Film, film manufacturing method, and water-repellent film

By transferring an uneven structure onto a film surface at specific temperature and vacuum conditions, the film achieves uniform surface properties and consistent water repellency.

JP7564728B2Active Publication Date: 2024-10-09SUMITOMO CHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021021727
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-15
Publication Date
2024-10-09
Estimated Expiration
2041-02-15

AI Technical Summary

Technical Problem

Existing films with uneven structures on their surfaces suffer from non-uniformity in surface properties such as water repellency.

Method used

A film with an uneven structure on at least one surface, having a coefficient of variation of arithmetic mean height Sa of 0.25 or less and coefficient of variation of average length ZSm of 0.082 or less, is produced by transferring the structure using a mold at temperatures of 100°C or higher and a vacuum of -0.07 MPa or less.

Benefits of technology

The method achieves a film with relatively uniform surface properties, enabling consistent water repellency and other functional properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564728000001
    Figure 0007564728000001
Patent Text Reader

Abstract

To provide a film having relatively uniform surface properties.SOLUTION: A film contains resin. At least one surface of the film has an uneven structure. In the one surface of the film having the uneven structure, a coefficient of variation in an arithmetical average height Sa is 0.25 or less, and a coefficient of variation in an average length ZSm of elements is 0.082 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin-containing film, a method for producing the film, and a water-repellent film made of the film. [Background technology]

[0002] Various films are used as packaging materials for food, medicine, etc., and as components for industrial products, etc. Surface properties required for such films include water repellency, oil repellency, low reflectivity, etc. Films having these surface properties are known to have a fine uneven structure on at least one surface. Examples of methods for producing films having such an uneven structure include a method of transferring a fine uneven structure to the surface of an original film using a mold having a fine unevenness on its surface (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-25053 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the film produced as described above has a problem in that the uniformity of surface properties such as water repellency is relatively low.

[0005] Therefore, an object of the present invention is to provide a film having relatively uniform surface properties, a method for producing the film, and a water-repellent film made of the film. [Means for solving the problem]

[0006] The film of the present invention is a film containing a resin and has a concave-convex structure on at least one of the film surfaces, and the one of the film surfaces having the concave-convex structure has a coefficient of variation of the arithmetic mean height Sa of 0.25 or less and a coefficient of variation of the average element length ZSm of 0.082 or less.

[0007] The water-repellent film according to the present invention comprises the above-mentioned film.

[0008] The film manufacturing method of the present invention is a film manufacturing method including a transfer step of using a mold having a concave-convex structure on its surface to transfer the concave-convex structure to at least one surface of an original film containing a resin, the transfer step being carried out under conditions of a temperature of 100°C or higher and a degree of vacuum of -0.07 MPa or lower in gauge pressure. Effect of the Invention

[0009] According to the present invention, it is possible to provide a film having relatively uniform surface properties, a method for producing the film, and a water-repellent film made of the film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The film according to this embodiment contains a resin (for example, is made of a resin formed into a sheet).

[0011] (resin) The resin constituting the film may be composed of only a polymer, or may contain additives other than the polymer. The mass ratio of the polymer in the resin is not particularly limited, and may be, for example, 50% or more, 70% or more, 90% or more, or 95% or more.

[0012] Examples of the additives include antioxidants, weather resistance agents, lubricants, antiblocking agents, antistatic agents, antifogging agents, anti-dripping agents, pigments, and fillers.

[0013] Examples of the resin constituting the film include polyolefin resins, (meth)acrylic resins, polycarbonate resins, polyetherimide resins, polyester resins, polystyrene resins, polyethersulfone resins, fluorine resins, ABS (acrylonitrile-butadiene-styrene) resins, AS (acrylonitrile-styrene) resins, polyvinyl chloride resins, etc. The resin constituting the film may be one selected from these resins, or a mixture of multiple resins. Among these resins, the resin constituting the film is preferably a polyolefin resin.

[0014] (Polyolefin resin) Examples of polyolefin resins include polyethylene resins and polypropylene resins.

[0015] (Polyethylene resin) The polyethylene resin includes an ethylene polymer. Examples of the ethylene polymer include an ethylene homopolymer, a copolymer of ethylene and an α-olefin, and a copolymer of ethylene and an α-olefin substituted with an alicyclic compound. The ethylene polymer may be a mixture of an ethylene homopolymer and a copolymer of ethylene and an α-olefin. The amount of structural units derived from an α-olefin in the ethylene polymer is not particularly limited, and may be, for example, 4.0 to 20% by mass.

[0016] Examples of ethylene homopolymers include high-pressure low-density polyethylene (LDPE) produced by high-pressure radical polymerization using a radical initiator. High-pressure low-density polyethylene (LDPE) is a polymer in which repeating units of ethylene are randomly bonded to form a branched structure. High-pressure low-density polyethylene (LDPE) has a density of, for example, 910 to 935 kg / m 3 may be also possible.

[0017] Examples of the copolymer of ethylene and an α-olefin include linear low density polyethylene having crystallinity, and elastomers of copolymers of ethylene and an α-olefin having low crystallinity and rubber-like elastic properties.

[0018] The density of the linear low density polyethylene is, for example, 900 to 940 kg / m 3 The density of the elastomer of the copolymer of ethylene and α-olefin may be, for example, 860 to 900 kg / m 3 may be also possible.

[0019] Examples of the α-olefin include α-olefins having 3 to 10 carbon atoms. Examples of the α-olefins having 3 to 10 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, and 3-methyl-1-butene. An α-olefin having 4 to 10 carbon atoms is preferable, and 1-butene, 1-hexene, or 1-octene is more preferable.

[0020] Examples of the copolymer of ethylene and an α-olefin include an ethylene-1-butene copolymer, an ethylene-1-hexene copolymer, an ethylene-1-octene copolymer, an ethylene-1-decene copolymer, an ethylene-(3-methyl-1-butene) copolymer, etc. The copolymer of ethylene and an α-olefin may be one of these alone or a mixture of two or more of them.

[0021] An example of an α-olefin substituted with an alicyclic compound is vinylcyclohexane.

[0022] The melt flow rate (MFR) of the ethylene polymer measured at a measurement temperature of 190° C. under a load of 2.16 kg is preferably 0.5 to 50 g / 10 min, more preferably 1 to 30 g / 10 min, and further preferably 1 to 20 g / 10 min.

[0023] The ethylene polymer can be produced by a known polymerization method using a known polymerization catalyst.

[0024] Examples of the polymerization catalyst include homogeneous catalyst systems such as metallocene catalysts, Ziegler-type catalyst systems, Ziegler-Natta-type catalyst systems, etc. Examples of the homogeneous catalyst systems include catalyst systems consisting of a transition metal compound of Group 4 of the periodic table having a cyclopentadienyl ring and an alkylaluminoxane, or catalyst systems consisting of a transition metal compound of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that reacts with the transition metal compound to form an ionic complex, and an organoaluminum compound, catalyst systems in which inorganic particles such as silica and clay minerals are supported and modified with catalyst components such as a transition metal compound of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that forms an ionic complex, and an organoaluminum compound, and prepolymerization catalyst systems prepared by prepolymerizing ethylene or α-olefins in the presence of the above catalyst systems.

[0025] Moreover, a radical initiator can be used as a polymerization catalyst for high-pressure low-density polyethylene (LDPE).

[0026] (Polypropylene resin) The polypropylene-based resin includes a propylene-based polymer. Examples of the propylene-based polymer include a propylene homopolymer and a copolymer of propylene and ethylene and / or an α-olefin having 4 to 10 carbon atoms. The propylene-based polymer may be a mixture of a propylene homopolymer and a copolymer of propylene and ethylene and / or an α-olefin having 4 to 10 carbon atoms.

[0027] The propylene homopolymer may have a melt flow rate (MFR) of 0.1 to 50 g / 10 min, measured at a measurement temperature of 230° C. under a load of 2.16 kg.

[0028] The copolymer of ethylene and / or an α-olefin having 4 to 10 carbon atoms with propylene may have a melt flow rate (MFR) of 10 to 200 g / 10 min, measured at a measurement temperature of 230° C. under a load of 2.16 kg.

[0029] When the total mass of the copolymer of ethylene and / or an α-olefin having 4 to 10 carbon atoms and propylene is taken as 100 mass%, the structural units derived from ethylene and / or an α-olefin having 4 to 10 carbon atoms may be 0.1 to 40 mass%, and the structural units derived from propylene may be 99.9 to 60 mass%.

[0030] As used herein, the term "structural unit" in a term such as "structural unit derived from ethylene" refers to a polymerized unit of a monomer. Thus, for example, a "structural unit derived from ethylene" refers to a -CH2CH2- structural unit.

[0031] Examples of the α-olefin having 4 to 10 carbon atoms include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene, and preferably 1-butene, 1-hexene, or 1-octene.

[0032] Examples of the copolymer of propylene with ethylene and / or an α-olefin having 4 to 10 carbon atoms include a random copolymer of propylene and ethylene, a random copolymer of propylene and an α-olefin having 4 to 10 carbon atoms, a random copolymer of propylene, ethylene and an α-olefin having 4 to 10 carbon atoms, a propylene block copolymer, etc. The copolymer of propylene with ethylene and / or an α-olefin having 4 to 10 carbon atoms may be one type selected from these alone or a mixture of two or more types.

[0033] Examples of the random copolymer of propylene and an α-olefin having 4 to 10 carbon atoms include a propylene-1-butene random copolymer, a propylene-1-hexene random copolymer, a propylene-1-octene random copolymer, and a propylene-1-decene random copolymer.

[0034] Examples of the random copolymer of propylene, ethylene, and an α-olefin having 4 to 10 carbon atoms include a propylene-ethylene-1-butene copolymer, a propylene-ethylene-1-hexene copolymer, a propylene-ethylene-1-octene copolymer, and a propylene-ethylene-1-decene copolymer.

[0035] The propylene polymer can be produced by a known polymerization method using a known olefin polymerization catalyst.

[0036] Examples of the polymerization catalyst include a Ziegler type catalyst system, a Ziegler-Natta type catalyst system, a catalyst system consisting of a transition metal compound of Group 4 of the periodic table having a cyclopentadienyl ring and an alkylaluminoxane, or a catalyst system consisting of a transition metal compound of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that reacts with it to form an ionic complex, and an organoaluminum compound, a catalyst system in which inorganic particles such as silica, clay minerals, etc. are supported and modified with catalytic components such as a transition metal compound of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that forms an ionic complex, and an organoaluminum compound, and a prepolymerization catalyst system prepared by prepolymerizing ethylene or an α-olefin in the presence of the above catalyst system.

[0037] (Acrylic resin) The acrylic resin includes an acrylic polymer, such as a polymer of an acrylic acid derivative, such as acrylic acid or an ester thereof, a polymer of a methacrylic acid derivative, such as methacrylic acid or an ester thereof, and a copolymer of an acrylic acid derivative and a methacrylic acid derivative.

[0038] Examples of acrylic polymers include methacrylic homopolymers containing only monomer units derived from alkyl methacrylates having an alkyl group with 1 to 4 carbon atoms; and methacrylic copolymers having 50% by mass or more and less than 100% by mass of monomer units derived from alkyl methacrylates having an alkyl group with 1 to 4 carbon atoms, and more than 0% by mass and 50% by mass or less of monomer units derived from other vinyl monomers copolymerizable with the monomer units derived from alkyl methacrylates having an alkyl group with 1 to 4 carbon atoms.

[0039] The above-mentioned "alkyl methacrylate having an alkyl group having 1 to 4 carbon atoms" is a compound represented by CH2=CH(CH3)COOR (R is an alkyl group having 1 to 4 carbon atoms). The vinyl monomer copolymerizable with the alkyl methacrylate having an alkyl group having 1 to 4 carbon atoms is a monomer which is copolymerizable with the alkyl methacrylate having an alkyl group having 1 to 4 carbon atoms and has a vinyl group.

[0040] Examples of the alkyl methacrylate having an alkyl group having 1 to 4 carbon atoms include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, sec-butyl methacrylate, and isobutyl methacrylate. The alkyl methacrylate having an alkyl group having 1 to 4 carbon atoms is preferably methyl methacrylate. The alkyl methacrylate may be used alone or in combination of two or more.

[0041] Examples of the vinyl monomer copolymerizable with the alkyl methacrylate having an alkyl group having 1 to 4 carbon atoms include methacrylic acid esters such as cyclohexyl methacrylate, benzyl methacrylate, 2-ethylhexyl methacrylate, 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, and monoglycerol methacrylate (excluding alkyl methacrylates having an alkyl group having 1 to 4 carbon atoms); methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, acrylic Examples of suitable monomers include acrylic acid esters such as 2-hydroxypropyl acetate and monoglycerol acrylate; unsaturated carboxylic acids or anhydrides thereof such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, maleic anhydride and itaconic anhydride; nitrogen-containing monomers such as acrylamide, methacrylamide, acrylonitrile, methacrylonitrile, diacetone acrylamide and dimethylaminoethyl methacrylate; epoxy group-containing monomers such as allyl glycidyl ether, glycidyl acrylate and glycidyl methacrylate; and styrene-based monomers such as styrene and α-methylstyrene.

[0042] Examples of a method for producing the acrylic polymer include a method of polymerizing an alkyl methacrylate having an alkyl group having 1 to 4 carbon atoms and, if necessary, a vinyl monomer copolymerizable with the alkyl methacrylate having an alkyl group having 1 to 4 carbon atoms by a method such as bulk polymerization, solution polymerization, suspension polymerization, or emulsion polymerization.

[0043] (Polycarbonate resin) The polycarbonate resin includes a polymer containing a structural unit derived from a dihydroxy compound. Examples of the polymer include those obtained by reacting a dihydroxy compound such as a dihydric phenol or isosorbide with a carbonylating agent by an interfacial polycondensation method or a melt transesterification method, those obtained by polymerizing a carbonate prepolymer by a solid-phase transesterification method, and those obtained by polymerizing a cyclic carbonate compound by a ring-opening polymerization method.

[0044] Examples of dihydric phenols include hydroquinone, resorcinol, 4,4'-dihydroxydiphenyl, bis(4-hydroxyphenyl)methane, bis{(4-hydroxy-3,5-dimethyl)phenyl}methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A), 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane, 2,2-bis{(4-hydroxy-3,5-di 2,2-bis{(4-hydroxy-3,5-dibromo)phenyl}propane, 2,2-bis{(3-isopropyl-4-hydroxy)phenyl}propane, 2,2-bis{(4-hydroxy-3-phenyl)phenyl}propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)-3-methylbutane, 2,2-bis(4-hydroxyphenyl)-3,3-dimethylbutane, 2,4-bis(4-hydroxyphenyl)-2-methylbutane, 2,2-bis(4-hydroxyphenyl)- 1,1-bis(4-hydroxyphenyl)pentane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-4-isopropylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis{(4-hydroxy-3-methyl)phenyl}fluorene, α,α'-bis(4-hydroxyphenyl)-o-diisopropylbenzene, α ,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene, α,α'-bis(4-hydroxyphenyl)-p-diisopropylbenzene, 1,3-bis(4-hydroxyphenyl)-5,7-dimethyladamantane, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenyl ether, and 4,4'-dihydroxydiphenyl ester. These may be used alone or in combination of two or more.

[0045] Among these dihydric phenols, bisphenol A, 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)-3-methylbutane, 2,2-bis(4-hydroxyphenyl)-3,3-dimethylbutane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, and α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene are preferred. In particular, the use of bisphenol A alone or the use of bisphenol A in combination with at least one selected from the group consisting of 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane, and α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene is preferred.

[0046] Examples of carbonylating agents include carbonyl halides (phosgene, etc.), carbonate esters (diphenyl carbonate, etc.), and haloformates (dihaloformates of dihydric phenols, etc.), which may be used alone or in combination of two or more.

[0047] The film according to the present embodiment has a concave-convex structure on at least one of the film surfaces (specifically, only one of the film surfaces or both of the film surfaces). The ratio of the area of ​​the region on one of the film surfaces where the concave-convex structure is formed to the entire area of ​​the one of the film surfaces may be, for example, 80% or more, or may be 100% (i.e., the concave-convex structure may be formed over the entire area of ​​the one of the film surfaces). In addition, the concave-convex structure of the film according to the present embodiment may be formed by assembling a plurality of truncated cone structures or a plurality of hemispherical structures.

[0048] In addition, in the film according to the present embodiment, the coefficient of variation of the arithmetic mean height Sa of one film surface (film surface having a concave-convex structure) is 0.25 or less, preferably 0.20 or less, more preferably 0.15 or less. The arithmetic mean height Sa is preferably 0.002 μm to 2.5 μm, more preferably 0.04 μm to 2.0 μm. In addition, in such a film, the coefficient of variation of the average element length ZSm of one film surface (film surface having a concave-convex structure) is 0.082 or less, preferably 0.080 or less. The average element length ZSm is preferably 1 μm to 20 μm, more preferably 1.2 μm to 18 μm. The arithmetic mean height Sa, the coefficient of variation of the arithmetic mean height Sa, the average element length ZSm, and the coefficient of variation of the average element length ZSm can be determined by the method described in the following examples.

[0049] The thickness of the film may be, for example, 10 μm or more and less than 250 μm, or 15 μm to 150 μm. The thickness of the film is the thickness of the entire film in the region having the concave-convex structure. The thickness of the film can be obtained by measuring the region having the concave-convex structure by pinching it with a micrometer.

[0050] <Film manufacturing method> Next, a method for producing the film configured as described above will be described. The method for producing such a film includes a transfer step of transferring a concave-convex structure to at least one surface of an original film containing a resin (for example, composed of a resin molded into a sheet shape) using a mold having a concave-convex structure on its surface.

[0051] The mold used in the transfer step is not particularly limited, and may be, for example, a flat mold or a cylindrical mold. In addition, it is preferable that the mold is capable of heating the original film to a predetermined temperature. When the transfer step is performed using a flat mold, the original film is sandwiched between a flat mold and a metal plate having a flat surface, and the original film is pressed between the flat mold and the metal plate to perform the transfer step. In addition, when the transfer step is performed using a cylindrical mold, the original film is sandwiched between a cylindrical mold and a nip roller, and the original film is pressed between the cylindrical mold and the nip roller while being unwound, to perform the transfer step.

[0052] The uneven structure of the mold may be formed by assembling a plurality of truncated cone structures or a plurality of hemispherical structures. The height of the uneven structure of the mold (specifically, the height of the convex structure) may be, for example, 0.25 μm to 4 μm, 0.25 μm to 1.5 μm, or 1.5 μm to 4 μm. The interval of the uneven structure of the mold (specifically, the interval (pitch) between the convex structures) may be, for example, 0.25 μm to 8 μm, 0.25 μm to 3 μm, or 3 μm to 8 μm.

[0053] The transfer step is carried out at 100°C or higher, preferably 150°C or higher, more preferably 150°C to 200°C. The temperature of the transfer step can be obtained by measuring the temperature of the mold (specifically, the surface of the mold having a concave-convex structure). The transfer step is carried out in an environment with a vacuum of -0.07MPa or lower, preferably -0.08MPa to -0.1MPa, in terms of gauge pressure. The vacuum degree (gauge pressure) represents the difference between the environment in which the transfer step is carried out (hereinafter also referred to as the transfer environment) and the atmospheric pressure. Examples of a method for setting the transfer environment to a predetermined vacuum degree include a method of degassing the air from the transfer environment. That is, the film manufacturing method may include a degassing step of degassing the air from the transfer environment in addition to the above transfer step. The degassing step is preferably carried out before the raw film comes into contact with the mold. In addition, when performing the transfer process, in order to prevent adhesion between the various types of molds described above and the original film, a release film may be sandwiched between the mold (e.g., a flat mold) and the original film, or a release process may be performed such as applying a release agent to the mold (e.g., a flat mold or a cylindrical mold).

[0054] The film manufacturing method may further include other steps. For example, the method may include a cooling step of cooling the film after the transfer step. The cooling step can be performed by sandwiching the film after the transfer step between cooling plates or cooling rolls at a relatively low temperature.

[0055] The film configured as described above can be used as, for example, a water-repellent film or a low-reflectivity film. These films (hereinafter also referred to as "functional films") can be used, for example, as the outermost layer of a laminate. When the functional film is used as the outermost layer of a laminate, the functional film is arranged so that the film surface having the uneven structure is the outermost surface of the laminate. By positioning the uneven structure on the outermost surface of the laminate, the surface properties of the functional film can be imparted to the laminate. The functional film may also be used alone without being laminated with other layers. Examples of applications of the water-repellent film include packaging materials for packaging food and the like. Specifically, a laminate having a water-repellent film on the outermost layer can be used as a packaging material for a lid material of a packaging container, a container body, and the like. When the water-repellent film is used as a packaging material, the uneven structure of the water-repellent film is used so as to be positioned on the content side, thereby suppressing adhesion or remaining of viscous contents such as liquids, semi-solids, and gel-like substances to the packaging material. Examples of applications of the low-reflectivity film include materials constituting liquid crystal displays and the like.

[0056] As described above, according to the present embodiment, it is possible to provide a film having a relatively uniform surface texture, a method for producing the film, and a water-repellent film made of the film.

[0057] In other words, by having a concave-convex structure on at least one of the film surfaces and the coefficient of variation of the arithmetic mean height Sa and the coefficient of variation of the average element length ZSm of one of the film surfaces having the concave-convex structure being within the above-mentioned ranges, a film having relatively uniform surface properties can be provided.

[0058] Furthermore, since the resin constituting the film is a polyolefin-based resin, such a film can be used as a heat seal layer of a packaging material.

[0059] Furthermore, since the polyolefin resin constituting the film is a polyethylene resin, the film can be used as a packaging material for heavy goods or for freezing purposes.

[0060] Furthermore, by making the film thickness 10 μm or more and less than 250 μm, a flexible functional film can be obtained.

[0061] Furthermore, by using the above-mentioned film as a water-repellent film, it is possible to provide a water-repellent film that exhibits relatively uniform water repellency.

[0062] In addition, in the film manufacturing method, a film having a relatively uniform surface property can be obtained by performing the transfer process under the above-mentioned temperature range and vacuum range. Specifically, in the past, when a concave-convex structure was transferred to an original film using a mold, air may get between the original film and the mold, and transfer failure may occur in the area where the air got in. When such transfer failure occurs, an area that does not show the desired surface property is formed in a part of the film, so that a film having a uniform surface property cannot be obtained. In contrast, by performing the transfer process under conditions of a predetermined temperature range and a predetermined vacuum range as in the above embodiment, it is possible to suppress air from getting between the mold and the original film, and to obtain a film having a uniform surface property. EXAMPLES

[0063] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.

[0064] <Density (unit: g / cm 3 )> The density of the polyethylene resin was measured according to the method A specified in JIS K7112-1980 after annealing as specified in JIS K6760-1995.

[0065] <Melt flow rate (MFR, unit: g / 10 min)> The MFR of the polyethylene resin was measured according to Method A specified in JIS K7210-1995 at a temperature of 190° C. and a load of 2.16 kg.

[0066] <Variation coefficient of arithmetic mean height Sa (unit: μm) of resin film surface> First, the resin film surface was measured using a white microscope (Hitachi High-Tech Science Corporation, product name: Nano 3D Optical Interference Measurement System VS1800). In Examples 1 to 4 and Comparative Example 1, the objective lens was set at 50x and the measurement mode was HiSlope HR (piezo), and in Example 5, the objective lens was set at 110x and the measurement mode was Phase (piezo). Next, a one-dimensional surface correction (a region where the sum of the squares of the absolute values ​​of the unevenness heights is smallest is calculated, and the inclination of the image is corrected so that the region is in the Z direction) was performed on the obtained image of the resin film surface using Hitachi High-Tech's "VS-viewer". Next, the arithmetic mean height Sa was measured according to the method specified in ISO 25178. By this method, Sa was measured at 12 points on the resin film surface (12 intersections between a straight line that divides the resin film into 5 equal parts vertically and a straight line that divides the resin film into 4 equal parts horizontally) and the variation coefficients of these were calculated.

[0067] <Coefficient of variation of the average length ZSm (unit: μm) of the elements on the resin film surface> First, the resin film surface was measured using a white microscope (Hitachi High-Tech Corporation, Nano 3D Optical Interference Measurement System VS1800). In Examples 1 to 4 and Comparative Example 1, the objective lens was set at 50x magnification and the measurement mode was HiSlope HR (piezo), and in Example 5, the objective lens was set at 110x magnification and the measurement mode was Phase (piezo). Next, a one-dimensional surface correction (a region where the sum of the squares of the absolute values ​​of the unevenness heights is smallest, and the inclination of the image is corrected so that the region is in the Z direction) was performed on the obtained image of the resin film surface using Hitachi High-Tech's "VS-viewer". Next, on the unevennesses that are arranged at equal intervals including the convex closest to the center of the Y axis and that are most parallel to the X axis, a line was selected so as to include both the left and right sides of the image, and a cross-sectional profile on that line was obtained. From the obtained cross-sectional profile, the average length ZSm of the elements on the resin film surface was measured according to the method specified in ISO 4287. Using this method, ZSm was measured at 12 points on the resin film surface (12 intersections of a line dividing the resin film into 5 equal parts vertically and a line dividing the resin film into 4 equal parts horizontally), and the coefficient of variation was calculated.

[0068] <Observation of the uneven structure of a resin film surface> The uneven structure of the resin film surface was observed using a reflection electron microscope (S-4800, manufactured by Hitachi High-Technologies Corporation).

[0069] <Water contact angle on the resin film surface (unit: °) and its standard deviation (unit: °)> First, the water contact angle of the resin film surface was measured using a contact angle measuring instrument (manufactured by Kyowa Interface Science Co., Ltd., product name: DM-301). Specifically, the resin film (5 cm square) was divided into two equal parts in the vertical and horizontal directions (i.e., the resin film was divided into four parts), and the water contact angle was measured at a total of 50 points, 5 points in the vertical direction and 10 points in the horizontal direction, in one area. Next, the standard deviation of the water contact angle of the resin film surface was calculated.

[0070] <Example 1: Preparation of resin film 1> Polyethylene resin (manufactured by Sumitomo Chemical Co., Ltd., product name "Sumikathene E (registered trademark) FV203N, density: 0.913 g / cm 3 A 50 μm thick original resin film made of a 50 μm thick resin having a surface roughness (HON70-3000, manufactured by Soken Chemical Industries, Ltd., height of the roughness: 1.5 μm, pitch of the roughness: 3 μm) was sandwiched between a metal plate having a flat surface and a mold having a roughness structure on the surface (HON70-3000, manufactured by Soken Chemical Industries, Ltd., height of the roughness structure: 1.5 μm, pitch of the roughness structure: 3 μm), and then pressed for 5 minutes at 150 ° C. and 0 MPa (vacuum degree is −0.1 MPa in gauge pressure) using a manual hydraulic vacuum heating press (IMC-19E6, manufactured by Imoto Manufacturing Co., Ltd.). The obtained resin film was pressed and cooled for 5 minutes at 30 ° C. and 0.1 MPa using a cooling press (IMC-19E7, manufactured by Imoto Manufacturing Co., Ltd.) to produce a resin film 1 having a roughness structure on the surface.

[0071] <Example 2: Preparation of resin film 2> A resin film 2 having an uneven surface structure was produced in the same manner as in Example 1, except that pressing was performed under conditions of 150° C. and 0.01 MPa (vacuum degree: −0.09 MPa in gauge pressure).

[0072] <Example 3: Preparation of resin film 3> A resin film 3 having an uneven surface structure was produced in the same manner as in Example 1, except that pressing was performed under conditions of 150° C. and 0.02 MPa (vacuum degree: −0.08 MPa in gauge pressure).

[0073] <Example 4: Preparation of resin film 4> A resin film 4 having a concave-convex structure on its surface was produced in the same manner as in Example 1, except that a mold having a concave-convex structure on its surface (manufactured by TOWA Corporation, microlens array, height of concave-convex structure: 4 μm, pitch of concave-convex structure: 8 μm) was used.

[0074] <Example 5: Preparation of resin film 5> A resin film 5 having a concave-convex structure on its surface was produced in the same manner as in Example 1, except that a mold having a concave-convex structure on its surface (HON70-250, manufactured by Soken Chemical Industry Co., Ltd., height of concave-convex structure: 0.25 μm, pitch of concave-convex structure: 0.25 μm) was used.

[0075] <Comparative Example 1: Preparation of resin film C1> A resin film C1 having an uneven surface structure was produced in the same manner as in Example 1, except that pressing was performed under conditions of 150° C. and 0.1 MPa (degree of vacuum: 0 MPa gauge pressure).

[0076] [Table 1]

[0077] <Summary> From Table 1, it can be seen that the standard deviation of the water contact angle is smaller in each Example (i.e., the water repellency is relatively uniform) than in Comparative Example 1. This indicates that the uneven structure is formed relatively uniformly on one side of the resin film. From the above, by transferring the uneven structure to the original resin film within the temperature and vacuum ranges of the present invention, it is possible to obtain a film with relatively uniform surface properties (i.e., a resin film in which the coefficient of variation of the arithmetic mean height Sa of the film surface and the coefficient of variation of the average element length ZSm are within the ranges of the present invention).

Claims

1. A film containing a resin, At least one of the film surfaces has an uneven structure, The one film surface having the uneven structure has a coefficient of variation of an arithmetic mean height Sa of 0.25 or less and a coefficient of variation of an average element length ZSm of 0.082 or less, The average length ZSm of the elements is 1 μm to 20 μm; The resin is a polyolefin resin. film.

2. The coefficient of variation of the arithmetic mean height Sa is 0.20 or less. The film of claim 1.

3. The coefficient of variation of the arithmetic mean height Sa is 0.15 or less. The film of claim 2.

4. The coefficient of variation of the average length ZSm of the elements is 0.080 or less. The film according to any one of claims 1 to 3.

5. The arithmetic mean height Sa is 0.002 μm to 2.5 μm. The film according to any one of claims 1 to 4.

6. The uneven structure is formed by assembling a plurality of truncated cone structures or a plurality of hemispherical structures. The film according to any one of claims 1 to 5.

7. The polyolefin resin is a polyethylene resin. The film according to any one of claims 1 to 6.

8. The thickness is 10 μm or more and less than 250 μm. The film according to any one of claims 1 to 7.

9. A water-repellent film comprising the film according to any one of claims 1 to 8.

10. A method for producing a film, comprising a transfer step of transferring a concave-convex structure to at least one surface of an original film containing a polyolefin resin using a mold having a concave-convex structure on the surface, The transfer step is carried out under conditions of a temperature of 100° C. or higher and a degree of vacuum of −0.07 MPa or lower in gauge pressure.

Citation Information

Patent Citations

  • Method for manufacturing recording medium, and recording medium manufacturing apparatus

    JP2002042387A

  • Method for manufacturing optical plate-like member

    JP2002192600A

  • Water-repellent film, laminate, and packaging material

    JP2015025053A

  • Optical sheet, edge light-type backlight unit, and optical sheet manufacturing method

    JP2016028275A

  • Plastic molded body

    JP2016088947A