Polyether carbonate polyol purification process
A solid absorbent-based process at moderate temperatures effectively removes cyclic alkylene carbonates from polyether carbonate polyols, addressing the capital-intensive and thermal decomposition issues of existing methods.
Patent Information
- Application Number
- JP2021542120
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-31
- Filing Date
- 2020-01-06
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2040-01-06
AI Technical Summary
Existing methods for removing cyclic alkylene carbonate impurities from polyether carbonate polyols are capital intensive and expose the polyols to high temperatures, leading to thermal decomposition.
A process involving contacting polyether carbonate containing cyclic alkylene carbonate with a solid absorbent at moderate temperatures (30 to 150°C) using absorbents like alumina, magnesium silicate, molecular sieves, or ion exchange resins to effectively remove the impurities.
The process achieves efficient and cost-effective removal of cyclic alkylene carbonates with minimal thermal degradation of the polyether carbonate, using simple equipment and moderate temperatures.
Smart Images

Figure 0007565283000001 
Figure 0007565283000002 
Figure 0007565283000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a process for purifying polyether carbonate polyols. [Background technology]
[0002] In some cases, it may be necessary to remove cyclic alkylene carbonate impurities from polyether carbonate polyols.
[0003] Polyether carbonate polyols can be made by copolymerizing carbon dioxide and oxiranes in the presence of a hydroxyl-functional initiator and certain catalysts. This process produces a cyclic alkylene carbonate by-product that is soluble in the product. Because it is undesirable for this alkylene carbonate to be present in significant amounts, processes have been developed to remove some or all of it. This is generally done by vaporizing the alkylene carbonate or stripping it from the polyol under reduced pressure, as described, for example, in US 8,324,419 and US Published Patent Application No. 2017-0152345. These processes are capital intensive and therefore expensive. Moreover, they subject the polyether carbonate to high temperatures where thermal decomposition can occur.
[0004] Ion exchange resins and various absorbents have been proposed to remove certain impurities from polyether polyols. For example, US 4,355,188 describes a process in which double metal cyanide catalyst residues are treated with a strong base to convert the catalyst residues to ionic species that can then be removed using ion exchange resins. US 5,144,093 describes a similar process in which the catalyst residues are oxidized to form solids that can be removed by absorption and / or by passing the polyol through an ion exchange resin bed. US 4,985,551 and US 5,254,227 describe methods for removing "strongly ionic" metal impurities from polyols by passing the polyol through an ion exchange medium while passing an electric current through the ion exchange medium.
[0005] US8,354,559 describes the removal of double metal cyanide catalyst residues from polyethers by treatment with particulate inorganic solids. US9,527,958 describes the purification of polycarbonate polyols by treatment with diatomaceous earth to remove double metal cyanide catalyst residues. US9,815,965 describes the removal of catalyst residues from polyether carbonates by carrying out adsorption, aggregation, coagulation, and / or flocculation steps to produce a solid residue which is then separated. Adsorption is carried out using activated clay, bleaching earth, synthetic silicates, activated carbon, activated silica, or diatomaceous earth. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention is a process for removing cyclic alkylene carbonates from polyether carbonate which comprises contacting a starting polyether carbonate containing at least 0.25% by weight of one or more cyclic alkylene carbonates, based on the weight of the starting polyether carbonate, with a solid absorbent at a temperature of from 30 to 150°C, at which temperature the starting polyether carbonate is a liquid.
[0007] The process effectively removes cyclic alkylene carbonates from polyether carbonate polyols in an inexpensive and time-efficient manner using simple equipment. The process requires only moderately high temperatures at which thermal decomposition of the polyol is minimized.
[0008] Polyether carbonates contain both ether and carbonate linkages. They are conveniently prepared by polymerizing one or more alkylene oxides with a carbonate precursor, especially carbon dioxide. The alkylene oxide can be, for example, ethylene oxide, 1,2-propylene oxide, 1,2-butane oxide, 2-methyl-1,2-butane oxide, 2,3-butane oxide, tetrahydrofuran, epichlorohydrin, hexane oxide, styrene oxide, cyclohexene oxide, or other polymerizable oxiranes, or a mixture of any two or more thereof.
[0009] Various polyether carbonate manufacturing processes have been previously described. Polyether carbonates can be in processes such as those described in U.S. Patent Nos. 6,762,278, 7,977,501, and 9,062,156, in which carbon dioxide and orixanes are polymerized using a double metal cyanide catalyst complex, such as a zinc hexacyanocobaltate complex. Alternatively, polyether carbonates can be polymerized in the presence of certain coordination catalysts described in WO2010 / 028362, WO2010 / 071505, and WO2012 / 071505, or in the presence of double metal coordination catalysts described in U.S. Patent No. 9,006,347, WO2014 / 184578, and WO2016 / 012786. Polyether carbonates can be made in a semi-batch process in the presence of double metal cyanide catalyst complexes, as described in WO2018 / 089568.
[0010] The polyether polycarbonates may have a carbonate content of, for example, at least 0.5%, at least 5%, at least 10%, at least 20%, or at least 30% by weight based on the weight of the polymer. The carbonate content may be up to about 40% by weight. The carbonate content is conveniently measured using NMR methods such as those described in U.S. Patent No. 9,062,156.
[0011] The polyether carbonate may or may not have terminal hydroxyl groups. If the polyether carbonate has terminal hydroxyl groups, it may have, for example, 1 to 8, 1 to 4, or 2 to 4 terminal hydroxyl groups. The polyether carbonate may have, for example, a number average molecular weight (measured by gel permeation chromatography) of 250 to 12,000, 500 to 8,000, 1000 to 8,000, or 1000 to 6000 g / mol. If the polyether carbonate has hydroxyl groups, it may have a hydroxyl equivalent weight of at least 125, at least 250, at least 400, at least 500, at least 700, or at least 900, and up to 6,000, up to 3000, up to 2500, or up to 2000 grams / equivalent.
[0012] The polyether carbonate is a liquid at the process temperatures described below, and preferably also at 22°C.
[0013] The cyclic alkylene carbonate is a compound (or a mixture of two or more thereof) which, in some embodiments, has the following structure: [ka] wherein each R is independently hydrogen, alkyl (e.g., C1-C4 alkyl, etc.), or halogen-substituted alkyl (preferably having 1-4 carbon atoms), provided that two R groups may together form a divalent group that forms a ring containing the carbon atoms to which the R groups are attached in the aforementioned structure. The alkylene carbonate in some embodiments is ethylene carbonate, propylene carbonate, or a mixture thereof.
[0014] The polyether carbonate may contain, for example, 0.25 to 25 weight percent alkylene carbonate, based on the combined weight of the polyether carbonate and the alkylene carbonate. In certain embodiments, the amount may be at least 0.5%, at least 1%, or at least 2%, and may be up to 15%, up to 10%, up to 7.5%, or up to 5%. The alkylene carbonate may be an impurity formed during the production of the polyether carbonate. For example, an alkylene carbonate by-product is often formed when carbon dioxide is copolymerized with an alkylene oxide, such as ethylene oxide or propylene oxide (to form ethylene carbonate or propylene carbonate, respectively).
[0015] Examples of useful solid (under the conditions of the contacting step) sorbents include alumina, magnesium silicate, molecular sieves (including various aluminosilicate materials such as natural and synthetic zeolites), silica gel, various clays (kaolin, montmorillonite, bentonite, etc.), and organic polymers, particularly crosslinked porous polymers. Such sorbents are conveniently used in the form of particulate solids.
[0016] The absorbent is preferably a porous material. The porous absorbent may have pores with an average pore size, for example, of at least 1 nm, at least 2 nm, at least 5 nm, at least 10 nm, or at least 20 nm, up to 200 nm, up to 100 nm, up to 50 nm, or up to 30 nm, as measured using a gas absorption method. The pore volume of the porous absorbent may be, for example, 0.25 to 2 mL / g. The porous absorbent may have a pore volume of, for example, 10 to 1250 m 2 / g of nitrogen BET surface area.
[0017] By the absorbent, it is meant that it does not degrade or decompose upon heating from 20° C. to the process temperature, nor does it undergo a phase transition (such as melting or transitioning from a glassy state to a rubbery state). If the absorbent is porous, it retains its porous structure at the process temperature.
[0018] Particularly useful absorbents include crosslinked polymer beads, including styrene-divinylbenzene copolymer beads, crosslinked polyolefins, or crosslinked acrylic monomer beads. The polymer beads can be lightly crosslinked "gel" type resin beads, such as those described in U.S. Pat. Nos. 4,419,245, 4,564,644, and 5,231,115, so-called "mesoporous" polymer beads, which may have an average pore size of about 2 nm to 50 nm, or highly crosslinked "macroporous" resin beads, such as those described in U.S. Pat. Nos. 4,221,871, 4,224,415, 4,256,840, 4,501,826, and 6,323,249, and U.S. Published Patent Application No. 2005-0261384. The macroporous resin beads can have an average pore size of, for example, 20 nm to 200 nm. The polymer beads may not be functionalized and therefore lack ion exchange capacity. They may have particle diameters, for example, in the range of 0.05 to 2.5 mm, particularly 250 to 1250 μm. Suitable polymer bead absorbents are sold under the trade names Amberlyst™ and Dowex™ by DuPont de Nemours, Inc. (DuPont, Wilmington, Delaware USA).
[0019] In a particularly preferred embodiment, the absorbent is one or more ion exchange resins or ion exchange membranes. Ion exchange resins include crosslinked polymer beads functionalized with acid or base functional groups that provide cation and anion exchange capacities, respectively, as described in the previous paragraph. Useful cation exchange resins include the so-called strong acid types, which contain strong acid functional groups, such as sulfonic or phosphonic acid groups, which are generally combined (before use) with counterions (cations), such as hydrogen, sodium, potassium, or potassium. Other useful cation exchange resins are the so-called weak acid resins, which contain weak acid functional groups, such as carboxylic acid groups, which may also be combined with counterions before use. Useful anion exchange resins include the so-called strong base and weak base types. The functional groups of the strong base types are usually quaternary ammonium or quaternary phosphonium groups (which combine with counter anions, such as hydroxide or halide), whereas the functional groups of the weak base types are usually non-quaternized primary, secondary, or tertiary amino or phosphine groups. The ion exchange resin may be of the gel type, but is preferably porous as described above. Thus, mesoporous and / or macroporous types are preferred. The ion exchange resin may have an ion exchange capacity of, for example, 0.5 to 5 equivalents / L. Examples of useful commercially available ion exchange resins include those sold by Dow-DuPont under the trade names Amberlyst™, Amberlite™, and Dowex™, and those sold by Purolite Americas under the trade name Purolite®.
[0020] In addition, chelating resins are crosslinked polymer beads having, for example, aminophosphonic acid, amidoxime, aminodiacetic acid, bis-picolylamine, thiourea, or isothiouronium functional groups. They may have particle sizes and ion exchange capacities as described above for ion exchange resins, and may have porosity as previously described. Suitable products are sold under the trade names Amberlite™, Dowex™, and Purolite™.
[0021] Ion exchange membranes are polymeric films functionalized with one or more strong acids, weak acids, strong bases, weak bases, and / or chelating groups, as described above. They may have ion exchange capacities similar to those described above for ion exchange resins, and porosity as previously described.
[0022] Among the useful molecular sieves are those commonly designated as 3A molecular sieves (having an approximate chemical formula of 2 / 3K2O·1 / 3Na2O·Al2O3·2SiO2·9 / 2H2O), 4A molecular sieve (having an approximate chemical formula of Na2O·Al2O3·2SiO2·9 / 2H2O), molecular sieve 5A (having an approximate chemical formula of 0.7CaO·0.30Na2O·Al2O3·2.0SiO2·4.5H2O), 5A molecular sieve (a calcium aluminosilicate with an effective pore diameter of 0.5 nm), 10X molecular sieve (having an approximate chemical formula of 4 / 5CaO·1 / 5Na2O·Al2O3·(2.8±0.2)SiO2·(6-7)H2O), 13X molecular sieve (Na 86 [(AlO2) 86 (SiO2) 106 There are various aluminosilicate materials with average pore sizes of 2 nm or greater, such as the 13X-AS molecular sieve, which has the approximate chemical formula of 1H·H2O, where n is a positive number, the 13X-AS molecular sieve, and the Cu-13X molecular sieve.
[0023] The alkylene carbonate is removed from the polyether carbonate by contacting the polyether carbonate containing the alkylene carbonate with a solid absorbent at a temperature of 30 to 150°C. The temperature can be at least 45°C, at least 50°C, or at least 60°C, and is preferably no more than 100°C, no more than 90°C, or no more than 85°C. A particularly preferred temperature range is 60 to 85°C. At these temperatures, the alkylene carbonate is effectively removed within a reasonable contact time and there is minimal, if any, degradation of the polyether carbonate and the absorbent. Within the aforementioned range, the temperature is selected such that the polyether carbonate is liquid.
[0024] The contacting is preferably carried out by mixing, for example by stirring the mixture of absorbent and polyether carbonate and / or by passing the polyether carbonate through the absorbent in contact with the absorbent. A bed of absorbent may be provided and the polyether carbonate may be passed through the bed one or more times to establish contact with the absorbent. Alternatively, the absorbent may be dispersed in the polyether carbonate and the dispersion may be ultrasonically or otherwise agitated mechanically (for example by stirring or shaking, or by passing the dispersion through a static mixture).
[0025] The amount of absorbent may be at least 1 wt.%, at least 2.5 wt.%, or at least 4 wt.%, based on the weight of the starting mixture of cyclic alkylene carbonate and polyether carbonate. While any greater amount can be used, it is generally advantageous for the amount of absorbent to be no more than 100%, no more than 50%, no more than 25%, no more than 15%, or no more than 12%, based on the aforementioned criteria. In certain embodiments, the amount of absorbent is between 4 and 12%, based on the aforementioned criteria. A larger amount of absorbent generally removes a larger amount of alkylene carbonate per unit time at a comparable operating temperature.
[0026] The contacting step may be carried out under an inert atmosphere, such as nitrogen, helium, or argon, to prevent oxidation of the polyether carbonate.
[0027] The time for which the absorbent and the polyether carbonate are in contact can be, for example, from 15 minutes to 72 hours. Generally, greater amounts of alkylene carbonate are removed with longer contact times. In some embodiments, the contact time is at least 1 hour, at least 2 hours, or at least 4 hours, and up to 48 hours or up to 24 hours.
[0028] The contact time is generally selected within the aforementioned ranges to achieve the desired reduction of the alkylene carbonate in the polyether carbonate. Generally, it is preferred to remove at least 10 wt%, at least 20 wt%, at least 30 wt%, or at least 40 wt% of the alkylene carbonate. Up to 100% of the alkylene carbonate can be removed, although in certain embodiments up to 90%, up to 85%, or up to 80% is removed.
[0029] The polyether carbonate obtained by the aforementioned process is useful in the same manner and for the same applications as the untreated polyether carbonate. It is useful as a component of thermal fluids, brakes, or other hydraulic fluids, and as a raw material for making a variety of thermoplastic and thermosetting polymers, particularly polyurethanes, which can be formed by reacting the hydroxyl-containing polyether carbonates with polyisocyanates. Among the polyurethane products that can be prepared using the polyether carbonate obtained by the aforementioned process are slabstock foams, molded foams, flexible foams, viscoelastic foams, combustion modified foams, rigid foams, elastomers, adhesives, sealants, and / or coatings. The polyurethane products can be useful in a variety of packaging applications, comfort applications (mattresses, mattress toppers, pillows, furniture, seat cushions, etc.), shock absorber applications (bumper pads, sports and medical equipment, helmet liners, etc.), insulation applications, antistatic packaging for electronic products, and noise and / or vibration damping applications (earplugs, automotive panels, etc.), and many others.
[0030] The following examples are provided to illustrate the invention, but are not intended to limit the scope of the invention. All parts and percentages are by weight unless otherwise indicated.
[0031] Examples 1 and 2 The polyether carbonate used in these and the following examples is a triol of nominal number average molecular weight of 3500 made by polymerizing a feed composition containing 2.63 wt% glycerin, 11.00 wt% ethylene oxide, 2.90 wt% carbon dioxide, and 83.47 wt% propylene oxide. It contains primarily secondary hydroxyl groups and contains residual propylene carbonate and ethylene carbonate.
[0032] In Example 1, a sample of polyether carbonate is introduced into a 20 mL scintillation vial at ambient temperature. 0.1 g of the mixture is removed, dissolved in 0.5 g of methanol, and analyzed by gas chromatography to confirm the starting alkylene carbonate concentration by comparison to a calibration curve generated using standards of known concentrations of propylene carbonate in polyether polyol. The starting alkylene carbonate concentration is approximately 3.5 wt%.
[0033] 0.25 g of strong acid type, macroporous styrene-divinylbenzene copolymer ion exchange resin beads (Amberlyst 70, DuPont) with sulfonic acid groups in the acid form and an average pore size of 22 nm are added and the resulting slurry is stirred for 48 h at 50 °C. Samples of the supernatant polyether carbonate are taken at 4, 24, and 48 h and analyzed for alkylene carbonate concentration as above.
[0034] Example 2 is carried out using the same general method, except that the temperature is 70 °C throughout. The amounts of absorbent and starting polyether carbonate / alkylene carbonate mixture and the results obtained are as shown in Table 1. [Table 1]
[0035] Strong acid ion exchange resins are effective absorbents at all temperatures tested, however, better performance is seen at higher temperatures, i.e., 70° C., as can be seen by comparing the results of Example 1 with those of Example 2.
[0036] Examples 3 to 6 Examples 3 and 4 are carried out by repeating Examples 1 and 2, but replacing the strong acid ion exchange resin with molecular sieve 13X, a synthetic zeolite in the sodium form. This material is 86 [(AlO2) 86 (SiO2) 106 It has an approximate empirical formula of ]·nH2O (where n is a variable value), a nominal pore size of approximately 10 Angstroms, and is provided in the form of a 1.4 mm diameter pellet. The results are shown in Table 2. [Table 2]
[0037] This synthetic zeolite absorbent is also effective, again with better performance seen at higher temperatures.
[0038] The effect of this absorbent concentration is evaluated by repeating Example 4 using two different levels of absorbent, as listed in Table 3. [Table 3]
[0039] These results indicate that the use of higher concentrations of absorbent results in more rapid removal of alkylene carbonate.
[0040] Examples 7 and 8 Examples 1 and 2 are repeated again, replacing the strong acid ion exchange resin with a weak base ion exchange resin. The weak base resin is a macroporous styrene-divinylbenzene copolymer functionalized with tertiary amino groups in the free base form, and is commercially available from DuPont as Amberlite™ IRA96 resin. The results are shown in Table 4. [Table 4]
[0041] Similar results as before are seen, with better performance seen at higher temperatures.
[0042] Examples 9 and 10 Examples 1 and 2 are repeated again, substituting a weak acid ion exchange resin for the strong acid ion exchange resin. The weak base resin is a macroporous crosslinked methacrylic acid copolymer containing carboxylic acid groups in the acid form, commercially available from DuPont as Amberlite™ CG50 resin. The results are shown in Table 5. [Table 5]
[0043] Similar results as before are seen, with again better performance at higher temperatures.
[0044] Examples 11 and 12 Example 2 is repeated two more times, substituting non-functionalized macroporous styrene-divinylbenzene copolymer beads for the strong acid ion exchange resin. The product has a nominal particle size of 1 mm, an average pore size of 34 Angstroms, a pore volume of 0.94 mL / g, and a pore volume of 1100 m 2 / g of surface area. It is commercially available from DuPont as Optipore™ V-503 resin. The results are shown in Table 6. [Table 6]
[0045] The macroporous copolymer beads are also effective in removing alkylene carbonates from polyethers.
Claims
1. 1. A process for removing alkylene carbonates from polyether carbonates, comprising contacting a starting polyether carbonate containing at least 0.25% by weight, based on the weight of the starting polyether carbonate, of one or more alkylene carbonates with a solid absorbent at a temperature of from 30 to 150° C., at which temperature the starting polyether carbonate is liquid, wherein the absorbent contains pores having an average pore size of at least 1 nm and up to 100 nm.
2. 2. The process of claim 1, wherein the absorbent is selected from one or more of alumina, magnesium silicate, molecular sieves, silica gel, clay, and organic polymers.
3. 3. The process of claim 1 or 2, wherein the sorbent has a pore volume of 0.25 to 2 mL / g.
4. The process of any one of claims 1 to 3, wherein the absorbent is a crosslinked porous polymer in the form of a particulate solid.
5. The process of claim 4, wherein the absorbent is a styrene-divinylbenzene copolymer, a crosslinked polyolefin, or a crosslinked acrylic polymer.
6. 5. The process of claim 3 or 4, wherein the crosslinked porous polymer is not functionalized and lacks ion exchange capacity.
7. 5. The process of claim 3 or 4, wherein the crosslinked porous polymer is an anion exchange resin.
8. 5. The process of claim 3 or 4, wherein the crosslinked porous polymer is a cation exchange resin.
9. The process of any one of claims 1 to 3, wherein the absorbent is a zeolite.
10. 10. The process of any one of claims 1 to 9, wherein the starting polyether carbonate contains 0.5 to 15 weight percent of said alkylene carbonate, based on the combined weight of polyether carbonate and alkylene carbonate.
11. The process of any one of claims 1 to 10, wherein the alkylene carbonate comprises propylene carbonate, ethylene carbonate, or both propylene carbonate and ethylene carbonate.
12. 12. The process of any one of claims 1 to 11, wherein from 40 to 100 wt. % of the alkylene carbonate is removed, based on the weight of the alkylene carbonate in the starting polyether carbonate.
13. The process according to any one of claims 1 to 12, wherein the temperature is from 60 to 85°C.
Citation Information
Patent Citations
Process for purification of polyether carbonate polyls
CN106459398A
Method for producing polyether carbonate polyol
JP2019508563A
Process for purification of polyether carbonate polyols
US20150315337A1
Method for producing polyalkylenecarbonate resin
WO2016089039A1