Glass Fiber Composite

A fiber-reinforced polypropylene composite with controlled polypropylene properties and metallocene catalysts reduces emissions and enhances stiffness and heat resistance, addressing the issues of commercial composites.

JP7566040B2Active Publication Date: 2024-10-11BOREALIS AG
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022568747
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-22
Filing Date
2021-05-17
Publication Date
2024-10-11
Estimated Expiration
2041-05-17

AI Technical Summary

Technical Problem

Commercial glass fiber reinforced polypropylene composites have high emissions due to oligomers produced in the polymerization process, compromising their stiffness and heat deformation resistance.

Method used

A fiber-reinforced polypropylene composite comprising 59 to 90% polypropylene, 9 to 40% glass fibers, and 0.05 to 5% compatibilizer, with polypropylene having a specific melting temperature, low molecular weight distribution, and produced without visbreaking, using metallocene catalysts to minimize emissions.

Benefits of technology

The composite achieves low emissions, high stiffness, and improved heat deformation resistance, with properties optimized by precise control of polypropylene characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566040000001
    Figure 0007566040000001
  • Figure 0007566040000002
    Figure 0007566040000002
  • Figure 0007566040000003
    Figure 0007566040000003
Patent Text Reader

Abstract

A fiber reinforced composite comprising polypropylene having a high melting temperature and narrow molecular weight distribution.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber reinforced composite comprising polypropylene and glass fibers, the manufacture of said fiber reinforced composite, and articles comprising said fiber reinforced composite. [Background technology]

[0002] Polypropylene is a material used in a wide variety of technical fields, and reinforced polypropylene has gained particular relevance in fields that previously relied exclusively on non-polymeric materials, especially metals. One specific example of reinforced polypropylene is glass fiber reinforced polypropylene composites. Such materials allow tailoring of the composite properties by selecting the type of polypropylene, the amount of glass fiber, and sometimes by selecting the type of compatibilizer used. Thus, today, glass fiber reinforced polypropylene composites are well established materials for applications requiring high stiffness, heat distortion resistance, and impact resistance, such as automobile parts with load-bearing functions in the engine compartment, support parts for polymer body panels, washing machine, and dishwasher parts. However, one disadvantage of commercially available fiber reinforced polypropylene composites is their rather high emissions, caused by the rather high amount of oligomers obtained as by-products in the polymerization process. Summary of the Invention [Problem to be solved by the invention]

[0003] Therefore, there is a need for a glass fiber reinforced polypropylene composite that is stiff, has a fairly high heat distortion resistance, and has low emissions. [Means for solving the problem]

[0004] The finding of the present invention is that a fiber reinforced polypropylene composite must comprise a polypropylene having a low molecular weight distribution and a fairly high melting temperature. Preferably, the polypropylene is not visbroken, i.e., has not been modified in a radical induced process to reduce the molecular weight.

[0005] Accordingly, the present invention provides a fiber reinforced polypropylene composite, comprising: (a) 59 to 90% by weight of polypropylene based on the fiber-reinforced composite material; (b) 9.0 to 40% by weight of glass fiber based on the fiber-reinforced composite material; (c) 0.05 to 5.0% by weight of a compatibilizer based on the fiber-reinforced composite material; Including, moreover, the total amount of polypropylene, glass fiber, and compatibilizer in the fiber-reinforced composite is at least 95% by weight; Furthermore, The polypropylene is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; and (iv) in the range of 0.10 to 0.90%; 13 2,1-site defects determined by C-NMR spectroscopy has.

[0006] In particular, the present invention relates to a fiber reinforced polypropylene composite, comprising: (a) 59 to 90% by weight of a propylene homopolymer based on the fiber reinforced composite material; (b) 9.0 to 40% by weight of glass fiber based on the fiber-reinforced composite material; (c) 0.05 to 5.0% by weight of a compatibilizer based on the fiber-reinforced composite material; (d) 0.1 to 5.0% by weight of an additive based on the fiber-reinforced composite material; It consists of: moreover, The propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; and (iv) in the range of 0.1 to 0.90% 13 2,1-site defects determined by C-NMR spectroscopy has.

[0007] Preferred embodiments of the fibre reinforced composite are defined in the dependent claims of the present invention.

[0008] The present invention further provides a process for producing a fiber-reinforced composite as defined in the present invention, comprising the steps of: (a) polypropylene, (b) glass fibre; (c) a compatibilizer, and (d) Optionally, additives and extruding them to obtain the fiber-reinforced composite.

[0009] Preferably, the polypropylene according to the invention is obtained by polymerizing propylene and optionally ethylene, more preferably only propylene, in the presence of a metallocene catalyst having formula (I) [ka] In formula (I), each R1 are independently the same or different and are hydrogen or a linear or branched C1-C6 alkyl group, and at least one R 1 is not hydrogen, R' is C1 to C 10 a hydrocarbyl group, preferably a C1 to C4 hydrocarbyl group, more preferably a methyl group; X is independently a hydrogen atom, a halogen atom, a C1 to C6 alkoxy group, a C1 to C6 alkyl group, a phenyl group, or a benzyl group.

[0010] Most preferably, X is a chlorine, benzyl or methyl group. Preferably, both X groups are the same. The most preferred options are two chlorides (chlorines), two methyls or two benzyl groups, especially two chlorides.

[0011] Furthermore, the present invention relates to an article, preferably an automotive article, comprising at least 90% by weight of the fiber reinforced composite material according to the invention.

[0012] The present invention will now be described in more detail.

[0013] Fiber Reinforced Composites The present invention relates to a fiber reinforced composite comprising polypropylene, glass fibers and a compatibilizer. The fiber reinforced composite is understood as known in the art, that is, the polypropylene forms a continuous phase in which the glass fibers are embedded. When the glass fibers are short glass fibers, the fibers are dispersed in the polypropylene, which acts as the continuous phase. The compatibilizer improves the adhesion between the non-polar polypropylene and the polar glass fibers.

[0014] Accordingly, the present invention provides a fiber reinforced polypropylene composite, comprising: (a) 59 to 90% by weight of polypropylene based on the fiber-reinforced composite material; (b) 9.0 to 40% by weight of glass fiber based on the fiber-reinforced composite material; (c) 0.05 to 5.0% by weight of a compatibilizer based on the fiber-reinforced composite material; and It relates to a fiber reinforced polypropylene composite, wherein the total amount of polypropylene, glass fiber and compatibilizer in said fiber reinforced composite is at least 95% by weight, preferably at least 98% by weight.

[0015] Besides the three components, typical additives, eg added to extend the life of polypropylene, may be present, namely antioxidants (see definition of additives below).

[0016] Thus, in a preferred embodiment, the fiber reinforced composite according to the invention preferably comprises: (a) 59 to 90% by weight of polypropylene based on the fiber-reinforced composite material; (b) 9.0 to 40% by weight of glass fiber based on the fiber-reinforced composite material; (c) 0.05 to 5.0% by weight of a compatibilizer based on the fiber-reinforced composite material; (d) 0.1 to 5.0% by weight of an additive based on the fiber-reinforced composite material; and The total amount of polypropylene, glass fiber, compatibilizer and additives in the fiber reinforced composite is at least 98% by weight, preferably in the range of 98 to 100% by weight, for example in the range of 99 to 100% by weight.

[0017] The fiber reinforced composition preferably does not contain elastomeric polymers. Elastomeric polymers are understood as polymers that do not form a continuous phase in the polypropylene. In other words, the elastomeric polymers are dispersed in the polypropylene, i.e. they form inclusions (inclusions) in the polypropylene. Polymers that contain elastomeric polymers as inclusions as a second phase are in contrast called heterophasic and are preferably not part of the present invention. The presence of a second phase or so-called inclusions is visible, for example, by high-resolution microscopy such as electron microscopy or atomic force microscopy, or by dynamic mechanical thermal analysis (DMTA). In particular, in DMTA, the presence of a multiphase structure can be identified by the presence of at least two distinct glass transition temperatures.

[0018] Therefore, in a particular embodiment, the fiber reinforced composite according to the invention preferably comprises: (a) 59 to 90% by weight of polypropylene based on the fiber-reinforced composite material; (b) 9.0 to 40% by weight of glass fiber based on the fiber-reinforced composite material; (c) 0.05 to 5.0% by weight of a compatibilizer based on the fiber-reinforced composite material; (d) 0.1 to 5.0% by weight of an additive based on the fiber-reinforced composite material; It consists of:

[0019] The fibre-reinforced composites according to the invention are characterised, inter alia, by low emissions, and therefore preferably have a VOC (volatile organic compounds) value, determined according to VDA 278 October 2011, of less than 12 μg / g, more preferably in the range 0.5-10 μg / g, even more preferably in the range 0.8-8.0 μg / g.

[0020] In addition or instead of the requirements of the previous paragraph, the fibre reinforced composite has a FOG (low volatile or condensable organic compounds) value determined according to VDA 278 October 2011 of less than 75 μg / g, more preferably in the range of 10-70 μg / g, even more preferably in the range of 15-65 μg / g.

[0021] It is further preferred that the fibre reinforced composite has a tensile modulus, determined at 1 mm / min according to ISO 527-1 for injection moulded articles, in the range of 3500-7000 MPa, more preferably in the range of 3800-6500 MPa, for example in the range of 4000-6300 MPa. The fibre reinforced composite also preferably has an elongation at break in the same tensile test of more than 2.0%, more preferably in the range of 2.1-10.0%, for example in the range of 2.2-8.0%.

[0022] In addition to or instead of the requirements of the preceding paragraph, the fiber-reinforced composite material has a thermal conductivity of 30.0 to 75.0 kJ / m 2More preferably, the range is 35.0 to 70.0 kJ / m 2 In the range of, for example, 40.0 to 65.0 kJ / m 2 The Charpy impact strength, determined at 23°C in accordance with ISO 179-1eU, is in the range of

[0023] In a very specific embodiment, the fibre reinforced composite has a heat deflection temperature (HDT) determined at a load of 0.46 MPa according to ISO 75B in the range of 146-160°C, more preferably in the range of 148-158°C, for example in the range of 150-156°C.

[0024] polypropylene An essential component of the present invention is the polypropylene, which must be carefully selected to achieve the desired properties. Thus, the polypropylene of the present invention requires a specific melting temperature and a fairly narrow molecular weight distribution (MWD).

[0025] Furthermore, the polypropylene according to the present invention is produced in the presence of a specific metallocene catalyst, which is defined in more detail below. In contrast to polypropylene produced in the presence of a Ziegler-Natta catalyst, polypropylene produced in the presence of a metallocene catalyst is characterized by the misinsertion of monomer units during the polymerization process. Therefore, the polypropylene according to the present invention has a certain amount of 2,1-position defects. That is, the polypropylene according to the present invention has a certain amount of 2,1-position defects in the range of 0.10 to 0.90%, more preferably in the range of 0.15 to 0.80%. 13 It has a 2,1 positional defect as determined by C-NMR spectroscopy. Therefore, the polypropylene according to the present invention has (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; and (iv) in the range of 0.10 to 0.90%; 13 2,1-site defects, as determined by C-NMR spectroscopy has.

[0026] More preferably, the polypropylene according to the present invention is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; and (iv) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy has.

[0027] It is especially preferred that the polypropylene is monophasic, i.e. does not contain polymer components that are not miscible with each other, as in the case of heterophasic propylene copolymers. As mentioned above, in contrast to monophasic systems, heterophasic systems contain a continuous polymer phase, such as polypropylene, in which further immiscible polymers, such as elastomeric polymers, are dispersed as inclusions. The above polypropylene systems containing a polypropylene matrix and inclusions as a second polymer phase are in contrast called heterophasic and are preferably not part of the present invention. The presence of a second polymer phase or so-called inclusions is visible, for example, by high-resolution microscopy, such as electron microscopy or atomic force microscopy, or by dynamic mechanical thermal analysis (DMTA). In particular, in DMTA, the presence of a multiphase structure can be identified by the presence of at least two distinct glass transition temperatures.

[0028] Therefore, the polypropylene according to the invention preferably has (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; and (iv) in the range of 0.10 to 0.90%; 13 2,1-site defects determined by C-NMR spectroscopy It is a single-phase polypropylene having the following properties:

[0029] Even more preferably, the polypropylene according to the invention has (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; and (iv) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy It is a single-phase polypropylene having the following properties:

[0030] It is especially preferred that said single-phase polypropylene is a propylene homopolymer, which by definition cannot be heterophasic since it contains only polymer chains of propylene, in other words, the propylene homopolymer according to the invention is always a single-phase polymer.

[0031] Therefore, the single-phase polypropylene according to the invention (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; and (iii) in the range of 0.10 to 0.90%; 13 2,1-site defects, as determined by C-NMR spectroscopy It is preferable that the propylene homopolymer has the formula:

[0032] Even more preferably, the single-phase polypropylene is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; and (iii) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy It is a propylene homopolymer having the formula:

[0033] As mentioned above, it is particularly preferred that the single-phase polypropylene is a propylene homopolymer. Thus, the single-phase polypropylene being a propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) in the range of 0.10 to 0.90%; 13 2,1-site defects as determined by C-NMR spectroscopy, and (iii) a molecular weight distribution (MWD) determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; has.

[0034] Even more preferably, the single-phase polypropylene is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) in the range of 0.15 to 0.80%; 13 2,1-site defects as determined by C-NMR spectroscopy, and (iii) a molecular weight distribution (MWD) determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; It is a propylene homopolymer having the formula:

[0035] More preferably, the polypropylene according to the present invention is characterized by a very low cold xylene solubles (XCS) content, which cannot be achieved with Ziegler-Natta catalysts.Thus, in a preferred embodiment, the polypropylene according to the present invention, more preferably the single-phase polypropylene, has a cold xylene solubles (XCS) percentage measured according to ISO 16152 (25°C) in the range of 0.05 to 1.00 wt%, more preferably in the range of 0.10 to 0.90 wt%, for example in the range of 0.15 to 0.85 wt%.

[0036] Therefore, (a) the polypropylene, more preferably the single-phase polypropylene, (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) a xylene cold solubles (XCS) percentage, measured in accordance with ISO 16152 (25°C), in the range of 0.05 to 1.00 weight percent; and (vi) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; or (b) the polypropylene, more preferably the single-phase polypropylene, (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) in the range of 0.10 to 0.90%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iv) a xylene cold solubles (XCS) percentage, measured in accordance with ISO 16152 (25°C), in the range of 0.05 to 1.00 weight percent; and (v) Molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0. It is preferred that the compound has the formula:

[0037] Even more preferably, (a) The polypropylene according to the present invention, preferably the single-phase polypropylene, (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) a xylene cold solubles (XCS) percentage, measured in accordance with ISO 16152 (25°C), in the range of 0.05 to 1.00 weight percent; and (iv) a molecular weight distribution (MWD) determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; or (b) The polypropylene according to the present invention, preferably the single-phase polypropylene, (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) 0.5% by weight or less 13comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iv) a xylene cold solubles (XCS) percentage, measured in accordance with ISO 16152 (25°C), in the range of 0.05 to 1.00 weight percent; and (v) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; has.

[0038] As mentioned above, it is particularly preferred that the single-phase polypropylene is a propylene homopolymer. Thus, the single-phase polypropylene being a propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) a xylene cold solubles (XCS) percentage, measured in accordance with ISO 16152 (25°C), in the range of 0.10 to 0.90 weight percent; and (iii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; has.

[0039] Even more preferably, the propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) in the range of 0.10 to 0.90%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iii) a xylene cold solubles (XCS) percentage, measured in accordance with ISO 16152 (25°C), in the range of 0.10 to 0.90 weight percent; and (iv) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; has.

[0040] In a highly preferred embodiment, the present invention comprises: (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) a xylene cold solubles (XCS) percentage, measured in accordance with ISO 16152 (25°C), in the range of 0.10 to 0.90 weight percent; and (iii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; The present invention relates to a propylene homopolymer having the formula:

[0041] Therefore, the propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iii) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.10 to 0.90% by weight; (iv) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; It is particularly preferred that

[0042] In addition, the polypropylene of the present invention preferably has a certain degree of molecular weight. Therefore, the polypropylene of the present invention preferably has a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO1133 in the range of 5.0 to 500 g / 10 min, preferably in the range of 5.5 to 300 g / 10 min, more preferably in the range of 6.0 to 250 g / 10 min.

[0043] Therefore, the polypropylene, more preferably the single-phase polypropylene, (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.05 to 1.00 weight percent; (iv) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 500 g / 10 min; and (v) Molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0. It is preferred that the compound has the formula:

[0044] In a particular embodiment, the polypropylene according to the present invention, preferably the single-phase polypropylene, (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iv) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.05 to 1.00 weight percent; (v) a melt flow rate MFR2 (230°C, 2.16 kg) measured in accordance with ISO 1133 in the range of 5.0 to 500 g / 10 min; and (vi) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; has.

[0045] As mentioned above, it is particularly preferred that the single-phase polypropylene is a propylene homopolymer. Therefore, the single-phase polypropylene being a propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.10 to 0.90% by weight; (iii) a melt flow rate MFR2 (230°C, 2.16 kg) measured in accordance with ISO 1133 in the range of 5.0 to 500 g / 10 min; and (iv) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; It is preferred that the compound has the formula:

[0046] Therefore, the propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iii) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.10 to 0.90% by weight; (iv) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 500 g / 10 min; and (v) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; It is particularly preferred that

[0047] As mentioned above, the polypropylene of the present invention is preferably produced in the presence of a specific metallocene catalyst. Thus, in a preferred embodiment, said polypropylene, more preferably single-phase polypropylene, is produced by polymerizing propylene and optionally ethylene in the presence of a metallocene catalyst having the formula (I): [ka] In formula (I), each R 1 are independently the same or different and are hydrogen or a linear or branched C1-C6 alkyl group, and at least one R 1 is not hydrogen, R' is C1 to C 10 a hydrocarbyl group, preferably a C1 to C4 hydrocarbyl group, more preferably a methyl group; X is independently a hydrogen atom, a halogen atom, a C1 to C6 alkoxy group, a C1 to C6 alkyl group, a phenyl group, or a benzyl group.

[0048] In the following, the term "Formula (I)" refers to the metallocene catalyst defined in the previous paragraph.

[0049] Thus, the polypropylene, more preferably the single-phase polypropylene, (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) in the range of 0.10 to 0.90%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iv) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.05 to 1.00 weight percent; (v) a melt flow rate MFR2 (230°C, 2.16 kg) measured in accordance with ISO 1133 in the range of 5.0 to 500 g / 10 min; and (vi) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; having It is especially preferred that this polypropylene, more preferably a single-phase polypropylene, is prepared by polymerizing propylene and optionally ethylene in the presence of a metallocene catalyst having formula (I) as defined above.

[0050] Even more preferably, the polypropylene according to the invention, preferably the single-phase polypropylene, (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iv) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.05 to 1.00 weight percent; (v) a melt flow rate MFR2 (230°C, 2.16 kg) measured in accordance with ISO 1133 in the range of 5.0 to 500 g / 10 min; and (vi) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; having This polypropylene, more preferably the single-phase polypropylene, is prepared by polymerizing propylene and optionally ethylene in the presence of a metallocene catalyst having formula (I) as defined above.

[0051] In certain preferred embodiments, the single-phase polypropylene is a propylene homopolymer. Thus, the propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iii) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.10 to 0.90% by weight; (iv) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 500 g / 10 min; and (v) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; having Preferably, the propylene homopolymer is prepared by polymerizing propylene in the presence of a metallocene catalyst having formula (I) as defined above.

[0052] In addition, it is preferred that the polypropylene is not visbroken. Visbreaking, or controlled degradation by radical-induced processes initiated by peroxides or other radical generators, is usually used to increase the melt flow rate and thus reduce the molecular weight and narrow the molecular weight distribution. However, the degradation of the polymer, i.e., visbreaking, is obtained by the use of peroxides. Visbreaking and the use of peroxides can increase the emission values ​​(in terms of VOCs or FOGs) due to undesirable side reactions that lead to an increase in the amount of oligomers. Furthermore, the presence of peroxides can lead to undesirable discoloration of the polypropylene. In other words, whether a polypropylene is visbroken or not can be identified by the decomposition products of peroxides or other radical generators and the discoloration of the polypropylene. Therefore, in the following, whenever the terms "non-visbroken" or "not visbroken" are used, it is understood that the melt flow rate, molecular weight and molecular weight distribution of the polypropylene have not been changed by chemical or physical treatments, and further, that the polypropylene does not contain the decomposition products of peroxides or other radical generators.

[0053] Thus, the polypropylene is not visbroken, and (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) in the range of 0.10 to 0.90%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iv) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.05 to 1.00 weight percent; (v) a melt flow rate MFR2 (230°C, 2.16 kg) measured in accordance with ISO 1133 in the range of 5.0 to 500 g / 10 min; and (vi) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; having Optionally, this polypropylene is preferably prepared by polymerizing propylene and optionally ethylene in the presence of a metallocene catalyst having formula (I) as defined above.

[0054] Even more preferably, the polypropylene in the preceding paragraph is a single-phase polypropylene that is not visbroken.

[0055] Even more preferably, the single-phase polypropylene according to the invention has (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) 0.5% by weight or less 13 comonomer content as determined by C-NMR spectroscopy, the comonomer being ethylene; (iii) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iv) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.05 to 1.00 weight percent; (v) a melt flow rate MFR2 (230°C, 2.16 kg) measured in accordance with ISO 1133 in the range of 5.0 to 500 g / 10 min; and (vi) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; a non-visbroken single-phase polypropylene having This non-visbroken, single-phase polypropylene is prepared by polymerizing propylene and optionally ethylene in the presence of a metallocene catalyst having formula (I) defined above.

[0056] More preferably, the single-phase polypropylene according to the present invention is a non-visbroken propylene homopolymer. Thus, the non-visbroken propylene homopolymer according to the present invention is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iii) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.10 to 0.90% by weight; (iv) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 500 g / 10 min; and (v) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; having Optionally and preferably, the non-visbroken propylene homopolymer has been prepared by polymerizing propylene in the presence of a metallocene catalyst having formula (I) as defined above.

[0057] The polymerization of polypropylene will be described in detail below.

[0058] The polypropylene according to the invention can be produced in one reactor or in a reactor cascade of two or more reactors, preferably two reactors. Several polymerization processes suitable for producing the polypropylene according to the invention are known in the prior art. They comprise at least one polymerization stage, the polymerization typically being carried out in solution, slurry, bulk or gas phase. Typically, the polymerization process comprises additional polymerization stages or reactors. In one particular embodiment, the process comprises at least one bulk reactor zone and optionally at least one gas phase reactor zone, each zone comprising at least one reactor, all reactors being arranged in a cascade. In one particularly preferred embodiment, the polymerization process comprises at least one bulk reactor and optionally at least one gas phase reactor arranged next to the bulk reactor. The process may further comprise a pre-reactor and a post-reactor. The pre-reactor typically comprises a pre-polymerization reactor. In this type of process, the use of higher polymerization temperatures is preferred to achieve certain properties of the polymer. Typical temperatures in these processes are above 70° C., preferably above 75° C. The higher polymerization temperatures mentioned above can be applied in some or all reactors of the reactor cascade.

[0059] A preferred multi-stage process is the "loop gas phase" process, such as that developed by Borealis (known as BORSTAR® technology), described in patent documents such as EP 0 887 379, WO 92 / 12182, WO 2004 / 000899, WO 2004 / 111095, WO 99 / 24478, WO 99 / 24479 or WO 00 / 68315. A further suitable slurry-gas phase process is the Spheripol® process from Basell.

[0060] As mentioned above, the polypropylene according to the invention is obtained in particular by a polymerization process using a metallocene catalyst having the formula (I) [ka] In formula (I), each R 1 are independently the same or different and are hydrogen or a linear or branched C1-C6 alkyl group, and at least one R 1 is not hydrogen, R' is C1 to C 10 a hydrocarbyl group, preferably a C1 to C4 hydrocarbyl group, more preferably a methyl group; X is independently a hydrogen atom, a halogen atom, a C1 to C6 alkoxy group, a C1 to C6 alkyl group, a phenyl group, or a benzyl group.

[0061] Most preferably, X is a chlorine, benzyl or methyl group. Preferably, both X groups are the same. The most preferred options are two chlorides, two methyls or two benzyl groups, especially two chlorides.

[0062] Specific preferred metallocene catalysts of the present invention include rac-anti-dimethylsilanediyl[2-methyl-4,8-bis-(4'-tert-butylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethyl-phenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride, rac-anti-dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-di-tert-butyl-phenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride or their corresponding zirconium dimethyl analogues.

[0063] The most preferred catalyst is rac-anti-dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-indacen-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride. [ka]

[0064] The ligands required to form the complexes and thus the catalysts of the present invention can be synthesized by any process, and an organic chemist skilled in the art will be able to devise various synthesis protocols to produce the required ligand materials. For example, WO 2007 / 116034 discloses the necessary chemical reactions. Synthesis protocols can also be found generally in WO 2002 / 02576, WO 2011 / 135004, WO 2012 / 084961, WO 2012 / 001052, WO 2011 / 076780, WO 2015 / 158790 and WO 2018 / 122134. In particular, reference is made to WO 2019 / 179959, in which the most preferred catalysts of the present invention are described. The Examples section also provides sufficient direction for the skilled artisan.

[0065] Cocatalyst To form an active catalytic species, it is usually necessary to employ a cocatalyst, as is well known in the art.

[0066] According to the present invention, a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst is used in combination with the metallocene catalyst complex defined above.

[0067] The aluminoxane cocatalyst can be of formula (III). [ka] In formula (III), n is usually 6 to 20, and R has the following meaning.

[0068] Aluminoxanes are formed by partial hydrolysis of organoaluminum compounds, such as compounds of formulae AlR3, AlR2Y and Al2R3Y3, where R is, for example, C1-C 10 -alkyl, preferably C1-C5-alkyl, or C3-C 10 -Cycloalkyl, C7-C 12 -arylalkyl or C7-C 12 -alkylaryl and / or phenyl or naphthyl, and Y is hydrogen, halogen, preferably chlorine or bromine, or C1-C 10 -alkoxy, preferably methoxy or ethoxy. The oxygen-containing aluminoxanes obtained are generally not pure compounds but are mixtures of oligomers of formula (III).

[0069] A preferred aluminoxane is methylaluminoxane (MAO). The aluminoxanes used as cocatalysts according to the present invention are not pure compounds due to the manner of their preparation, so the molar concentrations of the aluminoxane solutions hereinafter are based on their aluminum content.

[0070] According to the present invention, a boron-containing cocatalyst can also be used in place of the aluminoxane cocatalyst, or the aluminoxane cocatalyst can be used in combination with a boron-containing cocatalyst.

[0071] Those skilled in the art will appreciate that when a boron-based cocatalyst is used, it is common for the complex to be pre-alkylated by reaction with an aluminum alkyl compound such as TIBA. This procedure is well known and any suitable aluminum alkyl can be used, for example Al(C1-C6 alkyl)3. Preferred aluminum alkyl compounds are triethylaluminum, triisobutylaluminum, triisohexylaluminum, tri-n-octylaluminum and triisooctylaluminum.

[0072] Alternatively, when a borate (boron ate complex) cocatalyst is used, the metallocene catalyst complex can be an alkylated version thereof, ie, for example, a dimethyl or dibenzyl metallocene catalyst complex can be used.

[0073] Boron-based cocatalysts of interest include those of formula (IV): BY3(IV) In formula (IV), Y is the same or different and is a hydrogen atom, an alkyl group having 1 to about 20 carbon atoms, an aryl group having 6 to about 15 carbon atoms, an alkylaryl having 1 to 10 carbon atoms in the alkyl radical and 6 to 20 carbon atoms in the aryl radical, an arylalkyl, a haloalkyl or a haloaryl, or a fluorine, chlorine, bromine or iodine. Preferred examples of Y are methyl, propyl, isopropyl, isobutyl or trifluoromethyl, unsaturated groups such as aryl or haloaryl, for example phenyl, tolyl, benzyl group, p-fluorophenyl, 3,5-difluorophenyl, pentachlorophenyl, pentafluorophenyl, 3,4,5-trifluorophenyl and 3,5-di(trifluoromethyl)phenyl. Preferred choices are trifluoroborane, triphenylborane, tris(4-fluorophenyl)borane, tris(3,5-difluorophenyl)borane, tris(4-fluoromethylphenyl)borane, tris(2,4,6-trifluorophenyl)borane, tris(pentafluorophenyl)borane, tris(tolyl)borane, tris(3,5-dimethyl-phenyl)borane, tris(3,5-difluorophenyl)borane and / or tris(3,4,5-trifluorophenyl)borane.

[0074] Particularly preferred is tris(pentafluorophenyl)borane.

[0075] However, it is preferred to use borate, i.e. compounds containing borate 3+ ions. Such ionic cocatalysts preferably contain non-coordinating anions such as tetrakis(pentafluorophenyl)borate and tetraphenylborate. Suitable counterions are protonated amine or aniline derivatives, such as methylammonium, anilinium, dimethylammonium, diethylammonium, N-methylanilinium, diphenylammonium, N,N-dimethylanilinium, trimethylammonium, triethylammonium, tri-n-butylammonium, methyldiphenylammonium, pyridinium, p-bromo-N,N-dimethylanilinium or p-nitro-N,N-dimethylanilinium.

[0076] Preferred ionic compounds that can be used in accordance with the present invention include the following: triethylammonium tetra(phenyl)borate, tributylammonium tetra(phenyl)borate, trimethylammonium tetra(tolyl)borate, tributylammonium tetra(tolyl)borate, tributylammonium tetra(pentafluorophenyl)borate, tripropylammonium tetra(dimethylphenyl)borate, tributylammonium tetra(trifluoromethylphenyl)borate, tributylammonium tetra(4-fluorophenyl)borate, N,N-dimethylcyclohexylammonium tetrakis(pentafluorophenyl)borate, N,N-dimethylbenzylammonium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetra(phenyl)borate, N,N-diethylanilinium tetra(phenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, N,N-di(propyl)ammonium tetrakis(pentafluorophenyl)borate, di(cyclohexyl)ammonium tetrakis(pentafluorophenyl)borate, triphenylphosphonium tetrakis(phenyl)borate), triethylphosphonium tetrakis(phenyl)borate, diphenylphosphonium tetrakis(phenyl)borate, tri(methylphenyl)phosphonium tetrakis(phenyl)borate, tri(dimethylphenyl)phosphonium tetrakis(phenyl)borate, triphenylcarbenium tetrakis(pentafluorophenyl)borate, or Ferrocenium tetrakis(pentafluorophenyl)borate).

[0077] The preferred triphenylcarbenium tetrakis(pentafluorophenyl)borate, N,N-dimethylcyclohexylammonium tetrakis(pentafluorophenyl)borate, or N,N-Dimethylbenzylammonium tetrakis(pentafluorophenyl)borate It is.

[0078] Surprisingly, it has been found that certain boron cocatalysts are particularly preferred. Thus, the preferred borates used in the present invention contain trityl ions. Thus, the use of N,N-dimethylammonium-tetrakispentafluorophenylborate and Ph3CB(PhF5)4 and analogs thereof is particularly preferred.

[0079] In accordance with the present invention, preferred cocatalysts are alumoxanes, more preferably methylalumoxanes, combinations of alumoxanes with Al alkyls, boron or borate cocatalysts, and combinations of alumoxanes with boron-based cocatalysts.

[0080] Suitable amounts of cocatalyst are well known to those skilled in the art. The molar ratio of boron to the metal ion of the metallocene may range from 0.5:1 to 10:1 mol / mol, preferably from 1:1 to 10:1, especially from 1:1 to 5:1 mol / mol. The molar ratio of Al in the aluminoxane to the metal ion of the metallocene may be in the range of 1:1 to 2000:1 mol / mol, preferably 10:1 to 1000:1, more preferably 50:1 to 500:1 mol / mol.

[0081] The catalyst can be used in supported or unsupported form, preferably in supported form.The particulate support material used is preferably an organic or inorganic material, such as silica, alumina or zirconia, or a mixed oxide, such as silica-alumina, in particular silica, alumina or silica-alumina.The use of silica supports is preferred.Those skilled in the art are aware of the procedures required for supporting metallocene catalysts.

[0082] Especially preferably, the support is a porous material, so that the complex may be loaded into the pores of the support using processes similar to those described, for example, in WO 94 / 14856 (Mobil), WO 95 / 12622 (Borealis) and WO 2006 / 097497.

[0083] The average particle size of the silica support may typically be between 10 and 100 μm, however, it has been found that particular advantages are obtained when the support has an average particle size between 15 and 80 μm, preferably between 18 and 50 μm. The average pore size of the silica support can be in the range of 10 to 100 nm, and the pore volume can be 1 to 3 mL / g.

[0084] Examples of suitable support materials are, for example, ES757 manufactured and sold by PQ Corporation, Sylopol 948 manufactured and sold by Grace, or SUNSPERA DM-L-303 silica manufactured by AGC Si-Tech Co. The support can be optionally calcined prior to use in the catalyst preparation to obtain optimal silanol group content.

[0085] The use of these carriers is routine in the art.

[0086] Glass fiber The second essential component in the fiber reinforced composite is glass fiber. The glass fiber can be any type of glass fiber, such as long glass fiber or short glass fiber. However, it is particularly preferred that the glass fiber is short glass fiber, also known as cut glass fiber or chopped glass strand.

[0087] The short glass fibers used in the fiber reinforced composite material preferably have an average fiber length in the range of 2.0 to 10.0 mm, more preferably in the range of 2.0 to 8.0 mm, and even more preferably in the range of 2.0 to 5.0 mm.

[0088] It is further preferable that the short glass fibers used in the fiber reinforced composite material have an average diameter of preferably 5 to 20 μm, more preferably 8 to 18 μm, and even more preferably 8 to 15 μm.

[0089] Preferably, the short glass fibers have an aspect ratio, defined as the ratio between the average fiber length and the average fiber diameter, of 150 to 600, preferably 200 to 500, more preferably 250 to 400. The aspect ratio is the relationship between the average length and the average diameter of the fibers.

[0090] Compatibilizer A further component present in the fibre reinforced composite is a compatibiliser, also called a coupling agent or adhesion promoter. As mentioned above, the compatibiliser improves the adhesion between the non-polar polypropylene and the polar glass fibres.

[0091] The compatibilizer according to the present invention is preferably a polar modified polypropylene. Polar modified polypropylene, such as a polar modified propylene homopolymer or a polar modified copolymer, is highly compatible with the polypropylene of the fiber reinforced composite according to the present invention.

[0092] In terms of structure, the polar modified polypropylene is preferably selected from graft copolymers or block copolymers.

[0093] In this context, polar modified polypropylenes containing groups derived from polar compounds, in particular polar compounds selected from the group consisting of acid anhydrides, carboxylic acids, carboxylic acid derivatives, primary and secondary amines, hydroxyl compounds, oxazolines and epoxides, as well as ionic compounds, are preferred.

[0094] Specific examples of the polar compounds include unsaturated cyclic anhydrides and their aliphatic diesters and dibasic acid derivatives. In particular, maleic anhydride and maleic acid C1-C 10 Linear and branched dialkyl, C1-C fumarate 10 Linear and branched dialkyl, itaconic anhydride, itaconic acid C1-C 10 Compounds selected from linear and branched dialkyl esters, maleic acid, fumaric acid, itaconic acid and mixtures thereof can be used.

[0095] In certain preferred embodiments of the present invention, the polar modified polypropylene is maleic anhydride grafted polypropylene, which is either a propylene-ethylene copolymer or a propylene homopolymer. It is especially preferred that the polar modified polypropylene is maleic anhydride grafted polypropylene, which is a propylene homopolymer.

[0096] Polar modified polypropylene, especially maleic anhydride grafted polypropylene, can be prepared in a simple manner, for example by reactive extrusion of polypropylene with maleic anhydride in the presence of a free radical generator, such as an organic peroxide, as disclosed, for example, in EP-A-0 572 028.

[0097] The amount of groups derived from polar compounds in the polar modified polypropylene, for example the amount of maleic anhydride, is 0.1 to 5.0% by weight, preferably 0.5 to 4.0% by weight, more preferably 0.5 to 3.0% by weight.

[0098] Preferably, the polar modified polypropylene, such as maleic anhydride grafted polypropylene, has a melt flow rate MFR2 (190°C, 2.16 kg), measured according to ISO 1133, of at least 50 g / 10 min, more preferably at least 80 g / 10 min, even more preferably in the range of 50 to 500 g / 10 min, and even more preferably in the range of 80 to 250 g / 10 min.

[0099] Additives The fiber reinforced composite of the present invention may further comprise additives. Typical additives are acid scavengers, antioxidants, colorants, light stabilizers, slip agents, anti-scratch agents, dispersants, processing aids, lubricants, pigments, etc.

[0100] Such additives are commercially available and are described, for example, in "Plastic Additives Handbook" by Hans Zweifel, 6th Edition, 2009 (pp. 1141-1190).

[0101] The additives are typically provided in the form of a masterbatch, which is a composition in which an additive or an additive mixture is dispersed in a polymer in a significant amount. The term "additive" according to the present invention therefore also includes a carrier material, in particular a polymeric carrier material, in which an "active additive" or an "active additive mixture" is dispersed.

[0102] Manufacturing process for reinforced fiber composite materials The reinforced fiber composites are manufactured as is well known in the art. Thus, the fiber reinforced composites include: (a) polypropylene, (b) glass fibre; (c) a compatibilizer, and (d) Optionally, additives and extruding the resulting fiber-reinforced composite material, Preferably, said polypropylene is prepared by polymerizing propylene and optionally ethylene in the presence of a metallocene catalyst having formula (I), preferably having formula (II).

[0103] Conventional compounding or blending equipment may be used to extrude, i.e. melt blend, the individual components of the composite, such as a Banbury mixer, a two-roll rubber mill, a Buss-co-kneader or a twin screw extruder. The fiber reinforced composite material recovered from the extruder / mixer is usually in the form of granules. These granules are then preferably further processed, for example by injection molding, to produce the composite articles and products of the invention.

[0104] It is particularly preferred that the fibre reinforced composites according to the invention are prepared by melt blending the individual components in an extruder, preferably a twin screw extruder.

[0105] In particular, the fiber reinforced composite material of the present invention is (a) feeding polypropylene, a compatibilizer, and optionally additives into an extruder, preferably a twin screw extruder; (b) melt-kneading the composition obtained in step (a) at a temperature of 200 to 270°C; (c) feeding short glass fibers into an extruder, preferably a twin screw extruder, containing the composition obtained in step (b); (d) melt-kneading the composition obtained in step (c) at a temperature of 200 to 270°C to obtain the fiber-reinforced composite material; Preferably, the composition is obtained by a process comprising: Preferably, the polypropylene is prepared by polymerizing propylene and optionally ethylene in the presence of a metallocene catalyst having formula (I), preferably having formula (II).

[0106] Goods The present invention further relates to an article, preferably an automotive article, comprising at least 90% by weight, more preferably at least 95% by weight, of the fiber reinforced composite according to the present invention, even more preferably consisting of the fiber reinforced composite according to the present invention.

[0107] Particularly preferred automotive articles are dashboards and dashboard supports, bumper supports, door and tailgate load-bearing components, under-the-hood components such as ventilators and battery carriers, and under-floor protection elements.

[0108] Particularly preferred embodiments Based on the information provided above, the present invention relates to, inter alia, the following embodiments:

[0109] Thus, in a preferred embodiment, the fiber-reinforced composite according to the invention comprises: (a) 59 to 90% by weight of a propylene homopolymer based on the fiber reinforced composite material; (b) 9.0 to 40% by weight of short glass fibers based on the fiber-reinforced composite material; (c) 0.05 to 5.0% by weight of a compatibilizer based on the fiber-reinforced composite material; (d) 0.1 to 5.0% by weight of an additive based on the fiber-reinforced composite material; and the total amount of the propylene homopolymer, the short glass fiber, the compatibilizer and the additives in the fiber-reinforced composite is in the range of 98 to 100% by weight; Furthermore, The propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) in the range of 0.10 to 0.90%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iii) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.10 to 0.90% by weight; (iv) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 500 g / 10 min; and (v) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.0 to less than 4.0; having Preferably, the propylene homopolymer is not visbroken.

[0110] In another preferred embodiment, the fiber reinforced composite according to the present invention comprises: (a) 59 to 90% by weight of a propylene homopolymer based on the fiber reinforced composite material; (b) 9.0 to 40% by weight of short glass fibers based on the fiber-reinforced composite material; (c) 0.05 to 5.0% by weight of a compatibilizer based on the fiber-reinforced composite material; (d) 0.1 to 5.0% by weight of an additive based on the fiber-reinforced composite material; and the total amount of the propylene homopolymer, the short glass fiber, the compatibilizer and the additives in the fiber-reinforced composite is in the range of 98 to 100% by weight; Furthermore, The propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) in the range of 0.15 to 0.80% 13 2,1-site defects, as determined by C-NMR spectroscopy (iii) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.10 to 0.90% by weight; (iv) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 500 g / 10 min; and (v) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; having Preferably, the propylene homopolymer is not visbroken.

[0111] In yet another preferred embodiment, the fiber reinforced composite according to the invention preferably comprises: (a) 59 to 90% by weight of a propylene homopolymer based on the fiber reinforced composite material; (b) 9.0 to 40% by weight of short glass fibers based on the fiber-reinforced composite material; (c) 0.05 to 5.0% by weight of a compatibilizer based on the fiber-reinforced composite material; (d) 0.1 to 5.0% by weight of an additive based on the fiber-reinforced composite material; and the total amount of the propylene homopolymer, the short glass fiber, the compatibilizer and the additives in the fiber-reinforced composite is in the range of 98 to 100% by weight; Furthermore, The propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) in the range of 0.15 to 0.80%; 13 2,1-site defects, as determined by C-NMR spectroscopy (iii) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25°C) in the range of 0.10 to 0.90% by weight; (iv) a melt flow rate MFR2 (230°C, 2.16 kg) measured according to ISO 1133 in the range of 5.0 to 500 g / 10 min; and (v) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to less than 3.8; having Preferably, the propylene homopolymer is not visbroken, Furthermore, The short glass fibers have an average fiber length of 2.0 to 10.0 mm and an average diameter of 5 to 20 μm, The compatibilizer is maleic anhydride grafted polypropylene, and this maleic anhydride grafted polypropylene has a maleic anhydride content of 0.1 to 5% by weight.

[0112] In the following, the present invention will be illustrated by examples. EXAMPLES

[0113] 1. Determination method The following definitions of terms and determination methods apply to the above summary of the invention and the following examples, unless otherwise defined.

[0114] a) Melt flow rate The melt flow rate (MFR2) is determined according to ISO 1133 and is expressed in g / 10 min. The MFR2 of polypropylene is determined at a temperature of 230° C. and under a load of 2.16 kg.

[0115] b) Heat Deflection Temperature B (HDT B) Heat Deflection Temperature B (HDT B) is measured for an injection molded 80 x 10 x 4 mm 3 The test was performed at 0.45 MPa in accordance with ISO 75B using a test bar.

[0116] c) Cold xylene soluble fraction (XCS, wt%) The amount of polymer soluble in xylene is measured at 25.0°C according to ISO 16152; 1st edition; 2005-07-01.

[0117] d) Melting temperature T m and crystallization temperature Tc Melting temperature T m is determined by differential scanning calorimetry (DSC) according to ISO 11357-3 using a TA-Instruments 2920 Dual-Cell equipped with an RSC cooling device and a data station. Heating and cooling rates of 10 °C / min are applied in heat / cool / heat cycles between +23 and +210 °C. The crystallization temperature (T c ) is determined from the cooling process, and the melting temperature (T m ) and enthalpy of fusion (H m ) is determined in the second heating step.

[0118] e) Tensile modulus The tensile modulus and the elongation at break are determined according to ISO 527-2 using injection-molded test specimens (1B dog-bone shape, 4 mm thick) as described in EN ISO 1873-2.

[0119] f) Charpy impact strength Charpy impact strength was measured on 80x10x4mm specimens prepared according to EN ISO1873-2 3 The measurements were performed according to ISO 1791eU at +23°C using injection moulded bar specimens.

[0120] g) 13 Quantifying copolymer microstructure by C-NMR spectroscopy Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the comonomer content of the polymers. 13 C{ 1 The H}NMR spectrum 1 H and 13 All spectra were recorded in solution using a Bruker Advance III 400 NMR spectrometer operating at 400.15 MHz and 100.62 MHz for C, respectively. 13A 10 mm extended temperature probe head optimized for 3000 C was used and all air pressures were recorded using nitrogen gas. Approximately 200 mg of material was dissolved in 3 ml of 1,2-tetrachloroethane-d2 (TCE-d2) with chromium(III) acetylacetonate (Cr(acac)3) to give a 65 mM solution of the relaxation agent in the solvent (Singh, G., Kothari, A., Gupta, V., Polymer Testing 28 5 (2009), 475). To ensure a homogenous solution, the NMR tube was further heated in a rotating oven for at least 1 h after the initial sample preparation in a heat block. After insertion into the magnet, the tube was spun at 10 Hz. This setup was chosen mainly due to the high resolution and quantitativeness required for accurate ethylene content quantification. Standard single-pulse excitation without NOE was employed using an optimized tip angle, a recycle delay of 1 s and a bilevel WALTZ16 decoupling scheme (Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D., Winniford, B., J. Mag. Reson. 187 (2007) 225; Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J., Talarico, G., Macromol. Rapid Commun. 2007, 28, 1128). A total of 6144 (6k) transients were acquired per spectrum. quantitative 13 C{ 1 H}NMR spectra were processed and integrated using a proprietary computer program, and relevant quantitative properties were derived from the integrals. All chemical shifts were indirectly referenced to the central methylene group of the ethylene block (EEE) at 30.00 ppm using the chemical shift of the solvent. This approach allowed for comparable referencing in the absence of this structural unit. Characteristic signals corresponding to the incorporation of ethylene were observed (Cheng, HN, Macromolecules 17 (1984), 1950). If a characteristic signal corresponding to the 2,1-erythro regiodefect was observed (as described in L. Resconi, L. Cavallo, A. Fait, F. Piemontesi, Chem. Rev. 2000, 100(4), 1253; Cheng, HN Macromolecules 1984, 17, 1950; and WJ. Wang and S. Zhu, Macromolecules 2000, 33 1157), a correction for the effect of that regiodefect on the determined properties was necessary. No characteristic signals corresponding to other types of regiodefects were observed.

[0121] The comonomer fraction is 13 C{ 1 Quantification was performed using the method of Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000) 1157) by integration of multiple signals over the entire spectral range of the {H} spectrum. This method was chosen for its robustness and ability to take into account the presence of positional defects, if necessary. The integration range was slightly adjusted to increase applicability over the full range of comonomer contents encountered.

[0122] For systems in which only isolated ethylene in the PPEPP sequence is observed, the method of Wang et al. was modified to reduce the effect of non-zero integrals of sites known to be absent. This approach reduces the overestimation of ethylene content for such systems, which reduces the number of sites used to determine absolute ethylene content. E=0.5(Sββ+Sβγ+Sβδ+0.5(Sαβ+Sαγ)) This was accomplished by reducing it to With this set of sites, the corresponding integral equation can be written, using the same notation as used in Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157): E = 0.5(I H +I G +0.5(I C +I D )) The equation used for absolute propylene content was not modified. Comonomer incorporation in mole percent was calculated from the mole fraction. E [mol%] = 100 × fE Comonomer incorporation in weight percent was calculated from the mole fraction. E[weight%]=100×(fE×28.06) / ((fE×28.06)+((1-fE)×42.08))

[0123] h) Number average molecular weight (Mn), weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) Number average molecular weight (M n ), weight average molecular weight (M w ) and molecular weight distribution (M w / M n ) were determined by gel permeation chromatography (GPC) according to ISO16014-4:2003 and ASTM D6474-99. A PolymerChar GPC instrument equipped with an infrared (IR) detector was used with three Olexis columns and one Olexis Guard column from Polymer Laboratories, and 1,2,4-trichlorobenzene (TCB, stabilized with 250 mg / L of 2,6-di-tert-butyl-4-methyl-phenol) as the solvent at 160 °C and a constant flow rate of 1 mL / min. 200 μL of sample solution was injected per analysis. The above column set was calibrated using a universal calibration (according to ISO16014-2:2003) with at least 15 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol (mol) to 11500 kg / mol. The Mark Houwink constants for PS, PE and PP used are as described in ASTM D6474-99. All samples were prepared by dissolving 5.0-9.0 mg of polymer in 8 mL of stabilized TCB (same as mobile phase) (at 160 °C) for 2.5 h for PP or 3 h for PE at up to 160 °C with continuous slow shaking in the autosampler of the GPC instrument.

[0124] i) VOCs and FOGs VOC and FOG values ​​were determined according to VDA278 (October 2011; Thermal Desorption Analysis of Organic Emissions for the Characterization of Non-Metallic Materials for Automobiles, VDA Verband der Automobilindustrie) after sample preparation of injection molded plates according to EN ISO19069-2:2016. The plates were packed in aluminum composite foil immediately after production and the foil was sealed. According to VDA278 October 2011, the VOC value is defined as "the sum of readily to moderately volatile substances". It is calculated as toluene equivalent. The method described in this recommendation is to measure the VOC content of n-pentacosane (C 25 ) to determine and analyze substances with a boiling / elution range up to 1000 ppm. The FOG value is defined as the sum of the less volatile substances eluting from the retention time of n-tetradecane (including this). It is calculated as the hexadecane equivalent. 14 " ~ "C 32 " boiling point range substances are determined and analyzed.

[0125] j) Cloudy Haze was measured on compression molded specimens (diameter 80 mm ± 1 mm, thickness < 1 cm) cut from injection molded plates according to DIN 75201:2011-11, method B (gravimetric method). In this method, the mass in mg of the haze condensate on the aluminum foil is determined by weighing the foil before and after the haze test. The term "haze" refers to the fraction of volatile substances condensed on a glass part, such as for example the windshield of a vehicle.

[0126] k) Average fiber diameter The average fiber diameter is determined according to ISO 1888:2006(E), method B, microscope magnification 1000.

[0127] 2. Preparation of polypropylene a) Preparation of single-site catalytic system 1 Catalyst Complex The following metallocene complexes were used as described in WO 2019 / 179959: [ka]

[0128] Preparation of MAO-silica support A steel reactor equipped with a mechanical stirrer and a filter net was flushed with nitrogen and the reactor temperature was set at 20°C. Silica grade DM-L-303 (5.0 kg) from AGC Si-Tech Co, pre-calcined at 600°C, was then added from a feed drum followed by careful pressurization and depressurization with nitrogen using a manual valve. Toluene (22 kg) was then added. The mixture was stirred for 15 minutes. A 30 wt% solution of MAO in toluene (9.0 kg) from Lanxess was then added within 70 minutes via a feed line at the top of the reactor. The reaction mixture was then heated to 90°C and stirred at 90°C for another 2 hours. The slurry was allowed to settle and the mother liquor was filtered off. The catalyst was washed twice with toluene (22 kg) at 90°C followed by settling and filtration. The reactor was cooled to 60°C and the solid was washed with heptane (22.2 kg). Finally, the MAO-treated SiO2 was dried under nitrogen flow at 60° C. for 2 hours with stirring, then under vacuum (−0.5 barg) for 5 hours. The MAO-treated support was collected as a free-flowing white powder. The support was found to contain 12.2 wt. % Al.

[0129] Preparation of single-site catalytic system 1 0.7 kg of 30 wt% MAO in toluene was added to a steel nitrogen purged reactor via a burette at 20°C. 5.4 kg of toluene was then added with stirring. 93 g of the metallocene complex described in 2a) above was added from a metal cylinder followed by flushing with 1 kg of toluene. The mixture was stirred at 20°C for 60 minutes. 91 g of trityl tetrakis(pentafluorophenyl)borate was then added from a metal cylinder followed by flushing with 1 kg of toluene. The mixture was stirred at room temperature for 1 hour. The resulting solution was added over 1 hour to the stirred cake of MAO-silica support prepared as above. The cake was allowed to stand for 12 hours and then dried under stirring under N2 flow at 60°C for 2 hours and under vacuum (-0.5 barg) for a further 5 hours. The dried catalyst was sampled in the form of a pink free-flowing powder containing 13.9% Al and 0.11% Zr.

[0130] b) Preparation of single-site catalytic system 2 Catalyst Complex The following metallocene complexes were used as described in WO 2013 / 007650: [ka]

[0131] Preparation of MAO-silica support A steel reactor equipped with a mechanical stirrer and a filter net was flushed with nitrogen and the reactor temperature was set at 20°C. Silica grade DM-L-303 (7.4 kg) from AGC Si-Tech Co, pre-calcined at 600°C, was then added from a feed drum followed by careful pressurization and depressurization with nitrogen using a manual valve. Toluene (32.2 kg) was then added. The mixture was stirred (40 rpm) for 15 minutes. A 30 wt% solution of MAO in toluene (17.5 kg) from Lanxess was then added within 70 minutes via a 12 mm line at the top of the reactor. The reaction mixture was then heated to 90°C and stirred at 90°C for an additional 2 hours. The slurry was allowed to settle and the mother liquor was filtered off. The MAO treated silica support was washed twice with toluene (32.2 kg) at 90°C followed by settling and filtration. The reactor was cooled to 60°C and the solids were washed with heptane (32.2 kg). Finally, the MAO-treated SiO2 was dried at 60° C. for 2 hours under 0.3 barg pressure with 2 kg / h nitrogen flow and stirring at 5 rpm, then under vacuum (−0.5 barg) for 5 hours. The MAO-treated support was collected as a free-flowing white powder. The support was found to contain 12.7 wt. % Al.

[0132] Preparation of single-site catalytic system 2 In a nitrogen-filled glove box, a solution (1 mL) of 0.25 mL of MAO in dry toluene (30 wt% in toluene, AXION 1330 CA Lanxess) was added to an aliquot (30.0 mg, 38 μmol) of the metallocene complex described above in 2b). The mixture was stirred at room temperature for 60 minutes. The solution was then slowly added to 1.0 g of MAO-treated silica prepared as above, which was placed in a glass flask. The mixture was left overnight, washed with 5 mL of toluene, and then subjected to vacuum drying for 1 hour to obtain a pink, free-flowing powder, yielding 1.1 g of the above catalyst as a pink, free-flowing powder. Catalyst system 2 has an Al content of 12.5 wt%, a Zr content of 0.248 wt% and an Al / Zr molar ratio of 170 mol / mol.

[0133] c) Preparation of Ziegler-Natta catalyst system 3 A Ziegler-Natta catalyst system is used. Chemicals used: Butylethylmagnesium (Mg(Bu)(Et), BEM) 20% solution in toluene provided by Chemtura 2-Ethylhexanol provided by Amphochem; 3-Butoxy-2-propanol (DOWANOL™ PnB) provided by Dow; Bis(2-ethylhexyl) citraconic acid provided by SynphaBase TiCl4 provided by Millenium Chemicals, Toluene provided by Aspokem Viscoplex® 1-254 provided by Evonik; Heptane provided by Chevron.

[0134] Preparation of Mg alkoxy compounds The Mg-alkoxide solution was prepared in a 20 L stainless steel reactor by adding a mixture of 4.7 kg 2-ethylhexanol and 1.2 kg butoxypropanol to 11 kg of a 20 wt % solution of butylethylmagnesium (Mg(Bu)(Et)) in toluene with stirring (70 rpm). The reactor contents were maintained below 45° C. during the addition. After the addition was complete, mixing (70 rpm) of the reaction mixture was continued at 60° C. for 30 minutes. After cooling to room temperature, 2.3 kg of the donor bis(2-ethylhexyl) citraconic acid was added to the above Mg-alkoxide solution while maintaining the temperature below 25° C. Mixing was continued for 15 minutes with stirring (70 rpm).

[0135] Preparation of solid catalyst components 20.3 kg TiCl4 and 1.1 kg toluene were added to a 20 L stainless steel reactor. 14.5 kg of the prepared Mg alkoxy compound were added over 1.5 hours while mixing at 350 rpm and keeping the temperature at 0° C. 1.7 L Viscoplex® 1-254 and 7.5 kg heptane were added and after 1 hour of mixing at 0° C. the temperature of the formed emulsion was raised to 90° C. within 1 hour. After 30 minutes the mixing was stopped, the catalyst droplets were allowed to solidify and the formed catalyst particles were allowed to settle. After settling (1 hour) the supernatant liquid was siphoned off. The catalyst particles were then washed with 45 kg toluene at 90° C. for 20 minutes followed by two washes with heptane (30 kg, 15 minutes). During the first heptane wash the temperature was lowered to 50° C. and during the second wash it was lowered to room temperature. The catalyst thus obtained was used together with triethylaluminum (TEAL) as cocatalyst and dicyclopentyldimethoxysilane (D donor) as donor in the following ratios: TEAL / Ti: 250 mol / mol TEAL / donor: 10 mol / mol

[0136] [Table 1]

[0137] [Table 2]

[0138] Inventive Examples IE1 and IE2 and Comparative Examples CE1 and CE2 were prepared by compounding on a co-rotating twin screw extruder (Coperion ZSK40) with a mixing screw typical for glass fiber compounds and an L / D ratio of 43. The following process parameters were used: -Throughput of 100kg / h, Screw speed: 100~150rpm Barrel temperature of 220-250°C, rising from the feed zone and falling again towards the die plate, Die plate with 4mm diameter hole and 3 strands

[0139] Polypropylene and short glass fibers, as well as other additives, were fed into the extruder and melt-mixed in the second barrel. The first mixing zone for mixing polypropylene and additives is located between the third and fifth barrels. Short glass fibers were added in the sixth barrel using a side feeder. The second mixing zone for glass fiber dispersion is located between the seventh and twelfth barrels.

[0140] The composites and their properties are summarized in Table 3.

[0141] [Table 3]

[0142] The glass fibers used were ECS03T-480H, a commercially available product from Nippon Electric Glass, with an average fiber length of 3.0 mm and an average diameter of 10 μm. The following additive combination was used in the formulation: 0.2 wt.% tris(2,4-di-t-butylphenyl)phosphite (CAS number 31570-04-4, commercially available as Irgafos 168 from BASF AF, Germany), 0.1 wt.% pentaerythrityl-tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)-propionate (CAS number 6683-19-8, commercially available as Irganox 1010 from BASF AF, Germany), and 0.2 wt.% carbon black masterbatch "Plasblak PPP6331" from Cabot Corporation, Germany. The compatibilizer is a commercially available maleic anhydride grafted polypropylene from BYK, "Scona TPPP 8112 GA," with a maleic anhydride content of 1.4 wt. % and a MFR2 of greater than 80 g / 10 min.

Claims

1. A fiber-reinforced composite material, (a) 59 to 90 weight percent polypropylene, based on the fiber reinforced composite; (b) 9.0 to 40% by weight of short glass fibers having an average fiber length in the range of 2.0 to 10.0 mm, based on the fiber-reinforced composite material; (c) 0.05 to 5.0% by weight of a compatibilizer based on the fiber-reinforced composite material; and the total amount of the polypropylene, the short glass fibers, and the compatibilizer in the fiber reinforced composite is at least 95% by weight; Furthermore, The polypropylene is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 152-160°C; (ii) 0.5% by weight or less, 13 comonomer content determined by C-NMR spectroscopy, said comonomer being ethylene; (iii) a molecular weight distribution (MWD), as determined by gel permeation chromatography (GPC), in the range of 1.0 to less than 4.0; and (iv) in the range of 0.10 to 0.90%; 13 2,1-site defects determined by C-NMR spectroscopy A fiber-reinforced composite material having the structure.

2. 2. The fiber reinforced composite of claim 1, wherein the polypropylene has a xylene cold solubles (XCS) percentage measured according to ISO 16152 (25°C) in the range of 0.05 to 1.0 wt%.

3. 3. A fiber reinforced composite according to claim 1 or claim 2, wherein the polypropylene forms a continuous phase in which the fibers are embedded.

4. The polypropylene has a melt flow rate (MFR) measured according to ISO 1133 in the range of 5.0 to 500 g / 10 min. 2 The fiber-reinforced composite material according to any one of claims 1 to 3, having a compressive strength of 230°C, 2.16 kg.

5. 5. A fiber reinforced composite material according to any one of claims 1 to 4, wherein the polypropylene is a single-phase polypropylene.

6. The fiber reinforced composite material is (a) 59 to 90 weight percent of the polypropylene, based on the fiber reinforced composite; (b) 9.0 to 40% by weight of short glass fibers based on the fiber-reinforced composite material; (c) 0.05 to 5.0 wt. % of the compatibilizer, based on the fiber reinforced composite; and (d) 0.1 to 5.0 wt. % of an additive based on the fiber-reinforced composite material; The fiber-reinforced composite material according to any one of claims 1 to 5, comprising:

7. A fiber reinforced composite material according to any one of claims 1 to 6, wherein the polypropylene is not visbroken.

8. 6. The fiber reinforced composite of claim 5, wherein the single phase polypropylene is a propylene homopolymer.

9. The propylene homopolymer is (i) a melting temperature Tm, determined by DSC according to ISO 11357-3 (heating and cooling rate 10°C / min), in the range of 153-159°C; (ii) a molecular weight distribution (MWD) as determined by gel permeation chromatography (GPC) in the range of 1.6 to 3.8; (iii) a percentage of xylene cold solubles (XCS) measured in accordance with ISO 16152 (25° C.) in the range of 0.10 to 0.90 weight percent; and (iv) in the range of 0.15 to 0.80% 13 2,1-site defects determined by C-NMR spectroscopy The fiber reinforced composite material according to claim 8, having the formula:

10. the polypropylene being produced by polymerizing propylene and optionally ethylene in the presence of a metallocene catalyst having the formula (I): 【Chemistry 1】 In the formula (I), each R 1 are independently the same or different and are hydrogen or linear or branched C 1 ~C 6 alkyl group, at least one R per phenyl group 1 is not hydrogen, R' is C 1 ~C 10 is a hydrocarbyl group, X is independently a hydrogen atom, a halogen atom, 1 ~C 6 Alkoxy group, C 1 ~C 6 The method for producing a fiber-reinforced composite material according to any one of claims 1 to 9, wherein the group is an alkyl group, a phenyl group or a benzyl group.

11. 2. The fiber-reinforced composite material according to claim 1, wherein the short glass fibers have an average diameter of 5 to 20 μm.

12. The fiber reinforced composite material according to any one of claims 1 to 9 and claim 11, wherein the compatibilizer is a polar modified polypropylene.

13. The method of claim 1, wherein the compatibilizer has a maleic anhydride content of 0.1 to 5.0 wt. % and a melt flow rate MFR measured in accordance with ISO 1133 in the range of 80 to 250 g / 10 min. 2 13. The fiber reinforced composite material according to claim 12, which is a maleic anhydride grafted polypropylene having a compressive strength of 190° C., 2.16 kg.

14. A method for producing a fiber-reinforced composite material according to any one of claims 1 to 9 and claims 11 to 13, (a) the polypropylene; (b) the short glass fibers; (c) the compatibilizer, and (d) Optionally, additives and extruding the mixture to obtain the fiber-reinforced composite material. The polypropylene is produced by polymerizing propylene and optionally ethylene in the presence of a metallocene catalyst having the formula (I): 【Chemistry 2】 In the formula (I), each R 1 are independently the same or different and are hydrogen or linear or branched C 1 ~C 6 alkyl group, at least one R per phenyl group 1 is not hydrogen, R' is C 1 ~C 10 is a hydrocarbyl group, X is independently a hydrogen atom, a halogen atom, 1 ~C 6 Alkoxy group, C 1 ~C 6 is an alkyl group, a phenyl group, or a benzyl group. method.

15. 14. An article comprising at least 90% by weight of the fiber reinforced composite material of any one of claims 1 to 9 and claims 11 to 13.

Citation Information

Patent Citations

  • Propylene resin composition and pellet thereof and molded body made from the same

    JP2008179784A

  • Polypropylene modified with maleic anhydride and resin composition containing the same

    JP2009114435A

  • Filament-reinforced thermoplastic resin particle

    JP2010106263A

  • Catalysts for olefin polymerization

    WO2019179959A1