Polymer Composition

The polymer composition addresses the challenge of achieving low hardness and resistance to compression set by incorporating specific crosslinking sites in maleic anhydride graft-modified thermoplastic polymers, ensuring non-stickiness and flexibility for applications like human-touch interfaces.

JP7565164B2Active Publication Date: 2024-10-10ENEOS MATERIALS CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020079271
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-28
Publication Date
2024-10-10
Estimated Expiration
2040-04-28

AI Technical Summary

Technical Problem

Existing polymer compositions struggle to achieve both low hardness and resistance to compression set without being sticky, as exemplified by the limitations in International Publication No. 2020/027109.

Method used

A polymer composition is developed with specific side chains containing hydrogen-bonding and covalent crosslinking sites, using maleic anhydride graft-modified thermoplastic polymers and crosslinking agents, with controlled glass transition points and maleation rates to achieve non-sticky, low hardness, and reduced compression set.

Benefits of technology

The composition effectively achieves low hardness and resistance to compression set, maintaining flexibility and non-stickiness, suitable for applications requiring a soft tactile sensation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a polymer composition which has no stickiness and, moreover, can sufficiently lower both of a hardness value and a value of permanent compression set.SOLUTION: Provided is a polymer composition, comprising at least one polymer component selected from the group consisting of polymer (A) having a side chain (a) containing a hydrogen bonding cross-linking site with a carbonyl-containing group and / or a nitrogen heterocycle and having a glass transition temperature of 25°C or lower, and polymer (B) having a side chain containing a hydrogen bonding cross-linking site and a covalent bonding cross-linking site and having a glass transition temperature of 25°C or lower. Both of the polymer (A) and the polymer (B) are each a reaction product of a thermoplastic polymer graft-modified with maleic anhydride and a cross-linking agent, having a melting point of 64°C or lower and a degree of maleation of 0.1 to 3.0 mass% and have a type A durometer hardness of 0 to 49 as measured at a temperature condition of 20±5°C according to JIS K6253-3:2012.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polymer composition. [Background technology]

[0002] Conventionally, various polymer compositions have been studied to exhibit properties according to applications. For example, International Publication No. 2020 / 027109 (Patent Document 1) discloses a resin composition containing at least one resin component selected from the group consisting of a resin (A) having a side chain (a) containing a hydrogen-bond crosslinkable moiety having a carbonyl-containing group and / or a nitrogen-containing heterocycle and having a glass transition point of 25 ° C. or less, and a resin (B) having a hydrogen-bond crosslinkable moiety and a covalent crosslinking moiety in the side chain and having a glass transition point of 25 ° C. or less, and wherein both the resin (A) and the resin (B) have a melting point of 68 ° C. to 134 ° C. and a maleic anhydride-modified thermoplastic resin having a maleinization rate of 0.5 to 2.5 mass% and a crosslinking agent. Such a resin composition described in Patent Document 1 makes it possible to achieve both of the two properties, resistance to compression set and fluidity, with sufficient excellence. However, even in the resin composition described in Patent Document 1, there is still room for improvement in terms of being non-sticky, having a sufficiently low hardness, and having sufficiently excellent resistance to compression set (making both the hardness value and the compression set value sufficiently low). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2020 / 027109 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made in consideration of the problems associated with the prior art, and has an object to provide a polymer composition which is non-sticky and capable of sufficiently reducing both the hardness and compression set. [Means for solving the problem]

[0005] As a result of intensive research to achieve the above object, the present inventors have found that a polymer composition containing at least one polymer component selected from the group consisting of a polymer (A) having a side chain (a) containing a hydrogen-bond cross-linkable moiety having a carbonyl-containing group and / or a nitrogen-containing heterocycle and having a glass transition point of 25°C or less, and a polymer (B) containing a hydrogen-bond cross-linkable moiety and a covalent cross-linking moiety in a side chain and having a glass transition point of 25°C or less, and both of the polymers (A) and (B) being reaction products of a maleic anhydride graft-modified thermoplastic polymer having a melting point of 64°C or less and a maleinization rate of 0.1 to 3.0 mass% and a cross-linking agent, and that the type A durometer hardness measured under a temperature condition of 20±5°C in accordance with JIS K6253-3:2012 is 0 to 49, thereby making it possible to obtain a polymer composition that is not sticky and has sufficiently low hardness and compression set, thereby completing the present invention.

[0006] That is, the polymer composition of the present invention is At least one polymer component selected from the group consisting of a polymer (A) having a side chain (a) containing a hydrogen-bond cross-linkable moiety having a carbonyl-containing group and / or a nitrogen-containing heterocycle and having a glass transition point of 25° C. or lower, and a polymer (B) having a side chain containing a hydrogen-bond cross-linkable moiety and a covalent-bond cross-linking moiety and having a glass transition point of 25° C. or lower. and, At least one plasticizer selected from the group consisting of polybutene having no chemically bonded cross-linking sites and polyisobutylene having no chemically bonded cross-linking sites; Contains Both of the polymer (A) and the polymer (B) are reaction products of a maleic anhydride grafted thermoplastic polymer having a melting point of 64° C. or less and a maleation rate of 0.1 to 3.0% by mass with a crosslinking agent, and Type A durometer hardness measured under temperature conditions of 20±5℃ in accordance with JIS K6253-3:2012 0, and the type E durometer hardness measured under a temperature condition of 20±5°C in accordance with JIS K6253-3:2012 is 15 or less. The present invention is characterized by the following:

[0007] In the polymer composition of the present invention, the maleic acid content is preferably 0.1 to 0.9% by mass. In the polymer composition of the present invention, the crosslinking agent is preferably a compound having at least one of a hydroxyl group, an amino group, an imino group, and a thiol group.

[0008] In the polymer composition of the present invention, the maleic anhydride graft-modified thermoplastic polymer is preferably a polyolefin polymer graft-modified with maleic anhydride. The maleic anhydride graft-modified polyolefin polymer is preferably at least one polyolefin polymer selected from the group consisting of polypropylene, polyethylene, ethylene-butene copolymer, ethylene-propylene copolymer, ethylene-octene copolymer, and ethylene-propylene-diene copolymer graft-modified with maleic anhydride.

[0009] The polymer composition of the present invention preferably further contains clay. The polymer composition of the present invention preferably further contains a styrene block copolymer having no chemically bonded cross-linking site. 。 Effect of the Invention

[0010] According to the present invention, it is possible to provide a polymer composition which is non-sticky and capable of achieving sufficiently low values ​​of both hardness and compression set. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below based on preferred embodiments thereof.

[0012] The polymer composition of the present invention contains at least one polymer component selected from the group consisting of the polymer (A) and the polymer (B), and each of the polymer (A) and the polymer (B) is a reaction product of a maleic anhydride grafted thermoplastic polymer having a melting point of 64°C or less and a maleation rate of 0.1 to 3.0 mass% with a crosslinking agent, and is characterized in that the type A durometer hardness measured under a temperature condition of 20±5°C in accordance with JIS K6253-3:2012 is 0 to 49.

[0013] The polymer component according to the present invention comprises at least one polymer selected from the group consisting of a polymer (A) having a side chain (a) containing a hydrogen-bond crosslinkable moiety having a carbonyl-containing group and / or a nitrogen-containing heterocycle and having a glass transition point of 25°C or less, and a polymer (B) having a side chain containing a hydrogen-bond crosslinkable moiety and a covalent crosslinking moiety and having a glass transition point of 25°C or less. In such polymers (A) to (B), the "side chain" refers to the side chain and end of the polymer. In addition, the "side chain (a) containing a hydrogen-bond crosslinkable moiety having a carbonyl-containing group and / or a nitrogen-containing heterocycle" means that the carbonyl-containing group and / or the nitrogen-containing heterocycle (more preferably the carbonyl-containing group and the nitrogen-containing heterocycle) as the hydrogen-bond crosslinkable moiety is chemically stablely bonded (covalently bonded) to an atom (usually a carbon atom) forming the main chain of the polymer. In addition, the phrase "the side chain contains a hydrogen-bond cross-linkable moiety and a covalent-bond cross-linking moiety" refers to a concept including a case where both a side chain having a hydrogen-bond cross-linkable moiety (hereinafter, for convenience, sometimes referred to as "side chain (a')") and a side chain having a covalent-bond cross-linking moiety (hereinafter, for convenience, sometimes referred to as "side chain (b)") are contained in the side chain of the polymer, thereby containing both a hydrogen-bond cross-linkable moiety and a covalent-bond cross-linking moiety, as well as a case where a side chain having both a hydrogen-bond cross-linkable moiety and a covalent-bond cross-linking moiety (a side chain containing both a hydrogen-bond cross-linkable moiety and a covalent-bond cross-linking moiety in one side chain: hereinafter, such a side chain is referred to as "side chain (c)" for convenience, as the case may be).

[0014] As such a polymer component, from the viewpoint of achieving a lower hardness, at least one selected from the group consisting of polymers (B) which contain a hydrogen-bond cross-linkable moiety and a covalent-bond cross-linking moiety in their side chains and have a glass transition point of 25°C or lower is more preferable.

[0015] The main chains (types of polymers forming the main chain portion) of the polymers (A) to (B) in such polymer components are derived from the main chain of the maleic anhydride graft-modified thermoplastic polymer, since the polymers (A) to (B) are reaction products of the maleic anhydride graft-modified thermoplastic polymer and a crosslinking agent. The thermoplastic polymer forming the main chain portion of the polymers (A) to (B) (main chain of the maleic anhydride graft-modified thermoplastic polymer) will be described later.

[0016] Moreover, the glass transition points of all of these polymers (A) to (B) are 25° C. or lower, as described above. In the present invention, the "glass transition point" is a glass transition point measured by differential scanning calorimetry (DSC). The measurement is performed at a temperature rise rate of 10° C. / min. By setting the glass transition point of such a polymer to 25° C. or lower, it is possible to impart flexibility in a normal use temperature range (room temperature (25° C.) or higher).

[0017] As described above, the polymers (A) and (B) have at least one of the following side chains: a side chain (a) containing a hydrogen-bond cross-linkable moiety having a carbonyl-containing group and / or a nitrogen-containing heterocycle; a side chain (a') containing a hydrogen-bond cross-linkable moiety and a covalent-bond cross-linking moiety (b); and a side chain (c) containing a hydrogen-bond cross-linkable moiety and a covalent-bond cross-linking moiety. In the present invention, the side chain (c) can be said to be a side chain that functions as both the side chain (a') and the side chain (b). Each side chain will be described below.

[0018] <Side chain (a'): Side chain containing a hydrogen-bond cross-linking moiety> The side chain (a') containing such a hydrogen-bond cross-linking moiety has a group capable of forming a cross-link by hydrogen bonding (for example, a hydroxyl group, a hydrogen-bond cross-linking moiety contained in the side chain (a) described later, etc.), and may be a side chain that forms a hydrogen bond based on the group, and its structure is not particularly limited. Here, the hydrogen-bond cross-linking moiety is a moiety that cross-links the molecules of the polymer by hydrogen bonding. Note that a cross-link by hydrogen bonding is formed only when there is a hydrogen acceptor (a group containing an atom containing a lone electron pair, etc.) and a hydrogen donor (a group having a hydrogen atom covalently bonded to an atom with a large electronegativity, etc.). Therefore, a cross-link by hydrogen bonding is not formed when there is neither a hydrogen acceptor nor a hydrogen donor between the side chains of the polymer molecules. Therefore, only when there is both a hydrogen acceptor and a hydrogen donor between the side chains of the polymer molecules, a hydrogen-bond cross-linking moiety is present in the system. In the present invention, when a moiety capable of functioning as a hydrogen acceptor (e.g., a carbonyl group) and a moiety capable of functioning as a hydrogen donor (e.g., a hydroxyl group) are both present between side chains of polymer molecules, the moiety capable of functioning as a hydrogen acceptor and the moiety capable of functioning as a hydrogen donor in the side chain can be determined to be a hydrogen-bond cross-linkable site.

[0019] From the viewpoint of forming stronger hydrogen bonds, the hydrogen-bond cross-linkable moiety in the side chain (a') is more preferably the side chain (a) described below. From the same viewpoint, the hydrogen-bond cross-linkable moiety in the side chain (a') is more preferably a hydrogen-bond cross-linkable moiety having a carbonyl-containing group and a nitrogen-containing heterocycle.

[0020] <Side Chain (a): Side Chain Containing a Hydrogen-Bond Cross-Linking Moiety Having a Carbonyl-Containing Group and / or a Nitrogen-Containing Heterocycle> The side chain (a) containing a hydrogen-bond cross-linkable moiety having a carbonyl-containing group and / or a nitrogen-containing heterocycle is not particularly limited as long as it has a carbonyl-containing group and / or a nitrogen-containing heterocycle. As such a hydrogen-bond cross-linkable moiety, one having a carbonyl-containing group and a nitrogen-containing heterocycle is more preferable.

[0021] Such a carbonyl-containing group is not particularly limited as long as it contains a carbonyl group, and specific examples thereof include amide, ester, imide, carboxyl, carbonyl, thioester, acid anhydride, etc. In the present invention, both polymers (A) and (B) are reaction products of a maleic anhydride graft-modified thermoplastic polymer and a crosslinking agent, and therefore have a group derived from the "maleic anhydride group" of the maleic anhydride graft-modified thermoplastic polymer (for example, an ester group, a carbonyl group, an amide group, an imide group, a carboxyl group, an acid anhydride group, etc., depending on the type of crosslinking agent reacted).

[0022] In addition, when the side chain (a) has a nitrogen-containing heterocycle, the nitrogen-containing heterocycle may be introduced directly or via an organic group into the side chain (a), and the structure thereof is not particularly limited. Such a nitrogen-containing heterocycle may have a heteroatom other than a nitrogen atom, such as a sulfur atom, an oxygen atom, or a phosphorus atom, in the heterocycle, as long as the heterocycle contains a nitrogen atom. Such a nitrogen-containing heterocycle may have a substituent. Here, when a nitrogen-containing heterocycle is used in the side chain (a), the hydrogen bond forming the crosslink due to the heterocycle structure becomes stronger, and the stretchability and impact resistance of the polymer composition are further improved, which is preferable. In addition, such a nitrogen-containing heterocycle is preferably a 5-membered ring and / or a 6-membered ring from the viewpoint of strengthening the hydrogen bond and further improving the resistance to compression set and mechanical strength. In addition, such a nitrogen-containing heterocycle may be a nitrogen-containing heterocycle condensed with a benzene ring, or a nitrogen-containing heterocycle condensed with another nitrogen-containing heterocycle. As such a nitrogen-containing heterocycle, known ones (for example, those described in paragraphs

[0054] to

[0067] of Japanese Patent No. 5918878, those described in paragraphs

[0035] to

[0048] of Japanese Patent Publication No. 2017-206604, etc.) can be appropriately used. In addition, such a nitrogen-containing heterocycle may have a substituent. As such a nitrogen-containing heterocycle, for example, , Pi Rolidone, Oxindole (2-Oxindole), Indoxyl (3-Oxindole), Dioxindole, Isatin ,centre Thalimidine, β-isoindigo, monoporphyrin, diporphyrin, triporphyrin, azaporphyrin, phthalocyanine, hemoglobin, uroporphyrin, chlorophyll, phylloerythrin, imidazole, pyrazole, triazole, tetrazole, benzimidazole, benzopyrazole, benzotriazole, imidazoline, imidazolone, imidazolidone, hydantoin, pyrazoline, pyrazolone, pyrazolidone, indazole, pyridoindole, purine, cinnoline, pyrrole, pyrroline, indole, indoline ,mosquitoExamples of the arylamines include carbazole, phenothiazine, indolenine, isoindole, oxazole, thiazole, isoxazole, isothiazole, oxadiazole, thiadiazole, oxatriazole, thiatriazole, phenanthroline, oxazine, benzoxazine, phthalazine, pteridine, pyrazine, phenazine, tetrazine, benzoxazole, benzisoxazole, anthranil, benzothiazole, benzofurazan, pyridine, quinoline, isoquinoline, acridine, phenanthridine, anthrazoline, naphthyridine, thiazine, pyridazine, pyrimidine, quinazoline, quinoxaline, triazine, histidine, triazolidine, melamine, adenine, guanine, thymine, cytosine, hydroxyethyl isocyanurate, and derivatives thereof.

[0023] From the viewpoint of excellent recyclability, compression set, hardness, and mechanical strength (particularly tensile strength), such a nitrogen-containing heterocycle is preferably at least one selected from a triazole ring, an isocyanurate ring, a thiadiazole ring, a pyridine ring, an imidazole ring, a triazine ring, and a hydantoin ring, each of which may have a substituent, and more preferably at least one selected from a triazole ring, a thiadiazole ring, a pyridine ring, an imidazole ring, and a hydantoin ring, each of which may have a substituent.

[0024] Examples of the substituent that may be possessed by such a nitrogen-containing heterocycle include a hydroxyl group, an amino group, an imino group, a carboxy group, an isocyanate group, an epoxy group, an alkoxysilyl group, and a thiol group (mercapto group). Examples of such a substituent include alkyl groups such as a methyl group, an ethyl group, an (iso)propyl group, and a hexyl group; alkoxy groups such as a methoxy group, an ethoxy group, and a (iso)propoxy group; groups consisting of halogen atoms such as a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom; a cyano group; an amino group; an imino group; an aromatic hydrocarbon group; an ester group; an ether group; an acyl group; a thioether group; and the like. The substitution positions of these substituents are not particularly limited, and the number of the substituents is also not limited.

[0025] In addition, when both the carbonyl-containing group and the nitrogen-containing heterocycle are included in the side chain (a), the carbonyl-containing group and the nitrogen-containing heterocycle may be introduced into the main chain as independent side chains, but it is preferable that the carbonyl-containing group and the nitrogen-containing heterocycle are introduced into the main chain as one side chain in which they are bonded via different groups.The structure of such a side chain (a) may be, for example, the structure described in paragraphs

[0068] to

[0081] of Japanese Patent No. 5918878.

[0026] Moreover, such a side chain (a) is formed by the reaction of the maleic anhydride graft-modified thermoplastic polymer with a crosslinking agent. As a crosslinking agent used in forming such a side chain (a), a compound capable of reacting with a maleic anhydride group to form a hydrogen-bond crosslinking site (hereinafter, sometimes simply referred to as a "compound forming a hydrogen-bond crosslinking site") can be suitably used. As a "compound forming a hydrogen-bond crosslinking site" that can be used as such a crosslinking agent, a compound capable of introducing a nitrogen-containing heterocycle can be suitably used. In this way, as the crosslinking agent, a "compound forming a hydrogen-bond crosslinking site (more preferably, a compound capable of introducing a nitrogen-containing heterocycle)" can be suitably used. As such a "compound forming a hydrogen-bond crosslinking site (more preferably, a compound capable of introducing a nitrogen-containing heterocycle)", for example, a compound having a substituent (e.g., a hydroxyl group, a thiol group, an amino group, an imino group, etc.) that reacts with a maleic anhydride group is preferable, and a compound having at least one of a hydroxyl group, an amino group, an imino group, and a thiol group is more preferable. Furthermore, it is particularly preferable that such a compound having a substituent that reacts with a maleic anhydride group (more preferably a compound having at least one of a hydroxyl group, an amino group, an imino group, and a thiol group) has a nitrogen-containing heterocycle.

[0027] <Side chain (b): Side chain containing a covalent cross-linking moiety> In this specification, "side chain (b) containing a covalent cross-linking moiety" means a side chain that contains a moiety that cross-links polymer molecules forming the main chain together by a covalent bond (covalent cross-linking moiety: for example, a moiety that cross-links polymer molecules together by a chemically stable bond (covalent bond) such as at least one bond selected from the group consisting of amide, ester, and thioester, which can be formed by reacting a maleic anhydride group with a cross-linking agent). Incidentally, the side chain (b) is a side chain containing a covalent-bond cross-linking moiety. In the case where the side chain has a covalent-bonding moiety and further has a group capable of hydrogen bonding, thereby forming a cross-link by hydrogen bonding between side chains, the side chain is used as the side chain (c) described below. (In the case where the side chains of the polymer molecules do not contain both a hydrogen donor and a hydrogen acceptor capable of forming a hydrogen bond between each other, for example, when only a side chain containing an ester group (-COO-) is present in the system, hydrogen bonds are not formed between the ester groups (-COO-), and therefore such a group does not function as a hydrogen-bond cross-linking moiety. On the other hand, in ... a carboxyl group or a tetrahydrofuran group, such a group does not function as a hydrogen-bond cross-linking moiety. When the side chains of the polymer molecules each contain a structure having both a hydrogen donor site and a hydrogen acceptor site, such as a riazole ring, hydrogen bonds are formed between the side chains of the polymer molecules, and thus a hydrogen bond crosslinking site is contained. In addition, for example, when an ester group and a hydroxyl group coexist between the side chains of the polymer molecules and hydrogen bonds are formed between the side chains by these groups, the site that forms the hydrogen bond becomes a hydrogen bond crosslinking site. Therefore, depending on the structure of the side chain (b) itself, the structure of the side chain (b) and the type of substituents of the other side chains, it may be used as the side chain (c). ). In addition, the "covalent crosslinking site" referred to here is a site that crosslinks polymer molecules by a covalent bond.

[0028] The side chain (b) containing such a covalent cross-linking moiety is not particularly limited, but is preferably a side chain containing a covalent cross-linking moiety formed by reacting a maleic anhydride graft-modified thermoplastic polymer with a cross-linking agent made of a compound capable of forming a covalent cross-linking moiety by reacting with a maleic anhydride group (functional group) (hereinafter sometimes referred to as a "compound forming a covalent cross-linking moiety (compound generating a covalent bond)"). The cross-link at the covalent cross-linking moiety of such side chain (b) is preferably formed by at least one bond selected from the group consisting of amide, ester, and thioester.

[0029] As the "compound forming a covalent crosslinking moiety (compound forming a covalent bond)" that can be used as such a crosslinking agent, a compound having a substituent that reacts with a maleic anhydride group (e.g., a hydroxyl group, a thiol group, an amino group, an imino group, etc.) is preferred, and a compound having at least one of a hydroxyl group, an amino group, and an imino group is more preferred. In addition, such a compound having a substituent that reacts with a maleic anhydride group (more preferably, a compound having at least one of a hydroxyl group, an amino group, and an imino group) is particularly preferably one having a nitrogen-containing heterocycle.

[0030] Furthermore, examples of "compounds that form covalent cross-linking moieties (compounds that generate covalent bonds)" that can be used as such cross-linking agents include polyamine compounds having two or more amino groups and / or imino groups in one molecule (when both amino groups and imino groups are present, the total number of these groups is two or more); polyol compounds having two or more hydroxyl groups in one molecule; polyisocyanate compounds having two or more isocyanate (NCO) groups in one molecule; polythiol compounds having two or more thiol groups (mercapto groups) in one molecule; and the like. Here, the "compound forming a covalent cross-linking moiety (compound forming a covalent bond)" can be a compound capable of introducing both the hydrogen-bond cross-linking moiety and the covalent cross-linking moiety depending on the type of substituent possessed by such a compound, the degree of progress of the reaction when such a compound is used for the reaction, and the like (for example, when a compound having three or more hydroxyl groups is used as a cross-linking agent to form a cross-linking moiety by a covalent bond, depending on the degree of progress of the reaction, two hydroxyl groups may react with the functional group (maleic anhydride group) of the maleic anhydride graft-modified thermoplastic polymer, and the remaining hydroxyl group may remain as a hydroxyl group, in which case a moiety forming a hydrogen-bond cross-linking may also be introduced). Therefore, the "compound forming a covalent cross-linking moiety (compound forming a covalent bond)" exemplified here may also include a "compound forming both a hydrogen-bond cross-linking moiety and a covalent cross-linking moiety." From this viewpoint, when forming the side chain (b), a compound may be appropriately selected from "compounds forming a covalent cross-linking moiety (compounds generating a covalent bond)" according to the intended design, or the degree of reaction progress may be appropriately controlled to form the side chain (b). When the compound forming the covalent cross-linking moiety has a heterocycle, it becomes possible to simultaneously produce a hydrogen-bond cross-linking moiety more efficiently, and it becomes possible to efficiently form a side chain having the covalent cross-linking moiety as the side chain (c) described later. Therefore, specific examples of such compounds having a heterocycle will be described as suitable compounds for producing the side chain (c), particularly together with the side chain (c). It can be said that the side chain (c) is a suitable form of the side chain such as the side chain (a) or the side chain (b) from its structure.

[0031] As the polyamine compound, the polyol compound, the polyisocyanate compound, and the polythiol compound that can be used as such a "compound that forms a covalent cross-linking moiety (compound that generates a covalent bond)", known compounds (for example, those described in paragraphs

[0094] to

[0106] of Japanese Patent No. 5918878) can be appropriately used.

[0032] <Side chain (c): Side chain containing both hydrogen bond cross-linking moieties and covalent bond cross-linking moieties> Such a side chain (c) is a side chain containing both a hydrogen-bond cross-linkable moiety and a covalent-bond cross-linking moiety in one side chain. The hydrogen-bond cross-linkable moiety contained in such a side chain (c) is the same as the hydrogen-bond cross-linkable moiety described in the side chain (a'), and is preferably the same as the hydrogen-bond cross-linkable moiety in the side chain (a). In addition, as the covalent-bond cross-linking moiety contained in the side chain (c), the same as the covalent-bond cross-linking moiety in the side chain (b) can be used (the preferred cross-linking can also be the same).

[0033] Such a side chain (c) is preferably a side chain formed by reacting a maleic anhydride graft-modified thermoplastic polymer with a crosslinking agent consisting of a compound that reacts with a functional group (maleic anhydride group) of the maleic anhydride graft-modified thermoplastic polymer to form both a hydrogen-bond crosslinkable moiety and a covalent-bond crosslinking moiety (a compound that introduces both a hydrogen-bond crosslinkable moiety and a covalent-bond crosslinking moiety).

[0034] As the "compound that forms both hydrogen bond crosslinking moieties and covalent bond crosslinking moieties (compound that introduces both hydrogen bond crosslinking moieties and covalent bond crosslinking moieties)" that can be used as such a crosslinking agent, a compound having a substituent that reacts with a maleic anhydride group (e.g., a hydroxyl group, a thiol group, an amino group, an imino group, etc.) is preferred, and a compound having at least one of a hydroxyl group, an amino group, an imino group, and a thiol group is more preferred. In addition, as the compound that forms both hydrogen bond crosslinking moieties and covalent bond crosslinking moieties (compound that introduces both hydrogen bond crosslinking moieties and covalent bond crosslinking moieties), a compound that has a heterocycle (particularly preferably a nitrogen-containing heterocycle) and can form a covalent bond crosslinking moiety (a compound that forms a covalent bond) is preferred, and among them, a heterocycle-containing polyol, a heterocycle-containing polyamine, a heterocycle-containing polythiol, etc. are more preferred. In addition, the polyol, polyamine and polythiol containing such a heterocycle can be appropriately used similar to the polyol compound, polyamine compound and polythiol compound described in the above "compound capable of forming a covalent cross-linking site (compound that forms a covalent bond)" except that it has a heterocycle (particularly preferably a nitrogen-containing heterocycle). In addition, the polyol, polyamine and polythiol containing a heterocycle can be appropriately used known ones (for example, those described in paragraph

[0113] of Japanese Patent No. 5918878).

[0035] (Structures suitable for covalent cross-linking sites in side chains (b) to (c)) With regard to the side chains (b) and / or (c), when the crosslinking at the covalent crosslinking moiety contains a tertiary amino bond (-N=) or an ester bond (-COO-), and when these bond moieties also function as hydrogen-bond crosslinking moieties, this is preferable from the viewpoint that the crosslinking becomes stronger by hydrogen bonding with other hydrogen-bond crosslinking moieties. In this way, when the tertiary amino bond (-N=) or ester bond (-COO-) in the side chain having the covalent crosslinking moiety forms a hydrogen bond with another side chain, the covalent crosslinking moiety containing such a tertiary amino bond (-N=) or ester bond (-COO-) also has a hydrogen-bond crosslinking moiety and can function as the side chain (c).

[0036] As a compound capable of forming a covalent crosslinking site containing the tertiary amino bond and / or the ester bond by reacting with the maleic anhydride group, which is a functional group in the maleic anhydride graft-modified thermoplastic polymer (a compound capable of forming both a hydrogen bond crosslinking site and a covalent crosslinking site: one of the crosslinking agents), polyethylene glycol laurylamine (e.g., N,N-bis(2-hydroxyethyl)laurylamine), polypropylene glycol laurylamine (e.g., N,N-bis(2-methyl-2-hydroxyethyl)laurylamine), polyethylene glycol octylamine (e.g., N,N-bis(2-hydroxyethyl)octylamine), polypropylene glycol octylamine (e.g., N,N-bis(2-methyl-2-hydroxyethyl)octylamine), polyethylene glycol stearylamine (e.g., N,N-bis(2-hydroxyethyl)stearylamine), polypropylene glycol stearylamine (e.g., N,N-bis(2-methyl-2-hydroxyethyl)stearylamine) can be mentioned as a preferable example.

[0037] The crosslink at the covalent crosslinking moiety of the side chain (b) and / or side chain (c) may be, for example, the same as the structure described in paragraphs

[0100] to

[0109] of JP 2017-206604 A. For example, the crosslink at the covalent crosslinking moiety of the side chain (b) and / or side chain (c) may preferably contain at least one structure represented by any of the following general formulas (1) to (3) (note that, in the following structures, when a hydrogen-bond crosslinking moiety is contained, the side chain having the structure is used as the side chain (c)).

[0038] [ka]

[0039] In the above general formulae (1) to (3), E, ​​J, K and L each independently represent a single bond, an oxygen atom, an amino group NR' (R' is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms), or a sulfur atom; or an organic group which may contain these atoms or groups, and G represents a linear, branched or cyclic hydrocarbon group having 1 to 20 carbon atoms which may contain an oxygen atom, a sulfur atom or a nitrogen atom. Furthermore, as such a substituent G, groups represented by the following general formulae (111) to (114) are preferred.

[0040] [ka]

[0041] The side chain (a'), side chain (a), side chain (b), and side chain (c) have been described above, but each group (structure) of the side chain in such a polymer can be confirmed by commonly used analytical means such as NMR and IR spectroscopy.

[0042] The polymer (A) is a polymer having the side chain (a) and a glass transition point of 25° C. or lower, and the polymer (B) is a polymer containing a hydrogen-bond cross-linkable moiety and a covalent-bond cross-linking moiety in a side chain and having a glass transition point of 25° C. or lower (such as a polymer having both side chain (a') and side chain (b) as side chains or a polymer containing side chain (c) in a side chain). As the polymer component according to the present invention, one of the polymers (A) to (B) may be used alone, or two or more of them may be used in combination.

[0043] The polymer (B) may be a polymer having both the side chain (a') and the side chain (b), or may be a polymer having the side chain (c). However, the hydrogen-bond cross-linkable moiety contained in the side chain of the polymer (B) is preferably a hydrogen-bond cross-linkable moiety having a carbonyl-containing group and / or a nitrogen-containing heterocycle (more preferably a hydrogen-bond cross-linkable moiety having a carbonyl-containing group and a nitrogen-containing heterocycle) from the viewpoint of forming stronger hydrogen bonds. In addition, the cross-linking at the covalent cross-linking moiety contained in the side chain of the polymer (B) is preferably formed by at least one bond selected from the group consisting of amide, ester, and thioester from the viewpoint of being able to cause intermolecular interactions such as hydrogen bonds between side chains containing the cross-linking moiety.

[0044] Moreover, each of the polymers (A) and (B) according to the present invention is a reaction product between a maleic anhydride grafted thermoplastic polymer having a melting point of 64° C. or lower and a maleinization rate of 0.1 to 3.0 mass % and a crosslinking agent.

[0045] Thus, the maleic anhydride grafted thermoplastic polymer used to form the polymers (A) and (B) has a melting point of 64°C or less (more preferably 60°C to -100°C, and even more preferably 57°C to -50°C). If the melting point of such a maleic anhydride grafted thermoplastic polymer exceeds the upper limit, the hardness of the polymer composition increases, and the hardness cannot be sufficiently reduced. As such a melting point, a value measured by differential scanning calorimetry (DSC) is adopted. Note that, when measuring such a melting point, the measurement is performed at a temperature rise rate of 10°C / min.

[0046] Moreover, such maleic anhydride graft-modified thermoplastic polymer has a maleation rate of 0.1 to 3.0 mass % (more preferably 0.2 to 2.7 mass %, and even more preferably 0.3 to 2.5 mass %). If the maleation rate is less than the lower limit, the crosslinking density cannot be sufficiently increased even if a crosslinking reaction is carried out, and the mechanical properties of the polymer composition tend not to be sufficiently increased, whereas if it exceeds the upper limit, the flowability tends to decrease.

[0047] In the present invention, the value of "maleic acid ratio" (unit: mass %) is a value determined by the following [Method of measuring maleic acid ratio]. [Method for measuring maleic acid content] First, 400 mg of the maleic anhydride grafted modified thermoplastic polymer to be measured is dissolved in 80 mL of tetrahydrofuran (hereinafter, for convenience, sometimes abbreviated as "THF") to obtain a THF solution for measurement. Next, the THF solution for measurement is titrated with a 0.1 mol / L ethanol solution of potassium hydroxide for which a factor of three or more decimal places is required (a standard solution for volumetric analysis: a 0.1 mol / L ethanol solution of potassium hydroxide with correction: a commercially available solution for which a factor (characteristic value: correction value) of three or more decimal places is described may be used). Here, the end point (neutralization point) is determined by potentiometric titration using an instrument. The factor (characteristic value: correction value) of the 0.1 mol / L ethanol solution of potassium hydroxide may be determined by titration with an oxalic acid standard solution, or when a commercially available product for which a factor is required is used, the factor described in the commercially available reagent (for example, the factor described in the test report of the reagent) may be used as is. Next, a similar measurement (blank test) is performed except that no maleic anhydride graft-modified thermoplastic polymer is used, and titration is performed, and the amount of 0.1 mol / L potassium hydroxide ethanol solution dropped into 80 mL of THF (blank value) is also determined. Next, the acid value is calculated based on the "acid value calculation formula" below using the titration value (drop amount) obtained, and the maleinization ratio is calculated based on the "maleinization ratio calculation formula" below using the acid value obtained, thereby obtaining the maleinization ratio (unit: mass%). <Acid value calculation formula> [Acid value]=(AB)×M1×C×f / S (In the formula, A indicates the amount of 0.1 mol / L potassium hydroxide ethanol solution dropped (titration value: mL) required to neutralize the solution for measurement, B indicates the amount of 0.1 mol / L potassium hydroxide ethanol solution dropped in a blank (blank test) (titration value (blank value: mL) obtained by performing a similar measurement except that maleic anhydride graft-modified thermoplastic polymer is not used), M1 indicates the molecular weight of potassium hydroxide (56.1 (constant)), C indicates the concentration of potassium hydroxide in the potassium hydroxide ethanol solution (0.1 mol / L (constant)), f indicates the factor of the potassium hydroxide ethanol solution (correction value: the factor described in a commercially available reagent (for example, the factor described in the inspection report of the reagent) may be used as is), and S indicates the mass of the maleic anhydride graft-modified thermoplastic polymer used in the measurement (400 g (constant)). The unit of the "acid value" obtained by such calculation is "mgKOH / g".) <Formula for calculating maleic acid ratio> [Maleinization rate] = [Acid value] ÷ M1 × M2 ÷ 1000 × 100 ÷ 2 (In the formula, acid value is the value calculated using the above "Acid Value Calculation Formula" (unit: mgKOH / g), M1 is the molecular weight of potassium hydroxide (56.1 (constant)), and M2 is the molecular weight of maleic anhydride (98.1 (constant)). The unit of the "maleic acid content" calculated by this calculation is "mass %.")

[0048] The main chain of such a maleic anhydride graft-modified thermoplastic polymer (the polymer forming the main chain portion of the polymers (A) to (B)) can be appropriately selected from so-called thermoplastic polymers so that the melting point of the maleic anhydride graft-modified thermoplastic polymer is 64°C or lower. (Note that the "thermoplastic polymer" in the maleic anhydride graft-modified thermoplastic polymer referred to in this specification may be any polymer having thermoplastic properties and a melting point of 64°C or lower (more preferably a melting point in the range of 60°C to -100°C), and may be, for example, a so-called "elastomer" or "rubber.")

[0049] The main chain of such maleic anhydride graft-modified thermoplastic polymer (the polymer forming the main chain portion of polymers (A) to (B)) is not particularly limited, but is more preferably at least one selected from the group consisting of polyolefin-based polymers, polyester-based polymers, polyamide-based polymers, polystyrene-based polymers, polyacrylate-based polymers, polyacrylonitrile-based polymers, polyacetal-based polymers, polycarbonate-based polymers, and polyolefin-acrylate copolymers, further preferably polyolefin-based polymers, polyacrylate-based polymers, and polyolefin-acrylate copolymers, and particularly preferably polyolefin-based polymers.

[0050] The polyolefin-based polymer suitable as the main chain of such maleic anhydride graft modified thermoplastic polymer is not particularly limited, and may be a polymer of α-olefin or a polymer consisting of a copolymer of α-olefin and other copolymerizable monomers. Among these polyolefin-based polymers, from the viewpoint of easier reduction of hardness of the polymer composition, polypropylene (PP), polyethylene (PE), ethylene-butene copolymer (EBM), ethylene-propylene copolymer (EPM), ethylene-octene copolymer (EOM), ethylene-propylene-diene copolymer (EPDM) are preferred, ethylene-butene copolymer (EBM), ethylene-propylene copolymer (EPM), ethylene-octene copolymer (EOM), ethylene-propylene-diene copolymer (EPDM) are more preferred, and ethylene-butene copolymer (EBM), ethylene-octene copolymer (EOM), ethylene-propylene-diene copolymer (EPDM) are even more preferred.

[0051] The maleic anhydride graft-modified thermoplastic polymer is a graft-modified product (thermoplastic polymer graft-modified with maleic anhydride) obtained by graft-modifying the thermoplastic polymer described as the main chain with maleic anhydride. Therefore, the maleic anhydride graft-modified thermoplastic polymer is preferably a polyolefin polymer graft-modified with maleic anhydride, and more preferably a maleic anhydride graft-modified product of at least one polyolefin polymer selected from the group consisting of PP, PE, EBM, EPM, EOM and EPDM. Such maleic anhydride graft-modified thermoplastic polymers may be used alone or in combination of two or more.

[0052] The maleic anhydride graft-modified thermoplastic polymer is a graft-modified product (thermoplastic polymer graft-modified with maleic anhydride) obtained by graft-modifying the thermoplastic polymer with maleic anhydride, and may be any one that satisfies the above-mentioned conditions of melting point and maleinization rate, and the method of production is not particularly limited, and it can be easily produced by adopting a known method for preparing a maleic anhydride graft-modified thermoplastic polymer and appropriately adjusting the type of raw material and the amount used so as to satisfy the above-mentioned conditions. In addition, as for such a maleic anhydride graft-modified thermoplastic polymer, a commercially available product may be appropriately used as long as it satisfies the above-mentioned conditions.

[0053] The crosslinking agent is not particularly limited as long as it is capable of reacting with the maleic anhydride groups in the maleic anhydride graft-modified thermoplastic polymer to form either of the polymers (A) and (B). Depending on the intended design, a compound capable of reacting with the maleic anhydride groups to form various crosslinking sites (a compound capable of forming the intended side chain) may be appropriately selected and used.

[0054] As such a crosslinking agent, the above-mentioned "compounds that form a hydrogen-bond crosslinking site (more preferably, compounds that can introduce a nitrogen-containing heterocycle)" and "compounds that form a covalent crosslinking site (compounds that form a covalent bond)" can be suitably used. In addition, from the viewpoint of efficient reaction progress, such crosslinking agents are preferably compounds having at least one of a hydroxyl group, an amino group, an imino group, and a thiol group. In addition, as such compounds having at least one of a hydroxyl group, an amino group, an imino group, and a thiol group, those having a nitrogen-containing heterocycle (such a nitrogen-containing heterocycle is more preferably at least one selected from a triazole ring, an isocyanurate ring, a thiadiazole ring, a pyridine ring, an imidazole ring, a triazine ring, and a hydantoin ring) are more preferred (note that the "nitrogen-containing heterocycle" referred to here is the same as the above-mentioned, including preferred ones).Examples of such compounds having at least one of a hydroxyl group, an amino group, an imino group, and a thiol group include tris(2-hydroxyethyl)isocyanurate, 2,4-diamino-6-phenyl-1,3,5-triazine (benzoguanamine), 2,4-diamino-6-methyl-1,3,5-triazine (acetoguanamine), 3-amino-1,2,4-triazole, aminopyridine (2-, 3-, 4-), 3-amino-5-methylisoxazole, 2-aminomethylpiperidine, 1-(2-hydroxyethyl)imidazole, 2-butyl-5-hydroxymethylimidazole, 1,3-dihydro-1-phenyl-2H-benzimidazole-2-thione, chelidamic acid, kojic acid, 2,5-dimercapto-1,3,4-thiadiazole, 1-phenyl-5-methylisox ... mercapto-1,2,3,4-tetrazole, 1-methyl-5-mercapto-1,2,3,4-tetrazole, trishydroxyethyltriazine, tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, hydroxypyridine (2-, 3-, 4-), 1-hydroxybenzotriazole, 1-(2-aminoethyl)piperazine, bis(aminopropyl)piperazine, piperidineethanol (2-, 3-, 4-), piperidinemethanol (2-, 3-, 4-), pyridineethanol (2-, 3-, 4-), pyridinemethanol (2-, 3-, 4-), benzoguanamine, 4-methyl-5-(2'-hydroxyethyl)thiazole, 1-methylol-5,5-dimethylhydantoin, melamine, and mercaptopyridine (2-, 3-, 4-). Such compounds may be used alone or in combination of two or more.

[0055] In addition, from the viewpoint of high reactivity and industrial availability, such a crosslinking agent is preferably at least one compound selected from the group consisting of nitrogen-containing compounds which may have at least one substituent selected from the group consisting of hydroxyl groups, thiol groups, amino groups, and imino groups, oxygen-containing compounds which may have at least one substituent selected from the group consisting of hydroxyl groups, thiol groups, amino groups, and imino groups, and sulfur-containing compounds which may have at least one substituent selected from the group consisting of hydroxyl groups, thiol groups, amino groups, and imino groups. In addition, such "compounds that form hydrogen bond crosslinking sites (compounds that can introduce nitrogen-containing heterocycles)" and "compounds that form covalent crosslinking sites (compounds that form covalent bonds)" can be appropriately selected from known compounds (compounds described in JP 2017-57322 A and JP 5918878 A) as long as they are capable of reacting with maleic anhydride groups.

[0056] Furthermore, such a crosslinking agent is preferably a triazole which may have at least one substituent selected from the group consisting of a hydroxyl group, a thiol group, an amino group, and an imino group; a pyridine which may have at least one substituent selected from the group consisting of a hydroxyl group, a thiol group, an amino group, and an imino group; a thiadiazole which may have at least one substituent selected from the group consisting of a hydroxyl group, a thiol group, an amino group, and an imino group; an imidazole which may have at least one substituent selected from the group consisting of a hydroxyl group, a thiol group, an amino group, and an imino group; isocyanurate which may have at least one substituent selected from the group consisting of: isocyanurate which may have at least one substituent selected from a hydroxyl group, a thiol group, an amino group, and an imino group; hydantoin which may have at least one substituent selected from a hydroxyl group, a thiol group, an amino group, and an imino group; tris(2-hydroxyethyl)isocyanurate; 2,4-diamino-6-phenyl-1,3,5-triazine; pentaerythritol; sulfamide; and polyether polyol.

[0057] As such a crosslinking agent, from the viewpoint of compression set resistance, tris(2-hydroxyethyl)isocyanurate, sulfamide, pentaerythritol, 2,4-diamino-6-phenyl-1,3,5-triazine, 2,4-diamino-6-methyl-1,3,5-triazine, and polyether polyol are preferred, and pentaerythritol, 2,4-diamino-6-phenyl-1,3,5-triazine, 2,4-diamino-6-methyl-1,3,5-triazine, and tris(2-hydroxyethyl)isocyanurate are more preferred.

[0058] In addition, the method for obtaining the reaction product of the maleic anhydride graft-modified thermoplastic polymer and the crosslinking agent is not particularly limited, and any method capable of forming the polymers (A) and (B) by reacting the maleic anhydride group in the maleic anhydride graft-modified thermoplastic polymer with the functional group in the crosslinking agent (any method capable of forming the crosslinked sites described in the polymers (A) and (B)) may be used, and the reaction may be appropriately performed according to the type of crosslinking agent, etc. For example, a method may be adopted in which the maleic anhydride graft-modified thermoplastic polymer is mixed (kneaded) with a kneader or other kneading machine at a temperature (for example, about 100 to 250 ° C.) that can plasticize the maleic anhydride graft-modified thermoplastic polymer and can react with the added crosslinking agent and maleic anhydride group, while adding the crosslinking agent to react with the maleic anhydride group.

[0059] In addition, the polymer composition of the present invention containing such a polymer component has a type A durometer hardness (JIS-A hardness) of 0 to 49 (more preferably 0 to 45, and even more preferably 0 to 40) measured under a temperature condition of 20±5°C according to JIS K6253-3:2012. If the type A durometer hardness (JIS-A hardness) exceeds the upper limit, the hardness cannot be made sufficiently low, and the composition becomes too hard, making it impossible to obtain higher flexibility. It is possible to easily achieve such a type A durometer hardness (JIS-A hardness) by including the specific polymer component in the polymer composition (or, depending on the type of polymer component, by mixing the polymer component with other components). In the present invention, the method for measuring the type A durometer hardness (JIS-A hardness) value may be a measurement method in accordance with JIS K6253-3 (JIS K6253-3:2012) issued in 2012 under temperature conditions of 20±5°C. For example, the following measurement method may be used. That is, first, the polymer composition was heated to 200°C using a press machine equipped with a water-cooling function, and then 43 g of the polymer composition was placed in a mold measuring 15 cm in length, 15 cm in width, and 2 mm in thickness, and heated (preheated) at 200°C for 3 minutes before pressing. Next, the polymer composition was pressed (hot pressed) under conditions of a temperature of 200°C, a pressure of 20 MPa, and a pressing time of 5 minutes, and then further subjected to a water-cooling press under conditions of a pressure of 20 MPa and a pressing time of 2 minutes. The pressed polymer composition was removed from the mold, and a sheet for measurement of 2 mm in thickness was prepared. The sheet was punched out into a disk shape with a diameter of 29 mm, and seven of the obtained disk-shaped sheets were stacked together to prepare a measurement sample with a height (thickness) of 12.5±0.5 mm. Using the obtained measurement sample and a type A durometer (durometer A hardness tester), JIS hardness was measured at five points on the surface of the measurement sample under a temperature condition of 20±5°C. In accordance with K6253-3 (issued in 2012), the hardness of each material is measured and the hardness is calculated as the average value by adopting method (A).

[0060] In addition, from the viewpoint of having sufficient flexibility, the polymer composition of the present invention preferably has a type E durometer hardness (JIS-E hardness) measured under a temperature condition of 20±5°C in accordance with JIS K6253-3:2012 of 73 or less, more preferably 70 or less, and particularly preferably 67 or less. The method for measuring the value of such a type E durometer hardness (JIS-E hardness) may be a measurement method in accordance with JIS K6253-3 (JIS K6253-3:2012) issued in 2012 under a temperature condition of 20±5°C. For example, the same method as the above-mentioned method (A) may be used for measurement, except that a type E durometer (durometer E hardness tester) is used instead of a type A durometer.

[0061] In addition, from the viewpoint of obtaining a polymer composition having an ultra-low hardness depending on the application, it is preferable that the polymer composition of the present invention has a type A durometer hardness (JIS-A hardness) of 0 and a type E durometer hardness (JIS-E hardness) of 15 or less (more preferably 10 or less, and even more preferably 5 or less).

[0062] In addition, the polymer composition of the present invention may contain other components other than the polymer components from the viewpoint of appropriately adjusting the hardness and other properties according to the application. When such other components are contained, the content of the polymer components in the polymer composition of the present invention is preferably 3% by mass or more, more preferably 4% by mass to 99% by mass, even more preferably 4% by mass to 90% by mass, and particularly preferably 4% by mass to 80% by mass, from the viewpoint of sufficiently lowering the compression set value while setting the type A durometer hardness (JIS-A hardness) to 0 to 49. If the content of the polymer components in such a polymer composition is less than the lower limit, the effect obtained based on the polymer components tends to be low, while if it exceeds the upper limit, it tends to be difficult to mix.

[0063] In addition, from the viewpoint of improving the breaking properties (breaking strength, breaking elongation), the polymer composition of the present invention preferably contains a reinforcing agent (filler) as the other component. Such a reinforcing agent is not particularly limited, and a known reinforcing agent (which may be a hydrogen-bonding reinforcing agent (filler) or a filler into which an amino group has been introduced (hereinafter, sometimes simply referred to as an "amino group-introduced filler")) can be appropriately used. Suitable examples of such reinforcing agents include silica, carbon black, clay (which may be an organo-clay), and calcium carbonate (which may be surface-treated).

[0064] Among these reinforcing agents, clay is more preferable from the viewpoint of improving the tensile properties and the bleeding resistance. As such clay, known clays (for example, those described in paragraphs

[0146] to

[0156] of Japanese Patent No. 5918878, those described in paragraphs

[0146] to

[0155] of Japanese Patent Publication No. 2017-057393, etc.) can be appropriately used. Among such clays, from the viewpoint of high dispersibility, at least one selected from the group consisting of clays mainly composed of silicon and magnesium and organic clays is preferable, and organic clays are particularly preferable. Thus, it is preferable that the polymer composition of the present invention further contains clay, and it is particularly preferable that it contains organic clay.

[0065] In addition, when the polymer composition of the present invention contains the reinforcing agent (preferably clay, more preferably organo-clay), the content of the reinforcing agent is preferably 20 parts by mass or less, more preferably 0.01 to 10 parts by mass, based on 100 parts by mass of the polymer component. Note that such reinforcing agents may be used alone or in combination of two or more kinds depending on the application.

[0066] Furthermore, the polymer composition of the present invention preferably contains a plasticizer as the other component, from the viewpoint of improving the fluidity of the composition, improving the workability during use, and more efficiently adjusting the hardness of the polymer composition. Such plasticizers are not particularly limited, and known plasticizers can be appropriately used. Examples of such plasticizers include process oil, polybutene that does not have a crosslinking site of chemical bonding (more preferably, a copolymer mainly composed of isobutylene (isobutene) and partially reacted with normal butene), and polyisobutylene that does not have a crosslinking site of chemical bonding (homopolymer of isobutylene (isobutene)). In this specification, "having no crosslinking site of chemical bonding" refers to a state in which no site is formed in which crosslinks are formed by chemical bonds such as hydrogen bonds, covalent bonds, chelation between metal ions and polar functional groups, and bonds formed by σ-π interaction between metals and unsaturated bonds (double bonds, triple bonds).

[0067] In addition, as the process oil usable as such a plasticizer, paraffin oil, naphthene oil, and aromatic oil can be mentioned, among which paraffin oil is more preferable.In addition, as such a plasticizer, from the viewpoint of further improving compatibility between styrene block copolymer, α-olefin polymer, polymer (A) and polymer (B) (particularly between styrene block copolymer among these), it is more preferable to contain paraffin oil, and from the viewpoint of more efficiently achieving the polymer composition having a super-low hardness of JIS-A hardness of 0 and JIS-E hardness of 15 or less while being free of stickiness and bleeding, it is more preferable to contain polybutene without chemically bonded crosslinking sites and / or polyisobutylene without chemically bonded crosslinking sites. From the viewpoint of obtaining properties (hardness, etc.) according to the application, the polymer composition of the present invention preferably further contains at least one plasticizer selected from the group consisting of process oil, polybutene having no crosslinking site by chemical bonding, and polyisobutylene having no crosslinking site by chemical bonding. The content of such a plasticizer is preferably 10 to 5000 parts by mass, particularly preferably 30 to 3000 parts by mass, per 100 parts by mass of the polymer component.

[0068] There are no particular limitations on the paraffin oil suitable as such a plasticizer, and known paraffin oils can be appropriately used. For example, the one described in paragraphs

[0153] to

[0157] of JP 2017-57323 A can be suitably used. In addition, as for such paraffin oil, when correlation ring analysis (ndM ring analysis) according to ASTM D3238-85 is performed on the oil to determine the percentage of paraffin carbon number to the total carbon number (paraffin part: CP), the percentage of naphthene carbon number to the total carbon number (naphthene part: CN), and the percentage of aromatic carbon number to the total carbon number (aromatic part: CA), it is preferable that the percentage of paraffin carbon number to the total carbon number (CP) is 60% or more. In addition, from the viewpoint of fluidity and safety, the paraffin oil has a kinetic viscosity of 10 mm at 40° C. measured according to JIS K 2283 (published in 2000). 2 / s~700mm 2 / s. Furthermore, from the viewpoint of fluidity and safety, the paraffin oil preferably has an aniline point of 80°C to 150°C as measured by a U-tube method in accordance with JIS K2256 (published in 2013). The methods described in paragraphs

[0153] to

[0157] of JP2017-57323A can be used to measure the kinematic viscosity and aniline point. As such paraffin oil, commercially available products can be used as appropriate.

[0069] When such paraffin oil is contained in the polymer composition, the content of the paraffin oil is preferably 10 to 5000 parts by mass, and particularly preferably 30 to 3000 parts by mass, relative to 100 parts by mass of the polymer component. If the content of such paraffin oil is less than the lower limit, the content of the paraffin oil is too small, and the effect of adding the paraffin oil, such as improving fluidity and workability, tends to be insufficient, while if the content exceeds the upper limit, bleeding of the paraffin oil is easily induced, and it tends to be difficult to obtain a polymer composition in a uniform state.

[0070] The polybutene usable as the plasticizer is not particularly limited as long as it does not have a crosslinked site of chemical bond, but from the viewpoint of being able to achieve a lower hardness while being free of stickiness and bleeding and being able to further improve fluidity, it is more preferable that it is a copolymer mainly composed of isobutylene (isobutene) and partially reacted with normal butene (1-butene, 2-butene). As the polybutene as the plasticizer, a commercially available product can be appropriately used, for example, "Nippon Oil Polybutene" manufactured by JXTG Nippon Oil & Energy Corporation, "NOF Polybutene Emmawet" manufactured by NOF Corporation, "Oppanol" manufactured by BASF, etc. can be appropriately used.

[0071] When such polybutene is contained in the polymer composition, the content of polybutene is preferably 10 to 5000 parts by mass, and particularly preferably 30 to 3000 parts by mass, relative to 100 parts by mass of the polymer component. If the content of polybutene is less than the lower limit, the content of polybutene is too small, and it tends to be difficult to fully obtain the effects obtained by containing polybutene (reduced hardness and improved fluidity), while if the content of polybutene exceeds the upper limit, the content of polybutene becomes too high, which makes it easy to bleed, and instead tends to reduce strength.

[0072] Furthermore, the polyisobutylene usable as the plasticizer is not particularly limited as long as it does not have a chemically bonded crosslinking site, but it is more preferable that it is a homopolymer of isobutylene (isobutene) from the viewpoint of enabling a lower hardness and enabling a further improvement in fluidity. In addition, as the polyisobutylene used as the plasticizer, a commercially available product can be appropriately used, for example, the product names "Tetrax" and "Himol" manufactured by JXTG Nippon Oil & Energy Corporation can be appropriately used.

[0073] When such polyisobutylene is contained in the polymer composition, the content is preferably 10 to 5000 parts by mass, particularly preferably 30 to 3000 parts by mass, per 100 parts by mass of the polymer component. If the content of such polyisobutylene is less than the lower limit, the content of polyisobutylene is too small, and it tends to be difficult to fully obtain the effects obtained by containing polyisobutylene (reducing hardness and improving fluidity), while if the content exceeds the upper limit, the content of polyisobutylene becomes too high, which makes it easier to bleed, and instead tends to reduce strength.

[0074] In addition, the polymer composition of the present invention preferably contains a styrene block copolymer having no chemically bonded crosslinking site as the other component from the viewpoint of preventing bleeding when the plasticizer is used (particularly when oil is used), etc. Therefore, the polymer composition of the present invention preferably contains a combination of the plasticizer (more preferably at least one selected from the group consisting of the paraffin oil, the polybutene, and the polyisobutylene) and the styrene block copolymer having no chemically bonded crosslinking site.

[0075] In addition, in the polymer composition of the present invention, it is preferable to contain a combination of the paraffin oil as the plasticizer and the styrene block copolymer. This makes it possible to absorb oil into the styrene block copolymer, and while more sufficiently suppressing oil bleeding, it is possible to more highly improve the fluidity of the resulting polymer composition, and it is possible to more efficiently adjust the hardness. As such a styrene block copolymer that does not have a chemically bonded crosslinking site, those described in paragraphs

[0156] to

[0163] of JP 2017-57393 A can be suitably used. Note that the "styrene block copolymer" may be a polymer having a styrene block structure in any part.

[0076] In addition, the polymer composition of the present invention preferably contains a combination of polybutene and / or polyisobutylene as the plasticizer and a styrene block copolymer, which makes it easier to obtain a polymer composition having an ultralow hardness such that the JIS-A hardness is 0 and the JIS-E hardness is 15 or less, and further makes it possible to suppress surface bleeding to a higher degree when used in combination with a styrene block copolymer.

[0077] From the viewpoints of mechanical strength and oil absorbency, such a styrene block copolymer having no chemically bonded crosslinking site is preferably a styrene block copolymer having a styrene content of 10 to 50% by mass (more preferably 20 to 40% by mass). In addition, from the viewpoints of mechanical strength and oil absorbency, the weight average molecular weight (Mw), number average molecular weight (Mn) and dispersity of molecular weight distribution (Mw / Mn) of such a styrene block copolymer are preferably such that Mw is 200,000 or more and 700,000 or less (more preferably 350,000 or more and 550,000 or less), Mn is 100,000 or more and 600,000 or less (more preferably 200,000 or more and 500,000 or less), and Mw / Mn is 5 or less (more preferably 1 to 3). From the viewpoint of elastomer property (from the viewpoint of having sufficient elastomer property), the glass transition point of such a styrene block copolymer is preferably -80 to -30°C (more preferably -70 to -40°C). The methods for measuring such various properties (Mw, Mn, etc.) are as described in paragraphs

[0156] to

[0163] of JP2017-57393A.

[0078] As such a styrene block copolymer having no chemically bonded crosslinking site, known ones (e.g., SIS, SEPS, SBS, SIBS, SEEPS, SEBS, etc.) can be appropriately used, but from the viewpoints of high molecular weight, industrial availability, and economic efficiency, styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS) and styrene-ethylene-butylene-styrene block copolymer (SEBS) are more preferable. Such styrene block copolymers may be used alone or in combination of two or more. As such a styrene block copolymer, commercially available ones can be appropriately used. Note that, from the viewpoint of further improving oil bleeding resistance when used in combination with the plasticizer (particularly, paraffin oil, polybutene, polyisobutylene), SEBS and SEEPS are more preferable. From the viewpoint of obtaining a polymer composition having an ultra-low hardness such that the JIS-A hardness is 0 and the JIS-E hardness is 15 or less, it is particularly preferable that the polymer composition of the present invention contains the polymer component, the polybutene and / or the polyisobutylene, and the SEEPS.

[0079] In addition, when the polymer composition of the present invention contains a styrene block copolymer having no chemically bonded crosslinking site, the content of the styrene block copolymer is preferably 1 to 3000 parts by mass, more preferably 5 to 2000 parts by mass, relative to 100 parts by mass of the polymer component. In addition, when used in combination with the paraffin oil, the content of the styrene block copolymer is more preferably 1 to 3000 parts by mass, and even more preferably 5 to 2000 parts by mass. If the content ratio is less than the lower limit, the oil tends to bleed easily when oil is added, while if it exceeds the upper limit, the moldability tends to decrease. In addition, when used in combination with the polybutene and / or the polyisobutylene, the content of the styrene block copolymer is more preferably 1 to 3000 parts by mass, and even more preferably 5 to 2000 parts by mass. If the content ratio is less than the lower limit, it tends to be difficult to fully obtain the effect of including the styrene block copolymer (the effect of sufficiently suppressing oil bleeding). On the other hand, if the content ratio exceeds the upper limit, the content of the styrene block copolymer becomes too high, and thus moldability tends to decrease.

[0080] The polymer composition of the present invention may further contain an α-olefin-based polymer that does not have a crosslinking site of chemical bond as the other component. The term "α-olefin-based polymer" as used herein refers to a homopolymer of an α-olefin or a copolymer of an α-olefin, and the term "α-olefin" refers to an alkene having a carbon-carbon double bond at the α-position, such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, and 1-decene. However, since the polybutene and polyisobutylene are used as plasticizers in the present invention, the term "α-olefin-based polymer" as used herein refers to a polymer other than the polybutene and polyisobutylene. As such an α-olefin-based polymer that does not have a crosslinking site of chemical bond, for example, the α-olefin-based resins (excluding polybutene and polyisobutylene) described in paragraphs

[0204] to

[0214] of JP 2017-57322 A can be suitably used.

[0081] In addition, as such an α-olefin-based polymer having no chemically bonded crosslinking site, for example, polypropylene, polyethylene (PE, more preferably HDPE), ethylene-propylene copolymer, ethylene-butene copolymer (EBM), and ethylene-octene copolymer can be preferably used. In addition, as such an α-olefin-based polymer, among others, an α-olefin-based polymer having a crystallinity of 10% or more (polypropylene, ethylene-propylene copolymer, ethylene-butene copolymer, polyethylene, etc.) can be preferably used. There is no particular limitation on the method for producing such an α-olefin-based polymer having no chemically bonded crosslinking site, and a known method can be appropriately adopted. In addition, as such an α-olefin-based polymer, a commercially available product may be used. In addition, such an α-olefin-based polymer having no chemically bonded crosslinking site may be used alone or in combination of two or more.

[0082] When such an α-olefin polymer having no chemically bonded crosslinking site is contained in the polymer composition, the content of the α-olefin polymer is more preferably 500 parts by mass or less (more preferably 5 to 300 parts by mass, most preferably 35 to 200 parts by mass) relative to 100 parts by mass of the polymer component. If the content of such an α-olefin polymer is less than the lower limit, the effect tends to be low, while if it exceeds the upper limit, the hardness tends to be too high, making it difficult to impart a sufficiently high degree of flexibility to the polymer composition.

[0083] In addition, from the viewpoint of enabling the achievement of higher fluidity and higher moldability, it is preferable to incorporate such an α-olefin-based polymer having no chemically bonded cross-linking site in the composition in combination with the paraffin oil and the styrene block copolymer.

[0084] In addition, the polymer composition of the present invention preferably contains an antiaging agent and / or an antioxidant depending on its application. Such antiaging agents and antioxidants are not particularly limited, and known ones can be used as appropriate. The content of such antiaging agents and antioxidants is not particularly limited, but is preferably 20 parts by mass or less (more preferably 0.01 to 10 parts by mass) each relative to 100 parts by mass of the polymer component.

[0085] In addition, in the polymer composition of the present invention, in addition to the above-mentioned other components (the reinforcing agent (filler), the plasticizer (softener), the styrene block copolymer and the α-olefin-based polymer, the antioxidant, the antioxidant, etc.), known additives used in compositions containing polymers (for example, those described in paragraphs

[0169] to

[0174] of Japanese Patent No. 5,918,878) may be further used as other components depending on the intended use and design. The additives (other components) that can be further used are not particularly limited, and known components that can be used in the field of compositions containing polymers can be appropriately used, such as polymers other than the polymer components (A) to (B), amino group-containing compounds other than the amino group-introducing fillers, compounds containing metal elements, pigments (dyes), thixotropy-imparting agents, ultraviolet absorbers, flame retardants, solvents, surfactants (including leveling agents), various oils other than the process oils, dispersants, dehydrating agents, rust inhibitors, adhesion-imparting agents, antistatic agents, fillers, lubricants, processing aids (vulcanization accelerators such as stearic acid and zinc oxide in the case of vulcanization), etc. In addition, such other components may be used alone or in combination of two or more depending on the application.

[0086] In addition, the method for producing such a polymer composition is not particularly limited, and may be any method capable of containing the reaction product of the maleic anhydride graft-modified thermoplastic polymer and the crosslinking agent in the composition. For example, in the method described in paragraphs

[0181] to

[0215] of JP 2016-193970 A, except that the "raw material compound" described in the publication is replaced with "the crosslinking agent", the same method as the method described in the same paragraph of the publication may be adopted to react the maleic anhydride graft-modified thermoplastic polymer with the crosslinking agent to produce a polymer composition containing the polymer component consisting of the resulting reaction product.

[0087] As a method for producing such a polymer composition, for example, a method of mixing the maleic anhydride graft-modified thermoplastic polymer, the crosslinking agent, and other components (the reinforcing agent, the styrene block copolymer having no chemically bonded crosslinking site, the plasticizer (paraffin oil, polybutene, etc.), the α-olefin-based polymer having no chemically bonded crosslinking site, the antiaging agent, the antioxidant, the additives, etc.) as necessary to obtain a polymer composition containing the polymer components can be preferably adopted. In such a method, it is preferable to prepare polymer (A) and polymer (B) by reacting the maleic anhydride group in the maleic anhydride graft-modified thermoplastic polymer with the functional group in the crosslinking agent during mixing to form a specific crosslink. In addition, in such a method, it is possible to react the maleic anhydride graft-modified thermoplastic polymer with the crosslinking agent during mixing, and during the reaction, it is possible to ring-open the maleic anhydride group of the maleic anhydride graft-modified thermoplastic polymer and form a chemical bond with the crosslinking agent, thereby making it possible to efficiently form the desired "at least one polymer component selected from the group consisting of polymer (A) and polymer (B)" depending on the type of the component.

[0088] In addition, when the maleic anhydride graft-modified thermoplastic polymer is reacted with the crosslinking agent by the above method, the amount of the crosslinking agent used is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 5.0 parts by mass, relative to 100 parts by mass of the maleic anhydride graft-modified thermoplastic polymer. If the amount of the crosslinking agent added (amount based on parts by mass) is less than the lower limit, the amount of crosslinking agent is too small to increase the crosslink density, and the desired physical properties tend not to be expressed, while if the amount of the crosslinking agent exceeds the upper limit, the amount of the crosslinking agent is too large, resulting in an increase in branches (too much crosslinking agent, increasing the proportion of crosslinking agent not involved in crosslinking), and the crosslink density tends to decrease.

[0089] In addition, in such a method, the temperature conditions when the maleic anhydride graft-modified thermoplastic polymer and the crosslinking agent are reacted (the maleic anhydride group is opened) are not particularly limited, and may be adjusted to a temperature at which they can react depending on the type of the crosslinking agent, etc. For example, from the viewpoint of softening and instantly promoting the reaction, the temperature is preferably 100 to 250 ° C, and more preferably 120 to 230 ° C. In addition, the mixing method for carrying out such a reaction is not particularly limited, and known methods such as mixing with a roll or kneader can be appropriately adopted. Furthermore, when other components are added, the order of addition of each component is not particularly limited, and may be appropriately changed depending on the type of the component used. For example, when the styrene block copolymer not having a chemically bonded crosslinking site, the paraffin oil, and the α-olefin-based polymer not having a chemically bonded crosslinking site are added as other components when producing the polymer composition, the following method may be adopted. For example, the styrene block copolymer and the paraffin oil are mixed at a temperature of 100 to 250° C. to obtain a mixture, and then the maleic anhydride graft-modified thermoplastic polymer and the α-olefin-based polymer are added to the mixture under the temperature conditions, mixed and plasticized, and a crosslinking agent is added thereto under the temperature conditions and mixed to react the maleic anhydride graft-modified thermoplastic polymer with the crosslinking agent, thereby obtaining a polymer composition containing the reaction product of the maleic anhydride graft-modified thermoplastic polymer and the crosslinking agent, the styrene block copolymer, the paraffin oil, and the α-olefin-based polymer. When other components such as the reinforcing agent (filler) and the antiaging agent are further contained, the components may be appropriately added and mixed at any stage depending on the components used, and the order of addition of these components is not particularly limited, but when a reinforcing agent is added, it is preferable to mix the reinforcing agent with the maleic anhydride graft-modified thermoplastic polymer before adding and mixing the crosslinking agent from the viewpoint of further improving its dispersibility.The amounts of these other components added can be appropriately changed depending on the intended design (for example, the amounts added may be appropriately set so as to fall within the preferred content ranges described above).

[0090] The polymer composition of the present invention is useful as a material for producing polymer products used for applications such as daily necessities, automobile parts, electrical appliances, industrial parts, etc., and among them, since it is possible to sufficiently reduce the hardness, it is particularly preferable to use it for machines and housings and protective gear for electrical appliances, interior materials for houses and automobiles, skin for humanoid robots (androids, humanoids), toys, etc., which require a soft touch mainly for human touch. EXAMPLES

[0091] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0092] [Maleic anhydride modified thermoplastic polymers used in each example] Table 1 shows the abbreviations, polymer types, and characteristics of the maleic anhydride-modified thermoplastic polymers used in each Example. The "maleic ratio" in Table 1 is a value obtained by adopting the above-mentioned [method of measuring maleic ratio] (note that, for the titration, a potentiometric automatic titrator manufactured by Kyoto Electronics Manufacturing Co., Ltd. under the trade name "AT-710M") was used as the potentiometric automatic titrator, and a 0.1 mol / L ethanol solution of potassium hydroxide manufactured by Merck Ltd. under the trade name "potassium hydroxide ethanol solution". The correction factor of the 0.1 mol / L ethanol solution of potassium hydroxide used in this way was confirmed to be 1.00 from the inspection report of the solution). The "melting point" in Table 1 is a value measured by using 0.01 g of each polymer and a differential scanning calorimeter (manufactured by Hitachi High-Tech Science Corporation under the trade name "DSC7000X") at a heating rate of 10°C / min (value obtained by differential scanning calorimetry (DSC)).

[0093] [Table 1]

[0094] [Method for evaluating the properties of the polymer compositions obtained in each example, etc.] <Preparation of the measurement sheet> Using each of the polymer compositions obtained in each Example, a sheet for use in evaluating the properties of the composition was prepared as follows. That is, first, a press machine with a water-cooling function was used to heat the composition to 200°C, and then 43 g of the polymer composition was placed in a mold with a size of 15 cm long, 15 cm wide, and 2 mm thick, and the polymer composition was heated (preheated) at 200°C for 3 minutes before pressing, and then pressed (hot pressed) under the conditions of temperature: 200°C, operating pressure: 20 MPa, and pressing time: 5 minutes, and then water-cooled pressing was further performed under the conditions of operating pressure: 20 MPa, and pressing time: 2 minutes, and the pressed polymer composition was taken out of the mold to obtain a sheet for measurement with a thickness of 2 mm.

[0095] <Preparation of samples (measurement samples) for measuring compression set and hardness> Using the measurement sheets obtained as described above, measurement samples for use in measuring the compression set and hardness of the composition were prepared as follows: First, seven disk-shaped sheets were punched out of the measurement sheets to obtain disks with a diameter of 29 mm, and then the seven disk-shaped sheets were stacked together to obtain a height (thickness) of 12.5±0.5 mm to prepare a measurement sample.

[0096] <Measurement of compression set (C-Set)> The compression set (C-Set) of the polymer composition obtained in each Example was determined by using the measurement sample obtained as described above and a compression device manufactured by Dumbbell Co., Ltd. under the trade name "Vulcanized Rubber Compression Set Tester SCM-1008L" to compress the measurement sample by 25% with a dedicated tool, and measuring the compression set (unit: %) after leaving it at 70°C for 22 hours in accordance with JIS K6262 (issued in 2013).

[0097] <Measurement of hardness (JIS-A hardness and E hardness)> The hardness of the polymer composition obtained in each example was measured as follows using the measurement sample obtained as described above. That is, a type A durometer (Durometer A hardness meter: Trade name "Type A Durometer GSD-719K" manufactured by Teclock Corporation) was used to measure the JIS-A hardness, and a type E durometer (Durometer E hardness meter: Trade name "Type E Durometer GSD-721K" manufactured by Teclock Corporation) was used to measure the JIS-E hardness, and the hardness was measured according to JIS K6253-3 (published in 2012) at five measurement points (five measurement points) on the surface of the measurement sample under a temperature condition of 20±5°C, and the average value of the hardness at each measurement point (average value of five points) was obtained to obtain the A hardness and the E hardness, respectively.

[0098] <How to evaluate stickiness> The stickiness of the polymer compositions obtained in each Example was evaluated as follows: First, five testers touched the surface of the 2 mm-thick measuring sheet obtained as described above with their fingers and scored it from 1 to 5 points based on the following evaluation criteria, and a mean score of 3.0 points or more by the five testers was evaluated as "sticky" and a mean score of less than 3.0 points was evaluated as "not sticky." <Evaluation criteria (stickiness)> 1 point: No stickiness felt at all 2 points: Almost no stickiness 3 points: Slightly sticky 4 points: Sticky feeling 5 points: Very sticky feeling.

[0099] ( Reference example 1 to 6 and Comparative Examples 1 to 5) Reference example In each of Comparative Examples 1 to 6 and Comparative Examples 1 to 5, the amounts of each component used were adjusted to obtain the compositions shown in Tables 2 and 3 below, and the polymer compositions were produced by employing the "polymer composition production process" described below. The numerical values ​​of the compositions in Tables 2 and 3 below are Reference exampleetc., the amount of the maleic anhydride modified thermoplastic polymer (TP(1) to (11)) used is converted to 100 parts by mass (parts by mass), Reference example The amount of the maleic anhydride grafted modified thermoplastic polymer used was 10 g in each of Comparative Examples 1 to 6 and Comparative Examples 1 to 5. The evaluation results of the properties (C-Set, hardness, stickiness) of the polymer compositions thus obtained are shown in Tables 2 to 3, respectively.

[0100] <Production process of polymer composition> First, a styrene block copolymer (styrene-ethylene-butylene-styrene block copolymer, Kraton's product name "G1651HU", styrene content 33% by mass: hereinafter sometimes referred to as "SEBS") was put into a pressure kneader and mixed under a condition of 180 ° C. while dropping paraffin oil (SK Lubricants' product name "YUBASE8J") as a plasticizer into the pressure kneader, and the SEBS and paraffin oil were mixed for 1 minute. Next, maleic anhydride modified thermoplastic polymer, ethylene-butene copolymer (Mitsui Chemicals' product name "Tafmer DF7350": hereinafter sometimes referred to as "EBM"), high density polyethylene (Japan Polyethylene's product name "HJ590N": hereinafter sometimes referred to as "HDPE") and antioxidant (Adeka's product name "AO-50") were further added to the pressure kneader, and mixed (kneaded) at 180 ° C. for 2 minutes to plasticize and obtain a mixture (A). Then, the following steps (I) and (II): [Step (I)] A step of adding a crosslinking agent (crosslinking agent (1) or (2)) directly to the mixture (A) and mixing (kneading) the mixture at 180°C for 8 minutes; [Step (II)] A step of adding clay (organic clay, trade name "ESBEN WX" manufactured by HOJUN CO., LTD.) to the mixture (A) and mixing (kneading) at 180°C for 4 minutes, and then adding a crosslinking agent (crosslinking agent (1) or (2)) and mixing (kneading) at 180°C for 8 minutes; The polymer composition was produced by carrying out any one of the steps. Reference example In the comparative examples 1 to 2, 4 to 5 and 1 and 4, the mixture (A) was obtained, and then the step (I) was carried out. Reference example In Comparative Examples 3 and 6 and Comparative Examples 2 to 5, the mixture (A) was obtained and then subjected to step (II). Regarding the crosslinking agent, tris(2-hydroxyethyl)isocyanurate (trade name "Tanac P" manufactured by Nissei Corporation) was used as the "crosslinking agent (1)", and benzoguanamine (trade name "Benzoguanamine" manufactured by Nippon Shokubai Co., Ltd.) was used as the "crosslinking agent (2)".

[0101] Regarding Tables 2 and 3: (1) In Tables 2 and 3, Reference example For convenience, the types of maleic anhydride modified thermoplastic polymers used in the above are indicated using the abbreviations shown in Table 1. (2) In Tables 2 and 3, in the "evaluation of maleic acid anhydride modified thermoplastic polymers," those that satisfy the condition that the maleic acid ratio is in the range of 0.1 to 3.0 mass% are indicated with "S," while those that do not satisfy the condition that the maleic acid ratio is in the range of 0.1 to 3.0 mass% are indicated with "F." (3) In Tables 2 to 3, in the "evaluation of melting point" of the maleic anhydride graft-modified thermoplastic polymer, those that satisfy the condition that the melting point is 64°C or less are indicated with "S", while those that do not satisfy the condition that the melting point is 64°C or less (those with a melting point higher than 64°C) are indicated with "F".

[0102] [Table 2]

[0103] [Table 3]

[0104] Example 1~2 ) The above-mentioned procedures were repeated except that ethylene-butene copolymer (EBM) and high density polyethylene (HDPE) were not used, styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS) was used instead of SEBS as the styrene block copolymer, polybutene was used instead of paraffin oil as the plasticizer, and the amount of each component was adjusted so that the composition (parts by mass) was as shown in Table 4. Reference example The polymer compositions were produced by employing the same steps as in the "polymer composition production steps" employed in Examples 1 to 6 and Comparative Examples 1 to 5. 1 and 2 In all of the examples, tris(2-hydroxyethyl)isocyanurate (crosslinking agent (1)) was used as the crosslinking agent. 1 and examples 2 In this study, we used different types of commercially available SEEPS (Example 1 In the example, SEEPS was measured using the product "Septon 4099" manufactured by Kuraray Co., Ltd. 2 In the present embodiment, the SEEPS used was a product manufactured by Kuraray Co., Ltd. under the trade name "Hybra 7135R." 1 and 2 In the examples, the polybutene used was "Nippon Oil Polybutene LV-7" manufactured by JXTG Nippon Oil & Energy Corporation. 1 In Example 1, the step (I) was carried out without adding clay, and in Example 2, the step (I) was carried out without adding clay. 2 In the second case, the clay was added by carrying out step (II). The evaluation results of the properties (C-Set, hardness, stickiness) of the polymer composition thus obtained are shown in Table 4. The contents of the items "Evaluation of maleinization rate" and "Evaluation of melting point" are the same as those in Tables 2 and 3.

[0105] [Table 4]

[0106] As is apparent from Tables 1 to 4, the polymer composition ( Reference Examples 1 to 6 and Examples 1 to 2) had a compression set (C-Set) of 42% or less and a JIS-A hardness of 49 or less. Reference Examples 1 to 6 and Examples 1 to 2 All of the polymer compositions obtained in the above were non-sticky. Reference Examples 1 to 6 and Examples 1 to 2 The polymer composition obtained in Reference Examples 1 to 6 and Examples 1 to 2 ) were found to be able to achieve a sufficiently low hardness, such as a JIS-A hardness of 49 or less, and to be sufficiently excellent in resistance to compression set, such as a compression set (C-Set) value of 43% or less.

[0107] In contrast, in the case of a polymer composition (Comparative Examples 1-2) containing a reaction product of a maleic anhydride graft-modified thermoplastic polymer and a crosslinking agent that does not satisfy the condition (I) of a melting point of 64°C or less (hereinafter referred to as "condition (I)") and a maleinization rate of 0.1 to 3.0 mass% (hereinafter referred to as "condition (II)"), the JIS-A hardness was 66 or more, and it was not possible to achieve a sufficiently low hardness of JIS-A hardness of 49 or less. In addition, in the case of a polymer composition (Comparative Examples 1-2) containing a reaction product of a maleic anhydride graft-modified thermoplastic polymer and a crosslinking agent that does not satisfy the condition (I) of the above, the compression set (C-Set) was 58% or more, and it was not possible to sufficiently reduce the value of the compression set (C-Set).

[0108] In addition, from the results shown in Table 3, when a thermoplastic polymer modified by maleic anhydride by copolymerization (hereinafter sometimes referred to as "copolymerization type maleic anhydride modified thermoplastic polymer") was used as a maleic anhydride modified thermoplastic polymer (Comparative Examples 3 to 5), all of the polymer compositions (Comparative Examples 3 to 5) containing a reaction product of such copolymerization type maleic anhydride modified thermoplastic polymer and a crosslinking agent were sticky, and a non-sticky polymer composition could not be obtained. In addition, in the polymer composition (Comparative Example 3) obtained by using a copolymerization type maleic anhydride modified thermoplastic polymer (maleic anhydride modified thermoplastic polymer satisfying only condition (I)) having a melting point of 64°C or less and a maleinization rate of 3.1 mass%, a sufficiently low hardness was achieved with a JIS-A hardness of 40, but the compression set (C-Set) was 50%, and the value of the compression set could not be sufficiently low, and both the hardness and the compression set could not be sufficiently low. Furthermore, in the polymer composition (Comparative Example 4) obtained by using a copolymer type maleic anhydride copolymerized thermoplastic polymer having a melting point of 69°C and a maleination rate of 3.6% by mass (maleic anhydride modified thermoplastic polymer not satisfying both conditions (I) and (II)), the JIS-A hardness was 45, which was a sufficiently low hardness, but the compression set was 46%, and the value of the compression set (C-Set) could not be sufficiently low. Furthermore, in the polymer composition (Comparative Example 4) obtained by using a copolymer type maleic anhydride copolymerized thermoplastic polymer having a melting point of 65°C and a maleination rate of 2.8% by mass (maleic anhydride modified thermoplastic polymer satisfying only condition (II)), the JIS-A hardness was 40, which was a sufficiently low hardness, but the compression set (C-Set) was 52%, and the value of the compression set could not be sufficiently low, and both the hardness and the compression set could not be sufficiently low.As described above, the polymer compositions obtained in Comparative Examples 1 to 5 were unable to achieve both a sufficiently low hardness and a sufficiently excellent resistance to compression set, and were also unable to provide compositions that were not sticky.

[0109] From the results shown in Table 4, it can be seen that the polymer composition (Examples) containing a reaction product of a maleic anhydride graft-modified thermoplastic polymer having a melting point of 64° C. or less and a maleation rate of 0.1 to 3.0% by mass with a crosslinking agent in combination with polybutene (plasticizer) and SEEPS was 1 and 2 ), not only was the JIS-A hardness 0, but the JIS-E hardness was an extremely low hardness of 5 or less. In addition, from the results shown in Table 4 and the results shown in Table 2, it can be seen that the polymer composition ( Reference example 1 to 6) and a polymer composition using polybutene (Example 1~2 ) both are non-sticky, but it can be seen that when polybutene is used as a plasticizer, a composition with lower hardness can be obtained. [Industrial Applicability]

[0110] As described above, according to the present invention, it is possible to provide a polymer composition that is not sticky and can have sufficiently low hardness and compression set. Therefore, the polymer composition of the present invention is useful for applications such as machines and electrical appliances housings and protective gears, interior materials for houses and automobiles, skins for humanoid robots (androids, humanoids), toys, etc., which require a soft touch that is mainly felt by humans.

Claims

1. at least one polymer component selected from the group consisting of a polymer (A) having a side chain (a) containing a hydrogen-bond cross-linkable moiety having a carbonyl-containing group and / or a nitrogen-containing heterocycle and having a glass transition point of 25° C. or lower, and a polymer (B) having a side chain containing a hydrogen-bond cross-linkable moiety and a covalent-bond cross-linking moiety and having a glass transition point of 25° C. or lower; At least one plasticizer selected from the group consisting of polybutene having no chemically bonded cross-linking sites and polyisobutylene having no chemically bonded cross-linking sites; Contains Both of the polymer (A) and the polymer (B) are reaction products of a maleic anhydride graft-modified thermoplastic polymer having a melting point of 64° C. or less and a maleinization rate of 0.1 to 3.0 mass % and a crosslinking agent, and The type A durometer hardness measured under a temperature condition of 20±5°C in accordance with JIS K6253-3:2012 is 0, and the type E durometer hardness measured under a temperature condition of 20±5°C in accordance with JIS K6253-3:2012 is 15 or less; A polymer composition comprising:

2. 2. The polymer composition according to claim 1, wherein the malein content is 0.1 to 0.9% by mass.

3. 3. The polymer composition according to claim 1, wherein the crosslinking agent is a compound having at least one of a hydroxyl group, an amino group, an imino group, and a thiol group.

4. 4. The polymer composition according to claim 1, wherein the maleic anhydride graft-modified thermoplastic polymer is a polyolefin polymer graft-modified with maleic anhydride.

5. The polymer composition according to claim 4, wherein the polyolefin polymer graft-modified with maleic anhydride is at least one polyolefin polymer selected from the group consisting of polypropylene, polyethylene, ethylene-butene copolymer, ethylene-propylene copolymer, ethylene-octene copolymer, and ethylene-propylene-diene copolymer, grafted with maleic anhydride.

6. The polymer composition according to any one of claims 1 to 5, further comprising a clay.

7. 7. The polymer composition according to claim 1, further comprising a styrene block copolymer having no chemically bonded cross-linking sites.

Citation Information

Patent Citations

  • Thermoplastic elastomer composition and method for producing the same

    JP2016193970A

  • Thermoplastic elastomer composition and manufacturing method therefor

    JP2017057322A

  • Halogen-free flame-retardant resin composition, and halogen-free flame-retardant insulated wire

    JP2017160328A

  • Resin composition, molded article, and method for producing molded article

    JP2018087319A

  • Thermoplastic elastomer composition and method for preparing same

    WO2017047274A1