Polyacetal resin composition and its manufacturing method

By controlling moisture content during the blending of cellulose nanofibers with polyacetal resin within specific ranges, the issues of odor, surface irregularities, and void formation in molded products are mitigated, resulting in improved resin composition performance.

JP7564943B2Active Publication Date: 2024-10-09ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023513064
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-11-04
Filing Date
2022-04-08
Publication Date
2024-10-09
Estimated Expiration
2042-04-08

AI Technical Summary

Technical Problem

Conventional polyacetal resin compositions blended with cellulose nanofibers suffer from odor generation, surface irregularities due to gas formation, and variations in tensile properties due to voids in the molded products.

Method used

Control the moisture content of cellulose nanofibers within a specific range (0.01% to 5% by mass) during melt-kneading with polyacetal resin, and maintain the moisture content of the resin composition between 0.03% to 0.3% by mass to suppress decomposition and void formation.

Benefits of technology

Prevents odor and gas generation, reduces surface irregularities, and stabilizes tensile properties by minimizing voids in the molded products, enhancing the overall performance of the resin composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564943000001
    Figure 0007564943000001
  • Figure 0007564943000002
    Figure 0007564943000002
  • Figure 0007564943000003
    Figure 0007564943000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide a resin composition and a molded product thereof with which it is possible to avoid problems such as the generation of odor and gas from the resin composition and the occurrence of voids in the molded product, and methods for manufacturing the resin composition and the molded product. The present invention provides a method for manufacturing a resin composition containing cellulose nanofibers and a polyacetal resin, the method including a step for obtaining a resin composition by melt-mixing mixed ingredients that include cellulose nanofibers and a polyacetal resin in a state in which the water content of the cellulose nanofibers is 0.01–5 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyacetal resin composition and a method for producing the same. [Background technology]

[0002] Polyacetal resins have excellent mechanical properties, thermal properties, electrical properties, sliding properties, moldability, etc., and are widely used mainly as structural materials and mechanism parts in electrical equipment, automobile parts, precision machine parts, etc. In particular, polyacetal resins are widely used in gear applications because of their good mechanical properties and excellent sliding properties.

[0003] Patent Document 1 describes a polyacetal resin composition in which a specific cellulose powder is blended with a polyacetal resin. Patent Document 2 describes a polyacetal resin composition in which a cellulose nanofiber having a specific aspect ratio and average fiber length is blended with a polyacetal resin. Patent Document 3 describes a resin composition containing chemically modified cellulose nanofibers and a thermoplastic resin which may be polyacetal. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2010 / 119810 [Patent Document 2] International Publication No. 2012 / 049926 [Patent Document 3] International Publication No. 2016 / 148233 Summary of the Invention [Problem to be solved by the invention]

[0005] However, conventional techniques for compounding polyacetal resin with cellulose as described in Patent Documents 1 to 3 have problems such as the generation of odor from the resin composition, variations in tensile properties due to voids inside the molded product, and unevenness on the surface of the molded product due to gas generation from the resin composition, preventing the polyacetal resin composition from fully exhibiting its intended performance.

[0006] One aspect of the present invention aims to provide a resin composition and a molded product thereof, which can solve the above-mentioned problems and avoid the problems of odor generation from the resin composition, unevenness on the surface of the molded product due to gas generation from the resin composition, and variations in tensile properties due to void generation inside the molded product, as well as methods for producing the same. [Means for solving the problem]

[0007] The present invention includes the following aspects. [1] A method for producing a resin composition containing cellulose nanofibers and a polyacetal resin, comprising: The method includes a step of melt-kneading mixing components containing the cellulose nanofibers and a polyacetal resin while the moisture content of the cellulose nanofibers is 0.01% by mass or more and 5% by mass or less to obtain a resin composition. [2] The method according to item 1, wherein a part of the resin composition is used as a part of the kneading components. [3] The method according to item 1 or 2 above, wherein the cellulose nanofiber has a number average fiber diameter of 10 to 1,000 nm. [4] The method according to any one of items 1 to 3 above, wherein the cellulose nanofiber has an acyl substitution degree of 0.5 to 1.5. [5] The method according to any one of items 1 to 4 above, wherein the cellulose nanofiber has a degree of crystallinity of 60% or more. [6] The method according to any one of items 1 to 5, wherein the moisture content of the resin composition is 0.03% by mass or more and 0.3% by mass or less. [7] The kneading components contain a formaldehyde scavenger, and the content a1 [mass%] of the formaldehyde scavenger in the entire kneading components, the moisture content b [mass%] of the cellulose nanofiber subjected to the melt kneading, and the content c [mass%] of the cellulose nanofiber in the entire kneading components are expressed by the following formula: b×c×0.00012+0.04≦a1≦b×c×0.015+0.2 7. The method according to any one of items 1 to 6 above, which satisfies the following relationship. [8] The kneading components contain a formic acid scavenger, and the content a2 [mass%] of the formic acid scavenger in the entire kneading components, the moisture content b [mass%] of the cellulose nanofiber subjected to the melt kneading, and the content c [mass%] of the cellulose nanofiber in the entire kneading components are expressed by the following formula: b×c×0.00012+0.04≦a2≦b×c×0.015+0.2 The method according to any one of the above items 1 to 7, wherein the above relationship is satisfied. [9] A resin composition comprising cellulose nanofibers and a polyacetal resin, the resin composition having a moisture content of 0.03% by mass or more and 0.3% by mass or less.

[10] The resin composition according to item 9, wherein the cellulose nanofibers have a number average fiber diameter of 10 to 1,000 nm.

[11] The resin composition according to item 9 or 10, wherein the cellulose nanofiber has an acyl substitution degree of 0.5 to 1.5.

[12] The resin composition according to any one of items 9 to 11, wherein the cellulose nanofiber has a degree of crystallinity of 60% or more.

[13] Pellets of the resin composition according to any one of items 9 to 12.

[14] The pellet according to item 13, which has a moisture content of 0.3% by mass to 5.0% by mass when left to stand for 48 hours at 40° C. under saturated water vapor pressure.

[15] A molded body of a resin composition containing cellulose nanofibers and a polyacetal resin, the moisture content of the molded body being 0.03% by mass or more and 0.3% by mass or less.

[16] The molded article according to item 15, wherein the cellulose nanofibers have a number average fiber diameter of 10 to 1,000 nm.

[17] The molded article according to item 15 or 16, wherein the cellulose nanofiber has an acyl substitution degree of 0.5 to 1.5.

[18] The molded article according to any one of items 15 to 17, wherein the cellulose nanofiber has a degree of crystallinity of 60% or more.

[19] A method for producing a molded article of a resin composition containing cellulose nanofibers and a polyacetal resin, comprising: A step of obtaining a resin composition containing cellulose nanofibers and a polyacetal resin; and A step of molding the resin composition to obtain a molded body; Including, The resin composition is molded in a state where the moisture content of the resin composition is 0.03% by mass or more and 0.3% by mass or less.

[20] A method for producing a kneaded product of a resin composition containing cellulose nanofibers and a polyacetal resin, comprising: a storage step of storing a resin composition containing the cellulose nanofibers and the polyacetal resin at a moisture content of more than 0.3% by mass; A drying step of drying the stored resin composition at a temperature Td that is 70° C. or more lower than the melting point Tm of the polyacetal resin to a moisture content of 0.03% by mass or more and 0.3% by mass or less; and a heating step of heating and kneading the resin composition having a moisture content of 0.03% by mass or more and 0.3% by mass or less in the drying step; A method comprising:

[21] A method for producing a molded article of a resin composition containing cellulose nanofibers and a polyacetal resin, comprising: a storage step of storing a resin composition containing the cellulose nanofibers and the polyacetal resin at a moisture content of more than 0.3% by mass; A drying step of drying the stored resin composition at a temperature Td that is 70° C. or more lower than the melting point Tm of the polyacetal resin to a moisture content of 0.03% by mass or more and 0.3% by mass or less; and a molding step of heat-molding the resin composition having a moisture content of 0.03% by mass or more and 0.3% by mass or less in the drying step; A method comprising:

[22] The method according to any one of items 19 to 21, wherein the resin composition is obtained by the method according to any one of items 1 to 8.

[23] A resin composition containing cellulose nanofibers and polyacetal resin was prepared by subjecting the composition to a water vapor transmission rate of 1 g / (m2) at a relative humidity of 40% and a temperature of 90°C. 2 - A method for storing the resin composition by storing it in a sealed packaging bag for no longer than 24 hours.

[24] The method according to item 23, wherein the resin composition is the resin composition according to any one of items 9 to 12.

[25] A pellet container comprising pellets of a resin composition containing cellulose nanofibers and a polyacetal resin, and a container for containing the pellets, The pellet-containing material has a moisture content of 0.03% by mass or more and 0.3% by mass or less.

[26] The pellet-containing container according to item 25, wherein the moisture content when the pellets are allowed to stand for 48 hours at 40° C. under saturated water vapor pressure is 0.3% by mass to 5.0% by mass.

[27] The container has a water vapor transmission rate of 1 g / (m at a relative humidity of 40% and a temperature of 90°C. 2 27. The pellet container according to item 25 or 26, which is made of a material having a sealing means and has a sealing member. Effect of the Invention

[0008] According to one aspect of the present invention, a resin composition and a molded product thereof, which can avoid problems such as odor generation from the resin composition, unevenness on the surface of the molded product due to gas generation from the resin composition, and variations in tensile properties due to void generation inside the molded product, as well as methods for producing the same, can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Exemplary aspects of the present invention (hereinafter also referred to as the present embodiment) will be specifically described below, but the present invention is not limited to these aspects.

[0010] The present inventors have investigated various reasons why the molecular weight of the polyacetal resin decreases when a resin composition containing cellulose nanofibers and a polyacetal resin is heated and melted, which causes odors and gases from the resin composition and voids inside the molded product, and have found that one of the reasons is the decomposition of the polyacetal resin due to the presence of moisture in the resin composition when heated and melted. This discovery was unexpected for those skilled in the art, as it was previously thought that polyacetal resin was hardly deteriorated by moisture.

[0011] Based on the above findings, the inventors have conducted further research and found that controlling the moisture content of the cellulose nanofibers within a specific range during the production of a resin composition containing cellulose nanofibers and polyacetal resin, or controlling the moisture content of the resin composition within a specific range during molding of the resin composition, is advantageous in suppressing decomposition of the polyacetal resin, thereby suppressing odors and gases of the resin composition, and suppressing the occurrence of voids in the molded body.

[0012] One aspect of the present invention provides a method for producing a resin composition containing cellulose nanofibers and a polyacetal resin, the method comprising a step of melt-kneading mixing components containing the cellulose nanofibers and the polyacetal resin while the moisture content of the cellulose nanofibers is 5% by mass or less, particularly 0.01% by mass or more and 5% by mass or less, to obtain a resin composition.

[0013] The moisture content of the cellulose nanofibers when melt-kneaded with the polyacetal resin is, in one embodiment, 5% by mass or less, or 4% by mass or less, or 3% by mass or less from the viewpoint of suppressing the generation of odors and gases from the resin composition due to a decrease in the molecular weight of the polyacetal resin and the generation of voids in the molded body, and, in one embodiment, is 0.01% by mass or more from the viewpoint of avoiding deterioration of the cellulose nanofibers due to the heat required for drying and maintaining good physical properties of the resin composition and a molded body obtained using the same. The moisture content of the cellulose nanofibers is a value measured using a heat-drying moisture meter.

[0014] Another aspect of the present invention provides a resin composition comprising cellulose nanofibers and a polyacetal resin, the resin composition having a moisture content of 0.3 mass% or less, particularly 0.03 mass% or more and 0.3 mass% or less. Such a resin composition can be produced, for example, by the method for producing a resin composition described above.

[0015] The moisture content in the resin composition is, in one embodiment, 0.3% by mass or less, or 0.29% by mass or less, or 0.28% by mass or less, from the viewpoint of preventing the molecular weight of the polyacetal resin from decreasing, thereby suppressing the generation of odor and gas from the resin composition and the generation of voids in the molded product, and, in one embodiment, 0.03% by mass or more, 0.04% by mass or more, or 0.05% by mass or more, from the viewpoint of preventing the promotion of decomposition of polyacetal due to the heat required for drying and the deterioration of cellulose nanofibers, thereby maintaining good physical properties of the resin composition and the molded product obtained using the same. In the present disclosure, the moisture content of the resin composition, pellets, and molded product is a value measured using a Karl Fischer moisture meter in accordance with ISO15512.

[0016] Another aspect of the present invention provides a method for producing a molded article from a resin composition containing cellulose nanofibers and a polyacetal resin, the method comprising the steps of obtaining a resin composition containing cellulose nanofibers and a polyacetal resin, and molding the resin composition to obtain a molded article, wherein the resin composition is molded while the moisture content of the resin composition is within the aforementioned range (in one aspect, 0.3 mass% or less, particularly 0.03 mass% or more and 0.3 mass% or less).

[0017] Another aspect of the present invention provides a molded article of a resin composition containing cellulose nanofibers and a polyacetal resin, the molded article having a moisture content of 0.3% by mass or less, particularly 0.03% by mass or more and 0.3% by mass or less. Such a molded article can be produced, for example, by the above-mentioned method for producing a molded article.

[0018] ≪Resin composition≫ The mass ratio of the cellulose nanofibers to the total mass of the resin composition has a lower limit of preferably 0.05 mass% or more, or 0.1 mass% or more, or 1 mass% or more, from the viewpoint of obtaining a good effect of improving the mechanical properties and thermal stability of the resin composition, and an upper limit of preferably 50 mass% or less, or 40 mass% or less, or 30 mass% or less, or 20 mass% or less, from the viewpoint of maintaining the desired properties of the polyacetal resin in the resin composition.

[0019] The amount of cellulose nanofibers relative to 100 parts by mass of polyacetal resin is preferably 0.1 parts by mass or more, or 1 part by mass or more, or 2 parts by mass or more, or 3 parts by mass or more, and the upper limit is preferably 40 parts by mass or less, or 30 parts by mass or less, or 20 parts by mass or less, or 15 parts by mass or less, or 10 parts by mass or less. From the viewpoint of the balance between the fluidity and mechanical properties of the resin composition when melted, it is desirable to set the amount of cellulose nanofibers within the above-mentioned range. In one aspect, cellulose nanofibers in a dry state can be highly redispersed after being mixed into the polyacetal resin, and sufficient mechanical properties can be realized even if the amount of cellulose nanofibers relative to the resin is small.

[0020] Examples of the components of the resin composition will be described below. In the present disclosure, the charge ratio of the melt-kneaded components during the production of the resin composition may be regarded as the content of each component in the resin composition.

[0021] <Cellulose nanofiber> As the cellulose raw material for obtaining cellulose nanofibers, natural cellulose and regenerated cellulose can be used. As the natural cellulose, wood pulp obtained from wood species (broadleaf or coniferous), non-wood pulp obtained from non-wood species (cotton, bamboo, hemp, bagasse, kenaf, cotton linters, sisal, straw, etc.), and cellulose fiber aggregates produced by animals (e.g., sea squirts), algae, and microorganisms (e.g., acetic acid bacteria) can be used. As the regenerated cellulose, regenerated cellulose fibers (viscose, cupra, tencel, etc.), cellulose derivative fibers, and ultrafine threads of regenerated cellulose or cellulose derivatives obtained by electrospinning can be used.

[0022] Since the cellulose raw material contains alkali-soluble and sulfuric acid-insoluble components (lignin, etc.), the alkali-soluble and sulfuric acid-insoluble components may be reduced through a purification process such as delignification by cooking and a bleaching process. On the other hand, the purification process such as delignification by cooking and the bleaching process cut the molecular chains of cellulose, changing the weight-average molecular weight and number-average molecular weight, so that the purification process and bleaching process of the cellulose raw material are desirably controlled so that the weight-average molecular weight of cellulose and the ratio of the weight-average molecular weight to the number-average molecular weight do not deviate from appropriate ranges.

[0023] In addition, since the refining process such as delignification by cooking and the bleaching process reduce the molecular weight of cellulose molecules, there is a concern that these processes will result in a lower molecular weight of cellulose and an increase in the proportion of alkali-soluble matter present due to the alteration of the cellulose raw material. Since alkali-soluble matter has poor heat resistance, it is desirable to control the refining process and bleaching process of the cellulose raw material so that the amount of alkali-soluble matter contained in the cellulose raw material is within a certain range or less.

[0024] The cellulose raw material may be subjected to a dry grinding process. Any type of grinder may be used in the dry grinding process, but a high-speed rotary impact grinder is preferred because it provides a cellulose raw material with a good shape. A high-speed rotary impact grinder is a grinder in which a pin rotating in a grinding chamber or a rotor having a special structure applies impact or shear to the cellulose raw material to grind it. In addition, in order to suppress fiber damage during dry grinding, a certain amount of moisture may be contained relative to the weight of the cellulose raw material.

[0025] Examples of mills of this type include the Jiyuu mill, New Cosmomizer (manufactured by Nara Machinery Works, Ltd.), Victory Mill, Far in Victory Mill (all manufactured by Hosokawa Micron, Ltd.), Turbo Mill (manufactured by Turbo Kogyo, Ltd.), Ultra Rotor (manufactured by WIR, Ltd.), Makino type mill, Ultraplex (manufactured by Makino Sangyo, Ltd.), Fine Mill (manufactured by Nippon Pneumatic Industry Co., Ltd.), Impeller Mill (manufactured by Seishin Enterprise Co., Ltd.), and Disc Refiner (manufactured by Aikawa Iron Works, Ltd.).

[0026] As a method for reducing the fiber diameter to convert the cellulose raw material into cellulose nanofibers, wet or dry defibration is possible, but the defibration conditions (method of applying a shear field, shear field size, etc.) are appropriately designed so as to obtain cellulose nanofibers that can be dispersed very finely in a resin composition. From the viewpoint of suppressing a decrease in crystallinity due to shear, wet defibration using a solvent is preferred.

[0027] Examples of the solvent used for defibration include water and organic solvents. Water is preferable because it is an inexpensive solvent and does not require explosion-proofing of the production equipment. As the organic solvent, an aprotic solvent is preferable. When the cellulose raw material is immersed in an aprotic solvent, the cellulose swells in a short time, and is pulverized by applying only a small amount of stirring and shear energy. In addition, by adding a cellulose modifying agent before, during, or after defibration, chemically modified cellulose nanofibers can be obtained directly without solvent replacement. Therefore, an aprotic solvent is preferable from the viewpoint of production efficiency.

[0028] Examples of the aprotic solvent include alkyl sulfoxides, alkyl amides, pyrrolidones, etc. These solvents may be used alone or in combination of two or more kinds.

[0029] Examples of alkyl sulfoxides include di-C alkyl sulfoxides such as dimethyl sulfoxide (DMSO), methyl ethyl sulfoxide, and diethyl sulfoxide. 1-4 Alkyl sulfoxides and the like.

[0030] Examples of alkylamides include N,N-diC alkylamides such as N,N-dimethylformamide (DMF) and N,N-diethylformamide. 1-4 Alkylformamides; N,N-diC such as N,N-dimethylacetamide (DMAc) and N,N-diethylacetamide 1-4 Alkylacetamides and the like.

[0031] Examples of pyrrolidones include pyrrolidones such as 2-pyrrolidone and 3-pyrrolidone; NCs such as N-methyl-2-pyrrolidone (NMP); 1-4 Alkylpyrrolidone and the like.

[0032] These aprotic solvents can be used alone or in combination. Among these aprotic solvents, DMSO, DMF, DMAc, NMP, etc., especially DMSO, can be used to produce cellulose nanofibers more efficiently. Although the mechanism of this action is not entirely clear, it is presumed to be due to the homogeneous micro-swelling of the cellulose raw material in the aprotic solvent.

[0033] The cellulose raw material can be defibrated using a device that effectively applies shear to the cellulose raw material, such as a disintegrator, beater, refiner, low-pressure homogenizer, high-pressure homogenizer, ultra-high-pressure homogenizer, emulsifier, homomixer, grinder, mass colloider, cutter mill, ball mill, bead mill, jet mill, single-screw extruder, twin-screw extruder, ultrasonic agitator, household juicer mixer, etc. Among these, defibration using a homomixer using an aprotic solvent is preferred because it can be defibrated with low energy and enables, for example, chemical modification of cellulose nanofibers in a non-aqueous system.

[0034] When using a dispersant, it is preferable to dissolve the dispersant in advance (i.e., before supplying the cellulose) in the solvent used for defibrating the cellulose. In this case, the solvent is preferably DMSO, DMF, DMAc, NMP, etc., and DMSO is particularly preferable in terms of good fine dispersion of the cellulose nanofibers.

[0035] When a dispersant is used, the solvent may be replaced with a poor solvent for the dispersant after defibration to promote adhesion of the dispersant to the cellulose nanofibers. A poor solvent for a dispersant is a solvent that does not dissolve the dispersant, and more preferably, a solvent that does not dissolve the dispersant and is miscible with an organic solvent in which the dispersant is dissolved. For example, when the dispersant is a cellulose derivative, examples of the poor solvent include water with a pH range of 1 to 14, water containing inorganic salts (e.g., sodium chloride, calcium chloride, sodium silicate, etc.), alcohols (e.g., methanol, ethanol, isopropanol, 1-hexanol, etc.), water / alcohol mixed solvents, and the like.

[0036] From the viewpoint of obtaining a favorable effect of improving physical properties by the cellulose nanofibers, the number average fiber diameter of the cellulose nanofibers is, in one aspect, 2 nm or more, and preferably 4 nm or more, or 5 nm or more, or 10 nm or more, or 15 nm or more, or 20 nm or more, and in one aspect, 1000 nm or less, and preferably 500 nm or less, or 450 nm or less, or 400 nm or less, or 350 nm or less, or 300 nm or less, or 250 nm or less.

[0037] From the viewpoint of satisfactorily improving the mechanical properties of a resin composition containing cellulose nanofibers with a small amount of cellulose nanofibers, the average L / D of the cellulose nanofibers is preferably 50 or more, or 80 or more, or 100 or more, or 120 or more, or 150 or more. There is no particular upper limit, but from the viewpoint of handleability, it is preferably 5,000 or less.

[0038] In the present disclosure, the length, diameter, and L / D ratio of each cellulose nanofiber are determined by diluting an aqueous dispersion of cellulose nanofibers with a water-soluble solvent (e.g., water, ethanol, tert-butanol, etc.) to 0.01 to 0.1% by mass, dispersing the cellulose nanofibers using a high-shear homogenizer (e.g., IKA, product name "Ultra Turrax T18") under processing conditions: rotation speed 25,000 rpm x 5 minutes, casting the homogenized material on mica, and air-drying the material to obtain a measurement sample, which is then measured with a high-resolution scanning electron microscope (SEM) or atomic force microscope (AFM). Specifically, the length (L) and diameter (D) of 100 randomly selected fibrous substances are measured in an observation field where the magnification is adjusted so that at least 100 fibrous substances are observed, and the ratio (L / D) is calculated. The number average value of the length (L), the number average value of the diameter (D), and the number average value of the ratio (L / D) of the cellulose nanofibers are calculated.

[0039] The length, diameter, and L / D ratio of the cellulose nanofibers in the resin composition can be confirmed by measuring the solid resin composition as a measurement sample using the above-mentioned measurement method. Alternatively, the length, diameter, and L / D ratio of the cellulose nanofibers in the resin composition can be confirmed by dissolving the resin components in the resin composition in an organic or inorganic solvent that can dissolve the resin components of the resin composition, separating the cellulose nanofibers, thoroughly washing with the solvent, and then replacing with a water-soluble solvent (e.g., water, ethanol, tert-butanol, etc.), preparing a 0.01 to 0.1 mass% dispersion, and redispersing with a high-shear homogenizer (e.g., IKA, product name "Ultra Turrax T18"). The redispersion can be confirmed by casting the redispersion on mica, air-drying it, and measuring it as a measurement sample using the above-mentioned measurement method. At this time, the measurement is performed on 100 or more randomly selected cellulose nanofibers.

[0040] The crystallinity of the cellulose nanofiber is preferably 55% or more. When the crystallinity is within this range, the mechanical properties (strength, dimensional stability) of the cellulose fiber itself are high, and therefore when the cellulose fiber is dispersed in a resin, the strength and dimensional stability of the resin composition tend to be high. A more preferred lower limit of the crystallinity is 60%, 70%, or 80%. There is no particular upper limit for the crystallinity of the cellulose nanofiber, and the higher the better, but from the viewpoint of production, a preferred upper limit is 99%.

[0041] Alkali-soluble polysaccharides such as hemicellulose and acid-insoluble components such as lignin are present between the microfibrils and between the microfibril bundles of plant-derived cellulose. Hemicellulose is a polysaccharide composed of sugars such as mannan and xylan, and plays a role in connecting the microfibrils by hydrogen bonding with cellulose. Lignin is also a compound having an aromatic ring, and is known to be covalently bonded to hemicellulose in the cell walls of plants. If there is a large amount of impurities such as lignin remaining in the cellulose nanofibers, discoloration may occur due to heat during processing. Therefore, from the viewpoint of suppressing discoloration of the resin composition during extrusion processing and molding processing, it is desirable to set the crystallinity of the cellulose nanofibers within the above-mentioned range.

[0042] When the cellulose nanofiber is cellulose type I crystal (derived from natural cellulose), the degree of crystallinity is calculated from the diffraction pattern (2θ / deg. is 10 to 30) obtained by measuring the sample by wide-angle X-ray diffraction using the Segal method, as shown in the following formula. Crystallinity (%) = ([diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] - [diffraction intensity due to amorphous matter at 2θ / deg. = 18]) / [diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] × 100 Furthermore, when the cellulose nanofiber is a cellulose II type crystal, the degree of crystallinity can be calculated from the absolute peak intensity h0 at 2θ=12.6° assigned to the (110) plane peak of the cellulose II type crystal in wide-angle X-ray diffraction and the peak intensity h1 of the baseline at this interplanar spacing (the line connecting 2θ=8° and 15°) according to the following formula: Crystallinity (%) = (h0-h1) / h0 ×100 Known crystalline forms of cellulose include type I, type II, type III, and type IV, among which types I and II are particularly widely used, and types III and IV are obtained on a laboratory scale but are not widely used on an industrial scale. The cellulose nanofibers of the present disclosure are preferably cellulose fibers containing cellulose type I crystals or cellulose type II crystals, since they have relatively high structural mobility and can be dispersed in a resin to obtain a resin composition with a lower linear expansion coefficient and superior strength and elongation during tensile and bending deformation, and more preferably cellulose nanofibers containing cellulose type I crystals and having a crystallinity of 55% or more. In particular, cellulose nanofibers having a crystallinity of 60% or more are even more preferable, since it is easy to reduce the moisture content in the cellulose nanofibers.

[0043] In addition, the degree of polymerization of the cellulose nanofibers is preferably 100 or more, or 150 or more, or 200 or more, or 300 or more, or 400 or more, or 450 or more, and preferably 3500 or less, or 3300 or less, or 3200 or less, or 3100 or less, or 3000 or less.

[0044] From the viewpoint of processability and mechanical property expression, it is desirable that the degree of polymerization of the cellulose nanofiber is within the above-mentioned range. From the viewpoint of processability, it is preferable that the degree of polymerization is not too high, and from the viewpoint of mechanical property expression, it is desirable that the degree of polymerization is not too low.

[0045] The degree of polymerization of cellulose nanofibers refers to the average degree of polymerization measured according to the reduced specific viscosity method using a copper ethylenediamine solution described in the Verification Test (3) of the "15th Revised Japanese Pharmacopoeia Commentary (published by Hirokawa Shoten)."

[0046] In one embodiment, the weight average molecular weight (Mw) of the cellulose nanofiber is preferably 100,000 or more, or 200,000 or more. The ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) is preferably 6 or less, or 5.4 or less. The larger the weight average molecular weight, the fewer the number of terminal groups of the cellulose molecule. In addition, since the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight represents the width of the molecular weight distribution, the smaller the Mw / Mn, the fewer the number of terminals of the cellulose molecule. Since the terminals of the cellulose molecules are the starting points of thermal decomposition, when the cellulose molecules of the cellulose nanofibers not only have a large weight average molecular weight but also have a narrow molecular weight distribution, a particularly heat-resistant cellulose nanofiber and a resin composition containing the cellulose nanofiber and a resin can be obtained. The weight average molecular weight (Mw) of the cellulose nanofiber may be, for example, 600,000 or less, or 500,000 or less, from the viewpoint of the availability of the cellulose raw material. From the viewpoint of ease of production of cellulose nanofibers, the ratio (Mw / Mn) of weight average molecular weight to number average molecular weight (Mn) may be, for example, 1.5 or more, or 2 or more. Mw can be controlled to the above range by selecting a cellulose raw material having an Mw appropriate for the purpose, by appropriately performing physical and / or chemical treatment on the cellulose raw material within an appropriate range, etc. Mw / Mn can also be controlled to the above range by selecting a cellulose raw material having an Mw / Mn appropriate for the purpose, by appropriately performing physical and / or chemical treatment on the cellulose raw material within an appropriate range, etc. Each of the Mw and Mw / Mn of the cellulose raw material may be within the above range in one embodiment. In both the control of Mw and the control of Mw / Mn, examples of the physical treatment include dry or wet grinding using a microfluidizer, ball mill, disk mill, or the like, and physical treatments that apply mechanical forces such as impact, shear, friction, and the like using a crusher, homomixer, high-pressure homogenizer, ultrasonic device, or the like, and examples of the chemical treatment include digestion, bleaching, acid treatment, and conversion to regenerated cellulose.

[0047] The weight average molecular weight and number average molecular weight of cellulose referred to here are values ​​determined by dissolving cellulose in N,N-dimethylacetamide containing added lithium chloride and then subjecting the cellulose to gel permeation chromatography using N,N-dimethylacetamide as a solvent.

[0048] Methods for controlling the degree of polymerization (i.e., average degree of polymerization) or molecular weight of cellulose nanofibers include hydrolysis. Hydrolysis promotes depolymerization of amorphous cellulose inside the cellulose nanofibers, decreasing the average degree of polymerization. At the same time, hydrolysis removes impurities such as hemicellulose and lignin in addition to the above-mentioned amorphous cellulose, making the inside of the fiber more porous.

[0049] The hydrolysis method is not particularly limited, and examples thereof include acid hydrolysis, alkali hydrolysis, hydrothermal decomposition, steam explosion, and microwave decomposition. These methods may be used alone or in combination of two or more. In the acid hydrolysis method, for example, α-cellulose obtained as pulp from a fibrous plant is used as a cellulose raw material, and this is dispersed in an aqueous medium, and an appropriate amount of a protonic acid, a carboxylic acid, a Lewis acid, a heteropoly acid, etc. is added, and the mixture is heated while stirring, so that the average degree of polymerization can be easily controlled. The reaction conditions at this time, such as temperature, pressure, and time, vary depending on the cellulose type, cellulose concentration, acid type, acid concentration, etc., and are appropriately adjusted so that the desired average degree of polymerization is achieved. For example, a condition in which cellulose is treated for 10 minutes or more at 100°C or higher under pressure using an aqueous mineral acid solution of 2% by mass or less can be exemplified. Under these conditions, the catalyst component such as acid penetrates into the inside of the cellulose nanofiber, promoting hydrolysis, reducing the amount of catalyst component used, and making subsequent purification easier. The dispersion of the cellulose raw material during hydrolysis may contain, in addition to water, a small amount of an organic solvent within a range that does not impair the effects of the present invention.

[0050] Alkali-soluble polysaccharides that cellulose nanofibers may contain include hemicellulose, β-cellulose, and γ-cellulose. Alkali-soluble polysaccharides are understood by those skilled in the art as components obtained as the alkali-soluble portion of holocellulose obtained by solvent extraction and chlorine treatment of plants (e.g., wood) (i.e., components obtained by removing α-cellulose from holocellulose).

[0051] In one aspect, the average content of alkali-soluble polysaccharides in the cellulose nanofibers is preferably 20% by mass or less, 18% by mass or less, 15% by mass or less, or 12% by mass or less, relative to 100% by mass of the cellulose nanofibers, from the viewpoint of obtaining good dispersibility of the cellulose nanofibers. From the viewpoint of ease of production of the cellulose nanofibers, the above content may be 1% by mass or more, 2% by mass or more, or 3% by mass or more.

[0052] The average alkali-soluble polysaccharide content can be determined by the method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000), by subtracting the α-cellulose content from the holocellulose content (Wise method). This method is understood in the industry as a method for measuring the amount of hemicellulose. The alkali-soluble polysaccharide content is calculated three times for each sample, and the number average of the calculated alkali-soluble polysaccharide contents is taken as the average alkali-soluble polysaccharide content.

[0053] In one aspect, the average content of acid-insoluble components in the cellulose nanofibers is preferably 10% by mass or less, 5% by mass or less, or 3% by mass or less, relative to 100% by mass of the cellulose nanofibers, from the viewpoint of avoiding a decrease in heat resistance of the cellulose nanofibers and the associated discoloration. From the viewpoint of ease of production of the cellulose nanofibers, the above content may be 0.1% by mass or more, 0.2% by mass or more, or 0.3% by mass or more.

[0054] The average acid-insoluble content is determined as a quantitative determination of the acid-insoluble content using the Clason method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000). This method is understood in the industry as a method for measuring the amount of lignin. The sample is stirred in a sulfuric acid solution to dissolve cellulose, hemicellulose, etc., and then filtered through a glass fiber filter paper, and the resulting residue corresponds to the acid-insoluble content. The acid-insoluble content is calculated from the weight of the acid-insoluble content, and the number average of the acid-insoluble content calculated for the three samples is taken as the average acid-insoluble content.

[0055] In one embodiment, the cellulose nanofibers are chemically treated (e.g., oxidized or chemically modified using a modifying agent). In one embodiment, the cellulose nanofibers are acylated cellulose nanofibers. As an example, cellulose nanofibers obtained by oxidizing cellulose fibers with 2,2,6,6-tetramethylpiperidine-1-oxyl radical as shown in Cellulose (1998) 5, 153-164, followed by washing and mechanical fiberization, may be used.

[0056] The cellulose modification agent can be a compound that reacts with the hydroxyl group of cellulose, and includes an esterification agent, an etherification agent, and a silylating agent. In a preferred embodiment, the chemical modification is acylation using an esterification agent. The esterification agent is preferably an acid halide, an acid anhydride, a vinyl carboxylate, or a carboxylic acid.

[0057] The acid halide may be at least one selected from the group consisting of compounds represented by the following formula:

[0058] R1-C(=O)-X (In the formula, R1 represents an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 24 carbon atoms, or an aryl group having 6 to 24 carbon atoms, and X represents Cl, Br, or I.) Specific examples of acid halides include, but are not limited to, acetyl chloride, acetyl bromide, acetyl iodide, propionyl chloride, propionyl bromide, propionyl iodide, butyryl chloride, butyryl bromide, butyryl iodide, benzoyl chloride, benzoyl bromide, and benzoyl iodide. Among them, acid chlorides can be preferably used in terms of reactivity and handling. In addition, in the reaction of acid halides, one or more alkaline compounds may be added to act as a catalyst and neutralize the by-product acidic substances. Specific examples of alkaline compounds include, but are not limited to, tertiary amine compounds such as triethylamine and trimethylamine; and nitrogen-containing aromatic compounds such as pyridine and dimethylaminopyridine.

[0059] As the acid anhydride, any suitable acid anhydride can be used. For example, Saturated aliphatic monocarboxylic acid anhydrides, such as acetic acid, propionic acid, (iso)butyric acid, and valeric acid; unsaturated aliphatic monocarboxylic acid anhydrides, such as (meth)acrylic acid and oleic acid; Alicyclic monocarboxylic acid anhydrides such as cyclohexanecarboxylic acid and tetrahydrobenzoic acid; Aromatic monocarboxylic acid anhydrides such as benzoic acid and 4-methylbenzoic acid; Examples of dibasic carboxylic acid anhydrides include saturated aliphatic dicarboxylic acid anhydrides such as succinic anhydride and adipic acid, unsaturated aliphatic dicarboxylic acid anhydrides such as maleic anhydride and itaconic anhydride, alicyclic dicarboxylic acid anhydrides such as 1-cyclohexene-1,2-dicarboxylic acid anhydride, hexahydrophthalic anhydride and methyltetrahydrophthalic anhydride, and aromatic dicarboxylic acid anhydrides such as phthalic anhydride and naphthalic anhydride; Examples of polybasic carboxylic acid anhydrides having three or more bases include polycarboxylic acids (anhydrides) such as trimellitic anhydride and pyromellitic anhydride.

[0060] In addition, in the reaction of an acid anhydride, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.

[0061] The vinyl carboxylate may be represented by the following formula: R-COO-CH=CH2 Preferred is a vinyl carboxylate represented by the formula: {wherein R is any one of an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, and an aryl group having 6 to 24 carbon atoms.} The vinyl carboxylate is more preferably at least one selected from the group consisting of vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caproate, vinyl cyclohexanecarboxylate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate, vinyl pivalate, vinyl octylate, divinyl adipate, vinyl methacrylate, vinyl crotonate, vinyl pivalate, vinyl octylate, vinyl benzoate, and vinyl cinnamate. In the esterification reaction with a vinyl carboxylate, one or more catalysts selected from the group consisting of alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal hydrogencarbonates, primary to tertiary amines, quaternary ammonium salts, imidazole and derivatives thereof, pyridine and derivatives thereof, and alkoxides may be added.

[0062] Examples of the alkali metal hydroxides and alkaline earth metal hydroxides include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, barium hydroxide, etc. Examples of the alkali metal carbonates, alkaline earth metal carbonates, and alkali metal hydrogen carbonates include lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, barium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, cesium hydrogen carbonate, etc.

[0063] The primary, secondary and tertiary amines refer to primary, secondary and tertiary amines, and specific examples thereof include ethylenediamine, diethylamine, proline, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,3-propanediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, tris(3-dimethylaminopropyl)amine, N,N-dimethylcyclohexylamine and triethylamine.

[0064] Examples of imidazole and its derivatives include 1-methylimidazole, 3-aminopropylimidazole, and carbonyldiimidazole. Examples of pyridine and its derivatives include N,N-dimethyl-4-aminopyridine and picoline. Examples of the alkoxide include sodium methoxide, sodium ethoxide, and potassium t-butoxide.

[0065] The carboxylic acid may be at least one selected from the group consisting of compounds represented by the following formulas:

[0066] R-COOH (In the formula, R represents an alkyl group having 1 to 16 carbon atoms, an alkenyl group having 2 to 16 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms.) Specific examples of carboxylic acids include at least one selected from the group consisting of acetic acid, propionic acid, butyric acid, caproic acid, cyclohexane carboxylic acid, caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, pivalic acid, methacrylic acid, crotonic acid, pivalic acid, octylic acid, benzoic acid, and cinnamic acid.

[0067] Among these carboxylic acids, at least one selected from the group consisting of acetic acid, propionic acid, and butyric acid, and particularly acetic acid, is preferred from the viewpoint of reaction efficiency. In addition, in the reaction of carboxylic acid, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.

[0068] Among these esterification reactants, at least one selected from the group consisting of acetic anhydride, propionic anhydride, butyric anhydride, vinyl acetate, vinyl propionate, vinyl butyrate, and acetic acid, and among these, acetic anhydride and vinyl acetate are preferred from the viewpoint of reaction efficiency.

[0069] The degree of modification of the chemically modified cellulose nanofiber of this embodiment is expressed as the average degree of substitution of hydroxyl groups (also referred to as DS, the average number of hydroxyl groups substituted per glucose, which is the basic structural unit of cellulose). In one aspect, the DS of the chemically modified cellulose nanofiber is preferably 0.01 or more and 2.0 or less. If the DS is 0.01 or more, a resin composition containing chemically modified fine cellulose with a high thermal decomposition onset temperature can be obtained. On the other hand, if the DS is 2.0 or less, an unmodified cellulose skeleton remains in the chemically modified fine cellulose, so that a resin composition containing chemically modified fine cellulose having both high tensile strength and dimensional stability derived from cellulose and high thermal decomposition onset temperature derived from chemical modification can be obtained. The DS is more preferably 0.05 or more, or 0.1 or more, or 0.2 or more, or 0.3 or more, or 0.5 or more, and more preferably 1.8 or less, or 1.5 or less, or 1.3 or less. In a particularly preferred aspect, the cellulose nanofiber is an acylated cellulose nanofiber with an acylation degree of 0.5 to 1.5.

[0070] When the modification group of the chemically modified cellulose nanofiber is an acyl group, the degree of acyl substitution as DS can be calculated based on the peak intensity ratio of the peak derived from the acyl group to the peak derived from the cellulose skeleton from the reflection infrared absorption spectrum of the esterified cellulose nanofiber. The peak of the absorption band of C=O based on the acyl group is at 1730 cm -1 The absorption band of CO based on the cellulose backbone appears at 1030 cm -1 The DS of esterified cellulose nanofibers was calculated by plotting a correlation graph between the DS obtained from solid-state NMR measurements of esterified cellulose nanofibers (described below) and the modification ratio (IR index 1030), which is defined as the ratio of the peak intensity of the absorption band of C=O based on acyl groups to the peak intensity of the absorption band of CO in the cellulose backbone chain, and then calculating the calibration curve from the correlation graph. Degree of substitution DS = 4.13 × IR index (1030) It can be found by using

[0071] The method for calculating the DS of esterified cellulose nanofibers using solid-state NMR is as follows: 13 C solid-state NMR measurement was performed, and the intensity can be calculated using the area intensity (Inf) of a signal assigned to one carbon atom derived from the modifying group relative to the total area intensity (Inp) of signals assigned to carbons C1-C6 derived from the pyranose ring of cellulose, which appear in the range from 50 ppm to 110 ppm, using the following formula. DS = (Inf) x 6 / (Inp) For example, when the modifying group is an acetyl group, the signal at 23 ppm assigned to -CH3 may be used.

[0072] Use 13 The conditions for the C solid-state NMR measurement are, for example, as follows: Equipment:Bruker Biospin Avance500WB Frequency: 125.77MHz Measurement method: DD / MAS method Waiting time: 75sec NMR sample tube: 4mmφ Accumulation times: 640 times (approx. 14 hours) MAS: 14,500Hz Chemical shift reference: glycine (external reference: 176.03 ppm)

[0073] The DS heterogeneity ratio (DSs / DSt), defined as the ratio of the degree of substitution (DSs) of the fiber surface to the degree of substitution (DSt) of the entire fiber of the chemically modified cellulose nanofiber (which is synonymous with the above DS), is preferably 1.05 or more. The larger the value of the DS heterogeneity ratio, the more pronounced the sheath-core-like heterogeneous structure (i.e., a structure in which the fiber surface is highly chemically modified while the fiber center retains a cellulose structure close to the original unmodified structure), and while maintaining high tensile strength and dimensional stability derived from cellulose, it is possible to improve the affinity with the resin when composited with the resin and to improve the dimensional stability of the resin composition. The DS heterogeneity ratio is more preferably 1.1 or more, or 1.2 or more, or 1.3 or more, or 1.5 or more, or 2.0 or more, and from the viewpoint of ease of production of the chemically modified cellulose nanofiber, it is preferably 30 or less, or 20 or less, or 10 or less, or 6 or less, or 4 or less, or 3 or less.

[0074] The value of DSs varies depending on the degree of modification of the chemically modified cellulose nanofibers, but as an example, it is preferably 0.1 or more, or 0.2 or more, or 0.3 or more, or 0.5 or more, and preferably 3.0 or less, or 2.5 or less, or 2.0 or less, or 1.5 or less, or 1.2 or less, or 1.0 or less. The preferred range of DSt is as described above for DS.

[0075] The smaller the coefficient of variation (CV) of the DS heterogeneity ratio of the chemically modified cellulose nanofiber, the smaller the variation in various physical properties of the resin composition, and therefore the more preferable. The coefficient of variation is preferably 50% or less, or 40% or less, or 30% or less, or 20% or less. The coefficient of variation can be further reduced, for example, by a method in which a cellulose raw material is defibrated and then chemically modified to obtain chemically modified cellulose nanofibers (i.e., a sequential method), whereas it can be increased by a method in which defibration and chemical modification of the cellulose raw material are performed simultaneously (i.e., a simultaneous method). Although the mechanism of this action is not clear, in the simultaneous method, chemical modification is more likely to proceed in the thin fibers generated in the early stage of defibration, and when hydrogen bonds between cellulose microfibrils are reduced by chemical modification, defibration proceeds further, which is thought to result in an increase in the coefficient of variation of the DS heterogeneity ratio.

[0076] The coefficient of variation (CV) of the DS heterogeneity ratio is calculated by taking 100 g of an aqueous dispersion of chemically modified cellulose nanofiber (solid content of 10 mass% or more) and freeze-pulverizing 10 g portions to use as measurement samples. The DS heterogeneity ratio is calculated from the DSt and DSs of the 10 samples, and then the standard deviation (σ) and arithmetic mean (μ) of the DS heterogeneity ratio among the obtained 10 samples are used to calculate the coefficient of variation (CV) of the DS heterogeneity ratio using the following formula.

[0077] DS heterogeneity ratio = DSs / DSt Coefficient of variation (%) = standard deviation σ / arithmetic mean μ × 100 The DSs is calculated as follows. That is, the chemically modified cellulose nanofibers powdered by freeze-pulverization are placed on a dish-shaped sample stage with a diameter of 2.5 mm, the surface is pressed down to make it flat, and then measurement is performed by X-ray photoelectron spectroscopy (XPS). The XPS spectrum reflects the constituent elements and chemical bond state of only the surface layer of the sample (typically about a few nm). Peak separation is performed on the obtained C1s spectrum, and the DSs can be calculated by the following formula based on the area intensity (Ixf) of the peak assigned to one carbon atom derived from the modifying group relative to the area intensity (Ixp) of the peak (289 eV, CC bond) assigned to carbons C2-C6 derived from the pyranose ring of cellulose. DSs = (Ixf) x 5 / (Ixp) For example, when the modifying group is an acyl group, after performing peak separation of the C1s spectrum at 285 eV, 286 eV, 288 eV, and 289 eV, the peak at 289 eV can be used for Ixp, and the peak derived from the O-C=O bond of the acyl group (286 eV) can be used for Ixf.

[0078] The conditions for the XPS measurement are as follows, for example: Equipment used: ULVAC-Phi VersaProbe II Excitation source: mono.AlKα 15kV×3.33mA Analysis size: Approx. 200 μm φ Photoelectron extraction angle: 45° Capture Area Narrow scan: C 1s, O 1s Pass Energy: 23.5eV

[0079] <Polyacetal resin> Polyacetal resins are polymeric compounds whose main constituent unit is an oxymethylene group (-OCH2-), and are typically polyacetal homopolymers consisting essentially of repeating oxymethylene units, and polyacetal copolymers containing oxymethylene units and other monomer units. Polyacetal resins also include copolymers into which branched and / or crosslinked structures have been introduced by copolymerizing branch-forming components and / or crosslinking components, and block or graft copolymers having a polymer portion consisting of repeating oxymethylene groups and another polymer portion.

[0080] Generally, the polyacetal homopolymer is produced by polymerization of one or more monomers selected from anhydrous formaldehyde and cyclic formaldehyde oligomers such as trioxane (cyclic trimer of formaldehyde), tetraoxane (cyclic tetramer of formaldehyde), etc. Usually, the polymerization terminals are esterified to stabilize against thermal decomposition.

[0081] Polyacetal copolymers are generally produced using formaldehyde and / or acetal copolymers of the general formula (CHO) n Examples of such copolymers include those produced by copolymerizing the above-mentioned cyclic oligomers of formaldehyde (e.g., the above-mentioned trioxane) represented by the formula [wherein n is an integer of 3 or more] with comonomers such as cyclic ethers and / or cyclic formals (e.g., ethylene oxide, propylene oxide, epichlorohydrin, 1,3-dioxolane, and glycols such as 1,4-butanediol formal, or cyclic formals of diglycol, etc.). Usually, the unstable moieties at the terminals are removed by hydrolysis to stabilize the copolymer against thermal decomposition.

[0082] Further, examples of the polyacetal copolymer include a branched polyacetal copolymer obtained by copolymerizing a formaldehyde monomer and / or a cyclic oligomer with a monofunctional glycidyl ether; and a crosslinked polyacetal copolymer obtained by copolymerizing a formaldehyde monomer and / or a cyclic oligomer with a polyfunctional glycidyl ether.

[0083] Examples of the polyacetal resin include polyacetal homopolymers having block components obtained by polymerizing a formaldehyde monomer and / or a cyclic oligomer in the presence of a compound having a functional group such as a hydroxyl group at both ends or one end, for example, a polyalkylene glycol; and polyacetal copolymers having block components obtained by copolymerizing a formaldehyde monomer and / or a cyclic oligomer with a cyclic ether and / or a cyclic formal in the presence of a compound having a functional group such as a hydroxyl group at both ends or one end, for example, a hydrogenated polybutadiene glycol.

[0084] Among these, polyacetal copolymers are preferred from the viewpoint of the balance between thermal stability and mechanical properties. The polyacetal resins may be used alone or in combination of two or more.

[0085] The amount of the structure derived from the comonomer component (e.g., 1,3-dioxolane) is preferably 0.01 mol% or more, or 0.05 mol% or more, or 0.1 mol% or more, or 0.2 mol% or more from the viewpoint of thermal stability during extrusion processing and molding processing, and is preferably 4.0 mol% or less, or 3.5 mol% or less, or 3.0 mol% or less, or 2.5 mol% or less, or 2.3 mol% or less from the viewpoint of mechanical strength.

[0086] In one embodiment, the melting point of the polyacetal resin is 150° C. or higher, or 155° C. or higher, or 170° C. or higher, and in one embodiment, 185° C. or lower, or 180° C. or lower, or 175° C. or lower. The melting point refers to the peak top temperature of an endothermic peak that appears when a resin that has been melted at 200° C. once is cooled to 23° C. at 10° C. / min using a differential scanning calorimeter (DSC), and then heated from 23° C. at a heating rate of 10° C. / min. When two or more endothermic peaks appear, the melting point refers to the peak top temperature of the endothermic peak on the highest temperature side.

[0087] <Additional Ingredients> The resin composition of the present embodiment may further contain additional components as necessary to improve its performance. Examples of the additional components include dispersants, formaldehyde scavengers, formic acid scavengers, thermoplastic resins, thermoplastic elastomers, inorganic or organic fillers (e.g., filler components other than cellulose, zeolites, ceramics, talc, silica, metal oxides, metal powders, and other inorganic compounds), compatibilizers, plasticizers, polysaccharides such as starches and alginic acid, natural proteins such as gelatin, glue, and casein, colorants (e.g., dyes and pigments, pigments), fragrances, flow regulators, leveling agents, conductive agents, antioxidants, antistatic agents, weather stabilizers, ultraviolet absorbing agents, ultraviolet dispersants, release agents, lubricants, and deodorants. These components may be used alone or in combination of two or more. The content of any additional component in the resin composition is appropriately selected within a range that does not impair the desired effects of the present invention, and may be, for example, 0.01 to 50 mass %, or 0.1 to 30 mass %.

[0088] [Dispersant] As the dispersant, a compound capable of reacting with or hydrogen bonding with the hydroxyl group of cellulose is preferred. Suitable examples of the dispersant include one or more selected from the group consisting of cellulose derivatives, polyalkylene oxides, amides, and amines. Among them, cellulose derivatives are preferred because they have high affinity with cellulose as a cellulose-based substance, while they are also thermoplastic resins, and therefore have a high effect of improving the dispersion stability of cellulose in the resin composition. As the dispersant, one having a boiling point higher than that of water is preferred. Note that a boiling point higher than that of water refers to a boiling point higher than the boiling point of water at each pressure in the vapor pressure curve (for example, 100°C under 1 atmosphere).

[0089] In the resin composition, the amount of dispersant per 100 parts by mass of cellulose nanofibers is, from the viewpoint of good dispersion of cellulose and network formation, preferably 1 part by mass or more, or 5 parts by mass or more, or 10 parts by mass or more, or 20 parts by mass or more, and from the viewpoint of reducing variation in the performance of the resin composition, preferably 500 parts by mass or less, or 300 parts by mass or less, or 200 parts by mass or less.

[0090] [Formaldehyde scavenger] Polyacetal resins generate formaldehyde through decomposition, and the formaldehyde can promote further decomposition of the polyacetal resin. Formaldehyde scavengers contribute to suppressing further decomposition of the polyacetal resin by capturing such formaldehyde. Examples of formaldehyde scavengers include aminotriazine compounds, guanamine compounds, urea derivatives, hydrazide compounds, amide compounds (e.g., acrylamide polymers), polyamides, etc., which can be used alone or in combination of two or more. In a preferred embodiment, the formaldehyde scavengers are at least one selected from the group consisting of aminotriazine compounds, guanamine compounds, hydrazide compounds, and polyamides.

[0091] Examples of the aminotriazine compound include melamine, 2,4-diamino-sym-triazine, 2,4,6-triamino-sym-triazine, N-butylmelamine, N-phenylmelamine, N,N-diphenylmelamine, N,N-diallylmelamine, benzoguanamine (2,4-diamino-6-phenyl-sym-triazine), acetoguanamine (2,4-diamino-6-methyl-sym-triazine), and 2,4-diamino-6-butyl-sym-triazine.

[0092] Examples of the guanamine compound include aliphatic guanamine compounds (monoguanamines, alkylenebisguanamines, etc.), alicyclic guanamine compounds (monoguanamines, etc.), aromatic guanamine compounds [for example, monoguanamines (benzoguanamine and its functional group substituted derivatives, etc.), α- or β-naphthoguanamine and their functional group substituted derivatives, polyguanamines, aralkyl or aralkyleneguanamines, etc.], and heteroatom-containing guanamine compounds [for example, acetal group-containing guanamines, tetraoxospiro ring-containing guanamines (CTU-guanamine, CMTU-guanamine, etc.), isocyanuric ring-containing guanamines, imidazole ring-containing guanamines, etc.].

[0093] Examples of the urea derivative include N-substituted urea, urea condensates, ethylene urea, hydantoin compounds, and ureido compounds. Examples of the N-substituted urea include methyl urea having a substituent such as an alkyl group, alkylene bis urea, and aryl substituted urea. The urea condensate may, for example, be a condensate of urea and formaldehyde. Examples of the hydantoin compound include hydantoin, 5,5-dimethylhydantoin, and 5,5-diphenylhydantoin. The ureido compounds include, for example, allantoin.

[0094] The hydrazide compound may be a carboxylic acid mono- or dihydrazide compound synthesized by reacting a carboxylic acid (containing an aromatic ring and / or an alicyclic ring) with hydrazine, or an alkyl group-substituted mono- or dihydrazide compound. The carboxylic acid constituting the carboxylic acid mono- or dihydrazide compound may be a monocarboxylic acid, a dicarboxylic acid, or the like, which may be saturated or unsaturated.

[0095] Examples of monocarboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, lauric acid, myristic acid, palmitic acid, margaric acid, stearic acid, and behenic acid. Examples of dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, naphthalic acid, salicylic acid, gallic acid, mellitic acid, cinnamic acid, pyruvic acid, lactic acid, malic acid, citric acid, fumaric acid, maleic acid, aconitic acid, amino acid, and nitrocarboxylic acid. Examples of unsaturated carboxylic acids include oleic acid, linoleic acid, linolenic acid, arachidonic acid, docosahexaenoic acid, and eicosapentaenoic acid.

[0096] Examples of carboxylic acid mono(di)hydrazide compounds synthesized using these carboxylic acids include carbodihydrazine, oxalic acid mono(di)hydrazide, malonic acid mono(di)hydrazide, succinic acid mono(di)hydrazide, glutaric acid mono(di)hydrazide, adipic acid mono(di)hydrazide, sebacic acid mono(di)hydrazide, lauric acid mono(di)hydrazide, malic acid dihydrazide, tartaric acid dihydrazide, propionic acid monohydrazide, lauric acid monohydrazide, and stearic acid monohydrazide. hydrazide, phthalic dihydrazide, isophthalic dihydrazide, terephthalic dihydrazide, 2,6-naphthalic dihydrazide, p-hydroxybenzoic hydrazine, p-hydroxybenzoic hydrazine, 1,4-cyclohexanedicarboxylic dihydrazine, acetohydrazide, acrylohydrazide, maleic dihydrazide, fumaric dihydrazide, benzohydrazide, nicotinohydrazide, isonicotinohydrazide, isobutylhydrazine, and oleic hydrazide.

[0097] Among these carboxylic acids, dicarboxylic acids such as adipic acid, sebacic acid, and lauric acid are preferred, and adipic acid mono(di)hydrazide, sebacic acid mono(di)hydrazide, and lauric acid mono(di)hydrazide are the most preferred carboxylic acid hydrazide compounds.

[0098] Among the carboxylic acid hydrazide compounds, when the ratio of the monohydrazide compound to the dihydrazide compound is within a specific range, it is possible to suppress the generation of carbonized products and modified products during long-term continuous molding, and to suppress mold contamination. The content of the carboxylic acid monohydrazide compound is preferably in the range of 0.0001 to 1.0 mass% relative to 100 mass% of the total of the carboxylic acid monohydrazide compound and the carboxylic acid dihydrazide compound. The content is more preferably in the range of 0.0001 to 0.5 mass%, and even more preferably in the range of 0.0001 to 0.1 mass%.

[0099] The above-mentioned content of the carboxylic acid monohydrazide compound can be adjusted by adding a monohydrazide compound to the carboxylic acid dihydrazide compound, and by adjusting the synthesis reaction conditions in the reaction between the carboxylic acid and hydrazine. During the synthesis reaction between the carboxylic acid and hydrazine, a monohydrazide compound is generated as an intermediate. The content of the monohydrazide compound can be adjusted by washing and removing the monohydrazide compound.

[0100] Examples of the amide compound include polycarboxylic acid amides such as isophthalic acid diamide, anthranilamide, and acrylamide polymers.

[0101] The acrylamide polymer is preferably a particulate polymer containing 30 to 70 mol% primary amide groups and having an average particle size of 0.1 to 10 μm. Among them, a preferred acrylamide polymer is a crosslinked acrylamide polymer having an average particle size of 10 μm or less. More preferred is an acrylamide polymer having an average particle size of 5 μm or less, and most preferred is a crosslinked acrylamide polymer having an average particle size of 3 μm or less.

[0102] Examples of polyamides include polyamides derived from diamines and dicarboxylic acids, polyamides obtained by using aminocarboxylic acids, optionally in combination with diamines and / or dicarboxylic acids, polyamides derived by using lactams, optionally in combination with diamines and / or dicarboxylic acids, etc. The polyamide may be a copolymer polyamide formed by two or more polyamide forming components.

[0103] The melting point of the polyamide is preferably 240° C. or higher, more preferably 245° C. or higher, and even more preferably 250° C. or higher. By using a polyamide having a melting point of 240° C. or higher, a polyacetal resin composition that is more excellent in mold deposit property and color difference change after retention in a molding machine can be obtained.

[0104] Examples of polyamides having a melting point of 240° C. or higher include polyamide 66, polyamide 46, polyamide 66 / 6T, polyamide 66 / 6I / 6T, etc. Among these polyamides, polyamide 66, polyamide 66 / 6T, and polyamide 66 / 6I / 6T are preferred, and polyamide 66 is more preferred.

[0105] In the resin composition, the amount of formaldehyde scavenger relative to 100 parts by mass of polyacetal resin is preferably 0.01 parts by mass or more, or 0.02 parts by mass or more, or 0.03 parts by mass or more, and preferably 3 parts by mass or less, or 2 parts by mass or less, or 1 part by mass or less.

[0106] The amount of formaldehyde scavenger in 100% by mass of the resin composition is preferably 0.001% by mass or more, or 0.005% by mass or more, or 0.01% by mass or more, and preferably 1.5% by mass or less, or 1.2% by mass or less, or 1.0% by mass or less.

[0107] [Formic acid scavengers] Polyacetal resin generates formaldehyde by decomposition, and formaldehyde is easily oxidized to formic acid. Formic acid can promote further decomposition of polyacetal resin like formaldehyde. Formic acid scavengers can suppress further decomposition of polyacetal resin by scavenging such formic acid. Examples of formic acid scavengers include, but are not limited to, hydroxides, inorganic acid salts, carboxylates, and alkoxides of alkali metals or alkaline earth metals. Examples include hydroxides of sodium, potassium, magnesium, calcium, barium, etc.; carbonates, phosphates, silicates, borates, carboxylates, and layered double hydroxides of the above metals.

[0108] The carboxylic acid of the carboxylate is preferably a saturated or unsaturated aliphatic carboxylic acid having 10 to 36 carbon atoms, and these carboxylic acids may be substituted with a hydroxyl group. Examples of the saturated or unsaturated aliphatic carboxylate include, but are not limited to, calcium dimyristate, calcium dipalmitate, calcium distearate, calcium (myristate-palmitate), calcium (myristate-stearate), calcium (palmitate-stearate), calcium 12-hydroxystearate, and the like, and among these, calcium dipalmitate, calcium distearate, and calcium 12-hydroxydistearate are preferred. The formic acid scavenger may be used alone or in combination of two or more kinds.

[0109] In the resin composition, the amount of the formic acid scavenger relative to 100 parts by mass of the polyacetal resin is preferably 0.01 parts by mass or more, or 0.02 parts by mass or more, or 0.03 parts by mass or more, and preferably 3 parts by mass or less, or 2 parts by mass or less, or 1 part by mass or less.

[0110] The amount of formic acid scavenger in 100% by mass of the resin composition is preferably 0.001% by mass or more, or 0.005% by mass or more, or 0.01% by mass or more, and preferably 1.5% by mass or less, or 1.2% by mass or less, or 1.0% by mass or less.

[0111] [Amount of formaldehyde scavenger and formic acid scavenger used] In one embodiment, the amount of the formaldehyde scavenger or the amount of the formic acid scavenger is preferably adjusted according to the amount of water in the kneading components or the resin composition. Since the decomposition of the polyacetal resin is promoted by the presence of water, it tends to be preferable to use a larger amount of the formaldehyde scavenger or the formic acid scavenger when the water content in the system is high. On the other hand, from the viewpoint of the physical properties of the resin composition, it tends to be desirable that the formaldehyde scavenger or the formic acid scavenger is not present in an excessively large amount in the kneading components or the resin composition. In one embodiment, since the water in the kneading components and the resin composition is mainly derived from the cellulose nanofibers, the amount of the formaldehyde scavenger or the amount of the formic acid scavenger in the kneading components or the resin composition is preferably adjusted according to the amount of water derived from the cellulose nanofibers in the kneading components or the resin composition.

[0112] In one embodiment, the content a1 [mass%] of the formaldehyde scavenger in all the kneading components, the moisture content b [mass%] of the cellulose nanofibers to be melt-kneaded, and the content c [mass%] of the cellulose nanofibers in all the kneading components are expressed by the following formula: b×c×0.00012+0.04≦a1≦b×c×0.015+0.2 As a result of repeated experiments and investigations, the present inventors have found that when the content rate a1 of the formaldehyde scavenger is within the above range, the decomposition of the polyacetal resin is satisfactorily suppressed by the formaldehyde scavenger, and the promotion of decomposition and deterioration of physical properties caused by the presence of an excess amount of the formaldehyde scavenger can be reduced.

[0113] In one embodiment, the content a2 [mass%] of the formic acid scavenger in all the kneading components, the moisture content b [mass%] of the cellulose nanofibers to be melt-kneaded, and the content c [mass%] of the cellulose nanofibers in all the kneading components are expressed by the following formula: b×c×0.00012+0.04≦a2≦b×c×0.015+0.2 As a result of repeated experiments and investigations, the present inventors have found that when the content a2 of the formic acid scavenger is within the above range, the decomposition of the polyacetal resin is satisfactorily suppressed by the formic acid scavenger, and the promotion of decomposition and the deterioration of physical properties caused by the presence of an excess of the formic acid scavenger can be reduced.

[0114] <Production of Resin Composition> The resin composition can be produced by a method including a step of melt-kneading cellulose nanofibers and polyacetal resin. In a typical embodiment, a dispersion (slurry) containing cellulose nanofibers is dried to obtain a dried body, and then the dried body is melt-kneaded with a polyacetal resin, according to the procedure exemplified below.

[0115] [Preparation of slurry] In one embodiment, the cellulose nanofibers may be prepared as a slurry dispersed in a liquid medium. The slurry may contain cellulose nanofibers and a solvent, and optionally additional components (such as a dispersant). As the liquid medium, water, the above-mentioned aprotic solvent, and the like can be suitably used. The concentration of the cellulose nanofibers in the slurry is preferably 5% by mass or more, or 10% by mass or more, or 15% by mass or more, or 20% by mass or more, or 25% by mass or more from the viewpoint of process efficiency during subsequent drying, and is preferably 60% by mass or less, or 55% by mass or less, or 50% by mass or less, or 45% by mass or less from the viewpoint of maintaining good handleability by avoiding an excessive increase in the viscosity of the slurry and solidification due to aggregation.

[0116] [Dry body formation] The slurry may then be dried to prepare a dried body. Various mixers can be used for drying, but a mechanically stirred mixer granulator is preferred because it allows drying at a relatively high shear rate. In one embodiment, drying is performed in a batch process using a mechanically stirred mixer granulator. The mechanically stirred mixer granulator may be a commercially available product, and examples of the mechanically stirred mixer include a device equipped with a stirring blade and a chopper blade inside the can body, such as a Lödige mixer (e.g., manufactured by Matsubo Co., Ltd.) and a high-speed vacuum dryer (e.g., manufactured by Earth Technica Co., Ltd.), and a fluid mixer equipped with a plurality of stirring blades (typically upper and lower blades) inside the can body, such as a Henschel mixer (FM mixer) (e.g., manufactured by Nippon Coke & Engineering Co., Ltd.). Among the drying conditions, controlling the shear rate, drying rate, drying temperature, and / or pressure (degree of reduced pressure) is useful for producing the dried body of the present disclosure. For example, rotation-revolution mixing and vacuum drying may be performed simultaneously.

[0117] The drying may be terminated when the cellulose nanofibers have been dried to such an extent that they can have a desired moisture content when melt-kneaded with the polyacetal resin.

[0118] The drying temperature may be, for example, 20° C. or more, or 30° C. or more, or 40° C. or more, or 50° C. or more from the viewpoints of drying efficiency and easily forming a dried body having a desired moisture content, and may be, for example, 160° C. or less, or 150° C. or less, or 140° C. or less, or 130° C. or less, or 100° C. or less from the viewpoints of making it difficult for thermal degradation of the cellulose nanofibers and additional components to occur and avoiding excessive pulverization of the dried body due to rapid drying of the slurry. The drying temperature is the temperature of the heat source in contact with the slurry, and is defined, for example, by the surface temperature of the temperature-control jacket of the drying device, the surface temperature of the heating cylinder, or the temperature of the hot air.

[0119] Drying may be performed under reduced pressure. In this case, the degree of reduced pressure may be -1 kPa or less, or -10 kPa or less, or -20 kPa or less, or -30 kPa or less, or -40 kPa or less, or -50 kPa or less from the viewpoint of drying efficiency and easily forming a dried body having a desired moisture content, and may be -100 kPa or more, or -95 kPa or more, or -90 kPa or more from the viewpoint of avoiding excessive pulverization of the dried body due to rapid drying of the slurry. The pressure may be adjusted by fully operating a vacuum pump having an appropriate exhaust capacity, or air and / or an inert gas may be intentionally introduced using a vacuum regulator, a leak valve, or the like. When air and / or an inert gas is introduced, it is preferable to provide an intake section in the can body of the drying device or upstream of the can body, since the medium vapor can be efficiently exhausted.

[0120] In the drying step, the residence time of the slurry at a temperature of 40° C. to 100° C. may be set to preferably 30 minutes to 600 minutes, 45 minutes to 300 minutes, or 60 minutes to 200 minutes. Drying under such conditions satisfactorily produces a dried product having a desired moisture content.

[0121] <Melt mixing> The dried cellulose nanofiber obtained as described above may be melt-kneaded with a polyacetal resin and, optionally, additional components. The melt-kneading method may include the following: - A method in which a resin monomer is mixed with a dried product, a polymerization reaction is carried out, the resulting resin composition is extruded into a strand shape, and cooled and solidified in a water bath to obtain a pellet-shaped molded product; - A method in which a mixture of the resin and the dried material is melt-kneaded using a single-screw or twin-screw extruder, extruded into a strand shape, and cooled and solidified in a water bath to obtain a pellet-shaped molded product; - A method in which a mixture of the resin and the dried material is melt-kneaded using a single-screw or twin-screw extruder, extruded into a rod or tube, and cooled to obtain an extrusion molded product; - A method in which a mixture of resin and a dried material is melt-kneaded using a single-screw or twin-screw extruder, and extruded through a T-die to obtain a sheet or film-like molded product; In a preferred embodiment, a mixture of the resin and the dried material is melt-kneaded using a single-screw or twin-screw extruder, extruded into a strand shape, and cooled and solidified in a water bath to obtain a pellet-shaped molded product.

[0122] For example, the dried material may be introduced into and mixed with the resin in a desired ratio, and then melt-kneaded.

[0123] By maintaining the moisture content of the cellulose nanofibers within a specific range during melt kneading, the moisture content of the resin composition during melt kneading can be controlled to a specific range. The moisture content of the resin composition during melt kneading is usually unchanged. For example, the moisture content of the cellulose nanofibers may be controlled by vacuum drying or the like during the period from the formation of the dried cellulose nanofiber to the melt kneading, for example, immediately before feeding the cellulose nanofibers into an extruder.

[0124] The polyacetal resin to be melt-kneaded usually contains almost no moisture. The moisture content of the polyacetal resin may be, for example, 0.2% by mass or less, or 0.15% by mass or less, or 0.1% by mass or less, and from the viewpoint of ease of process control, may be, for example, 0.0001% by mass or more, or 0.001% by mass or more.

[0125] For melt kneading, an extruder such as a single screw extruder or a twin screw extruder can be used, but a twin screw extruder is preferred in terms of controlling the dispersibility of the cellulose nanofibers. The L / D ratio, obtained by dividing the cylinder length (L) of the extruder by the screw diameter (D), is preferably 30 or more, and particularly preferably 40 or more. The screw rotation speed during kneading is preferably in the range of 50 to 800 rpm, and more preferably in the range of 100 to 600 rpm.

[0126] Each screw in the cylinder of the extruder is optimized by combining a conveying screw with an elliptical two-wing screw shape, a kneading element called a kneading disk, and the like.

[0127] The minimum processing temperature recommended by thermoplastic resin suppliers for polyacetal resin is 170°C to 190°C. The heating temperature setting is preferably in the range of 20°C higher than this recommended minimum processing temperature. By setting the mixing temperature in this temperature range, the cellulose nanofibers and the resin can be mixed more uniformly.

[0128] In one embodiment, a part of the resin composition obtained by melt kneading may be melt kneaded again as a part of the kneading components. In this case, for example, scraps and waste materials generated during molding of the resin composition can be recycled as materials for the resin composition, so that costs can be reduced by reducing waste. In 100% by mass of the kneading components, the mass ratio of the part derived from the resin composition is preferably 5% by mass or more, 10% by mass or more, or 15% by mass or more from the viewpoint of good recycling efficiency, and is preferably 65% ​​by mass or less, 60% by mass or less, or 50% by mass or less from the viewpoint of maintaining the intended properties of the resin composition well.

[0129] The resin composition of the present embodiment can be provided in various shapes, such as pellets, sheets, fibers, plates, rods, etc., with the pellet shape being preferred from the viewpoint of ease of post-processing and transportation.

[0130] <Pellets and pellet containers> One aspect of the present invention provides a pellet of the resin composition of this embodiment. Preferred pellet shapes include round, elliptical, and cylindrical shapes, and the shape may vary depending on the cutting method used during extrusion processing. For example, pellets cut by a cutting method called underwater cutting are often round, pellets cut by a cutting method called hot cutting are often round or elliptical, and pellets cut by a cutting method called strand cutting are often cylindrical. The preferred pellet diameter of round pellets is 1 mm or more and 3 mm or less. The preferred diameter of cylindrical pellets is 1 mm or more and 3 mm or less, and the preferred length is 2 mm or more and 10 mm or less. It is desirable to set the above diameter and length to be equal to or greater than the lower limit from the viewpoint of operational stability during extrusion, and it is desirable to set them to be equal to or less than the upper limit from the viewpoint of biteability into a molding machine during post-processing.

[0131] Another aspect of the present invention provides a pellet container that includes pellets of a resin composition containing cellulose nanofibers and a polyacetal resin, and a container that contains the pellets. In one aspect, the pellets in the pellet container are pellets of the resin composition of the present embodiment, and therefore have one or more of the properties exemplified in this disclosure for the resin composition and pellets. For example, the moisture content of the pellets (for the pellets in the pellet container, the pellets immediately after being removed from the container) is, in one aspect, 0.3% by mass or less, or 0.29% by mass or less, or 0.28% by mass or less, and in one aspect, 0.03% by mass or more, 0.04% by mass or more, or 0.05% by mass or more.

[0132] The moisture content of the pellets of this embodiment (in the case of pellets in a pellet storage container, pellets immediately after removal from the storage container) when allowed to stand for 48 hours at 40°C and saturated water vapor pressure may, in one embodiment, be 0.3 mass% or more, 0.4 mass% or more, 0.5 mass% or more, or 0.6 mass% or more, or 0.7 mass% or more, and in one embodiment, may be 5.0 mass% or less, or 4.0 mass% or less, or 3.0 mass% or less.

[0133] In one embodiment, the container for the pellet storage preferably has a water vapor transmission rate of 1 g / (m 2 24h) or less, or 0.5g / (m 2 24h) or less, or 0.1g / (m 2 .24h) or less. Examples of such materials include polyolefin and / or metal (particularly preferably aluminum). In the present disclosure, the water vapor permeability is a value measured in accordance with JIS Z0208.

[0134] The container preferably has a sealing means. Examples of the sealing means include solvent adhesion, heat welding, high frequency welding, laser welding, and a zipper, and heat welding by a heat sealer is preferred. In a preferred embodiment, the container is a packaging bag.

[0135] Conventionally, it has been thought that polyacetal resins do not cause problems due to moisture absorption during storage, and therefore no particular attention has been paid to the storage conditions of polyacetal resins. In the pellet storage of the present embodiment, contrary to conventional technical common sense, pellets, which are resin compositions containing polyacetal resins, are sealed and stored in an environment isolated from the outside air, thereby suppressing the molecular weight reduction caused by the decomposition of polyacetal resins due to moisture, which was not previously expected, and thus suppressing the generation of odors and gases from the resin composition and the generation of voids in the molded product.

[0136] <Kneaded product and molded product of resin composition> The resin composition of the present embodiment can be used as various molded articles. There is no particular limitation on the manufacturing method of the molded article, and the injection molding method, extrusion molding method, blow molding method, inflation molding method, foam molding method, etc. can be used. Among these, the injection molding method is particularly preferred from the viewpoint of design and cost.

[0137] When the moisture content of the resin composition of the present embodiment is controlled within the above-mentioned range, the decomposition of the polyacetal resin due to melt kneading during the production of the resin composition is suppressed, and the decomposition of the polyacetal resin due to heating when the resin composition is further heated and kneaded to produce a kneaded product, or when the resin composition is further molded to produce a molded product, can also be suppressed. In order to suppress the decomposition of the polyacetal resin during kneading or molding, the resin composition may be further dried after production. The resin composition may have the specific moisture content of the present embodiment by being stored in a state of high moisture content and then dried. By subjecting the resin composition that has undergone such a drying process to heat kneading or heat molding, a kneaded product or molded product in which the decomposition of the polyacetal resin is suppressed can be obtained.

[0138] One aspect of the present invention provides a method for producing a molded article from a resin composition containing cellulose nanofibers and polyacetal resin, the method comprising the steps of obtaining a resin composition containing cellulose nanofibers and polyacetal resin, and molding the resin composition to obtain a molded article, wherein the resin composition is molded in a state where the moisture content of the resin composition is 0.3 mass% or less, particularly 0.03 mass% or more and 0.3 mass% or less.

[0139] One aspect of the present invention provides a method for producing a kneaded product of a resin composition containing cellulose nanofibers and a polyacetal resin, the method including a storage step of storing the resin composition containing cellulose nanofibers and a polyacetal resin at a moisture content of more than 0.3 mass%, a drying step of drying the stored resin composition at a temperature Td that is 70°C or more lower than the melting point Tm of the polyacetal resin to a moisture content of 0.3 mass% or less, particularly 0.03 mass% or more and 0.3 mass% or less, and a heating step of heating and kneading the resin composition whose moisture content has been reduced to 0.3 mass% or less, particularly 0.03 mass% or more and 0.3 mass% or less in the drying step. In one aspect, the heating and kneading temperature is 175°C or more, or 180°C or more, or 190°C or more, and in one aspect, 230°C or less, or 220°C or less, or 210°C or less.

[0140] One aspect of the present invention provides a method for producing a molded article of a resin composition containing cellulose nanofibers and a polyacetal resin, the method comprising: a storage step of storing the resin composition containing cellulose nanofibers and a polyacetal resin at a moisture content of more than 0.3% by mass; a drying step of drying the stored resin composition at a temperature Td that is 70° C. or more lower than the melting point Tm of the polyacetal resin to a moisture content of 0.3% by mass or less, particularly 0.03% by mass or more and 0.3% by mass or less; and a molding step of hot molding the resin composition whose moisture content has been reduced to 0.3% by mass or less, particularly 0.03% by mass or more and 0.3% by mass or less in the drying step. In one aspect, the molding temperature is 175° C. or more, or 180° C. or more, or 190° C. or more, and in one aspect, 230° C. or less, or 220° C. or less, or 210° C. or less.

[0141] Even if the resin composition has a high moisture content due to the above-mentioned storage process, by undergoing the above-mentioned predetermined drying process, it is possible to produce a kneaded product and a molded article in which decomposition of the polyacetal resin is suppressed.

[0142] In the drying step, the difference (Tm-Td) between the melting point Tm and the temperature Td of the polyacetal resin is preferably 70° C. or more, 75° C. or more, or 80° C. or more from the viewpoint of suppressing decomposition of the polyacetal resin, and is 120° C. or less, 110° C. or less, or 100° C. or less from the viewpoint of drying efficiency. Examples of drying means include vacuum drying and hot air drying.

[0143] In one embodiment, the moisture content of the resin composition subjected to melt kneading or heat molding is 0.3% by mass or less, or 0.29% by mass or less, or 0.28% by mass or less. In one embodiment, the moisture content of the resin composition is 0.03% by mass or more, 0.04% by mass or more, or 0.05% by mass or more, from the viewpoint of improving the physical properties of the resin composition and the molded body by avoiding the promotion of decomposition of polyacetal and deterioration of cellulose nanofibers due to the heat required for drying. In one embodiment, the moisture content of the resin composition subjected to heat kneading or heat molding may be constant throughout the heat kneading or heat molding. Therefore, the moisture content of the kneaded product or molded product obtained by each of the above methods may be the same as the moisture content of the above resin composition.

[0144] <Storage method of resin composition> Another aspect of the present invention provides a method for storing a resin composition, comprising sealing and storing the resin composition containing cellulose nanofibers and a polyacetal resin in an environment not exposed to the outside air. In one aspect, the resin composition may be the resin composition of the present embodiment described above, and may be, for example, pellets of the resin composition. In one aspect, the environment not exposed to the outside air is an environment in which the water vapor transmission rate is 1 g / (m2 at a relative humidity of 40% and a temperature of 90°C. 2 The water vapor permeability is preferably 0.5 g / (m 2 24h) or less, or 0.1g / (m 2 The method for realizing the environment without contact with the outside air is not particularly limited, but an example of the method is a method of storing the resin composition (e.g., pellets of the resin composition) in a storage container (e.g., a packaging bag such as an aluminum bag) of the present disclosure.

[0145] As described above, it has been believed that polyacetal resins do not suffer from problems due to moisture absorption during storage, and therefore no particular attention has been paid to the storage conditions of polyacetal resins. In the method for storing a resin composition according to the present embodiment, contrary to conventional technical common sense, a resin composition containing a polyacetal resin is sealed and stored in an environment isolated from the outside air, thereby suppressing a molecular weight reduction caused by decomposition of the polyacetal resin due to moisture, which was not previously expected, and thereby suppressing the generation of odors and gases from the resin composition and the generation of voids in the molded product.

[0146] <Uses of resin composition and molded article> The resin composition and molded article of this embodiment are useful as substitutes for steel plates, fiber-reinforced plastics (e.g., carbon fiber-reinforced plastics, glass fiber-reinforced plastics, etc.), resin composites containing inorganic fillers, etc. Suitable applications of the resin composition and molded article include industrial machine parts, general machine parts, automobile, railway, vehicle, ship, and aerospace-related parts, electronic and electrical parts, building and civil engineering materials, daily necessities, sports and leisure goods, wind power generation housing members, containers and packaging members, etc. The resin composition and molded article of this embodiment use a polyacetal resin with suppressed molecular weight reduction in combination with cellulose nanofibers, and therefore can have excellent mechanical properties and sliding properties that are particularly suitable for gears in automobile applications, for example.

[0147] <Characteristics of resin composition and molded article> <Coefficient of variation of tensile breaking strength> In the resin composition and molded article of the present embodiment, the deterioration of the polyacetal resin is suppressed, so that the generation of voids inside the molded article can be suppressed. If voids exist inside the molded article, cracks originating from the voids will occur, causing variations in the tensile properties of the molded article, so reducing such voids is advantageous for improving the physical properties of the molded article. In the molded article, the coefficient of variation of the tensile breaking strength as an index of the variation of the tensile properties is preferably 0.1 or less, or 0.07 or less, or 0.05 or less. Although a smaller coefficient of variation is preferable, in one embodiment, from the viewpoint of ease of production of the resin composition and the molded article, it may be 0.005 or more, or 0.01 or more, or 0.02 or more. The tensile breaking strength and its coefficient of variation are values ​​measured by the method described in the [Examples] section of this disclosure.

[0148] <Maximum mountain height Sz> In the resin composition and molded article of the present embodiment, the deterioration of the polyacetal resin is suppressed, so that gas generation from the resin composition can be reduced. Since gas is one of the causes of the unevenness of the molded article surface, such suppression of gas generation is advantageous for improving the appearance and physical properties of the molded article. The maximum peak height Sz as an index of the unevenness of the molded article surface is preferably 70 μm or less, or 50 μm or less. Although it is desirable that the maximum peak height Sz is small, in one embodiment, from the viewpoint of ease of production of the resin composition and the molded article, it may be 1 μm or more, 5 μm or more, or 10 μm or more. The maximum peak height Sz is a value measured according to ISO25178 by the method described in the [Example] section of this disclosure. EXAMPLES

[0149] The following examples further illustrate exemplary embodiments of the present invention, but the present invention is not limited to these examples.

[0150] Evaluation method <Cellulose nanofiber> (Number average fiber diameter and L / D of cellulose nanofibers) The wet cake was diluted to 0.01% by mass with tert-butanol, dispersed using a high-shear homogenizer (manufactured by IKA, product name "Ultra Turrax T18") at a processing condition of 25,000 rpm for 5 minutes, cast onto mica, air-dried, and measured with a high-resolution scanning electron microscope. The measurement was performed by adjusting the magnification so that at least 100 cellulose nanofibers were observed, and the length (L), major axis (D) and ratio of these of 100 randomly selected cellulose nanofibers were obtained, and the arithmetic average of the 100 cellulose nanofibers was calculated.

[0151] (Mw of cellulose nanofiber) The wet cake was added to tert-butanol, and further dispersed in a mixer or the like until no aggregates were found. The concentration was adjusted to 0.5% by mass for 0.5 g of cellulose nanofiber solids. 100 g of the obtained tert-butanol dispersion was filtered on filter paper, dried at 150°C, and the filter paper was peeled off to obtain a sheet. The sheet had an air resistance of 100 sec / 100 ml or less per 10 g / m2 of sheet basis weight, and was obtained as a porous sheet. 0.88 g of the porous sheet was weighed, cut into small pieces with scissors, lightly stirred, and then 20 mL of pure water was added and left for one day. Next, the water and solids were separated by centrifugation. Next, 20 mL of acetone was added, lightly stirred, and left for one day. Next, the acetone and solids were separated by centrifugation. Next, 20 mL of N,N-dimethylacetamide was added, lightly stirred, and left for one day. The N,N-dimethylacetamide and solids were separated again by centrifugation, 20 mL of N,N-dimethylacetamide was added, and the mixture was left to stand for one day after lightly stirring. The N,N-dimethylacetamide and solids were separated by centrifugation, and 19.2 g of N,N-dimethylacetamide solution, which had been adjusted to have 8 mass percent lithium chloride, was added to the solids, and the mixture was stirred with a stirrer and visually confirmed to have dissolved. The solution in which the cellulose had been dissolved was filtered through a 0.45 μm filter, and the filtrate was used as a sample for gel permeation chromatography. The equipment and measurement conditions used are as follows.

[0152] Equipment: Tosoh HLC-8120 Column: TSKgel SuperAWM-H (6.0mm I.D. x 15cm) x 2 Detector: RI detector Eluent: N,N-dimethylacetamide (lithium chloride 0.2%) Flow rate: 0.6mL / min Calibration curve: Pullulan conversion

[0153] (Crystallization degree of cellulose nanofiber) The porous sheet was subjected to X-ray diffraction measurement, and the crystallinity was calculated according to the following formula. Crystallinity (%)=[I (200) -I (amorphous) ] / I (200) ×100 I (200) : Diffraction peak intensity due to 200 plane (2θ=22.5°) in cellulose I crystal I (amorphous) : The halo peak intensity due to the amorphous phase in cellulose I crystals, which is the peak intensity at an angle 4.5° lower than the diffraction angle of the 200 plane (2θ=18.0°) X-ray diffraction measurement conditions Equipment: MiniFlex (Rigaku Corporation) Operation axis 2θ / θ Source CuKα Measurement method: Continuous Voltage 40kV Current 15mA Starting angle 2θ=5° End angle 2θ=30° Sampling width 0.020° Scan speed: 2.0° / min Sample: A porous sheet is attached onto the sample holder.

[0154] (Degree of acetylation (DS) of acetylated cellulose nanofiber) The infrared spectrum of the porous sheet at five points was measured by the ATR-IR method using a Fourier transform infrared spectrophotometer (FT / IR-6200 manufactured by JASCO Co., Ltd.) The infrared spectrum measurement was performed under the following conditions. Number of times accumulated: 64 times, Wavenumber resolution: 4cm -1 , Measurement wave number range: 4000~600cm -1 , ATR crystal: Diamond, Incident angle: 45°

[0155] From the obtained IR spectrum, the IR index was calculated using the following formula: IR index = H1730 / H1030 In the formula, H1730 and H1030 are at 1730 cm -1 , 1030cm -1 (absorption band of CO stretching vibration of cellulose backbone chain) -1 and 1500cm -1 The line connecting the -1 and 1500cm -1 The line connecting these points is taken as the baseline, and the absorbance is calculated when this baseline is taken as 0. The average degree of substitution at each measurement site was calculated from the IR index according to the following formula, and the average value was taken as DS. DS = 4.13 × IR index

[0156] (Moisture percentage) The moisture content in cellulose nanofiber or pulp was measured under the following conditions using an A&D heat-drying moisture meter (MX-50). Heating temperature: 120℃ Measurement mode: Standard mode, standard heating Measurement accuracy: MID. (Measurement end condition: less than 0.05% / min)

[0157] <Resin composition and molded article> (Moisture percentage) The moisture content of the resin composition was measured using a Karl Fischer moisture meter in accordance with ISO15512.

[0158] (Amount of formaldehyde scavenger and formic acid scavenger present in resin composition) It was calculated from the mixing ratio of the ingredients.

[0159] (Coefficient of variation of tensile breaking strength) A multipurpose test piece (A type) was molded in accordance with ISO 3167 using an injection molding machine (PS-40E: manufactured by Nissei Plastics Co., Ltd.) with a cylinder temperature set to 200°C. The mold temperature was set to 80°C. A tensile test was performed in accordance with ISO 527 using the obtained tensile test piece. The crosshead speed was set to 5 mm / min, and the tensile breaking strength was measured. The number of pieces was 5, and the coefficient of variation for the tensile breaking strength of n=5 was calculated from the following formula. CV = (σ / μ) × 100 Here, μ and σ are given by the following equations:

number

[0160] (Odor during extrusion process) The odor around the extruder die during processing in the extruder was evaluated according to the following criteria. Good: No odor at all or a slightly sweet odor. Possible: A pungent odor of formaldehyde is felt. Poor: Strong, irritating odor of formaldehyde. Regarding odor, good and fair are passable levels, and poor is an unacceptable level.

[0161] (Odor during injection molding) The odor around the mold mounting position of the injection molding machine was evaluated using the same criteria as for the odor during the extrusion process described above.

[0162] (Maximum mountain height Sz) The maximum peak height Sz was measured in accordance with ISO 25178 for an area of ​​2 mm × 4 mm at the center of the mold fixing side of the dumbbell pieces obtained in accordance with ISO 3167, and the number average value for five dumbbells was calculated as the target maximum peak height Sz. The maximum peak height Sz was measured using a white light interference optical microscope (Contour-GT-K, manufactured by Bruker). Sz is at a pass level of 50 or less and at a fail level of over 50.

[0163] ≪Materials used≫ <Polyacetal resin> Polyacetal homopolymer (Tenac 4010, melting point 175°C, available from Asahi Kasei Corporation) Polyacetal copolymer (Tenac 4520, melting point 165°C, available from Asahi Kasei Corporation) Polyacetal copolymer (Tenac HC450, melting point 168°C, available from Asahi Kasei Corporation)

[0164] <Acetylated cellulose nanofiber> [Preparation Example 1] Cotton linter pulp was stirred in dimethyl sulfoxide (DMSO) at room temperature for 1 hour at 500 rpm using a single-shaft mixer (IMEX DKV-1 φ125 mm dissolver).Then, the mixture was fed to a bead mill (IMEX NVM-1.5) using a hose pump and circulated for 120 minutes using only DMSO to obtain a defibrated slurry.

[0165] Then, 11 parts by mass of vinyl acetate and 1.63 parts by mass of sodium bicarbonate were added to the bead mill device per 100 parts by mass of the defibrated slurry, and the device was further circulated for 60 minutes to obtain an acetylated cellulose nanofiber slurry.

[0166] During circulation operation, the rotation speed of the bead mill was 2500 rpm and the peripheral speed was 12 m / s. The beads used were made of zirconia and had a diameter of 2.0 mm, and the filling rate was 70% (the slit gap of the bead mill at this time was 0.6 mm). During circulation operation, the slurry temperature was controlled at 40°C using a chiller to absorb heat generated by friction.

[0167] The acetylated cellulose nanofiber slurry was mixed with 192 parts by mass of pure water per 100 parts by mass of the defibrated slurry, and the mixture was thoroughly stirred and then concentrated in a dehydrator. The wet cake was dispersed again in the same amount of pure water, stirred, and concentrated, and this washing procedure was repeated a total of five times.

[0168] To the obtained aqueous dispersion of acetylated cellulose nanofibers (solid content: 10% by mass), 5 parts by mass of polyethylene glycol derivative (GL3000) was added per 100 parts by mass of acetylated cellulose nanofiber, and the mixture was then vacuum dried at approximately 40°C using a revolution / rotation type mixer (EME V-mini300) to obtain acetylated cellulose nanofiber powder.

[0169] The properties of the resulting wet cake of acetylated cellulose nanofibers were evaluated, and the following results were obtained.

[0170] DS: 0.96, number average fiber diameter: 65 nm, L / D: approx. 450, Mw: 340,000, crystallinity: 75% This acetylated cellulose nanofiber is referred to as CNF(0.96).

[0171] [Preparation Examples 2-4] By adjusting the circulation operation time after adding vinyl acetate and sodium bicarbonate to the bead mill device, three types of acetylated cellulose nanofibers with different degrees of acetylation were obtained. (Preparation Example 2) CNF (0.41) DS: 0.41, number average fiber diameter: 60 nm, L / D: about 470, Mw: 370,000, crystallinity: 80% (Preparation Example 3) CNF (0.71) DS: 0.71, number average fiber diameter: 64 nm, L / D: about 450, Mw: 350,000, crystallinity: 79% (Preparation Example 4) CNF (1.29) DS: 1.29, number average fiber diameter: 69 nm, L / D: about 430, Mw: 330,000, crystallinity: 78%

[0172] <Non-modified cellulose nanofiber> [Preparation Example 5] Celish KY-100G (manufactured by Daicel FineChem Co., Ltd.) powder was diluted with pure water to a concentration of 1% by mass, and mixed in a single-shaft stirrer at 500 rpm for 20 minutes. The water content was then adjusted by filtration to a solid content of 10% by mass, to obtain a cellulose nanofiber aqueous dispersion. Polyethylene glycol (PEG20000, available from Sanyo Chemical Industries, Ltd.) was then added to the cellulose nanofiber aqueous dispersion in an amount of 5 parts by mass per 100 parts by mass of cellulose nanofiber, and the mixture was vacuum-dried at about 40°C using a revolution / rotation stirrer to obtain cellulose nanofiber powder CNF(0). The properties were evaluated, and the following results were obtained. CNF(0) DS: 0, number average fiber diameter: 71 nm, L / D: about 220, Mw: 250,000, crystallinity: 66%

[0173] <Additional Ingredients> Dispersing agent: Polyethylene glycol (GL3000), available from Sigma-Aldrich Hindered phenolic antioxidant: Irganox, available from BASF Japan Ltd. Additives: Ethylene bis-stearylamide Kaowax EB-FF Available from Kao Corporation Formaldehyde scavenger: melamine, available from Nissan Chemical Industries, Ltd. Formic acid scavenger: calcium stearate, available from Sakai Chemical Industry Co., Ltd.

[0174] <Production of Resin Composition>

[0175] The screw configuration was such that two kneading discs (RKD) with a feeding function were arranged in the center of the extruder, and one kneading disc (LKD) with a return function was arranged next to one RKD just before the reduced pressure degassing on the downstream side, in that order.

[0176] The screw speed of the extruder was set to 150 rpm, and the feeder was set to give a total extrusion output of 5 kg / hour. Various tests were carried out using the obtained pellets. The results are shown in Table 1 as Reference Example 1.

[0177] [Example 1] The cylinder temperature of the co-rotating twin screw extruder ZSK26MC (manufactured by Coperion) with L / D=48 and one inlet each on the upstream side and the center of the extruder was set to 200 ° C., and 100 parts by mass of Tenac 4520 as a polyacetal resin, 0.25 parts by mass of a hindered phenol-based antioxidant, 0.15 parts by mass of a nitrogen-containing compound, and 0.2 parts by mass of melamine were dry blended and fed at a fixed amount from a loss-in-weight feeder installed at the upstream inlet, and 10.5 parts by mass of CNF (0) was fed at a fixed amount from a loss-in-weight feeder installed at the central inlet of the extruder so that the amount was 10.5 parts by mass per 100 parts by mass of the polyacetal resin, and melt-kneaded, extruded into a strand shape, and cooled and cut to obtain a pellet-shaped polyacetal resin composition. The downstream of the extruder was made degassable under reduced pressure, and the air and generated gas in the extruder were removed.

[0178] The CNF(0) used here was vacuum dried at 80°C for 5 hours using a vacuum dryer immediately before being fed into the extruder, and was melt-kneaded at a moisture content of 1.6% by mass.

[0179] The screw configuration was such that three RKDs were placed upstream of the central supply port of the extruder, and three RKDs and one LKD were placed in that order just before the downstream decompression degassing. The screw rotation speed of the extruder was set to 150 rpm, and the feeder was set to a total extrusion discharge rate of 5 kg / hour. Various tests were carried out using the obtained pellets. The results are shown in Table 1 as Example 1.

[0180] [Comparative Example 1] The CNF(0) used was extruded and evaluated in the same manner as in Example 1, except that the vacuum drying treatment before melt kneading was not performed. The moisture content of the CNF before melt kneading was 12% by mass. The results are shown in Table 1.

[0181] [Examples 2 to 6] The same procedures as in Example 1 were carried out except that the types of polyacetal resin and cellulose were changed as shown in Table 1, and various tests were carried out using the obtained pellets. The results are shown in Table 1.

[0182] [Comparative Examples 2 to 6] Except for changing the types of polyacetal resin and cellulose as shown in Table 1, the same procedures as in Comparative Example 1 were carried out, and various tests were carried out using the obtained pellets. The results are shown in Table 1.

[0183] [Comparative Example 7] Except for changing the type of cellulose to cotton linter pulp shown in Table 1, the same procedures as in Example 1 were carried out, and various tests were carried out using the obtained pellets. The results are shown in Table 1. In Comparative Example 7, pulp was used in place of cellulose nanofibers in kneading with polyacetal resin, and therefore drying did not progress to the inside of the pulp in the vacuum drying treatment under the above-mentioned conditions of 80°C for 5 hours, and as the pulp was defibrated during extrusion, fibers with high water retention were exposed, which is thought to have accelerated the decomposition of the polyacetal resin.

[0184] <Production of resin compositions with various moisture contents> [Examples 7 to 8, Comparative Example 8] The drying time of the cellulose before melt-kneading in the extruder was changed to Example 7: 90 minutes, Example 8: 45 minutes, and Comparative Example 8: 30 minutes, respectively, so that the moisture content was as shown in Table 2. Except for this, all operations were carried out in the same manner as in Example 1, and various tests were carried out using the obtained pellets. The results are shown in Table 2.

[0185] <Production of Molded Product> [Example 9] The resin composition obtained in Example 1 was placed in an aluminum bag (water vapor transmission rate at a relative humidity of 40% and a temperature of 90°C measured according to JIS Z0208: 0.5 to 1.0 g / (m 224h), the same applies below.) for 2 days, and then, in a state where the moisture content of the resin composition was 0.03% by mass to 0.3% by mass, it was molded into an ISO37 Type 3 tensile test piece with a thickness of 2 mm using an EC5P injection molding machine (manufactured by Shibaura Machine Co., Ltd.) with a cylinder temperature set to 200°C. The mold temperature was set to 60°C. Various tests were carried out using the obtained tensile test piece.

[0186] [Examples 10 and 11] After obtaining the resin composition, the storage method was changed to Example 10: in air, and Example 11: indoors at 23°C and 50 RH%, and the moisture content of the resin composition showed the values ​​shown in Table 3. Therefore, the resin composition was vacuum dried under conditions of 80°C for 48 hours, and test pieces were molded in the same manner as in Example 9 when the moisture content of the resin composition was 0.03% by mass to 0.3% by mass, and various tests were carried out. The results are shown in Table 3.

[0187] [Example 12] The resin composition obtained in Comparative Example 1 was placed in an aluminum bag and stored for two days, after which the moisture content of the resin composition showed the value shown in Table 3. Therefore, it was vacuum dried under conditions of 80°C for 48 hours, and in a state in which the moisture content of the resin composition was 0.03% by mass to 0.3% by mass, it was molded into an ISO37 Type 3 tensile test piece having a thickness of 2 mm using an EC5P injection molding machine (manufactured by Shibaura Machine Co., Ltd.) with a cylinder temperature set to 200°C. The mold temperature was set to 60°C. Various tests were carried out using the obtained tensile test piece.

[0188] [Example 13] Except for changing the storage method to air, the same procedure as in Example 12 was carried out, and various tests were carried out using the obtained test pieces. The results are shown in Table 3.

[0189] [Comparative Examples 9 to 12] The type of resin composition and the storage method were changed as shown in Table 3, and the vacuum drying treatment was not performed. Except for this, the same procedures as in Example 10 were carried out, and various tests were carried out using the obtained test pieces. The results are shown in Table 3.

[0190] [Examples 14 to 16] The same procedures as in Example 9 were carried out except that the cellulose was changed as shown in Table 4, and various tests were carried out using the obtained test pieces. The results are shown in Table 4.

[0191] [Examples a-1 to a-12, b-1 to b-9] As in Example 7, the drying time of the cellulose was changed, and CNF(0.96) was produced with a moisture content of 0.2 mass%, 2 mass%, or 5 mass%. The same procedure was carried out as in Example 1, except that the formulations shown in Tables 5 and 6 were changed, to obtain pellets. The water vapor transmission rate at a relative humidity of 40% and a temperature of 90°C was 1 g / (m 2 100 g of the obtained pellets were placed in a packaging bag (aluminum bag) with a shelf life of 100 minutes or less (24 hours), which was then heat sealed and left to stand at 23°C for 24 hours. The packaging bag was then opened and the odor was evaluated according to the following criteria. Good: No odor Possible: Slight odor. Bad: Strong odor. Regarding odor, "good" and "fair" are acceptable levels, and "poor" is unacceptable level. The results are shown in Tables 5 and 6.

[0192] [Table 1]

[0193] [Table 2]

[0194] [Table 3]

[0195] [Table 4]

[0196] [Table 5]

[0197] [Table 6] [Industrial Applicability]

[0198] INDUSTRIAL APPLICABILITY The resin composition according to one aspect of the present invention reduces odor and gas generation and can suppress void generation in a molded article, and therefore can be suitably applied to various applications.

Claims

1. A method for producing a resin composition containing cellulose nanofibers and a polyacetal resin, comprising: A step of melt-kneading a kneading component containing the cellulose nanofiber and a polyacetal resin in a state in which the moisture content of the cellulose nanofiber is 0.01% by mass or more and 5% by mass or less to obtain a resin composition; and storing the resin composition at a moisture content of 0.03% by mass or more and 0.3% by mass or less; A method comprising:

2. The method according to claim 1 , wherein a portion of the stored resin composition is used as part of the kneading ingredients.

3. The method according to claim 1, wherein the number average fiber diameter of the cellulose nanofibers is 10 to 1000 nm.

4. The method according to claim 1, wherein the acyl substitution degree of the cellulose nanofiber is 0.5 to 1.

5.

5. The method according to claim 1 , wherein the crystallinity of the cellulose nanofiber is 60% or more.

6. The method according to claim 1 , wherein the moisture content of the stored resin composition is 0.03% by mass or more and 0.3% by mass or less.

7. The kneading components contain a formaldehyde scavenger, and a content a1 [mass%] of the formaldehyde scavenger in the entire kneading components, a moisture content b [mass%] of the cellulose nanofibers subjected to the melt kneading, and a content c [mass%] of the cellulose nanofibers in the entire kneading components are expressed by the following formula: b×c×0.00012+0.04≦a1≦b×c×0.015+0.2 The method according to any one of claims 1 to 6, wherein the following relationship is satisfied:

8. The kneading components contain a formic acid scavenger, and the content a2 [mass%] of the formic acid scavenger in the entire kneading components, the moisture content b [mass%] of the cellulose nanofibers subjected to the melt kneading, and the content c [mass%] of the cellulose nanofibers in the entire kneading components are expressed by the following formula: b×c×0.00012+0.04≦a2≦b×c×0.015+0.2 The method according to any one of claims 1 to 6, wherein the following relationship is satisfied:

9. A pellet of a resin composition containing cellulose nanofibers and a polyacetal resin, the moisture content of the resin composition being 0.03% by mass or more and 0.3% by mass or less.

10. The pellet according to claim 9, wherein the number average fiber diameter of the cellulose nanofibers is 10 to 1000 nm.

11. The pellet according to claim 9, wherein the cellulose nanofiber has an acyl substitution degree of 0.5 to 1.

5.

12. The pellet according to claim 9, wherein the cellulose nanofiber has a crystallinity of 60% or more.

13. The pellet according to claim 9, which has a moisture content of 0.3% by mass to 5.0% by mass when left to stand at 40° C. under saturated water vapor pressure for 48 hours.

14. A molded body of a resin composition containing cellulose nanofibers and a polyacetal resin, the moisture content of the molded body being 0.03 mass% or more and 0.3 mass% or less.

15. The molded body according to claim 14, wherein the number average fiber diameter of the cellulose nanofibers is 10 to 1000 nm.

16. The molded article according to claim 14, wherein the cellulose nanofiber has an acyl substitution degree of 0.5 to 1.

5.

17. The molded article according to claim 14, wherein the cellulose nanofiber has a degree of crystallinity of 60% or more.

18. A method for producing a molded article of a resin composition containing cellulose nanofibers and a polyacetal resin, comprising: A step of obtaining a resin composition containing cellulose nanofibers and a polyacetal resin; A step of adjusting the moisture content of the resin composition to 0.03% by mass or more and 0.3% by mass or less; and A step of molding the resin composition in a state where the moisture content of the resin composition is 0.03% by mass or more and 0.3% by mass or less to obtain a molded product; A method comprising:

19. A method for producing a kneaded product of a resin composition containing cellulose nanofibers and a polyacetal resin, comprising: a storage step of storing a resin composition containing the cellulose nanofibers and the polyacetal resin at a moisture content of more than 0.3% by mass; A drying process of drying the stored resin composition at a temperature Td that is 70° C. or more lower than the melting point Tm of the polyacetal resin to a moisture content of 0.03% by mass or more and 0.3% by mass or less; and a heating step of heating and kneading the resin composition having a moisture content of 0.03% by mass or more and 0.3% by mass or less in the drying step; A method comprising:

20. A method for producing a molded article of a resin composition containing cellulose nanofibers and a polyacetal resin, comprising: a storage step of storing a resin composition containing the cellulose nanofibers and the polyacetal resin at a moisture content of more than 0.3% by mass; A drying process of drying the stored resin composition at a temperature Td that is 70° C. or more lower than the melting point Tm of the polyacetal resin to a moisture content of 0.03% by mass or more and 0.3% by mass or less; and a molding step of hot-molding the resin composition having a moisture content of 0.03% by mass or more and 0.3% by mass or less in the drying step; A method comprising:

21. The method according to any one of claims 18 to 20, wherein the resin composition is obtained by the method according to claim 1.

22. A resin composition containing cellulose nanofibers and a polyacetal resin was prepared using a resin having a water vapor transmission rate of 1 g / (m2) at a relative humidity of 40% and a temperature of 90°C. 2 A method for storing a resin composition, comprising storing the composition in a sealed packaging bag for no longer than 24 hours.

23. The method according to claim 22, wherein the resin composition is a pellet according to any one of claims 9 to 13.

24. A pellet-containing product comprising pellets of a resin composition containing cellulose nanofibers and a polyacetal resin, and a container for containing the pellets, The pellet-containing item has a moisture content of 0.03% by mass or more and 0.3% by mass or less.

25. The pellet-containing item according to claim 24, wherein the moisture content when the pellets are allowed to stand at 40° C. under saturated water vapor pressure for 48 hours is 0.3% by mass to 5.0% by mass.

26. The container has a water vapor transmission rate of 1 g / (m 2 The pellet container according to claim 24 or 25, which is made of a material having a thickness of 24h or less and has a sealing means.

Citation Information

Patent Citations

  • Polyacetal resin composition

    WO2010119810A1

  • Polyacetal resin composition and method for producing same

    WO2012049926A1

  • Fiber-reinforced resin composition comprising chemically modified cellulose nanofibers and thermoplastic resin