Tempered glass

The tempered glass with a tailored stress profile, achieved through controlled ion exchange, addresses the issue of insufficient impact resistance, resulting in enhanced durability.

JP7565000B2Active Publication Date: 2024-10-10NIPPON ELECTRIC GLASS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023097009
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-10
Filing Date
2023-06-13
Publication Date
2024-10-10
Estimated Expiration
2039-10-08

AI Technical Summary

Technical Problem

Existing tempered glass lacks sufficient impact resistance, particularly in applications requiring higher durability.

Method used

A tempered glass design with a specific stress profile characterized by a compressive stress layer and tensile stress layer, featuring inflection points and stress values optimized to enhance impact resistance, achieved through controlled ion exchange processes.

Benefits of technology

The optimized stress profile results in tempered glass with significantly improved impact resistance, demonstrated by higher pseudo-casing drop strength tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565000000006
    Figure 0007565000000006
  • Figure 0007565000000007
    Figure 0007565000000007
  • Figure 0007565000000008
    Figure 0007565000000008
Patent Text Reader

Abstract

To provide a strengthened glass having higher impact resistance in comparison to a prior art.SOLUTION: A strengthened glass has a surface and a thickness T, where the thickness T is thicker than 0.3 mm, the maximum value of a compression stress on the surface is more than 661 MPa when a compression stress is a positive number and a tensile stress is a negative number, a stress profile obtained by measuring a stress in a depth direction from the surface has a point of inflection where the secondary derivative of a stress profile becomes zero between the surface and a depth half the thickness T from the surface, the stress profile has a stress zero point where the stress becomes zero, and the stress zero point exists at a position deeper than 17% of thickness T from the surface.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to tempered glass and a manufacturing method thereof, and more particularly to tempered glass suitable for use as cover glass for mobile phones, digital cameras, PDAs (personal digital assistants), and touch panel displays, and a manufacturing method thereof. [Background technology]

[0002] Devices such as mobile phones (especially smartphones), digital cameras, PDAs, touch panel displays, large TVs, and non-contact power supplies are becoming more and more popular. Ion-exchanged tempered glass is used for these applications. In recent years, tempered glass has also been increasingly used for the exterior parts of digital signage, mice, smartphones, etc.

[0003] The tempered glass has a compressive stress layer formed by ion exchange treatment on its surface, which suppresses the formation and propagation of cracks on the surface and provides high strength. It is believed that the strength of tempered glass can be improved by adjusting the formation mode of such a compressive stress layer (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2013 / 088856 Summary of the Invention [Problem to be solved by the invention]

[0005] However, there is still room for improvement in terms of achieving higher impact resistance.

[0006] An object of the present invention is to provide a tempered glass having higher impact resistance than the prior art. [Means for solving the problem]

[0007] (1) The present invention, which has been invented to solve the above problems, is a tempered glass having a surface and a thickness T, the thickness T being greater than 0.3 mm, and a maximum value of the compressive stress at the surface being 661 MPa or more when compressive stress is a positive number and tensile stress is a negative number, and a stress profile obtained by measuring stress in a depth direction from the surface has an inflection point where a second derivative of the stress profile is zero between the surface and a depth that is half the thickness T, and the stress profile has a zero stress point where stress is zero, and the zero stress point is located at a position deeper than 17% of the thickness T from the surface.

[0008] (2) In the above configuration (1), the maximum value of the compressive stress on the surface is preferably 750 MPa or more.

[0009] (3) In the above (1) or (2), the glass composition preferably contains Li2O.

[0010] (4) In the above configuration (3), the glass composition preferably contains, by mass, 40-70% SiO2, 10-30% Al2O3, 0-10% B2O3, 2-11% Li2O, 5-25% Na2O, 0-10% K2O, 0-6% MgO, and 50-20% P2O.

[0011] (5) In any one of the above configurations (1) to (3), it is preferable that the depth from the surface of a first inflection point, which is located closest to the surface among the inflection points, is less than 50 μm.

[0012] (6) In the above configuration (5), the compressive stress at the first inflection point is preferably 40 MPa or more.

[0013] (7) In the above configuration (5) or (6), the compressive stress at the first inflection point is preferably 150 MPa or less.

[0014] (8) In any one of the above configurations (5) to (7), the second inflection point is preferably located deeper than the first inflection point.

[0015] (9) In the above configuration (8), it is preferable that the second inflection point has a depth from the surface of 60 μm or more.

[0016] (10) In the above configuration (8) or (9), when the stress at the first inflection point is σ1, the depth from the surface of the first inflection point is d1, the stress at the second inflection point is σ2, and the depth from the surface of the second inflection point is d2, it is preferable that (σ1-σ2) / (d1-d2) is -1.0 MPa / μm or more.

[0017] (11) In any one of the above configurations (8) to (10), the compressive stress at the second inflection point is preferably 45 MPa or less. Effect of the Invention

[0018] According to the present invention, it is possible to obtain tempered glass having higher impact resistance than conventional techniques. [Brief description of the drawings]

[0019] [Figure 1] 1 is a schematic diagram showing a cross section of tempered glass according to an embodiment of the present invention. [Diagram 2] 1 is a graph showing an outline of a stress profile in a thickness direction of a strengthened glass according to an embodiment of the present invention. [Diagram 3] 1 is a graph showing an outline of a stress profile in a thickness direction of a strengthened glass according to an embodiment of the present invention. [Figure 4] FIG. 1 is a flow diagram of a method for producing tempered glass according to an embodiment of the present invention. [Diagram 5] 1 is a graph showing a stress profile of tempered glass according to Sample No. 4. [Figure 6] 1 is a graph showing a stress profile of tempered glass according to Sample No. 6. [Figure 7]4 is a graph showing stress profiles of tempered glasses according to Samples No. 1 to 3 after a first ion exchange process. [Figure 8] 1 is a graph showing stress profiles of tempered glasses according to Samples Nos. 4 to 7 after a first ion exchange process. [Figure 9] FIG. 2 is a schematic diagram showing a drop test method in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, the tempered glass according to an embodiment of the present invention will be described.

[0021] (Tempered glass) As shown in FIG. 1, the tempered glass 1 according to this embodiment is a plate-shaped chemically tempered glass that has been chemically tempered by ion exchange, and includes a compressive stress layer 2 and a tensile stress layer 3.

[0022] The thickness T of the tempered glass 1 is preferably 2.0 mm or less, 1.8 mm or less, 1.6 mm or less, 1.4 mm or less, 1.2 mm or less, 1.0 mm or less, 0.9 mm or less, 0.85 mm or less, or 0.8 mm or less. The thickness T of the tempered glass 1 is preferably 0.03 mm or more, 0.05 mm or more, 0.1 mm or more, 0.15 mm or more, 0.2 mm or more, 0.25 mm or more, 0.3 mm or more, 0.35 mm or more, 0.4 mm or more, 0.45 mm or more, 0.5 mm or more, 0.6 mm or more, or 0.65 mm or more. The thickness T of the tempered glass 1 is not limited thereto and may be determined arbitrarily.

[0023] The compressive stress layer 2 is formed on a surface layer portion including the main surface 1a and the end face 1b of the strengthened glass 1. The tensile stress layer 3 is formed inside the strengthened glass 1, that is, at a position deeper than the compressive stress layer 2.

[0024] The stress profile (stress distribution) of the tempered glass 1 is obtained by measuring the stress in the depth direction (direction perpendicular to the main surface 1a) from the main surface 1a side, with compressive stress being a positive number and tensile stress being a negative number. The stress profile of the tempered glass 1 thus obtained is shown, for example, in FIG. 2. In the graph of FIG. 2, the vertical axis indicates stress, and the horizontal axis indicates the position (depth) in the thickness direction based on one of the main surfaces 1a. In the graph of FIG. 2, a positive value of stress indicates compressive stress, and a negative value of stress indicates tensile stress. That is, the larger the absolute value of the stress in the graph of FIG. 2, the larger the stress. Note that FIG. 2 is a conceptual diagram, and the stress profile of the tempered glass 1 is not limited to this embodiment.

[0025] The stress profile of the tempered glass 1 has a maximum compressive stress CSmax at point A corresponding to the main surface 1a. The maximum compressive stress CSmax is 400 MPa or more, preferably 450 MPa or more, 500 MPa or more, 550 MPa or more, 600 MPa to 1200 MPa, 600 MPa to 1150 MPa, 600 MPa to 1100 MPa, 600 MPa to 1050 MPa, 600 MPa to 1000 MPa, 700 MPa to 950 MPa, 700 MPa to 900 MPa, or 750 MPa to 900 MPa.

[0026] The stress profile of the strengthened glass 1 has an inflection point where the second derivative of the stress profile becomes zero between the main surface 1a (point A) and a depth (point B) that is half the thickness T. In this embodiment, the stress profile has a plurality of inflection points. Of the plurality of inflection points, the inflection point closest to the main surface 1a is defined as a first inflection point C, and the inflection point deeper than the first inflection point (i.e., the inflection point next closest to the main surface 1a after the first inflection point C) is defined as a second inflection point D.

[0027] The stress σ1 at the first inflection point C is a compressive stress. The stress σ1 at the first inflection point C is 150 MPa or less, preferably 140 MPa or less, 130 MPa or less, 120 MPa or less, 110 MPa or less, 100 MPa or less, 90 MPa or less, 80 MPa or less, 70 MPa or less, 30 MPa to 80 MPa, or 40 MPa to 75 MPa.

[0028] At the first inflection point C, the value of the second derivative of the stress profile changes from positive to negative.

[0029] The depth d1 of the first inflection point C from the main surface 1a is preferably 50 μm or less, 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, or 25 μm or less.

[0030] The stress σ2 at the second inflection point D is preferably 45 MPa or less, 40 MPa or less, 35 MPa or less, 30 MPa or less, 25 MPa or less, 20 MPa or less, 15 MPa or less, or 10 MPa or less. The stress σ2 at the second inflection point D may be a negative value, that is, a tensile stress.

[0031] At the second inflection point D, the value of the second derivative of the stress profile changes from negative to positive.

[0032] The depth of the second inflection point D from the main surface 1a is preferably 60 μm or deeper, 70 μm or deeper, 80 μm or deeper, 90 μm or deeper, 95 μm or deeper, 100 μm or deeper, 110 μm or deeper, 120 μm or deeper, or 130 μm or deeper.

[0033] It is preferable that the following relationship be established among the stress σ1 at the first inflection point C, the depth d1 of the first inflection point C, the stress σ2 at the second inflection point D, and the depth d2 of the second inflection point D. In other words, it is preferable that (σ1-σ2) / (d1-d2) is -1.0 MPa / μm or more. (σ1-σ2) / (d1-d2) is more preferably -0.9 MPa / μm or more, -0.8 MPa / μm or more, -0.7 MPa / μm or more, -0.6 MPa / μm or more, -0.5 MPa / μm or more, or -0.4 MPa / μm or more.

[0034] The stress profile of the tempered glass 1 has a zero stress point E where the stress is zero. Normally, it is difficult for the depth DOLzero of the zero stress point E from the main surface 1a to exceed 20% of the thickness T, and the physical limit is about 22%, but in this embodiment, it is possible to obtain a DOLzero that exceeds this limit. The greater the depth DOLzero of the zero stress point E, the higher the strength against penetration by a protrusion. The depth DOLzero of the stress zero point E from the main surface 1a is preferably 12% or more, 12.5% ​​or more, 13% or more, 13.5% or more, 14% or more, 14.5% or more, 15% or more, 15.5% or more, 16% or more, 16.5% or more, 17% or more, 17.5% or more, 18% or more, 18.5% or more, 19% or more, 19.5% or more, 20% or more, 20.5% or more, 21% or more, 21.5% or more, 22.0% or more, 22.5% or more, 23% or more, 23.5% or less, 24% or more of the thickness T. However, if the depth DOLzero of the stress zero point E is excessively large, for example, there is a risk of excessive tensile stress being generated at a depth (point B) that is half the thickness T from the main surface 1a. Therefore, the depth DOLzero of the stress zero point E is preferably 35% or less, 34.5% or less, 34% or less, 33.5% or less, 33% or less, 32.5% or less, 32% or less, 31.5% or less, 31% or less, 30.5% or less, 30% or less, 29.5% or less, 29% or less, 28.5% or less, 28% or less, or 27% or less of the thickness T.

[0035] The integral value of the compressive stress from the main surface 1a (point A) to the zero stress point E is S CS (MPa mm), S CS / T is preferably 16.0 MPa or less. CS / T is more preferably 15.5 MPa or less, 15.0 MPa or less, 14.5 MPa or less, 14.0 MPa or less, 13.5 MPa or less, 13.0 MPa or less, 12.5 MPa or less, 12.0 MPa or less, 11.5 MPa or less, or 11.0 MPa or less.

[0036] The stress profile of the tempered glass 1 has a maximum tensile stress CT where the tensile stress exhibits a maximum absolute value at a point B corresponding to a depth half the thickness T from the main surface 1a. The absolute value of the maximum tensile stress CT is preferably 70 MPa or less, 65 MPa or less, 60 MPa or less, 40 MPa to 55 MPa, 45 MPa to 55 MPa, or 50 MPa to 55 MPa.

[0037] 3, the stress profile of the strengthened glass 1 may have a peak point F indicating a maximum value of the compressive stress between the first inflection point C and the second inflection point D. In other words, between the first inflection point C and the peak point F, the compressive stress gradually increases toward a deeper position in the depth direction, and between the peak point F and the second inflection point D, the compressive stress gradually decreases toward a deeper position in the depth direction. As a result, a hump-shaped stress peak with the peak point F as its apex is formed between the first inflection point C and the second inflection point D. The compressive stress CSp at the peak point F is preferably 15MPa to 250MPa, 15MPa to 240MPa, 15MPa to 230MPa, 15MPa to 220MPa, 15MPa to 210MPa, 15MPa to 200MPa, 15MPa to 190MPa, 15MPa to 180MPa, 15MPa to 175MPa, 15MPa to 170MPa, 15MPa to 165MPa, or 15MPa to 160MPa. The depth DOLp of the peak point F is preferably 4% to 20%, 4% to 19%, 4% to 18.5%, 4% to 18%, 4% to 17.5%, 4% to 17%, 4.5% to 17%, 5% to 17%, 6% to 17%, 7.3% to 17%, or 8% to 15% of the thickness T.

[0038] In the case of having a peak point F showing the maximum value of compressive stress, between point A (main surface) and peak point F, there is a bottom point G where the stress gradually decreases from point A in the depth direction and the stress takes a minimum value. In other words, in this case, between bottom point G and peak point F, the stress gradually increases from bottom point G in the depth direction and the stress takes a maximum value at peak point F. Although the stress CSb at bottom point G is illustrated as a compressive stress (positive value) in FIG. 3, it may also be a tensile stress (negative value). The lower the stress CSb at bottom point G, the lower the tensile stress CT, and the slower the behavior at the time of breakage. The stress CSb at bottom point G is preferably +100 MPa or less, more preferably +90 MPa or less, +80 MPa or less, +70 MPa or less, or +60 MPa or less. However, if the stress CSb at bottom point G is too low, cracks will occur on the surface during the strengthening process, deteriorating visibility. The stress CSb at the bottom point G is preferably -50 MPa or more, more preferably -45 MPa or more, -40 MPa or more, -35 MPa or more, or -30 MPa or more. The stress CSb at the bottom point G may be 0 MPa or more and +65 MPa or less, or may be -30 MPa or more and less than 0 MPa. The depth DOLb of the bottom point G is preferably 0.5% to 12% of the thickness T, more preferably 1% to 7% of the thickness T.

[0039] Here, in this embodiment, the strengthened glass 1 has a similar stress profile at the end face 1b. In other words, in the case where the compressive stress is a positive number and the tensile stress is a negative number, the compressive stress at the end face 1b is 400 MPa or more, and the stress profile obtained by measuring the stress in the depth direction (direction perpendicular to the end face 1b) from the end face 1b has an inflection point where the second derivative of the stress profile becomes zero between the end face 1b and a depth of half the thickness T, and the compressive stress at the first inflection point located closest to the end face 1b among the inflection points is 150 MPa or less, and the compressive stress at the second inflection point located deeper than the first inflection point is 45 MPa or less. The preferred range of the stress profile for the end face 1b can be similarly applied to the preferred range of the stress profile for the main surface 1a.

[0040] The stress and its distribution in the tempered glass 1 can be measured using, for example, FSM-6000LE and SLP-1000 manufactured by Orihara Manufacturing Co., Ltd., and a composite value can be used.

[0041] (Method of manufacturing tempered glass) The tempered glass 1 configured as above can be manufactured, for example, in the following manner. That is, the manufacturing method of the tempered glass 1 includes a preparation step of preparing a plate-shaped glass containing an alkali metal oxide as a composition and to be subjected to a tempering treatment (hereinafter referred to as glass to be tempered), and an ion exchange step of performing an ion exchange treatment on the glass to be tempered.

[0042] The glass to be tempered prepared in the preparation step is preferably lithium aluminosilicate glass containing, by mass %, 2% or more of Li2O and 5% or more of Na2O.

[0043] In detail, the glass to be strengthened preferably contains, for example, as a glass composition, in mass %, 40 to 70% SiO2, 10 to 30% Al2O3, 0 to 10% B2O3, 2 to 11% Li2O, 5 to 25% Na2O, 0 to 10% K2O, 0 to 6% MgO, and 50 to 20% P2O.

[0044] The above composition is preferable for the following reasons: In the explanation of the content range of each component, % indicates mass % unless otherwise specified.

[0045] SiO2 is a component that forms a glass network. If the SiO2 content is too low, vitrification becomes difficult and acid resistance is easily reduced. Therefore, the preferred lower limit range of SiO2 is 40% or more, 42% or more, 44% or more, 46% or more, 48% or more, 49% or more, 50% or more, or 51% or more. On the other hand, if the SiO2 content is too high, meltability and moldability are easily reduced, and the thermal expansion coefficient becomes too low, making it difficult to match the thermal expansion coefficient of surrounding materials. Therefore, the preferred upper limit range of SiO2 is 70% or less, 68% or less, 65% or less, 62% or less, 60% or less, 58% or less, 57% or less, or 56% or less.

[0046] Al2O3 is a component that increases the ion exchange rate, and also increases the Young's modulus and Vickers hardness. It is also a component that increases the phase separation viscosity. If the content of Al2O3 is too low, the ion exchange rate and Young's modulus tend to decrease. Therefore, the preferable lower limit range of Al2O3 is 10% or more, 11% or more, 12% or more, 13% or more, 14% or more, 14.5% or more, 15% or more, 15.5% or more, 16% or more, 16.5% or more, 17% or more, 17.5% or more, 18% or more, 18.5% or more, 19% or more, 21% or more, 22% or more, 23% or more, or 24% or more. On the other hand, if the content of Al2O3 is too high, devitrification crystals tend to precipitate in the glass, making it difficult to form the glass into a plate shape by the overflow downdraw method or the like. In particular, when an alumina refractory is used as the molded refractory and formed into a plate by the overflow down-draw method, devitrified crystals of spinel are likely to precipitate at the interface with the alumina refractory. In addition, acid resistance is also reduced, making it difficult to apply to an acid treatment process. Furthermore, high-temperature viscosity is increased, and melting property is likely to be reduced. Therefore, the preferable upper limit range of Al2O3 is 30% or less, 29% or less, or 28% or less.

[0047] B2O3 is a component that reduces high-temperature viscosity and density and increases devitrification resistance. However, if the content of B2O3 is too high, the ion exchange rate (especially the stress depth) is likely to decrease. In addition, ion exchange can cause coloring of the glass surface, known as tarnish, and can easily reduce acid resistance and water resistance. Therefore, the preferred range of B2O3 is 0% to 10%, 0% to 5%, or 0% to 1%.

[0048] Li2O is an ion exchange component, and also a component that reduces high-temperature viscosity and improves meltability and moldability. It also increases Young's modulus. The preferred lower limit of Li2O is 2% or more, 2.5% or more, or 2.8% or more, and the preferred upper limit of Li2O is 11% or less, 10% or less, 5% or less, or 4.5% or less.

[0049] Na2O is an ion exchange component, and also a component that reduces high-temperature viscosity and improves melting and moldability. Na2O is also a component that improves devitrification resistance and reaction devitrification resistance with a shaped refractory, especially an alumina refractory. If the Na2O content is too low, the melting property decreases, the thermal expansion coefficient decreases too much, and the ion exchange rate tends to decrease. Therefore, the preferable lower limit range of Na2O is 5% or more, 6% or more, or 7% or more. On the other hand, if the Na2O content is too high, the phase separation generation viscosity tends to decrease. In addition, acid resistance may decrease, and the glass composition may lack a component balance, resulting in a decrease in devitrification resistance. Therefore, the preferable upper limit range of Na2O is 25% or less, 22% or less, 20% or less, 19.5% or less, 19% or less, 18% or less, 17% or less, 16.5% or less, 16% or less, 15.5% or less, particularly 15% or less.

[0050] K2O is a component that reduces high-temperature viscosity and improves melting and moldability. It also improves devitrification resistance and increases Vickers hardness. However, if the content of K2O is too high, the phase separation viscosity is likely to decrease. In addition, acid resistance decreases and the glass composition loses its component balance, which tends to decrease devitrification resistance. Therefore, the preferred lower limit range of K2O is 0% or more, 0.01% or more, 0.02% or more, 0.1% or more, or 0.5% or more, and the preferred upper limit range is 10% or less, 5.5% or less, 5% or less, or less than 4.5%.

[0051] MgO is a component that reduces high-temperature viscosity and improves melting and moldability. It is also a component that increases Young's modulus, Vickers hardness, and acid resistance. Therefore, the preferred lower limit range of MgO is 0% or more, 0.1% or more, 0.5% or more, 1% or more, 1.5% or more, or 2% or more. However, if the content of MgO is too high, the ion exchange rate tends to decrease and the glass tends to become devitrified. In particular, when an alumina refractory is used as the molded body refractory and the glass is molded into a plate shape by the overflow downdraw method, devitrified crystals of spinel tend to precipitate at the interface with the alumina refractory. Therefore, the preferred upper limit range of MgO is 6% or less, 5.5% or less, 4.5% or less, 4% or less, 3.5% or less, 3% or less, or 2.5% or less.

[0052] P2O5 is a component that increases the ion exchange rate while maintaining the compressive stress value. Therefore, the preferred lower limit range of P2O5 is 0% or more, 2% or more, 2.1% or more, 2.5% or more, 3% or more, 4% or more, or 4.5% or more. However, if the content of P2O5 is too high, the glass may become cloudy due to phase separation, or the water resistance may be easily reduced. Therefore, the preferred upper limit range of P2O5 is 20% or less, 10% or less, or 8.5% or less.

[0053] In addition to the above components, the following components may be added:

[0054] ZnO is a component that increases the ion exchange rate, and is particularly effective in increasing the compressive stress value. It is also a component that reduces the high-temperature viscosity without reducing the low-temperature viscosity. However, if the ZnO content is too high, the glass tends to undergo phase separation, the devitrification resistance to decrease, the density to increase, and the stress depth to decrease. Therefore, the preferred ZnO content is 0-10%, 0-3%, particularly 0-7%, 0-5%, 0-3%, and 0-1%.

[0055] SnO2 has the effect of enhancing ion exchange performance, and therefore the content of SnO2 is preferably 0% to 3%, 0.01% to 3%, 0.05% to 3%, and particularly preferably 0.1% to 3%.

[0056] As a fining agent, one or more selected from the group consisting of Cl, SO3 and CeO2 (preferably Cl and SO3) may be added in an amount of 0% to 3%.

[0057] The content of Fe2O3 is preferably less than 1000 ppm (less than 0.1%), less than 800 ppm, less than 600 ppm, less than 400 ppm, and particularly preferably less than 300 ppm. In this way, the transmittance (400 nm to 770 nm) at a thickness of 1 mm is easily improved.

[0058] Rare earth oxides such as Nb2O5 and La2O3 are components that increase the Young's modulus. However, the cost of the raw materials themselves is high, and adding a large amount of them tends to reduce devitrification resistance. Therefore, the content of rare earth oxides is preferably 3% or less, 2% or less, 1% or less, 0.5% or less, and particularly preferably 0.1% or less.

[0059] From an environmental perspective, the glass to be tempered preferably does not substantially contain As2O3, Sb2O3, or PbO as a glass composition. From an environmental perspective, it also preferably does not substantially contain Bi2O3 or F.

[0060] The composition of the tempered glass described above is an example, and any tempered glass having a known composition may be used as long as it is capable of chemical tempering by ion exchange. The composition of the tempered glass obtained by subjecting the tempered glass described above to ion exchange treatment is the same as the composition of the tempered glass before the ion exchange treatment.

[0061] The above-mentioned glass to be tempered can be produced as follows.

[0062] First, glass raw materials prepared to obtain the above-mentioned glass composition are charged into a continuous melting furnace, heated and melted at 1500°C to 1600°C, and clarified. Thereafter, the glass is fed into a forming device and formed into a plate or the like, and slowly cooled to produce glass to be tempered.

[0063] As a method for forming a glass sheet, it is preferable to adopt an overflow downdraw method. The overflow downdraw method is a method that can mass-produce high-quality glass sheets and can easily produce large glass sheets, and can also reduce scratches on the surface of the glass sheet as much as possible. In the overflow downdraw method, alumina or dense zircon is used as the forming body. The glass to be strengthened according to the present invention has good compatibility with alumina and dense zircon, particularly alumina (it is unlikely to react with the forming body to generate bubbles, bumps, etc.).

[0064] In addition to the overflow downdraw method, various other forming methods can be used, such as the float method, the downdraw method (slot down method, redraw method, etc.), the roll-out method, and the press method.

[0065] After or simultaneously with forming the glass to be tempered, the glass may be subjected to bending, if necessary. In addition, the glass may be subjected to cutting, drilling, surface polishing, chamfering, edge polishing, etching, or other processes, if necessary.

[0066] The dimensions of the glass to be tempered may be determined arbitrarily, but the thickness T is preferably 2.0 mm or less, more preferably 1.0 mm or less, and further preferably 0.3 mm to 0.9 mm.

[0067] 4, in this embodiment, the ion exchange process includes a first ion exchange process (first strengthening process) T1 in which a first molten salt (first metal salt) is brought into contact with the surface of the glass to be strengthened, and a second ion exchange process (second strengthening process) T2 in which a second molten salt (second metal salt) is brought into contact with the surface of the glass to be strengthened. In each ion exchange process, the glass to be strengthened is preferably immersed in a molten salt.

[0068] In the first ion exchange step T1, the glass to be strengthened is immersed in a treatment tank filled with a first molten salt containing Na ions having a larger ionic radius than the Li ions contained in the glass to be strengthened, and is held at a predetermined temperature for a predetermined time, thereby performing an ion exchange treatment on the surface of the glass to be strengthened. This causes ion exchange between the Li ions contained in the glass to be strengthened and the Na ions contained in the first molten salt, and introduces Na ions near the surface (in this embodiment, the main surface and end faces) of the glass to be strengthened. As a result, a compressive stress layer is formed in the surface layer portion of the glass to be strengthened, and the glass to be strengthened is strengthened.

[0069] In the first ion exchange step T1, Li ions become extracted ions that are extracted from the glass to be strengthened, and Na ions become introduced ions that are introduced into the glass to be strengthened.

[0070] In the first ion exchange step T1, the region into which Na ions are introduced into the glass to be strengthened is preferably a region from the surface of the glass to be strengthened to a depth of 10% or more of the thickness T, and more preferably a region from the surface of the glass to be strengthened to a depth of 12% or more, 14% or more, 15% or more, or 15% or more and 40% or less of the thickness T.

[0071] In the second ion exchange step T2, the glass to be strengthened is immersed in a treatment tank filled with a second molten salt containing K ions, which have an ionic radius larger than that of Na ions, and Li ions, and is held at a predetermined temperature for a predetermined time, thereby performing an ion exchange treatment on the surface of the glass to be strengthened. As a result, the Li ions are reverse ion-exchanged with the Na ions contained in the glass to be strengthened, and at least a portion of the Na ions are removed from the glass to be strengthened. At the same time, the K ions are ion-exchanged with the Li ions or Na ions contained in the glass to be strengthened, and the K ions are introduced into the glass from the surface to a region shallower than 7% of the thickness T. In other words, the compressive stress formed in the surface layer of the glass to be strengthened by the reverse ion exchange is relaxed, while the glass to be strengthened by the ion exchange is strengthened, and high compressive stress is formed only in the vicinity of the surface of the surface layer.

[0072] Here, in the second ion exchange step T2, the rate of reverse ion exchange is greater than the rate of ion exchange, so that relaxation of the compressive stress in the surface layer progresses first to a deeper portion, and then compressive stress is formed again on the surface.

[0073] In the second ion exchange step T2, the region where Na ions are removed from the glass to be strengthened is preferably a region from the surface of the glass to a depth of 15% or less of the thickness T, more preferably a region from the surface of the glass to a depth of 14% or less, 13% or less, 12% or less, 11% or less, 10% or less, 1% or more and 10% or less, 2% or more and 10% or less, 3% or more and 10% or less, 4% or more and 10% or less, or 5% or more and 10% or less of the thickness T. In the second ion exchange step T2, the region where K ions are introduced into the glass to be strengthened is preferably a region from the surface of the glass to a depth of 7% or less of the thickness T, more preferably a region from the surface of the glass to be strengthened to a depth of 6.5% or less, 6% or less, 5.5% or less, or 5% or less of the thickness T.

[0074] By appropriately adjusting the treatment time and treatment temperature within the condition ranges of the first ion exchange step T1 and the second ion exchange step T2 described above, it is possible to obtain the strengthened glass 1 having the above-mentioned properties.

[0075] Here, in the first ion exchange step T1, no inflection point is formed in the stress profile of the glass to be strengthened, where the second derivative of the stress profile is zero. That is, in the second ion exchange step T2, the first inflection point C and the second inflection point D, where the second derivative of the stress profile is zero, are formed for the first time in the stress profile of the glass to be strengthened (strengthened glass 1).

[0076] The first molten salt may be a molten salt consisting of NaNO3 alone or a mixed salt mainly composed of NaNO3 and KNO3. The first molten salt may contain LiNO3. In this case, the Li2O content of the glass to be strengthened is preferably 2.5 to 5.0 mass%, more preferably 2.8 to 4.5 mass%.

[0077] The first molten salt used in the first ion exchange step T1 is preferably a mixed salt of NaNO3 and KNO3. If the first molten salt contains K ions, it is easy to measure the stress and its distribution in the glass to be tempered after the first ion exchange step T1, and this is suitable for quality control of the tempered glass obtained. The concentration of NaNO3 in the first molten salt is preferably 100 to 20%, 100 to 30%, 100 to 40%, 100 to 50%, or 100 to 60% by mass, and the remainder is preferably KNO3. The concentration of NaNO3 in the first molten salt is preferably higher than the concentration of KNO3 in the first molten salt. The first molten salt may be configured to contain only NaNO3 and not KNO3. The ion exchange treatment temperature in the first ion exchange step T1 is preferably 350 to 480°C, more preferably 360 to 430°C, and even more preferably 370 to 400°C, or 370 to 390°C. The ion exchange treatment time in the first ion exchange step T1 is preferably 1 to 20 hours, more preferably 1.5 to 15 hours, and further preferably 2 to 10 hours.

[0078] The second molten salt used in the second ion exchange step T2 is preferably a mixed salt of LiNO3 and KNO3. The concentration of LiNO3 in the second molten salt is preferably lower than the concentration of KNO3 in the second molten salt. In detail, the concentration of LiNO3 in the second molten salt is preferably 0.1 to 5%, 0.2 to 5%, 0.3 to 5%, 0.4 to 5%, 0.5 to 5%, 0.5 to 4%, 0.5 to 3%, 0.5 to 2.5%, 0.5 to 2%, or 1 to 2% by mass, and the remainder is preferably KNO3. In addition, the Li ion concentration contained in the second molten salt is preferably 100 mass ppm or more. In this case, the Li ion concentration in the second molten salt is obtained by multiplying LiNO3 expressed in mass% by 0.101. The ion exchange treatment temperature in the second ion exchange step T2 is preferably 350 to 480° C., more preferably 360 to 430° C., even more preferably 370 to 400° C., or 370 to 390° C. The ion exchange treatment time in the second ion exchange step T2 is preferably shorter than the ion exchange treatment time in the first ion exchange step T1. The ion exchange treatment time in the second ion exchange step T2 is preferably 0.2 hours or more, more preferably 0.3 to 2 hours, 0.4 to 1.5 hours, or even more preferably 0.5 to 1 hour.

[0079] After the second ion exchange step T2, various processes such as cutting, drilling, surface polishing, chamfering, end face polishing, etching, and film formation may be carried out.

[0080] Although the embodiment of the present invention has been described above, the present invention is of course not limited to this embodiment, and various other embodiments are possible within the scope of the present invention.

[0081] In the above embodiment, the case where the strengthened glass 1 has the compressive stress layer 2 on both sides of the front and back main surfaces 1a and on the end surface 1b side has been exemplified, but the compressive stress layer 2 may be provided only on a part of the surface layer of the strengthened glass 1, such as providing the compressive stress layer 2 only on one main surface 1a side. As a method for forming the compressive stress layer 2 only on a part of the surface layer of the strengthened glass 1, for example, there is a method in which an inhibitory film (e.g., a SiO2 film) that inhibits the permeation of introduced ions in the ion exchange treatment is formed in advance in an area of ​​the glass to be strengthened where the compressive stress layer is not to be formed, and the ion exchange treatment is partially performed on the part excluding the inhibitory film.

[0082] In the above embodiment, a method for manufacturing the tempered glass 1 by performing two ion exchange steps on the glass to be strengthened has been exemplified, but the method for manufacturing the tempered glass 1 is not limited thereto. For example, the glass to be strengthened may be subjected to three or more ion exchange steps, or the glass to be strengthened may be subjected to two ion exchange steps and a heat treatment step. In the latter case, the heat treatment step is preferably performed between the first ion exchange step and the second ion exchange step in order to relieve the compressive stress of the glass to be strengthened.

[0083] In the above embodiment, the tempered glass 1 is in the form of a flat plate, but the concept of a plate in the present invention also includes a bent plate shape having a curved surface.

[0084] The present application includes the following inventions.

[0085] (1) A tempered glass having a surface and a thickness T, characterized in that, when compressive stress is a positive number and tensile stress is a negative number, the compressive stress at the surface is 400 MPa or more, a stress profile obtained by measuring stress in a depth direction from the surface has an inflection point at which a second derivative of the stress profile is zero between the surface and a depth that is half the thickness T, and the compressive stress at a first inflection point that is closest to the surface is 150 MPa or less.

[0086] (2) In the above configuration (1), it is preferable that the second inflection point is located deeper than the first inflection point.

[0087] According to such a configuration, a stress profile is obtained in which a rapid attenuation of the compressive stress beyond the first inflection point is suppressed, and the tempered glass of the present invention can obtain higher impact resistance.

[0088] (3) In the above configuration (2), the compressive stress at the second inflection point is preferably 45 MPa or less.

[0089] According to this configuration, the compressive stress value at the second inflection point is suppressed, thereby reducing the tensile stress value, and the tempered glass of the present invention can obtain higher impact resistance.

[0090] (4) In the above configuration (2) or (3), when the stress at the first inflection point is σ1, the depth from the surface of the first inflection point is d1, the stress at the second inflection point is σ2, and the depth from the surface of the second inflection point is d2, it is preferable that (σ1-σ2) / (d1-d2) is -1.0 MPa / μm or more.

[0091] According to such a configuration, the second inflection point is located relatively deep, resulting in a stress profile in which abrupt attenuation of compressive stress is suppressed, and the tempered glass of the present invention can obtain higher impact resistance.

[0092] (5) In any one of the above configurations (2) to (4), the depth of the first inflection point from the surface is preferably 50 μm or less.

[0093] According to such a configuration, the stress profile has a compressive stress that decreases rapidly from the surface to the first inflection point, and the tensile stress value is reduced, thereby obtaining higher impact resistance.

[0094] (6) In any one of the above configurations (2) to (5), the second inflection point is preferably located at a depth from the surface of 60 μm or deeper.

[0095] According to such a configuration, the second inflection point is located relatively deep, resulting in a stress profile in which abrupt attenuation of compressive stress is suppressed, and the tempered glass of the present invention can obtain higher impact resistance.

[0096] (7) In any of the above configurations (1) to (6), it is preferable that the stress profile has a zero stress point where the stress is zero, and that the zero stress point is located at a position deeper than 12% of the thickness T from the surface.

[0097] According to such a configuration, a compressive stress layer is formed from the surface to a relatively deep position, so that the tempered glass of the present invention can obtain higher impact resistance.

[0098] (8) In the above configuration (7), the integral value of the compressive stress from the surface to the zero stress point is S CS (MPa mm), S CS It is preferable that / T is 16.0 MPa or less.

[0099] According to this configuration, the integral value of the compressive stress is suppressed to be small, thereby reducing the tensile stress value, and thus the tempered glass of the present invention can obtain higher impact resistance.

[0100] (9) In any one of the above configurations (1) to (8), the maximum absolute value of the tensile stress is preferably 70 MPa or less.

[0101] (10) In any of the above configurations (1) to (9), it is preferable that the thickness T is within the range of 0.3 mm or more and 1.0 mm or less, and that the main surfaces and end faces have the above stress profile.

[0102] (11) In any of the configurations (1) to (10) above, it is preferable that the thickness T is within the range of 0.45 mm or more and 0.85 mm or less, the maximum value of the compressive stress at the surface is within the range of 700 MPa or more and 850 MPa or less, the maximum absolute value of the tensile stress is within the range of 42 MPa or more and 65 MPa or less, the stress profile has a zero stress point where the stress is zero, the zero stress point is located at a position within the range of 17% to 25% of the thickness T from the surface, and the compressive stress at the first inflection point is within the range of 30 MPa or more and 80 MPa or less.

[0103] (12) In any of the above configurations (1) to (11), the glass composition preferably contains, by mass, 40 to 70% SiO2, 10 to 30% Al2O3, 0 to 10% B2O3, 2 to 11% Li2O, 5 to 25% Na2O, 0 to 10% K2O, 0 to 6% MgO, and 50 to 20% P2O.

[0104] (13) A method for producing tempered glass having a surface and a thickness T, comprising: a first ion exchange step of contacting tempered glass containing LiO and NaO with a first molten salt containing Na ions to introduce the Na ions into the glass to be tempered; and a second ion exchange step of contacting the glass to be tempered with a second molten salt containing Li ions and K ions after the first ion exchange step to remove at least a portion of the Na ions from the glass to be tempered and introduce K ions into the glass to be tempered, characterized in that the first ion exchange step and the second ion exchange step are performed so that a stress profile obtained by measuring stress in a depth direction from the surface, with compressive stress being a positive number and tensile stress being a negative number, has an inflection point where a second derivative of the stress profile becomes zero between the surface and a depth that is half the thickness T.

[0105] According to this configuration, the tempered glass of the present invention having a complicated stress profile can be obtained with a small number of steps.

[0106] (14) In the above configuration (13), it is preferable that an inflection point is formed in the second ion exchange step. EXAMPLES

[0107] The tempered glass according to the present invention will be described below based on examples. Note that the following examples are merely illustrative, and the present invention is not limited to the following examples in any way.

[0108] The samples were prepared as follows: First, tempered glass having the composition shown in Table 1 was prepared.

[0109] [Table 1]

[0110] Glass raw materials were mixed according to the composition in Table 1 and melted in a platinum pot at 1600°C for 21 hours. The resulting molten glass was then formed into a plate having a thickness of 0.7 mm by flow-down-draw molding through a refractory molding.

[0111] Next, the above glass to be tempered was immersed in a molten salt bath under the conditions shown in Table 2 to perform a total of two ion exchange processes, a first ion exchange process (tempering process) and a second ion exchange process (tempering process), to obtain a plate-shaped tempered glass. Samples Nos. 1 to 7 are examples of the present invention, and Sample No. 8 is a comparative example.

[0112] The tempered glass thus obtained was subjected to various measurements of properties and strength tests as described below, and the results are shown in Table 2.

[0113] [Table 2]

[0114] First, the stress profile of each sample was measured using a surface stress meter FSM-6000LE and SLP-1000 manufactured by Orihara Seisakusho. The measurement results were synthesized using the data synthesis function provided in advance in the above-mentioned device to obtain a phase difference profile. The application range of each data in the synthesis was set to 10 μm from the surface for FSM-6000LE and 30 μm from the surface for SLP-1000. From the obtained phase difference profile, the stress profile was obtained through the analysis described below. First, the initial values ​​shown in the table below were set, and the following formula R(x) was calculated at each depth x of the obtained phase difference profile. Here, Δ=0.01 [μm]. The sum of squared differences between that R(x) and the obtained phase difference profile was calculated, and various variables A1, A2, A3, B1, B2, B3, and C1 were determined so that the sum of squared differences was minimized. More specifically, the solution was performed using the "GRG nonlinear" solver function of Excel, and the ranges and constraints for various variables were given according to the table below to perform approximation. This approximation calculation was repeated until the correlation coefficient between R(x) and the phase difference profile exceeded 0.9995. If the correlation coefficient did not reach 0.9995, multiple measurements were performed, and the averaged measurement data was used for analysis. The following formula σ(x) expressed using the various variables obtained as described above was used as the stress profile. The photoelastic constant C [nm / cm / MPa] was measured using the optical heterodyne interferometry, more specifically, using PEL-3A-XR manufactured by Uniopto Co., Ltd. The instrument constant k is a constant calculated by inputting the refractive index into the SLP-1000, and more specifically, the value obtained by dividing the kDP value described in the measurement result file by the stress calibration coefficient. The refractive index was measured using the V-block method, more specifically, using KPR-2000 manufactured by Shimadzu Corporation.

number

number

[0115] Examples of the measured stress profiles are shown in Figures 5 and 6. Figure 5 is a graph showing the stress profile in the thickness direction of the tempered glass of sample No. 4, and Figure 6 is a graph showing the stress profile in the thickness direction of the tempered glass of sample No. 6. In Figures 5 and 6, the horizontal axis indicates the depth (μm) from one main surface, and the vertical axis indicates the magnitude of stress (MPa). In Figures 5 and 6, compressive stress is indicated by a positive value, and tensile stress is indicated by a negative value.

[0116] Based on the stress profile measured as described above, the properties shown in Table 2 were calculated. The inflection point was defined as the point where the second derivative of the above σ(x) becomes 0, and the first inflection point and the second inflection point were defined in order from the point closest to the surface, but the surface x=0, which is a discontinuous point, is not considered to be an inflection point. Samples No. 2, 3, and 6 according to the embodiment have a compressive stress maximum value CSp (hump-shaped stress peak) between the first inflection point and the second inflection point, while the other samples according to the embodiment do not have a compressive stress maximum value between the first inflection point and the second inflection point. Sample No. 8, which is a comparative example, does not have an inflection point either.

[0117] In Table 2, CSmax indicates the maximum value of compressive stress in the compressive stress layer. DOLzero indicates the depth from the main surface to the zero stress point E. CT indicates the maximum absolute value of tensile stress in the tensile stress layer. CSp indicates the stress (maximum value) at the peak point F formed between the first inflection point C and the second inflection point D, and DOLp indicates the depth from the main surface to the peak point F. CSb indicates the stress (minimum value) at the bottom point G formed between the main surface and the peak point F, and DOLb indicates the depth from the main surface to the bottom point G. Scs indicates the integral value of the compressive stress from the main surface to the zero stress point E. d1 indicates the depth from the main surface to the first inflection point C. σ1 indicates the stress at the first inflection point C. d2 indicates the depth from the main surface to the second inflection point D. σ2 indicates the stress at the second inflection point D.

[0118] Here, all of the examples (samples No. 1 to No. 7) have a first inflection point C and a second inflection point D, but as shown in Figure 7, no inflection points are formed in the stress profiles of samples No. 1 to 3 after the first ion exchange process. Similarly, as shown in Figure 8, no inflection points are formed in the stress profiles of samples No. 4 to 7 after the first ion exchange process. This also shows that the inflection points in the stress profiles of all of the examples (samples No. 1 to No. 7) are formed in the second ion exchange process.

[0119] The pseudo housing drop strength indicates the height at which the glass sample 20 breaks when the pseudo housing 10, the glass sample 20 made of the tempered glass 1, and the sandpaper 30 are layered in this order and dropped onto an iron platen 40 as shown in FIG. 9. Specifically, the pseudo housing 10 is attached to one main surface of the glass sample 20, which is processed to have a width of 65 mm, a length of 130 mm, and a thickness T shown in Table 1. The pseudo housing 10 is a polycarbonate thick plate member simulating a mobile terminal, with a width of 70 mm, a length of 140 mm, a thickness of 8 mm, and a mass of 110 g. The pseudo housing 10 and the glass sample 20 are bonded together by sandwiching an optical adhesive film 50 having a thickness of 150 μm between them.

[0120] Next, the sandpaper 30 is attached to the other main surface of the glass sample 20 (the main surface opposite to the main surface bonded to the pseudo housing) so that the surface of the sandpaper 30 (the surface on which the abrasive is provided) abuts against the other main surface of the glass sample 20. The sandpaper 30 has dimensions of 60 mm in width and 120 mm in length, and is placed in the center of the other main surface of the glass sample 20. At this time, the peripheral portion of the glass sample 20 is placed so as to protrude beyond the sandpaper 30. The sandpaper 30 is attached to the glass sample 20 by attaching the protruding peripheral portion of the back surface (the surface on which the abrasive is not provided) of the glass sample 20 and the end of the sandpaper 30 at multiple locations with multiple pieces of vinyl tape 60. The vinyl tape pieces 60 are 19 mm in width, 10 mm in length, and 0.1 mm in thickness, and are attached to the center of each short side of the sandpaper 30. As the sandpaper 30, Riken Corundum SiC sandpaper P180, P120, P100, and P80 having different abrasive grain coarseness (grit) were used, and the drop strength of a simulated housing was measured for each case.

[0121] The test specimen thus obtained was held in a horizontal position with the sandpaper 30 facing downward, and was repeatedly dropped toward the platen 40 while increasing the drop height until the glass sample 20 was broken. More specifically, in this application, the test specimen was clamped by a clamping means consisting of an air cylinder, dropped together with the clamping means, and the clamping by the air cylinder was released at a position 20 cm in front of the platen 40, so that the test specimen was dropped toward the platen 40 while maintaining the horizontal position. The sandpaper 30 was replaced with a new one after each drop test. The drop height was set to a height of 20 cm from the drop surface, and if the glass sample 20 was not broken, the drop height was increased by 10 cm.

[0122] It was confirmed that all of the examples (samples No. 1 to No. 7) for which the pseudo-housing drop strength was measured had a higher pseudo-housing drop strength than the comparative example (sample No. 8), and thus had high impact resistance. [Industrial Applicability]

[0123] The tempered glass of the present invention can be used as a component part of, for example, a mobile phone (particularly a smartphone), a tablet computer, a digital camera, a touch panel display, a large television, and the like. [Explanation of symbols]

[0124] 1. Tempered glass 2. Compressive stress layer 3 Tensile stress layer 10 Pseudo-Chassis 20 Glass sample (tempered glass) 30 Sandpaper 40 Fixed Plate 50 Optical adhesive film 60 Vinyl tape strip C 1st inflection point D 2nd inflection point

Claims

1. A tempered glass having a surface and a thickness T, The thickness T is greater than 0.3 mm; When compressive stress is a positive number and tensile stress is a negative number, the maximum value of the compressive stress on the surface is 661 MPa or more; a stress profile obtained by measuring stress in a depth direction from the surface has an inflection point at which a second derivative of the stress profile becomes zero between the surface and a depth half the thickness T; The stress profile has a zero stress point where the stress is zero, and the zero stress point exists at a position deeper than 17% of the thickness T from the surface; The depth from the surface of a first inflection point that is closest to the surface among the inflection points is 50 μm or less; The compressive stress at the first inflection point is 40 MPa or more. The tempered glass is characterized by

2. The tempered glass according to claim 1 , wherein the compressive stress at the first inflection point is 150 MPa or less.

3. A tempered glass having a surface and a thickness T, The thickness T is greater than 0.3 mm; When compressive stress is a positive number and tensile stress is a negative number, the maximum value of the compressive stress on the surface is 661 MPa or more; a stress profile obtained by measuring stress in a depth direction from the surface has an inflection point at which a second derivative of the stress profile becomes zero between the surface and a depth half the thickness T; The stress profile has a zero stress point where the stress is zero, and the zero stress point exists at a position deeper than 17% of the thickness T from the surface; The depth from the surface of a first inflection point that is closest to the surface among the inflection points is 50 μm or less; The compressive stress at the first inflection point is 150 MPa or less. The tempered glass is characterized by

4. The tempered glass according to any one of claims 1 to 3, wherein a maximum value of compressive stress on the surface is 750 MPa or more.

5. As a glass composition, Li 2 The tempered glass according to any one of claims 1 to 4, which contains O.

6. The glass composition is, in mass%, SiO 2 40-70%, Al 2 O 3 10-30%, B 2 O 3 0-10%, Li 2 O 2-11%, Na 2 O 5-25%, K 2 O 0-10%, MgO 0-6%, P 2 O 5 The tempered glass according to claim 5, containing 0 to 20%.

7. The tempered glass according to any one of claims 1 to 6, wherein a second inflection point is present at a position deeper than the first inflection point.

8. The tempered glass according to claim 7 , wherein the second inflection point has a depth from the surface of 60 μm or more.

9. When the stress at the first inflection point is σ1, the depth of the first inflection point from the surface is d1, the stress at the second inflection point is σ2, and the depth of the second inflection point from the surface is d2, (σ1-σ2) / (d1-d2) is -1.0 MPa / μm or more. The tempered glass according to claim 7 or 8.

10. The tempered glass according to any one of claims 7 to 9, wherein the compressive stress at the second inflection point is 45 MPa or less.

11. A tempered glass having a surface and a thickness T, The thickness T is greater than 0.3 mm; When compressive stress is a positive number and tensile stress is a negative number, the maximum value of the compressive stress on the surface is 661 MPa or more; a stress profile obtained by measuring stress in a depth direction from the surface has an inflection point at which a second derivative of the stress profile becomes zero between the surface and a depth half the thickness T; The stress profile has a zero stress point where the stress is zero, and the zero stress point exists at a position deeper than 17% of the thickness T from the surface; The depth from the surface of a first inflection point that is closest to the surface among the inflection points is 50 μm or less; A second inflection point is present at a position deeper than the first inflection point, When the stress at the first inflection point is σ1, the depth of the first inflection point from the surface is d1, the stress at the second inflection point is σ2, and the depth of the second inflection point from the surface is d2, (σ1-σ2) / (d1-d2) is -1.0 MPa / μm or more. The tempered glass is characterized by

12. The tempered glass of claim 11, wherein the compressive stress at the second inflection point is 45 MPa or less.

13. A tempered glass having a surface and a thickness T, The thickness T is greater than 0.3 mm; When compressive stress is a positive number and tensile stress is a negative number, the maximum value of the compressive stress on the surface is 661 MPa or more; a stress profile obtained by measuring stress in a depth direction from the surface has an inflection point at which a second derivative of the stress profile becomes zero between the surface and a depth half the thickness T; The stress profile has a zero stress point where the stress is zero, and the zero stress point exists at a position deeper than 17% of the thickness T from the surface; The depth from the surface of a first inflection point that is closest to the surface among the inflection points is 50 μm or less; A second inflection point is present at a position deeper than the first inflection point, The compressive stress at the second inflection point is 45 MPa or less. The tempered glass is characterized by

14. The tempered glass according to any one of claims 11 to 13, wherein the depth of the second inflection point from the surface is 60 μm or more.

Citation Information

Patent Citations

  • Ion exchange glass with non-error function compressive stress profile

    JP2015511573A

  • Display cover glass and display cover glass fabrication method

    WO2013088856A1

  • Ultra-thin, non-frangible glass and methods of making

    WO2017123596A1

  • Glass-based articles including a stress profile comprising two regions, and methods of making

    WO2017177109A1