 to 400°C.
[0096] The temperature of the mold is preferably set within the range of room temperature (for example, 23° C.) to 180° C. in terms of the cooling rate of the liquid crystal polymer resin composition and productivity.
[0097] It may be understood that the composition and properties of the liquid crystal polymer in the liquid crystal polymer resin composition of the molded article do not change from the composition and properties of the liquid crystal polymer as the raw material. It may be understood that the volume resistivity of the carbon precursor in the liquid crystal polymer resin composition of the molded article does not change from the volume resistivity of the carbon precursor as a raw material. It may be understood that the weight average fiber length of the carbon fibers in the liquid crystal polymer resin composition of a molded article obtained by injection molding from the pellet-shaped liquid crystal polymer resin composition does not change from the weight average fiber length of the carbon fibers in the pellet-shaped liquid crystal polymer resin composition.
[0098] The molded article obtained by molding the liquid crystal polymer resin composition of the present embodiment exhibits a surface resistance value in a suitable static electricity dissipation region and has excellent tape peelability, and therefore can be suitably applied to a wide range of fields that require control of static electricity, antistatic, electromagnetic wave shielding, dust adsorption prevention, etc. For example, the molded article can be suitably applied to the use of semiconductor transport carriers.
[0099] <Semiconductor transport carrier> The semiconductor transport carrier of this embodiment has a main body made of the liquid crystal polymer resin composition.
[0100] The molded article obtained from the liquid crystal polymer resin composition has a viscosity of 1.0×10 5 ~1.0×10 11 The liquid crystal polymer resin composition exhibits a surface resistance value in the appropriate static electricity dissipation region of Ω and can be molded into a molded article having excellent tape peelability, and therefore is suitably applicable to the use of semiconductor transport carriers.
[0101] Examples of semiconductor transport carriers include wafer carriers, wafer cassettes, IC chip trays, IC chip carriers, IC transport tubes, storage trays, transport device parts, MR head carriers, GMR head carriers, and liquid crystal panel carriers.
[0102] 1 is a perspective view showing a schematic example of a semiconductor transport carrier of this embodiment. The semiconductor transport carrier 1 of this embodiment has a main body 11 made of the liquid crystal polymer resin composition, and a tape attachment part 12 at a visible position on the outside of the main body 11. The main body 11 is formed by molding the liquid crystal polymer resin composition. The main body 11 is designed to be capable of transporting or storing semiconductor parts or semiconductor products such as wafers, ICs, MR heads, GMR heads, and liquid crystal panels.
[0103] The tape attachment portion 12 of the semiconductor transport carrier 1 is 1.0×10 5 ~1.0×10 11 The semiconductor transport carrier 1 has a surface resistance of Ω, which is an appropriate static electricity dissipation region, and has excellent tape peeling properties. Therefore, the semiconductor transport carrier 1 has excellent antistatic properties and dust adsorption resistance, and can be repeatedly used by sticking strong adhesive sticky tape to the tape attachment portion 12 and peeling it off.
[0104] The surface resistance of the tape attachment portion 12 of the semiconductor transport carrier 1 is 1.0×10 5 ~1.0×10 11 Ω, which is 4×10 5 ~4×1010 Ω is preferred, 1.0×10 6 ~1.0×10 10 Ω is more preferred. EXAMPLES
[0105] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the following examples.
[0106] (A) Liquid crystal polymer <Production of Liquid Crystal Polymer> [Production Example 1: Production of Liquid Crystal Polymer (L1)] Into a reactor equipped with a stirrer, a torque meter, a nitrogen gas inlet tube, a thermometer, and a reflux condenser, 994.5 g (7.2 mol) of p-hydroxybenzoic acid, 299.0 g (1.8 mol) of terephthalic acid, 99.7 g (0.6 mol) of isophthalic acid, 446.9 g (2.4 mol) of 4,4'-dihydroxybiphenyl, and 1347.6 g (13.2 mol) of acetic anhydride were placed, and the gas in the reactor was replaced with nitrogen gas. Then, 0.18 g of 1-methylimidazole was added, and the mixture was heated from room temperature to 150°C over 30 minutes while stirring under a nitrogen gas stream, and refluxed at 150°C for 30 minutes. Next, 2.4 g of 1-methylimidazole was added, and the temperature was raised from 150°C to 320°C over 2 hours and 50 minutes while distilling off the by-product acetic acid and unreacted acetic anhydride. When an increase in torque was observed, the contents were removed from the reactor and cooled to room temperature to obtain a solid prepolymer. Next, this prepolymer was pulverized using a pulverizer, and the resulting pulverized material was heated from room temperature to 250°C over 1 hour in a nitrogen atmosphere, then heated from 250°C to 295°C over 5 hours, and held at 295°C for 3 hours to carry out solid-state polymerization. The obtained solid-phase polymer was cooled to room temperature to obtain a powdered liquid crystal polymer (L1). The flow-initiation temperature of the obtained liquid crystal polymer (L1) was 327°C.
[0107] (B) Carbon fiber The following commercially available carbon fiber filler was used as a raw material. (B-1) PANTEX35-MF150 (weight average fiber length: 150 μm, diameter 7 μm), manufactured by Zoltek Corporation, USA (B-2) Mitsubishi Chemical Corporation, DIALEAD (registered trademark) K233HE (weight average fiber length: 6.0 mm, diameter 11 μm)
[0108] <Measurement of weight average fiber length of raw carbon fiber> 0.3 g of the raw carbon fiber filler ((B-1) PANTEX35-MF150, manufactured by Zoltek, USA) was added to 50 mL of pure water, and a surfactant (0.5% by volume of micro-90 (manufactured by Sigma-Aldrich Japan, LLC) aqueous solution) was added to improve dispersibility, and a mixed liquid was obtained. The resulting mixed liquid was ultrasonically dispersed for 5 minutes to obtain a sample liquid in which the carbon fibers were uniformly dispersed in the solution. Next, 5 mL of the resulting sample liquid was collected, placed in a sample cup, and diluted 5 times with pure water to obtain a diluted sample liquid. Using a particle shape image analyzer ("PITA3" manufactured by Seishin Enterprise Co., Ltd.), the resulting diluted sample liquid was passed through a flow cell, and the carbon fibers moving in the liquid were imaged one by one. In this measurement method, the measurement was terminated when the total number of carbon fibers accumulated from the start of the measurement reached 30,000. The obtained image was binarized, the circumscribed rectangle major axis of the carbon fibers in the processed image was measured, and the weight average fiber length of the raw carbon fibers was calculated using the following formula (5). As a result, the weight average fiber length of the raw carbon fibers (B-1) was 150 μm. Lw=Σ Li 2 / Σ Li (5) Lw: Weight average fiber length Li: Circumscribed rectangle major axis of the i-th carbon fiber Number of measurements: 30,000
[0109] (B-2) 0.3 g of DIALEAD (registered trademark) K233HE (manufactured by Mitsubishi Chemical Corporation) was added to 50 mL of pure water, and a surfactant (0.5 vol% aqueous solution of micro-90 (manufactured by Sigma-Aldrich Japan LLC)) was added to improve dispersibility, and a mixed solution was obtained. The resulting mixed solution was ultrasonically dispersed for 5 minutes to obtain a sample solution in which the carbon fibers were uniformly dispersed in the solution. Then, a part of the sample solution was taken out and the fibers were photographed at a magnification of 10 to 20 times using a microscope (manufactured by Keyence Corporation, VH-Z25). The fiber length of the photographed image was measured using image processing software (manufactured by Mitani Shoji Co., Ltd., WinROOF2018) as follows.
[0110] (How to measure fiber length) (a) The captured image is subjected to monochrome pixelation processing. (b) A binarization process is performed so that only the photographed carbon fibers are colored. (c) Fiber length measurements are performed using the needle separation function of the image processing software. (d) The fiber lengths of fibers that could not be binarized in (c) and curved fibers are measured by multi-point measurement, and fibers that contact the edges of the image are not measured. However, if n>500, and the number of fibers measured, n, does not exceed 500, additional microscope images are taken and measurements are continued until n exceeds 500. Using the obtained measurement results, the weight average fiber length of the raw carbon fibers was calculated according to the following formula (5). As a result, the weight average fiber length of the raw carbon fibers (B-2) was 6.0 mm. Lw=Σ Li 2 / Σ Li (5) Lw: Weight average fiber length Li: Circumscribed rectangle major axis of the i-th carbon fiber
[0111] (C) Volume resistivity is 10 2 ~10 10 Carbon precursor with a density of Ω cm Krefine (registered trademark) KH-CP, (volume resistivity: 3×10 7 Ω·cm, average particle size 22 μm) was used as the raw material.
[0112] <Measurement of volume resistivity of carbon precursor> 15 g of carbon precursor (Crefine® KH-CP) was placed in a container with a cross-sectional area of 80 cm 2 The mixture was filled into a cylindrical mold and molded at a pressure of 200 MPa to obtain a disk-shaped molded body. This disk-shaped molded body was heat-treated at 580°C in a nitrogen gas flow for 1 hour to obtain a measurement sample. The volume resistivity of this measurement sample was measured in accordance with JIS K 7194. As a result, the volume resistivity was 3×10 7 The value was Ω·cm.
[0113] (D) Conductive carbon black Ketjen Black (registered trademark) EC-300J (manufactured by Lion Corporation) Primary particle size 39.5 nm
[0114] <Method of producing liquid crystal polymer resin composition> In producing the pellet-shaped liquid crystal polymer resin composition, a twin-screw extruder (manufactured by Ikegai Iron Works Co., Ltd., "PCM30-HS") having a main raw material feeder at the upstream portion and a side feeder at the downstream portion was used.
[0115] Example 1 The liquid crystal polymer (L1) and the carbon precursor (Crefine (registered trademark) KH-CP) were fed from the main raw material feeder of the twin-screw extruder, and the carbon fiber filler ((B-1) PANTEX35-MF150) was fed from the side feeder according to the compounding ratio shown in Table 1. Each raw material was melt-kneaded at a cylinder temperature of 340°C and a screw rotation speed of 150 rpm, and a strand-shaped liquid crystal polymer resin composition was extruded through a circular nozzle (extrusion port) with a diameter of 3 mm at an extrusion rate of 300 kg / h. Thereafter, the mixture was cooled and pelletized to prepare the liquid crystal polymer resin composition of Example 1 in a cylindrical shape (length 3 mm, ie, pellet shape).
[0116] (Examples 2 to 5, 10, Comparative Examples 1 to 3, 6, 8) Similarly, according to the compounding ratios shown in Table 1, pellet-shaped liquid crystal polymer resin compositions of Examples 2 to 5 and 10 and Comparative Examples 1 to 3, 6 and 8 were prepared.
[0117] Example 6 According to the compounding ratio shown in Table 1, the above (A) liquid crystal polymer and (C) having a volume resistivity of 10 2 ~10 10 The raw materials, carbon precursor having a resistivity of Ω·cm, (D) conductive carbon black (conductive CB), and (B) carbon fiber were fed from a side feeder. The raw materials were melt-kneaded at a cylinder temperature of 340°C and a screw rotation speed of 150 rpm, and a strand-shaped liquid crystal polymer resin composition was extruded through a circular nozzle (extrusion port) with a diameter of 3 mm at an extrusion rate of 300 kg / h. Thereafter, the mixture was cooled and pelletized to prepare the liquid crystal polymer resin composition of Example 1 in a cylindrical shape (length 3 mm, ie, pellet shape).
[0118] (Examples 7 to 9, Comparative Examples 4 to 5, 7, and 9) Similarly, according to the compounding ratios shown in Table 1, pellet-shaped liquid crystal polymer resin compositions of Examples 7 to 9 and Comparative Examples 4 to 5, 7, and 9 were prepared.
[0119] Comparative Example 10 Except for changing the carbon fiber filler of Example 1 to (B-2) Mitsubishi Chemical Corporation's DIALEAD (registered trademark) K233HE), the pellet-shaped liquid crystal polymer resin composition of Comparative Example 10 was prepared in the same manner as in Example 1 according to the compounding ratio shown in Table 1.
[0120] <Measurement of weight average fiber length of carbon fibers in resin composition> Of the pellet-shaped liquid crystal polymer resin compositions of the examples and comparative examples, 5 g of each was heated in a muffle furnace (manufactured by Yamato Scientific Co., Ltd., "FP410") in an air atmosphere at 600°C for 4 hours to remove the resin, and an ashing residue containing carbon fibers was obtained. 0.3 g of the ashing residue was put into 50 mL of pure water, and a surfactant (0.5 volume % aqueous solution of micro-90 (manufactured by Sigma-Aldrich Japan LLC)) was added to improve dispersibility, and a mixed liquid was obtained. The resulting mixed liquid was ultrasonically dispersed for 5 minutes to obtain a sample liquid in which the carbon fibers contained in the ashing residue were uniformly dispersed in the solution. Next, 5 mL of the resulting sample liquid was collected, placed in a sample cup, and diluted 5 times with pure water to obtain a diluted sample liquid. Using a particle shape image analyzer (manufactured by Seishin Enterprise Co., Ltd., "PITA3"), the resulting diluted sample liquid was passed through a flow cell, and images of the carbon fibers moving in the liquid were taken one by one. In addition, since the circumscribed rectangle major axis less than 30 μm was ashing residue of carbon precursor or conductive carbon black, in this measurement method, the circumscribed rectangle major axis less than 30 μm was set to be excluded when capturing the image, and the measurement was terminated when the total number of carbon fibers accumulated from the start of the measurement reached 30,000. The obtained image was binarized, the circumscribed rectangle major axis of the carbon fibers in the processed image was measured, and the weight average fiber length of the carbon fibers in the pellet-shaped liquid crystal polymer resin composition was calculated by the following formula (5). The results are shown in Table 1. Lw=Σ Li 2 / Σ Li (5) Lw: Weight average fiber length Li: Circumscribed rectangle major axis of the i-th carbon fiber Number of measurements: 30,000
[0121] <Preparation of injection molded test pieces> The pellet-shaped liquid crystal polymer resin compositions of Examples 1 to 10 and Comparative Examples 1 to 10 were loaded into an injection molding machine UH1000 (Nissei Plastics Industry) with a cylinder temperature of 340°C, and injected into a mold with a mold temperature of 120°C at an injection speed of 20 mm / s, a screw rotation speed of 100 rpm, a holding pressure of 50 MPa, and a back pressure of 3 MPa to produce injection-molded test pieces (surface roughness Ra = 3 μm) of 64 mm x 64 mm x 3 mmt.
[0122] <Measurement of surface resistance of injection molded test pieces> Using a resistance measurement system (PRS-801) and a sensor electrode (PRF-912) manufactured by PROSTAT, Inc., USA, the surface resistance value of each of the injection-molded test pieces of 64 mm × 64 mm × 3 mmt made of the resin compositions of Examples 1 to 10 and Comparative Examples 1 to 10 was measured. The results are shown in Table 1.
[0123] <Tape peelability test> A 25 mm wide electroplating tape (3M, 470 Electroplating Tape S10258) was attached to the injection molded test piece of 64 mm x 64 mm x 3 mmt made of the resin composition of Example 1 in the molding direction (MD) of the test piece using a pressure roller of 2.0 kg mass according to JIS Z0237, and after leaving it for 24 hours, it was peeled off to observe whether the skin layer of the liquid crystal polymer on the surface of the injection molded test piece peeled off. The electroplating tape was similarly attached to the same location in the molding direction (MD) of the test piece, left for 24 hours, and peeled off to observe whether the skin layer of the liquid crystal polymer on the surface of the injection molded test piece peeled off. This was repeated four times, for a total of five times. The electroplating tape was similarly applied to the same location of the same injection-molded test piece in the MD and perpendicular direction (TD) of the test piece, left for 24 hours, and then peeled off to observe whether or not the liquid crystal polymer skin layer on the surface of the injection-molded test piece had peeled off. This process was repeated five times. The peeling test was repeated 10 times and the tape peelability was evaluated according to the following criteria. Tape peelability criteria E (Excellent): No peeling of the skin layer occurred in 9 to 10 sheets out of N=10. G (Good): Skin layer not peeling off in 5 to 9 sheets out of N=10 F (Failure): Fewer than 5 out of 10 sheets had no peeling of the skin layer
[0124] The same evaluation was performed on injection-molded test pieces of 64 mm×64 mm×3 mmt made of the resin compositions of Examples 2 to 10 and Comparative Examples 1 to 10. The results are shown in Table 1.
[0125] [Table 1]
[0126] As can be seen from the results in Table 1, the liquid crystal polymer resin compositions of Examples 1 to 10 to which the present invention is applied, in which the content ratio of the component (B') is 10 to 30 parts by mass relative to 100 parts by mass of the component (A), the content ratio of the component (C) is 5 to 35 parts by mass relative to 100 parts by mass of the component (A), and the total content ratio of the components (B') and (C) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A), had a 1.0×10 5 ~1.0×10 11 It was shown that a molded article having a surface resistance value in a suitable static electricity dissipation region of Ω and excellent tape peelability could be molded.
[0127] In contrast, as shown in Table 1, the molded articles made of the liquid crystal polymer resin compositions of Comparative Examples 1, 5, 7 to 8, and 10 have excellent tape peelability, but the tape peelability is 1.0×10 5 ~1.0×10 11 The molded articles made of the liquid crystal polymer resin compositions of Comparative Examples 2 to 4, 6, and 9 did not exhibit a surface resistance value of 1.0×10 5 ~1.0×10 11 Although it exhibits a surface resistance value of Ω, which is in a moderate static electricity dissipation region, there is a problem with tape peelability.
[0128] Therefore, the liquid crystal polymer resin composition of the present invention can be suitably used for semiconductor transport carriers. [Explanation of symbols]
[0129] 1 semiconductor transport carrier, 11 main body, 12 tape attachment section
Claims
1. A liquid crystal polymer resin composition comprising the following components (A), (B'), and (C): (A) Liquid crystal polymer (B') Carbon fiber having a weight average fiber length of less than 150 μm (C) Volume resistivity is 10 2 ~10 10 Carbon precursor with a density of Ω cm the content ratio of the component (B') is 10 to 30 parts by mass relative to 100 parts by mass of the component (A), the content ratio of the component (C) is 5 to 35 parts by mass relative to 100 parts by mass of the component (A), and the total content ratio of the components (B') and (C) is 25 to 60 parts by mass relative to 100 parts by mass of the component (A); Further, the composition contains component (D) conductive carbon black, The liquid crystal polymer resin composition, wherein the total content of the components (B'), (C) and (D) is 25 to 60 parts by mass per 100 parts by mass of the component (A).
2. A semiconductor transport carrier having a body made of the liquid crystal polymer resin composition according to claim 1.
3. A method for producing a liquid crystal polymer resin composition by melt-kneading the following components (A), (B), and (C): (A) Liquid crystal polymer (B) Carbon fiber having a weight average fiber length of less than 3000 μm (C) Volume resistivity is 10 2 ~10 10 Carbon precursor with a density of Ω cm the blending ratio of the component (B) is 10 to 30 parts by mass with respect to 100 parts by mass of the component (A), the blending ratio of the component (C) is 5 to 35 parts by mass with respect to 100 parts by mass of the component (A), and the blending ratio of the total of the components (B) and (C) is 25 to 60 parts by mass with respect to 100 parts by mass of the component (A); The liquid crystal polymer resin composition further contains component (D) conductive carbon black, A method for producing a liquid crystal polymer resin composition, wherein the total blending ratio of the components (B), (C) and (D) is 25 to 60 parts by mass per 100 parts by mass of the component (A).
Citation Information
Patent Citations
Synthetic resin composition and synthetic resin molding
JP1997087418A
Semiconductive resin composition
JP2002121402A
Resin composition, method for producing the same and use of the same
JP2009127038A
IC socket
WO2002082592A1