Aluminum alloy forged member and manufacturing method thereof

Optimized aluminum alloy composition and controlled forging processes form fine recrystallized structures to address uneven stress distribution, enhancing tensile properties and reliability in aluminum alloy members for various applications.

JP7565728B2Active Publication Date: 2024-10-11NIKKEIKIN ALUMINIUM CORE TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020150309
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-08
Publication Date
2024-10-11
Estimated Expiration
2040-09-08

AI Technical Summary

Technical Problem

Existing aluminum alloys struggle to maintain consistent microstructural control and mechanical properties, particularly in areas of significant shape change, leading to potential cracking and reduced reliability due to uneven stress distribution.

Method used

Optimized aluminum alloy composition with elements like Si, Fe, Cu, Mg, Cr, Mn, and Zr, combined with controlled forging processes to form fine recrystallized or recovery structures in high-stress areas, ensuring uniform strength and reliability.

Benefits of technology

The solution provides aluminum alloy members with enhanced tensile properties, suppressing variations in microstructure and ensuring high strength and reliability, suitable for applications in automobiles, aircraft, and high-pressure gas storage containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565728000005
    Figure 0007565728000005
  • Figure 0007565728000006
    Figure 0007565728000006
  • Figure 0007565728000007
    Figure 0007565728000007
Patent Text Reader

Abstract

To provide an aluminum alloy-made forged member that has excellent tensile characteristics and sufficiently secures strength and reliability as a whole, in which variations in microstructures and tensile characteristics are suppressed, and an efficient method for producing the same.SOLUTION: An aluminum alloy-made forged member is composed of an aluminum alloy containing Si: 0.6-1.2 mass%, Fe: 0.1-0.25 mass%, Cu: 0.3-1.1 mass%, Mg: 0.9-1.2 mass%, Cr: 0.1-0.4 mass%, Ti: more than 0 to 0.1 mass%, with the balance being Al and unavoidable impurities, with the content of Mg2Si of 1.4-1.8 mass%, the amount of excessive Si not constituting Mg2Si being 0.1-0.7 mass%. The region where maximum stress is applied during use includes recrystallized structure or recovered structure with an average particle size of 500 μm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminum alloy forged member which is required to have high strength and reliability, and to a method for manufacturing the same. [Background technology]

[0002] Aluminum has a specific gravity of about one-third that of iron, and depending on the type of alloy and manufacturing process, it can achieve extremely high strength. As a result, it has a high specific strength compared to other metals, and is therefore used to reduce the weight of automobiles, aircraft, bicycles, various storage containers, etc.

[0003] In addition, aluminum is easy to process plastically, and extrusion can produce extruded products with complex shapes, while forging can produce even more complex shapes. In other words, by performing plastic processing on high-strength aluminum alloys, it is possible to efficiently manufacture various components that require high reliability.

[0004] However, the demands on the mechanical properties of structural members are getting higher day by day, and it is becoming difficult for existing aluminum alloys to meet these demands. In particular, when an aluminum alloy part has a portion with a large shape change such as a rounded portion or a recessed portion, the portion is subjected to a large stress during use, which may lead to cracks or breakage even if the strength of the other portions is sufficiently ensured.

[0005] In contrast, for example, Patent Document 1 (Japanese Patent No. 5561846) describes an Al-Cu-Mg-Si aluminum alloy material obtained by extrusion and cold working, which contains 1.0 to 3.0% (mass%, the same applies below) of Cu, 0.4 to 1.8% of Mg, 0.2 to 1.6% of Si, and the balance being Al and impurities. In this material, rod-shaped precipitates are formed within the crystal grains of the matrix. <100> The precipitates are aligned in the

[0001] direction, the average length of the precipitates is 10 to 70 nm, the maximum length is 120 nm or less, and the number density of precipitates in the

[0001] direction measured in the observation field from the (001) plane is 500 pieces / μm 2 The proposed high-strength aluminum alloy material is characterized in that the matrix has a structure consisting of equiaxed crystal grains formed by recrystallization, the average aspect ratio (L / ST) is 1.5 to 4.0, where L is the average grain size of the crystal grains in the extrusion direction and ST is the average grain size in the thickness direction, and the tensile strength is 450 MPa or more, the yield strength is 400 MPa or more, and the elongation is 7% or more.

[0006] The high-strength aluminum alloy material described in the above Patent Document 1 is a heat-treated Al-Cu-Mg-Si high-strength aluminum alloy cold-worked material that has excellent extrusion processability, can be produced into hollow extrusion materials by porthole extrusion method, and has high strength, and in particular, the cold-worked pipe material in a pipe shape can be suitably used as a transportation equipment component such as a motorcycle structural material.

[0007] Also, in Patent Document 2 (JP 2017-43802 A), an aluminum alloy extrusion material is described, which contains, by mass%, 2.5 to 3.3% Cu, 1.3 to 2.5% Mg, 0.50 to 1.3% Ni, 0.50 to 1.5% Fe, less than 0.50% Mn, 0.15 to 0.40% Si, 0.06 to 0.20% Zr, less than 0.05% Ti, and the balance being Al and unavoidable impurities, and in a cross section, the grain size of the intermetallic compound is 20 μm or less in terms of circle equivalent diameter, and the density of the intermetallic compound having a grain size of 0.3 to 20 μm in terms of circle equivalent diameter is 5×10 3 pieces / mm 2The aluminum alloy extrusion material is characterized in that the average grain size of the subgrains is 20 μm or less in terms of circle equivalent diameter.

[0008] The aluminum alloy extrusion material of Patent Document 2 can improve the strength and creep resistance at high temperatures, for example, above 200°C, and can improve not only the strength in the extrusion direction (L direction) but also the strength in the direction perpendicular to the extrusion direction (LT direction). It also improves the creep resistance, particularly in the LT direction, and is applicable to parts of internal combustion engines and superchargers of automobiles and the like that are used in high-temperature environments. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 5561846 [Patent Document 2] JP 2017-43802 A Summary of the Invention [Problem to be solved by the invention]

[0010] In the high-strength aluminum alloy material of Patent Document 1, the tensile properties at room temperature are improved by the composition, the shape and size of precipitates, etc. In the aluminum alloy extrusion material of Patent Document 2, the strength and creep resistance at high temperatures are improved by the composition, the grain size of intermetallic compounds, and the average grain size of subgrains. However, these aluminum alloy materials do not take into consideration the variations in microstructure and mechanical properties in the entire aluminum alloy material actually obtained. In particular, when an aluminum alloy part is used, the strength and reliability of the aluminum alloy part as a whole are determined mainly by the characteristics of the region where the maximum stress is applied, and no method has been considered for achieving both structure control and high strength from this perspective.

[0011] In view of the problems in the conventional techniques as described above, an object of the present invention is to provide an aluminum alloy forged component having excellent tensile properties while fully ensuring the strength and reliability of the component as a whole, in which variations in microstructure and tensile properties are suppressed, and to provide an efficient method for manufacturing the same. [Means for solving the problem]

[0012] In order to achieve the above-mentioned object, the inventors have conducted extensive research into aluminum alloy forged components and methods for manufacturing the same, and as a result, have discovered that it is extremely effective to optimize the composition, etc. of the aluminum alloy and, when the final product shape is formed by forging or other processing, to form a fine recrystallized structure or recovered structure in the area to which the maximum stress is applied during use, thereby arriving at the present invention.

[0013] That is, the present invention provides: Si:0.6~1.2% by mass, Fe: 0.1~0.25% by mass, Cu:0.3~1.1% by mass, Mg: 0.9~1.2% by mass, Cr:0.1~0.4% by mass, Ti: more than 0 to 0.1 mass%, The balance is an aluminum alloy containing Al and unavoidable impurities, The content of Mg2Si is 1.4 to 1.8 mass%, The amount of excess Si that does not constitute the MgSi is 0.1 to 0.7 mass%, A recrystallized or recovered structure having an average grain size of 500 μm or less is formed in the area where maximum stress is applied during use. The present invention provides an aluminum alloy forged member, characterized by the above.

[0014] In the aluminum alloy forged member of the present invention, it is preferable that Mn: 0.1-0.8 mass% is further contained, and the total content of Cr and Mn is 0.1-0.9 mass%. By adding Mn and Cr in combination, Al-Fe(Mn, Cr)-Si-based dispersed particles are formed (substituting for Fe), which can suppress grain boundary migration and recrystallization during T6 treatment of high-temperature forged material. In addition, there is an effect of accumulating strain during low-temperature forging and forming a fine recrystallized structure during T6 treatment, and the crystal structure of the forged material can be controlled more effectively. In addition, the effect of trapping hydrogen atoms and suppressing hydrogen embrittlement can be expected.

[0015] The aluminum alloy forged member of the present invention preferably further contains 0.1 to 0.3 mass% Zr. Zr is finely crystallized in the metal structure as an Al-Zr intermetallic compound, suppresses grain boundary migration during T6 treatment of high-temperature forged material, and suppresses recrystallization. In addition, it accumulates strain during low-temperature forging, allowing the formation of a fine recrystallized structure.

[0016] In the aluminum alloy forged member of the present invention, the type and content of added elements are optimized for the purpose of improving tensile properties (tensile strength, 0.2% proof stress, and elongation) and controlling the structure. In addition, by controlling the Mg2Si content, high strength and excellent ductility are achieved at the same time, and by specifying the Cr content (the total of the Cr content and the Mn content, or the Zr content, as necessary), it is designed to facilitate the formation of a fine recrystallized structure or a recovered structure after forging.

[0017] In addition, since a recrystallized structure or a recovered structure having an average grain size of 500 μm or less is formed in the region where the maximum stress is applied during use, the aluminum alloy forged component as a whole has high strength and reliability. Here, the "region where the maximum stress is applied during use" can be determined by carrying out a load test or the like on the finally obtained aluminum alloy forged component. Basically, the "region where the maximum stress is applied during use" is the region where deformation or cracks first occur in a tensile test, a bending test, a load test, or the like. In addition, when it is difficult to actually carry out a load test or the like, the stress applied during use may be evaluated using various simulations.

[0018] In addition, the aluminum alloy forged member of the present invention preferably has tensile properties of tensile strength: 350 MPa or more and proof stress: 310 MPa or more. Since the lightweight aluminum alloy forged member has these tensile properties, it can be suitably used as a member for manufacturing parts for automobiles, aircraft, bicycles, various high-pressure gas storage containers, etc.

[0019] Furthermore, in the aluminum alloy forged member of the present invention, not only is a desired shape imparted to the aluminum alloy member by forging, but the microstructure obtained by the forging can be a fine recrystallized structure or a recovered structure. Furthermore, the aluminum alloy forged member can be efficiently manufactured by various conventionally known forging methods.

[0020] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: A method for producing an aluminum alloy forged member by forging an aluminum alloy billet, comprising the steps of: The aluminum alloy billet is Si:0.6~1.2% by mass, Fe: 0.1~0.25% by mass, Cu:0.3~1.1% by mass, Mg: 0.9~1.2% by mass, Cr:0.1~0.4% by mass, Ti: more than 0 to 0.1 mass%, The balance is an aluminum alloy containing Al and unavoidable impurities, The content of Mg2Si is 1.4 to 1.8 mass%, The amount of excess Si that does not constitute the MgSi is 0.1 to 0.7 mass%, The forging temperature is set to room temperature to 350°C or 450 to 550°C. The present invention also provides a method for producing an aluminum alloy forged member, comprising the steps of:

[0021] In the method for producing an aluminum alloy forged member of the present invention, it is preferable that the aluminum alloy further contains 0.1 to 0.8 mass % of Mn, and the total content of the Cr and Mn is 0.1 to 0.9 mass %.

[0022] In the method for producing an aluminum alloy forged member of the present invention, it is preferable that the aluminum alloy further contains 0.1 to 0.3 mass % of Zr.

[0023] In the manufacturing method of the aluminum alloy forged member of the present invention, the additive elements are designed to give the aluminum alloy forged member high strength and excellent ductility, and to facilitate the formation of fine recrystallized structure or recovery structure after forging. In addition, by strictly excluding the processing temperature at which the recrystallized grains are inevitably coarsened by the forging process even with the alloy design, the formation of coarse recrystallized grains in the aluminum alloy forged member is suppressed. More specifically, by setting the forging temperature at room temperature to 350°C, strain is left during the forging process, and a fine recrystallized structure can be formed after the subsequent solution treatment. In addition, by setting the forging temperature at 450 to 550°C, recovery during the forging process is promoted, and by not leaving strain, a fine recovery structure can be formed after the subsequent solution treatment.

[0024] In addition, in the manufacturing method of the aluminum alloy forged member of the present invention, not only can the aluminum alloy member be given any shape by forging, but also the forging temperature can be easily set to room temperature to 350°C or 450 to 550°C, and the microstructure obtained by the forging can be a fine recrystallized structure or a recovered structure. Here, by forging the extruded member, the aluminum alloy member can be efficiently manufactured.

[0025] In addition, in the method for producing an aluminum alloy forged member of the present invention, a homogenization heat treatment step of maintaining the aluminum alloy billet at 520 to 570°C before the forging process; A solution treatment process in which the forged member obtained by the forging process is maintained at 520 to 575 ° C.; and an artificial aging step of holding the solution-treated member obtained in the solution treatment step at 170 to 195°C for 6 to 15 hours. It is preferable that the time from the solution treatment step to the artificial aging step (natural aging time) is 100 minutes or less.

[0026] By undergoing these heat treatment processes, it is possible to impart high tensile properties to the aluminum alloy forged member obtained by precipitation strengthening. Particularly important is the time from the solution treatment process to the artificial aging process (time of natural aging), and by setting this to 100 minutes or less, it is possible to form favorable clusters composed of Mg and Si that contribute to improving the strength of the aluminum alloy. On the other hand, if the time of natural aging is longer than 100 minutes, Si-rich clusters are formed, making it difficult to improve the strength of the aluminum alloy forged member.

[0027] In the method for producing an aluminum alloy forged member of the present invention, it is preferable to form a recrystallized structure or a recovered structure having an average grain size of 500 μm or less in an area to which maximum stress is applied during use. It is also preferable to set the tensile properties of the aluminum alloy forged member to tensile strength of 350 MPa or more and proof stress of 310 MPa or more. By imparting these tensile properties to the obtained aluminum alloy forged member, it can be suitably used as a member for producing parts for automobiles, aircraft, bicycles, various high-pressure gas storage containers, etc. Effect of the Invention

[0028] According to the present invention, it is possible to provide an aluminum alloy forged component having excellent tensile properties while fully ensuring the strength and reliability of the component as a whole, in which variations in microstructure and tensile properties are suppressed, and an efficient method for manufacturing the same. [Brief description of the drawings]

[0029] [Figure 1] 1 is a schematic cross-sectional view showing an example of an aluminum alloy forged member of the present invention (a metal cap for a hydrogen container). [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of an aluminum alloy forged member of the present invention (a valve for a hydrogen container). [Diagram 3] 1 is an example of a process diagram relating to a manufacturing method of an aluminum alloy forged member of the present invention. [Figure 4] 1 is an optical microscope photograph of a cross section of an aluminum alloy forged member obtained in Example 8. [Diagram 5] 1 is a graph showing the relationship between the average grain size of recrystallized grains and the forging temperature for the aluminum alloy forged members obtained in Examples 7 to 10 and Comparative Example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Representative embodiments of the aluminum alloy forged member and its manufacturing method according to the present invention will be described in detail below with reference to the drawings, but the present invention is not limited to these. In the following description, the same or equivalent parts are given the same reference numerals, and duplicated descriptions may be omitted. In addition, since the drawings are intended to conceptually explain the present invention, the dimensions of each component shown and their ratios may differ from the actual ones.

[0031] 1. Aluminum alloy forged parts The aluminum alloy forged member of the present invention is a member for obtaining various aluminum alloy forged parts, and is characterized in that the composition of the aluminum alloy is optimized and a fine recrystallized structure or recovered structure is formed in the area to which the maximum stress is applied during use when the aluminum alloy is processed to obtain a final product shape, thereby imparting high strength and reliability to the aluminum alloy forged part. The composition, structure, mechanical properties, etc. of the aluminum alloy forged member will be described in detail below.

[0032] (1) Composition The aluminum alloy used for the aluminum alloy member is an aluminum alloy containing Si: 0.6-1.2 mass%, Fe: 0.1-0.25 mass%, Cu: 0.3-1.1 mass%, Mg: 0.9-1.2 mass%, Cr: 0.1-0.4 mass%, Ti: more than 0-0.1 mass%, and the balance being Al and unavoidable impurities. In addition, Mn and Zr can be added as optional additive elements. Each component element will be described below.

[0033] (1-1) Essential additive elements Si:0.6~1.2% by mass Si forms Mg-Si precipitates together with Mg, and has the effect of enhancing mechanical strength and fatigue strength. If the Si content is less than 0.6 mass%, the solid solution strengthening and age hardening ability are insufficient, and the mechanical strength and fatigue strength required for aluminum alloy members cannot be obtained. On the other hand, if the Si content is more than 1.2 mass%, the corrosion resistance and hydrogen embrittlement resistance are reduced. By imparting high strength and excellent hydrogen embrittlement resistance to aluminum alloy forged members, they can also be suitably used as aluminum alloy forged members for obtaining various hydrogen container members (mouthpieces, valves, etc.). In addition, if the Si content is more than 1.2 mass%, coarse crystallized particles and precipitates are formed, which may reduce ductility and workability.

[0034] Fe:0.10~0.25% by mass Fe is an effective element for forming Al-Fe(Mn, Cr)-Si dispersed particles. It suppresses the recrystallization of Al and contributes to improving strength, but if it is less than 0.10 mass%, this effect is not fully obtained. However, if added in excess, it reduces the precipitates and precipitated Si, Mn, and Cr that contribute to strength, and forms coarse intermetallic compounds, reducing strength, so the upper limit of the amount added is set to 0.25 mass%.

[0035] Cu:0.3~1.1% by mass Cu forms Al-Cu precipitates and has the effect of increasing mechanical strength and fatigue strength. If the Cu content is less than 0.3 mass%, these effects cannot be fully obtained, and the mechanical strength and fatigue strength required for aluminum alloy forged members cannot be obtained. On the other hand, if the Cu content exceeds 1.1 mass%, there is a risk of reducing corrosion resistance.

[0036] Mg:0.9~1.2% by mass Mg forms Mg-Si precipitates together with Si, and has the effect of increasing mechanical strength and fatigue strength. This effect is significant at 0.9 mass% or more, but even if added in excess of 1.2 mass%, little contribution to hardness can be expected, and there is a risk of forming coarse intermetallic compounds that become the starting point of fracture, reducing mechanical strength and ductility.

[0037] Cr:0.1~0.4% by mass Cr crystallizes finely in the metal structure as an Al-Cr intermetallic compound, suppressing grain boundary migration and recrystallization during T6 treatment of high-temperature forged material. It also accumulates strain during low-temperature forging, forming a fine recrystallized structure. It is also expected to trap hydrogen atoms and suppress hydrogen embrittlement. This effect is particularly noticeable at 0.1 mass% or more, but if it is contained in excess of 0.4 mass%, it forms undesirable compounds that impair ductility.

[0038] Ti: more than 0~0.1% by mass Ti refines the cast structure and prevents casting cracks.

[0039] (1-2) Optional additive elements Mn:0.1~0.8% by mass By adding Mn and Cr in combination, dispersed particles of Al-Fe(Mn, Cr)-Si system are formed (substituting for Fe), which suppresses grain boundary migration during T6 treatment of high-temperature forged material and suppresses recrystallization. In addition, there is an effect of accumulating strain during low-temperature forging and forming a fine recrystallized structure, and it is possible to more effectively control the crystal structure of the forged material. In addition, it is expected to have an effect of trapping hydrogen atoms and suppressing hydrogen embrittlement. This effect is particularly remarkable when it is 0.1 mass% or more, but if it is contained in excess of 0.8 mass%, it increases the quenching sensitivity and inhibits the solution treatment property (if quenching is delayed, the strength decreases). For these reasons, the total amount of Cr and Mn is preferably 0.1 to 0.9 wt%.

[0040] Zr:0.1~0.3% by mass Zr crystallizes finely in the metal structure as an Al-Zr intermetallic compound, suppressing grain boundary migration and recrystallization during T6 treatment of high-temperature forged material. It also accumulates strain during low-temperature forging, forming a fine recrystallized structure. This effect is particularly noticeable at 0.1% by mass or more, but if it is contained in excess of 0.4% by mass, it forms a material compound that inhibits ductility, etc.

[0041] (1-3) Other conditions regarding composition Mg2Si content: 1.4-1.8 mass% By setting the Mg2Si content to 1.4 mass% or more, the strength required for the aluminum alloy forged member can be achieved by precipitation strengthening, while by setting the Mg2Si content to 1.8 mass% or less, the decrease in ductility of the aluminum alloy forged member can be suppressed.

[0042] Excess Si content: 0.1 to 0.7 mass% By setting the amount of excess Si to 0.1 mass % or more, the effect of precipitation strengthening can be sufficiently obtained. Furthermore, by setting the amount of excess Si to 0.7 mass % or less, deterioration of corrosion resistance and hydrogen embrittlement resistance can be suppressed.

[0043] (2) Organization The aluminum alloy forged member of the present invention is characterized in that a recrystallized structure or recovered structure having an average grain size of 500 μm or less is formed in the region to which maximum stress is applied during use.

[0044] As described above, the "region where maximum stress is applied during use" can be determined by performing load tests and simulations simulating the usage conditions on the aluminum alloy forged parts finally obtained from the aluminum alloy forged members, and examples of representative aluminum alloy forged members and the region where maximum stress is applied during use are shown in Figures 1 and 2. Here, these figures show schematic cross-sectional views of aluminum alloy forged members 2 having different shapes, with Figure 1 being suitable for manufacturing a nozzle for a hydrogen container and Figure 2 being suitable for manufacturing a valve for a hydrogen container. In addition, the "region where maximum stress is applied during use" in the aluminum alloy forged member 2 when it has the final product shape is surrounded by a dotted line.

[0045] Here, the "area to which maximum stress is applied during use" differs depending on the aluminum alloy forged part in question, and there are a wide variety of types of aluminum alloy forged parts, but it is sufficient to identify the area in question for the aluminum alloy forged part and compare its positional relationship with the aluminum alloy forged member 2. The aluminum alloy forged member 2 that has been forged often has a shape as close as possible to the aluminum alloy forged part, and so comparison of the positional relationship can be easily performed.

[0046] The method for determining the average grain size is not particularly limited as long as it does not impair the effects of the present invention, and various conventionally known methods may be used. For example, the aluminum alloy forged member 2 may be cut at an arbitrary cross section, the obtained cross section sample may be observed with an optical microscope or a scanning electron microscope, and the average grain size of the matrix grains may be calculated. In this case, for example, the grain size may be measured by the intersection method. Alternatively, the grain size may be measured with a backscattered electron diffraction measurement device (SEM-EBSD) attached to a scanning electron microscope. The observation area for determining the average grain size depends on the aluminum alloy forged member 2 and the "region to which the maximum stress is applied during use", but an accurate value can be obtained by determining the observation area so that at least 20 grains are to be measured. In addition, depending on the observation method, the cross section sample may be subjected to mechanical polishing, buff polishing, electrolytic polishing, etching, etc.

[0047] The strength and reliability of an aluminum alloy forged part are basically determined by the mechanical properties of the "region where maximum stress is applied during use," and if coarse recrystallized grains are present in that region, the strength and reliability of the aluminum alloy forged part as a whole cannot be guaranteed. In contrast, in the aluminum alloy forged part obtained from the aluminum alloy forged member 2 of the present invention, fine recrystallized grains or recovered structures are formed in that region, and the strength and reliability required for various aluminum alloy forged parts can be fully realized.

[0048] The aluminum alloy forged member 2 preferably has tensile properties of tensile strength: 350 MPa or more and proof stress: 310 MPa or more. The elongation is preferably 5% or more, and more preferably 8% or more. Since the lightweight aluminum alloy forged member 2 has these tensile properties, it can be suitably used as a member for manufacturing parts for automobiles, aircraft, bicycles, various high-pressure gas storage containers, etc.

[0049] Furthermore, the aluminum alloy forged member 2 can be formed into any shape by forging, and the microstructure obtained by the forging can be a fine recrystallized structure or a recovered structure. By forging the extruded member, the aluminum alloy forged member 2 can be efficiently manufactured.

[0050] 2. Manufacturing method of aluminum alloy forged components The method for manufacturing an aluminum alloy forged member of the present invention involves forging an aluminum alloy material to be forged (extruded bar or cast material), and its greatest feature is the combination of the aluminum alloy composition and the forging temperature.

[0051] Specifically, the aluminum alloy forged material contains 0.6-1.2 mass% Si, 0.1-0.25 mass% Fe, 0.3-1.1 mass% Cu, 0.9-1.2 mass% Mg, 0.1-0.4 mass% Cr, and more than 0-0.1 mass% Ti, with the balance being Al and unavoidable impurities. The content of Mg2Si is 1.4-1.8 mass%, and the amount of excess Si that does not constitute the Mg2Si is 0.1-0.7 mass%.

[0052] The aluminum alloy forged material preferably further contains 0.1-0.8 mass% Mn and the total content of Cr and Mn is 0.1-0.9 mass%. The aluminum alloy forged material preferably further contains 0.1-0.3 mass% Zr.

[0053] In addition, the forging temperature is room temperature to 350°C or 450 to 550°C, and by performing forging in either of these two temperature ranges on the aluminum alloy forged material having the above compositional characteristics, the formation of coarse recrystallized grains can be suppressed extremely effectively. More specifically, when the total of the Mn content and the Cr content is 0.1% by mass or more and less than 0.4% by mass, it is preferable to form fine recrystallized grains by setting the forging temperature at a relatively low temperature of room temperature to 350°C. On the other hand, when the total of the Mn content and the Cr content is 0.4% by mass or more and 0.9% by mass or less, it is preferable to form a fine recovery structure by setting the forging temperature at a relatively high temperature of 450 to 550°C. In addition, when an extruded bar is used for the aluminum alloy forged material, the extrusion temperature is also preferably room temperature to 350°C or 450 to 550°C.

[0054] An example of a process flow of the method for manufacturing an aluminum alloy forged member of the present invention is shown in Fig. 3. The manufacturing process includes a homogenization heat treatment process (S01) for an aluminum alloy forged material, a forging process (S02), a solution treatment process (S03) for the forged member, and an artificial aging process (S04) for the solution treatment member. Each process will be described below.

[0055] (1) Casting In order to obtain an aluminum alloy forging material, a molten aluminum alloy having the above composition is prepared, and then the molten aluminum alloy is subjected to a conventionally known degassing treatment and filtration treatment (such as a filtration method using a filter such as a ceramic foam filter or a porous tube filter). The effect of the degassing treatment can be measured by a known hydrogen quantification method such as the Lansley method or the LECO method, and the effect of removing inclusions by the filtration treatment can be measured, for example, by a fracture surface observation method.

[0056] Thereafter, a rod hardener (Al-Ti-B alloy) is added before the mold as necessary for the purpose of refining the structure, and a cylindrical ingot (hereinafter referred to as a "billet") is obtained by DC continuous casting or the like. Here, the DC continuous casting method is a casting method in which molten metal is introduced through a launder into a quench casting mold whose inner wall surface is water-cooled, the molten metal is rapidly solidified on the inner wall surface of the quench casting mold, and the billet immediately after solidification is successively drawn downward or to the side, and further cooled by injecting cooling water onto the billet, and is known as a casting method for aluminum alloys with excellent productivity.

[0057] (2) Homogenization heat treatment process (S01) The resulting billet is preferably subjected to homogenization treatment, which is preferably performed at a temperature of 520 to 570° C., and more preferably maintained at that temperature for 2 hours or more.

[0058] (3) Forging process (S02) The forging step (S02) is a step for forging an aluminum alloy billet or an aluminum alloy extrusion obtained by casting and heat treatment to give it a shape. In the method for producing an aluminum alloy forged member of the present invention, an aluminum alloy designed to form a fine recrystallized structure or a recovered structure after forging is used, so that the formation of coarse recrystallized grains can be suppressed.

[0059] By forging, not only can any shape be given to an aluminum alloy member, but also the processing temperature can be easily set to room temperature to 350°C or 450 to 550°C, and the microstructure obtained by the processing can be a fine recrystallized structure or a recovered structure. Here, by performing forging on an extruded member, an aluminum alloy forged member can be efficiently manufactured. Also, when the aluminum alloy forged member is large or when the aluminum alloy forged part has a complex shape, any shape can be efficiently given by setting the processing temperature to 450 to 550°C. On the other hand, when the aluminum alloy forged member is not so large, the processing temperature can be set to room temperature to 350°C, which can reduce the energy consumption required for heating and improve the dimensional accuracy.

[0060] The processing conditions other than the processing temperature used in the forging process are not particularly limited as long as they do not impair the effects of the present invention, and various processing conditions known in the art can be used. Although the strain rate applied during forging is not constant, a desired structure can be formed by appropriately selecting the composition of the aluminum alloy and the forging temperature.

[0061] (4) Solution treatment process (S03) The solution treatment is a process in which the forged aluminum alloy member is held at 520 to 575°C. The holding time is preferably 90 minutes or more, more preferably 120 minutes or more. This treatment allows the Mg-Si compounds and Al-Cu compounds precipitated during cooling after the homogenization heat treatment and forging to be dissolved in the matrix.

[0062] Next, the solution-treated aluminum alloy forged component is quenched in water or warm water (preferably water at 70°C or less), thereby making it possible to suppress reprecipitation of elements such as Mg, Si, and Cu that have been dissolved in the parent phase during the solution treatment.

[0063] (5) Artificial aging process (S04) By subjecting a solution-treated aluminum alloy forged member to artificial aging, elements such as Mg, Si, and Cu dissolved in the matrix can be precipitated as intermetallic compounds that contribute to mechanical strength. Specifically, by holding the solution-treated member at 170 to 195°C for 6 to 15 hours, the intermetallic compounds can be sufficiently precipitated.

[0064] The time from the solution treatment step (S03) to the artificial aging step (S04) (natural aging time) is preferably 100 minutes or less. By setting the natural aging time to 100 minutes or less, it is possible to form preferable clusters that are mainly composed of Mg and Si and contribute to improving the strength of the aluminum alloy. On the other hand, if the natural aging time is longer than 100 minutes, Si-rich clusters are formed, making it difficult to improve the strength of the aluminum alloy forged member.

[0065] (6) Cutting, etc. An aluminum alloy forged part having a desired shape can be obtained by subjecting the aluminum alloy forged part that has been subjected to the artificial aging process (S04) to appropriate cutting or other processes as necessary. Here, the formation of coarse recrystallized grains is suppressed in the aluminum alloy forged part, and the "region to which maximum stress is applied during use" of the aluminum alloy forged part can be made into a fine recrystallized or recovered structure with an average grain size of 500 μm or less. Here, the region removed by cutting or other processes may contain coarse recrystallized grains, since it does not affect the mechanical properties of the aluminum alloy forged part.

[0066] By optimizing the composition and structure of an aluminum alloy forged member, and in particular by controlling the structure of the "region to which the maximum stress is applied during use," it is possible to impart tensile properties of tensile strength: 350 MPa or more and proof stress: 310 MPa or more to the aluminum alloy forged member. As a result, aluminum alloy forged parts obtained from the aluminum alloy forged member can be suitably used as members for manufacturing parts for automobiles, aircraft, bicycles, various high-pressure gas storage containers, etc.

[0067] Representative embodiments of the present invention have been described above, but the present invention is not limited to these, and various design modifications are possible, all of which are included in the technical scope of the present invention. EXAMPLES

[0068] Example An aluminum alloy billet having the composition shown in Table 1 was obtained by DC continuous casting. Table 1 also shows the "total Mn content and Cr content," the "Mg2Si content," and the "excess Si content."

[0069] [Table 1]

[0070] Next, the aluminum alloy billet was subjected to homogenization heat treatment, and then extrusion processing was performed, and the resulting extruded material was subjected to forging processing. In Example 14, the cast bar was forged. Here, the aluminum alloy forged member had the shape shown in FIG. 1. The conditions of the homogenization heat treatment, extrusion processing, and forging processing are shown in Table 2. As shown in Table 2, in the examples, the extrusion processing and forging processing temperatures were room temperature to 350°C, or 450 to 550°C.

[0071] Next, the obtained forged materials (Examples 1 to 17) were subjected to solution treatment, natural aging, and artificial aging under the treatment conditions shown in Table 2 to obtain the aluminum alloy forged members of the present invention.

[0072] [Table 2]

[0073] Each aluminum alloy forged member obtained in Examples 1 to 17 was cut, mirror-polished and etched to prepare a cross-sectional observation sample, and the structure was observed by an optical microscope. When a fine recrystallized structure or a recovered structure with an average grain size of 500 μm or less was formed in the "region to which the maximum stress is applied during use", it was marked with an O, and when a coarse recrystallized structure with an average grain size of more than 500 μm was formed, it was marked with an X. The results are shown in Table 2. The structure observation region corresponds to the region to which the maximum stress is applied shown in FIG. 1. Here, the average grain size of the crystal grains was measured from an observation image of a region containing at least 20 crystal grains. For the aluminum alloy forged members obtained in Examples 7 to 10, the measured values ​​of the average grain size obtained are shown in Table 2. In addition, as a representative example of a cross-sectional observation sample, an optical microscope photograph of the aluminum alloy forged member obtained in Example 8 is shown in FIG. 4.

[0074] From the results shown in Table 2, a fine recrystallized structure or a recovered structure is formed in the "region where maximum stress is applied during use" of the aluminum alloy forged members obtained in Examples 1 to 17. That is, in all cases, the formation of coarse recrystallized grains with an average grain size of 500 μm or more is effectively suppressed. Here, a fine recovered structure is formed in the "region where maximum stress is applied during use" of the aluminum alloy forged members obtained in Examples 10 and 12 to 15, and a fine recrystallized structure is formed in the "region where maximum stress is applied during use" of the aluminum alloy forged members obtained in the other Examples.

[0075] The tensile properties of each aluminum alloy member obtained in Examples 1 to 17 are shown in Table 2. The tensile test specimens used were No. 14A test specimens specified in JIS Z 2241, and the test specimens were cut out so that the "region to which the maximum stress is applied during use" was included in the parallel portion. The tensile speed was in accordance with JIS Z 2241, and was 2 mm / min up to 0.2% yield strength and 5 mm / min after 0.2% yield strength. From the results shown in Table 2, the aluminum alloy members obtained as examples had a tensile strength of 350 MPa or more.

[0076] The aluminum alloy part obtained in Example 14, in which the amount of Cu added was increased, had extremely high strength, with a tensile strength of 410 MPa and a 0.2% yield strength of 375 MPa. The aluminum alloy part obtained in Example 15, in which the amount of Zr added was increased, also showed extremely good tensile properties, with an elongation of 14%, a tensile strength of 398 MPa and a 0.2% yield strength of 371 MPa.

[0077] Here, the 0.2% proof stress of the aluminum alloy member obtained in Example 6 is low at 294 MPa, but this is due to the low artificial aging temperature (168° C.).

[0078] In order to confirm the effect of the time from solution treatment to artificial aging on the mechanical properties (tensile properties) of aluminum alloy parts, aluminum alloy parts (extruded bars) were obtained using the compositions shown in Table 3 and the manufacturing conditions shown in Table 4. Here, the time from solution treatment to artificial aging was 50 minutes for sample 1 and 1500 minutes for sample 2, and the other manufacturing conditions and compositions were the same.

[0079] [Table 3]

[0080] [Table 4]

[0081] Similarly to the aluminum alloy forged members obtained in Examples 1 to 17, the aluminum alloy forged members obtained as Samples 1 and 2 were subjected to structural observation and tensile testing. The obtained results are shown in Table 4. There is no significant difference in the microstructure between Samples 1 and 2, but Sample 2, which had a long time from solution treatment to artificial aging of 1500 minutes, had a significant decrease in 0.2% yield strength, indicating that management of the time from solution treatment to artificial aging is important in order to obtain aluminum alloy forged members with excellent strength.

[0082] Comparative Example Aluminum alloy members were obtained in the same manner as in the Examples, except that the compositions and processing conditions shown as Comparative Examples in Tables 1 and 2 were used. The tensile properties and microstructures were evaluated in the same manner as in the Examples, and the results are shown in Table 2.

[0083] The composition of the aluminum alloy used in the comparative example satisfies the composition range of the aluminum alloy of the present invention, but the forging process is performed at 425° C. As a result, a coarse recrystallized structure with an average grain size of 700 μm is formed in the “region to which the maximum stress is applied during use.”

[0084] FIG. 5 is a graph comparing the average grain size of the "region where maximum stress is applied during use" for the aluminum alloy members obtained in Examples 7 to 10 and Comparative Example, which have the same composition. The main difference in the processing conditions is the forging temperature, and it can be seen that when the temperature is 350°C or less and 450°C or more, coarsening of the grain size is suppressed. More specifically, in Examples 7 to 9, where the forging temperature is in the range of room temperature to 350°C, a fine recrystallized structure is obtained, and in Example 10, where the forging temperature is in the range of 450 to 550°C, a fine recovered structure is obtained. In contrast, in the Comparative Example, where the forging temperature is 425°C, the grains are most coarsened. [Explanation of symbols]

[0085] 2. Aluminum alloy forged components.

Claims

1. Si: 0.6 to 1.2% by mass, Fe: 0.1 to 0.25% by mass, Cu: 0.3 to 1.1% by mass, Mg: 0.9 to 1.2% by mass, Cr: 0.1 to 0.4% by mass, Ti: more than 0 to 0.1 mass %, The balance is an aluminum alloy containing Al and unavoidable impurities, Mg 2 The Si content is 1.4 to 1.8 mass %, The Mg 2 The amount of excess Si that does not constitute Si is 0.1 to 0.7 mass %, A recrystallized or recovered structure having an average grain size of 500 μm or less is formed in the region where the maximum stress is applied during use. An aluminum alloy forged component characterized by the above.

2. Further, Mn: 0.1 to 0.8 mass %, The total content of the Cr and the Mn is 0.1 to 0.9 mass %; 2. The aluminum alloy forged member according to claim 1,

3. Further, Zr: 0.1 to 0.3 mass % is contained; 3. The aluminum alloy forged member according to claim 1 or 2,

4. Tensile strength: 350 MPa or more, proof stress: 310 MPa or more; 4. The aluminum alloy forged member according to claim 1, wherein the aluminum alloy forged member has a diameter of 100 mm or less.

5. A method for producing an aluminum alloy forged member by forging an aluminum alloy billet, comprising the steps of: The aluminum alloy billet is Si: 0.6 to 1.2% by mass, Fe: 0.1 to 0.25% by mass, Cu: 0.3 to 1.1% by mass, Mg: 0.9 to 1.2% by mass, Cr: 0.1 to 0.4% by mass, Ti: more than 0 to 0.1 mass %, The balance is an aluminum alloy containing Al and unavoidable impurities, Mg 2 The Si content is 1.4 to 1.8 mass %, The Mg 2 The amount of excess Si that does not constitute Si is 0.1 to 0.7 mass %, The forging temperature is from room temperature to 350°C or from 450°C to 550°C; A method for manufacturing an aluminum alloy forged member, comprising the steps of:

6. The aluminum alloy further contains Mn: 0.1 to 0.8 mass %, The total content of the Cr and the Mn is 0.1 to 0.9 mass %; 6. The method for producing an aluminum alloy forged member according to claim 5, further comprising the steps of:

7. The aluminum alloy further contains Zr: 0.1 to 0.3 mass %; 7. The method for producing an aluminum alloy forged member according to claim 5 or 6, characterized in that

8. a homogenization heat treatment step of holding the aluminum alloy billet at 520 to 570°C before the forging process; A solution treatment process in which the forged member obtained by the forging process is maintained at 520 to 575 ° C.; an artificial aging step of holding the solution treated member obtained in the solution treatment step at 170 to 195°C for 6 to 15 hours; The time from the solution treatment step to the artificial aging step (natural aging time) is 100 minutes or less; The method for producing an aluminum alloy forged member according to any one of claims 5 to 7, characterized in that

9. Forming a recrystallized or restored structure having an average grain size of 500 μm or less in an area where maximum stress is applied during use; The method for producing an aluminum alloy forged member according to any one of claims 5 to 8, characterized in that

10. The tensile properties of the aluminum alloy forged member are tensile strength: 350 MPa or more and yield strength: 310 MPa or more; 10. The method for producing an aluminum alloy forged member according to claim 5, wherein

Citation Information

Patent Citations

  • Code conversion circuit

    JP1980061846A

  • Heat treatment method of al-mg-si aluminum alloy forged material

    JP1994065695A

  • Aluminum alloy for forging

    JP1996003675A

  • Automobile chassis parts and its manufacturing method

    JP2008163445A

  • HIGH-TOUGHNESS Al ALLOY FORGING MATERIAL, AND METHOD FOR PRODUCING THE SAME

    JP2012001756A